Copper-containing conductive pastes

A copper-containing conductive paste with Ge-coated Cu particles and glass frit allows air firing, addressing the cost and oxidation issues of copper, achieving low resistance electrodes.

DE112014006910B4Active Publication Date: 2024-11-28SOLAR PASTE LLC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
DE112014006910
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Filing Date
2014-08-28
Publication Date
2024-11-28
Estimated Expiration
2034-08-28

AI Technical Summary

Technical Problem

The use of precious metals like silver and palladium in conductive pastes for electronics increases material costs, and copper, although cheaper, cannot be air-fired due to oxidation, necessitating a solution that allows for low-cost copper use while maintaining low resistance and enabling air firing.

Method used

A copper-containing conductive paste comprising coated Cu particles with germanium (Ge) and optionally boron (B), dispersed in an organic medium with glass frit, allowing air firing and achieving low resistance electrodes.

Benefits of technology

The solution reduces material costs by using copper and enables air firing, resulting in electrodes with specific resistance ranging from 3E-06 to 5E-02 ohm-cm, maintaining high conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

Copper-containing (Cu-containing) conductive paste comprising: (a) about 10-95 wt% of a powder of coated Cu particles and (b) about 0.1-15 wt.% of a glass frit, which is in (c) are dispersed in an organic medium, wherein the total weight percentage of all components comprising the paste is 100 wt% and wherein (i) the coated Cu particles consist of core Cu particles surface-coated with germanium (Ge) and the Ge content level is about 0.01-35 parts by weight per 100 parts by weight of the core Cu particles; and (ii) the organic medium consists of at least one organic polymer dissolved in at least one solvent.
Need to check novelty before this filing date? Find Prior Art

Description

FIELD OF THE INVENTION

[0001] The invention relates to copper-containing conductive pastes. STATE OF THE ART

[0002] Precious metal powder, such as silver powder, is used in the electronics industry to produce conductive pastes. The conductive pastes are screen-printed onto substrates to form conductive circuit patterns. These circuits are then dried and fired to evaporate and burn out the liquid organic medium and sinter the metal particles.

[0003] Capital investment for the furnace can be reduced by using precious metals such as gold, silver, and palladium as conductors because these metals can be fired in air. However, the use of precious metals causes a sharp increase in material costs because precious metals are expensive.

[0004] Copper is widely used as a conductive component in semiconductor circuits and the like. Copper has the advantage of being less expensive than silver or other precious metals. However, copper cannot be fired in air because it oxidizes quickly, and this increases capital investment because firing under a nitrogen atmosphere and the like is required.

[0005] Thus, in the process of forming an electrode using a conductive paste, the development of technology is required that meets the following requirements: 1) enabling the use of inexpensive copper powder, 2) enabling the firing to be carried out in air, and 3) enabling low resistance in the electrodes.

[0006] The patent application US 2014 / 0 008 587 A1 describes a conductive paste comprising a conductive powder containing at least one of copper and nickel as main components.

[0007] Patent application JP 2011-6 739 A discloses a conductive paste containing a copper powder comprising 0.1 to 10 atm% Al, Mg, Ge and Ga in the interior of each particle and further comprising 0.1 to 10 atm% In.

[0008] US patent US 8 129 088 B2 describes a paste comprising an inorganic component containing copper powder, boron powder and glass frit. BRIEF SUMMARY OF THE INVENTION

[0009] Provided herein is a copper-containing (Cu-containing) conductive paste comprising: (a) about 10-95 wt.% of a powder of coated Cu particles, and (b) about 0.1-15 wt.% of a glass frit dispersed in (c) an organic medium, wherein the total weight percentage of all components comprising the paste totals 100 wt.%, and wherein (i) the coated Cu particles consist of core Cu particles surface-coated with germanium (Ge), and the content level of Ge is about 0.01-35 parts by weight based on 100 parts by weight of the core Cu particles; and (ii) the organic medium consists of at least one organic polymer dissolved in at least one solvent.

[0010] In one embodiment of the Cu-containing conductive paste, the content level of Ge contained in the coated Cu particles is about 0.1-30 parts by weight based on 100 parts by weight of the core Cu particles.

[0011] In another embodiment of the Cu-containing conductive paste, the content level of Ge contained in the coated Cu particles is about 0.2-25 parts by weight based on 100 parts by weight of the core Cu particles.

[0012] In yet another embodiment of the Cu-containing conductive paste, the coated Cu particles further comprise boron (B) coated over the core Cu particles, and the content level of B is about 0-15 parts by weight based on 100 parts by weight of the core Cu particles.

[0013] In yet another embodiment of the Cu-containing conductive paste, the content level of B is about 0.05-10 parts by weight based on 100 parts by weight of the core Cu particles.

[0014] In yet another embodiment of the Cu-containing conductive paste, the content level of B is about 0.05-3 parts by weight based on 100 parts by weight of the core Cu particles.

[0015] In yet another embodiment of the Cu-containing conductive paste, the core Cu particles contained in the coated Cu particles have a particle diameter (D50) of about 0.08-50 µm.

[0016] In yet another embodiment of the Cu-containing conductive paste, the core Cu particles contained in the coated Cu particles have a particle diameter (D50) of about 1-30 µm.

[0017] In yet another embodiment of the Cu-containing conductive paste, the core Cu particles contained in the coated Cu particles have a particle diameter (D50) of about 1-15 µm.

[0018] Further described herein is an article comprising a structural element, wherein the structural element consists of a substrate and at least one Cu electrode, wherein the at least one Cu electrode is formed as follows: (I) applying a Cu-containing conductive paste to one side of the substrate in a predetermined shape and at a predetermined position; (II) drying the Cu-containing conductive paste; and (III) firing the Cu-containing conductive paste to form the at least one Cu electrode, and wherein the Cu-containing conductive paste comprises: (a) about 10-95 wt.% of a powder of coated Cu particles and (b) about 0.1-15 wt.% of a glass frit dispersed in (c) an organic medium, wherein the total weight percentage of all components contained in the paste totals 100 wt.-% and wherein (i) the coated Cu particles consist of core Cu particles surface-coated with Ge, and the Ge content level is about 0.01-35 parts by weight based on 100 parts by weight of the core Cu particles; and (ii) the organic medium consists of at least one organic polymer dissolved in at least one solvent. During step (III), the Cu-containing conductive paste can be fired in air. It is further described that the article can be an electronic article selected from the group consisting of displays, solar cells, capacitors, transistors, inductors, and resistance heaters.

[0019] Furthermore, a solar cell is described which comprises a semiconductor substrate and at least one Cu electrode attached to a front or back side thereof, wherein the at least one Cu electrode is formed as follows: (I) applying a Cu-containing conductive paste to the front or back side of the semiconductor substrate in a predetermined shape and at a predetermined position; (II) drying the Cu-containing conductive paste; and (III) firing the Cu-containing conductive paste to form the at least one Cu electrode, and wherein the Cu-containing conductive paste comprises: (a) about 10-95 wt.% of a powder of coated Cu particles and (b) about 0.1-15 wt.% of a glass frit dispersed in (c) an organic medium, wherein the total weight percentage of all components contained in the paste totals 100 wt.-% and wherein (i) the coated Cu particles consist of core Cu particles surface-coated with Ge, and the Ge content level is approximately 0.01-35 parts by weight, based on 100 parts by weight of the core Cu particles; and (ii) the organic medium consists of at least one organic polymer dissolved in at least one solvent. During step (III), the Cu-containing paste can be fired in air. It is further described that the semiconductor substrate can be selected from the group consisting of single-crystal silicon species and multi-crystalline silicon species. The at least one Cu electrode can be formed on the front side of the semiconductor substrate and in the form of a multiple number of parallel conductive fingers and one or more front-side busbars perpendicular to the conductive fingers.The at least one Cu electrode can be formed on the back side of the semiconductor substrate and in the form of one or more back side bus bars. BRIEF DESCRIPTION OF THE DRAWINGS Fig. Figure 1(a) is a scanning electron microscopy (SEM) image of uncoated Cu particles. Fig. Figure 1(b) is an SEM image of coated Cu particles. The Fig. 1(c) and Fig. 1(d) are SEM images of the cross section of a coated Cu particle. Fig. Figure 2(a) is a planar view of the front surface of a solar cell. The Fig. 2(b) and Fig. 2(c) are cross-sectional views of solar cells with different back electrode designs. DETAILED DESCRIPTION OF THE INVENTION

[0020] Disclosed herein are copper-containing (Cu-containing) conductive pastes, copper (Cu) electrodes formed by firing the Cu-containing conductive paste over a substrate, and articles comprising a structural member having such Cu electrodes. CONDUCTIVE PASTES CONTAINING CU

[0021] The Cu-containing conductive pastes disclosed herein contain an inorganic powder, such as powder of coated Cu particles and glass frits, dispersed in an organic medium to form the "paste" having a suitable viscosity for application to a substrate.

[0022] The glass frit comprises fusible oxides, such as crystal formers, intermediate oxides, and / or modifiers. The term "fusible," as used herein, refers to the ability of a material to become fluid upon heating, such as the heating used in firing processes. In some embodiments, the fusible material consists of one or more fusible subcomponents. For example, the fusible material may comprise a glass material or a mixture of two or more glass materials. Glass material in the form of a fine powder, e.g., from a comminution process, is often called "frit" and is readily incorporated into the present paste composition. The glass frit may be crystalline, partially crystalline, amorphous, partially amorphous, or a combination thereof.

[0023] As used herein, the term "glass" refers to a particulate solid form, such as an oxide or oxyfluoride, that is at least predominantly amorphous, meaning that short-range atomic order is preserved in the immediate vicinity of any selected atom, i.e., in the first coordination shell, but disperses at higher atomic-level distances (i.e., there is no periodic long-range order). Therefore, the X-ray scattering pattern of a completely amorphous material exhibits broad, diffuse peaks, rather than the well-defined, narrow peaks of a crystalline material. In the latter, the regular spacing of characteristic crystallographic planes results in narrow peaks whose position is in reciprocal space according to Bragg's law.A glass material also exhibits no significant crystallization exotherm upon heating near or above its glass transition temperature or softening point, Tg, which is defined as the second transition point seen in a differential thermal analysis (DTA) scan. In one embodiment, the softening point of the glass material used in the present paste composition is in the range of 300 to 800°C.

[0024] It is also contemplated that some or all of the oxides in glass frits may be composed of material exhibiting some degree of crystallinity. For example, in some embodiments, a plurality of oxides are fused together, resulting in a material that is partially amorphous and partially crystalline. As one of ordinary skill in the art would appreciate, such a material would produce an X-ray diffraction pattern exhibiting narrow crystalline peaks superimposed over a pattern of broad diffuse peaks. Alternatively, one or more constituents, or even substantially all of the fusible material, may be predominantly or even substantially entirely crystalline. In one embodiment, crystalline material useful in the fusible material of the present paste composition may have a melting point of at most 800°C.In particular, the Cu-containing conductive paste disclosed herein comprises (i) a powder of coated Cu particles and (ii) a glass frit dispersed in (iii) an organic medium. The paste has a suitable viscosity for application to a substrate. The viscosity of the Cu-containing conductive paste may be about 0.05-5000 Pa s at a shear rate between about 0.2-350 s. -1 In certain embodiments, a viscosity of 5-800 Pa·s is preferred when screen printing is used. (i) Powder coated Cu particles

[0025] The powder-coated Cu particles used here are formed from core Cu particles surface-coated with a coating material comprising germanium (Ge). For example, during a dry coating process, fine-sized Ge powder (preferably nano-sized particles) is applied to the surface of the core Cu particles, forming a thin coating layer. Alternatively, during a wet coating process, Ge colloids are coated or grown on the surface of the core Cu particles, followed by drying. Or Ge atoms are deposited over the surface of the core Cu particles during a vacuum deposition process. Preferably, the Ge coating layer has a thickness of no more than one micron or no more than 500 nanometers.

[0026] The core Cu may be pure Cu or a Cu alloy with nickel, silver, aluminum, zinc, tin, silicon, iron, manganese, germanium, boron, or a mixture thereof. Among these, Cu alloys with zinc, tin, aluminum, silicon, or mixtures thereof are preferred. The pure Cu may have a purity of at least about 80% Cu in one embodiment, at least about 90% Cu in another embodiment, or at least about 95% Cu in yet another embodiment.

[0027] One of ordinary skill in the art would recognize that the choice of raw materials could inadvertently include impurities that could be incorporated into the Cu during processing. For example, impurities may be present in the range of hundreds to thousands of parts per million. Impurities commonly found in industrial metals used herein are known to one of ordinary skill in the art.

[0028] The particle diameter (D50) of the core Cu particles can be about 0.08-50 µm in one embodiment, about 0.5-30 µm in another embodiment, or about 0.5-15 µm in yet another embodiment. As used herein, "particle diameter (D50)" shall mean the 50% volume distribution size. The particle diameter (D50) can be obtained by measuring the particle diameter distribution using light scattering methods, for example, according to ASTM B822-10.

[0029] The powder can be well dispersed in the organic medium if the particle diameter (D50) of the core Cu particles is within the disclosed range. And the conductive paste can be fired to form an electrode with a certain conductivity if the particle diameter (D50) of the core Cu particles is within the disclosed range.

[0030] The core Cu used here can have any shape. For example, it can be spherical, flake-shaped, or irregular. When certain processes, such as dry coating or melt coating, are used to produce the coated Cu particles, the use of spherical core Cu can be advantageous.

[0031] The coated Cu particles can be coated with about 0.01-35 parts by weight, about 0.1-30 parts by weight, or about 0.2-25 parts by weight of Ge, based on 100 parts by weight of core Cu.

[0032] In certain embodiments, the coating material used herein to coat the core Cu may further comprise boron (B).

[0033] The boron may be present in the coated Cu particles at a level of up to about 15 parts by weight, or about 0.05-10 parts by weight, or about 0.05-3 parts by weight, based on 100 parts by weight of core Cu.

[0034] The Ge-containing coating material used herein to form the coated Cu particles may be about 0.1-40 parts by weight in one embodiment, about 0.2-30 parts by weight in another embodiment, or about 0.4-25 parts by weight in yet another embodiment, based on 100 parts by weight of the core Cu. And the Ge-containing coating material is applied to and covers at least about 50%, or at least about 60%, or at least about 80% of the surface area of ​​the core Cu particles. Also, the thickness of the Ge-containing coating layer over the core Cu particles may be in the range of about 1-500 nm, or about 1-300 nm, or about 1-150 nm.

[0035] The particle diameter (D50) of the coated Cu particles can be about 0.08-50 µm in one embodiment, about 0.5-30 µm in another embodiment, or about 0.5-15 µm in yet another embodiment. The Cu-containing conductive paste can be well dispersed in the organic medium if the particle diameter of the coated Cu particles is within the disclosed range. Also, the particle diameter (D50) of the coated Cu particles should not be too large so that processability can be maintained when applying the Cu-containing paste over a substrate. And the particle diameter (D50) of the coated Cu particles should not be too small so that the conductivity of the electrodes produced therefrom has a certain high conductivity level. The particle diameter (D50) can be measured in the same way as for the core Cu particles described above.

[0036] The coated Cu particles can be in flake form, spherical form or other irregular shapes and mixtures thereof.

[0037] The coated Cu powder can be present in the Cu-containing conductive paste at a level of about 10-95 wt%, about 40-95 wt%, or about 60-95 wt%, based on the total weight of the Cu-containing conductive paste. The coated Cu powder in the above range provides sufficient conductivity to the electrode.

[0038] In addition to the coated Cu powder, any other additional metal powder may be added to the Cu-containing conductive paste. For example, a powder of silver (Ag), gold (Au), palladium (Pd), aluminum (Al), platinum (Pt), nickel (Ni), tin (Sn), or mixtures or alloys of two or more of these metals may be added to the Cu-containing paste. In one embodiment, the Cu-containing conductive paste may comprise one or more of the following: Ag, Pt, Al, Ni, alloys of Ag and Pd, and alloys of Pt and Au. Such additional metals may be present in the Cu-containing conductive paste at a total content level of up to about 60 wt.%, based on the total weight of the paste.

[0039] The coated Cu particles can be produced by any suitable method, for example, wet coating, dry coating, melt coating, encapsulation, vapor processing, plasma processing, or a combination of two or more of these techniques. Coating equipment includes a fluidized bed coater, spray bed coater, Wurster coater, rotary drum, pan and plate coater, fluidized bed reactor with chemical vapor deposition, and plasma-enhanced chemical vapor deposition. (ii) GLASS FRIT

[0040] Glass frit can serve several purposes, including assisting in the sintering of the conductive powder and improving the adhesion of the electrode to the substrate. Complex oxides that can behave exactly like glass frit during firing can also be considered glass frit.

[0041] The glass frit used herein can be incorporated into the Cu-containing conductive paste at a level of about 0.1-15 wt%, or about 0.2-10 wt%, or about 0.5-8 wt%, based on the total weight of the paste. With such an amount, the glass frit can achieve the above-mentioned objective. The particle diameter (D50) of the glass frit in the paste can be about 0.1-10 µm in one embodiment, about 0.3-6 µm in another embodiment, or about 0.6-4 µm in yet another embodiment. A uniform dispersion of the glass frit within the paste can be obtained if the particle diameter (D50) of the glass frit is kept within the disclosed range. The particle diameter (D50) can be measured in the same manner as for the core Cu particles described above.

[0042] The chemical composition of the glass frit used here is not limited. Any glass frit may be suitable for use in the Cu-containing conductive paste. For example, a lead-boron-silicon glass frit or a lead-free bismuth glass frit, such as the bismuth-based oxide compositions disclosed in Table 1 of US 2012 / 0312368, may be used here. The softening point of the glass frit may be approximately 300-800°C. When the softening point is within the disclosed range, the glass frit melts properly to achieve the aforementioned effects. The softening point can be determined by differential thermal analysis (DTA). (iii) ORGANIC MEDIUM

[0043] The inorganic powders, such as coated Cu powder and glass frit, are dispersed in the inorganic medium to form a viscous composition called a "paste" with a suitable viscosity for application to a substrate in a desired pattern. Suitable organic media should have rheological properties that provide a stable dispersion of solids, suitable viscosity and thixotropy for applying the paste to a substrate, suitable wettability on the substrate and the paste solids, a good drying rate, and good firing properties.

[0044] There is no restriction on the composition of the organic medium used here. The organic medium used here may be a solution consisting of at least one organic polymer dissolved in at least one solvent.

[0045] A variety of organic polymers can be used herein, for example, sugar, starch, cellulose, wood rosin, epoxy resin, phenolic resin, acrylic resin, polyacrylates, polyesters, polylactones, phenoxy resins, or a mixture of two or more thereof. Among these, preferred celluloses include, without limitation, ethylcellulose, cellulose nitrate, hydroxyethylcellulose, ethylhydroxyethylcellulose, carboxymethylcellulose, hydroxypropylcellulose, and mixtures and derivatives thereof.

[0046] Suitable solvents may include, without limitation, terpenes (e.g., alpha- or beta-terpineol), kerosene, dibutyl phthalate, butyl carbitol, butyl carbitol acetate, hexylene glycol, alcohols with boiling points above 150°C, alcohol esters, bis(2-(2-butoxyethoxy)ethyl adipate, dibasic esters, octyl epoxide tallate, isotetradecanol, pentaerythritol esters of hydrogenated rosin, and mixtures thereof.

[0047] The solvents may also include volatile liquids to assist in rapid curing after the paste is applied to a substrate.

[0048] The organic medium may further contain thickeners, stabilizers, surfactants and / or other common additives to improve the performance of the paste such as better printability, better dispersion and / or better stability.

[0049] The optimal amount of organic medium in the Cu-containing conductive paste depends on the method of applying the paste and the specific organic medium used. Typically, the Cu-containing conductive paste disclosed herein may contain about 3-70 wt.%, about 3-65 wt.%, or about 5-58 wt.% of the organic medium, based on the total weight of the paste. (iv) ADDITIONAL INORGANIC POWDER

[0050] An additional inorganic powder can optionally be added to the Cu-containing conductive paste. The additional inorganic powder is not absolutely necessary. However, the additional inorganic powder can improve various properties of the electrode, such as adhesion and conductivity.

[0051] In one embodiment, the additional inorganic powders used herein can be selected from metals, metal oxides, or mixtures thereof. Exemplary metals used herein can be selected from Zn, Gd, Ce, Zr, Ti, Mn, Sn, Ru, Co, Fe, Cr, or mixtures of two or more thereof. Exemplary metal oxides used herein can be one or more oxides of Zn, Gd, Ce, Zr, Ti, Mn, Sn, Ru, Co, Fe, or Cr. The metal oxides used herein also include any compounds capable of producing the metal oxides upon firing, as described above.

[0052] The additional inorganic powder may be present in the Cu-containing conductive paste at a level of about 0.05-10 wt% in one embodiment, about 0.1-7 wt% in another embodiment, or about 0.2-6 wt% in yet another embodiment, based on the total weight of the paste.

[0053] The particle diameter (D50) of the additional inorganic powder is not particularly limited, although an average particle size of not more than 10 µm and preferably not more than 5 µm is desirable.

[0054] The Cu-containing conductive paste disclosed herein can be formed by any suitable mixing method. For example, the paste can be formed by simply mixing and dispersing the powder of coated Cu particles, glass frits, and optionally other inorganic particles in the organic medium. Cu electrodes and methods for producing the same

[0055] The Cu electrode is formed by first applying (e.g., dispensing, casting, coating, or printing) the Cu-containing conductive paste onto the surface of a substrate in a predetermined shape and at a predetermined position, drying the Cu-containing conductive paste at an elevated temperature (e.g., about 70-240 °C) for a certain period of time (e.g., about 2-20 min) to partially remove the organic medium, and then firing the Cu-containing conductive paste to remove the remaining organic medium and sintering the coated Cu particles with the glass frit and the other inorganic materials comprising the paste.

[0056] There are no restrictions on the substrate. The substrate material can be selected from glass, ceramics, semiconductors, metal, or other materials that can withstand the high temperature during firing. If the substrate is a metal or semiconductor substrate, an insulating layer can be formed on the side where the electrode is formed.

[0057] The method of applying the Cu-containing conductive paste to the substrate is not limited, and any suitable method can be used. Exemplary application methods useful herein include, without limitation, dispensing, screen printing, inkjet printing, casting, spraying, gravure printing, flexographic printing, stencil printing, nozzle dispensing, syringe dispensing, plating, extrusion, multi-layer printing or offset printing, direct writing, and the like. In particular, screen printing is often used because it is cost-effective. Also, when screen printing is used, the Cu-containing conductive paste can be applied to the substrate within a relatively short time. The pattern of the Cu-containing conductive paste on the substrate can be any desired electrode pattern, such as line(s), circle, or square.

[0058] The Cu-containing conductive paste applied to the substrate can optionally be dried in an oven at approximately 70°C–250°C for approximately 2–20 minutes. The drying process can be carried out at a moderate temperature to cure the paste by removing its most volatile organic substances.

[0059] The Cu-containing conductive paste is then fired onto the substrate in any atmosphere. A furnace set to a predetermined temperature and time profile can be used here.

[0060] The coated Cu powder sinters during firing to form the electrode with sufficient conductivity. The organic medium is removed by burning off and / or carbonization during firing.

[0061] Firing may be carried out in an atmosphere consisting of nitrogen, argon, or any other inert gas or an oxygen-containing mixture such as air or a mixed gas of oxygen and nitrogen. In one embodiment of the present disclosure, the Cu-containing conductive paste on the substrate is fired in air. The term "firing in air" or "air firing" essentially refers to firing without replacing the atmosphere in the firing chamber with a gas that contains no oxygen or contains less oxygen than the ambient atmosphere around the firing chamber. In one embodiment, the air surrounding the firing device is used as the firing atmosphere without replacing the firing atmosphere with another gas.

[0062] The firing condition may vary depending on the substrate type, the properties of the Cu-containing conductive paste, or the pattern of the Cu-containing conductive paste on the substrate. However, the electrode can generally be obtained by firing the Cu-containing conductive paste at a set peak temperature of about 400-1200°C and for a firing time of about 5 seconds to about 3 hours. The set peak temperature may be about 500-1100°C in one embodiment or about 550-1000°C in another embodiment. The firing time may be about 10 seconds to about 2 hours in one embodiment or about 30 seconds to about 1.5 hours in another embodiment. The firing condition can be adjusted by considering the firing temperature and firing time.For example, the Cu-containing conductive paste can be fired at a high temperature for a short time or a low temperature for a long time if the substrate is quickly damaged by the high temperature.

[0063] In certain applications, after firing, the paste-bearing substrate may need to be placed in a cooling device for slow cooling.

[0064] In one embodiment, firing is achieved by passing the substrate bearing the printed paste pattern through a belt furnace at high transport rates, for example, about 2.5-760 cm / min, with a firing time of about 10 seconds to about 3 hours. The firing time used here is the time from the start to the end of the firing. In certain embodiments, the paste-bearing substrate is first dried before entering a belt furnace, fired while passing through the belt furnace, and then cooled after exiting the belt furnace. In such embodiments, the firing time is the time from entry to exit from the furnace. Multiple temperature zones can be set for the belt furnace to regulate the desired heat profile, and the number of zones can vary, for example, from 3 to 11 zones.The firing temperature in a belt furnace is conventionally determined by the furnace setpoint in the hottest zone of the furnace, but it is known that the peak temperature achieved by passing the substrate through such a process is somewhat lower than the highest setpoint. Other batch and continuous rapid firing furnace designs known to those skilled in the art are also contemplated.

[0065] Electrodes are formed over the substrate after firing. The average width of the electrode may be about 10 µm to 100 mm in one embodiment, about 30 µm to 70 mm in another embodiment, or about 50 µm to 50 mm in yet another embodiment, and the average thickness may be about 1-200 µm in one embodiment, about 1-100 µm in another embodiment, or about 1-50 µm in yet another embodiment. In those embodiments where the electrodes are used in solar cells, the average width of the electrodes may be about 10 µm to 10 mm in one embodiment, about 30 µm to 7 mm in another embodiment, or about 50 µm to 5 mm in yet another embodiment.

[0066] As demonstrated by the examples below, replacing the more expensive Ag particles with less expensive coated Cu particles (as disclosed herein) in the conductive paste not only greatly reduces material costs, but the paste can also be fired in air, thus yielding electrodes with low resistivity. Specifically, the resistivity of the electrodes thus obtained ranges from about 3E-0.6 to about 5E-0.2 ohm-cm, or preferably from about 3E-0.6 to about 2E-0.4 ohm-cm.

[0067] Without being bound by any specific theory, it is believed that when Ge coats the surface of the core Cu particles, it reduces the oxidation of the Cu powder during firing in air. The Ge coating can also accelerate the sintering of the inorganic materials contained in the Cu-containing conductive paste. Consequently, the resistivity of electrodes derived from such a paste is reduced. ARTICLES INCLUDING THE STRUCTURAL ELEMENTS WITH THE CU ELECTRODES

[0068] Further disclosed herein are articles comprising a structural element, and the structural element consists of a substrate and Cu electrodes (described above) formed thereon. The articles disclosed herein include, without limitation, displays, solar cells, capacitors, transistors, inductors, resistance heaters, and the like.

[0069] A solar cell is described as an article comprising a semiconductor substrate and Cu electrodes formed thereon. The semiconductor substrates include, without limitation, single-crystal silicon, multicrystalline silicon, and the like.

[0070] The semiconductor substrates used here can be doped with phosphorus and boron to form a p / n junction. The semiconductor substrates also vary in size (length x width) and thickness. For example, the thickness of the semiconductor substrate used here can be approximately 50-500 µm, approximately 100-300 µm, or approximately 140-200 µm. The length and width of the semiconductor substrate can be approximately 100-250 mm, approximately 125-200 mm, or approximately 125-156 mm, respectively.

[0071] The semiconductor substrates of solar cells typically have a front side and a back side, with the front side of the semiconductor substrates facing a light source during use. And the Cu-containing conductive paste disclosed herein can be used to form the Cu electrodes on the front and / or back sides of the semiconductor substrates. And as described in the Fig. As illustrated in Figures 2(a)-2(c), the front-side electrodes may be formed from a multiple number of parallel conductive fingers (2) and one or more front-side busbars (4) perpendicular to the conductive fingers (2), while the back-side electrodes are formed from at least one back-side busbar (4') and Al paste (3). The back-side busbars (4') are also called tabbing and are typically positioned in mirror positions to the front-side busbars (4).

[0072] Typically, an anti-reflective coating and / or insulating coating can be formed on the front side of the semiconductor substrate of the solar cell. Exemplary anti-reflective coating or insulating coating materials used herein include, without limitation, silicon nitride, silicon oxide, titanium oxide, SiNx:H, hydrogenated amorphous silicon nitride, and silicon oxide / titanium oxide. The coating can be formed by plasma-enhanced chemical vapor deposition (PECVD), CVD, and / or other known techniques. Therefore, in fabricating the front-side electrodes on the semiconductor substrates, the Cu-containing conductive paste disclosed herein is applied over the anti-reflective coating and / or insulating coating on the semiconductor substrate by a variety of methods, as described above, in a predetermined pattern, shape, and position.

[0073] The front-side busbar(s) (4) of the semiconductor substrate can be formed from the Cu electrodes disclosed herein. The front-side busbars (4) can be in the form of continuous or discontinuous lines across the front side. And the front-side busbars (4) can have a width of about 0.5-4 mm or about 1-2 mm and a thickness of about 2-40 µm, about 2-30 µm, or about 3-20 µm. In addition, the conductive front-side fingers (2) can also be formed from the Cu electrodes disclosed herein. And each of the conductive fingers (2) can have a width of about 20-200 µm, about 30-150 µm, or about 30-100 µm and a thickness of about 3-100 µm, about 3-50 µm, or about 5-30 µm.When forming the front-side busbar(s) (4) and / or the conductive fingers (2), the Cu-containing conductive paste disclosed herein is first applied (e.g., by screen printing) over the front side of the semiconductor substrate in a predetermined pattern, shape, and position corresponding to the front-side busbars (4) and / or the conductive fingers (2) of the semiconductor substrate, then dried, for example, for about 0.5-10 minutes, during which time the volatile solvents of the organic medium are removed or partially removed. The dried paste is then fired by heating to a maximum temperature of about 500°C-1000°C for about 1 second to 2 minutes. Firing can be carried out in any atmosphere, preferably in air. During firing, the glass frit in the fired Cu electrodes (e.g.,the conductive fingers and optionally the front busbars) with the anti-reflective coating and / or insulating coating, thereby making electrical contact with and / or mechanical adhesion to the semiconductor substrate.

[0074] Furthermore, the Cu-containing conductive paste can be used to form the backside busbars (4') of the semiconductor substrate of the solar cell. The backside busbar(s) (4') can also be in the form of continuous or discontinuous lines across the backside. And the backside busbars (4') can have a width of about 0.5-5 mm or about 1-4 mm and a thickness of about 2-40 µm, about 2-30 µm, or about 3-20 µm. The Cu-containing conductive paste disclosed herein is applied over the backside of the semiconductor substrate in a predetermined pattern and shape and at a predetermined position. The predetermined pattern, shape, and position correspond to the backside busbars (4') of the semiconductor substrate.Other conductive materials containing aluminum or aluminum and silver may be deposited over the back surface of the semiconductor substrate, which are not compatible with the Cu-containing conductive paste (the Al paste (3) of . Fig. 2(b)). Other conductive materials containing aluminum or aluminum and silver may be coated over the entire back side of the semiconductor substrate before applying the Cu-containing conductive paste (the Al paste (3) in Fig. 2(c)). The Cu-containing conductive paste is applied over the coating formed from the other conductive materials. The paste-bearing semiconductor substrate is then subjected to firing in any atmosphere, preferably in air, to form the backside electrodes.

[0075] In practice, the front electrodes and the back electrodes of the semiconductor substrate can be formed sequentially or simultaneously. When the front electrodes and back electrodes are formed simultaneously, conductive pastes are first applied and dried on a first side of the substrate, then conductive pastes are applied and dried on a second side of the substrate, and finally, the paste-bearing substrate is fired in any suitable atmosphere, or preferably in air. Cu electrodes can thus be formed on both sides of the semiconductor substrates. EXAMPLE CONDUCTIVE PARTICLES

[0076] To form the Cu-containing conductive paste used in the examples, the following inorganic powders were used: TABLE 1 With D50 (µm) In-1 0,78 With-2 3,6 to-3 5,4 With-4 8,3 Mixed with Ge. D50 of Cu (µm) Cu:Ge (auf das Gewicht bezogen) Cu-Ge-1 0,78 100:5 Cu-Ge-2 3,6 100:5 Cu-Ge-3 5,4 100:5 Cu-Ge-4 5,4 100:8 Cu-Ge-5 8,3 100:5 Cu-Ge-6 5,4 100:20 Cu mixed with Ge and B D50 of Cu (µm) Cu:Ge:B (auf das Gewicht bezogen) Cu-Ge-B-1 5,4 100:5:1 Cu-Ge-B-2 5,4 100:8:1 Ag-coated Cu D50 of Cu (µm) Cu:Ag (auf das Gewicht bezogen) *Cu / Ag 3,5 80:20 Ge coated Cu D50 of Cu (µm) Cu:Ge (auf das Gewicht bezogen) Cu / Ge-1 5,4 100:2 Cu / Ge-2 5,4 100:5 Cu / Ge-3 5,4 100:8 Cu / Ge-4 5,4 100:20 Cu / Ge-5 0,78 100:5 Cu / Ge-6 3,6 100:5 Cu / Ge-7 8,3 100:5 Cu / Ge-8 5,4 100:4 Cu / Ge-9 5,4 100:6 Cu / Ge-10 5,4 100:6,7 Ge and B coated Cu D50 of Cu (µm) Cu:Ge:B (auf das Gewicht bezogen) Cu / Ge-B-1 5,4 100:5:0,5 Cu / Ge-B-2 5,4 100:5:1 Cu / Ge-B-3 5,4 100:5:8 Cu / Ge-B-4 5,4 100:8:1 Cu / Ge-B-5 5,4 100:4:1 Cu / Ge-B-6 5,4 100:6:1 Cu / Ge-B-7 5,4 100:2:0,1 Cu / Ge-B-8 5,4 100:2:2 Cu / Ge-B-9 5,4 100:5:4 Notes: • All copper (Cu) powders used here were purchased from Mitsui Mining & Smelting Co., Ltd. (Japan); • All germanium (Ge) nanoparticles used here were those with D50 of 70-120 nm and they were purchased from Forsman Scientific (Beijing) Co., Ltd. (China); • All boron (B) nanoparticles used here were those with D50 of 100 nm and they were purchased from Beijing Dk nano S&T Ltd. (China); • * The powder of Cu / Ag was purchased from Ningbo Guangbo New Nanomaterials Stock Co., Ltd. (China) with D50 of 3.5 µm.

[0077] The coated Cu powders (listed in Table 1 above) were prepared using a dry coating process in an oxygen-free environment with a rotor speed set at 3000-6000 rpm for a duration of 3 minutes.

[0078] The Fig. 1(a) and Fig.1(b) are scanning electron microscopy (SEM) images of uncoated Cu particles (Cu-3) and coated Cu particles (Cu / Ge-3), respectively. Fig. Figure 1(c) is an SEM image of the cross-section of coated Cu particles (Cu / Ge-3). The sample of the cross-section SEM image was prepared by mixing Cu / Ge-3 particles with epoxy resin, followed by thermal curing and ion beam cross-section polishing. Furthermore, using energy-dispersive X-ray spectroscopy (EDS), a Cu / Ge-3 particle was randomly picked, and an elemental analysis was performed at two randomly selected locations, A and B, on the particle surface ( Fig. 1(c) and Fig. 1(d)) and the results are listed in Table 2. The results show the difference in the surface morphology of uncoated and coated Cu particles. In particular, the uncoated Cu particles typically have smooth surfaces (see Fig.1(a)), while the coated Cu particles have roughened surfaces (see Fig. 1(b)). Also, as described in the Fig. 1(c)-1(d) and Table 2, core Cu particles were successfully coated by Ge into Cu / Ge-3 particles. TABLE 2 Elements Stella A Stella B C (wt.-%) 17,73 22,28 O (wt.-%) 02,07 02,60 Ge (wt.-%) 01,82 06,53 With (wt.-%) 78,38 68,59 COMPARISON EXAMPLES CE1-CE10 AND EXAMPLES E1-E15

[0079] In each of CE1-CE10 and E1-E15, a thick-film paste was prepared as follows: 8.3 g of inorganic powder (as listed in Table 3 for each sample), 0.29 g of Bi-Zn-B-Al-Ba-Si oxide glass frit similar to the bismuth-based oxide compositions disclosed in Table 1 of US 2012 / 0312368 (with D50 of 0.8 µm), 0.02 g of hydrogenated castor oil, 1.1 g of a solution comprising 10-20 wt% ethylcellulose dissolved in terpineol, and 0.29 g of 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate were mixed in a mixer (manufactured by Thinky USA Inc. (USA) with the model name ARE-3 10) at 2000 rpm for 1 min, followed by 5 min long grinding by hand.

[0080] For each sample, a stencil was used to cast a 30 µm thick line of paste layer (2 mm wide and 30 mm long) onto the front surface of a silicon cell (a 6-inch (180 µm thick) silicon wafer coated with silicon nitride, obtained from JA Solar Holdings Co. Ltd.). The silicon cell served as a substrate for supporting the paste. The paste layer was then dried at 100 °C for 5–10 min. The dried paste was fired in air using an IR oven (manufactured by Despatch Instruments (PRC) with the model name CF-7210). The temperature profile of the IR oven was set at 580–610–630–650–820–900 °C, and the belt speed was approximately 560 cm / min. Electrodes were then obtained on the silicon cell.

[0081] The plate resistance of the electrode on the surface of the silicon cell was measured using a four-probe method with a plate resistivity meter (manufactured by Napson Corp. (Japan) with the model name RT3000 / RG7), and the thickness of the electrode was measured using a Veeco surface profiler (manufactured by Veeco Instruments Inc. with the model name Dektak 150). The electrode resistivity was calculated using the equation below and listed in Table 3: ρ (specific resistance) = plate resistance × thickness × geometry correction = plate resistance × thickness × 1.9475 / 4.5324

[0082] The results show that when uncoated Cu was used in the thick-film paste (CE1), the resulting electrodes exhibited very high resistivity. When powdered Cu particles surface-coated with Ag were used in the thick-film paste (CE10), the resulting electrodes still exhibited very high resistivity. However, it was found that when Ge and optionally B were added to the thick-film paste in addition to uncoated Cu (CE2-CE9), the resistivity of the electrodes made from such thick-film pastes dropped dramatically.Even more surprisingly, it was further found that when Ge, and optionally Ge and B, were coated on the surface of the Cu particles and such coated Cu particles were used in the thick-film paste (E1-E15), the resistivity of the electrodes made from such thick-film pastes was further reduced. Furthermore, comparing E2 and E3 with E1 or E10, and E11 with E6, another advantage of coating both Ge and B on the surface of the Cu particles was demonstrated. That is, when Cu particles were coated by a mixture of Ge and B and such coated Cu particles were used in the thick-film paste (E2-E3 and E10-E11), the resistivity of the electrodes made from such thick-film pastes was further reduced. TABLE 3 Samples Inorganic powder Cu:Ge:B (auf das Gewicht bezogen) Spezifischer Widerstand (Ohm-cm) Type D50 of Cu (µm) EC1 With 5,4 100:0:0 9.37E+02 E1 Cu / Ge-1 5,4 100:2:0 8.94E-05 E2 Cu / Ge-B-7 5,4 100:2:0,1 2.96E-05 E3 Cu / Ge-B-8 5,4 100:2:2 2.07E-05 E4 Cu / Ge-5 0,78 100:5:0 4.51E-02 CE2 Cu-Ge-1 0,78 100:5:0 3.60E+02 E5 Cu / Ge-6 3,6 100:5:0 1.74E-05 EC3 Cu-Ge-2 3,6 100:5:0 1.08E-04 E6 Cu / Ge-2 5,4 100:5:0 2.30E-05 EC4 Cu-Ge-3 5,4 100:5:0 3.37E-05 E7 Cu / Ge-3 5,4 100:8:0 1.67E-05 CE5 Cu-Ge-4 5,4 100:8:0 3.30E-05 E8 Cu / Ge-4 5,4 100:20 1.45E-04 EC6 Cu-Ge-6 5,4 100:20 1.73E-04 E9 Cu / Ge-7 8,3 100:5:0 1.34E-05 EC7 Cu-Ge-5 8,3 100:5:0 5.24E-05 E10 Cu / Ge-B-1 5,4 100:5:0,5 1.34E-05 E11 Cu / Ge-B-2 5,4 100:5:1 1.13E-05 *E12 Cu / Ge-B-2 5,4 100:5:1 7.62E-06 CE8 Cu-Ge-B-1 5,4 100:5:1 2.13E-05 E13 Cu / Ge-B-9 5,4 100:5:4 3.67E-5 E14 Cu / Ge-B-3 5,4 100:5:8 6.66E-05 E15 Cu / Ge-B-4 5,4 100:8:1 1.67E-05 CE9 Cu-Ge-B-2 5,4 100:8:1 2.28E-05 CE10 Cu / Ag 3,5 - 4.98E+02

[0083] Notes:*For E12, the temperature profile of the IR oven was set to 580-610-630-650-820-1000 °C and the belt speed to approximately 660 cm / min. EXAMPLES E16-E19

[0084] In the same manner as described for E1, a thick film paste was prepared for each of E16-E19, and the thus-prepared thick film paste was fired over a silicon cell to form an electrode. During the firing process, the temperature profile was set at 580-610-630-650-700-700 °C, and the belt speed was set at 127 cm / min or 254 cm / min. The specific resistance of the electrode was determined and is tabulated in Table 4. For E16 and E18, the coated Cu particles were coated with Ge, while for E17 and E19, the coated Cu particles were coated with Ge and B. As shown, the addition of B to the coating material further reduces the specific resistance of the resulting electrodes. Furthermore, such an effect is even more obvious at a low belt speed, i.e., when a longer firing time was applied. TABLE 4 powder Specific resistance (Ohm-cm) type D50 of Cu (µm) Cu:Ge:B (by weight) Belt speed @ 127 cm / min Belt speed @ 254 cm / min E16 Cu / Ge-8 5,4 100:4:0 1,25E-03 1,36E-04 E17 Cu / Ge-B-5 5,4 100:4:1 3,96E-05 4,81E-05 E18 Cu / Ge-9 5,4 100:6:0 2,83E-04 1,34E-04 E19 Cu / Ge-B-6 5,4 100:6:1 3,10E-05 6,14E-05 COMPARISON EXAMPLE CE11 AND EXAMPLES E20-E21

[0085] Fig. Figure 2 illustrates a solar cell with electrodes. Fig. Figure 2(a) shows the front surface of a solar cell (1). The front electrodes of the solar cell (1) are formed from a multiple number of fingers (2) arranged parallel to each other and three front-side busbars (4) arranged perpendicular to the fingers (2). Additionally, ribbons (6) can later be electrically bonded (e.g., soldered) across the busbars (4). Fig. Figure 2(b) is a cross-sectional view of the solar cell (1) with electrodes. As shown in Fig. As shown in Figure 2(b), the back electrodes are formed from three back bus bars (4') which are in mirror position to the front bus bars (4) and an Al paste (3) covers the entire area of ​​the back surface of the solar cell (1) (except for the areas covered by the three back bus bars (4')).

[0086] At CE11 (as in Fig. 2(b)), the electrodes of a silicon cell were prepared as follows. First, a DuPont wz Solamet® PV17F silver paste for photovoltaic front-side metallization (obtained from EI du Pont de Nemours and Company (USA), hereinafter referred to as “DuPont”) was screen-printed over the front surface of the silicon cell at the position of the conductive fingers (2) and the front-side busbars (4), followed by drying at 240 °C for 3 min. Then, DuPont wzSolamet® PV505 silver paste for backside photovoltaic metallization (obtained from DuPont) was screen-printed onto the back surface of the silicon cell at the position of backside busbars (4'), followed by drying at 240°C for 3 min. Al paste PV35A (obtained from DuPont) was screen-printed over the backside of the silicon cell (except for the area covered by the backside silver paste), followed by drying at 240°C for 3 min. Finally, the silicon cell was fired in air using an IR oven. The temperature profile of the IR oven was set to 580-610-630-650-800-900°C, and the line speed was set to 560 cm / min. The Voc (open terminal voltage), Rs (series resistance), Rsh (shunt resistance), FF (fill factor) and Eff (cell efficiency) values ​​of the solar cell obtained above were measured on a Burger IV test fixture (supplied by Berger Lichttechnik GmbH & Co.(Germany), model name Berger Pulsed Solar Simulator, manufactured) and the results are tabulated in Table 5.

[0087] For E20 and E21, a Cu-containing conductive paste was prepared as follows: 150 g of powder of coated Cu (Cu / Ge-10), 6 g of glass frit, 1 g of hydrogenated castor oil, 0.2 g of caprylic acid, and 42.8 g of a solution consisting of 10-20 wt% ethylcellulose dissolved in terpineol were mixed in a mixer at 2000 rpm for 1 min; and the final Cu-containing conductive paste was obtained by passing the mixture twice through a three-roll machine (manufactured by EXAKT Technologies, Inc., model name EXAKT 50).

[0088] At E20 (as in Fig.2(b)), a solar cell with front and back electrodes was obtained in a similar manner as for CE1 1, except that the Cu-containing conductive paste was used as prepared above instead of the DuPont wz Solamet® PV505 silver paste was used for backside photovoltaic metallization to form the backside busbars.

[0089] At E21 (as in Fig. 2(c)), the electrodes of a silicon cell were prepared as follows. First, DuPont wzSolamet® PV17F silver paste for front-side photovoltaic metallization was screen-printed over the front surface of the silicon cell at the position of the fingers (2) and the front-side busbars (4), followed by drying at 240°C for 3 min. The Cu-containing conductive paste, prepared as above, was screen-printed at the position of the back-side busbars (4'), followed by drying at 240°C for 3 min. And Al paste PV35A was screen-printed over the entire surface of the backside of the silicon cell (except for the area covered by the Cu-containing conductive paste), followed by drying at 240°C for 3 min. Finally, the silicon cell was fired in air using an IR oven. Again, the temperature profile of the IR oven was set to 580-610-630-650-800-900 °C and the belt speed to 560 cm / min.The Voc, Rs, Rsh, FF, and Eff values ​​of the solar cell obtained above were measured on a Burger IV test fixture, and the results are tabulated in the table. As shown here, by replacing the expensive Ag-containing paste (CE 11) with less expensive Cu-containing paste (as disclosed here, E20 and E21) for forming the backside busbars, the cell efficiency was maintained. TABLE 5 Voc Rs Rsh FF (%) Eff (%) CE11 0,630 0,00241 337,1 79,39 18,0 E20 0,629 0,00238 129,8 78,31 17,8 E21 0,633 0,00267 341,1 79,24 18,1

Claims

[1] Copper-containing (Cu-containing) conductive paste comprising: (a) about 10-95 wt.% of a powder of coated Cu particles and (b) about 0.1-15 wt.% of a glass frit which is (c) an organic medium, wherein the total weight percentage of all components comprising the paste totals 100 wt%, and wherein (i) the coated Cu particles consist of core Cu particles surface-coated with germanium (Ge), and the content level of Ge is about 0.01-35 parts by weight based on 100 parts by weight of the core Cu particles; and (ii) the organic medium consists of at least one organic polymer dissolved in at least one solvent. [2] The copper-containing conductive paste according to claim 1, wherein the content level of Ge contained in the coated Cu particles is about 0.1-30 parts by weight based on 100 parts by weight of the core Cu particles. [3] The Cu-containing conductive paste according to claim 2, wherein the content level of Ge contained in the coated Cu particles is about 0.2-25 parts by weight based on 100 parts by weight of the core Cu particles. [4] The Cu-containing conductive paste according to claim 1, wherein the coated Cu particles further comprise boron (B) coated over the core Cu particles, and the content level of B is about 0-15 parts by weight based on 100 parts by weight of the core Cu particles. [5] The Cu-containing conductive paste according to claim 4, wherein the content level of B is about 0.05-10 parts by weight based on 100 parts by weight of the core Cu particles. [6] The Cu-containing conductive paste according to claim 5, wherein the content level of B is about 0.05-3 parts by weight based on 100 parts by weight of the core Cu particles. [7] The Cu-containing conductive paste according to claim 1, wherein the core Cu particles contained in the coated Cu particles have a particle diameter (D50) of about 0.08-50 µm. [8] The Cu-containing conductive paste according to claim 7, wherein the core Cu particles contained in the coated Cu particles have a particle diameter (D50) of about 1-30 µm. [9] The Cu-containing conductive paste according to claim 8, wherein the core Cu particles contained in the coated Cu particles have a particle diameter (D50) of about 1-15 µm.

Citation Information

Patent Citations

  • Thick film paste containing bismuth-based oxide and its use in the manufacture of semiconductor devices

    US20120312368A1

  • Imaging part holding unit, lens barrel and imaging apparatus

    JP2008116739A

  • Conductive paste

    US20140008587A1

  • Electrode and method for manufacturing the same

    US8129088B2

  • JP002011006739A