Carrier substrate and method for producing a carrier substrate

The carrier substrate with a high surface resistance bonding layer and controlled active metal proportion addresses the bonding challenges in metal-ceramic substrates, enhancing peel strength and service life by minimizing brittle intermetallic phases.

DE102020111700B4Active Publication Date: 2024-12-05ROGERS GERMANY
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
DE102020111700
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-04-29
Publication Date
2024-12-05
Estimated Expiration
2040-04-29

AI Technical Summary

Technical Problem

Existing metal-ceramic substrates face challenges in achieving strong and durable bonding between metal layers and ceramic elements, particularly due to the formation of brittle intermetallic phases which affect peel strength and service life.

Method used

A carrier substrate with a bonding layer having a surface resistance greater than 20 ohms/sq, comprising a thin adhesion promoter layer with a controlled proportion of active metal, is used to enhance the bonding between metal and ceramic layers, achieved through methods like chemical vapor deposition and hot isostatic pressing.

Benefits of technology

The solution results in improved peel strength and extended service life by reducing the formation of brittle intermetallic phases, allowing for thinner bonding layers and more reliable connections.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

Support substrate (1), in the form of a metal-ceramic substrate as a support for electrical components, comprising: - at least one metal layer (10) and - an insulating element (30), in the form of a ceramic element, a glass element, a glass-ceramic element and / or a high-temperature-resistant plastic element, wherein the at least one metal layer (10) and the insulating element (30) extend along a principal extension plane (HSE) and are arranged one above the other along a stacking direction (S) perpendicular to the principal extension plane (HSE), wherein in the manufactured support substrate (1) a bonding layer (12) is formed between the at least one metal layer (10) and the insulating element (30) with a soldering system comprising an active metal layer and a phosphorus-free soldering layer comprising several materials, and wherein an adhesion promoter layer (13) of the bonding layer (12) has a surface resistance greater than 20 ohms / sq.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to a carrier substrate and a method for producing a carrier substrate.

[0002] Carrier substrates, such as metal-ceramic substrates, are well known as printed circuit boards or circuit boards from the prior art, for example from DE 10 2013 104 739 A1, DE 199 27 046 B4, and DE 10 2009 033 029 A1. Typically, connection pads for electrical components and conductor tracks are arranged on one component side of the metal-ceramic substrate or the carrier substrate, wherein the electrical components and the conductor tracks can be interconnected to form electrical circuits. Essential components of the metal-ceramic substrates are an insulating layer, preferably made of a ceramic, and at least one metal layer bonded to the insulating layer. Due to their comparatively high insulation strengths, insulating layers made of ceramic have proven particularly advantageous in power electronics.By structuring the metal layer, conductor tracks and / or connection surfaces for the electrical components can then be realized.

[0003] A prerequisite for the successful provision of a metal-ceramic substrate is a permanent bond between the metal layer and the ceramic layer. In addition to a so-called direct metal bonding process, i.e., a DCB or DAB process, it is known from the state of the art to bond the metal layer to the ceramic layer using a solder material (AMB process).

[0004] An active soldering process, e.g., for joining metal layers or metal foils, in particular copper layers or copper foils, to ceramic material, is understood here to be a process specifically used to manufacture metal-ceramic substrates. This process involves creating a bond between a metal foil, e.g., a copper foil, and a ceramic substrate, e.g., an aluminum nitride ceramic, at a temperature of approximately 650-1000°C using a brazing alloy that, in addition to a main component such as copper, silver, and / or gold, also contains an active metal. This active metal, which is, for example, at least one element from the group consisting of Hf, Ti, Zr, Nb, and Ce, creates a bond between the solder and the ceramic through a chemical reaction, while the bond between the solder and the metal is a metallic brazing alloy.

[0005] Furthermore, a process is known, for example, from DE 10 2013 113 734 B4 and from JP H04-325 470 A, in which a metal layer is bonded to a ceramic layer by means of hot isostatic pressing to form a metal-ceramic substrate. Hot isostatic pressing is also used for post-treatment to reduce the number of voids formed during bonding using a soldering process or a direct metal bonding process.

[0006] EP 0 153 618 A2 discloses the use of a separate active metal layer as a solder system in addition to a solder base layer. EP 3 041 042 A1 also proposes a separate active metal layer in addition to a phosphorus-containing solder base material. DE 10 2015 108 668 A1 relates to the provision of a solder material provided as a foil. JP 2019-81 690 A relates to a metal-ceramic substrate with improved adhesion.

[0007] Based on the prior art, the present invention has for its object to provide a carrier substrate, in particular a metal-ceramic substrate, which is further improved compared to the known carrier substrates, in particular with regard to the bonding behavior of the metal to an insulating element, for example to a ceramic element.

[0008] The present invention solves this problem with a carrier substrate according to claim 1 and a method for producing a carrier substrate according to claim 7. Further embodiments can be found in the dependent claims and the description.

[0009] According to a first aspect of the present invention, a carrier substrate, namely a metal-ceramic substrate, is provided as a carrier for electrical components, comprising: - at least one metal layer and - an insulation element, namely a ceramic element, a glass element, a glass-ceramic element and / or a high-temperature-resistant plastic element, wherein the at least one metal layer and the insulation element extend along a main extension plane and are arranged one above the other along a stacking direction running perpendicular to the main extension plane, wherein a bonding layer is formed between the at least one metal layer and the insulation element in the manufactured carrier substrate, wherein an adhesion promoter layer of the bonding layer has a surface resistance which is greater than 20 ohms / sq.

[0010] Compared to the carrier substrates known from the prior art, the invention provides that the sheet resistance of an adhesion promoter layer of the bonding layer is greater than 5 ohms / sq, preferably greater than 10 ohms / sq, and particularly preferably greater than 20 ohms / sq. The determined sheet resistance is directly related to the active metal content in the adhesion promoter layer, which is crucial for bonding the at least one metal layer to the insulation element. The sheet resistance increases with a decreasing active metal content in the bonding layer. A correspondingly high sheet resistance thus corresponds to a low active metal content in the adhesion promoter layer.

[0011] It has been found that increasing the active metal content promotes the formation of brittle intermetallic phases, which in turn is detrimental to the peel strength of the metal layer on the insulation layer. In other words, the claimed sheet resistances describe bonding layers whose peel strength is improved, i.e., increased, due to the reduced formation of brittle intermetallic phases. By specifically adjusting the claimed sheet resistances, particularly strong bonds between the at least one metal layer and the ceramic element can be achieved. Such increased bond strength has a beneficial effect on the service life of the carrier substrate.

[0012] To determine the sheet resistance, the metal layer and, if present, a solder base layer are first removed from the manufactured carrier substrate, for example by etching. Using a four-point measurement, a sheet resistance is then measured on the top or bottom side of the carrier substrate, which has been freed of at least one metal layer and the solder base layer. In particular, the sheet resistance of a material sample is understood as its resistance relative to a square surface area. It is customary to indicate the surface resistance with the unit ohm / sq(square). The physical unit of sheet resistance is ohm.

[0013] Preferably, it is provided that a thickness of the bonding layer measured in the stacking direction, averaged over several measuring points within a predetermined area or in several areas that run or run parallel to the main extension plane, assumes a value that is less than 0.20 mm, preferably less than 10 µm and particularly preferably less than 6 µm. When multiple areas are mentioned, this means in particular that the at least one metal layer is divided into areas that are as equal as possible and that in each of these areas dividing the at least one metal layer, at least one value, preferably several measured values, for the thickness are recorded. The thicknesses determined in this way at different points are arithmetically averaged.

[0014] Compared to the carrier substrates known from the prior art, a comparatively thin bonding layer is thus formed between the at least one metal layer and the insulating element. In this case, it is provided that, in order to determine the relevant thickness of the bonding layer, the measured thicknesses are averaged over a large number of measuring points which lie within a predetermined or fixed area or areas. This advantageously takes into account that the insulating element, in particular the ceramic element, is generally subject to undulation, i.e. the insulating element is to be attributed a waviness. In particular, the person skilled in the art understands waviness to be a modulation of the generally flat course of the insulating element, seen over several millimeters or centimeters along a direction which runs parallel to the main plane of extension.This distinguishes such undulation from surface roughness of the insulation element, which is usually also present on the insulation element. By including such, generally unavoidable undulation of the insulation element in the thickness determination, it is taken into account that the bonding layer may vary due to the undulation, in particular, it may be larger in valley areas of the insulation element than in peak areas.

[0015] Despite this undulation, the average thickness value is nevertheless significantly lower than that known in prior art carrier substrates. This is achieved, in particular, or for example, by arranging a required active metal layer between the insulating element and the at least one metal layer, which is arranged individually, i.e. separately, between the insulating element and the at least one metal layer, for example, in addition to a solder base material (which, for example, does not contain any active metal or is free of active metal).The active metal is preferably applied to the solder base material and / or the at least one metal layer and / or the insulating element by means of chemical and / or physical vapor deposition, for example by sputtering, in order to create comparatively thin active metal layers, which in turn lead to a comparatively thin bonding layer, in particular to a homogeneous and thin adhesion promoter layer. It is also conceivable to provide the active metal layer on the solder base material, the insulating element and / or the at least one metal layer using a plasma, in a vacuum and / or by vapor deposition. It is also conceivable to create the active metal layer galvanically. It is particularly preferred that the active metal layer and / or the solder base material be provided as a foil.

[0016] Furthermore, it is conceivable for the solder base material and / or the active metal layer to have recesses. In such a case, it is possible to use a thicker layer for the solder base material and / or the active metal layer, since during the bonding process the solder base material and / or the active metal layer liquefies and fills the previous recesses or recess areas. This makes it possible to provide a desirable, comparatively low proportion of active metal for forming the adhesion promoter layer, even if, for example, a greater thickness is assigned to the active metal layer. For example, the solder base material and / or the active metal layer with recesses is a grid or expanded metal, which is formed, for example, from a mesh- or fence-like braid and is arranged between the insulation element and the at least one metal layer.The solder base material and / or active metal layer are preferably provided as foils.

[0017] The formation of comparatively thin bonding layers reduces in particular the effort that must be expended, for example in a “second etching”, to remove the bonding layer again, at least in part, in order to structure the carrier substrate, in particular its at least one metal layer and the bonding layer. This structuring, which serves to electrically insulate several metal sections of the at least one metal layer from one another, is preferably carried out by etching and / or a mechanical processing step and / or with laser light. Furthermore, it has proven advantageous that the number of possible defects in the bonding layer, for example caused by material defects in the solder material, can be advantageously reduced by using small layer thicknesses. A defect in the bonding layer orA material defect in the solder material is understood to mean, for example, a large grain in the solder material, such as an active metal grain, which can lead to the formation of a giant grain in the bonding layer and / or which does not melt completely and thus prevents minimal solder gaps as a spacer. Application, particularly by sputtering, can easily prevent relatively large grains from becoming part of the active metal layer, which can also be seen in the bonding layer or adhesion promoter layer. Finally, it is advantageous that a thin bonding layer forms homogeneously over the produced carrier substrate.

[0018] In particular, the average thickness of the bonding layer means that thicknesses are determined or measured stochastically or statistically distributed in a defined area or several areas, and their arithmetic mean is then determined. For this purpose, for example, several microscopic images of various cross-sectional images are first taken, preferably using a scanning electron microscope (SEM), with the cross-sectional images each extending through the carrier substrate in a direction perpendicular to the main extension plane. The cross-sectional images run along a cross-sectional plane that is perpendicular to the main extension plane. The thicknesses are then determined in the cross-sectional plane.In other words: several cross-sectional images are taken, each running perpendicular to the main plane of extension and distributed evenly or irregularly at measuring points within the area or in several different areas. For example, several cross-sectional images offset parallel to one another are used, e.g. by removing slices from the carrier substrate. Subsequently, preferably more than 25 or 100 thicknesses, more preferably more than 200 and particularly preferably more than 500 thicknesses of the bonding layer are measured in the specified area on the substrate, i.e. in the various cross-sectional images, and the arithmetic mean is determined. The distance between two measuring points is at least 100 µm in order to reduce the influence of undulation on the measurement result.Since a carrier substrate typically contains two bonding layers facing each other on either side of the ceramic, the same number of layer thickness measurements must be taken on the opposite side. The larger the area chosen, the lower the probability that the undulation will produce an erroneous or distorted image of the measured bonding layer thicknesses. The predetermined or fixed area, which runs particularly parallel to the main extension plane, has a size of more than 25 cm for large-scale maps. 2 , preferably more than 50 cm 2 , especially preferably more than 100 cm 2 For a carrier substrate separated from the large card, the size can be more than 1 cm 2 , preferably more than 1.5 cm 2 and especially preferably more than 5 cm 2 be.

[0019] Particularly preferred is the following method for determining and selecting the measuring ranges contributing to the determination - regardless of the size of the carrier substrate: In a first step, the at least one metal layer of the carrier substrate is divided into nine equal-sized rectangles, in particular squares, i.e. into several approximately equal-sized areas. In each of the measurement areas defined in this way, two or three sectional images are generated which are used to determine an average thickness for the at least one metal layer in each of the sectional images. The sectional images are preferably recorded using an SEM method, for example at a magnification of 2000 or 2500 times. Subsequently, in a second step, the average is calculated over the total of 18 or 27 thicknesses recorded in the sectional images, which are distributed across all nine rectangular measurement areas. In this way, it is advantageously ensured that the average thickness represents a representative value for the bonding layer between the at least one metal layer and the insulating element for the entire carrier substrate.In other words, the procedure described in this section provides for an average thickness determined across the at least one metal layer in uniformly distributed measurement areas. The method described here for selecting the measurement area, which contributes to determining an average thickness value, can be used analogously for determining the sheet resistance.

[0020] The carrier substrate is preferably provided as a printed circuit board in which, in the manufactured state, the at least one metal layer which is connected to the insulation element is structured. For example, it is provided for this purpose that after the connection step, structuring is also carried out, for example by lasering, etching and / or mechanical processing, with which conductor tracks and / or connections for electrical or electronic components are created. It is preferably provided that on a manufactured metal-ceramic substrate, on the ceramic element, on the side opposite the metal layer, a further metal layer, in particular a back-side metallization and / or a cooling element, is provided. The back-side metallization preferably serves to counteract bending and the cooling element serves to effectively dissipate heat which is generated during operation of electrical or electronic components.electronic components that are connected to the circuit board or the metal-ceramic substrate.

[0021] Conceivable materials for the at least one metal layer and / or the at least one further metal layer in the metal-ceramic substrate or insulation element include copper, aluminum, molybdenum, tungsten, nickel, and / or their alloys, such as CuZr, AlSi, or AlMgSi, as well as laminates such as CuW, CuMo, CuAl, and / or AlCu, or MMC (metal matrix composite), such as CuW, CuM, or AlSiC. Furthermore, it is preferably provided that the at least one metal layer on the manufactured metal-ceramic substrate is surface-modified, in particular as component metallization. A possible surface modification could, for example, be a sealing with a precious metal, in particular silver and / or gold, or (electroless) nickel or ENIG ("electroless nickel immersion gold"), or edge encapsulation on the metallization to suppress crack formation or crack widening.

[0022] The ceramic element preferably comprises Al2O3, Si3N4, AIN, an HPSX ceramic (i.e., a ceramic with an Al2O3 matrix containing an x-percent ZrO2 content, for example, Al2O3 with 9% ZrO2 = HPS9 or Al2O3 with 25% ZrO2 = HPS25), SiC, BeO, MgO, high-density MgO (> 90% of the theoretical density), TSZ (tetragonally stabilized zirconium oxide) as the ceramic material. It is also conceivable for the ceramic element to be designed as a composite or hybrid ceramic, in which, in order to combine various desired properties, several ceramic layers, each differing in terms of their material composition, are arranged one above the other and joined together to form an insulating element.

[0023] The bonding layer is preferably formed flatly, in particular without interruption, i.e. continuously, between the at least one metal layer and the ceramic element. It is preferably provided that a ratio of an area in which no bonding layer is formed between the at least one metal layer and the insulating element to the areas in which a bonding layer is formed between the at least one bonding layer and the insulating element is less than 0.05 mm, preferably less than 0.02 mm and particularly preferably less than 0.007 mm. The person skilled in the art will understand in particular that in order to form this ratio, the areas which are free of metal of the at least one metal layer due to the structuring are not taken into account.

[0024] It is preferably provided that the carrier substrate comprises at least one further metal layer which is bonded to the insulation element on a side opposite the at least one metal layer, wherein in the manufactured carrier substrate a further bonding layer is formed between the at least one further metal layer and the insulation element, wherein here too a summed thickness of the bonding layer and the further bonding layer measured in the stacking direction, averaged over several measuring points within a predetermined area or several areas which run or run parallel to the main extension plane, assumes a value which is less than 0.045 mm, preferably less than 0.0225 mm and particularly preferably less than 0.0135 mm.

[0025] Preferably, the bonding layer and / or the further bonding layer comprises silver from a solder material and / or a solder base material. In general, this layer forms a solder base layer in which the main component of the solder base material collects in the manufactured carrier substrate. For example, a bonding layer is understood to be the layer that forms between the at least one metal layer and the insulation element in the case of a silver-based solder material. This essentially comprises silver and can be identified accordingly in a cross-sectional image of the metal-ceramic substrate produced along the stacking direction. The thickness to be used or measured relates to the massive portions of silver-rich phases and excludes in particular those inclusions that are found in the at least one metal layer, especially in the edge region to the silver layer.

[0026] Preferably, in addition to the silver, which is attributable to a silver-based solder material or a silver-based solder base material, an adhesion promoter layer is formed in the bonding layer. In the case of a metal-ceramic substrate, the adhesion promoter layer is preferably realized or formed by a compound which, on the one hand, comprises the active metal, for example titanium, and, on the other hand, the constituents of the ceramic element, for example oxygen O, nitrogen N and / or carbon C and / or silicon Si and / or aluminum Al and / or magnesium Mg and / or calcium Ca. Correspondingly, the adhesion promoter layer comprises, for example, titanium nitride, titanium carbide and / or titanium oxide, in particular in various oxidation states.

[0027] Furthermore, it is conceivable that the solder base material is provided as a foil, as a paste, as a layer formed by physical and / or chemical vapor deposition, and / or as a galvanically formed layer.

[0028] Preferably, the bonding layer and / or the further bonding layer is an adhesion promoter layer comprising an active metal. In particular, the bonding layer is formed only from the adhesion promoter layer comprising the active metal. In this case, the adhesion promoter layer in the bonding layer has a connection with a constituent of the ceramic element, such as nitrogen, oxygen or carbon, and the other constituents of the ceramic. Accordingly, the adhesion promoter layer comprises, for example, titanium nitride, titanium oxide and / or titanium carbide. For example, the bonding layer exclusively comprises the adhesion promoter layer comprising the active metal, i.e., the bonding layer does not contain any silver or other base solder constituents.In this case, it is intended that a thickness of the bonding layer measured in the stacking direction, averaged over several measuring points within a surface running parallel to the main extension plane, or the several surfaces, assumes a value that is less than 0.003 mm (3000 nm), preferably less than 0.001 mm (1500 nm), and particularly preferably less than 0.0005 mm (500 nm) or even less than 0.00035 mm (350 nm). In particular, for bonding layers that do not contain a solder base material and / or a silver content, an even thinner bonding layer can be formed accordingly.

[0029] In particular, it is provided that the adhesion promoter layer comprising an active metal has a substantially constant thickness, in particular in contrast to the solder base layer, which is modulated due to the undulation in the insulation element. In particular, the measured thickness values ​​determined within the area or areas have a distribution to which a standard deviation can be assigned that is less than 0.2 µm, preferably less than 0.1 µm, and particularly preferably less than 0.05 µm. In particular, the physical and / or chemical vapor deposition of an active metal layer and the resulting bonding layer make it possible to achieve a homogeneous and evenly distributed thickness of the bonding layer, which in particular consists only of the adhesion promoter layer. The adhesion promoter layer can also have a constant thickness if it is formed in addition to the solder base material.

[0030] Another object of the present invention is a method for producing a carrier substrate, namely a metal-ceramic substrate according to the present invention, comprising: - Providing at least one metal layer and one insulating element, in particular a ceramic element, a glass element, a glass-ceramic element and / or a high-temperature-resistant plastic element, wherein the at least one metal layer and the insulating element extend along a main extension plane, - arranging the at least one metal layer and the insulation element one above the other in a stacking direction running perpendicular to the main extension plane, wherein an active metal layer is arranged between the at least one metal layer and the insulation element and - Bonding the at least one metal layer to the insulating element via the active metal layer to form a bonding layer between the at least one metal layer and the insulating element.

[0031] All advantages and properties described for the carrier substrate can be transferred or analogously transferred to the process and vice versa.

[0032] Preferably, the active metal layer is formed by chemical or electrochemical deposition and / or gas-physical vapor deposition (PVD) of an active metal. The active metal layer can be formed on the insulation element, the solder base material, and / or the at least one metal layer. Alternatively or additionally, it is conceivable for the active metal layer to be provided as a separate foil or as a foil that is provided in combination with the solder base material layer and / or a solder foil and / or with the at least one metal layer.

[0033] In particular, the use of a separately applied active metal layer makes it possible to make it comparatively thin, thereby achieving the claimed comparatively thin thicknesses of the bonding layer, particularly averaged over various thickness values ​​within the specified area(s). Examples of active metals are titanium (Ti), zirconium (Zr), hafnium (Hf), chromium (Cr), niobium (Nb), cerium (Ce), tantalum (Ta), magnesium (Mg), lanthanum (La), and vanadium (V). It should be noted that the metals La, Ce, Ca, and Mg can easily oxidize. Furthermore, it should be noted that the elements Cr, Mo, and W are not classic active metals, but are suitable as a contact layer between Si3N4 and the at least one metal layer or the solder system or solder material, since they do not form intermetallic phases with the at least one metal layer, for example, copper, and do not have edge solubility.

[0034] In particular, the solder base material is a metal-based base material, preferably a silver-based or copper-based base material. In a silver-based base material, silver is the main component, i.e., the component with the highest proportion by weight, whereas in a copper-based base material, copper is the main component. Examples of a silver-based base material are AgCu, in particular AgCu28, AgCuln, AgCuSn, and AgCuGa. Examples of a copper-based base material are copper CuSn, CuAg, Culn, CuGa, CulnSn, CuInMn, and CuGaSn. It is also conceivable to use a solder base material based on NiCrMn or SnCu.

[0035] Preferably, the active metal layer contains a proportion of non-metallic impurities of less than 0.1 wt. %, preferably less than 0.05 wt. %, and particularly preferably less than 0.01 wt. %. By minimizing impurities, it is advantageously possible to make the layer thickness smaller, since in the event of contamination, only a portion of the active metal present can contribute to bonding the at least one metal layer to the insulating element, while the remainder of the active metal is bound by the impurities. By ensuring a comparatively low proportion of impurities, a more effective bond is achieved, which allows the proportion of active metal to be reduced, which in turn allows the bonding layer to be made thinner.

[0036] Furthermore, it is preferably provided that physical and / or chemical vapor deposition or electrochemical deposition is carried out in such a way that a density of the active metal applied to the insulation element is achieved which is greater than 90% of a theoretical density of the active metal, preferably greater than 95% of the theoretical density and particularly preferably greater than 99% of the theoretical density. The theoretical density of the active metal is understood by those skilled in the art to mean in particular the density which can be found in a data sheet for the active metal without artificial cavities or pores being introduced into the active metal. In particular, the comparatively high densities prevent oxygen, nitrogen and / or carbon from being present in the active metal layer during binding, which in turn could lead to undesired binding of the active metal as an impurity.Accordingly, the increased density in the active metal layer increases the proportion that can be effectively used for the connection between the at least one metal layer and the ceramic element, which in turn means that the active metal layer as such can be made thinner.

[0037] Preferably, an active metal layer is used whose thickness is between 10 nm and 1000 nm, preferably between 50 nm and 750 nm, particularly preferably between 100 and 500 nm. Furthermore, it is preferably provided that the active metal is applied to the insulation element and / or the solder base material, which is preferably also in the form of a foil, by means of physical and / or chemical vapor deposition. For example, it is also conceivable that the active metal is rolled down to the desired thickness together with the solder material in order to form a comparatively thin bonding layer between the at least one metal layer and the insulation element.

[0038] Preferably, a solder foil is used that is smaller than 20 µm, preferably smaller than 12 µm, and particularly preferably smaller than 8 µm. For example, the thickness of the solder layer assumes a value between 2 and 20 µm or between 2 and 5 µm, preferably between 8 and 15 µm, and particularly preferably between 5 and 10 µm. Furthermore, it is conceivable that the solder base material is provided as a foil, as a paste, as a layer formed by physical and / or chemical deposition, and / or as a galvanically formed layer.

[0039] Furthermore, it is preferably provided that a roughness R aa surface of the insulation element is at least partially smaller than 1.0 µm, preferably smaller than 0.7 µm, and particularly preferably smaller than 0.5 µm. By reducing the roughness on the surface of the insulation element, it is advantageously possible to avoid air pockets or hollow areas in which oxygen can accumulate, which in turn would be detrimental to the effective use of the active metal for bonding the at least one metal layer to the insulation element. In particular, a mean roughness is assumed. The mean roughness value, represented by the symbol R a , indicates the average distance of a measuring point on the surface from a centerline. The centerline intersects the actual profile within a reference distance such that the sum of the profile deviations in a plane parallel to the centerline is distributed over the length of the reference distance.

[0040] Furthermore, it is preferably provided that the at least one metal layer and / or the at least one further metal layer is bonded to the insulation element by means of an active soldering process and / or a hot isostatic pressing process and / or a DCB process.

[0041] For example, it is provided that a method for producing a metal-ceramic substrate is provided, comprising: - Providing a soldering layer, in particular in the form of at least one soldering foil or brazing foil, - coating the insulation element and / or the at least one metal layer and / or the at least one solder layer with at least one active metal layer, - Arranging the at least one solder layer between the insulation element and the at least one metal layer along a stacking direction to form a solder system comprising the at least one solder layer and the at least one active metal layer, wherein a solder material of the at least one solder layer is preferably free of a melting point-lowering material or of a phosphorus-free material, and - Bonding the at least one metal layer to the at least one ceramic layer via the soldering system by means of an active soldering process.

[0042] According to the invention, a multi-layer soldering system is provided comprising at least one phosphorus-free solder layer and at least one active metal layer. The separation of the at least one active metal layer and the at least one solder layer proves to be particularly advantageous because it allows for the realization of comparatively thin solder layers, especially when the solder layer is a foil. For solder materials containing active metals, comparatively large solder layer thicknesses would otherwise be required due to the brittle intermetallic phases or the high elastic modulus and high yield strength of the common active metals and their intermetallic Phases that hinder the forming of the solder paste or solder layer are realized, whereby the minimum layer thickness is limited by the manufacturing properties of the active metal-containing solder material. Accordingly, for solder layers containing active metals, it is not the minimum thickness required for the joining process that determines the minimum solder layer thickness of the solder layer, but rather the technically feasible minimum solder layer thickness that determines the minimum solder layer thickness of the solder layer. As a result, this thicker, active metal-containing solder layer is more expensive than thin layers. The person skilled in the art understands "phosphorus-free" to mean, in particular, that the proportion of phosphorus in the solder layer is less than 150 ppm, less than 100 ppm, and particularly preferably less than 50 ppm.

[0043] According to the invention, the solder layer comprises the phosphorus-free solder layer and several materials in addition to the pure metal. For example, indium is a component of the solder material used in the solder layer.

[0044] Furthermore, it is conceivable that the solder material for forming the solder layer is applied to the active metal layer and / or the at least one metal layer by physical and / or chemical vapor deposition and / or galvanically. This advantageously makes it possible to realize comparatively thin solder layers in the soldering system, particularly with a homogeneous distribution.

[0045] For example, in the production of the carrier substrate, in particular the metal-ceramic substrate, further steps are provided, comprising: - Providing a ceramic element and a metal layer, - providing a gas-tight container enclosing the ceramic element, wherein the container is preferably formed from the metal layer or comprises the metal layer, - Forming the metal-ceramic substrate by bonding the metal layer to the ceramic element by means of hot isostatic pressing, wherein, to form the metal-ceramic substrate, an active metal layer or a contact layer comprising an active metal is arranged at least partially between the metal layer and the ceramic element to support the bonding of the metal layer to the ceramic element. The container is preferably formed as a metal container made of a metal layer and / or another metal layer. Alternatively, it is also conceivable to use a glass container.

[0046] In hot isostatic pressing, it is particularly intended that bonding occurs by heating under pressure, during which the first and / or second metal layer of the metal container, in particular the subsequent metal layer of the metal-ceramic substrate and any eutectic layer present there, does not enter the melt phase. Accordingly, lower temperatures are required for hot isostatic pressing than for a direct metal bonding process, in particular a DCB process.

[0047] In comparison to the bonding of a metal layer to a ceramic layer using a solder material, which typically uses temperatures below the melting temperature of the at least one metal layer, the present procedure advantageously dispenses with the need for a solder base material, and only requires an active metal. The use or utilization of pressure during hot isostatic pressing also proves advantageous because it can reduce air inclusions or cavities between the first metal layer and / or the second metal layer on the one hand and the ceramic element on the other, whereby the frequency of voids forming in the formed or manufactured metal-ceramic substrate can be reduced or even avoided. This has a beneficial effect on the quality of the bond between the metal layer or the first and / or second metal layer of the metal container and the ceramic element.In addition, it is advantageously possible to simplify the “second etching” and avoid solder residues and silver migration.

[0048] It is also conceivable that during hot isostatic pressing an additional solder material is introduced between the ceramic element and the at least one metal layer, wherein a melting temperature of the additional solder material can be lower than the temperature at which the hot isostatic pressing is carried out, ie lower than the melting temperature of the at least one metal layer.

[0049] It is preferably provided that during hot isostatic pressing, the metal container is exposed in a heating and pressure device to a gas pressure between 100 and 2000 bar, preferably between 150 and 1200 bar and particularly preferably between 300 and 1000 bar and a process temperature of 300°C up to a melting temperature of the at least one metal layer, in particular up to a temperature below the melting temperature. It has advantageously been found that it is thus possible to bond a metal layer, i.e. a first and / or second metal layer of the metal container, to the ceramic element without the required temperatures of a direct metal bonding process, for example a DCB or a DAB process, and / or without a solder base material that is used in active soldering. In addition, the use or application of an appropriate gas pressure allows the possibility of producing a process that is as void-free as possible, i.e.to produce a metal-ceramic substrate without gas inclusions between the metal layer and the ceramic element. In particular, process parameters mentioned in DE 2013 113 734 A1 are used, and are hereby explicitly referenced.

[0050] Further advantages and features will become apparent from the following description of preferred embodiments of the subject matter of the invention with reference to the accompanying figures. They show: Fig. 1: Carrier substrate according to a first exemplary embodiment of the present invention; Fig. 2 Component of the carrier substrate made of Fig. 1 before joining; Fig. 3: Carrier substrate according to a second exemplary embodiment of the present invention; Fig. 4 Component of the carrier substrate made of Fig. 3 before joining and Fig. 5 Detailed view of a carrier substrate according to a third exemplary embodiment of the present invention

[0051] In the Fig. 1 shows a carrier substrate 1 according to a first exemplary embodiment of the present invention. Such carrier substrates 1, in particular in the form of a metal-ceramic substrate, preferably serve as carriers or circuit boards for electronic or electrical components that can be bonded to the at least one metal layer 10 of the carrier substrate 1 on its component side. It is preferably provided that the at least one metal layer 10 is structured in order to form corresponding conductor tracks and / or connection surfaces, i.e., in the manufactured carrier substrate 1, the at least one metal layer 10 comprises a plurality of metal sections that are electrically insulated from one another.The at least one metal layer 10, which extends essentially along a main extension plane HSE, and an insulation element 30 extending along the main extension plane HSE are arranged one above the other along a stacking direction S running perpendicular to the main extension plane HSE and are preferably joined or connected to one another via a bonding layer 12. Preferably, in addition to the at least one metal layer 10, the carrier substrate 1 comprises at least one further metal layer 20, which, viewed in the stacking direction S, is arranged on the side of the insulation element 30 opposite the at least one metal layer 10 and is bonded to the insulation element 30 via a further bonding layer 12'.

[0052] The at least one further metal layer 20 serves as a backside metallization, which counteracts a bending of the carrier substrate 1, in particular of the metal-ceramic element, and / or as a heat sink, which is designed to dissipate heat input caused by electrical or electronic components on the metal-ceramic substrate 1.

[0053] In particular, the carrier substrate 1 has a bonding layer 12 arranged between the at least one metal layer 10 and the insulation element 30. It has proven advantageous if a thickness of the bonding layer 12 measured in the stacking direction S is comparatively thin. Furthermore, a comparatively thin thickness of the bonding layer 12 between the at least one metal layer 10 and the insulation element 30 proves advantageous if an etching process is provided for the purpose of structuring the at least one metal layer 10. For example, this allows narrower insulation trenches, i.e., distances between individual metal sections of the at least one metal layer 10, to be realized.For example, widths z, measured in the direction parallel to the main extension plane HSE, for the isolation trench between two metal sections whose thickness is 200 µm to 400 µm, can be realized that are less than 700 µm, preferably less than 600 µm and particularly preferably less than 500 µm.

[0054] Furthermore, the formation of a thinner bonding layer 12 proves to be advantageous in that it can further reduce the number of possible defects in the bonding layer 12 caused by material defects in a solder material that may be used.

[0055] In the Fig. In the example shown in Figure 1, the bonding layer 12 is, in particular, an adhesion promoter layer 13 comprising an active metal. Preferably, the carrier substrate 1 is a metal-ceramic substrate, in which the insulating element 30 is a ceramic element. In this case, the adhesion promoter layer 13 is preferably formed from a material composition comprising a compound of components of the ceramic element on the one hand and an active metal on the other. Since these are very brittle compounds, the thinnest possible design of this adhesion promoter layer 13 is advantageous for the adhesive strength of the at least one metal layer 10 on the insulating element 30.

[0056] In Fig. 2 is the carrier substrate 1 made of Fig. 1 before joining. Before the joining process, it is provided that, viewed in the stacking direction S, the insulating element 30, ie in particular the ceramic element, and the at least one metal layer 10 are arranged one above the other, wherein an active metal layer 15 is arranged between the at least one metal layer 10 and the insulating element 30.

[0057] Furthermore, it is particularly preferably provided that, in order to bond the at least one further metal layer 20 to the side of the insulating element 30 opposite the at least one metal layer 10, an active metal layer 15 is also arranged between the insulating element 30 and the at least one further metal layer 20. In this case, the at least one further metal layer 20 and the insulating element 30 are likewise arranged one above the other in the stacking direction S. For example, the bonding of the at least one metal layer 10 to the insulating element 30 takes place here by means of hot isostatic pressing, in which a bond is created under the influence of pressure and temperature on an ensemble consisting of the insulating element 30, the active metal layer 15 and the at least one metal layer 10. For this purpose, a container is preferably used in which the ensemble consisting of the insulating element 30 and the active metal layer 15 is arranged.Preferably, a portion of the gas-tight metal container forms the at least one metal layer 10 and thus forms part of the ensemble. Alternatively, it is also conceivable that the active metal layer 15 is supported by an energy input, for example, by applying flashes of light as part of a "flash light annealing" process. ss a connection of the at least one metal layer 10 to the insulation element 30 via the active metal layer 15 takes place. Preferably, the "flash light annealing" takes place after the arrangement of the active metal layer 15 on the insulation element 30 and / or the at least one metal layer 10.

[0058] Through the bonding process, the active metal layer 15 becomes the bonding layer 12, in particular the active metal-containing adhesion promoter layer 13. In particular, the bonding layer 12 comprises an active metal-containing material which, depending on the ceramic, can be, for example, titanium carbide, titanium nitride and / or titanium oxide, preferably in different oxidation states.

[0059] The active metal layer 15 is preferably applied to the insulation element 30 and / or to the at least one metal layer 10 by physical and / or chemical vapor deposition, for example sputtering. For this purpose, it is particularly preferably provided that, during the physical vapor deposition, an active metal layer 15 is realized whose density is greater than 90% of a theoretical density of the active metal, preferably greater than 95% of the theoretical density of the active metal, and particularly preferably greater than 99% of the theoretical density of the active metal. This advantageously reduces the proportion of air, in particular the proportion of oxygen, in the active metal layer 15 during the bonding process, which would otherwise result in only a reduced proportion of the active metal, i.e., not the maximum possible proportion, being able to be used to bond the at least one metal layer 10 to the insulation element 30.

[0060] In particular, it has proven advantageous if the proportion of impurities in the active metal layer 15 is less than 1% by weight, preferably less than 0.7% by weight, and particularly preferably less than 0.5% by weight. This allows the active metal layer 15 to be applied as thinly as possible, which leads to the formation of a comparatively thin bonding layer 12. The extent of the impurity depends, for example, on the purity of a carrier material. For example, the layer thickness of the active metal layer 15, measured in the stacking direction S, has a thickness of 10 nm - 1000 nm, preferably between 50 nm - 150 nm, and particularly preferably between 100 nm - 500 nm, before the at least one metal layer 10 is joined to the insulation element 30 via the active metal layer 15. Furthermore, it is particularly preferably provided that after the joining orStructuring is performed, in particular by means of an etching or etching process, to bond the at least one metal layer 10 to the insulation element 30. Structuring is performed by removing both the sections or partial regions of the at least one metal layer 10 and the bonding layer 12 in order to electrically insulate the metal sections in the at least one metal layer 10 from one another.

[0061] In the Fig. 3 shows a carrier substrate 1 according to a second exemplary embodiment. The embodiment of the Fig. 3 of those from the Fig. 1 only in that the carrier substrate 1 has a solder base layer 14 as a bonding layer 12 in addition to an adhesion promoter layer 13. The solder base layer 14 comprises, in particular, as material a main solder component of the solder base material 16 used or the essential component of the solder base material 16. Preferably, the solder base layer 14 is formed from silver, in particular if it is a silver-based solder base material 16.

[0062] In Fig. 4 is the embodiment from Fig. 3 before joining. In contrast to the system from the Fig. 2, it is provided that, in addition to the active metal layer 15, a solder base material 16 is provided, wherein the solder base material 16 is arranged between the insulation element 30 and the at least one metal layer 10 as seen in the stacking direction S. Preferably, the solder base material 16 is arranged between the active metal layer 15 and the at least one metal layer 10 as seen in the stacking direction S. By means of a soldering process, in which the assembled ensemble of insulation element 30, active metal layer 15, solder material 16 and at least one metal layer 10 is exposed to a corresponding process temperature, the bonding of the at least one metal layer 10 to the insulation element 30 takes place via a solder system which comprises the active metal layer 15 and the solder base material 16. The same applies to the bonding of the at least one further metal layer 20 to the insulation element 30 in the example of Fig. 4. The solder base material 16 is preferably a foil that is arranged for joining between the at least one metal layer 10 and / or the at least one further metal layer 20, on the one hand, and the insulating element 30, on the other. It is conceivable that the active metal layer 15 is applied to the solder material or solder base material 16 formed as a foil by physical and / or chemical vapor deposition. In particular, it has been found that by using a separate active metal layer 15, in particular together with a solder base material 16, it is possible to realize comparatively thin bonding layers 12.

[0063] Furthermore, it has been found to be advantageous that by using a separate active metal layer 15, as in the embodiments of the Fig. 1 to 4, it is possible to realize a flat and continuous bonding layer 12. This is not guaranteed, for example, when using a paste material that comprises both solder base material 16 and active metal, if an equal amount of titanium is assumed or a solder system of the same thickness is used. In this case, statistically distributed bonding errors arise in the region of the bonding layer. In a corresponding manner, the targeted flat or continuous bonding of the at least one metal layer 10 to the insulating element 30 makes it possible to realize an uninterrupted, ie continuous, bonding layer 12, which significantly improves the bonding behavior of the at least one metal layer 10 to the insulating element 30.Preferably, a ratio between regions in which no bonding layer 12 is formed between the at least one metal layer 10 and the insulating element 30, to regions in which a bonding layer 12 is formed between the at least one metal layer 10 and the insulating element 30, assumes a value that is less than 0.05, preferably less than 0.025 and particularly preferably less than 0.01. In particular, it is provided that only those sections of the carrier substrate 1 that are not structured are used to determine this ratio. In other words: on the manufactured carrier substrate 1, the said ratio relates to a metal section and / or a plurality of metal sections of the at least one metal layer 10 or the at least one further metal layer 20. Preferably, the ratio is established over the entire metal-ceramic substrate orthe entire carrier substrate 1, whereby the individual sub-areas are summed up over the separate metal sections.

[0064] In Fig. 5 shows a carrier substrate 1 according to a third exemplary embodiment of the present invention. In particular, the upper half shows a plan view of the carrier substrate 1 in a viewing direction that essentially corresponds to the stacking direction S. Accordingly, the at least one metal layer 10 can be seen, as can the upper side of the insulating element 30 protruding relative to the outermost edge of the at least one metal layer 10. This protruding or projecting partial section, a so-called pull-back, serves in particular to prevent an electrical flashover between the at least one metal layer 10 and the at least one further metal layer 20 on a rear side of the insulating element 30.In order to quantitatively determine the thickness D of the bonding layer 12, it is preferably provided that this is determined at different positions within different areas F, preferably in several rectangles which together form the at least one metal layer 10 or which together extend over the entire surface of the carrier substrate, and then an average value is determined. In the example shown, the metal layer is divided into nine approximately equally sized rectangles or squares, i.e. areas. In each of the nine areas F, at least two, preferably three, sectional images are taken using an SEM method. In the individual sectional images, average thicknesses D for the bonding layer 12, in particular the adhesion promoter layer 13, are determined along the sectional plane. The sectional plane runs perpendicular to the main extension plane HSE. The arithmetic mean of all determined thicknesses in the sectional images is then determined.This advantageously takes into account the fact that the carrier substrate 1 or the insulation element 30 generally has an undulation, i.e., a waviness, which leads to the solder base material 16 flowing into valleys of the insulation element 30 on its upper side during a manufacturing process or bonding process, which leads to a modulated thickness D of the bonding layer 12 being established along the main extension plane HSE. Nevertheless, it has been found that the advantageously described effects and impacts also occur when the thickness D is comparatively thin, in particular thinner than a comparable bonding layer 12 that is established when using conventional pasty solder materials 16. To determine the thickness D assigned to the cross-sectional image, the thickness D can, for example, be continuously recorded along a cutting plane, i.e.integrated, or captured in the image by several discrete measurements followed by averaging.

[0065] It is preferably provided that a summed thickness of the bonding layer 12 and the further bonding layer 12', which is formed between the at least one further metal layer 20 and the insulation element 30, is used. In this case, the thicknesses D of the bonding layer 12 and the further bonding layer 12', which are arranged opposite one another or congruent with one another as seen in the stacking direction S, are to be summed up. The summed thickness D is in turn determined at different positions in the area F or the areas F and then preferably determined over a plurality of areas or a plurality of rectangles which together form the at least one metal layer 10. In particular, the term averaged means that over the entire at least one metal layer 10 in different area regions orRectangles a certain number, preferably a total of more than 25 measured values, particularly preferably more than 100 measured values ​​and particularly preferably more than 500 measured values, are used, wherein in each surface area or rectangle the measured values ​​are distributed stochastically over the area F.

[0066] In the Fig. 6a and Fig. 6b shows two exemplary cross-sectional images through a carrier substrate 1. In particular, these are copper-ceramic substrates. While in the Fig. 6a shows a copper-ceramic substrate, for the production of which a classic solder paste was used, the copper-ceramic substrate of the Fig. 6b by means of an active metal layer 15 applied by means of a PVD process and by means of a solder base material 16.

[0067] The classic silver-based solder paste contained titanium as the active metal, and the titanium content in the solder paste can be assigned to a 1.5 µm active metal equivalent layer thickness, while the active metal layer applied using the PVD process has a thickness D of 300 nm. AgCuln with a layer thickness of 20 µm was used as solder base material 16.

[0068] First, the figures shown reveal the solder base layer 14 as a bright stripe. Both cross-sectional images also reveal silver inclusions 42 in the copper layer, i.e., the at least one metal layer 10. These inclusions 42 in the copper layer are not to be taken into account when measuring the thickness of the bonding layer 13.

[0069] The sections shown from the SEM images show that a homogeneously distributed bonding layer 13 is formed in cross-sectional image 6b. Furthermore, it can be seen that the number of brittle intermetallic phases 41 is primarily found in the bonding layer 13, which was produced using the conventional solder paste. The brittle intermetallic phases 41 are found in both the solder base layer 14 and the adhesion promoter layer 13.

[0070] The number, frequency, or size of the brittle intermetallic phases 41, in turn, influences the peel strength, in particular in such a way that the peel strength increases with a decrease in the number of brittle intermetallic phases 41. The formation of the brittle intermetallic phases 41 is linked to the amount of active metal, in this case titanium.

[0071] This leads to the relationship between the peel strength and the thickness of the adhesion promoter layer 13, which is Fig. 7. It can be seen that with decreasing thickness of the titanium layer or the equivalent thickness based on the amount of titanium used in solder pastes, the peel strength in N / mm increases.

[0072] The peel strengths determined here were determined as follows: First, a carrier substrate 1 is provided, to which a 0.8 mm thick copper layer has been bonded to a ceramic element on both sides using a soldering process. For a peel test, the copper is structured as follows: length x width: 105 mm x 5 mm. The carrier substrate is clamped in a tensile testing machine. The copper strip is peeled from the ceramic surface at a uniform speed of 10 mm / min at an angle of 90° (+ / - 5°). The force to be applied is continuously recorded over the length of the strip or measurement. The average value is calculated from the value range of the peel forces to be applied between 10% and 90% of the measuring length and then normalized to the width of the peel strip in N / mm.

[0073] In particular, it has been shown that the proportion of brittle intermetallic phases 42 depends on an active metal content in the bonding layer 13, in particular in the adhesion promoter layer 13. The proportion of the active metal, in particular of titanium, can in turn be determined by a surface resistance which increases with decreasing proportion of active metal.

[0074] In the Fig. 8a and Fig. Figure 8b shows a method for determining the sheet resistance. Here, at least one metal layer 10 and then the solder base layer 14 are etched away from the carrier substrate 1, so that essentially only the adhesion promoter layer 13 remains (see Fig. 8a). The sheet resistance is then determined using a four-point method.

[0075] For this purpose, an arrangement of four measuring probes 45 is used, which are arranged next to each other in a row with the same distance s of 5 mm. This arrangement is shown in Fig. 8b. The rounded measuring tips 45 are placed onto the etched-off adhesion promoter layer 13 with a contact force of 1.5 N or less. Care is taken to ensure that the measuring tips 45 are sufficiently spaced from the edge of the sample, namely more than three times the distance s between two adjacent measuring tips 45. While the two outer measuring tips 45 generate a current I, the two inner measuring tips 45 determine a voltage V. To avoid heating in the sample, a current I below 50 mA is used. Accordingly, the resistance R is determined from the ratio of the voltage V to the current I. Subsequently, the surface resistance R is determined. ▪ in Ohm / sq according to the following formula R■=ρd=πln(2)⋅R≈4.5324⋅R

[0076] According to the manner described above, adhesion promoter layers 13 were measured, which were produced using the following solder materials: Probe Lot Form Titan Referenz 1 AgCu26Ti5In2 Paste 30 µm In Paste 1500 nm Referenz 2 AgCu26Ti5In2 Paste 30 µm In Paste 1500 nm AMB V 1 AgCu27.4In2 Folie 8 µm PVD 300 nm AMB V 2 AgCu27.4In2 Folie 8 µm PVD 300 nm AMB V 3 AgCu27.4In2 Folie 8 µm PVD 300 nm AMB V 4 AgCu27.4In2 Folie 6 µm PVD 300 nm AMB V 5 AgCu27.4In2 Folie 10 µm PVD 300 nm

[0077] The references used here (Reference 1 and Reference 2) are conventional solder pastes containing titanium as an active metal. The titanium content of the paste corresponds to an active metal equivalent layer thickness of 1500 nm. In this case, the paste thickness is approximately 30 µm. This equivalent layer thickness is determined based on the titanium content of the paste, as titanium is a component of the paste and is evenly distributed throughout it. The paste was applied with a layer thickness of approximately 30 µm between a copper layer and a Si3N4 ceramic layer, and the bonding process was then carried out.

[0078] The solder systems from samples AMB V1 to AMB V5 consisted of a 300 nm thick titanium active metal layer deposited onto the Si3N4 ceramic layer using PVD. The solder base material 16 corresponds to the composition of the conventional solder paste (without titanium) used in references 1 and 2 and was provided as a solder foil. The solder system was placed between the Si3N4 ceramic layer and the copper layer and then bonded.

[0079] To determine the sheet resistance, the copper layer and the solder base layer 14 were removed again by etching. As a result, the adhesion promoter layer 13 remains on the top and bottom of the ceramic layer, respectively.

[0080] Using an XRF measurement, the component contents on the top surfaces of the samples were determined. The results show the following element contents on the top and bottom surfaces of the ceramic layer with the adhesion promoter layer in at%: Probe Y Si Ti Ag Cu Referenz 1 3.85 83.36 12.60 0.05 0.16 Referenz 2 3.84 85.52 10.48 0.04 0.14 AMB V 1 1.73 95.49 2.72 0.01 0.06 AMB V 2 3.09 94.18 2.67 0.02 0.06 AMB V 3 1.75 95.37 2.81 0.02 0.06 AMB V 4 1.67 95.41 2.85 0.02 0.06 AMB V 5 1.97 95.53 2.44 0.02 0.06

[0081] The table shows that the silver and copper contents on the top and bottom of the sample are negligible, so that they have no significant influence on the sheet resistance.

[0082] In Fig.Figure 9 summarizes the results for the sheet resistances, determined using the method described above. It can be seen that the sheet resistances for samples AMB V1 to AMB V5 are more than 15 times greater than the sheet resistances for references 1 and 2. For samples AMB V1 to AMB V5, ceramics from different manufacturers and different PVD systems were also used. The sheet resistances reflect the proportion of titanium in the bonding layer 12 and the adhesion promoter layer 13, respectively, as can also be seen from the XRF measurements. This reduced titanium content has a significant influence on the formation of brittle intermetallic phases 42 in the bonding layer 12, and particularly in the adhesion promoter layer 13, which in turn adversely affect the peel strength.The reduced sheet resistance thus indicates that there is a reduced formation of intermetallic phases when the sheet resistance is greater than 5 Ohm / sq, preferably greater than 10 Ohm / sq and particularly preferably greater than 20 Ohm / sq. Reference symbol. 1 carrier substrate 10 metal layer 12 binding layer 12' additional binding layer 13 Adhesion promoter layer 14 Solder base layer 15 Active metal layer 16 Solder base material 20 additional metal layers 30 insulation layer 41 brittle intermetallic phases 42 inclusions 45 measuring tips s distance D Thickness HSE main extension level S Stacking direction

Claims

[1] Carrier substrate (1), in the form of a metal-ceramic substrate as a carrier for electrical components, comprising: - at least one metal layer (10) and - an insulation element (30) in the form of a ceramic element, a glass element, a glass-ceramic element and / or a high-temperature-resistant plastic element, wherein the at least one metal layer (10) and the insulation element (30) extend along a main extension plane (HSE) and are arranged one above the other along a stacking direction (S) running perpendicular to the main extension plane (HSE), wherein in the manufactured carrier substrate (1) a bonding layer (12) is formed between the at least one metal layer (10) and the insulation element (30) with a soldering system which has an active metal layer and a phosphorus-free soldering layer comprising a plurality of materials, and wherein an adhesion promoter layer (13) of the bonding layer (12) has a surface resistance which is greater than 20 ohms / sq. [2] Carrier substrate (1) according to claim 1, wherein a thickness (D) of the bonding layer (12) measured in the stacking direction (S), averaged over several measuring points within one or more predetermined areas (F) which run or run parallel to the main extension plane (HSE), assumes a value which is less than 10 µm. [3] Carrier substrate (1) according to one of the preceding claims, wherein the carrier substrate (1) comprises at least one further metal layer (20) which is bonded to the insulation element (30) on a side opposite the at least one metal layer (10), wherein in the manufactured carrier substrate (1) a further bonding layer (12') is formed between the at least one further metal layer (20) and the insulation element (30), wherein a summed thickness of the bonding layer (12) and the further bonding layer (12'), measured in the stacking direction (S), averaged over a plurality of measuring points within the area (F) or areas (F) which run parallel to the main extension plane (HSE), assumes a value which is less than 0 0.0225 mm. [4] Carrier substrate (1) according to one of the preceding claims, wherein the bonding layer (12) and / or the further bonding layer (12') comprises a silver-rich layer of a solder material and / or a solder base material (16). [5] Carrier substrate (1) according to one of claims 1 to 3, wherein the bonding layer (12) and / or the further bonding layer (12') is an adhesion-promoting layer (13) comprising an active metal. [6] Carrier substrate (1) according to claim 5, wherein a thickness (D) of the bonding layer (12) and the further bonding layer (12) measured in the stacking direction (S) and summed up, averaged over several measuring points within the area (F) which runs parallel to the main extension plane (HSE), assumes a value which is less than 0.0005 mm. [7] A method for producing a carrier substrate (1), namely a metal-ceramic substrate, according to one of the preceding claims, comprising: - Providing at least one metal layer (10) and one insulating element (30), namely a ceramic element (30), a glass element, a glass-ceramic element and / or a high-temperature-resistant plastic element, wherein the at least one metal layer (10) and the insulating element (30) extend along a main extension plane (HSE), - arranging the at least one metal layer (10) and the insulation element (30) one above the other in a stacking direction (S) running perpendicular to the main extension plane (HSE), wherein a soldering system with an active metal layer (15) and a phosphorus-free solder layer comprising several materials is arranged between the at least one metal layer (10) and the insulation element (30), and - Bonding the at least one metal layer (10) to the insulation element (30) via the soldering system to form a bonding layer (12) between the at least one metal layer (10) and the insulation element (30). [8] Method according to claim 7, wherein a proportion of impurities in the arranged active metal layer (15) is less than 0.5 wt.%. [9] Method according to one of the preceding claims, wherein a physical and / or chemical vapor deposition or vapor deposition or an electrochemical deposition is carried out such that a density of the active metal arranged on the insulating element is greater than 99% of the theoretical density of the active metal. [10] Method according to one of the preceding claims, wherein a roughness R a a surface of the insulation element (30) is at least partially smaller than 1.0 µm.

Citation Information

Patent Citations

  • Electronic device

    DE102009033029A1

  • Metal-ceramic substrates and methods for producing a metal-ceramic substrate

    DE102013104739A1

  • Method for producing a metal-ceramic substrate

    DE102013113734A1

  • Method of making a metal-ceramic substrate

    DE102013113734B4

  • Method for producing a composite material

    DE102015108668A1