Organic carrier for solar cell conductive paste, preparation method and application
By using PaMS resin and organic solvent in the conductive paste in solar cell, the stability and volatility of the paste in long-term printing is solved, and the printing performance and photoelectric conversion efficiency of the conductive silver paste are improved. Achieve higher cell performance and stability.
Patent Information
- Application Number
- CN202411516102.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-29
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-10-29
AI Technical Summary
The existing conductive paste of solar cells is likely to cause the slurry phase separation and dryness during long-term printing, resulting in gate breakage, affecting battery efficiency and production efficiency.
Use PaMS resin as an elastomer to combine with organic solvents to improve the stability and bonding strength of the slurry, reduce volatility, combine appropriate thickeners and surfactants to form an organic carrier with high solubility for Prepare conductive silver paste.
It effectively improves the printing durability and photoelectric conversion efficiency of conductive pastes, avoids the phenomenon of gate breakage, maintains stable cell performance, and improves printing performance and storage stability.
Abstract
Description
Technical Field
[0001] The present application relates to the field of crystalline silicon solar energy technology, and in particular to an organic carrier for solar cell conductive paste, a preparation method and application thereof. Background Art
[0002] Crystalline silicon solar cells are the mainstream technology in photovoltaic power generation technology. Photovoltaic cells are based on silicon materials and cannot directly conduct current for use by contacting wires. Therefore, it is necessary to metalize the metal electrodes at both ends of the P-type semiconductor and the N-type semiconductor to reduce resistance and allow the current generated by light to enter the electronic device through the metal wires. Among them, the metalization process refers to coating or printing the metal paste at the corresponding position according to the needs, and then sintering the silicon material and the metal together at high temperature. Silver paste is usually selected as the material for metalization with silicon material. At present, most manufacturers use screen printing as a way to apply silver paste on silicon material. Compared with other methods of applying silver paste on photovoltaic silicon wafers to form grid lines, screen printing has the advantages of fast production speed and low cost. Therefore, the screen printing characteristics of silver paste have always been the main focus of silver paste product improvement. With the continuous iteration and upgrading of technology, the photoelectric conversion efficiency of solar cells is an important indicator for measuring the technology of crystalline silicon solar cells, and the aspect ratio of the grid line after printing directly affects the efficiency of the cell. In recent years, in addition to the requirements for the aspect ratio of the cross-section of the electrode made of silver paste, there are also higher requirements for printing durability. After the silver paste is printed on the screen for a long time and many times, the grid lines must remain unbroken, and the line shape and cross-sectional aspect ratio must not change. Traditional thixotropic agents are limited by their own characteristics and complex dispersion processes, which can easily cause the screen to become blocked, greatly affecting the photoelectric conversion efficiency of solar cells. At the same time, downtime processing problems can also reduce production efficiency. With the advancement of technology, the printing performance of the paste has become increasingly important. In addition to unbroken grids, the grid line width, aspect ratio and long-term printability must also be taken into account.
[0003] In order to increase the ink permeability, the existing solar cell conductive paste on the market usually chooses to reduce the concentration of resin (thickener), which easily leads to phase separation of the paste; or after a long period of printing, the solvent evaporates and causes the paste to dry, which easily causes the grid break phenomenon. Summary of the invention
[0004] In order to solve at least one of the above technical problems, an organic carrier with low volatility, good dispersibility and stable combination with conductive silver powder is developed. The present application provides an organic carrier for solar cell conductive paste, a preparation method and application.
[0005] On the one hand, the present application provides an organic carrier for a conductive paste for solar cells, wherein the organic carrier comprises the following raw materials in parts by weight: 1-30 parts of an elastomer, 6-20 parts of a thickener, 52-90 parts of an organic solvent, and 3-10 parts of an auxiliary agent; the elastomer is a PaMS resin; the auxiliary agent comprises a dispersant and a first surfactant in a weight ratio of 1-3:1-2.
[0006] By adopting the above technical solution, PaMS (poly alpha-methylstyrene) is used as an elastomer resin and a thickener in the organic carrier formula of the solar cell paste. Since PaMS has high solubility in most organic solvents, its carrier and paste have good stability; at the same time, adding PaMS as an elastomer to the organic solvent can greatly improve the initial viscosity and bonding strength of the organic carrier, and can also greatly reduce the overall volatility of the organic carrier; under long-term screen printing operation, it is not easy to produce a broken grid phenomenon, which can solve the problem of production line stoppage due to poor printing. Poly alpha-methylstyrene can absorb ultraviolet rays with a wavelength of 270 to 330nm, so it can improve the weather resistance of the prepared electrode to a certain extent.
[0007] Preferably, the organic carrier comprises the following raw materials in parts by weight: 22-30 parts of elastomer, 6-17 parts of thickener, 52-69 parts of organic solvent and 3-10 parts of auxiliary agent.
[0008] Preferably, the organic vehicle comprises the following raw materials in parts by weight: 26 parts of elastomer, 14 parts of thickener, 65 parts of organic solvent and 5 parts of first auxiliary agent.
[0009] Optionally, the glass transition temperature of the elastomer is 160°C-200°C.
[0010] Optionally, the molecular weight of the elastomer is 800-1000.
[0011] Optionally, the Mooney viscosity (ML) of the elastomer at 100°C is 1+4 ) is 20-56.
[0012] By adopting the above technical scheme, the Tg value, molecular weight and viscosity of the elastomer are selected so that it can have better compatibility and fluid state when compounded with the thickener, so that the prepared organic carrier has better fluidity, the conductive paste has better dispersibility, and agglomeration is avoided.
[0013] Optionally, the thickener is selected from at least one of polybutyl methacrylate, ethyl cellulose, cellulose acetate butyrate, carboxymethyl cellulose, hydroxyethyl cellulose, polyvinyl butyral, rosin resin, and polyvinyl pyrrolidone.
[0014] By adopting the above technical solution, the thickener and the elastomer are compounded to increase the viscosity of the organic carrier and the silver paste prepared therefrom, so that it does not flow, thereby helping to improve the printing performance of the subsequently prepared paste and improve the aspect ratio of the printed cutout lines.
[0015] Preferably, the thickener is a mixture of cellulose acetate butyrate and polyvinyl butyral in a weight ratio of 1:2-5.
[0016] The adoption of the above technical solution is helpful to further improve the printing performance of the solar cell conductive paste prepared using the organic carrier.
[0017] Optionally, the organic solvent is selected from at least one of ethylene glycol butyl ether, diethylene glycol butyl ether, dipropylene glycol methyl ether, tripropylene glycol methyl ether, ethylene glycol phenyl ether, propylene glycol phenyl ether, ethylene glycol butyl ether acetate, diethylene glycol butyl ether acetate, dipropylene glycol methyl ether acetate, ethylene glycol phenyl ether acetate, propylene glycol phenyl ether acetate, alcohol ester dodecahydrate, alcohol ester hexadecene, terpineol, terpineol and dimethyl adipate.
[0018] Preferably, the organic solvent is a mixture of diethylene glycol butyl ether and diethylene glycol butyl ether acetate in a weight ratio of 2-3:1.
[0019] By adopting the above technical solution, the mixed solvent can better dissolve the elastic resin, thickener and auxiliary agent in the organic carrier.
[0020] Optionally, the dispersant is selected from at least one of polyethylene wax, polyethylene glycol, vinyl bisstearamide, stearic acid monoglyceride and microcrystalline wax.
[0021] Optionally, the first surfactant includes but is not limited to commercially available surfactants, which may be saturated and unsaturated fatty acids (such as oleic acid), saturated and unsaturated fatty acid amides, coupling agents and polyoxyethylene surfactants (such as TritonX-100, Tween-20).
[0022] In a second aspect, the present application provides a method for preparing the above-mentioned organic carrier for solar cell conductive paste, comprising the following steps: The organic solvent, elastomer, thickener and auxiliary agent are added into a container, heated to 160-200° C. for 15-30 minutes, stirred while heating, and cooled to obtain the organic carrier for solar cell conductive paste.
[0023] In a third aspect, the present application provides the use of the above-mentioned organic carrier in a conductive paste for solar cells.
[0024] Optionally, the solar cell conductive paste comprises the following raw materials in weight percentage: 4.5-17wt% of organic vehicle, 60-92wt% of silver powder, 1-12wt% of glass powder, 0-7wt% of aluminum powder, and 1-5 wt% of a second surfactant.
[0025] In the present application, the shape of the silver powder used can be, for example, spherical, flaky or irregular, and the particle size range of the silver powder is 0.1~10μm; the shape of the aluminum powder used can be, for example, spherical, flaky or irregular, and the particle size range of the aluminum powder is 0.1~10μm; the particle size range of the glass powder used is 0.1~10μm.
[0026] Preferably, the solar cell conductive paste comprises the following raw materials in weight percentage: 12.5-15.5wt% of organic vehicle, 70-92wt% of silver powder, 5.2-7.5wt% of glass powder, 0-5wt% of aluminum powder, and 1-2wt% of a second surfactant.
[0027] Optionally, the second surfactant includes one or more of silicone oil, silicone oil derivatives, fatty alcohol polyoxyethylene ether, castor oil polyoxyethylene ether, sodium dodecylbenzene sulfonate, saturated and unsaturated fatty acid amides, and other polyoxyethylene surfactants.
[0028] The preparation method of the solar cell conductive paste comprises the following steps: (1) placing silver powder, aluminum powder, glass powder, an organic carrier and a second surfactant into a pre-dispersion container for pre-dispersion to obtain a pre-dispersed slurry; (2) Grinding and dispersing the pre-dispersed slurry obtained in step (1), and stirring to obtain the solar cell conductive slurry.
[0029] In summary, the present invention includes at least one of the following beneficial technical effects: 1. The organic carrier for the solar cell conductive paste in the present application adopts PaMS resin as the elastomer, which has high solubility in most organic solvents. Therefore, the prepared organic carrier has good stability in the conductive paste. At the same time, after adding PaMS resin to the organic solvent, the volatility of the organic solvent is greatly reduced, which effectively solves the problem of the durability of the paste printing, and can maintain a stable photoelectric conversion efficiency of the solar cell. In addition, there is no need to clean and wipe the screen due to clogging during the printing process, which causes the trouble of downtime.
[0030] 2. Adding PaMS resin as an elastomer to the organic solvent can greatly improve the initial viscosity and bonding strength of the organic carrier as a whole, so that during the printing process of the conductive paste, the continuous expansion of the fine grid printing due to low viscosity can be avoided, so that the prepared grid line has a higher aspect ratio, thereby improving the photoelectric conversion efficiency of solar cells. DETAILED DESCRIPTION
[0031] The present application is further described in detail below with reference to the embodiments.
[0032] The present application designs an organic carrier for solar cell conductive paste, characterized in that the organic carrier comprises the following raw materials in parts by weight: 1-30 parts of elastomer, 6-20 parts of thickener, 52-90 parts of organic solvent and 3-10 parts of auxiliary agent; the elastomer is PaMS resin; The auxiliary agent comprises a dispersant and a second surfactant in a weight ratio of 1-3:1-2.
[0033] The organic carrier for the solar cell conductive paste of the present application is prepared by the following method, comprising the following steps: The organic solvent, elastomer, thickener and auxiliary agent are added into a container, heated to 160-200° C. for 15-30 minutes, stirred while heating, and cooled to obtain the organic carrier for solar cell conductive paste.
[0034] The organic carrier for solar cell conductive paste of the present application can be used in solar cell conductive paste, and the solar cell conductive paste includes the following raw materials in percentage by weight: The solar cell conductive paste comprises 4.5-17 wt % of an organic carrier, 60-92 wt % of silver powder, 1-12 wt % of glass powder, 0-7 wt % of aluminum powder and 1-5 wt % of a second surfactant.
[0035] The technical problem to be solved by this application is that the existing solar cell conductive paste on the market usually chooses to reduce the concentration of resin (thickener) in order to increase the ink permeability, which easily leads to phase separation of the paste; or after long-term printing, the solvent evaporates and causes the paste to dry, which easily causes the grid break phenomenon. This application adopts PaMS resin as an elastomer in the organic carrier of solar cell conductive paste, and utilizes its high solubility in most organic solvents to make the prepared organic carrier have good stability in the conductive paste. At the same time, after adding PaMS resin to the organic solvent, the volatility of the organic solvent is greatly reduced, which effectively solves the problem of paste printing durability and can maintain a stable solar cell photoelectric conversion efficiency.
[0036] In this application, the sources of raw materials used in the examples are as follows: PaMS resin (poly alpha-methylstyrene resin), CAS number: 25014-31; Cellulose acetate butyrate, CAS number: 9004-36-8; Polyvinyl butyral, CAS No.: 63148-65-2; Diethylene glycol butyl ether, CAS number: 112-34-5; Diethylene glycol butyl ether acetate, CAS number: 124-17-4; Polyethylene glycol, CAS No.: 25322-68-3; Tween-20, CAS No.: 9005-64-5; Silver powder, CAS number: 7440-22-4; Aluminum powder, CAS number: 7439-89-6.
[0037] Examples 1-7 are organic carriers for solar cell conductive pastes made with different raw material ratios. The specific raw material ratios are shown in Table 1.
[0038] Table 1 Elastic body (kg) Thickener (kg) Dispersant (kg) First surfactant (kg) Organic solvent (kg) Example 1 1 11 3 1 84 Example 2 12 11 3 1 73 Example 3 24 11 3 1 61 Example 4 30 11 3 1 55 Example 5 1 6 2 1 90 Example 6 24 20 3 1 52 Example 7 24 11 6 4 55
[0039] The elastomer used in Examples 1-7 is PaMS resin; the glass transition temperature of the PaMS resin is 175°C, the average molecular weight of the PaMS resin is 850, and the Mooney viscosity (ML) of the elastomer of the PaMS resin at 100°C is 1+4 ) is 32.
[0040] The thickener used in Examples 1-7 is a mixture of cellulose acetate butyrate and polyvinyl butyral in a weight ratio of 1:3.
[0041] The organic solvent used in Examples 1-7 is a mixture of diethylene glycol butyl ether and diethylene glycol butyl ether acetate in a weight ratio of 2.5:1.
[0042] Wherein, the dispersant used in Examples 1-7 is polyethylene glycol, and the first surfactant used in Examples 1-7 is Tween-20.
[0043] The preparation process of Examples 1-7 is: The organic solvent, elastomer, thickener and additive are added into a container, heated to 180° C. for 25 min, stirred while heating, and cooled to room temperature to obtain an organic carrier for solar cell conductive paste.
[0044] Example 8 is based on Example 3, except that the glass transition temperature of the elastomer, namely PaMS resin, used in Example 8 is changed to 160°C.
[0045] Example 9 is based on Example 3, except that the glass transition temperature of the elastomer, i.e., PaMS resin, used in Example 9 is changed to 200°C.
[0046] Example 10 is based on Example 3, except that the average molecular weight of the elastomer, i.e., PaMS resin, used in Example 10 is changed to 1000.
[0047] Example 11 is based on Example 3, except that the average molecular weight of the elastomer, i.e., PaMS resin, used in Example 11 is changed to 1200.
[0048] Example 12 is based on Example 3, except that the thickener used in Example 12 is cellulose acetate butyrate.
[0049] Example 13 is based on Example 3, except that the thickener used in Example 13 is polyvinyl butyral.
[0050] Example 14 is based on Example 3, except that the thickener used in Example 14 is rosin resin.
[0051] Example 15 is based on Example 3, except that the thickener used in Example 15 is a mixture of cellulose acetate butyrate and polyvinyl butyral in a weight ratio of 1:1.
[0052] Example 16 is based on Example 3, except that the thickener used in Example 16 is a mixture of ethyl cellulose and polyvinyl butyral in a weight ratio of 1:3.
[0053] Example 17 is based on Example 3, except that the organic solvent used in Example 17 is diethylene glycol butyl ether.
[0054] Example 18 is based on Example 3, except that the organic solvent used in Example 18 is a mixture of diethylene glycol butyl ether and ethylene glycol butyl ether acetate in a weight ratio of 1:1.
[0055] Comparative Example 1 is based on Example 3, except that the elastomer used in Comparative Example 1 is replaced by polyamide wax THIXOTROL®MAX.
[0056] Comparative Example 2 is based on Example 3, except that the elastomer used in Comparative Example 2 is replaced by a mixture of polyamide wax THIXOTROL® MAX and PaMS in a weight ratio of 1:1.
[0057] Comparative Example 3 is based on Example 3, with the difference that the amount of PaMS resin in Comparative Example 3 is changed to 40 kg, and the amount of organic solvent is changed to 45 kg, that is, Comparative Example 3 includes 40 kg of PaMS resin, 11 kg of thickener, 3 kg of dispersant, 1 kg of first surfactant, and 45 kg of organic solvent.
[0058] Application Example 1-18 is a solar cell conductive paste prepared using an organic carrier for the solar cell conductive paste prepared in Example 1-18, wherein the solar cell conductive paste comprises the following raw materials in weight percentage: 12.5wt% organic carrier, 77.5wt% silver powder, 7wt% glass powder, 2wt% aluminum powder, and 1wt% second surfactant; wherein the second surfactant is fatty alcohol polyoxyethylene ether; the average particle size of silver powder, glass powder and aluminum powder is 10um.
[0059] The preparation process of Application Example 1-18 is as follows: The organic carrier, silver powder, aluminum powder, glass powder and the second surfactant are added to the pre-dispersion container, and then the pre-dispersion container is placed in a rotary dispersion device for pre-dispersion. The dispersed slurry is placed in a three-roll mill and rolled 6 times for grinding and dispersion. The ground and dispersed slurry is stirred once again with a stirrer to obtain a conductive slurry for solar cells.
[0060] Comparative Application Examples 1-3 are solar cell conductive pastes prepared using organic carriers for the solar cell conductive pastes prepared in Comparative Application Examples 1-3 of the embodiments, and other components are the same as those in Application Example 1.
[0061] Performance testing: 1. The solar cell conductive paste prepared in Application Examples 1-18 and Comparative Application Examples 1-3 was screen-printed and sintered with 10 N-type TOPCon silicon wafers, using a screen with an opening of 14um and a film thickness of 2.5um, to obtain solar cells with grid lines printed on them. The line height and line width of the grid lines were measured using a 3D optical microscope, and the number of broken grids on each piece was observed. The photoelectric conversion efficiency of the solar cells made of each conductive silver paste was tested under standard test conditions (STC) using a device model HSC1 / XSCM-9 produced by Shanghai Jiaotong University Heshuang Technology Co., Ltd. The test results are shown in Table 2.
[0062] 2. Storage stability test: The solar cell conductive pastes prepared in Application Examples 1-18 and Comparative Application Examples 1-3 were sealed and stored at 25°C. After three months, the viscosity change of the lower layer of the conductive paste was detected, and whether the silver powder was precipitated was observed. The test results are shown in Table 3.
[0063] 3. Visually observe the appearance of the solar cell conductive pastes prepared in Application Examples 1-18 and Comparative Application Examples 1-3 after screen printing to observe whether the surface is smooth, whether there are bubbles, and the uniformity of screen printing. The measurement results are shown in Table 3.
[0064] Table 2 Average line width (um) Average line height (um) Aspect ratio (%) Number of gates per fragment (average) Fixed position broken grid number (average value) Photoelectric conversion efficiency (%) Application Example 1 28.11 11.86 42.19 4.6 4.2 23.78 Application Example 2 26.94 12.25 45.47 4.2 4 24.55 Application Example 3 24.18 12.43 51.4 2.4 1.6 26.32 Application Example 4 25.24 11.93 47.26 3.9 3.3 24.83 Application Example 5 28.85 11.85 41.08 4.9 4.4 23.42 Application Example 6 24.5 12.22 49.8 2.8 1.9 26.09 Application Example 7 23.25 11.59 48.86 3.5 2.6 25.59 Application Example 8 25.07 11.99 47.82 4.2 3.5 25.33 Application Example 9 24.18 11.65 48.19 3.7 3.1 25.51 Application Example 10 24.26 11.73 48.35 3.6 3 25.59 Application Example 11 26.17 12.11 46.28 4 3.3 24.83 Application Example 12 24.85 11.28 45.39 4.2 3.5 24.38 Application Example 13 24.42 11.62 47.58 4 3.5 24.96 Application Example 14 24.21 11.76 48.58 3.6 3 25.64 Application Example 15 24.06 11.57 48.08 3.8 3.3 25.42 Application Example 16 23.47 11.18 47.64 4.1 3.6 25.13 Application Example 17 23.57 11.35 48.15 3.7 3.2 25.47 Application Example 18 24.48 12.04 49.18 3.2 3.6 25.89 Comparative application example 1 30.08 10.93 36.34 17.7 9.4 21.21 Comparative Application Example 2 28.8 11.02 38.26 13.4 7.6 21.45 Comparative Application Example 3 27.01 10.76 39.83 10.5 6.1 22.37 Table 3 Slurry appearance Storage stability Application Example 1 The surface is smooth with a small amount of bubbles and is evenly printed. No subsidence for three months Application Example 2 The surface is smooth without bubbles and even after printing No subsidence for three months Application Example 3 The surface is smooth without bubbles and even after printing No subsidence for three months Application Example 4 The surface is smooth without bubbles and even after printing No subsidence for three months Application Example 5 The surface is smooth with a small amount of bubbles and is evenly printed. No subsidence for three months Application Example 6 The surface is smooth without bubbles and even after printing No subsidence for three months Application Example 7 The surface is smooth without bubbles and even after printing No subsidence for three months Application Example 8 The surface is smooth with a small amount of bubbles and is evenly printed. No subsidence for three months Application Example 9 The surface is smooth without bubbles and even after printing No subsidence for three months Application Example 10 The surface is smooth without bubbles and even after printing No subsidence for three months Application Example 11 The surface is smooth without bubbles and even after printing No subsidence for three months Application Example 12 The surface is smooth without bubbles and even after printing No subsidence for three months Application Example 13 The surface is smooth without bubbles and even after printing No subsidence for three months Application Example 14 The surface is smooth without bubbles and even after printing No subsidence for three months Application Example 15 The surface is smooth without bubbles and even after printing No subsidence for three months Application Example 16 The surface is smooth without bubbles and even after printing No subsidence for three months Application Example 17 The surface is smooth without bubbles and even after printing No subsidence for three months Application Example 18 The surface is smooth without bubbles and even after printing No subsidence for three months Comparative application example 1 The surface is not smooth and has bubbles Three months of slurry bottom layer agglomeration Comparative Application Example 2 The surface is not smooth and has bubbles Three months of slurry bottom layer agglomeration Comparative Application Example 3 The surface is smooth without bubbles and even after printing No subsidence for three months By analyzing the data in Table 2 and Table 3, Application Examples 1-7 are compared with Comparative Application Examples 1-2. After the present application uses PaMS resin as the elastomer of the organic carrier, the printing performance of the conductive silver paste can be significantly improved. The number of broken grids in Application Examples 1-7 is significantly less than that in Comparative Application Examples 1-2, and the average line width in Example 1-7 is also narrower, so that the photoelectric conversion efficiency of the solar cell of Example 1-7 is significantly higher. The organic carrier in the conductive paste in Application Examples 1-7 has better bonding with the powder, the conductive paste is not easy to produce phase separation, has good storage stability, and has better surface smoothness and uniformity after screen printing, and no bubbles will appear.
[0065] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.
Claims
1. An organic carrier for a solar cell conductive paste, characterized in that: The organic carrier comprises the following raw materials in parts by weight: 1-30 parts of elastomer, 6-20 parts of thickener, 52-90 parts of organic solvent and 3-10 parts of auxiliary agent; The elastomer is PaMS resin; The auxiliary agent comprises a dispersant and a second surfactant in a weight ratio of 1-3:1-2.
2. The organic carrier according to claim 1, characterized in that The glass transition temperature of the elastomer is 160°C-200°C.
3. The organic carrier according to claim 1, characterized in that The molecular weight of the elastomer is 800-1000.
4. The organic carrier according to claim 1, characterized in that The Mooney viscosity (ML) of the elastomer at 100°C 1+4 ) is 20-56.
5. The organic carrier according to claim 1, characterized in that The thickener is selected from at least one of polybutyl methacrylate, ethyl cellulose, cellulose acetate butyrate, carboxymethyl cellulose, hydroxyethyl cellulose, polyvinyl butyral, rosin resin, and polyvinyl pyrrolidone.
6. The organic carrier according to claim 1, characterized in that The organic solvent is selected from at least one of ethylene glycol butyl ether, diethylene glycol butyl ether, dipropylene glycol methyl ether, tripropylene glycol methyl ether, ethylene glycol phenyl ether, propylene glycol phenyl ether, ethylene glycol butyl ether acetate, diethylene glycol butyl ether acetate, dipropylene glycol methyl ether acetate, ethylene glycol phenyl ether acetate, propylene glycol phenyl ether acetate, alcohol ester dodecahydrate, alcohol ester hexahydrate, terpineol, terpineol and dimethyl adipate.
7. The organic carrier according to claim 1, characterized in that The dispersant is selected from at least one of polyethylene wax, polyethylene glycol, vinyl bisstearamide, stearic acid monoglyceride and microcrystalline wax.
8. A method for preparing an organic carrier according to any one of claims 1 to 7, characterized in that: The following steps are involved: The organic solvent, elastomer, thickener and auxiliary agent are added into a container, heated to 160-200° C. for 15-30 minutes, stirred while heating, and cooled to obtain the organic carrier for solar cell conductive paste.
9. Use of the organic carrier according to any one of claims 1 to 7 in a conductive paste for solar cells.
10. The use of the organic carrier for solar cell conductive paste according to claim 9 in solar cell conductive paste, characterized in that: The solar cell conductive paste comprises the following raw materials in weight percentage: 4.5-17 wt % of the organic carrier according to any one of claims 1 to 7, 60-92 wt % of silver powder, 1-12 wt % of glass powder, 0-7 wt % of aluminum powder, and 1-5 wt % of a second surfactant.
Citation Information
Patent Citations
Preparation method of flexible poly-alpha-methylstyrene resin
CN114230705A
Low-VOCs environment-friendly PERC back silver and preparation method thereof
CN115036055A
Organic carrier containing poly (styrene-co-alpha-methylstyrene) resin and application
CN117777612A
Organic carrier for conductive silver paste as well as preparation method and application of organic carrier
CN117903624A
Conductive paste composite for screen printing and screen printing method using the same
KR1020100020564A
Cited By
Organic carrier for N-type TOPCon back fine grid slurry and application thereof
CN121182275A
N-type topcon back surface fine grid paste organic carrier and application thereof
CN121182275B