WELDED COMPONENT WITH EXCELLENT STRESS CORROSION CRACK RESISTANCE AND METHOD FOR MANUFACTURING THE SAME

A two-step artificial aging and heat treatment process for 7000 series aluminum alloys with specific compositions and structures addresses the challenges of stress corrosion cracking and strength, resulting in improved resistance and mechanical properties in welded components.

DE112020004885B4Active Publication Date: 2024-12-05UACJ CORP
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
DE112020004885
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-10-09
Filing Date
2020-10-08
Publication Date
2024-12-05
Estimated Expiration
2040-10-08

AI Technical Summary

Technical Problem

Existing methods for improving stress corrosion cracking resistance and strength in 7000 series aluminum alloy materials, such as those used in transportation equipment, face challenges with lengthy treatment periods, insufficient mechanical properties post-welding, and increased costs due to heat treatment processes.

Method used

A two-step artificial aging treatment followed by heat treatment of a 7000 series aluminum alloy material with specific chemical compositions and metallographic structures, including Zn, Mg, Zr, Ti, and optionally Cu, Mn, and Cr, to enhance stress corrosion cracking resistance and strength, with controlled electrical conductivity differences between welded and unaffected zones.

Benefits of technology

The method achieves improved stress corrosion cracking resistance and increased strength in welded aluminum alloy components, ensuring a fibrous metallographic structure and controlled electrical conductivity differences, thereby enhancing mechanical properties and corrosion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

Welded component with excellent stress corrosion cracking resistance, wherein the welded component comprises: an aluminum alloy material of the 7000 series, having a chemical composition comprising 6.6 wt% to 8.5 wt% Zn, 1.0 wt% to 2.1 wt% Mg, 0.10 wt% to 0.20 wt% Zr, 0.001 wt% to 0.05 wt% Ti, 0.02 wt% to 0.50 wt% Cu, 0.40 wt% or less Mn and 0.20 wt% or less Cr, the remainder comprising Al and unavoidable impurities, and having a metallographic structure that is fibrous; and another aluminum alloy material welded to the 7000 series aluminum alloy material, wherein in the aluminum alloy material of the 7000 series, the difference in the electrical conductivity of the aluminum alloy of the 7000 series between a mother part other than a zone affected by welding heat and the zone affected by welding heat is 1.2% IACS to 5% IACS, and the yield strength YS of the mother part is 350 MPa or higher.
Need to check novelty before this filing date? Find Prior Art

Description

Technical area

[0001] The present disclosure relates to a welded component having excellent stress corrosion cracking resistance and a method for producing the same. Technical background

[0002] High-strength and lightweight 7000 series aluminum alloy materials have been increasingly used as a material for elements that require weight reduction, such as transportation equipment.

[0003] Although 7000 series aluminum alloy materials have excellent mechanical properties, they are prone to stress corrosion cracking. Furthermore, when 7000 series aluminum alloy materials are joined by arc welding or similar processes, not only will the strength be reduced by the thermal effects of arc welding or similar processes, but the corrosion resistance and stress corrosion cracking resistance near the welded part will also be compromised.

[0004] As a method for improving the stress corrosion cracking resistance of a 7000 series aluminum alloy material, Patent Literature 1 discloses a method in which a material is subjected to aging treatment to obtain maximum strength and then brought into an overaged state by reheating treatment in the coating firing step.

[0005] Furthermore, Patent Literature 2 proposes a method for producing an extruded 7000 series aluminum alloy material, which method is characterized by performing a two-stage artificial aging treatment.

[0006] Furthermore, Patent Literature 3 proposes improving stress corrosion cracking resistance by subjecting a weld material to a solution heat treatment followed by an artificial aging treatment. US 2007 / 0 074 791 A1 relates to a high-strength aluminum extruded product with excellent shock absorption and stress corrosion cracking resistance, and a method for producing the same.

[0007] US 2012 / 0 024 433 A1 discloses a multi-alloy assembly having corrosion resistance and a method for its production.

[0008] US 2004 / 0 056 075 A1 concerns a welded aluminum alloy structure.

[0009] US 2007 / 0 204 937 A1 discloses a wrought aluminum alloy product of the AA7000 series and a method for producing the product.

[0010] US 2013 / 0 213 533 A1 relates to an extruded aluminum alloy material for electromagnetic forming. List of citationsPatent literature sources Patent Literature 1: Unexamined Japanese Patent Application No. 2006-233336 Patent Literature 2: Unexamined Japanese Patent Application No. 2010-275611 Patent Literature 3: Unexamined Japanese Patent Application No. 2000-317676 Summary of the inventionTechnical problem

[0011] In Patent Literature 1, aging treatment is performed under the conditions of "117 to 123°C for 18 to 24 hours or 127 to 133°C for 11 to 14 hours" to achieve maximum strength, followed by overaging treatment. However, these conditions require a long treatment time. In addition, if the matrix is ​​excessively aged, sufficient mechanical properties may not be achieved after welding. Furthermore, at a low treatment temperature of less than 145°C, η' phase (MgZn2) continuously precipitates at the grain boundaries; however, this is a factor that leads to a reduction in stress corrosion cracking resistance.

[0012] Patent Literature 2 describes the conditions for two-stage aging as follows: "the heat treatment temperature of the first step is in a range of 70 to 100°C, and the heat treatment temperature of the second step is in a range of 140 to 170°C." Patent Literature 2 further states: "In the two-stage aging treatment under production conditions, the heat treatment temperature of the second step was set to 140°C to 170°C, and the treatment time was set to 20 hours or shorter." However, the residence time of the heat treatment temperature in the second step is unclear. For example, even if the heat treatment temperature condition in the second step is 140°C to 170°C, a short residence time will result in under-aging, so sufficient stress corrosion cracking resistance cannot be achieved.In addition, even if the heat treatment temperature condition of the second step is 140°C to 170°C, sufficient strength cannot be achieved with a long residence time.

[0013] In Patent Literature 3, solution heat treatment and quenching of the weld material are performed after welding. However, this heat treatment method is associated with high costs.

[0014] The present disclosure has been made in view of the circumstances described above, and it is an object of the present disclosure to provide a welded component having excellent stress corrosion cracking resistance in which not only the corrosion resistance and stress corrosion cracking resistance of a 7000 series aluminum alloy material in its mother part and in the vicinity of a welded part are improved, but also the strength of the welded part is increased, and a method for producing the same. Solution to the problem

[0015] To achieve the above-described objective, the welded component according to a first aspect of the present disclosure is characterized in that it comprises: a 7000 series aluminum alloy material having a chemical composition containing 6.6 mass% to 8.5 mass% Zn, 1.0 mass% to 2.1 mass% Mg, 0.10 mass% to 0.20 mass% Zr, and 0.001 mass% to 0.05 mass% Ti, the balance containing Al and unavoidable impurities, and having a metallographic structure that is a fibrous structure; and another aluminum alloy material welded to the 7000 series aluminum alloy material, where If the electrical conductivity of the 7000 series aluminum alloy material before artificial aging treatment is defined as X% IACS and the electrical conductivity of the 7000 series aluminum alloy material after artificial aging treatment is defined as Y% IACS, the following equation is satisfied: 0.120≤(Y / X−1)≤0.250, and a difference in the electrical conductivity of the 7000 Series aluminum alloy material between a mating part other than the weld heat affected zone and the weld heat affected zone is 5% IACS or less.

[0016] The 7000 series aluminum alloy material may further contain 0.50 mass% or less of Cu.

[0017] The 7000 series aluminum alloy material may further contain 0.40 mass% or less of Mn and / or 0.20 mass% or less of Cr.

[0018] The 7000 series aluminum alloy material can contain 6.6 to 7.6 mass% Zn and 1.0 to 1.6 mass% Mg.

[0019] To achieve the above-described object, the manufacturing method according to a second aspect of the present disclosure is characterized in that it comprises: the first artificial aging treatment step of maintaining a 7000 series aluminum alloy material at a temperature of 90 to 110°C for 1 to 5 hours, wherein the 7000 series aluminum alloy material has a chemical composition containing 6.6 mass% to 8.5 mass% of Zn, 1.0 mass% to 2.1 mass% of Mg, 0.10 mass% to 0.20 mass% of Zr, and 0.001 mass% to 0.05 mass% of Ti, with a balance including Al and unavoidable impurities, and has a metallographic structure that is a fibrous structure; the second artificial aging treatment step of keeping the 7000 series aluminum alloy material subjected to the first artificial aging treatment step at a temperature of 145 to 160°C for 4 to 12 hours; the welding step of welding the 7000 series aluminum alloy material subjected to the second artificial aging treatment step with other aluminum alloy material to form a welded structure; and the heat treatment step of heat treating the welded structure at a temperature of 165 to 195°C for 10 to 60 minutes.

[0020] The 7000 series aluminum alloy material may further contain 0.50 mass% or less of Cu.

[0021] The 7000 series aluminum alloy material may further contain 0.40 mass% or less of Mn and / or 0.20 mass% or less of Cr.

[0022] The 7000 series aluminum alloy material can contain 6.6 to 7.6 mass% Zn and 1.0 to 1.6 mass% Mg. Advantageous effects of the invention

[0023] The welded component according to the present disclosure is manufactured by artificially aging a 7000 series aluminum alloy material in two steps to improve stress corrosion cracking resistance, and then heat-treating a welded structure in which the aluminum alloy material is welded at 165 to 195°C. This adjusts the electrical conductivity difference of the 7000 series aluminum alloy material between a mother part and a weld heat-affected zone to 5% IACS or less. Therefore, an increase in strength, as well as an improvement in corrosion resistance and stress corrosion cracking resistance, can be easily achieved. Brief description of the drawings Fig. 1 is a drawing showing a build-up welding mode and positions of electrical conductivity measurements in Examples; Fig.2 is a drawing illustrating a method used in the examples for observing the metallographic structure; and Fig. Figure 3 is a drawing illustrating a stress loading mode in the SCC test conducted in the examples. Description of embodiments

[0024] The 7000 series aluminum alloy material used in the present embodiment preferably has a composition containing 6.6 mass% to 8.5 mass% of Zn, 1.0 mass% to 2.1 mass% of Mg, 0.10 mass% to 0.20 mass% of Zr, and 0.001 mass% to 0.05 mass% of Ti, the balance including Al and unavoidable impurities.

[0025] First, the prescribed ranges of chemical composition are described with regard to the 7000 series aluminum alloy material.

[0026] A 7000 series aluminum alloy is a precipitation-hardened alloy. In the 7000 series aluminum alloy material, Zn and Mg coexist in the aluminum to cause the precipitation of the η' phase, which contributes to the improvement of mechanical properties. The 7000 series aluminum alloy material contains 6.6 to 8.5 mass% Zn and 1.0 to 2.1 mass% Mg. Zn: 6.6 mass% to 8.5 mass%

[0027] At a Zn content of less than 6.6 mass%, sufficient mechanical properties cannot be achieved because the amount of the η' phase coprecipitating with Mg is reduced. However, if the Zn content exceeds 8.5 mass%, stress corrosion cracking resistance decreases. Therefore, the Zn content is set at 6.6 mass% to 8.5 mass%. A more preferred range is 6.6 mass% to 7.6 mass%. Mg: 1.0 mass% to 2.1 mass%

[0028] At a Mg content of less than 1.0 mass%, sufficient mechanical properties cannot be achieved because the amount of the η' phase coprecipitating with Zn is reduced. However, if the Mg content exceeds 2.1 mass%, hot formability and thus productivity deteriorate. Therefore, the Mg content is set at 1.0 mass% to 2.1 mass%. A more preferred range is 1.0 mass% to 1.6 mass%.

[0029] The aluminum alloy material described above further contains, in addition to the elements described above, 0.10 mass% to 0.20 mass% Zr and 0.001 mass% to 0.05 mass% Ti as trace additive elements. Zr: 0.10 mass% to 0.20 mass%

[0030] The incorporation of Zr improves stress corrosion cracking resistance.

[0031] Furthermore, an Al-Zr intermetallic compound is formed, preventing the formation of a recrystallized structure, giving a cross-section a fibrous structure and improving stress corrosion cracking resistance. When the Zr content is less than 0.10 mass%, a fibrous structure cannot be obtained. However, when the incorporated Zr content exceeds 0.20 mass%, a coarse Al-Zr intermetallic compound is formed, and formability deteriorates. A more preferred range for the Zr content is 0.10 to 0.15 mass%. Ti: 0.001 mass% to 0.05 mass%

[0032] Incorporating Ti into an ingot has the effect of refining the ingot structure. Refining the ingot structure prevents cracking in the ingot and ultimately achieves a fine structure, which is beneficial to stress corrosion cracking resistance. When the Ti content is less than 0.001 mass%, the refining effects are not sufficiently achieved. If Ti is incorporated in an amount exceeding 0.05 mass%, point defects are likely to be generated, for example, due to coarsening of an Al-Ti intermetallic compound. It should be noted here that when Ti is incorporated into an ingot together with B as a TiB compound or the like, it refines the ingot structure in the same way as when incorporated alone. When Ti is incorporated as a TiB compound, less than 0.003 mass% of B is contained in it.

[0033] In addition to the composition described above, 0.50 mass% or less of Cu may also be incorporated. Cu: 0.50 mass% or less

[0034] The incorporation of Cu reduces the electrical potential difference between the crystal grain boundaries and the interior of the crystal grains, thus inhibiting sacrificial dissolution at the crystal grain boundaries. As a result, stress corrosion cracking resistance is improved. However, with a Cu content of more than 0.50 mass%, there is a risk of a reduction in overall corrosion resistance.

[0035] In addition to the composition described above, 0.40 mass% or less of Mn and / or 0.20 mass% and less of Cr may also be incorporated. Mn: 0.40 mass% or less, Cr: 0.20 mass% or less

[0036] In the same way as Zr, the incorporation of Cr and / or Mn prevents the formation of a recrystallized structure and imparts a fibrous structure to the cross-section, thereby improving stress corrosion cracking resistance. However, if Cr or Mn is added in an amount greater than the respective specified amount, hot formability deteriorates. In particular, if Cr is added in an amount greater than the specified amount, quench sensitivity increases.

[0037] The aluminum alloy material described above contains a metallographic structure that is a fibrous structure. The term "fibrous structure" used here refers to a metallographic structure formed by crystal grains with a high aspect ratio in a specific direction. For example, when viewed in a cross-section from a plane parallel to a processing direction (e.g., the extrusion direction in the case of an extruded material) and perpendicular to the width direction of the material, the metallographic structure can be regarded as a fibrous structure when the aspect ratio of the crystal grain size in the processing direction with respect to the crystal grain size in the thickness direction is 5 or higher.By controlling the metallographic structure to make it fibrous, not only can a strength-enhancing effect be achieved, but stress corrosion cracking resistance can also be improved. The metallographic structure can be examined, for example, by observing a cross-section of the aluminum alloy material under a polarizing microscope.

[0038] In the aluminum alloy material, the proportion of the area occupied by the fiber structure is preferably 70% or higher in a cross section parallel to the processing direction of the aluminum alloy material and perpendicular to the width direction of the material.

[0039] The aluminum alloy material has a yield strength, as defined in JIS Z2241 (ISO6892-1), of preferably 350 MPa or higher, more preferably 380 MPa or higher. This allows the strength properties required for reducing the thickness and weight of a component to be achieved.

[0040] Next, a method for manufacturing a welded component is described.

[0041] The welded component of the present disclosure can be divided into a 7000 series aluminum alloy material and another aluminum alloy material welded to the 7000 series aluminum alloy material (hereinafter, the other aluminum alloy material is also referred to as a "weldment"). For example, a hot-rolled or hot-extruded material can be used as the 7000 series aluminum alloy material. The welding element is not particularly limited as long as it is an aluminum alloy material. In the present embodiment, a case where the 7000 series aluminum alloy material is processed into an extruded profile will be described in particular.

[0042] A 7000 series extruded aluminum alloy material is produced by preparing an ingot from a melt having the chemical composition of the present disclosure and subjecting this ingot to homogenization treatment, hot extrusion treatment, solution heat treatment, and artificial aging treatment. This 7000 series extruded aluminum alloy material is joined by welding with a welding element. The 7000 series extruded aluminum alloy material and the welding element, which are welded together, are used as a welded structure, and this welded structure is heat-treated, thereby obtaining a welded component / structural member of the present disclosure. Homogenization treatment step

[0043] First, a homogenization treatment is carried out in which an ingot with the chemical composition values ​​described above is kept at a temperature of 450 to 500°C for 5 to 12 hours.

[0044] At temperatures below 450°C, the ingot is not sufficiently homogenized. At temperatures above 500°C, the crystal structure of an Al-Zr intermetallic compound deteriorates and coarsens. Due to this deterioration and coarsening of the crystal structure of the Al-Zr intermetallic compound, a fibrous metal structure cannot be obtained, and the effect of improving stress corrosion cracking resistance is thereby impaired. In addition, if the residence time during the homogenization treatment is shorter than 5 hours, sufficient homogenization is not achieved. Since the ingot is in a sufficiently homogenized state once the residence time exceeds 12 hours, a longer residence time is not expected to have any further effect. Therefore, it is desirable to keep the ingot at a temperature of 450 to 500°C for 5 to 12 hours during the homogenization treatment. Hot extrusion and solution heat treatment step

[0045] From the ingot subjected to the homogenization treatment described above, an extruded profile is produced by hot extrusion. The temperature before hot extrusion is controlled at 450 to 500°C. If this temperature is below 450°C, the deformation resistance increases. At a temperature above 500°C, the crystal structure of the Al-Zr intermetallic compound formed during the homogenization treatment is altered and coarsened. As a result, a fibrous metal structure cannot be obtained, and the effect of improving stress corrosion cracking resistance is impaired.

[0046] After hot extrusion, the resulting extruded profile is cooled to a temperature of 150°C or less. During hot extrusion, the temperature of the extruded profile after extrusion reaches the solution heat treatment temperature. By controlling the average cooling rate between 25°C / min and 1000°C / s during the subsequent cooling, the same effect as solution heat treatment can be achieved. At a cooling rate of less than 25°C / min, sufficient mechanical properties cannot be achieved due to the reduction in the amount of dissolved elements in the solid solution. At a cooling rate exceeding 1000°C / s, excessively large equipment is required and the appropriate effect cannot be achieved.

[0047] Furthermore, after cooling to a temperature of 150°C or less, the extruded profile may be reheated to a solution heat treatment temperature and then cooled at the cooling rate described above.

[0048] After the cooling process described above, the extruded profile is further cooled to room temperature. To achieve this, the extruded profile can be cooled to room temperature using the cooling process described above or can be cooled using another method. Step of artificial aging treatment

[0049] Next, an artificial aging treatment is performed on the extruded profile. This artificial aging treatment causes the precipitation of an η' phase, which is a strengthening phase, and thus improves the mechanical properties of the extruded profile. Artificial aging is achieved through a first artificial aging treatment (first artificial aging treatment step) and a second artificial aging treatment (second artificial aging treatment step). During the first artificial aging treatment, the extruded profile is held at a temperature of 90 to 110 °C for 1 to 5 hours. Then, following the first artificial aging treatment, the second artificial aging treatment is performed, in which the extruded profile is held at a temperature of 145 to 160 °C for 4 to 12 hours.During the first artificial aging treatment, GP(II) is formed, which will transition into an η' phase. During the second artificial aging treatment, the thus formed GP(II) will transition into an η' phase.

[0050] In the first artificial aging treatment, GP(II) is not densely formed if the temperature of the first artificial aging is below 90°C or the aging time is shorter than 1 hour. This leads to insufficient formation of the η' phase in the second artificial aging, and sufficient precipitation strengthening effect cannot be achieved. If the temperature of the first artificial aging is above 110°C, the formation of the η' phase begins without sufficient formation of GP(II), and even in this case, the precipitation of the η' phase may be insufficient. If the first artificial aging lasts for 5 hours or longer, the effect achieved by the first artificial aging is saturated.

[0051] Regarding the second artificial aging treatment, if the temperature of the second artificial aging is lower than 145°C or the aging time is shorter than 4 hours, the extruded profile will not be sufficiently aged. In this case, the stress corrosion cracking resistance of the female part will be reduced. In addition, when the aging temperature is below 145°C, although the η' phase precipitates uniformly, the η' phase is in a continuous state at the grain boundaries. By performing the artificial aging treatment at 145°C or higher, the η' phase is aggregated and coarsened at the grain boundaries, causing the η' phase with a diameter of 0.02 μm or more to become scattered at the grain boundaries, and thereby improving the stress corrosion cracking resistance.If the temperature of the second artificial aging exceeds 160 °C or the aging time exceeds 12 hours, sufficient mechanical properties cannot be achieved due to excessive aging. Furthermore, the additional post-welding heat treatment described below may not achieve sufficient improvement in the strength of a welded part.

[0052] As an indicator for determining whether the artificial aging treatment described above has been properly completed, the rate of change of the electrical conductivity of the extruded profile before and after the artificial aging treatment is defined. That is, if the electrical conductivity before the artificial aging treatment is defined as X and the electrical conductivity after the artificial aging treatment is defined as Y, the present disclosure is satisfied when the equation 0.120 ≤ (Y / X - 1) ≤ 0.250 is satisfied. If (Y / X - 1) < 0.120, since the extruded profile is not sufficiently aged, the stress corrosion cracking resistance is reduced. If 0.250 < (Y / X - 1), the strength of the extruded profile is reduced, and sufficient improvement in the strength of a welded part cannot be achieved by additional heat treatment after welding.

[0053] Continuously performing the first artificial aging treatment and the second artificial aging treatment means performing the second artificial aging treatment while maintaining the treatment temperature after the first artificial aging treatment. In other words, after the first artificial aging treatment, the process can continue with the second artificial aging treatment without opening a furnace, thus shortening the entire heat treatment time.

[0054] It is not essential to perform the first artificial aging treatment and the second artificial aging treatment continuously. For example, after the first artificial aging treatment is completed, the second artificial aging treatment may be performed once the extruded profile has cooled to a desired or lower temperature, e.g., room temperature. In these artificial aging treatments, the extruded profile is treated at a desired temperature not only between the first and second artificial aging treatments, but also between the respective artificial aging treatments, even if the extruded profile has been cooled to the desired appropriate temperature or lower once, whereby the present disclosure can be achieved.

[0055] The extruded profile obtained in the manner described above is welded with another aluminum alloy material, namely a welding element, by a method such as tungsten inert gas (TIG) welding or metal inert gas (MIG) welding, whereby a welded structure can be obtained (welding step).

[0056] The welded structure obtained after the welding described above is subjected to heat treatment at a temperature of 165 to 195°C for 10 to 60 minutes as a heat treatment step. This heat treatment step produces the welded component of the present disclosure. For example, the coating firing step can also be used as this step.

[0057] When a heat-treated aluminum alloy material, such as a 7000 series aluminum alloy material, is welded, a solid solution region (also synonymously referred to as a solid solution region) is formed near a welded part due to the thermal effect during welding, where the precipitated η' phase is dissolved into the matrix. In this solid solution region, the strength, corrosion resistance, and stress corrosion cracking resistance are reduced; however, these properties can be improved by reprecipitation of the η' phase through the heat treatment described above.

[0058] An indicator for judging whether strength, corrosion resistance, and stress corrosion cracking resistance have been improved is the difference in electrical conductivity between an unaffected mother part and a solid solution region. In the solid solution region, the electrical conductivity is at least 5% IACS lower than that in the unaffected mother part. By subjecting the welded structure obtained after welding to heat treatment at a temperature of 165 to 195°C for 10 to 60 minutes, the difference in electrical conductivity between the unaffected part and the solid solution region is controlled to 5% IACS or less. If the heat treatment temperature is below 165°C or the heat treatment time is shorter than 10 minutes, the difference in electrical conductivity may not be 5% IACS or less, and the properties described above are not sufficiently improved.At a heat treatment temperature above 195°C or a heat treatment duration of more than 60 minutes, the progression of softening leads to a deterioration in mechanical properties. It should be noted that in the following descriptions, a solid solution region formed by the thermal effect during welding is also referred to as a "welding heat-affected zone." In the examples, the electrical conductivity of an unaffected mother component and that of a solid solution region are compared. Examples

[0059] Examples of the present disclosure are described below in comparison with comparative examples to demonstrate the effects of the present disclosure. The examples described below represent only one embodiment of the present disclosure, and the present disclosure is in no way limited thereto. (Example 1)

[0060] An example relating to the welded component described above will now be described with reference to Tables 1 to 3.

[0061] In this example, extruded sections were manufactured under the same conditions for 7000 series aluminum alloys whose chemical compositions were varied within the alloy composition ranges described above. The electrical conductivity before and after artificial aging and the strength of the female part were measured for the resulting extruded sections. Furthermore, for samples produced by welding the surfaces of the female part samples described above and subsequently heat-treating them under the same conditions, the electrical conductivity of a weld heat-affected zone and the strength were measured, and a stress corrosion cracking (SCC) test was performed.

[0062] The following describes the sample preparation conditions, a method for measuring strength, a method for measuring electrical conductivity, and an SCC test method. <probenherstellungsbedingungen>Process for the production of extruded profiles

[0063] A 6-inch (152.4 mm) diameter ingot with the chemical composition shown in Table 1 was produced by semi-continuous casting. In Table 1, the term "residue" includes unavoidable impurities. Furthermore, Mn and Cr are included in the unavoidable impurities if these elements were present in a given sample number in an amount of less than 0.01 mass%. After a homogenization treatment in which the ingot was kept at a temperature of 470 °C for 6 hours, the ingot was reheated to 480 °C and hot extruded to obtain an extruded profile with a thickness of 3 mm. After this hot extrusion, the resulting extruded profile was quenched by air cooling.This extruded profile was kept at a temperature of 100°C for 3 hours to perform a first artificial aging treatment, and the sample thus obtained was heated to 150°C and left at that temperature for 8 hours without removing it from the furnace to perform a second artificial aging treatment. [Table 1] Sample No. Alloy composition (mass%) Zn Mg Cu Zr Mn Cr Ti Al Nr. 1 6.6 1.1 0.15 0.15 - - 0.01 rest Nr. 2 7.4 1.1 0.15 0.13 - - 0.01 rest Nr. 3 8.2 1.1 0.15 0.14 - - 0.01 rest Nr. 4 6.7 1.6 0.15 0.13 - - 0.01 rest Nr. 5 6.8 2.1 0.15 0.14 - - 0.01 rest Nr. 6 7.5 1.6 0.15 0.14 - - 0.01 rest Nr. 7 8.2 2.0 0.15 0.15 - - 0.01 rest Nr. 8 6.9 1.3 0.02 0.12 - - 0.01 rest Nr. 9 7.0 1.3 0.38 0.14 - - 0.01 rest Nr. 10 7.1 1.3 0.15 0.11 - - 0.01 rest Nr. 11 7.1 1.3 0.15 0.20 - - 0.01 rest Nr. 12 7.0 1.3 0.15 0.12 0.30 - 0.01 rest Nr. 13 7.1 1.3 0.15 0.13 - 0.16 0.01 rest Nr. 14 7.1 1.3 0.16 0.14 0.16 0.16 0.01 rest Nr. 15 6.0 1.4 0.15 0.11 - - 0.01 rest Nr. 16 9.1 1.3 0.15 0.15 - - 0.01 rest Nr. 17 5.5 0.7 0.15 0.13 - - 0.01 rest Nr. 18 7.0 2.5 0.15 0.15 - - 0.01 rest Nr. 19 7.0 1.4 0.59 0.13 - - 0.01 rest Nr. 20 7.0 1.4 0.15 0.01 - - 0.01 rest Nr. 21 6.9 1.3 0.17 0.28 - - 0.01 rest Nr. 22 7.1 1.3 0.15 0.13 0.43 - 0.01 rest Nr. 23 7.2 1.3 0.15 0.12 - 0.32 0.01 rest Welding processes

[0064] On the surface of a Fig. On the extruded profile 10 shown in Figure 1, overlay welding was performed under the conditions specified in Table 2 to form a weld bead 20. The weld bead 20 was formed along an LT direction (direction perpendicular to the extrusion direction of the extruded profile) in the center of an L direction (extrusion direction) of the cut extruded profile 10. For an SCC test piece 11, which will be described below, only its position is indicated by a dashed line because the SCC test piece 11 had not yet been manufactured from the extruded profile 10 at the time of overlay welding. [Table 2] Welding processes MIG welding Filler metal Alloy species 5356 diameter 1.2 mm Welding voltage 19 V Welding current 110 A Welding speed 800 mm / min protective gas Gas species Argon gas flow rate 20 rpm Heat treatment method

[0065] After overlay welding, the extruded profile was subjected to heat treatment at 170 °C for 20 minutes. <festigkeitsmessmethode>Strength of the nut part

[0066] A test piece was taken from the extruded profile sample subjected to artificial aging and heat treatment using a method in accordance with JIS Z2241 (ISO 6892-1). This test piece was formed into a mold in accordance with JIS No. 13B, and the yield strength YS (MPa) of the female part was measured. As a result of the measurement, a test piece with a yield strength YS of 350 MPa or higher was considered acceptable. Strength after welding

[0067] A test piece was taken from the extruded profile sample subjected to build-up welding and heat treatment using the method described in JIS Z3121 (ISO 4136). This test piece was formed into a shape according to JIS No. 1A, and the yield strength YS (MPa) of the heat-affected zone was measured. As a result of the measurement, a test piece with a yield strength YS of 285 MPa or more was considered acceptable. <Verfahren zum Beobachten der metallographischen Struktur>

[0068] For each sample, a cross section parallel to the L-direction, which is a processing direction (in this case the extrusion direction), and to the t-direction of the thickness, as shown in Fig. 2, the structure of a part near the center in the LT direction, the width direction, was observed. As shown in Fig. 2, an extruded material was cut out as a sample, mechanically polished and then electrolytically polished, after which a microphotograph of a cross-section (e.g. the photo below in Fig. 2) was taken under a polarizing microscope at 25x magnification. The resulting micrograph was examined to determine whether the metallographic structure was a fibrous structure extending in the machining direction. As a result of the observation, a metallographic structure with a fibrous structure content of 70% or more was judged to be a fibrous structure. <Verfahren zum Messen der elektrischen Leitfähigkeit>

[0069] Using an eddy current conductivity meter "SIGMATEST" from Foerster Japan Ltd., the electrical conductivity of the extruded profile before and after the artificial aging treatments as well as the electrical conductivity of an unaffected part and a heat-affected zone of the extruded profile 10 after build-up welding and heat treatment were measured. With regard to the extruded profile after build-up welding and heat treatment, as shown in Fig. As shown in Figure 1, the measurement was performed at two positions A (untouched nut part) and B (solid solution area created by welding), which were 60 mm and 5 mm away from the weld line of weld bead 20, respectively. The electrical conductivity was measured at room temperature and a frequency of 60 kHz. <SCC-Prüfverfahren>

[0070] From the extruded profile 10 welded in the LT direction, an SCC test piece 11 was prepared as a three-point bending test piece according to JIS H8711 such that a maximum stress was applied at a position at the boundary between the weld bead 20 and the female part surface. This SCC test piece 11 in the form of a flat plate was cut into a Fig. 3 shown SCC test device 30 is integrated.

[0071] The SCC test fixture 30 includes a frame 31, a press member 32, and insulators 33a to 33c. The frame 31 is substantially C-shaped as viewed in the drawing direction. Insulators 33b and 33c are connected to the frame 31 at two points. The press member 32 is screwed into the frame 31 and is movable in the vertical direction of the drawing. The insulator 33a is fixed to the upper end of the press member 32.

[0072] Fig. Figure 3 shows a state in which, after the SCC test piece 11 has been integrated into the SCC testing fixture 30, the pressing part 32 has been moved in the upward direction of the drawing. This bends the SCC test piece 11 at three locations where it is in contact with the insulators 33a to 33c.

[0073] A stress of 70% of the yield strength of the weld material was applied to the SCC test piece 11 in the L direction by three-point bending as shown in Fig. 3. In a room maintained at a room temperature of 25 ± 3 °C and a humidity of 40 to 75%, the SCC specimen 11, with the applied stress, was subjected to a 672-hour alternating immersion test, which involved repeated immersion in a 3.5 mass% NaCl aqueous solution for 10 minutes and drying in the room for 50 minutes. Here, a specimen that showed no cracking after the 672-hour test was considered acceptable. From the perspective of corrosion resistance, a specimen with a maximum corrosion depth of 400 µm or more, even without cracking, was considered unacceptable.

[0074] The evaluation results of each test are shown in Table 3. In the SCC test results shown in Table 3, "◯" means acceptable and "×" means unacceptable.

[0075] Samples No. 1 to No. 14 were acceptable in all respects and exhibited excellent properties.

[0076] Sample No. 15 was considered unacceptable because the yield strength YS of the weld material was below 285 MPa due to too low Zn content.

[0077] Sample No. 16 was considered unacceptable because cracks occurred during the SCC test due to excessive Zn content.

[0078] Sample No. 17 was considered unacceptable because, due to too low Mg content, the yield strength YS of the nut part was lower than 350 MPa and the yield strength YS of the weld material was lower than 285 MPa.

[0079] Sample No. 18 had too high a Mg content, so that its hot extrusion was not possible with practical equipment.

[0080] Sample No. 19 was deemed unacceptable because corrosion with a depth of 400 µm or more occurred during the SCC test due to excessive Cu content.

[0081] Sample No. 20 was considered unacceptable because the metallographic structure was a recrystallized structure due to too low Zr content and cracks appeared during the SCC test.

[0082] Sample No. 21 was considered unacceptable because coarse bonding was observed in the metallographic structure due to excessive Zr content.

[0083] Sample No. 22 had too high a Mn content, so its hot extrusion was not possible with practical equipment.

[0084] Sample No. 23 had too high a Cr content, so its hot extrusion was not possible with practical equipment. (Example 2)

[0085] An example relating to the above-described method for producing a welded component will now be described with reference to Tables 4 to 6.

[0086] In this example, for 7000 series aluminum alloy materials with the respective alloy composition ranges described above, extruded profiles were manufactured under the same conditions. Samples were prepared by subjecting the thus-obtained extruded profiles to artificial aging treatments under various conditions, and the strength of the female part was measured. Furthermore, for samples obtained by welding the surfaces of the female part samples described above and then subjecting them to heat treatment under various conditions, the electrical conductivity of a weld heat-affected zone was measured and an SCC test was conducted. The sample manufacturing conditions, a strength measurement method, an electrical conductivity measurement method, and an SCC test method are described below. <probenherstellungsbedingungen>Process for the production of extruded profiles

[0087] A 6-inch (152.4 mm) diameter ingot with the composition shown in Table 4 was produced by semi-continuous casting. In Table 4, the term "residue" includes unavoidable impurities. In addition, Mn and Cr were present in all sample numbers in an amount of 0.01 mass% and thus included in the unavoidable impurities. After a homogenization treatment in which the ingot was kept at a temperature of 470 °C for 6 hours, the ingot was heated again to 480 °C and hot-extruded to obtain an extruded profile with a thickness of 3 mm. After this hot extrusion, the resulting extruded profile was quenched by air cooling. This extruded profile was subjected to artificial aging treatments under the conditions shown in Table 5 to produce Samples No. a to No. i. [Table 4] Sample No. Alloy composition (mass%) Zn Mg Cu Zr Mn Cr Ti Al No. a - No. i 7.0 1.4 0.15 0.12 - - 0.01 rest [Table 5] Sample No. First artificial aging treatment Second artificial aging treatment Heat treatment after welding Temperature (°C) Time (h) Temperature (°C) Time (h) Temperature (°C) Time (h) No. a 90 1 150 8 170 20 No. b 110 5 150 8 170 20 No. c 100 3 160 12 170 20 No. d 100 3 150 8 170 10 No. e 100 3 150 8 190 60 No. f 100 3 140 4 170 20 No. g 100 3 175 8 170 20 No. h 100 3 150 8 as if welded No. i 100 3 150 8 200 60 Welding processes

[0088] In the same manner as in Example 1, on the surface of the Fig. 1, a build-up welding was carried out under the conditions specified in Table 2. Heat treatment processes

[0089] Samples No. a to No. i were subjected to heat treatment after build-up welding under the respective conditions shown in Table 5. <festigkeitsmessverfahren>Strength of the nut part

[0090] A test piece was taken from each sample of the extruded profile subjected to artificial aging and heat treatment according to JIS Z2241 (ISO 6892-1). This test piece was molded according to JIS No. 13B, and the yield strength YS (MPa) of the female part was measured. As a result of the measurement, a test piece with a yield strength YS of 350 MPa or higher was considered acceptable. Strength after welding

[0091] A test piece was taken from each sample of the extruded profile subjected to build-up welding and heat treatment, using the procedure described in JIS Z3121 (ISO 4136). This test piece was molded according to JIS No. 1A, and the yield strength YS (MPa) of the heat-affected zone was measured. As a result of the measurement, a test piece with a yield strength YS of 285 MPa or higher was considered acceptable. <Verfahren zum Messen der elektrischen Leitfähigkeit>

[0092] Using an eddy current conductivity meter "SIGMATEST" from Foerster Japan Ltd., the electrical conductivity of the extruded profile before and after the artificial aging treatments as well as the electrical conductivity of an unaffected part and a heat-affected zone of the extruded profile 10 after the build-up welding and the heat treatment were measured. With regard to the extruded profile after the build-up welding and the heat treatment, as shown in Fig. As shown in Figure 1, the measurement was performed at two positions A (unaffected mother part) and B (solid solution area created by welding), located 60 mm and 5 mm, respectively, from the weld line of weld bead 20. The electrical conductivity was measured at room temperature and a frequency of 60 kHz. <SCC-Prüfverfahren>

[0093] From the extruded profile 10 welded in the LT direction, an SCC test piece 11 was prepared as a three-point bending test piece according to JIS H8711, with the solid solution region formed during welding in the center. A stress of 70% of the yield strength of the weld material was applied to the SCC test piece 11 in the L direction by three-point bending as shown in Fig. 3, in the same manner as in Example 1. In a room maintained at a room temperature of 25 ± 3 °C and a humidity of 40 to 75%, the stress-loaded SCC test piece 11 was subjected to a 672-hour alternating immersion test, which included repeated immersion in a 3.5 mass% NaCl aqueous solution for 10 minutes and drying in the room for 50 minutes. A test piece with no cracking after the 672-hour test and a test piece with a maximum corrosion depth of 400 µm or less were evaluated as acceptable.

[0094] The evaluation results of the individual tests are shown in Table 6. For the SCC test results shown in Table 6, "O" means acceptable and "×" means unacceptable. [Table 6] Sample No. Extruded profile Welding material assessment Electrical conductivity (% LACS) YS (MPa) Electrical conductivity (% LACS) YS (MPa) SCC test results Before artificial aging treatment (X) After artificial aging treatment (Y) Y / X-1 Position A Position B Position A - Position B No. a 36.97 43.02 0.164 418 43.4 41.0 2.4 318 ◯ ◯ No. b 36.85 43.03 0.168 420 43.5 40.9 2.6 322 ◯ ◯ No. c 37.05 45.04 0.216 392 45.4 40.5 4.8 304 ◯ ◯ No. d 37.01 42.94 0.160 431 42.9 39.6 3.3 292 ◯ ◯ No. e 36.98 42.96 0.162 373 45.1 43.9 1.2 345 ◯ ◯ No. f 36.91 41.09 0.113 418 41.4 40.7 0.7 334 × (Rise) × No. g 37.02 47.60 0.286 334 47.3 41.5 5.8 281 ◯ × No. h 36.89 42.97 0.165 424 43.0 36.1 6.9 278 × (Corrosion) × No. in 36.95 43.02 0.164 325 45.6 43.7 1.9 316 ◯ ×

[0095] Samples No. a to No. e were acceptable in all respects and showed excellent properties.

[0096] Sample No. f was considered unacceptable because cracks occurred during the SCC test due to a low temperature of the second artificial aging.

[0097] Sample No. g was considered unacceptable because sufficient mechanical properties were not achieved due to a high temperature of the second artificial aging.

[0098] Sample No. h was deemed unacceptable because it remained as welded (in the as-welded condition) and showed corrosion of 400 µm or more in depth during the SCC test.

[0099] Sample No. i was considered unacceptable because sufficient mechanical properties were not achieved due to a high heat treatment temperature after welding.

[0100] The foregoing describes some examples of embodiments for illustrative purposes. While specific embodiments have been presented in the foregoing discussion, those skilled in the art will recognize that changes may be made in form and detail without departing from the broader spirit and scope of the invention. Accordingly, the specification and drawings are to be regarded in an illustrative rather than a restrictive sense. This detailed description, therefore, is not to be taken in a limiting sense, and the scope of the invention is defined only by the appended claims, along with the full scope of equivalents to which such claims are entitled.

[0101] This application claims the benefit of Japanese Patent Application No. 2019-186120, filed on October 9, 2019, the entire disclosure of which is incorporated herein by reference. Industrial applicability

[0102] The welded component according to the present disclosure and the method for producing the same according to the present disclosure can preferably be used, for example, for transportation equipment. List of reference symbols 10 extruded profile 11 SCC test piece 20 weld beads 30 SCC test device 31 frames 32 Pressed part 33a, 33b, 33c Insulator A, B Position< / festigkeitsmessverfahren> < / probenherstellungsbedingungen> < / festigkeitsmessmethode> < / probenherstellungsbedingungen>

Claims

[1] Welded component with excellent stress corrosion cracking resistance, the welded component comprising: a 7000 series aluminum alloy material having a chemical composition comprising 6.6 mass% to 8.5 mass% Zn, 1.0 mass% to 2.1 mass% Mg, 0.10 mass% to 0.20 mass% Zr, 0.001 mass% to 0.05 mass% Ti, 0.02 mass% to 0.50 mass% Cu, 0.40 mass% or less Mn, and 0.20 mass% or less Cr, the balance comprising Al and unavoidable impurities, and having a metallographic structure that is a fibrous structure; and another aluminum alloy material welded to the 7000 series aluminum alloy material, wherein in the 7000 series aluminum alloy material, a difference in electrical conductivity of the 7000 series aluminum alloy between a mother part other than a weld heat affected zone and the weld heat affected zone is 1.2% IACS to 5% IACS and a yield strength YS of the mother part is 350 MPa or higher. [2] The welded component according to claim 1, wherein the 7000 series aluminum alloy material comprises 0.16 mass% to 0.40 mass% Mn. [3] A welded component according to claim 1 or 2, wherein the 7000 series aluminum alloy material comprises 0.16 mass% to 0.20 mass% Cr. [4] A welded component according to any one of claims 1 to 3, wherein the 7000 series aluminum alloy material comprises 6.6 mass% to 7.6 mass% Zn and 1.0 mass% to 1.6 mass% Mg. [5] A manufacturing process for producing a welded component with excellent stress corrosion cracking resistance, the process comprising: the first artificial aging treatment step of maintaining a 7000 series aluminum alloy material at a temperature of 90 to 110°C for 1 to 5 hours, wherein the 7000 series aluminum alloy material has a chemical composition comprising 6.6 mass% to 8.5 mass% of Zn, 1.0 mass% to 2.1 mass% of Mg, 0.10 mass% to 0.20 mass% of Zr, 0.001 mass% to 0.05 mass% of Ti, 0.02 mass% to 0.50 mass% of Cu, 0.40 mass% or less of Mn, and 0.20 mass% or less of Cr, with a balance comprising Al and unavoidable impurities, and has a metallographic structure that is a fibrous structure; the second artificial aging treatment step, in which the 7000 series aluminum alloy material subjected to the first artificial aging treatment step is kept at a temperature of 145 to 160°C for 4 to 12 hours; the welding step of welding the 7000 series aluminum alloy material subjected to the second artificial aging treatment step with another aluminum alloy material to form a welded structure; and the heat treatment step of heat treating the welded structure at a temperature of 165 to 195°C for 10 to 60 minutes. [6] The manufacturing method according to claim 5, wherein the 7000 series aluminum alloy material comprises 0.16 mass% to 0.40 mass% Mn. [7] The manufacturing method according to claim 5 or 6, wherein the 7000 series aluminum alloy material comprises 0.16 mass% to 0.20 mass% Cr. [8] A manufacturing method according to any one of claims 5 to 7, wherein the 7000 series aluminum alloy material comprises 6.6 mass% to 7.6 mass% of Zn and 1.0 mass% to 1.6 mass% of Mg.

Citation Information

Patent Citations

  • Cover and luminaire

    JP2019186120A

  • Filler metal for welding of al-zn-mg-cu base alloy and heat treatment of welding material using the filler metal

    JP2000317676A

  • Method for producing automobile energy absorbing member

    JP2006233336A

  • 7,000 series aluminum alloy extruded material having excellent SCC resistance and method for producing the same