Novel metal-organic frameworks and their use for encapsulating fluorescent dyes

Novel MOFs with tetradentate tetraphenylanthraquinone units encapsulate fluorescent dyes, suppressing their fluorescence until release, addressing the lack of characterization in host-guest complexes and enabling efficient fluorescence-based applications.

DE112019007923B4Active Publication Date: 2024-10-17LATVIAN INST OF ORGANIC SYNTHESIS +37
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE112019007923
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-11-29
Publication Date
2024-10-17
Estimated Expiration
2039-11-29

AI Technical Summary

Technical Problem

There is a lack of research and characterization of host-guest complexes formed when fluorescent molecules are adsorbed in the pores of metal-organic frameworks (MOFs), particularly in terms of solid-state fluorescence measurements, which are crucial for understanding the interaction between the host MOF lattice and guest molecules.

Method used

Development of novel organometallic framework materials with tetradentate tetraphenylanthraquinone connecting units, specifically Cu-Anth-MOF and Ni-Anth-MOF, which encapsulate fluorescent dyes like methylene blue (MB), suppressing their fluorescence when inside the MOF pores but allowing it to be restored upon extraction.

Benefits of technology

The new MOFs effectively suppress the fluorescence of encapsulated dyes within their pores, providing a reversible interaction that maintains fluorescence intensity upon release, facilitating efficient characterization and potential applications in fluorescence-based sensing and pollutant removal.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

Microporous metal-organic framework (MOF) comprising tetradentatetetraphenylanthraquinone linkage units and at least one secondary structural unit (SBU), wherein the secondary structural unit comprises only metal ions or metal ions and oxygen atoms with an O / metal ratio > 0.5.
Need to check novelty before this filing date? Find Prior Art

Description

Field of the invention

[0001] The present invention relates to novel microporous metal-organic frameworks (MOFs), novel host-guest Complexes of the mentioned MOFs with dye molecules, as well as their fluorescence properties. State of the art

[0002] The synthesis and application of microporous metal-organic frameworks (MOFs) is an area of materials science, which has attracted much attention in recent years. Compared to traditional porous Materials such as silica or zeolites, MOFs have open channels with a much wider variety of pore sizes, Volume of internal cavities and type of pore surface. Compared to other types of porous materials, MOFs have one of the highest relative surface areas. A large number of components combined with a flexible design makes MOFs a versatile platform for a wide range of applications, including gas storage or separation, Catalysis, sensing, drug encapsulation and many others (Cui, Y; Li, B.; He, H.; Zhou, W.; Chen, B.; Qian, G. Acc. Chem. Res. 2016, 49(3), 483-493).

[0003] MOFs are coordination network compounds consisting of nodes containing metal-containing inorganic groups which are linked to polydentate organic ligands. The ligand is bound by coordinating functional groups such as carboxylates and amines are connected to the node. Together they form one-, two-, or three-dimensional lattices, which often have a crystalline structure. In many cases they contain pores as channels and cavities of various Diameters that may contain solvents or other organic molecules. In many cases, when the size of a molecule is comparable to the diameter of a channel, such molecules can be introduced into pores or Diffusion can be extracted from them. (Cirujano, FG; Llabrés i Xamena, FX Metal Organic Frameworks as Nanoreactors and Wirt Matrices for Encapsulation. In Organic Nanoreactors; Elsevier, 2016; pp 305-340).

[0004] The encapsulation of small organic molecules in MOFs and the formation of host-guest complexes involves the Interaction of guests with the walls of channels and cavities where they are contained. Different types of Interactions between host and guest include sorption, coordination, and chemical reactions. Understanding the details the interaction between host MOF lattice and organic guest molecules is a prerequisite for the creation new composite materials with useful functions. While coordination and chemical reaction often have well-defined host generate guest complexes that can be characterized by a number of methods, sorption is inherently reversible and produces much weaker host-guest complexes. In one aspect, it is advantageous to use fluorescent molecules as guests and evaluate their interaction with hosts by changing their fluorescence properties. (Karmakar, A.; Samanta, P.; Desai, AV; Ghosh, SK Acc. Chem. Res. 2017, 50(10), 2457-2469).

[0005] The sorption of various ions and molecules from solution by porous MOFs is described in several publications described (Gao, Q.; Xu, J.; Bu, X.-H. Coordination Chemistry Reviews 2019, 378, 17-31). This effect is important for the selective Removal of specific pollutants from water streams of interest. (Cui, Z.; Zhang, X.; Liu, S.; Zhou, L.; Li, W.; Zhang, J. Inorg. Chem. 2018, 57(18), 11463-11473; Guo, H.; Sun, Y.; Zhang, F.; Ma, R.; Wang, F.; Sun, S.; Guo, X.; Liu, S.; Zhou, T. Inorganic Chemistry Communications 2019, 107, 107492) or for their degradation (Li, H.-P.; Dou, Z.; Chen, S.-Q.; Hu, M.; Li, S.; Sun, H.-M.; Jiang, Y.; Zhai, Q.-G. Inorg. Chem. 2019, 58(16), 11220-11230; Qiao, X.; Ge, Y.; Li, Y.; Niu, Y.; Wu, B. ACS Omega 2019, 4(7), 12402-12409). The efficiency of the sorption process is determined by measurements of ultraviolet-visible spectra in solution. However, there is a lack of research and characterization of host-guest complexes that form when a molecule is adsorbed in the MOF pores. It would be particularly interesting to study the properties of guest molecules which have their own emission spectra. There are no literature data for solid-state fluorescence measurements of fluorescent molecules encapsulated in the MOF pores. Detailed description

[0006] Disclosed herein are novel metal-organic framework materials with tetradentate tetraphenylanthraquinone connecting units and one or more secondary structural units.

[0007] In one embodiment, a secondary structural unit comprises metal ions selected from Cu or Ni. In a In another embodiment, a secondary structural unit consists of the same metal ions (Cu or Ni) and oxygen atoms with an O / metal ratio >0.5, preferably >0.6. In one aspect, a schematic Representation of Cu-Anth-MOF is shown in Fig. 1. In another aspect, a schematic representation of Ni-Anth- MOF shown in Fig. 2.

[0008] In one embodiment, the present disclosure is directed to the preparation of a novel MOF material, which may consist of a compound represented by the formula (Formula 1): MLA *B *nSolv Formula 1 where wxyz M is selected from: Cu, Ni; L represents tetradentate tetraphenylanthraquinone ligands of formula L1; A independently represents a ligand selected - - - - from (OH), HO, alkyl-(SO), aryl-(SO), (NO), halide anion; 2 3 3 2 - - - - B independently represents a ligand selected from (OH) , HO, alkyl-(SO ) , aryl-(SO ) , (NO ) , halide anion; 2 3 3 2 Solv stands for any solvent that can be coordinated with the MOF metal ions. It can be a Solvent involved in MOF formation, selected from the list: water, dimethylformamide, Diethyl formamide, dimethyl acetamide, diethyl acetamide, dimethyl sulfoxide.

[0009] w stands for the number of M atoms in the structural unit; x stands for the number of ligands L in the structural units; y stands for the number of ligands A in the structural unit; z stands for the number of ligands B in the structural unit; n stands for the average number of solvent molecules ´´Solv´´ that interact with the metal centers M per structural unit are coordinated in the MOF material.

[0010] Preferably, the ratio y / x is ≥1.0, particularly preferably ≥1.5.

[0011] Preferably, the ratio z / x is in the range ≥0 and ≤3.

[0012] Ligand L1 was synthesized and used as an organic linker as described in the Examples section. There are No literature methods for the preparation of the ligand of the L1 formula. According to the present invention, A new and efficient synthesis method has been developed, as shown in Scheme 1. A short four-step sequence begins with a cross-coupling step, followed by the oxidation of sulfur, which produces substituted Thiophene 1,1-dioxide 4. It was pleasing that substance 4 is reactive in Diels-Alder cycloaddition and a correspondingly tetrasubstituted anthraquinone 6. For the first time it was shown that a tetrasubstituted anthraquinone 6, substituted at positions 3 and 4, Thiophene-1,1-dioxide can undergo such a transformation by phenyls with an electron-withdrawing group. Finally, hydrolysis of ester 6 provided the ligand L1.

[0013] In one embodiment, Cu(NO ) 2.5H O salt was selected to form a metal node for producing Cu- 3 2 2 Anth-MOF. In another embodiment, Ni(NO ) 6H O salt was selected to form a metal node 3 2 2 for the production of Ni-Anth-MOF.

[0014] The experimental conditions for the preparation of Cu-Anth-MOF and Ni-Anth-MOF were optimized so that the reaction of a metal salt and the organic ligand L1 single crystals could be formed. Preferably, the Crystal topology with a monoclinic crystal system and the P21 / c or P2 / m space group or a subgroup in Cell parameters and other data for Cu-Anth-MOF are shown in Table 1. Cell parameters and Other data for Ni-Anth-MOF are shown in Table 2. Both Cu-Anth-MOF and Ni-Anth-MOF showed a excellent robustness during insulation and storage. Together with a permanent porosity of the manufactured MOFs are ideal candidates for the production of host-guest complexes with organic molecules.

[0015] In one aspect, the method for producing Cu-Anth-MOF comprises the solvent used for producing is used, a mixture of water and an organic solvent in the ratio organic solvent / water from 90:10 to 65:35, expressed as volume percent of the organic solvent. Organic solvent is preferably selected from the list: dimethylformamide, diethylformamide, dimethylacetamide, diethylacetamide, Dimethyl sulfoxide; preferably dimethyl carboxylic acid amide; preferably dimethylformamide.

[0016] In another aspect, the method for producing Ni-Anth-MOF comprises the solvent used for used in the preparation, a mixture of water, an organic solvent 1 and an organic Solvent 2. The water content in volume percent is preferably less than 50 vol.%, preferably less than 30%. The ratio of organic solvent 1 / organic solvent 2 is preferably 50:50, preferably 60:40. The organic solvent 1 is preferably selected from the list: dioxane, tetrahydrofuran, preferably dioxane. Organic solvent 2 is preferably selected from the list: dimethylformamide, Diethylformamide, dimethylacetamide, diethylacetamide, dimethyl sulfoxide; preferably carboxylic acid diethylamide; preferably diethylformamide.

[0017] According to the current disclosure, MOFs based on the tetraphenylanthraquinone ligand of formula L1 can be in a form in which the coordination polymer is ordered, preferably in single-crystalline form. The structure of the MOFs disclosed therein was confirmed by single-crystal X-ray diffraction.

[0018] In one embodiment, a spatial arrangement of the Cu-Anth-MOF elements is exemplified by Fig. 3 which shows a single-crystal X-ray structure of Cu-Anth-MOF.

[0019] In a further embodiment, a spatial arrangement of the Ni-Anth-MOF elements is exemplified by Fig. 4 illustrates a single-crystal X-ray structure of Ni-Anth-MOF.

[0020] In another example, the crystalline nature of the material produced is confirmed by powder X-ray diffraction confirmed, as illustrated in Fig. 5 for Cu-Anth-MOF.

[0021] In another example, the crystalline nature of the material produced is confirmed by powder X-ray diffraction confirmed, as illustrated in Fig. 6 for Ni-Anth-MOF.

[0022] In one embodiment, Cu-Anth-MOF and Ni-Anth-MOF are stable in water.

[0023] Preferably, the three-dimensional structure of Cu-Anth-MOF comprises channels with an inner diameter between 7.9 and 10.2 Å and are accessible through pores with diameters of 7.9 and 10.2 Å. Advantageously, The three-dimensional structure of Ni-Anth-MOF channels with an inner diameter between 6.4 and 8.5 Å and are characterized by Pores with diameters of 6.4 to 8.5 Å are accessible.

[0024] The present invention relates to a guest encapsulated in a host and a method for encapsulation. The host consists of a MOF and the guest consists of a molecule that is smaller than the pore size of the MOF. In In one embodiment, a dye called methylene blue (MB) is used as a guest. The molecular representation of MB is shown in Fig. 9. The size of the MB molecule was defined as a rectangular box with approximate dimensions of 17.0 x 7.6 x 3.3 Å. The fluorescence of the solution of MB in water at a concentration c=1 µmol / L and a pH of 7 with excitation at 290 nm is shown in Fig. 11. This emission spectrum is characterized by a strong Peak in a range of 650-750 nm with a signal intensity of more than 100,000 arbitrary units.

[0025] In one aspect, MOF materials disclosed herein, in particular Cu-Anth-MOF or Ni-Anth-MOF, were prepared by Fluorescence spectroscopy. The spectrum of the solid-state fluorescence sion properties of Cu-Anth-MOF is shown in Fig. 12. The spectrum of Solid-state fluorescence emission properties of Ni-Anth-MOF are shown in Fig. 14. Both spectra are characterized by a very low fluorescence intensity in the range of 650-750 nm. In particular, signals in this range lower than 500 arbitrary units.

[0026] In one embodiment, the present invention provides a process for preparing a host-guest complex Scheme 200 of the preparation of host-guest complexes of Cu-Anth-MOF and Ni-Anth-MOF with MB and measurement of their Fluorescence properties are shown in Fig. 10. In step 205, the method may include mixing a MOF with water In step 210, a solution of a guest in the same solvent is prepared. In step 215, the components obtained in steps 205 and 210 are mixed and without stirring according to the procedure described in the current Incubated in the example given in the disclosure.

[0027] In one embodiment, when MB is used as guest and Cu-Anth-MOF is used as host, a new host-guest Complex is prepared in step 215. The fluorescence spectrum of said complex is determined in step 220 measured.

[0028] A graph showing the solid-state emission properties of a host-guest complex consisting of MB containing encapsulated in Cu-Anth-MOF (excited at 290 nm) is shown in Fig. 13. A graph showing the Solid-state emission properties of a host-guest complex consisting of MB embedded in Ni-Anth-MOF (excited at 290 nm) is shown in Fig. 15 for Ni-Anth-MOF. Both Fig. 13 and Fig. 15 show that the Fluorescence intensity in the range 650-750 nm is below 2000 arbitrary units, which means that MB, which is present in the pores of Cu-Anth-MOF or Ni-Anth-MOF, exhibits no fluorescence. These data illustrate the unique property of the new MOFs, as described. When a dye molecule is trapped in the pores of the MOFs encapsulated, its fluorescence is completely suppressed.

[0029] In step 225, a digestion of a host-guest complex with encapsulated MB in aq. HCl solution is carried out. Under these conditions, a complete decomposition of the polymeric structure of the MOF to starting ligands and Metal salt instead. MB is released from the solution. In step 230, the solution is neutralized to pH 7 after digestion. and their fluorescence was measured directly from the aqueous solution. In one aspect, as shown in Fig. 16 for Cu-Anth-MOF, the fluorescence of MB is restored after digestion and its emission spectrum contains a strong signal in the Range of 650-750 nm with an intensity of more than 30,000 arbitrary units. In another aspect, as in As shown in Fig. 17 for Ni-Anth-MOF, the fluorescence of MB is restored after digestion and its Emission spectrum contains a strong signal in the range of 650-750 nm with an intensity of more than 15000 arbitrary units. The presented data show that interactions in the host-guest complex of the Dye molecules in the pores of the new MOFs suppress dye fluorescence with excellent efficiency. At the same time, the interactions mentioned are reversible and as soon as the dye is extracted from the pores, its fluorescence restored. Examples

[0030] All reagents were purchased from commercial sources and used without further purification. Emission fluorescence spectra were recorded at room temperature using an Edinburgh Instruments FS5 spectrofluorometer recorded.

[0031] Scheme 1 shows the reaction pathway for the preparation of the ligand of formula L1 from the starting materials. 3,4-Dibromothiophene 1 was arylated by boronic acid 2 in a Suzuki-Miyaura cross-coupling reaction. The resulting ® Diarylthiophene 3 was oxidized by oxone to the corresponding thiophene-1,1-dioxide 4. A double Diels-Alder Reaction of thiophene-1,1-dioxide 4 and 1,4-benzoquinone 5 yielded tetrasubstituted anthraquinone 6. Finally, the Hydrolysis of the ethyl ester groups in 6 yields the target ligand L1. Abbreviations AcOH acetic acid CDCl Chloroform-d 3 Cu(NO ) ·2.5HO Copper nitrate hemi (pentahydrate) 3 2 2 DCM Dichloromethane DEF N,N'-Diethylformamide DMSO dimethyl sulfoxide EtOAc Ethyl acetate EtOH ethanol HCl hydrochloric acid KOH potassium hydroxide NaCO Sodium carbonate 2 3 Well SO Sodium thiosulfate 2 2 3 NaHCO Sodium bicarbonate 3 Ni(NO) ·6HO Nickel(II) nitrate hexahydrate 3 2 2 Pd(OAc) Palladium(II) acetate 2 PPh Triphenylphosphin 3

[0032] Preparation of diethyl 4,4'-(thiophene-3,4-diyl)dibenzoate 3. In a 100 ml vial with Screw cap was added under argon flow and stirring (4-(ethoxycarbonyl)phenyl)-boronic acid 2 (7.0 g, 36.21 mmol, 4.0 equiv.), solid Na CO (3.8 g, 36.21 mmol, 4.0 equiv.), Pd(OAc) (0.2 g, 0.91 mmol, 10 mol%) and PPh3 (0.6 g, 2.26 mmol, 2 3 2 25 mol%) was successfully added, followed by 3,4-dibromothiophene 1 (1.0 ml, 2.19 g, 9.05 mmol) and the mixture was further purged with argon for 15 min at RT. In the meantime, dry toluene and water were separately Degassing by connecting the vacuum line and then flushing with argon through a rubber septum This measure was min repeated at least 3 times. Finally, degassed toluene (45 mL) and water (15 mL) were added to the reaction vessel which was then sealed and heated to 100-110 °C for 24 h. It was cooled to RT. The The reaction mixture was diluted with EtOAc (100 mL), the aq. phase was separated and further washed with EtOAc (3 × 30 mL) The organic phases were combined, washed with water (30 ml) and brine (50 ml) and concentrated to 35 g of silica. The crude compound was purified by column flash chromatography using EtOAc 1 / hexane gradient from 0 to 30%. Yield of 3: 2.5 g (6.6 mmol, 72%), as a white solid. H-NMR (400 13 MHz, CDCl ) δ: 7.94 (d, 2H), 7.41 (s, 2H), 7.23 (d, 2H), 4.37 (q, 2H), 1.39 (t, 3H); C-NMR (100 MHz, CDCl ) δ: 3 3 + 166.6, 140.9, 140.8, 129.7, 129.3, 129.0, 125.5, 61.1, 14.5; GC-MS (EI): m / z 380 [M].

[0033] Preparation of diethyl 4,4'-(1,1-dioxidothiophene-3,4-diyl)dibenzoate 4. A solution of thiophene diester 3 (5.5 g, 14.5 mmol) in DCM / acetone / water (2:1:2) solvent mixture (500 ml total volume) was cooled with ice water and vigorous stirring into a 1000 ml round-bottom flask. Next, NaHCO (59 g, 690 mmol, 45 equiv.) 3 ® added in one portion, followed by Oxone (96 g, 146 mmol, 10.0 equiv.) in small portions of 5-7 g each within 5 h, and the reaction mixture was left at RT overnight. The mixture was then washed with water (400 mL), the organic phase was separated, and the aq. phase was further extracted with DCM (5 × 100 mL). organic phases were combined, with 10% aq. solution of Na SO (2×50 mL), water (50 mL) and brine (50 2 2 3 mL) and evaporated to 35 g of silica. The crude compound was purified by column flash chromatography and eluted with a MeOH / DCM gradient from 0 to 5%. Yield of 4: 2.7 g (6.5 mmol, 45%), as a light yellow 1 Foam that solidifies when standing. H-NMR (300 MHz, CDCl ) δ: 7.97 (d, 2H), 7.12 (d, 2H), 6.73 (s, 2H), 4.38 (q, 2H), 3 + + 1.39 (t, 3H); LC-MS (ES): m / z 413 [M+H].

[0034] Preparation of tetraethyl 4,4',4'',4'''-(9,10-dioxo-9,10-dihydroanthracene-2,3,6,7-tetrayl)tetrabenzoate 6. In a A solution of thiophene-1,1-dioxide was added to a 100 ml screw-capped vial under argon flow and stirring. 4 (2.0 g, 4.85 mmol) was introduced into glacial acetic acid (25 mL), followed by 1,4-benzoquinone 5 (0.3 g, 2.78 mmol, 0.5 equiv.). The vessel was then sealed and heated to 110-120 °C for 48 h. The reaction mixture was then cooled to RT cooled and poured into water (250 ml) and extracted with DCM (5×50 mL), the organic phases were combined, washed with saturated aq. NaHCO (2×50 ml), water (50 ml) and brine (50 ml) and evaporated to 35 g of silica 3 evaporated. The crude compound was purified by column flash chromatography and chromatographed with an EtOAc / hexane 1 Eluted with gradients from 0 to 30%. Yield of 6: 1.2 g (1.5 mmol, 31%) as a light yellow solid. H NMR (400 MHz, CDCl ) 3 13 δ: 8.42 (s, 4H), 7.99 (d, 8H), 7.31 (d, 8H), 4.41 (q, 8H), 1.42 (t, 12H); C-NMR (100 MHz, CDCl ) δ: 182.3, 166.2, 3 145.7, 143.7, 132.9, 130.1, 129.8, 129.8, 61.3, 14.5.

[0035] Preparation of 4,4',4'',4'''-(9,10-dioxo-9,10-dihydroanthracene-2, 3, 6, 7-tetrayl) tetrabenzoic acid L1. In a 25- A solution of ester 6 (350 mg, 0.44 mmol) in EtOH was added to a 10 ml screw-capped vial with stirring. (5.0 ml) followed by KOH (0.15 g, 2.65 mmol, 6.0 equiv.). The container was then sealed and stored for 24 h at The reaction was heated to 100-110 °C, which indicated complete conversion. The mixture was cooled to RT and added to water (50 ml). poured and acidified with 1N aq. HCl to pH 3, precipitated solids were filtered off, with water (5 × 10 ml) and dried under reduced pressure to constant weight. Yield of L1: 260 mg (0.37 mmol, 1 84%), as a light yellow solid. H-NMR (400 MHz, DMSO-d ) δ: 13.08 (br.s, 4H), 8.27 (s, 4H), 7.90 (d, 8H), 7.39 (d, 8H), 6 - - LC-MS (ES ): m / z 687 [MH] .

[0036] Synthesis of Cu-Anth-MOF. A mixture of L1 (10 mg, 0.015 mmol) and Cu(NO ) 2.5H O (14 mg, 0.060 mmol) 3 2 2 was dissolved in a solvent mixture of DEF (1.0 ml) and water (0.1 ml). After addition of 10 µL 6 M aq. HCl The vial was sealed and heated at 90 °C for 24 hours. After cooling to room temperature Green crystals formed. They were collected by filtration and dried at room temperature. Yield of Cu-Anth-MOF: 8 mg (65%).

[0037] Synthesis of Ni-Anth-MOF. A mixture of L1 (17 mg, 0.025 mmol) and Ni(NO ) 6H O (22 mg, 0.058 mmol) 3 2 2 was dissolved in a solvent mixture of DEF (1.0 ml), water (0.5 ml) and dioxane (1.5 ml). After addition of 30 µL 1M aq. HCl, the vial was sealed and heated at 100 °C for 4 days. After cooling to Greenish crystals formed at room temperature. They were collected by filtration and dried at room temperature. Yield of Ni-Anth-MOF: 10 mg (51%).

[0038] Single-crystal XRD and crystal structure of Cu-Anth-MOF. SCXRD data of Cu-Anth-MOF were collected using an XtaLAB Synergy, Dualflex, HyPix, diffractometer with Cu Kα (λ = 1.54178 Å) radiation. The data indexing, - integration and reduction was performed with the software CrysAlis PRO 1.171.40.35a (Rigaku OD, 2018). Absorption correction was performed using the multi-scan method. The structure was analyzed with direct methods (SHELXT 2014 / 4, Sheldrick, 2014) and refined with SHELXL2017 / 1 (Sheldrick, 2017) 2 (Full least squares matrix on F ). Crystal data and refinement conditions are shown in Table 1. All Attempts to refine peaks of the residual electron density of disordered solvent molecules were unsuccessful. The data were augmented to include the contribution of a disordered solvent density using the SQUEEZE method, as Implemented in PLATON, corrected. The total solvent-capable void volume is 3141 Å. Table 1. Crystal data and structure refinement conditions for Cu-Anth-MOF CH Cu O Chemical formula 42 24 2 12 M 847.69 r Monoclinic, P2 / c Crystal system, space group 1 Temperature (K) 170 a, b, c (Å) 18.7415 (2), 23.1192 (2), 14.4500 (1) β (°) 106.064 (1) 3 6016.55 (10) V (Å ) Z4 Radiation type Cu Kα -1 1.22 µ (mm ) Crystal size (mm) 0.08 × 0.06 × 0.05 Diffractometers XtaLAB Synergy, Dualflex, HyPix Absorption correction multi-scan T, T 0.741, 1.000 min max Number of measured, independent and observed [I > 2σ(I)] reflections 58543, 12227, 10165 R 0.055 int -1 (sin θ / λ) (Å ) 0.631 max 2 2 2 0.059, 0.182, 1.04 R[F > 2σ(F )], wR(F ), S Number of reflections 12227 Number of parameters 507 H-atom treatment H-atom parameters restricted -3 &Dgr;&rgr; , &Dgr;&rgr; (e Å ) 0.98, -0.56 max min

[0039] Single-crystal XRD and crystal structure of Ni-Anth-MOF. SCXRD data of Ni-Anth-MOF were collected using an XtaLAB Synergy, Dualflex, HyPix, diffractometer with Cu Kα (λ = 1.54178 Å) radiation. The data indexing, - integration and reduction was performed using the software CrysAlis PRO 1.171.40.35a (Rigaku OD, 2018). Absorption correction was performed using the multi-scan method. The structure was determined using direct methods (SHELXT 2 2014 / 4, Sheldrick, 2014) and refined with SHELXL2017 / 1 (Sheldrick, 2017) (full least squares matrix on F ). Crystal data and refinement conditions are shown in Table 2. All experiments, peaks of the residual electron density Attempts to refine the data using disordered solvent molecules were unsuccessful. Therefore, the data were extended to include the contribution of disordered solvent density using the SQUEEZE method as implemented in PLATON. The total solvent-capable void volume is 1423 Å. Table 2. Crystal data and Structure refinement conditions for Ni-Anth-MOF CH NiO Chemical formula 22 12 0.75 6 M 416.35 r Crystal system, space group monoclinic, P2 / m 11.7483 (2), 20.6778 (3), 13.1192 a, b, c (Å) (2) β (°) 113.923 (2) 3 2913.24 (9) V (Å ) Z4 Radiation type Cu Kα -1 1.01 µ (mm ) Crystal size (mm) 0.10 × 0.08 × 0.05 Diffractometers XtaLAB Synergy, Dualflex, HyPix Absorption correction multi-scan T , T 0.475, 1.000 min max Number of measured, independent and observed [I > 2σ(I)] 28104, 6144, 5300 reflections R 0.078 int -1 (sin θ / λ) (Å ) 0.630 max 2 2 2 0.091, 0.290, 1.14 R[F > 2σ(F )], wR(F ), S Number of reflections 6144 Number of parameters 272 H-atom treatment H-atom parameters restricted -3 &Dgr;&rgr; , &Dgr;&rgr; (e Å ) 1.28, -0.58 max min

[0040] The powder X-ray diffraction patterns for Cu-Anth-MOF and Ni-Anth-MOF were measured using a Bruker D8 Advance (Bruker AXS GmbH, Karlsruhe, Germany) diffractometer equipped with a LynxEye position detector which uses copper radiation (CuK ) at a wavelength of 1.54180 Å. Tube voltage and - α current were set to 40 kV and 40 mA, respectively. The divergence slot was set to 1.0 mm and the anti-scatter slot to 8.0 mm. The PXRD patterns were scanned at a speed of 0.25 s / 0.02° on the 2θ scale from 3 to 35°, see Fig. 5 for PXRD of Cu-Anth-MOF, see Fig. 6 for PXRD of Ni-Anth-MOF.

[0041] High-resolution dynamic thermal gravimetric analysis (TGA). Thermogravimetric analysis (TGA) was performed using a TGA / DSC2 (Mettler Toledo). Open 100 µL aluminum crucibles were used. Heating -1 of the samples: from 25 to 400 °C for Cu-Anth-MOF; from 25 to 600 °C for Ni-Anth-MOF. Heating rate: 10 °C min . -1 Samples with a mass of ~ 3.3 mg were used, and the nitrogen flow rate was 100±10 ml·min . See Fig. 7 for the thermogravimetric curve for Cu-Anth-MOF, see Fig. 8 for the thermogravimetric curve for Ni-Anth-MOF.

[0042] Fluorescence in solution. The solution of MB in water was prepared with a final concentration of 1 µmol / L, pH 7. The fluorescence emission spectrum was recorded with excitation at 290 nm (Fig. 11).

[0043] Solid-state fluorescence. The crystals synthesized in this way were isolated by filtration, washed on filters, but not dried. Background fluorescence was measured with excitation at 290 nm ( Fig. 12 for Cu-Anth-MOF and Fig. 14 for Ni-Anth-MOF). MoF crystals were soaked in aq. MB solution for 3 days at room temperature. Crystals were isolated by filtration and washed with water. The solid-state fluorescence emission spectrum was with excitation at 290 nm (Fig. 13 for Cu-Anth-MOF and Fig. 15 for Ni-Anth-MOF). Then, the Host-guest complexes of MOF with MB were suspended in water and the same amount of conc. aq. HCl was added. The The mixture was incubated at 50 °C for 8 h. All insoluble materials were filtered off, and the filtrate was washed with saturated NaHCO 3 neutralized to pH 7 and the fluorescence emission spectrum was recorded with excitation at 290 nm (Fig. 16 for Cu- Anth-MOF and Fig. 17 for Ni-Anth-MOF).

Claims

1. A microporous metal-organic framework (MOF) comprising tetradentate tetraphenylanthraquinone Connection units and at least one secondary structural unit (SBU), where the secondary structural unit only metal ions or metal ions and oxygen atoms with an O / metal ratio > 0.

5.

2. A metal-organic framework compound according to claim 1, wherein the metal ions are selected from Cu or Ni.

3. The metal-organic framework compound according to claim 2, wherein the metal ion is Cu.

4. The metal-organic framework compound according to claim 2, wherein the metal ion is Ni.

5. The metal-organic framework compound according to any one of the preceding claims further comprising an encapsulated Dye molecule.

6. The metal-organic framework compound according to claim 1, wherein the O / metal ratio is preferably >0.

6.

7. The metal-organic framework compound according to claim 1, in which the coordination polymer is ordered.

8. The metal-organic framework compound of claim 1, which reversibly encapsulates a dye molecule.

9. The metal-organic framework compound according to claim 1, wherein pore openings have an average diameter of 1-10 Angstroms.

10. Use of MOF according to any one of claims 1-9 for suppressing the fluorescence of an encapsulated molecule.