Crosslinkable rubber compound, vulcanizate thereof, and use of the rubber compound or vulcanizate
A crosslinkable rubber mixture with a peroxide-sulfur combination and specific diene rubbers and fillers enhances snow performance in tires and rubber articles without compromising other essential properties like wet and dry braking and handling.
Patent Information
- Application Number
- DE102019212916
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-08-28
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2039-08-28
AI Technical Summary
Existing rubber compositions for tires and other rubber articles face a challenge in achieving improved snow performance, such as traction and braking on snowy roads, without negatively affecting wet and dry braking, handling behavior, and rolling resistance.
A crosslinkable rubber mixture combining a peroxide crosslinking system with a sulfur vulcanization system, incorporating specific diene rubbers, fillers like silica and carbon black, and additives to enhance snow performance while maintaining or improving other properties.
The rubber mixture achieves enhanced snow traction and braking on snowy roads while maintaining or improving wet and dry braking, handling behavior, and rolling resistance.
Abstract
Description
[0001] The invention relates to a crosslinkable rubber mixture, a vulcanizate thereof, and a use of the Rubber mixture or vulcanizate.
[0002] The rubber composition of the tread largely determines the driving characteristics of a tire, especially of a pneumatic vehicle tire. Likewise, the rubber compounds used in belts, hoses and straps Used especially in areas subject to high mechanical stress, for stability and longevity of these Rubber products are essentially responsible for these rubber compounds. Therefore, these rubber compounds are used for pneumatic vehicle tires, belts, Belts and hoses are subject to very high demands.
[0003] It is known in the prior art that a rubber compound is vulcanized either with peroxide or with sulfur US 20170247533 A1 discloses rubber compounds with either a peroxide or a Sulfur vulcanization system comprising sulfur and vulcanization accelerator.
[0004] EP 1 033 386 A1 discloses a composition containing 0.5 to 10 phr of a peroxide and 0.05 to 0.6 phr elemental sulfur.
[0005] WO 2016 / 169945 A1, WO 2017 / 055168 A1 and WO 2018 / 111274 A1 each disclose a composition containing an organic peroxide and sulfur.
[0006] WO 2016 / 069012 A1 discloses a rubber part based on a composition containing a two- Components crosslinking system consisting of a peroxide and sulfur.
[0007] WO 2017 / 019235 A1 discloses a composition containing 1.8 to 3.6 phr of a sulfur donor / - accelerator and 0.2 to 2 phr of a peroxide.
[0008] US 2017 / 0314631 A1 discloses an SBR-containing composition further comprising a crosslinking system comprising sulfur, a sulfur-donating compound and an organic peroxide.
[0009] DE 10 2017 101 817 A1 discloses a sealing profile with a composition preferably containing Sulfur and a peroxide.
[0010] It is known that when the composition of the tyre, especially the tread, is changed, targeted Improvements can be achieved. Many properties are in conflict with each other, so that the Improvement in one characteristic leads to deterioration in another characteristic.
[0011] For tires used particularly in winter conditions, properties on snow and ice, such as snow traction, but also braking on wet roads. Furthermore, the tire should but also under normal conditions continue to meet the requirements, especially with regard to handling and Dry braking is sufficient.
[0012] It is also known that the influence of a formulation measure on the tire properties can be determined by indicators / Predictors can be determined on laboratory mixtures or vulcanizates.
[0013] The invention is based on the object of providing a crosslinkable rubber mixture by means of which better snow performance, such as traction and braking on snowy roads, is achieved, while the remaining Properties such as wet and dry braking and handling, for example when cornering, and the Rolling resistance behavior is not significantly negatively affected or may even be improved.
[0014] The object is achieved according to the invention by the crosslinkable rubber mixture according to claim 1.
[0015] Surprisingly, it was found that such a rubber mixture has an improved level of properties and in particular shows improved snow performance without the further physical properties significantly negatively. In particular, the combination according to the invention of at least one peroxidic compound and a Sulphur vulcanization system improved snow performance indicators, especially snow traction and Snow braking, while the indicators for wet and dry braking and handling behavior were not be significantly negatively affected or even improved.
[0016] A further subject of the present invention is a vulcanizate of at least one inventive Rubber compound. A further object of the present invention is the use of the vulcanizate according to the invention in at least a component of a vehicle tire. Preferably, the vehicle tire comprises the at least one vulcanizate at least in Tread on. The vulcanizate according to the invention and its use according to the invention in at least one component of a Vehicle tires are characterized by an improvement in snow performance. At the same time, they have a very good handling and very good braking performance.
[0017] In the case of two-part treads (upper part: cap and lower part: base), the inventive Rubber compound can be used for both the cap and the base. Preferably, at least the cap or at least the base or at least the cap and the base at least one vulcanizate according to the invention of the rubber mixture according to the invention. The rubber mixture according to the invention is also suitable for treads made of different and / or tread compounds arranged one below the other (multi-component tread).
[0018] In the context of the present invention, vehicle tires are understood to mean pneumatic vehicle tires and solid rubber tires, including tires for industrial and construction vehicles, truck, car and two-wheel tires. The rubber mixture according to the invention is also suitable for other components of vehicle tires, such as especially the horn profile, as well as for internal tire components. The rubber mixture according to the invention is also suitable for other technical rubber articles, such as bellows, Suitable for conveyor belts, air springs, belts, straps or hoses, as well as shoe soles. A further object of the present invention is the use of the rubber mixture according to the invention for Manufacture of a rubber article, in particular an air spring, a bellows, conveyor belt, strap, belt, hose, Rubber band, profile, seal, membrane, tactile sensors for medical applications or Robotic applications, or a shoe sole or parts thereof.
[0019] In the following, the components of the crosslinkable rubber mixture according to the invention are described in more detail All statements also apply to the vulcanizate according to the invention and the Use of the vulcanizate according to the invention in at least one component of a vehicle tire.
[0020] The term phr (parts per hundred parts of rubber by weight) used in this document is the term used in the The dosage of the parts by weight of the individual substances is calculated in this document to 100 parts by weight of the total mass of all rubbers present in the mixture related to a molecular weight M according to GPC of greater than 20000 g / mol. w
[0021] The rubber mixture according to the present text generally contains at least one diene rubber, whereby the Rubber compound a diene rubber or a mixture of two or more different diene rubbers may contain.
[0022] Diene rubbers are rubbers obtained by polymerization or copolymerization of dienes and / or cycloalkenes and thus C=C double bonds either in the main chain or in the side groups have. The diene rubber is preferably selected from the group consisting of natural polyisoprene (NR), synthetic polyisoprene (IR), epoxidized polyisoprene (ENR), butadiene rubber (BR), butadiene-isoprene rubber, solution-polymerized styrene-butadiene rubber (SSBR), emulsion-polymerized styrene-butadiene rubber (ESBR), Styrene-isoprene rubber, liquid rubbers with a molecular weight M of greater than 20000 g / mol, halobutyl w Rubber, polynorbornene, isoprene-isobutylene copolymer, ethylene-propylene-diene rubber, nitrile rubber, chloroprene Rubber, acrylate rubber, fluorine rubber schuk, silicone rubber, polysulfide rubber, epichlorohydrin rubber, styrene-isoprene-butadiene terpolymer, hydrogenated Acrylonitrile butadiene rubber and hydrogenated styrene butadiene rubber.
[0023] In particular, nitrile rubber, hydrogenated acrylonitrile butadiene rubber, chloroprene rubber, butyl rubber, Halobutyl rubber and / or ethylene-propylene-diene rubber are used in the production of technical Rubber articles such as belts, straps and hoses, and / or shoe soles. The specialist for these rubbers known - with regard to fillers, plasticizers, vulcanization systems and additives special - mixture compositions preferred application.
[0024] The natural and / or synthetic polyisoprene of all embodiments can be either cis- 1,4-polyisoprene as well as 3,4-polyisoprene.
[0025] However, the use of cis-1,4-polyisoprenes with a cis-1,4 content of > 90 wt.% is preferred. Such a polyisoprene can be prepared by stereospecific polymerization in solution with Ziegler-Natta catalysts or under using finely dispersed lithium alkyls. On the other hand, natural rubber (NR) is such a cis-1,4 polyisoprene in which the cis-1,4 content in the natural rubber is greater than 99 wt.%. Furthermore, a mixture of one or more natural polyisoprenes with one or more synthetic Polyisoprene(s) are conceivable.
[0026] In the context of the present invention, the term ´´natural rubber´´ means naturally occurring rubber which can be obtained from Hevea rubber trees and non-Hevea sources. Non-Hevea sources Examples include Guayule shrubs and dandelions such as TKS (Taraxacum kok-saghyz; Russian dandelion).
[0027] If the rubber mixture according to this text contains butadiene rubber (= BR, polybutadiene), can be any type known to the expert, including the so-called high-cis and low-cis Types, where polybutadiene with a cis content greater than or equal to 90 wt.% is considered high-cis type and polybutadiene with a cis content of less than 90 wt.% is referred to as low-cis type. A low-cis polybutadiene is, for example, Li-BR (lithium-catalyzed Butadiene rubber) with a cis content of 20 to 50 wt.%. With a high-cis BR, particularly good Properties and low hysteresis of the rubber compound are achieved. The polybutadiene(s) used can be modified and functionalized end-group modified and / or functionalized along the polymer chains. The modification can be those with hydroxy groups and / or ethoxy groups and / or epoxy groups and / or siloxane groups and / or amino- Groups and / or aminosiloxane and / or carboxy groups and / or phthalocyanine groups and / or silane sulfide groups However, there are also other modifications known to the expert, also known as functionalizations Metal atoms can be a component of such functionalizations.
[0028] In the event that at least one styrene-butadiene rubber (styrene-butadiene copolymer) is present in the rubber mixture It can be either solution-polymerized styrene-butadiene rubber (SSBR) or emulsion-polymerized styrene-butadiene rubber (ESBR), whereby a mixture of at least one SSBR and at least one ESBR. The terms ´´styrene-butadiene rubber´´ and ´´styrene-butadiene Copolymer'' are used synonymously in the present invention. The styrene-butadiene copolymer used can be modified with the polybutadiene modifications mentioned above and Functionalizations can be end-group modified and / or functionalized along the polymer chains.
[0029] Preferably, the at least one diene rubber is selected from the group consisting of natural Polyisoprene (NR, natural rubber), synthetic polyisoprene (IR), butadiene rubber (BR), solution-polymerized styrene- Butadiene rubber (SSBR), emulsion-polymerized styrene-butadiene rubber (ESBR), butyl rubber (IIR) and Halobutyl rubber.
[0030] According to a particularly preferred embodiment, the at least one diene rubber is selected from the Group consisting of natural polyisoprene (NR), synthetic polyisoprene (IR), butadiene rubber (BR), solution-polymerized styrene-butadiene rubber (SSBR) and emulsion-polymerized styrene-butadiene rubber (ESBR). A polymer system made of one or more of the rubbers mentioned above performs the task particularly well solved. This allows the properties of the rubber compound to be optimized, both in terms of the underlying task and other properties can be adjusted, especially by blending different polymers (Rubbers) certain tire properties can be adjusted more precisely.
[0031] The rubber mixture according to the invention therefore contains at least one natural polyisoprene (NR) in Amounts of 5 to 25 phr, preferably 5 to 20 phr. Such a rubber mixture shows good processability and Reversion stability as well as optimized tear properties and optimal rolling resistance behavior.
[0032] The rubber mixture according to the invention therefore contains at least one polybutadiene (BR, butadiene rubber) and in amounts of 10 to 50 phr, and according to a particularly advantageous embodiment of the invention 15 to 40 phr. This results in particularly good tear and abrasion properties of the rubber mixture according to the invention and a optimal braking performance is achieved.
[0033] The rubber mixture according to the invention therefore contains at least one solution-polymerized styrene-butadiene Rubber (SSBR) in amounts of 30 to 80 phr, and according to a particularly advantageous embodiment of the Invention 50 to 70 phr. This ensures particularly good rolling resistance properties of the inventive rubber compound. SSBR is used in combination with at least one other rubber to create a to achieve an optimal and balanced property profile.
[0034] Preferably, the crosslinkable rubber mixture according to the present text contains at least one filler, preferably in amounts of 30 to 500 phr, particularly preferably 50 to 400 phr, again preferably 80 to 300 phr. According to advantageous embodiments, the filler is a reinforcing filler, which is preferably selected from the Group consisting of carbon blacks and silicas.
[0035] The rubber mixture according to the invention contains at least one silica as filler in amounts of 30 to 500 phr, particularly preferably 50 to 400 phr, again preferably 80 to 300 phr. In these amounts, silica is particularly suitable as the sole or main filler (more than 50 wt.% based on the total filler content).
[0036] According to further advantageous embodiments, the rubber mixture according to the present text contains at least one silica as a further filler, preferably in amounts of 5 to 100 phr, particularly preferably 5 to 80 phr, again preferably 10 to 60 phr. In these quantities, silica is particularly suitable as an additional filler in addition to another main filler, such as in particular soot.
[0037] The silica can be the silica types known to the person skilled in the art which are used as fillers for Tire rubber compounds are suitable. However, it is particularly preferred if a finely divided, precipitated Silica is used which has a nitrogen surface area (BET surface area) (according to DIN ISO 9277 and DIN 66132) of 35 2 2 2 to 400 m / g, preferably from 35 to 350 m / g, particularly preferably from 85 to 320 m / g and most particularly preferably from 2 2 2 120 to 235 m / g, and a CTAB surface area (according to ASTM D 3765) of 30 to 400 m / g, preferably of 30 to 330 m / g, 2 2 particularly preferably from 80 to 300 m / g and most preferably from 115 to 200 m / g. Such Silica, for example, leads to particularly good physical properties in rubber compounds for tire treads of the vulcanizates. In addition, advantages in compound processing can be achieved by reducing the mixing time while maintaining consistent product properties, leading to improved productivity. As silicas can be used, for example, both those of the type Ultrasil® VN3 (trade name) from Evonik and highly dispersible Silicas, so-called HD silicas (e.g. Zeosil® 1165 MP from Solvay), are used.
[0038] In the case that at least two different silicas, which differ, for example, by their BET surface area differ, are contained in the rubber mixture according to the invention, the above-mentioned Quantities refer to the total amount of all silicas contained.
[0039] The terms ´´silicic acid´´ and ´´silica´´ are used synonymously in the context of the present invention.
[0040] The rubber mixture may also contain other fillers, such as carbon black, especially industrial carbon black or Pyrolysis carbon blacks, or other fillers that have a reinforcing or non-reinforcing effect. Other (non-reinforcing) fillers in the context of the present invention include alumosilicates, kaolin, Chalk, starch, magnesium oxide, titanium dioxide or rubber gels as well as fibers (such as aramid fibers, glass fibers, carbon fibers, cellulose fibers). Other reinforcing fillers include carbon nanotubes (CNTs) including discrete CNTs, so-called hollow carbon fibers (HCF) and modified CNTs containing one or more functional groups, such as Hydroxy, carboxy and carbonyl groups), graphite and graphene and so-called ´´carbon-silica dual-phase filler´´. Zinc oxide is not considered a filler in the context of the present invention.
[0041] According to particularly advantageous embodiments of the invention, the rubber mixture according to the invention contains 0.1 to 60 phr, preferably 3 to 40 phr, particularly preferably 5 to 30 phr, most preferably 5 to 15 phr, at least one carbon black. In these amounts, carbon black is particularly suitable as an additional filler in addition to a main filler, such as especially silica.
[0042] According to further advantageous embodiments, the rubber mixture according to the present text contains 30 to 300 phr, preferably 30 to 200 phr, particularly preferably 40 to 100 phr of at least one carbon black. In these amounts, carbon black is as sole or main filler and possibly in combination with silica in the above mentioned lower quantities contained. All types of soot known to the expert person can be considered as soot. In one embodiment, the carbon black has an iodine number, according to ASTM D 1510, also referred to as iodine adsorption number, between 30 and 250 g / kg, preferably 30 to 180 g / kg, particularly preferably 40 to 180 g / kg, and most preferably 80 to 150 g / kg, and a DBP number according to ASTM D 2414 of 30 to 200 ml / 100 g, preferably 70 to 200 ml / 100 g, especially preferably 90 to 200 ml / 100g.
[0043] The DBP number according to ASTM D 2414 determines the specific absorption volume of a carbon black or a light Filler using dibutyl phthalate. The use of such a type of carbon black in the rubber compound, especially for vehicle tires, ensures a best possible compromise between abrasion resistance and heat build-up, which in turn meets the ecologically relevant Rolling resistance is influenced. It is preferred if only one type of carbon black is used in the respective rubber compound but different types of carbon black can also be mixed into the rubber mixture.
[0044] According to a particularly advantageous embodiment of the invention, the rubber mixture contains 5 to 60 phr, particularly preferably 5 to 40 phr, of at least one carbon black and 50 to 300 phr, preferably 80 to 200 phr of at least one Silica.
[0045] The rubber mixture according to the invention is crosslinkable and contains vulcanization chemicals as described in Claim 1 stated. The special feature of the rubber mixture according to the invention is that it contains a combination of chemicals for the Peroxide crosslinking and sulfur crosslinking. It is known in the art that a rubber compound is vulcanized either with peroxide or with sulfur can be, see above.
[0046] The terms ´´vulcanized´´ and ´´crosslinked´´ are used synonymously in the context of the present invention.
[0047] The crosslinkable rubber mixture according to the invention contains 0.5 phr or more of a peroxidic compound. The peroxidic compound can in principle be any peroxidic compound that is capable of To crosslink a rubber mixture containing at least one diene rubber.
[0048] According to particularly advantageous embodiments of the invention, the peroxidic compound used is at least Contains dicumyl peroxide.
[0049] According to particularly advantageous embodiments of the invention, the amount of at least one peroxidic compound 0.5 to 5 phr, preferably 0.5 to 4 phr and particularly preferably 0.5 to 3 phr, again preferably 1 to 3 phr.
[0050] The quantity refers to the total amount of peroxidic compounds. However, this does not include the preferred Possibility includes containing at least dicumyl peroxide as at least one peroxidic compound, wherein the amount of dicumyl peroxide to the total amount and preferably 0.1 to 5 phr, particularly preferably 0.5 to 5 phr, particularly preferably 0.5 to 4 phr and again particularly preferably 0.5 to 3 phr, again very particularly preferably 1 up to 3 phr.
[0051] The crosslinkable rubber mixture according to the invention contains a sulfur vulcanization system. Suitable Chemicals which cause sulfur crosslinking of a rubber mixture comprising at least one diene rubber, are known to the person skilled in the art. These include in particular sulfur and / or sulfur donors, ie sulphur-donating substances, and if necessary one or more suitable for sulphur vulcanization Vulcanization accelerator. Some vulcanization accelerators can also act as sulfur donors and vice versa.
[0052] The terms ´´vulcanization accelerator´´ and ´´accelerator´´ are used in the context of the present invention used synonymously.
[0053] According to advantageous embodiments of the invention, the rubber mixture contains sulfur and / or Sulphur donor and preferably also one or more accelerators, especially if the sulphur donor does not already act as an accelerator.
[0054] The accelerator is preferably selected from the group consisting of thiazole accelerators and / or Mercapto accelerators and / or sulfenamide accelerators and / or thiocarbamate accelerators and / or Thiuram accelerators and / or thiophosphate accelerators and / or thiourea accelerators and / or xanthate Accelerators and / or guanidine accelerators and / or polyetheramine accelerators.
[0055] According to advantageous embodiments of the invention, it is preferred that at least one Sulfenamide accelerator is included, which is preferably selected from the group consisting of N-cyclohexyl-2- benzothiazolesufenamide (CBS) and / or N,N-dicyclohexylbenzothiazole-2-sulfenamide (DCBS) and / or benzothiazyl-2- sulfenemorpholide (MBS) and / or N-tert.butyl-2-benzothiazylsulfenamide (TBBS).
[0056] As a sulphur-donating substance, all sulphur-donating substances known to the person skilled in the art If the rubber mixture contains a sulfur-donating substance, this is preferably selected from the group containing, for example, thiuram disulfides, such as tetrabenzylthiuram disulfide (TBzTD) and / or Tetramethylthiuram disulfide (TMTD) and / or tetraethylthiuram disulfide (TETD), and / or thiuram tetrasulfides, such as Dipentamethylenethiuram tetrasulfide (DPTT), and / or dithiophosphates, such as DipDis (bis-(diisopropyl)thiophosphoryl disulfide) and / or bis(O,O-2-ethylhexyl-thiophosphoryl)polysulfide (e.g. Rhenocure SDT 50®, Rheinchemie GmbH) and / or zinc dichloryldithiophosphate (e.g. Rhenocure ZDT / S®, Rheinchemie GmbH) and / or zinc alkyl dithiophosphate, and / or 1,6-bis(N,N-dibenzylthiocarbamoyldithio)hexane and / or diaryl polysulfides and / or Dialkyl polysulfides.
[0057] According to advantageous embodiments of the invention, it is preferred that at least thiuram disulfides, such as particularly preferably tetrabenzylthiuram disulfide (TBzTD), as a sulfur-donating substance. TBzTD has at the same time an accelerating effect. Other network-forming systems, such as those sold under the trade names Vulkuren®, Duralink® or Perkalink® or network-forming systems as described in WO 2010 / 049216 A2 can be used in The rubber compound can be used. This system contains a vulcanizing agent which has a functionality greater than four cross-linked and at least one vulcanization accelerator.
[0058] Elemental sulfur can be added to the rubber mixture in dosage forms known to the person skilled in the art for example as pure elemental sulfur or oil-extended sulfur.
[0059] The required amount of additional sulfur in the form of elemental sulfur and / or additional sulfur donor depends on the area of application of the respective rubber compound.
[0060] According to advantageous embodiments, the crosslinkable rubber mixture contains 0.3 to 4.0 phr, preferably 0.3 to 3.5 phr, particularly preferably 0.4 to 3.0 phr elemental sulfur. According to advantageous embodiments, the crosslinkable rubber mixture contains 0 to 4.0 phr, preferably 0.5 to 3.2 phr, particularly preferably 0.75 to 3.0 phr of sulphur donor, in particular a thiuram disulfide such as TBzTD as Sulfur donor.
[0061] According to an advantageous development of the invention, several accelerators are used. According to an advantageous embodiment of the invention, at least one sulfenamide accelerator, especially preferably TBBS, in combination with at least one guanidine accelerator, preferably DPG (diphenylguanidine), and at least one sulfur donor, preferably TBzTD.
[0062] According to advantageous embodiments, the crosslinkable rubber mixture contains 0 to 6.0 phr, preferably 0.5 to 4.5 phr particularly preferably 0.8 to 3.5 guanidine accelerators, such as in particular DPG.
[0063] According to advantageous embodiments, the crosslinkable rubber mixture contains 0.5 to 6.0 phr, preferably 1.0 to 4.5, particularly preferably 1.1 to 3.8 phr of sulfenamide accelerators, such as in particular TBBS and / or CBS.
[0064] In addition, vulcanization retarders may be present in the rubber mixture.
[0065] The vulcanization chemicals mentioned, i.e. peroxide and sulfur vulcanization system, are used in the Production of the rubber mixture especially in the last mixing step.
[0066] According to advantageous embodiments of the invention, the rubber mixture contains at least one Anti-aging agents, preferably in total amounts of 0.5 to 15 phr, particularly preferably 0.5 to 10 phr, in turn preferably 2 to 7 phr.
[0067] The at least one anti-aging agent can in principle be any anti-aging agent which is suitable for preventing or slowing down the aging of a rubber compound. Ozone protection waxes are not considered anti-aging agents in the context of the invention.
[0068] According to advantageous embodiments of the invention, the anti-aging agent is selected from para- Phenylenediamines and secondary aromatic amines, especially dihydroquinolines.
[0069] According to advantageous embodiments of the invention, the rubber mixture contains as an anti-aging agent at least one dihydroquinoline and at least one para-phenylenediamine, in particular at least two para- Phenylenediamines, for example two para-phenylenediamines.
[0070] It is preferred that the dihydroquinoline is selected from the group consisting of 2,2,4-trimethyl-1,2- dihydroquinoline (TMQ) and 6-ethoxy-2,2,4-trimethyl-1,2-dihydroquinoline (ETMQ).
[0071] According to a particularly advantageous embodiment of the invention, the dihydroquinoline is 2,2,4-trimethyl-1,2- dihydroquinoline (TMQ). The object of the invention is achieved particularly well with the preferably selected dihydroquinolines.
[0072] The para-phenylenediamine can be any substance known to the person skilled in the art, such as N-phenyl- N'-(1,3-dimethylbutyl)-p-phenylenediamine (6PPD), N,N'-diphenyl-p-phenylenediamine (DPPD), N,N'-ditolyl-p-phenylenediamine (DTPD), N-Isopropyl-N'-phenyl-p-phenylenediamine (IPPD), Phenyl[4-({[4-({[4-(phenylamino)phenyl]amino}ethyl)phenyl]ethyl} amino)phenyl]amine, phenyl{4-[2-{[4-(phenylamino)phenyl]amino}ethyl)amino]phenyl}amine, (1-methyl-2-{[-(phenylamino) phenyl]amino}propyl)[4-(phenylamino)phenyl]amine, N-(1,3-dimethylbutyl) -N'-(4-cumylphenyl)-p-phenylenediamine, N,N'-Di (1,4dimethylpentyl)-p-phenylenediamine (77PD), N,N'-Di(1-ethyl, 4-methyl-hexyl)-p-phenylenediamine (88PD), N,N'Bis-(1-ethyl-3- methylpentyl)-p-phenylenediamine (DOPD) and N,N'-di-β-naphthyl-p-phenylenediamine (DNPD).
[0073] It is preferred that the para-phenylenediamine is selected from the group consisting of N-phenyl-N'-(1,3- dimethylbutyl)-p-phenylenediamine (6PPD), N,N'-diphenyl-p-phenylenediamine (DPPD), N,N'-ditolyl-p-phenylenediamine (DTPD), N- Isopropyl-N'-phenyl-p-phenylenediamine (IPPD).
[0074] The object of the invention is achieved particularly well with the preferably selected para-phenylenediamines. According to advantageous embodiments of the invention, the rubber mixture contains 0 to 15.0, preferably 0.5 to 10.0 particularly preferably 0.5 to 5.0 phr DTPD.
[0075] According to advantageous embodiments of the invention, the rubber mixture contains 0 to 15.0, preferably 0.5 to 10.0 particularly preferably 1.0 to 5.0 phr 6PPD.
[0076] According to advantageous embodiments of the invention, the rubber mixture contains 0 to 15.0, preferably 0.5 to 10.0 particularly preferably 0.5 to 5.0 phr TMQ.
[0077] According to further advantageous embodiments of the invention, the rubber mixture is free from anti-aging agents, ie it contains 0 phr anti-aging agents.
[0078] With the advantageous embodiments, the underlying object is achieved within the scope of the present Invention particularly well solved.
[0079] Furthermore, the rubber mixture may contain conventional additives in conventional parts by weight, which Production preferably in at least one basic mixing stage. These additives include a) Activators such as zinc oxide and fatty acids (e.g. stearic acid) and / or other activators such as Zinc complexes such as zinc ethylhexanoate, b) activators and / or agents for the binding of fillers, in particular carbon black or silica, such as S-(3-aminopropyl)thiosulfuric acid and / or its metal salts (binding to soot) and silane coupling agents (binding to silica). c) waxes, in particular ozone-protective waxes, d) mastication aids, such as 2,2'-dibenzamidodiphenyl disulfide (DBD) and e) Processing aids, such as fatty acid esters and metal soaps, such as zinc soaps and / or Calcium soaps f) plasticizers.
[0080] According to particularly advantageous embodiments of the invention, the rubber mixture according to the invention contains at least one silane coupling agent, preferably in amounts of 1 to 22 phf, preferably 5 to 15 phf. The The term phf (parts per hundred parts of filler by weight) used is the term commonly used in the rubber industry. Quantity for coupling agents for fillers. In the context of this application, phf refers to the present silica, which means that other fillers such as carbon black are not included in the calculation of the Silane quantity included.
[0081] The silane coupling agents may be any type known to the person skilled in the art. Furthermore, one or more different silane coupling agents can be used in combination. Rubber compound can therefore contain a mixture of different silanes. The silane coupling agents react with the surface silanol groups of the silica or other polar Groups during the mixing of the rubber or rubber compound (in situ) or even before the addition of the Filler to the rubber in the sense of pretreatment (premodification). Coupling agents known from the state of the art are bifunctional organosilanes which are bonded to the silicon atom have at least one alkoxy, cycloalkoxy or phenoxy group as leaving group and which as other functionality have a group which, after cleavage, may undergo a chemical reaction with the double bonds of the polymer The latter group can include, for example, the following chemical groups: -SCN, -SH, -NH or -S - (with x = 2 to 8). 2 x For example, 3-mercaptopropyltriethoxysilane, 3-thiocyanatopropyltrimethoxysilane or 3,3'- Bis(triethoxysilylpropyl)polysulfides with 2 to 8 sulfur atoms, such as 3,3'-bis(triethoxysilylpropyl)tetrasulfide (TESPT), which corresponding disulfide (TESPD) or mixtures of sulfides with 1 to 8 sulfur atoms with different TESPT can also be used as a mixture with Carbon black (trade name X50S® from Evonik) can be added. Blocked mercaptosilanes, such as those known from WO 99 / 09036, can also be used as silane coupling agents Silanes, as described in WO 2008 / 083241 A1, WO 2008 / 083242 A1, WO 2008 / 083243 A1 and The methods described in WO 2008 / 083244 A1 can be used. For example, silanes are available under the name NXT in various versions from Momentive, USA, or those sold under the name VP Si 363® by Evonik Industries.
[0082] The plasticizers used in the present invention include all those known to the person skilled in the art Plasticizers such as aromatic, naphthenic or paraffinic mineral oil plasticizers, such as MES (mild extraction solvate) or RAE (Residual Aromatic Extract) or TDAE (treated distillate aromatic extract), or rubberto-liquid oils (RTL) or biomass-to-liquid oils (BTL), preferably with a polycyclic aromatics content of less than 3 wt.% according to method IP 346 or triglycerides, such as rapeseed oil, or factice or hydrocarbon resins or liquid Polymers whose average molecular weight (determined by GPC = gel permeation chromatography, based on BS ISO 11344:2004) is between 500 and 20000 g / mol. If additional If liquid polymers are used as plasticizers, they are not considered as rubber in the calculation of the composition the polymer matrix.
[0083] The plasticizer is preferably selected from the group consisting of the above-mentioned plasticizers. The plasticizer is particularly preferably selected from the group consisting of hydrocarbon resins, liquid polymers and mineral oils.
[0084] When using mineral oil, this is preferably selected from the group consisting of DAE (Distilled Aromatic Extracts) and / or RAE (Residual Aromatic Extract) and / or TDAE (Treated Distilled Aromatic Extracts) and / or MES (Mild Extracted Solvents) and / or naphthenic oils.
[0085] According to advantageous embodiments of the invention, the rubber mixture contains at least one Mineral oil plasticizers, preferably at least TDAE and / or RAE as plasticizers. This results in particularly good Processability, especially good miscibility of the rubber compound.
[0086] According to a preferred embodiment of the invention, the rubber mixture contains at least one liquid Polymer as a plasticizer.
[0087] According to a preferred embodiment of the invention, the rubber mixture contains at least one Hydrocarbon resin as plasticizer.
[0088] It is clear to the person skilled in the art that hydrocarbon resins are polymers composed of monomers, the Hydrocarbon resin is formally constructed from derivatives of the monomers by linking the monomers to each other. However, these hydrocarbon resins are not considered rubbers in the context of the present invention. The term ´´Hydrocarbon resins´´ in the context of the present application includes resins containing carbon atoms and hydrogen atoms and optionally heteroatoms, such as oxygen atoms. Hydrocarbon resin can be a homopolymer or a copolymer. In this document, homopolymer is defined as Application a polymer which according to Römpp Online Version 3.28 'is made of monomers of only one kind is.´´ The monomers can be any monomers of hydrocarbon resins known to the person skilled in the art, such as aliphatic C monomers, other unsaturated compounds which can be cationically polymerized, containing 5 Aromatics and / or terpenes and / or alkenes and / or cycloalkenes. In a preferred embodiment of the invention, the hydrocarbon resin is selected from the group consisting of from aliphatic C resins and hydrocarbon resins from alpha-methylstyrene and styrene. 5 The hydrocarbon resin preferably has a softening point according to ASTM E 28 (Ring and Ball) of 10 to 180 °C, particularly preferably from 60 to 150 °C, most preferably from 80 to 99 °C. Furthermore, the Hydrocarbon resin preferably has a molecular weight Mw of 500 to 4000 g / mol, preferably of 1300 to 2500 g / mol.
[0089] The proportion of the total amount of further additives is preferably 3 to 150 phr, preferably 3 to 100 phr and particularly preferably 5 to 80 phr.
[0090] The total amount of other additives may contain zinc oxide (ZnO). This can be all types of zinc oxide known to the person skilled in the art, such as ZnO granules or powder. 2 The zinc oxide used usually has a BET surface area of less than 10 m / g. However, it can also be a zinc oxide 2 with a BET surface area of 10 to 100 m / g, such as so-called ´´nano-zinc oxides´´, can be used.
[0091] According to advantageous embodiments of the invention, the rubber mixture contains 0.5 to 15.0, preferably 0.8 to 10.0 particularly preferably 1.0 to 5.0 phr zinc oxide (ZnO).
[0092] According to advantageous embodiments of the invention, the rubber mixture contains 0.5 to 5.0, preferably 0.5 to 3.3 particularly preferably 1.0 to 3.0 phr stearic acid.
[0093] The rubber mixture according to the invention is produced according to the procedure customary in the rubber industry Process in which a basic mixture with all components except the vulcanization system (peroxides and sulfur and / or sulfur donors and accelerators). The final mix is created by adding the vulcanization system in a final mixing stage. The final mix is used, for example, B. further processed through an extrusion process and brought into the appropriate shape. The subsequent processing is carried out by vulcanisation, whereby due to the scope of the present Invention added vulcanization system a sulfur crosslinking and at the same time a peroxide crosslinking takes place.
[0094] The rubber mixture according to the invention described above is particularly suitable for use in vehicle tires, Particularly suitable for pneumatic vehicle tires. In principle, application in all tire components is conceivable, in particular in a tread, in particular in the cap of a tread with cap / base construction, as above already described.
[0095] For use in vehicle tires, the mixture is preferably prepared as a ready-mix before vulcanization in the form a tread and applied as known during the production of the green vehicle tire. The production of the rubber mixture according to the invention for use as a sidewall or other body mixture in vehicle tires is carried out as already described. The difference lies in the shaping after the extrusion process or calendering the mixture. The resulting shapes of the unvulcanized rubber mixture for a or several different body mixtures are then used to build a tire blank. The body compound refers to the rubber mixtures for the other components of a tire, as in the Essentially separator plate, inner core (inner layer), core profile, belt, shoulder, belt profile, carcass, bead reinforcement, Bead profile, horn profile and bandage. For the use of the rubber mixture according to the invention in belts and belts, especially in conveyor belts, the extruded, still unvulcanized mixture is molded into the appropriate shape and often provided with reinforcements, e.g. synthetic fibres or steel cords, during or after the process. This usually results in a multi-layer structure consisting of one and / or more layers of rubber mixture, a and / or several layers of the same and / or different strength members and one and / or several further layers the like and / or another rubber compound.
[0096] The invention will now be described by means of comparative and exemplary embodiments, which are summarized in Table 1. be explained in more detail. The comparison mixtures are marked with V, the mixtures according to the invention are marked with E. The quantity of silanes in phf refers to the respective amount of silica. Substances used a
[0097] Natural rubber b Butadiene rubber, Nd-catalyzed, c functionalized solution-polymerized styrene-butadiene rubber: Sprintan™ SLR 3402, Trinseo d Plasticizers: TDAE, MES e Zeosil® 1165 MP, Solvay f NXT-Silane, Performance Materials Inc. G Anti-aging agents: 1.0 phr DTPD, 3.1 phr 6PPD, 1.0 phr TMQ h Ozone protection wax, zinc oxide and stearic acid, processing aid (calcium soap) i Luperox ® DCP, Arkema
[0098] The mixture was prepared under conventional conditions in several stages in a laboratory tangential mixer. Test specimens were produced from all mixtures by vulcanization and These test specimens were used to determine material properties typical for the rubber industry. For the tests described above The following test procedures were applied to test specimens: • Dynamic storage modulus E' averaged over the strain at -15°C from dynamic-mechanical Measurement based on DIN 53513: Strain sweep at a pre-compression of 20%, the strain range from 0.15% to 8% and a frequency of 10 Hz • Dynamic storage modulus E' averaged over the strain at +25°C from dynamic-mechanical Measurement based on DIN 53513: Strain sweep at a pre-compression of 20%, the strain range from 0.15% to 8% and a frequency of 10 Hz • Dynamic storage modulus E' averaged over the strain at +55°C from dynamic-mechanical Measurement based on DIN 53513: Strain sweep at a pre-compression of 20%, the strain range from 0.15% to 8% and a frequency of 10 Hz • Shore A hardness at room temperature and 70°C using a durometer according to DIN ISO 7619-1 • Conditioned Shore A hardness in accordance with DIN ISO 7619-1, preconditioned ten times with 5 MPa and subsequently tested according to ISO 868. • Rebound resilience at room temperature and 70°C according to ISO 4662
[0099] The rubber mixtures E1 and E2 according to the invention containing the combination according to the invention of Peroxide and sulfur vulcanization systems show lower values for E' at -15 °C compared to V1 and thus improved indicators for snow performance, especially traction on snow. The smaller this value, the This is better for snow performance. Furthermore, E1 and E2 show the same or not significantly negatively affected or even improved indicators for braking performance (E' at 25 °C) and handling performance (E' at 55 °C). The higher these values are, the better This applies to braking performance (E' at 25 °C) and handling performance (E' at 55 °C). Furthermore, E1 and E2 show improved rolling resistance indicators (rebound at 70 °C).
[0100] Thus, the vulcanizate according to the invention and the vehicle tire according to the invention show an improvement in Conflict of objectives between snow performance and braking behavior as well as handling behavior and in particular a improved snow performance. Table 1 Components Unit V1 E1 E2 a) N phr 15 15 15 R b) B phr 20 20 20 R c) phr 65 65 65 SSBR d) phr 55 55 55 plasticizers. Carbon black N 121 phr 8.0 8.0 8.0 e) phr 120 120 120 Silica f) pH 10.2 10.2 10.2 Silane G) phr 5.1 - 5.1 Anti-aging agents Zinc oxide phr 2.0 2.0 2.0 Stearic acid phr 1.0 1.0 1.0 h) phr 6.0 6.0 6.0 Other additives TBzTD phr 1.6 1.6 1.6 DPG phr 1.5 1.5 1.5 Sulfur phr 0.6 0.6 0.6 i) phr - 2.0 2.0 peroxide Characteristics Shore hardness RT Shore A 61 67 63 Shore hardness 70 °C Shore A 54 62 57 Condition Shore RT Shore A 57 65 60 Cond. Shore 70 °C Shore A 52 62 57 Rebound load. RT% 28 34 31 Rebound load. 70°C % 45 56 52 E' (-15 °C) MPa 46 42 43 E' (25 °C) MPa 17 19 16 E' (55 °C) MPa 11 13 11
Claims
1. Crosslinkable rubber mixture containing at least the following components: - 5 to 25 phr of at least one natural polyisoprene (NR); and - 10 to 50 phr of at least one polybutadiene (BR); and - 30 to 80 phr of at least one solution-polymerized styrene-butadiene rubber (SSBR); and - 30 to 500 phr of at least one silica as filler; and - 0.5 phr or more of at least one peroxidic compound, and - a sulfur vulcanization system.
2. Rubber mixture according to claim 1, characterized in that it contains at least one anti-aging agent.
3. Rubber mixture according to one of the preceding claims, characterized in that the anti-aging agent is selected from para-phenylenediamines and secondary aromatic amines, such as in particular dihydroquinolines.
4. Rubber mixture according to claim 3, characterized in that the dihydroquinoline is selected from the group consisting of 2,2,4-trimethyl-1,2-dihydroquinoline (TMQ) and 6-ethoxy-2,2,4-trimethyl-1,2-dihydroquinoline (ETMQ).
5. Rubber mixture according to claim 3, characterized in that the para-phenylenediamine is selected from the Group consisting of N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine (6PPD), N,N'-diphenyl-p-phenylenediamine (DPPD), N,N'-Ditolyl-p-phenylenediamine (DTPD), N-Isopropyl-N'-phenyl-p-phenylenediamine (IPPD), Phenyl[4-({[4-({[4-(phenylamino) phenyl] amino} ethyl)phenyl] ethyl} amino)phenyl] amine, Phenyl{4-[2-{[4-(phenylamino)phenyl]amino}ethyl)amino] phenyl}amine, (1-Methyl-2-{[-(phenylamino)phenyl]amino}propyl)[4-(phenylamino)phenyl]amine, N-(1,3-dimethylbutyl) -N'-(4- cumylphenyl)-p-phenylenediamine, N,N'-Di(1,4dimethylpentyl)-p-phenylenediamine (77PD), N,N'-Di(1-ethyl, 4-methylhexyl)-p- phenylenediamine (88PD), N,N'Bis-(1-ethyl-3-methylpentyl)-p-phenylenediamine (DOPD) and N,N'-Di-β-naphthyl-p- phenylenediamine (DNPD).
6. Rubber mixture according to claim 1, characterized in that it is free from ageing inhibitors, ie 0 phr Contains anti-aging agents.
7. Rubber mixture according to one of the preceding claims, characterized in that the peroxidic compound at least dicumyl peroxide is contained.
8. Vulcanizate which is obtained by the sulfur vulcanization of at least one rubber mixture according to one of claims 1 to 7 is preserved.
9. Use of a vulcanizate according to claim 8 in at least one component of a vehicle tire, in particular at least in the tread.
10. Use of a rubber mixture according to one of claims 1 to 7 for the production of a rubber article, in particular an air spring, a bellows, conveyor belt, belt, strap, hose, rubber band, profile, a seal, a membrane, tactile sensors for medical or robotic applications, or a shoe sole or Share it.
Citation Information
Patent Citations
material mixture for a sealing profile
DE102017101817A1
Preparation of peroxide vulcanized rubber composition and articles having at least one component thereof
EP1033386A1
Tread for a tire formed from rubber composition cured with peroxide
US20170247533A1
SBR composition for torsional damper, and torsional damper
US20170314631A1
Blocked mercaptosilane coupling agents for filled rubbers
WO1999009036A1