Method for producing a resin film using a 3D printer and polishing pads, resulting in a polished layer

By applying pressure and heat to 3D-printed resin films, the method enhances mechanical properties and abrasion resistance, addressing the weakness of 3D-printed resin films and extending the life of polishing pads.

DE112023000751T5Pending Publication Date: 2024-11-21KURARAY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
DE112023000751
Authority / Receiving Office
DE · DE
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-01-31
Filing Date
2023-01-30
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Resin films produced using 3D printing exhibit inferior mechanical properties, leading to polishing pads with low strength and abrasion resistance, resulting in a shortened service life.

Method used

A method involving the application of pressure and heat to a sheet-shaped resin-modeled article formed by a 3D printer, followed by deformation into a compressed film, with specific conditions on pressure, temperature, and atmosphere to enhance mechanical properties.

Benefits of technology

The method significantly improves the mechanical properties of resin films, enhancing their strength and abrasion resistance, thereby extending the service life of polishing pads used in processes like CMP.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

The present invention relates to a method for producing a resin film, comprising at least the following step P: a step of applying pressure (p) to a film-shaped, resin-modeled object formed by a 3D printer while it is heated, and of deforming the film-shaped, resin-modeled object to obtain a compressed film; and relates to a polishing pad containing a polishing layer obtained by using the manufacturing method.
Need to check novelty before this filing date? Find Prior Art

Description

Field of expertise

[0001] The present invention relates to a method for producing a resin film using a 3D printer and a polishing pad comprising a polishing layer obtained thereby. State of the art

[0002] In recent years, the so-called 3D printing technology has been used as a technology for three-dimensional molding of resin materials based on designs from three-dimensional data, such as 3D CAD and 3D CG.

[0003] 3D printers are becoming increasingly popular among the public as devices that utilize 3D printing technology. For example, when a modeled object is formed from resin using a 3D printer, it is possible to create a resin-modeled object without using a modeling machine (e.g., a mold or a mold for forming a specific shape) customized for a specific modeled object, as was the case in the past.

[0004] As examples of a molding method for molding resin materials using 3D printing technology, various methods are known, such as the fused deposition modeling (FDM) method in which a modeled object is formed by heating and melting a thermoplastic resin and then extruding it from a nozzle and laminating it layer by layer on a modeling table; the stereolithography method (SLA (Stereo Lithography Apparatus)) in which a three-dimensional modeled object is formed while a curable resin is deposited layer by layer by irradiating it with high-energy rays such as lasers.ultraviolet rays, into a light-curable liquid resin; and an inkjet method in which a cured resin product is laminated during curing with energy rays after injection from an ink head, whereby an ink in an inkjet printer is replaced by an energy-curable resin.

[0005] Furthermore, an example of the modeled object formed using 3D printing technology includes a polishing layer used for a polishing pad used in a polishing process for planarizing a surface of a semiconductor wafer. A typical example of the polishing pad includes a polishing pad used in a polishing process for planarizing a surface of a semiconductor wafer by a CMP (Chemical Mechanical Polishing (Planarization)) polishing process.

[0006] For example, in Patent Document 1, a 3D printing method is described as a method for forming a groove on a polishing pad for CMP.

[0007] Furthermore, Patent Document 2 describes a method for manufacturing a polishing layer of a polishing pad, which includes sequentially laminating multiple layers using a 3D printer, and laminates each layer of the multiple polishing layers by ejecting a pad material precursor from a nozzle and solidifying the pad material precursor to form a solidified pad material. Furthermore, Patent Document 3 describes a method for manufacturing a polishing layer of the polishing pad formed from a polymer matrix in which particles are embedded in a desired distribution using a 3D printer.

[0008] Furthermore, Patent Document 4 describes a method for producing a porous polishing pad by evaporating a porosity-generating agent by means of a thermal treatment by heating at low temperatures (e.g., 100°C) under low pressure. Reference listPatent literature Patent Document 1: JP 2008-507417 A Patent Document 2: JP 2015-517922 A Patent Document 3: JP 2016-536151 A Patent Document 4: JP 2021-523025 A Summary of the inventionTechnical problem

[0009] By using 3D printing technology, it is possible to reduce the loss of resin materials, for example, compared to conventional processes such as extrusion molding and injection molding, which leads to advantages such as cost reduction and effective resource utilization.

[0010] On the other hand, the inventors of the present invention have investigated and found that when resin is molded by using a 3D printer, unlike the conventional method, the physical properties of the obtained resin film, particularly the mechanical properties, tend to be inferior.

[0011] Therefore, in the polishing pads described in Patent Documents 1 to 4, the polishing layer has low strength and low abrasion resistance and is easily worn by the skin pass treatment, so it is considered that the service life (useful life) when used as a polishing pad is shortened.

[0012] An object of the present invention is to provide a method for producing a resin film which can improve the mechanical properties of the resin film when the resin film is formed using a 3D printer. Solution to the task

[0013] The present invention includes the following inventions. [1] A process for producing a resin film comprising at least the following step P, Step P: a step of applying pressure (p) to a sheet-shaped resin modeled article formed by a 3D printer while heating it, and deforming the sheet-shaped resin modeled article to obtain a compressed sheet. [2] The method for producing a resin film according to the above item [1], wherein the heating temperature in the step P is 80°C or higher. [3] The method for producing a resin film according to the above item [1] or [2], wherein the pressure (p) in step P is 0.1 MPa or more. [4] The method for producing a resin film according to any one of the above items [1] to [3], wherein a spacer is used in step P. [5] The method for producing a resin film according to any one of the above items [1] to [4], wherein the product of the pressure (p) and the time (t) for applying the pressure (p) in the step P satisfies the following formula (i); Formula (i): 5 ≤ p × t ≤ 5000 [one unit of p is MPa, one unit of t is second]. [6] The method for producing a resin film according to any one of the above items [1] to [5], wherein step P is carried out under a reduced pressure atmosphere. [7] The method for producing a resin film according to any one of the above items [1] to [6], wherein the resin-modeled article in step P is a polyurethane-modeled article. [8] The method for producing a resin film according to any one of the above items [1] to [7], further comprising the following step M before the step P, Step M: using a 3D printer, a step of discharging a melt or a precursor of a resin from a nozzle and solidifying the same to form a sheet-shaped resin modeled article. [9] The method for producing a resin film according to the above item [8], wherein the melt or precursor of the resin in step M passes through a filter before being discharged from the nozzle of the 3D printer.

[10] The method for producing a resin film according to the above item [8] or [9], wherein the resin is a thermoplastic resin and the solidification of the thermoplastic resin in the step M is carried out by cooling.

[11] The method for producing a resin film according to the above item

[10] , wherein the thermoplastic resin in the step M is a thermoplastic polyurethane.

[12] The method for producing a resin film according to any one of the above items [1] to

[11] , further comprising the following step T after the step P, Step T: a step of making a thickness of the compressed film obtained in the step P thin using one or more methods selected from the group consisting of cutting, machining, and grinding.

[13] The method for producing a resin film according to any one of the above items [1] to

[12] , wherein the resin film is a polishing layer for a polishing pad.

[14] A polishing pad containing a polishing layer obtained by using the method for producing a resin film according to the above item

[13] . Advantageous effects of the invention

[0014] According to the present invention, it is possible to provide a method for producing a resin film which can improve the mechanical properties of the resin film when a resin film is formed using a 3D printer. Short description of the drawings Fig. 1 is a schematic diagram illustrating an example of a method for forming a sheet-shaped resin-modeled article using a 3D printer. Fig. 2 is a schematic cross-sectional view illustrating an example of a sheet-shaped resin modeled article formed using a 3D printer before being subjected to a step P according to the present invention. Fig. 3 is a schematic cross-sectional view illustrating an example of a compressed sheet obtained by subjecting the sheet-shaped resin modeled article formed using the 3D printer to step P according to the present invention. Fig. 4 is a schematic plan view showing the outline of a disk-shaped film and a test piece used in the measurement of storage modulus in Examples. Description of the embodiments

[0015] The following explanation will be given based on an example of the embodiments of the present invention. The embodiments shown below are an example for embodying the technical idea of ​​the present invention, and the present invention is not limited to the following description.

[0016] The present invention also includes embodiments in which the items described in this description are arbitrarily selected or arbitrarily combined. In this description, preferred arrangements can be arbitrarily selected, and it can be said that the combination of preferred arrangements is more preferred.

[0017] Throughout this specification, unless otherwise specified, the term "XX to YY" as a numerical range means "XX or more and YY or less." For example, simply specifying "10 to 90" as a numerical range represents a range of 10 or more and 90 or less.

[0018] In this specification, the lower limits and upper limits specified in stages for the numerical ranges (the content of each component, values ​​calculated for each component, each property, and the like) may be combined independently. For example, the expression "preferably 10 to 90, more preferably 30 to 60" may mean "10 to 60" for the same item when "the preferred lower limit (10)" and "the more preferred upper limit (60)" are combined.

[0019] Furthermore, for the numerical range, for example, with respect to the statement "preferably 10 to 90, more preferably 30 to 60", only the lower limit may be specified as "10 or more" or "30 or more" without specifically specifying the upper limit, and similarly only the upper limit may be specified as "90 or less" or "60 or less" without specifically specifying the lower limit.

[0020] For example, as described above, the expression "preferably 10 or more, more preferably 30 or more" and the expression "preferably 90 or less, more preferably 60 or less" for the same item may mean "10 or more and 60 or less" by combining "the preferred lower limit (10)" and "the more preferred upper limit (60)". Furthermore, as described above, only the lower limit may be expressed as "10 or more" or "30 or more", and similarly, only the upper limit may be expressed as "90 or less" or "60 or less".Furthermore, in this specification, unless otherwise stated, the term "mechanical properties" refers more specifically to "storage modulus", "breaking stress", "breaking elongation" and "abrasion resistance" of the resin film and the polishing layer obtained by a method for producing a resin film which is an embodiment of the present invention. [Method for producing a resin film]

[0021] A method for producing a resin film which is an embodiment of the present invention is characterized in that at least the following step P is included.

[0022] Step P: a step of applying pressure (p) to a sheet-shaped resin modeled article formed by a 3D printer while heating it, and deforming the sheet-shaped resin modeled article to obtain a compressed sheet.

[0023] Furthermore, a method for producing a resin film which is an embodiment of the present invention preferably further includes the following step M before the step P. Step M: using a 3D printer, a step of discharging a melt or a precursor of a resin from a nozzle and solidifying the same or the same to form a film-shaped resin modeled article.

[0024] Furthermore, a method for producing a resin film which is an embodiment of the present invention preferably further includes the following step T after the step P.

[0025] Step T: a step of making a thickness of the compressed film obtained in step P thin using one or more methods selected from the group consisting of cutting, machining, and grinding.

[0026] Furthermore, a method for producing a resin film which is an embodiment of the present invention is not particularly limited as long as at least the above-described step P is included as described above, and it may be an embodiment including the step M and the step P, may be an embodiment including the step P and the step T, and may be an embodiment including the step M, the step P, and the step T in this order. Further, each embodiment may additionally include steps other than the respective step, and it may be an embodiment in which these steps can be directly carried out without going through other steps.

[0027] Each step of the method for producing a resin film which is an embodiment of the present invention will be described below. < Step P >

[0028] Step P is a step of applying pressure (p) to a sheet-shaped resin molded article formed by a 3D printer while heating it, and deforming the sheet-shaped resin molded article to obtain a compressed sheet. Hereinafter, in this specification, the "sheet-shaped resin molded article" is also simply referred to as "resin molded article." For the following reasons, it is believed that the mechanical properties of the resin film formed by a 3D printer are improved by undergoing process P. As described above, there are various methods for forming a sheet-shaped resin molded article using a 3D printer. For example, a schematic diagram of an example of a method for molding a resin using a 3D printer is shown in Fig. 1 shown. Fig. 1 shows that, as shown in the above-mentioned FDM method, a melt or its precursor 1 of the resin as a raw material is extruded from a nozzle 2, and a resin modeled article 10 is formed by laminating one layer after another from below on a modeling table 3. In the formation of one layer, the melt or its precursor 1 of the resin extruded from the nozzle 2 is arranged in order in the plane direction (two-dimensionally) to form a first layer A, and then a layer B, which is the second layer, is formed in a similar manner by disposing the melt or precursor 1 of the resin extruded from the nozzle 2 on the formed layer A, and the layer B is laminated on the layer A. Fig. 1 illustrates the stage in which a layer C is further formed on the layer B. By repeating this process several times, multiple layers are laminated, and finally, a sheet-shaped resin-modeled article is formed. Further, for example, as an embodiment of the sheet-shaped resin-modeled article formed using a 3D printer, it may be a sheet-shaped resin-modeled article consisting of a single layer (for example, only the first layer A shown in Fig. 1), preferably it is a sheet-shaped resin-modeled article formed by laminating several layers, as shown in Fig. 1 shown.

[0029] Fig. Fig. 2 shows a schematic cross-sectional view according to an example of the sheet-shaped resin-molded article formed in this way. The sheet-shaped resin-molded article 10 formed by a 3D printer, which is shown in Fig. 2, for example, consists of layer A as the first layer formed on the modeling table, layer B as the second layer, and layer C as the third layer, in descending order from the bottom.

[0030] As shown in the schematic cross-sectional view of Fig. 2, it is assumed here that there is a cavity 12 between the adjacently arranged resin blocks 11 and the contact area of ​​the contact surfaces 11a between the resin blocks 11 is limited, which leads to insufficient fusion of the resin blocks 11. In this description, a portion shown in the schematic cross-sectional views in the Fig. 2 and Fig. 3, which will be described later (in Fig. 2 the section is shown as a circle, and in Fig. 3, the section is shown as a substantially rectangular section), for explanation purposes referred to as a “resin block”. However, the resin block may be a cross section of a continuously arranged resin filament or a cross section of an arranged drop-shaped resin, and there is no particular limitation on the embodiment of the arrangement of the resin and its cross-sectional shape. However, a resin block 11 shown in the schematic cross-sectional representation of Fig. 2 and Fig. 3, and the adjacent resin blocks 11 may have been arranged with a small time interval, or, for example, they may be considered to have been extruded from different nozzles even if they were arranged at the same time due to the use of multiple nozzles.

[0031] Next, a schematic cross-sectional view of an example of a compressed film obtained by step P is shown in Fig. 3. More precisely, Fig. 3 is a schematic cross-sectional view of an example of a compressed film 20 obtained by applying the pressure (p) to the film-shaped resin-modeled article 10 formed by a 3D printer shown in Fig. 2, while being in relation to the lamination direction (direction indicated by the arrow P in Fig. 3) when the sheet-shaped resin-modeled article 10 has been formed by a 3D printer, and by deforming the sheet-shaped resin-modeled article 10.

[0032] In step P, the direction of pressure applied to the sheet-shaped resin-modeled article is not particularly limited as long as the effect of the present invention can be achieved. For example, similar to the direction indicated by the arrow P in Fig. 3, it is preferable to apply the pressure (p) in the thickness direction of the resin-modeled article while heating it. In addition, as shown in Fig. 3, more preferably, the pressure (p) in the thickness direction of the sheet-shaped resin-modeled article and the lamination direction (direction indicated by the arrow P in Fig. 3) when a sheet-shaped resin-modeled article is formed with a 3D printer while being heated.

[0033] By performing step P, ie, by applying pressure (p) to a sheet-shaped resin-modeled article formed by a 3D printer while heating it, the sheet-shaped resin-modeled article is deformed. By step P, as shown in Fig. 3 shown in Fig. 2, the existing cavity 12 is reduced or eliminated, and the contact area of ​​the contact surfaces 11a of the adjacent resin blocks 11 is also increased. It is believed that by heating and compressing the sheet-shaped resin-modeled article, not only does the contact area of ​​the contact surfaces 11a between the resin blocks 11 increase, but the entanglement of the polymer molecules constituting each resin block 11 at the contact surfaces 11a between the resin blocks 11 also increases. It is believed that these changes further promote the fusion of the resin blocks 11 and further increase the entanglement of the polymers at the molecular level, thereby significantly improving the mechanical properties of the ultimately obtained resin film.

[0034] Furthermore, it is believed that the significant improvement in the mechanical properties of the resin film obtained by the resin film manufacturing method according to the present invention and the polishing layer described below is mainly due to an improvement in the contact area between the resin blocks and the increase in entanglement between the polymer molecules, as mentioned above. However, it is extremely difficult for the current technology to accurately evaluate the extent of the contact area between the resin blocks in the entire obtained resin film, and further to confirm the state of entanglement of polymer molecules between the resin blocks and define the degree of entanglement.

[0035] Therefore, a resin film obtained using the method for producing a resin film, a polishing layer obtained using the method for producing a resin film, and a polishing pad having a polishing layer obtained using the method for producing a resin film are each defined by the method for producing a resin film, which is one embodiment of the present invention. This is because there are circumstances that cannot avoid specification according to the method for producing a resin film.

[0036] The heating temperature in step P is preferably higher than room temperature (23°C), more preferably 60°C or higher, even more preferably 80°C or higher, even more preferably 90°C or higher, even more preferably 100°C or higher, even more preferably 110°C or higher, even more preferably 120°C or higher, from the viewpoint of being able to more easily achieve the effects of the present invention.

[0037] The upper limit of the heating temperature is not particularly limited, but it is, for example, from the viewpoint of further preventing excessive compression of the resin film and thermal decomposition of the resin, and from the viewpoint of improving productivity, preferably 210°C or less, more preferably 200°C or less, even more preferably 190°C or less, even more preferably 180°C or less.

[0038] As described above, these lower limits and upper limits, indicated in steps, can be independently combined. For example, as one embodiment of the manufacturing process, the heating temperature in step P is preferably 60 to 210°C, more preferably 80 to 200°C, even more preferably 90 to 200°C, even more preferably 100 to 190°C, even more preferably 110 to 190°C, even more preferably 120 to 180°C.

[0039] In one embodiment of the manufacturing method, the pressure (p) in the step P is preferably 0.1 MPa or more, more preferably 0.3 MPa or more, even more preferably 0.5 MPa or more, from the viewpoint of more easily achieving the effect of the present invention, and is preferably 20 MPa or less, more preferably 15 MPa or less, even more preferably 10 MPa or less, from the viewpoint of further preventing excessive compression of the resin film, from the viewpoint of improving productivity, and the like.

[0040] As described above, these lower limits and upper limits, which are specified in steps, can be combined independently. For example, in one embodiment of the manufacturing process, the pressure (p) in step P is preferably 0.1 to 20 MPa, more preferably 0.3 to 15 MPa, even more preferably 0.5 to 10 MPa.

[0041] Further, in one embodiment of the manufacturing method, the time (t) for applying the pressure (p) in the step P is preferably 1 second or more, more preferably 5 seconds or more, even more preferably 8 seconds or more, even more preferably 10 seconds or more, from the viewpoint of more easily achieving the effects of the present invention, and is preferably 10,000 seconds or less, more preferably 5,000 seconds or less, even more preferably 500 seconds or less, even more preferably 200 seconds or less, from the viewpoint of further preventing thermal decomposition of the resin, from the viewpoint of improving productivity, and the like.

[0042] As described above, these lower limits and upper limits, which are specified in steps, can be combined independently. For example, in one embodiment of the manufacturing method, the time (t) for applying the pressure (p) in step P is preferably 1 to 10,000 seconds, more preferably 5 to 5,000 seconds, even more preferably 8 to 500 seconds, and even more preferably 10 to 200 seconds.

[0043] In one embodiment of the manufacturing method, from the viewpoint of more easily achieving the effects of the present invention, it is preferable that the product of the pressure (p) and time (t) for applying the pressure (p) in the step P satisfies the following formula (i). 5≤p×t≤5000[one unit of p is MPa, one unit of t is second].

[0044] The value calculated by the above formula (i) is more preferably 10 or more, even more preferably 13 or more, from the viewpoint of more easily achieving the effects of the present invention, and more preferably 4,500 or less from the viewpoint of further preventing excessive compression of the resin film and thermal decomposition of the resin, from the viewpoint of improving productivity, and the like, and it is even more preferably 4,000 or less; even more preferably 2,000 or less, even more preferably 1,000 or less, even more preferably 500 or less from the viewpoint of more easily achieving the effects of the present invention, from the viewpoint of improving productivity, and the like.

[0045] As described above, these lower limits and upper limits, which are indicated in steps, can be combined independently. For example, as one embodiment of the manufacturing method, the value calculated using the above formula (i) is more preferably 5 to 4,500, even more preferably 10 to 4,000, even more preferably 10 to 2,000, even more preferably 10 to 1,000, even more preferably 13 to 500.

[0046] Further, it is preferable to use a spacer having a smaller thickness than the resin-modeled article before heat-pressing in the step P, from the viewpoint of further preventing excessive compression of the resin film and thermal decomposition of the resin, from the viewpoint of being able to more easily control the thickness of the obtained compressed film, and the like.

[0047] More specifically, for example, the heat pressing in step P can be performed using a known pressing machine, such as a heat press machine that heats an article by sandwiching it between heated upper and lower flat heating plates while applying pressure, or a calender roll that applies pressure with heated rollers. It is preferable to use a heat press machine from the viewpoint of being able to more easily control the heating time and the applied pressure.When performing heat pressing, it is more preferable that a spacer is placed as the outer frame of the sheet-shaped resin molded article formed by a 3D printer, and pressure (p) is applied to the sheet-shaped resin molded article in the state where the spacer is sandwiched with the sheet-shaped resin molded article while heating it. In this way, in the early stage of heat pressing, only pressure is applied to the resin molded article, and the thickness quickly becomes thin. Once the thickness of the resin molded article equals the thickness of the spacer, no further compression is applied, whereby a sheet with a predetermined thickness can be easily obtained.

[0048] Further, as described above, when the spacer is used in the step P, the spacer may be manufactured and used in a state independent of the heat press machine, or it may be used in a state in which it has been previously installed in a pressing section of the heat press machine.

[0049] Furthermore, the shape of the spacer is not particularly limited as long as it can be used as an outer frame of the sheet-shaped resin modeled article formed by a 3D printer as described above, and examples include a circular ring or one whose outer edge is square and whose inner edge is circular or square.

[0050] Furthermore, the thickness of the spacer is not particularly limited as long as the effect of the present invention is achieved, but it is preferably equal to or smaller than the thickness of the sheet-shaped resin-molded article before pressure is applied, and preferably smaller than the thickness of the sheet-shaped resin-molded article before pressure is applied. Furthermore, as one embodiment of the spacer, the ratio of the thickness (unit: mm) of the spacer to the thickness (unit: mm) of the sheet-shaped resin-molded article before pressure is applied [thickness of a spacer / thickness of a sheet-shaped resin-molded article before pressure is applied] is preferably 1.0 or less, more preferably less than 1.0, even more preferably 0.9 or less, and is preferably 0.3 or more, more preferably 0.5 or more, even more preferably 0.7 or more.

[0051] As described above, these lower limit values ​​and upper limit values, which are indicated in steps, can be combined independently. For example, as one embodiment of the manufacturing method, the ratio [thickness of a spacer / thickness of a sheet-shaped resin-molded article] is preferably 0.3 or more and 1.0 or less, more preferably 0.5 or more and less than 1.0, even more preferably 0.7 or more and 0.9 or less.

[0052] The spacer is preferably one that has removability with respect to the resin-molded article, and examples include a spacer formed of at least one selected from the group consisting of fluororesins such as polytetrafluoroethylene and ethylene-tetrafluoroethylene copolymer, epoxy resins, glass-epoxy resins, and polyimide resins. Further, for example, as one embodiment of the method for producing a resin film, when thermoplastic polyurethane is used as a resin for forming the resin-molded article, it is preferable to use a spacer made of polytetrafluoroethylene.

[0053] In addition, from the viewpoint of more easily achieving the effect of the present invention, it is preferable that step P is carried out under a reduced pressure atmosphere.

[0054] The reason why the effect of the present invention is more easily achieved by carrying out the step P under a reduced pressure atmosphere is presumably that it becomes easier to remove air bubbles and voids remaining in the resin molded article and, for example, it becomes easier to control the contact area of ​​the contact surface 11a between the resin blocks 11 in Fig. 3 to enlarge.

[0055] The degree of vacuum in the step P under the reduced pressure atmosphere is preferably 101 kPa or less, more preferably 50 kPa or less, even more preferably 10 kPa or less, even more preferably 5 kPa or less, in terms of absolute pressure. The degree of vacuum in the step P under the reduced pressure atmosphere is 0 kPa or more in terms of absolute pressure, and preferably 1 kPa or more from the viewpoint of cost reduction during production. In other words, in one embodiment of the production method, the degree of vacuum in the step P under the reduced pressure atmosphere is preferably 0 to 101 kPa, more preferably 0 to 50 kPa, even more preferably 0 to 10 kPa, even more preferably 0 to 5 kPa, even more preferably 1 to 5 kPa, in terms of absolute pressure. (Resin)

[0056] The resin which is the starting material for the resin-molded article in the step P may be a thermoplastic resin or a thermosetting resin as long as it can be molded with a 3D printer, and there are no particular restrictions, but a thermoplastic resin is preferable.

[0057] Examples of the thermoplastic resin include polyurethane; polyolefin resins such as polyethylene, polypropylene, polybutene, or copolymers polymerized from two or more selected from ethylene, α-olefins, cyclic olefins, vinyl acetate, styrene; olefin-based thermoplastic elastomers (TPO); polyvinyl chloride; polyvinyl acetate; styrene resins such as polystyrene and acrylonitrile-styrene copolymers; acrylic resins such as a copolymer polymerized from one or more selected from methacrylic acid, methacrylic acid ester, acrylic ester, styrene; polyester resins such as polyethylene terephthalate, polybutylene terephthalate, and polylactic acid; polyester-based thermoplastic elastomers; polyamides such as aliphatic polyamides, alicyclic polyamides, and aromatic polyamides; polyamide-based thermoplastic elastomers; polycarbonate; Silicone-based elastomers, such asSilicone rubber; polylactic acid; natural rubber; a diene rubber, which is a copolymer of one or more types selected from polybutadiene, polyisoprene, polychloroprene, or diene monomers such as butadiene, isoprene, and chloroprene, and one or more types of vinyl monomers such as styrene, ethylene, propylene, various butenes, styrene, and acrylonitrile; acrylic acid alkyl ester rubber (acrylic rubber), which is a copolymer containing acrylic acid ester as the main monomer; fluororesins such as polytetrafluoroethylene; and fluorine-based thermoplastic elastomers. These can be used alone or in combination of two or more.

[0058] Examples of the thermosetting resin include epoxy resin, thermosetting polyurethane and thermosetting acrylic resin. (Thermoplastic polyurethane)

[0059] As an embodiment of the method for producing a resin film, the resin molded article in the step P is preferably a polyurethane molded article, and more preferably a thermoplastic polyurethane molded article.

[0060] The thermoplastic polyurethane is not particularly limited as long as the effects of the present invention are achieved, but, for example, from the viewpoint of ease of production of the thermoplastic polyurethane, it is preferable to contain at least one structural unit derived from polyols, one structural unit derived from polyisocyanate, and one structural unit derived from a chain extender, and it is more preferable to contain only one structural unit derived from a polyol, one structural unit derived from a polyisocyanate, and one structural unit derived from a chain extender.

[0061] The total content of the structural unit derived from polyol, the structural unit derived from polyisocyanate, and the structural unit derived from a chain extender, based on the total structural units in the thermoplastic polyurethane, is preferably 80 mass% or more, more preferably 85 mass% or more, even more preferably 90 mass% or more, even more preferably 95 mass% or more, even more preferably 100 mass%.In other words, in one embodiment of the production process, the total content of the polyol-derived structural unit, the polyisocyanate-derived structural unit, and the chain extender-derived structural unit, based on the total structural units in the thermoplastic polyurethane, is preferably 80 to 100 mass%, more preferably 85 to 100 mass%, even more preferably 90 to 100 mass%, even more preferably 95 to 100 mass%, even more preferably 100 mass%. [Polyol]

[0062] Examples of the polyol include polymer diols, such as polyether diols such as polyethylene glycol (PEG) and polytetramethylene ether glycol (PTMG); polyester diol; and polycarbonate diol. These can be used alone or in combination of two or more.

[0063] Among them, one or more selected from the group consisting of polyetherdiol and polyesterdiol are preferred from the viewpoint of easy availability and excellent reactivity. When the resin-molded article is used as a polishing layer of a polishing pad described later, it is preferable that at least one is selected from the group consisting of a polyetherdiol selected from polyethylene glycol and polytetramethylene ether glycol; a polyesterdiol selected from poly(nonamethylene adipate), poly(2-methyl-1,8-octamethylene adipate), poly(2-methyl-1,8-octamethylene-co-nonamethylene adipate), poly(methylpentane adipate); and derivatives thereof from the viewpoint of excellent hydrophilicity.

[0064] The number-average molecular weight of the polyol is preferably 450 to 3,000, more preferably 500 to 2,700, even more preferably 550 to 2,400, even more preferably 650 to 1,400, and even more preferably 800 to 1,200. When the number-average molecular weight of the polyol is within the above range, a polishing layer having good properties such as rigidity, hardness, and hydrophilicity can be easily obtained, which is therefore preferable in the case of using the resin-modeled article as a polishing layer, which will be described later. Note that the number-average molecular weight of the polyol means a number-average molecular weight calculated based on the hydroxyl value measured according to JIS K 1557-1:2007. {Polyetherdiol}

[0065] Examples of the polyether diol include polyethylene glycol, polypropylene glycol, polytetramethylene ether glycol, poly(methyltetramethylene ether) glycol, and glycerin-based polyalkylene ether glycol. These can be used alone or in combination of two or more.

[0066] Among these, polyethylene glycol (PEG) and polytetramethylene ether glycol (PTMG) are preferred. {Polyesterdiol}

[0067] Examples of the polyester diol include polyester diols obtained by direct esterification or transesterification of a dicarboxylic acid or an ester-forming derivative such as its ester or anhydride and a low molecular weight diol.

[0068] Examples of the dicarboxylic acid include aliphatic dicarboxylic acids having 2 to 12 carbon atoms, such as oxalic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, dodecanedicarboxylic acid, 2-methylsuccinic acid, 2-methyladipic acid, 3-methyladipic acid, 3-methylpentanedicarboxylic acid, 2-methyloctanedioic acid, 3,8-dimethyldecanedioic acid, and 3,7-dimethyldecanedioic acid; aliphatic dicarboxylic acids such as dimerized aliphatic dicarboxylic acids (dimer acids) having 14 to 48 carbon atoms obtained by dimerizing unsaturated fatty acids obtained by fractional distillation of triglycerides, and their hydrogenated products (hydrogenated dimer acids); alicyclic dicarboxylic acids such as 2-methyldimethylammonium chloride, ... B. 1,4-cyclohexanedicarboxylic acid; and aromatic dicarboxylic acids, such as terephthalic acid, isophthalic acid, orthophthalic acid. These can be used alone or in combination of two or more.

[0069] Examples of the low molecular weight diol include aliphatic diols such as ethylene glycol, 1,3-propanediol, 1,2-propanediol, 2-methyl-1,3-propanediol, 1,4-butanediol, neopentyl glycol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 2-methyl-1,8-octanediol, 1,9-nonanediol, and 1,10-decanediol; and alicyclic diols such as cyclohexanedimethanol and cyclohexanediol. These can be used alone or in combination of two or more. Among these, diols having 6 to 12 carbon atoms are preferred, diols having 8 to 10 carbon atoms are more preferred, and diols having 9 carbon atoms are even more preferred. {Polycarbonatediol}

[0070] Examples of the polycarbonate diol include that obtained by reacting low-molecular-weight diols with carbonate compounds. Examples of the low-molecular-weight diol for producing polycarbonate diol include the low-molecular-weight diols described above.

[0071] Examples of the carbonate compounds for producing polycarbonate diol include dialkyl carbonate, alkylene carbonate and diaryl carbonate.

[0072] Examples of the dialkyl carbonate include dimethyl carbonate and diethyl carbonate, examples of the alkylene carbonate include ethylene carbonate, and examples of the diaryl carbonate include diphenyl carbonate. {polyisocyanate}

[0073] As for the polyisocyanate, it is not limited as long as it is a polyisocyanate used to produce the usual thermoplastic polyurethane, and the examples include aliphatic or alicyclic diisocyanates such as isocyanate, isocyanate, isocyanate, and the like. B. ethylene diisocyanate, tetramethylene diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, dodecamethylene diisocyanate, isophorone diisocyanate, isopropylidenebis(4-cyclohexyl isocyanate), cyclohexylmethane diisocyanate, methylcyclohexane diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, lysine diisocyanate, 2,6-diisocyanatomethyl caproate, bis(2-isocyanatoethyl) fumarate, bis(2-isocyanatoethyl) carbonate, 2-isocyanatoethyl 2,6-diisocyanatohexanoate, cyclohexylene diisocyanate, methylcyclohexylene diisocyanate and bis(2-isocyanatoethyl)-4-cyclohexene; and aromatic diisocyanates, such as B.2,4'-Diphenylmethane diisocyanate, 4,4'-diphenylmethane diisocyanate (MDI), 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, m-phenylene diisocyanate, p-phenylene diisocyanate, m-xylylene diisocyanate, p-xylylene diisocyanate, 1,5-naphthylene diisocyanate, 4,4'-diisocyanatobiphenyl, 3,3'-dimethyl-4,4'-diisocyanatobiphenyl, 3,3'-dimethyl-4,4'-diisocyanatodiphenylmethane, chlorophenylene 2,4-diisocyanate, and tetramethylxylylene diisocyanate. These can be used alone or in combination with two or more of them.

[0074] Among them, when the resin-modeled article is used for the polishing layer of the polishing pad described later, 4,4'-diphenylmethane diisocyanate (MDI) is preferable from the viewpoint of improving the abrasion resistance of the obtained polishing layer. [Chain extender]

[0075] As the chain extender, any chain extender conventionally used in the production of conventional thermoplastic polyurethane can be used. Specifically, a low-molecular-weight compound having a molecular weight of 300 or less and containing two or more active hydrogen atoms capable of reacting with the isocyanate group in one molecule is preferably used. Examples include diols such as diols, diols, and diols. Ethylene glycol, diethylene glycol (DEG), 1,2-propanediol, 1,3-propanediol, 2,2-diethyl-1,3-propanediol, 2,2,4-trimethyl-1,3-propanediol, 2-butyl-2-ethyl-1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 2,3-butanediol, 1,4-Butanediol (BD), 1,5-Pentanediol (PD), neopentyl glycol, 1,6-hexanediol, 2,5-dimethyl-2,5-hexanediol, 3-methyl-1,5-pentanediol (MPD), 1,4-bis(β-hydroxyethoxy)benzene, 1,4-cyclohexanediol, cyclohexanedimethanol (1,4-cyclohexanedimethanol etc.), Bis(β-hydroxyethyl) terephthalate, 1,9-nonanediol (ND), m-xylylene glycol,p-Xylylenglycol, Triethylenglycol; und Diamine, wie z. B. Ethylendiamin, Trimethylendiamin, Tetramethylendiamin, Hexamethylendiamin, Heptamethylendiamin, Octamethylendiamin, Nonamethylendiamin, Decamethylendiamin, Undecamethylendiamin, Dodecamethylendiamin, 2,2,4-Trimethylhexamethylendiamin, 2,4,4-Trimethylhexamethylendiamin, 3-Methylpentamethylendiamin, 1,2-Cyclohexandiamin, 1,3-Cyclohexandiamin, 1,4-Cyclohexandiamin, 1,2-Diaminopropan, 1,3-Diaminopropan, Hydrazin, Xylylendiamin, Isophorondiamin, Piperazin, o-Phenylendiamin, m-Phenylendiamin, p-Phenylendiamin, Toluylendiamin, Xyloldiamin, Adipinsäuredihydrazid, Isophthalsäuredihydrazid, 4,4'-Diaminodiphenylmethan, 4,4'-Diaminodiphenylether, 4,4'-Bis(4-amino-phenoxy)biphenyl, 4,4'-Bis(3-aminophenoxy)biphenyl, 1,4-Bis(4-aminophenoxy)benzol, 1,3-Bis(4-aminophenoxy)benzol, 1,3-Bis(3-aminophenoxy)benzol, 3,4'-Diaminodiphenylether, 4,4'-Diaminodiphenylsulfon, 3,4-Diaminodiphenylsulfon, 3,3'-Diaminodiphenylsulfon, 4,4'-methylene-bis(2-chloroaniline), 3,3'-dimethyl-4,4'-diaminobiphenyl, 4,4'-diaminodiphenyl sulfide, 2,6-diaminotoluene, 2,4-diaminochlorobenzene, 1,2-diaminoanthraquinone, 1,4-diaminoanthraquinone, 3,3'-diaminobenzophenone, 3,4-diaminobenzophenone, 4,4'-diaminobenzophenone, 4,4'-diaminobibenzyl, 2,2'-diamino-1,1'-binaphthalene, 1,n-bis(4-aminophenoxy)alkanes (n is 3 to 10), such as. Examples include 1,3-bis(4-aminophenoxy)alkane, 1,4-bis(4-aminophenoxy)alkane, 1,5-bis(4-aminophenoxy)alkane; 1,2-bis[2-(4-aminophenoxy)ethoxy]ethane, 9,9-bis(4-aminophenyl)fluorene, and 4,4'-diaminobenzanilide. These can be used alone or in combination of two or more.

[0076] Among these, at least one selected from the group consisting of 1,3-propanediol, 1,4-butanediol (BD), neopentyl glycol, 1,5-pentanediol (PD), 1,6-hexanediol and cyclohexanedimethanol is preferred.

[0077] The mixing ratio of each component of a monomer polyol used in the polymerization of the thermoplastic polyurethane, a polyisocyanate, and a chain extender is appropriately selected taking into account the desired physical properties such as abrasion resistance. For example, from the viewpoint of excellent mechanical strength, abrasion resistance, productivity, and storage stability of the thermoplastic polyurethane, the ratio of the isocyanate group contained in the polyisocyanate is preferably 0.80 to 1.30 mol, more preferably 0.85 to 1.20 mol, even more preferably 0.90 to 1.10 mol, and even more preferably 0.95 to 1.05 mol, based on 1 mol of active hydrogen atoms contained in the polyol and a chain extender.This is preferable because when the proportion is 0.80 mol or more, the mechanical properties of the resin-modeled article formed from the thermoplastic polyurethane tend to be further improved, and when it is 1.30 mol or less, the productivity and storage stability of the thermoplastic polyurethane tend to be further improved.

[0078] As for the mass ratio of polyol, polyisocyanate and chain extender, the [amount of polyol / (total amount of polyisocyanate and a chain extender)] is preferably 10 / 90 to 50 / 50, more preferably 15 / 85 to 45 / 55, even more preferably 20 / 80 to 40 / 60. [Process for producing thermoplastic polyurethane]

[0079] The thermoplastic polyurethane can be obtained by polymerizing the above-described starting materials through a urethanization reaction using the known prepolymer method or the known one-shot method. Specifically, examples include a melt polymerization method in which the above-described components are mixed in a predetermined ratio and melt-blended using a single-screw or multi-screw extruder to produce in the substantial absence of a solvent (continuous melt polymerization method); and a polymerization method to produce using a prepolymer method in the presence of a solvent.

[0080] The proportion of the nitrogen content derived from the isocyanate group of the polyisocyanate of the thermoplastic polyurethane is preferably 4.0 to 8.0 mass%, more preferably 4.5 to 7.5 mass%, even more preferably 5.0 to 7.0 mass%.

[0081] It should be noted that the nitrogen content ratio means “(mass fraction of structural units derived from polyisocyanate contained in thermoplastic polyurethane) × ((total mass of nitrogen atoms present in isocyanate groups contained in one polyisocyanate molecule) / (mass of one polyisocyanate molecule)) × 100”, and it can be measured by the methods described below.

[0082] First, the total nitrogen content is calculated by elemental analysis methods under the following conditions. - Instrument: Fully automatic elemental analyzer, Type 2400 Series II (standard equipment for automatic sampling) C•H•N•S / O analyzer, manufactured by PerkinElmer Inc. - Electric oven temperature: 975°C - Sample amount: 2 mg - Combustion improver: None - Sample container: tin foil (with combustion-supporting effect, 1 sheet is used) - Standard material for preparing a calibration curve: Sulfanilamide Next, nitrogen atoms derived from the polyisocyanate and nitrogen atoms derived from the chain extender are detected by NMR measurement under the following conditions. - Equipment: Lambda500 magnetic resonance imaging device, manufactured by JEOL Ltd. - Measurement conditions: Resonance frequency: 1H 500 MHz / probe; TH5FG2 - Solvent: DMSO-d6, concentration 5 wt% / vol. - Measuring temperature: 80 °C - Accumulation number: 64 s

[0083] Then, the proportion of nitrogen content originating from the isocyanate groups of the polyisocyanate is calculated from the results of elemental analysis and NMR. (Additive)

[0084] The resin may contain additives such as crosslinking agents, fillers, crosslinking accelerators, crosslinking aids, plasticizers, tackifiers, anti-aging agents, foaming agents, processing aids, coupling agents, inorganic fillers, organic fillers, crystal nucleating agents, heat-resistant stabilizers, weathering stabilizers, antistatic agents, colorants, lubricants, flame retardants, flame retardant aids (antimony oxide and the like), anti-blooming agents, mold release agents, thickeners, antioxidants, conductive agents, as required.

[0085] When the resin contains additives, the total content of the additives in the resin is not particularly limited, but it is preferably 50 mass% or less, more preferably 20 mass% or less, even more preferably 10 mass% or less, and even more preferably 5 mass% or less. Furthermore, when the resin contains additives, the lower limit for the total content of the additives in the resin is not particularly limited, but it is preferably, for example, 0.01 mass%.

[0086] As described above, these lower limits and upper limits, which are indicated in steps, can be combined independently. As one embodiment of the production method, for example, the total content of these additives in the resin is preferably 0.01 to 50 mass%, more preferably 0.01 to 20 mass%, even more preferably 0.01 to 10 mass%, and even more preferably 0.01 to 5 mass%. < Step M >

[0087] Step M is a step in which a melt or a precursor of a resin is discharged from a nozzle and solidified to form a sheet-shaped resin-modeled article using a 3D printer.

[0088] It is preferable that step M is a step of laminating multiple layers, wherein discharging a melt or a precursor of a resin from a nozzle and solidifying it are repeated to form a sheet-shaped resin-modeled article using a 3D printer. (3D printer)

[0089] A 3D printer is a device capable of three-dimensional modeling, using 3D printing technology that three-dimensionally shapes raw materials based on a design from three-dimensional data, such as 3D CAD or 3D CG. The 3D printer that can be used in step M is not particularly limited, as long as it is at least a device that can form a sheet-shaped resin modeled article by discharging and solidifying a melt or precursor of a resin from a nozzle.However, it is preferable to use, for example, a 3D printer that can form the sheet-shaped resin modeled article by a fused deposition modeling method (hereinafter also referred to simply as "FDM method") in which a modeled article is formed by extruding a melt or a precursor of the resin from a nozzle and laminating it layer by layer on a modeling table.

[0090] There are no particular restrictions regarding the direction in which the layers are arranged on the modeling table. For example, in the case of a rectangular resin sheet, a layer can be formed by arranging the resin one row at a time and in multiple rows. Alternatively, in the case of a disc-shaped resin sheet, for example, a layer can be formed by arranging the resin in a concentric pattern.

[0091] The 3D printer can be equipped with a single nozzle or multiple nozzles. The nozzle is not particularly limited as long as it does not impair the effects of the present invention. However, for example, a nozzle with a nozzle tip hole diameter of preferably 0.1 to 10 mm, more preferably 0.3 to 7.0 mm, and even more preferably 0.5 to 3.0 mm can be used.

[0092] Furthermore, the nozzle can discharge the melt or resin precursor while moving. The melt or resin precursor discharged from the nozzle is preferably discharged in the form of, for example, a filament or droplet, and by the nozzle movement, the melt material is placed on a modeling table provided at the lower portion of the nozzle at a position previously specified based on a design from 3D data. Then, a sheet-shaped resin modeled article is formed by placing only one layer of the resin modeled article formed by the resin on the modeling table, or by laminating the sheets layer by layer from the lower layer to the upper layer.

[0093] Furthermore, as an embodiment of step M, the resin-molded article may be formed while the nozzle remains fixed and the molding table, onto which the melt or resin precursor discharged from the nozzle is placed, is moved. Alternatively, the resin-molded article may be formed while both the nozzle and the molding table are moved.

[0094] Furthermore, in step M, from the viewpoint of preventing foreign matter from entering the obtained resin-modeled article, it is preferable that the melt or the precursor of the resin passes through a filter before being discharged from the nozzle of the 3D printer.

[0095] The filter is not particularly limited as long as it does not impair the effects of the present invention, and, for example, filters made of metal, thermoplastic resin, or thermosetting resin can be used. Among them, filters made of metal are preferred from the viewpoint of being able to be used even when the temperature of the melt or precursor of the resin is higher, and from the viewpoint of durability.

[0096] Examples of metal filters include stainless steel wire (mesh) filters.

[0097] In addition, the filtration accuracy of the filter is preferably 200 µm or less, more preferably 150 µm or less, even more preferably 100 µm or less, even more preferably 50 µm or less, even more preferably 20 µm or less, from the viewpoint of more effectively preventing foreign matter from entering the resin-modeled article.

[0098] Here, the above-mentioned “filtration accuracy of the filter” refers to the “nominal filtration accuracy”, and, for example, “filtration accuracy of 100 μm or less” means that the filter is capable of removing 95% or more of particles with a particle size of 100 μm or more.

[0099] Furthermore, the filter can be appropriately selected from the viewpoint of the type of foreign matter to be prevented from being mixed into the resin-molded article, productivity, and the like, and there is no particular limitation as long as it does not impair the effects of the present invention. However, as one embodiment of the filter, for example, it is preferable that a filter in which the vertical and horizontal mesh sizes are each independently 20 to 2800 mesh, and the vertical and horizontal wire diameters are each independently 20 to 200 μm can be used.

[0100] The filter is installed before the melt of the resin or precursor is discharged from the nozzle, and the installation location is not particularly limited as long as it does not impair the effects of the present invention. For example, the installation location of the filter is preferably in a resin inflow path in the nozzle after the resin or resin precursor is supplied to the 3D printer and before it is discharged from the nozzle, from the viewpoint of more effectively preventing foreign matter from entering the resin-modeled article, for example, to be able to remove foreign matter generated or mixed after the resin or resin precursor is melted in the 3D printer.

[0101] Furthermore, in step M, when the resin is a thermoplastic resin, the form in which the thermoplastic resin is supplied to the 3D printer is not particularly limited, but it can be in the form of powder, pellets, and strands, for example. In one embodiment of step M, it is preferred that the thermoplastic resin be supplied to the 3D printer in the form of pellets.

[0102] Furthermore, when supplying the thermoplastic resin to the 3D printer, it is preferable that dry nitrogen having a dew point temperature of -30°C or lower or dry air having a dew point temperature of -30°C or lower be supplied to the 3D printer along with the pelletized thermoplastic resin. It is preferable that by supplying the thermoplastic resin in the form of pellets using this method, it is possible to further reduce molding defects and deterioration of the physical properties of the resin-modeled articles due to foaming, cavitation, discoloration, decomposition, and the like caused by moisture absorption of the thermoplastic resin in the 3D printer, and it is also possible to more effectively prevent the intrusion of foreign matter into the resin-modeled article, for example, by suppressing the generation of foreign matter due to resin deterioration.From this point of view, the dew point temperatures of the dry nitrogen and the dry air are each independently more preferably -40°C or lower, even more preferably -50°C or lower. Further, it is preferable that the lower limit value for the dew point temperature of the dry nitrogen and the lower limit value for the dew point temperature of the dry air are each independently, for example, -100°C. As described above, these lower limit values ​​and upper limit values, which are indicated in stages, can be independently combined. For example, as one embodiment of the manufacturing method, the dew point temperatures of the dry nitrogen and the dry air are each independently preferably -100°C or higher and -30°C or lower, more preferably -100°C or higher and -40°C or lower, and even more preferably -100°C or higher and -50°C or lower.

[0103] Furthermore, from the same point of view, it is desirable to further reduce the moisture content in the thermoplastic resin, and it is preferable to perform dehumidification drying before the thermoplastic resin is supplied to a 3D printer.

[0104] The resin in step M may be a thermoplastic resin or a thermosetting resin as long as it can be molded with the 3D printer used in step M, and there is no limitation, but the thermoplastic resin is preferable.

[0105] Furthermore, when a resin precursor is used, it is converted into a resin-molded article after being discharged from a nozzle. One method for converting the resin precursor into a resin is, for example, a method for forming a resin-molded article by increasing the molecular weight of the precursor through chemical reactions such as polymerization and crosslinking reactions using light irradiation and heat curing methods.

[0106] Examples of the thermoplastic resin in the step M include those similar to the thermoplastic resins described above in the section of step P, and the thermoplastic resins may be used alone or in combination of two or more.

[0107] As one embodiment of step M, the resin in step M is preferably polyurethane, and more preferably thermoplastic polyurethane. That is, the thermoplastic resin in step M is more preferably thermoplastic polyurethane.

[0108] Examples of the thermoplastic polyurethane in the step M include those similar to the thermoplastic polyurethane described above in the section of step P, and the same applies to preferred embodiments thereof.

[0109] Furthermore, in step M, the resin can be solidified by cooling, light irradiation, heat curing, and the like. In one embodiment of step M, it is preferred that the resin is a thermoplastic resin, and the thermoplastic resin is solidified by cooling.

[0110] The cooling method is not particularly limited and may be natural cooling or forced cooling by cooling the modeling table, blowing cold air onto the resin modeled article, or the like, but natural cooling is preferred.

[0111] When the method for producing a resin film includes step M, step M is a step performed before step P as described above.

[0112] In one embodiment of the method for producing a resin film, the film-shaped resin-molded article obtained in step M may be a film-shaped resin-molded article obtained by performing step M once, or may be a film-shaped resin-molded article obtained by performing step M multiple times. When step M is performed multiple times, the film-shaped resin-molded article may be a multi-layer film-shaped resin-molded article made of different resins (a laminate formed of film-shaped resin-molded articles). Further, in this case, it may be a laminate in which a plurality of film-shaped resin-molded articles obtained in the plurality of steps M are laminated to each other via another layer, such as an adhesive layer.Further, it may be, for example, a sheet-shaped resin-modeled article obtained by continuously or discontinuously changing the type of resin or resin precursor when a sheet-shaped resin-modeled article is obtained in a step M.

[0113] Further, as an embodiment of the method for producing a resin film, the film-shaped resin-molded article obtained in the step M can be used as it is as the film-shaped resin-molded article in the step P. From the viewpoint of reducing the number of steps, it is preferable to use the film-shaped resin-molded article obtained in the step M as it is as the film-shaped resin-molded article in the step P.

[0114] Furthermore, as an embodiment of the method for producing a resin film, a laminate obtained by laminating the film-shaped resin-modeled article obtained in step M and a resin film and the like produced by another production method can be used as the film-shaped resin-modeled article in step P. In this case, the film-shaped resin-modeled article in step M can be formed by laminating it directly onto the surface of a resin film and the like produced by another production method by the method of step M. It can also be a laminate in which the film-shaped resin-modeled article obtained in step M and a resin film and the like produced by another production method are laminated via another layer such as a film.an adhesive layer, laminated together.

[0115] Furthermore, as an embodiment of the method for producing a resin film, the film-shaped resin-molded article obtained in the step M or any of the above-mentioned laminates can be used as the film-shaped resin-molded article in the step P by forming it into the desired shape by using one or more methods selected from the group consisting of cutting, machining, grinding, and punching before the step P is performed.

[0116] Further, as an embodiment of the method for producing a resin film, when the resin molded article obtained in the step M or any of the above-mentioned laminates is used as the film-shaped resin molded article in the step P, the thickness of the film-shaped resin molded article can be appropriately adjusted depending on the use of the film obtained by the step P, but it is preferably 0.5 to 15 mm, more preferably 1.0 to 10 mm, even more preferably 1.5 to 5.0 mm. < Step T >

[0117] Step T is a step in which the thickness of the compressed film obtained in step P is made thin using one or more methods selected from the group consisting of cutting, machining and grinding.

[0118] When step T is included as an embodiment of the method for producing a resin film, it is preferable because it becomes easier to adjust the thickness of the obtained resin film to a more uniform thickness.

[0119] As the above-mentioned cutting, machining and grinding methods, known methods for processing a resin-modeled article can be used. < Further steps >

[0120] An embodiment of the method for producing a resin film may include further steps in addition to the steps described above.

[0121] As further included steps, for example, there may be a step C after step P, or when step T is included, there may be step C between step P and step T. Step C is a cooling press step, which is a cooling step in which sandwiching and cooling are performed while pressure is applied between an upper and a lower flat plate having a lower temperature. When the cooling step is included, the hot press (step P) and the cool press (step C) may be performed sequentially using a hot press, or the hot press (step P) and the cool press (step C) may be performed using separate press machines. The temperature during the cool press is preferably 55°C or lower, more preferably -50 to 50°C, even more preferably 0 to 45°C, and even more preferably 10 to 40°C.The pressure during the cooling pressing is preferably 0.01 to 10 MPa, more preferably 0.05 to 5 MPa, even more preferably 0.1 to 3 MPa, even more preferably 0.2 to 1 MPa.

[0122] When the step C is included, by cooling the sheet-shaped resin-molded article heated in the step P while keeping it flat, deformation of the resin-molded article softened by heating can be prevented, and the resin-molded article does not have a high temperature, and therefore it is preferable from the viewpoint that it can be quickly conveyed to the next step. < Resin film obtained by the manufacturing process >

[0123] The thickness of the resin film (hereinafter also simply referred to as "film") obtained by the above production method can be appropriately adjusted depending on the use of the film, but, as one embodiment of the film, is preferably 0.5 to 5.0 mm, more preferably 1.0 to 3.0 mm, even more preferably 1.2 to 2.5 mm.

[0124] In one embodiment of the resin film, the storage modulus of the resin film, measured under conditions of a temperature of 21°C, a frequency of 11 Hz and a tensile condition, is preferably 250 MPa or more, more preferably 400 to 4,000 MPa, even more preferably 600 to 3,000 MPa.

[0125] In one embodiment of the resin film, the breaking stress of the resin film, measured under conditions of a temperature of 23°C, a tensile speed of 500 mm / min, is preferably 15 MPa or more, more preferably 30 to 90 MPa, even more preferably 35 to 70 MPa.

[0126] More specifically, the storage modulus and breaking stress values ​​of the resin film are measured by the method described below in the examples.

[0127] The use of the film obtained by the manufacturing process is not particularly limited, but it is preferably a polishing layer used in a polishing pad described below. That is, the resin film obtained by the manufacturing process is preferably a polishing layer for a polishing pad. [Polishing pad]

[0128] A polishing pad embodying the present invention has a polishing layer obtained by using the method for producing a resin film embodying the present invention.

[0129] As the polishing layer of the polishing pad, the film obtained by the manufacturing process may be used as it is, or a film obtained by further processing the film obtained by the manufacturing process into a desired film shape using one or more methods selected from the group consisting of cutting, machining, grinding, and punching may be used.

[0130] Furthermore, the polishing layer is more preferably a polishing layer formed using the above-mentioned thermoplastic polyurethane as a resin, and can be either a foamed or non-foamed material of the thermoplastic polyurethane, but is even more preferably a non-foamed material. When the polishing layer is a non-foamed material of the thermoplastic polyurethane, the polishing uniformity of the polishing pad having the polishing layer becomes high, and it is also possible to suppress the variation due to foam distribution and the occurrence of defects caused by aggregates in the foam formation, thereby achieving stable polishing in which the polishing properties are less susceptible to fluctuation.

[0131] Furthermore, the density of the polishing layer formed using the thermoplastic polyurethane is preferably 0.75 g / cm3 or more, more preferably 0.85 g / cm 3 or more, more preferably 1.0 g / cm 3 or more, even more preferably 1.1 g / cm 3 or more. When the density is equal to or greater than the above-described lower limit, the polishing layer exhibits suitable flexibility. Furthermore, the upper limit of the density is not particularly limited, but is preferably 1.3 g / cm, for example. 3 As described above, these lower and upper limits, which are indicated in steps, can be combined independently. For example, as one embodiment of the polishing layer, the density of the polishing layer is preferably 0.75 to 1.3 g / cm 3 , more preferably 0.85 to 1.3 g / cm 3 , more preferably 1.0 to 1.3 g / cm 3 , even more preferably 1.1 to 1.3 g / cm 3 .

[0132] Further, it is preferable that the polishing layer formed using the thermoplastic polyurethane is a polishing layer formed using a non-foamed thermoplastic polyurethane from the viewpoint of its excellent polishing stability due to its higher rigidity and the uniformity of the material.

[0133] The shape of the polishing layer is not particularly limited, and examples include a circular shape in plan view. As described above, when manufacturing by the resin sheet manufacturing method and designing in advance based on 3D data, the shape of the polishing layer can be formed directly during formation with a 3D printer, for example, by considering the compression ratio in step P. Alternatively, as described above, the resin-modeled article obtained by the manufacturing method can be further appropriately manufactured by one or more processing types selected from the group consisting of cutting, machining, grinding, and punching, or the like.

[0134] The thickness of the polishing layer is not particularly limited, but is preferably 0.5 to 5.0 mm, more preferably 1.0 to 3.0 mm, and even more preferably 1.2 to 2.5 mm. When the thickness of the polishing layer is within the above-described range, it is preferable because productivity and handling properties are improved, and the stability of the polishing properties is also improved.

[0135] Further, it is preferable that recesses such as grooves and holes be formed on the polishing surface of the polishing layer in a predetermined pattern such as concentric, lattice, spiral, and radial patterns. Such recesses supply a slurry evenly and sufficiently to the polishing surface and are useful for discharging polishing residues that cause scratches and preventing damage to a wafer by adsorption of the polishing layer. For example, when a groove is formed in the shape of a concentric circle, the pitch between the grooves is preferably 1.0 to 50 mm, more preferably 1.5 to 30 mm, even more preferably 2.0 to 15 mm. Furthermore, the width of the groove is preferably 0.1 to 3.0 mm, more preferably 0.2 to 2.0 mm.Furthermore, the depth of the groove is less than the thickness of the polishing layer and is preferably 0.2 to 1.8 mm, more preferably 0.4 to 1.5 mm. Furthermore, the cross-sectional shape of the groove is suitably selected from, for example, a rectangle, a trapezoid, a triangle, and a semicircle, depending on the intended use.

[0136] The recesses on the polishing surface can be formed directly during formation with a 3D printer by designing them in advance from 3D data when manufacturing with the resin sheet manufacturing method. Alternatively, the recesses can be formed by methods such as grinding, laser machining, transfer using a mold, and the like, and embossing with a heated mold on the resin-molded article obtained by the resin-molded article manufacturing method.

[0137] The hardness of the polishing layer is such that the D hardness value measured according to JIS K 7311:1995 is preferably 45 or more, more preferably 50 or more, even more preferably 55 or more, and preferably 90 or less, more preferably 85 or less, even more preferably 80 or less. As described above, these lower and upper limits, which are indicated in stages, can be combined independently. For example, as one embodiment of the polishing layer, the D hardness value of the polishing layer is preferably 45 to 90, more preferably 50 to 85, even more preferably 55 to 80. In one embodiment of the polishing layer, the wear rate of the polishing layer, which is evaluated by the method described in the examples below, is preferably 100 µm / h or less, more preferably 90 µm / h or less, even more preferably 75 µm / h, even more preferably 60 µm / h or less.Furthermore, the lower limit of the wear rate is not particularly limited, but is preferably 10 µm / h, for example.

[0138] As described above, these lower and upper limits, which are indicated in steps, can be combined independently. For example, as one embodiment of the polishing layer, the wear rate of the polishing layer is preferably 10 to 100 µm / h, more preferably 10 to 90 µm / h, even more preferably 10 to 75 µm / h, and even more preferably 10 to 60 µm / h.

[0139] The polishing pad may consist only of the polishing layer obtained by the method for producing a resin film which is an embodiment of the present invention, or may be a laminate in which a cushion layer is laminated on the surface other than the polishing surface of the polishing layer.

[0140] The cushion layer preferably has a hardness lower than that of the polishing layer. If the hardness of the cushion layer is lower than the hardness of the polishing layer, this is preferable because the stiff polishing layer follows local asperities on the surface to be polished, and the cushion layer makes it easier to follow the curvature and warpage of the entire substrate to be polished. Therefore, polishing with an excellent balance between global planarity (a state in which the asperity of a wafer substrate is reduced with long cycles) and local planarity (a state in which local asperities are reduced) can be achieved.

[0141] The thickness of the cushioning layer is not particularly limited, but is preferably 0.3 to 5.0 mm, for example.

[0142] Examples of materials used as the cushioning layer include composites of polyurethane-impregnated nonwoven fabric (e.g., "Suba (registered trademark) 400" (manufactured by Nitta Haas Incorporated.)); rubbers such as natural rubber, nitrile rubber, polybutadiene rubber, and silicone rubber; thermoplastic elastomers such as polyester-based thermoplastic elastomers, polyamide-based thermoplastic elastomers, and fluorine-based thermoplastic elastomers; foams; and polyurethane.

[0143] Among them, the polyurethane with a foamed structure is particularly preferred because the appropriate flexibility for the cushioning layer can be easily achieved.

[0144] It should be noted that the polyurethane in the description regarding the cushioning layer includes both thermoplastic polyurethane and thermosetting polyurethane.

[0145] The polishing layer and the cushion layer can be laminated together, for example, with double-sided adhesive tape or can be laminated together via an adhesive layer. Furthermore, when the polishing layer is formed by the method for manufacturing a resin-molded article, it can be laminated by a method in which all or part of the polishing layer is formed directly on the cushion layer or another intermediate layer (for example, an adhesive layer).

[0146] Since the polishing pad has a polishing layer obtained using the resin-molded article manufacturing method, the abrasion resistance of the polishing layer can be improved. Therefore, by using a polishing pad with a polishing layer obtained using the resin-molded article manufacturing method, it is possible to contribute to extending the service life of the polishing pad.

[0147] Accordingly, it can be suitably used, for example, as a polishing pad used in a polishing method for planarizing the surface of a semiconductor wafer, and it can be even more suitably used as a polishing pad for planarizing the surface of a semiconductor wafer by a CMP (Chemical Mechanical Polishing (Planarization)) polishing method. Note that CMP is a method for polishing an object to be polished with high precision, which uses a polishing pad while supplying a slurry containing abrasive grains and a reaction solution to the surface of the object to be polished, and is known as a method suitable for polishing semiconductor materials and the like, such as silicon wafers. Example

[0148] Next, the present invention will be described in more detail by way of examples, but the present invention is not limited to these examples.

[0149] Each component used in examples or comparative examples is described below with abbreviations. [Production example 1]

[0150] Polytetramethylene ether glycol (PTMG) with a number-average molecular weight of 850, 1,4-butanediol (BD), and 4,4'-diphenylmethane diisocyanate (MDI) were used in a ratio of PTMG:BD:MDI = 32.5:15.6:51.9 (mass ratio) and continuously fed by a metering pump into a coaxially rotating twin-screw extruder to conduct continuous melt polymerization and produce thermoplastic polyurethane. Then, the melt of the polymerized thermoplastic polyurethane was continuously extruded into water in the form of a strand and then crushed by a pelletizer to obtain thermoplastic polyurethane pellets. The pellets were dehumidified and dried at 70°C for 20 hours and then sealed in a moisture-proof bag. [Example 1]

[0151] In a fused deposition modeling 3D printer, a stainless steel wire mesh with a filtration accuracy of 70 μm (plain Dutch weave, vertical mesh size 50, horizontal mesh size 250, vertical wire diameter 140 μm, horizontal wire diameter 110 μm) was installed in the resin flow path in a nozzle (tip hole diameter 1 mm). The thermoplastic polyurethane pellets obtained in Preparation Example 1 were supplied together with dry air with a dew point temperature of -60 °C and formed into a disc shape with a diameter of 40 cm in a concentric pattern. Five layers were laminated on it in the same way (a total of six layers) to obtain a disc-shaped film with a thickness of 3 mm and a diameter of 40 cm.

[0152] Next, a pressure of 3 MPa was uniformly applied from above to the film surface under a reduced pressure atmosphere with a vacuum degree of 3 kPa using a vacuum hot press (i.e., uniformly applied in the thickness direction of the disc-shaped film and in the lamination direction when the disc-shaped film is formed by the 3D printer), and the film was processed at 140 °C for 2 min to obtain a compressed film. The product of the pressure (p) [MPa] and the time (t) [seconds] in this step is 360.

[0153] Then, by grinding the surface of the resulting compressed film, a disc-shaped film with a thickness of 1.5 mm and a disc-shaped film with a thickness of 500 µm were obtained. The storage modulus, stress at break, and elongation at break of the film with a thickness of 500 µm, measured using the method described below, were 713 MPa, 50 MPa, and 315%, respectively. The results are shown in Table 1 below.

[0154] Furthermore, after cutting out the film with a thickness of 1.5 mm and a diameter of 38 cm, spiral grooves with a width of 1.0 mm, a depth of 0.8 mm, and a pitch of 3.5 mm were formed on the polishing surface. Next, double-sided tape ("#5605HG", manufactured by Sekisui Chemical Co., Ltd.) was attached to the back side, which is the side opposite the polishing surface, to prepare a polishing pad. The wear rate of this polishing pad was evaluated using the method described below and was found to be 58 µm / h. The results are shown in Table 1 below. [Example 2]

[0155] In the same manner as in Example 1, the thermoplastic polyurethane pellets obtained in Production Example 1 were fed into a 3D printer to obtain a disc-shaped film with a thickness of 3 mm and a diameter of 40 cm. Next, a pressure of 0.5 MPa was uniformly applied from above to the film surface of the disc-shaped film under an atmospheric pressure atmosphere using a heat press, and the treatment was carried out at 120 °C for 1 h to obtain a compressed film. The product of the pressure (p) [MPa] and the time (t) [seconds] in this step is 1800.

[0156] Then, by grinding the surface of the resulting compressed film, a disc-shaped film with a thickness of 1.5 mm and a disc-shaped film with a thickness of 500 µm were obtained. The storage modulus, stress at break, and elongation at break of the film with a thickness of 500 µm, measured using the method described below, were 691 MPa, 43 MPa, and 216%, respectively. The results are shown in Table 1 below.

[0157] Furthermore, a 1.5 mm thick film polishing pad was prepared in the same manner as in Example 1, and the wear rate was measured, which was found to be 64 µm / h. The results are shown in Table 1 below. [Example 3]

[0158] In the same manner as in Example 1, the thermoplastic polyurethane pellets obtained in Production Example 1 were fed into a 3D printer to obtain a disc-shaped sheet with a thickness of 3 mm and a diameter of 40 cm. Next, a spacer made of polytetrafluoroethylene with a thickness of 2.5 mm was placed as the outer frame of the disc-shaped sheet, and a pressure of 3 MPa was evenly applied from above to the film surface of the disc-shaped sheet under a reduced pressure atmosphere with a vacuum degree of 3 kPa using a vacuum heat press, and the treatment was carried out at 160° for 30 seconds to obtain a compressed sheet. The product of the pressure (p) [MPa] and the time (t) [seconds] in this step is 90.

[0159] Then, by grinding the surface of the resulting compressed film, a disc-shaped film with a thickness of 1.5 mm and a disc-shaped film with a thickness of 500 µm were obtained. The storage modulus, ultimate stress, and ultimate elongation of the film with a thickness of 500 µm, measured using the method described below, were 729 MPa, 56 MPa, and 323%, respectively. The results are shown in Table 1 below.

[0160] Furthermore, in the same manner as in Example 1, a polishing pad was made from the film with a thickness of 1.5 mm and the abrasion rate was measured, which was found to be 55 µm / h.

[0161] The results are shown in Table 1 below. [Example 4]

[0162] In the same manner as in Example 1, the thermoplastic polyurethane pellets obtained in Production Example 1 were fed into a 3D printer to obtain a disc-shaped sheet with a thickness of 3 mm and a diameter of 40 cm. Next, a pressure of 7 MPa was evenly applied from above to the film surface of the disc-shaped sheet under an atmospheric pressure atmosphere using a heat press, and the treatment was carried out at 100°C for 10 minutes to obtain a compressed sheet. The product of the pressure (p) [MPa] and the time (t) [seconds] in this step is 4200.

[0163] Then, by grinding the surface of the resulting compressed film, a disc-shaped film with a thickness of 1.5 mm and a disc-shaped film with a thickness of 500 µm were obtained. The storage modulus, ultimate stress, and ultimate elongation of the film with a thickness of 500 µm, measured using the method described below, were 688 MPa, 42 MPa, and 240%, respectively. The results are shown in Table 1 below.

[0164] Furthermore, a polishing pad was fabricated from the foil with a thickness of 1.5 mm in the same manner as in Example 1, and the wear rate was measured, which was found to be 71 µm / h. The results are shown in Table 1 below. [Example 5]

[0165] In the same manner as in Example 1, the thermoplastic polyurethane pellets obtained in Production Example 1 were fed into a 3D printer to obtain a disc-shaped sheet with a thickness of 3 mm and a diameter of 40 cm. Next, a spacer made of polytetrafluoroethylene with a thickness of 2.5 mm was placed as the outer frame of the disc-shaped sheet, and a pressure of 1 MPa was evenly applied from above to the film surface of the disc-shaped sheet under a reduced pressure atmosphere with a vacuum degree of 3 kPa using a vacuum heat press, and the treatment was carried out at 180 °C for 15 seconds to obtain a compressed sheet. The product of the pressure (p) [MPa] and the time (t) [seconds] in this step is 15.

[0166] Then, by grinding the surface of the resulting compressed film, a disc-shaped film with a thickness of 1.5 mm and a disc-shaped film with a thickness of 500 µm were obtained. The storage modulus, stress at break, and elongation at break of the film with a thickness of 500 µm, measured using the method described below, were 725 MPa, 54 MPa, and 314%, respectively. The results are shown in Table 1 below.

[0167] Furthermore, a polishing pad was made from the film with a thickness of 1.5 mm in the same manner as in Example 1, and the abrasion rate was measured, which was found to be 57 µm / h. The results are shown in Table 1 below. [Example 6]

[0168] In the same manner as in Example 1, the thermoplastic polyurethane pellets obtained in Production Example 1 were fed into a 3D printer to obtain a disc-shaped sheet with a thickness of 3 mm and a diameter of 40 cm. Next, a pressure of 3 MPa was evenly applied from above to the film surface of the disc-shaped sheet under a reduced pressure atmosphere with a vacuum degree of 3 kPa using a vacuum heat press, and the treatment was carried out at 140 °C for 3 seconds to obtain a compressed sheet. The product of the pressure (p) [MPa] and the time (t) [seconds] in this step is 9.

[0169] Then, by grinding the surface of the resulting compressed film, a disc-shaped film with a thickness of 1.5 mm and a disc-shaped film with a thickness of 500 µm were obtained. The storage modulus, ultimate stress, and ultimate elongation of the film with a thickness of 500 µm, measured using the method described below, were 552 MPa, 33 MPa, and 169%, respectively. The results are shown in Table 1 below.

[0170] Furthermore, a polishing pad was fabricated from the foil with a thickness of 1.5 mm in the same manner as in Example 1, and the wear rate was measured, which was found to be 94 µm / h. The results are shown in Table 1 below. [Comparison example 1]

[0171] In the same manner as in Example 1, the pellets of thermoplastic polyurethane components obtained in Preparation Example 1 were fed into a 3D printer to obtain a disc-shaped film having a thickness of 3 mm and a diameter of 40 cm.

[0172] Next, it was treated in a vacuum dryer at 120 °C for 1 hour under a reduced pressure atmosphere with a vacuum level of 3 kPa. No pressure was applied during this step.

[0173] Then, by grinding the surface of the film after heat treatment, a disc-shaped film with a thickness of 1.5 mm and a disc-shaped film with a thickness of 500 µm were obtained. The storage modulus, ultimate stress, and ultimate elongation of the film with a thickness of 500 µm, measured using the method described below, were 369 MPa, 26 MPa, and 140%, respectively. The results are shown in Table 1 below.

[0174] Furthermore, a polishing pad was made from the foil with a thickness of 1.5 mm in the same manner as in Example 1, and the wear rate was measured, which was found to be 103 µm / h. The results are shown in Table 1 below. [Comparison example 2]

[0175] In the same manner as in Example 1, the pellets of thermoplastic polyurethane components obtained in Preparation Example 1 were fed into a 3D printer to obtain a disc-shaped film having a thickness of 3 mm and a diameter of 40 cm.

[0176] Next, a pressure of 7 MPa was uniformly applied from above to the film surface of the disc-shaped film under an atmospheric pressure atmosphere using a heat press, and the treatment was carried out at room temperature (23 °C) for 1 hour. The product of pressure (p) [MPa] and time (t) [seconds] in this step is 25,200. Note that no heat was applied in this step.

[0177] Then, by grinding the surface of the film after pressure treatment, a disc-shaped film with a thickness of 1.5 mm and a disc-shaped film with a thickness of 500 µm were obtained. The storage modulus, stress at break, and elongation at break of the film with a thickness of 500 µm, measured using the method described below, were 273 MPa, 12 MPa, and 9%, respectively. The results are shown in Table 1 below.

[0178] Furthermore, a polishing pad was fabricated from the foil with a thickness of 1.5 mm in the same manner as in Example 1, and the wear rate was measured, which was found to be 158 µm / h. The results are shown in Table 1 below. [Comparison example 3]

[0179] In the same manner as in Example 1, the pellets of thermoplastic polyurethane components obtained in Preparation Example 1 were fed into a 3D printer to obtain a disc-shaped film having a thickness of 3 mm and a diameter of 40 cm.

[0180] Then, by grinding the surface of the disc-shaped film, a disc-shaped film with a thickness of 1.5 mm and a disc-shaped film with a thickness of 500 µm were obtained. The storage modulus, ultimate stress, and ultimate elongation of the 500 µm-thick film, measured using the method described below, were 242 MPa, 11 MPa, and 12%, respectively. The results are shown in Table 1 below.

[0181] Furthermore, a polishing pad was fabricated from the foil with a thickness of 1.5 mm in the same manner as in Example 1, and the wear rate was measured, which was found to be 166 µm / h. The results are shown in Table 1 below. [Comparison example 4]

[0182] In the same manner as in Example 1, the pellets of thermoplastic polyurethane components obtained in Preparation Example 1 were fed into a 3D printer to obtain a disc-shaped film having a thickness of 3 mm and a diameter of 40 cm.

[0183] Next, a pressure of 3 MPa was uniformly applied from above to the film surface of the disc-shaped film under a reduced pressure atmosphere with a vacuum degree of 3 kPa using a vacuum heat press, and the treatment was carried out at room temperature (23 °C) for 2 minutes. The product of pressure (p) [MPa] and time (t) [seconds] in this step is 360. Note that no heat was applied in this step.

[0184] Then, by grinding the surface of the film after pressure treatment, a disc-shaped film with a thickness of 1.5 mm and a disc-shaped film with a thickness of 500 µm were obtained. The storage modulus, stress at break, and elongation at break of the film with a thickness of 500 µm, measured using the method described below, were 250 MPa, 12 MPa, and 11%, respectively. The results are shown in Table 1 below.

[0185] Furthermore, a polishing pad was fabricated from the foil with a thickness of 1.5 mm in the same manner as in Example 1, and the wear rate was measured, which was found to be 163 µm / h. The results are shown in Table 1 below. < Storage modulus of the resin film >

[0186] A test specimen with a width of 5 mm and a length of 30 mm was cut from the disc-shaped film with a thickness of 500 μm obtained in Examples and Comparative Examples, such that the tensile direction was perpendicular to the pattern formed by the 3D printer as the radial direction of the disc. Then, the test specimen was measured using a dynamic viscoelasticity measuring device ("DVE Rheo Spectral", manufactured by Rheology Co., Ltd.) at a temperature of 21 °C, a frequency of 11 Hz, and a tensile condition to determine the storage modulus. Note that as a reference, Fig. Figure 4 is a schematic plan view illustrating the outline of the disc-shaped film and the test specimen used in the storage modulus measurement. Cutting out a test specimen means the radial direction of the disc, as shown in Fig. 4, for a disc-shaped film 30, cutting out a test specimen 32 in the radial direction of the disc-shaped film 30 so that it is perpendicular to a formed pattern 31 when a disc-shaped film is formed by a 3D printer. Fig. Figure 4 is a schematic plan view illustrating the meaning and outline of the radial direction of the film corresponding to the cutting out of the test piece, where the distance from the center of the disc to the point where the test piece is cut out need not be as shown in Fig. 4 shown. < Breaking stress and breaking strain of the resin film >

[0187] A dumbbell-shaped test specimen No. 3 (40 mm between the marked lines) was prepared by cutting it from the 500 μm thick disc-shaped film obtained in Examples and Comparative Examples, such that the tensile direction was perpendicular to the pattern formed by the 3D printer, rather than the radial direction of the disc. Then, using a tensile tester "3367" manufactured by Instron, a tensile test was conducted under conditions of a temperature of 23°C and a tensile speed of 500 mm / min to determine the ultimate stress and ultimate elongation. Note that the average value of 5 or more points was used. < Abrasion resistance (wear rate of the polishing pad (polishing layer)) >

[0188] The polishing pads obtained in Examples and Comparative Examples were attached to a polishing plate surface of a BC-15 polishing machine manufactured by MAT Inc. Then, under conditions including a dresser rotation speed of 49 rpm, a polishing pad rotation speed of 50 rpm, and a dresser load of 25 N, the surface of the polishing pad (polishing surface of the polishing layer) was conditioned with a diamond dresser for 2 hours while pure water flowed at a rate of 150 ml / min. A dresser manufactured by Asahi Diamond Industrial Co., Ltd. (diamond number No. 100, irregular diamond shape, base metal diameter 100 mm) was used as the dresser.The depth of the groove before and after conditioning was measured at a point 100 mm from the center of the polishing pad in the radial direction of the wheel, and the wear rate of the polishing layer of the polishing pad was measured.

[0189] From Examples 1 to 6 and Comparative Examples 1 to 4, it was found that by applying pressure under heating after forming a sheet-shaped resin modeled article using a 3D printer, the storage modulus, breaking stress, and breaking elongation of the obtained resin film were improved.

[0190] Furthermore, it was found that when the resin films obtained in Examples 1 to 6 were used as the polishing layer of the polishing pad, the abrasion resistance was significantly improved because the wear rate was lower than that of the resin films obtained in Comparative Examples 1 to 4. Therefore, it was found that the polishing pads using the resin films obtained in Examples 1 to 6 as the polishing layer had improved abrasion resistance of the polishing layer and had a longer service life.

[0191] On the other hand, in Comparative Example 1 in which only heating was applied and in Comparative Examples 2 and 4 in which only pressure was applied, it was found that the physical properties of the obtained resin film were insufficiently improved or hardly improved.

[0192] It is believed that if only heat treatment is performed on a resin film obtained by a 3D printer, it can be seen, for example, from the schematic cross-sectional representation in Fig. 2, by improving the mobility of the polymer molecules, it is expected that the fusion is improved due to the increase in the movement and entanglement of the polymer molecules at the contact surfaces 11a between the resin blocks 11, but the extent of improvement in the contact area is insufficient and the effect of improving the mechanical properties is limited.

[0193] Furthermore, it is assumed, for example, that if only one printing treatment is carried out on a resin film obtained by a 3D printer, for example, based on the schematic cross-sectional representation in Fig.2, deformation of the resin block 11 is less likely to occur, and even if it occurs, the fusion of the resin blocks 11 at the contact surface 11a is insufficient, and there will be only a slight increase in the movement and entanglement of the polymer molecules between the resin blocks, resulting in the failure to achieve the effect of improving the mechanical properties. Industrial applicability

[0194] By using the resin film manufacturing method, the mechanical properties of a resin film obtained using a 3D printer can be significantly improved.

[0195] Therefore, when using a resin film obtained using a 3D printer, it is possible to obtain a resin film with further improved mechanical properties, depending on the application. Furthermore, by using the above-described method for producing a resin film, the mechanical properties of the resin film itself are improved, making it possible to use it in applications where it was previously not possible to use the resin film obtained using a 3D printer and which require higher modulus, higher strength, and higher elongation.

[0196] Moreover, since the resin film obtained by using the above method for producing a resin film has significantly improved abrasion resistance, for example, by using a polishing pad having a polishing layer obtained by using the above-described method for producing a resin film, the abrasion resistance of the polishing layer can be improved, which contributes to a longer life of the polishing pad. List of reference symbols 1 Melt of the resin or precursor of the resin 2 nozzle of the 3D printer 3 modeling table 10 Foil-shaped resin modeled object formed by a 3D printer 11 resin block 11a Contact surface of the resin blocks 12 Cavity 20 Compressed film obtained by step P A First layer, formed by a 3D printer B Second layer, formed by a 3D printer C Third layer, formed by a 3D printer P Direction in which pressure was applied during heating in step P 30 Disc-shaped foil used to measure the storage modulus 31 Pattern formed when the disc-shaped film is formed by a 3D printer 32 test specimens, cut out for the memory module test QUOTES CONTAINED IN THE DESCRIPTION

[0000] This list of documents submitted by the applicant was generated automatically and is included solely for the convenience of the reader. This list is not part of the German patent or utility model application. The DPMA assumes no liability for any errors or omissions. Cited patent literature

[0000] JP 2008-507417 A

[0008] JP 2015-517922 A

[0008] JP 2016-536151 A

[0008] JP 2021-523025 A

[0008]

Claims

[1] A method for producing a resin film, comprising at least the following step P, Step P: a step of applying pressure (p) to a sheet-shaped resin modeled article formed by a 3D printer while heating it, and deforming the sheet-shaped resin modeled article to obtain a compressed film. [2] The method for producing a resin film according to claim 1, wherein the heating temperature in the step P is 80 °C or more. [3] The method for producing a resin film according to claim 1 or 2, wherein the pressure (p) in the step P is 0.1 MPa or more. [4] The method for producing a resin film according to any one of claims 1 to 3, wherein a spacer is used in the step P. [5] The method for producing a resin film according to any one of claims 1 to 4, wherein the product of the pressure (p) and the time (t) for applying the pressure (p) in the step P satisfies the following formula (i); Formula (i): 5 ≤ p × t ≤ 5000 [a unit of p is MPa, a unit of t is second]. [6] The method for producing a resin film according to any one of claims 1 to 5, wherein the step P is carried out under a reduced pressure atmosphere. [7] The method for producing a resin film according to any one of claims 1 to 6, wherein the resin molded article in the step P is a polyurethane molded article. [8] The method for producing a resin film according to any one of claims 1 to 7, further comprising the following step M before the step P, step M: using a 3D printer, a step of discharging a melt or a precursor of a resin from a nozzle and solidifying it to form a film-shaped resin modeled article. [9] The method for producing a resin film according to claim 8, wherein the melt or the resin precursor in step M passes through a filter before being discharged from the nozzle of the 3D printer. [10] The method for producing a resin film according to claim 8 or 9, wherein the resin is a thermoplastic resin and the solidification of the thermoplastic resin in the step M is carried out by cooling. [11] The method for producing a resin film according to claim 10, wherein the thermoplastic resin in the step M is a thermoplastic polyurethane. [12] The method for producing a resin film according to any one of claims 1 to 11, further comprising the following step T after the step P, step T: a step of making a thickness of the compressed film obtained in the step P thin by using one or more methods selected from the group consisting of cutting, machining and grinding. [13] The method for producing a resin film according to any one of claims 1 to 12, wherein the resin film is a polishing layer for a polishing pad. [14] A polishing pad comprising a polishing layer obtained by using the method for producing a resin film according to claim 13.

Citation Information

Patent Citations

  • A method for generating in-situ grooves in chemical-mechanical planarization (cmp) pads and novel cmppad designs

    JP2008507417A

  • Printed chemical mechanical polishing pads

    JP2015517922A

  • Printed chemical mechanical polishing pad having abrasive therein

    JP2016536151A

  • Chemical mechanical polishing pad with adjustable hydrophilicity and zeta potential