Coated pigments for coloring PVC

DE502013016542D1Inactive Publication Date: 2024-10-02LANXESS DEUTSCHLAND GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502013016542
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2012-12-13
Filing Date
2013-12-13
Publication Date
2024-10-02
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

PVC products colored with existing inorganic pigments like iron oxides and ferrites often experience undesirable homogeneous or inhomogeneous discoloration, especially in outdoor applications, and lack sufficient thermal stability.

Method used

Coated pigments with inorganic pigments such as iron oxides, iron oxide hydroxides, zinc ferrites, magnesium ferrites, and manganese ferrites, where the pigments are coated with hydroxides and/or oxides of magnesium and/or calcium, providing a specific weight percentage range to enhance thermal stability and prevent discoloration.

Benefits of technology

The coated pigments significantly improve the thermal stability of PVC products, as demonstrated by increased resistance to degradation during thermal treatment and UV exposure, maintaining color consistency and performance in various environmental conditions.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to coated pigments comprising at least one inorganic pigment from the group of iron oxides, iron oxide hydroxides, zinc, magnesium or manganese ferrites, which are provided with a coating comprising hydroxides and / or oxides of magnesium and / or calcium, processes for their preparation, their use for coloring polyvinyl chloride (PVC) and processes for coloring PVC and PVC colored with such coated pigments, as well as plastic products comprising such coated pigments.

[0002] PVC is primarily used as a raw material in the construction sector, for example, for window profiles, pipes, flooring, and roofing membranes. Rigid and flexible films are also made from PVC. PVC is also often used as insulation material for electrical cables, electrical switch boxes, cable pull-in tubes, cable ducts, and cable covers.

[0003] PVC belongs to the group of amorphous thermoplastics. The plastic is typically hard and brittle and is usually adapted for different applications by adding plasticizers and stabilizers.

[0004] PVC is typically used with varying plasticizer contents. PVC with a plasticizer content of 0 to 12% is also called rigid PVC. PVC with a plasticizer content of more than 12% is also called soft PVC (Römpp Chemical Encyclopedia, online version 3.28, article last updated: December 2009, document ID: RD-16-03650). Plasticizer contents are usually given as a percentage by weight.

[0005] PVC is often colored with organic and inorganic pigments. Examples of organic pigments used include isoindoles, naphthol AS, copper phthalocyanine pigments, or monoazo calcium salts. Mixed-phase metal oxide pigments such as nickel rutile pigments, chromium rutile pigments, iron chromites, inverse cobalt or copper spinels, or iron cobalt chromite spinels are frequently used. These pigments are highly weather- and light-stable, but have the disadvantage of being several times more expensive than other iron-containing inorganic pigments.

[0006] The coloring of PVC with inorganic pigments such as iron oxides or iron oxide hydroxides, zinc, magnesium, or manganese ferrites is also known. Iron oxides and iron oxide hydroxides are characterized by being particularly lightfast pigments that maintain a consistent color over time, even under a wide range of weather conditions. However, when coloring PVC with iron oxides or iron oxide hydroxides, zinc, magnesium, or manganese ferrites using state-of-the-art technology, homogeneous or inhomogeneous discoloration of the product can occur, both during processing at the required high temperatures and when the molded plastic is exposed to light, UV light, or heat. This undesirable phenomenon is significantly more serious with rigid PVC, as rigid PVC products are frequently used in outdoor areas where weather-related influences are naturally more intense.Such discoloration also occasionally occurs in soft PVC products, which are primarily used indoors, for example, shortly after processing. These negative effects have been known for a long time and are described, for example, in SS Lele, J. Vinyl Tech. 1984, Vol. 6, No. 2, pp. 77 to 81, or P. Carty et al., Polymer 1992, Vol. 33, No. 13, pp. 2704-2708.

[0007] EP 799865-A2 describes coated pigments consisting of a core consisting of iron oxide and titanium dioxide and an outer coating containing oxides of magnesium and / or calcium.

[0008] DE 3539306 A1 describes heat-resistant yellow pigments coated with aluminum phosphate hydroxides of the general formula [AlO] x PO 4 [OH] x-3 for coloring thermoplastics. However, our own tests have shown that PVC colored with these coated pigments does not exhibit sufficiently higher thermal stability than PVC colored with the uncoated pigment. Our own tests have also shown that PVC colored with iron oxides coated with other inorganic aluminum compounds, e.g., aluminum oxide, aluminum hydroxide, or magnesium phosphate, also does not exhibit higher thermal stability than PVC colored with uncoated iron oxides.Therefore, the object of the present invention was to provide inorganic pigments from the group of iron oxides, iron oxide hydroxides, zinc ferrites, magnesium ferrites and / or manganese ferrites which do not lead to undesired homogeneous or inhomogeneous discolorations of the PVC colored therewith, both in the form of plastic products and products made therefrom.

[0009] EP262503 A2 describes iron oxide pigments which have a coating consisting of compounds of one or more of the group Mg, Ca, Al and / or Zn, wherein the specifically coated pigments each have a Mg content of less than 3 wt.% or a Ca content of less than 5 wt.%, based on the total weight of the coated pigment.

[0010] Surprisingly, it has now been found that coated pigments comprising at least one inorganic pigment from the group consisting of iron oxides, iron oxide hydroxides, zinc ferrites, magnesium ferrites and / or manganese ferrites, wherein the at least one inorganic pigment is provided with a coating comprising hydroxides and / or oxides of magnesium and / or calcium, wherein the coated pigment contains from 3.1 to 30 wt.% magnesium or from 5.0 to 30 wt.% calcium, based on the total weight of the coated pigment, achieve this object and overcome the above-described disadvantages of the pigments of the prior art.

[0011] As iron oxides, the coated pigments according to the invention contain, for example, hematite (iron oxide red, α-Fe 2 O 3 ), maghemite (brown iron oxide, γ-Fe 2 O 3 ) or magnetite (iron oxide black, Fe 3 O 4 ), preferably hematite (iron oxide red, α-Fe 2 O 3 ).

[0012] From the group of iron oxide hydroxides, the coated pigments according to the invention contain, for example, goethite (iron oxide yellow, α-FeOOH) or lepidocrocite (γ-FeOOH).

[0013] Zinc ferrites, magnesium ferrites, and / or manganese ferrites belong to the group of mixed-phase pigments of the general formula M x Fe 3-x O 4 , where M stands for Zn, Mg, or Mn, and x comprises values ​​greater than 0 and less than or equal to 1. The coated pigment according to the invention can also contain one or more different from the aforementioned mixed-phase pigments. Preferably, the coated pigment according to the invention contains only one inorganic pigment.

[0014] The coated pigments according to the invention are coated with hydroxides and / or oxides of magnesium and / or calcium. Coated, in the context of the present invention, means that the surface of a core composed of the inorganic pigment is directly bonded to a surrounding layer of hydroxides and / or oxides of magnesium and / or calcium. The coating can be detected, for example, via electron micrographs of the pigments.

[0015] In addition to the first coating of hydroxides and / or oxides of magnesium and / or calcium, the coated pigments according to the invention may or may not be provided with at least one further coating, either an organic coating, preferably an organic coating of oils and / or waxes and / or fatty acid salts, or an inorganic coating. Preferably, the coated pigments according to the invention are not provided with any organic coating. This means that the coated pigments according to this invention are preferably provided exclusively with an inorganic coating containing hydroxides and / or oxides of magnesium and / or calcium.

[0016] In the context of the invention, oils are understood to mean non-polar or slightly polar, non-volatile substances that are liquid at room temperature. Preference is given to oils with a kinematic viscosity of 1.6 to 1,500 mm² / s at 40°C (measured according to DIN 51562). In the agents according to the invention, the oils are furthermore preferably selected from the group of synthetic oils, which consist essentially of the elements carbon and hydrogen and / or nitrogen and / or oxygen and / or sulfur and / or halogens (preferably fluorine, chlorine, bromine and / or iodine) and / or boron, mineral oils, animal and / or vegetable oils. The agents according to the invention particularly preferably contain synthetic oils based on hydrocarbons or mineral oils (obtained from petroleum or coal).

[0017] Waxes can be selected from the group of Fischer-Tropsch waxes, mineral waxes, montan waxes, vegetable waxes, and / or animal waxes. Fischer-Tropsch waxes are synthetic aliphatic hydrocarbons, i.e., synthetic paraffin waxes with a high molecular mass and a chain length of 20 to 120 carbon atoms. Oxidized Fischer-Tropsch waxes also belong to the group of Fischer-Tropsch waxes. Fischer-Tropsch waxes generally have a freezing point greater than 70°C. They are relatively hard, which can be measured by needle penetration at 25°C in the unit "mm." For measuring needle penetration at different temperatures, such as 25°C or 65°C, there are methods according to ASTM D 1321 or DIN 51579, for example. For these waxes, typical needle penetration values ​​at 25°C are in the range of 0.1 mm to 1 mm.Fischer-Tropsch waxes are produced using the Fischer-Tropsch process from synthesis gas (hydrogen, carbon monoxide) from coal gasification or from natural gas in the presence of catalysts. Mineral waxes are mixtures of normal, branched-chain, and cyclic saturated hydrocarbons obtained by refining waxes of fossil origin, such as ceresin. Microcrystalline hard waxes also belong to the mineral wax group. Montan waxes are natural waxes extractable from lignite. These are derived from the resins, waxes, and fats of tertiary plants. Vegetable waxes include sugarcane wax and carnauba wax. Animal waxes include spermaceti, wool wax, and beeswax. The waxes can be in their original, i.e., unchemically modified, form or in their chemically modified form.

[0018] Fatty acid salts, also called metal soaps, are preferably selected from the group of zinc, calcium, magnesium and / or barium salts of lauric acid (dodecanoic acid), myristic acid (tetradecanoic acid) and / or stearic acid (octadecanoic acid), particularly preferably from magnesium stearate, zinc stearate and / or calcium stearate.

[0019] In the coated pigment according to the invention, the pigment present from the group of iron oxides is preferably hematite, and this coated pigment preferably has an isoelectric point of <7, particularly preferably <6.8. In a further preferred embodiment, the pigment present is selected from the group of iron oxides, iron oxide hydroxides, zinc ferrites, magnesium ferrites, and / or manganese ferrites, excluding hematite, and the coated pigment preferably has an isoelectric point of 2 to 12. The isoelectric point (IEP), also called zeta potential, is measured according to ISO 13099-2.

[0020] The isoelectric point of the coated iron oxide hydroxides is typically between 3 and 11. The lower limit of the IEP for the coated pigments according to the invention is typically 2.

[0021] In a further preferred embodiment, the coated pigment contains from 3.5 to 25 wt.% magnesium or from 5.5 to 25 wt.% calcium, based on the total weight of the coated pigment. The magnesium or calcium content of the coated pigment is determined as the content of the respective element, unless otherwise stated, using inductively coupled plasma optical emission spectrometry (ICP-OES). For this purpose, the magnesium or calcium content of the entire coated pigment is determined. The weight percentages indicate the total content as the sum of the magnesium and calcium contents.

[0022] In a further preferred embodiment, the pigments are coated exclusively with magnesium hydroxides and / or oxides. The uncoated pigments used typically contain traces of calcium salts. Therefore, the pigments coated with magnesium hydroxides and / or oxides in this preferred embodiment typically contain from 0.3 to 30 wt.%, particularly preferably from 0.5 to 25 wt.%, most preferably from 0.5 to 20 wt.% magnesium, and from 0.001 to 0.1 wt.% calcium.

[0023] The coated pigments according to the invention preferably have DIN pH values ​​according to EN ISO 787-9 of 8 to 12, particularly preferably of 8.5 to 12, very particularly preferably of 9 to 12. Furthermore, the coated pigments according to the invention preferably have specific BET surface areas, measured according to DIN ISO 9277, of 7 to 150 m 2 / g, preferably of 12 to 90 m 2 / g.

[0024] In a further preferred embodiment, the coated pigments consist of at least one inorganic pigment from the group consisting of iron oxides, iron oxide hydroxides, zinc ferrites, magnesium ferrites and / or manganese ferrites, wherein the at least one inorganic pigment is provided with a coating containing hydroxides and / or oxides of magnesium and / or calcium, particularly preferably containing hydroxides of magnesium and / or calcium.

[0025] In a further preferred embodiment, the coated pigment contains at least one inorganic pigment from the group of iron oxides, iron oxide hydroxides, zinc ferrites, magnesium ferrites and / or manganese ferrites, wherein the at least one inorganic pigment is provided with a coating containing hydroxides and / or oxides of magnesium and / or calcium, wherein the surface of a core made of the inorganic pigment is directly connected to a layer of the hydroxides and / or oxides of magnesium and / or calcium surrounding it.

[0026] The invention encompasses every conceivable combination of the various defined process and material parameters and their preferred ranges.

[0027] Surprisingly, it has now been found that PVC colored with the coated pigments according to the invention exhibits higher thermal stability than PVC colored with the corresponding uncoated pigments. The increased thermal stability of PVC colored with the coated pigments according to the invention can be demonstrated, firstly, by means of a thermal treatment with a kneader, when the temporal progression of the torque applied to the kneader and the temperature of the kneaded product are recorded and compared for different samples. During the decomposition of the PVC, degradation of the polymer occurs, which leads to a reduction in viscosity and thus to a decrease in the torque applied to the kneader.

[0028] Furthermore, the increased thermal stability of PVC colored with the coated pigment according to the invention can be measured by testing specimens in a Mathis oven. Details of the measurement methods and their evaluation can be found in the "Examples and Methods" section.

[0029] The present invention also relates to the use of the coated pigment according to the invention for coloring PVC, preferably rigid PVC.

[0030] The present invention also relates to a process for coloring PVC, preferably rigid PVC, with the coated pigment according to the invention. Coloring can be carried out by conventional methods, e.g., by mixing, kneading, or extruding uncolored PVC with the coated pigment in the melt, or by melting PVC dry blends containing the coated pigment according to the invention.

[0031] The present invention also relates to plastic products, for which the terms masterbatch, compounds or colored end product are used synonymously, comprising at least one coated pigment according to the invention and also containing PVC, preferably rigid PVC. Preferred plastic products are those which contain colored PVC. Alternatively preferred plastic products are those which contain at least one coated pigment according to the invention and at least one polymer, where the at least one polymer is a PVC homopolymer, i.e. a polymer which is composed exclusively of the monomer vinyl chloride. Further alternatively preferred plastic products are those which have at least one polymer as plastic, where the plastic is preferably composed of at least 50% by weight, particularly preferably at least 80% by weight, of the monomer vinyl chloride.This applies, on the one hand, to the case where the plastic is a PVC copolymer which, in addition to vinyl chloride, is also made up of other monomers, e.g. vinyl acetate or butyl acrylate. In this case, the copolymer is preferably made up of at least 50% by weight, particularly preferably at least 80% by weight, of the monomer vinyl chloride. This also applies if the plastic is a mixture or blend of different polymers, one of which is a PVC homopolymer or a PVC copolymer. In this case, the mixture or blend is preferably made up of at least 50% by weight, particularly preferably at least 80% by weight, of the monomer vinyl chloride. For the purposes of the invention, colored PVC is understood to mean PVC in which the coated pigment according to the invention is embedded in the polymer matrix of the polyvinyl chloride.

[0032] Compounds contain, for example, processing aids, reinforcing agents, fillers, dyes, additional pigments, and other organic and inorganic additives, thus enabling the production of a wide variety of molded parts by, for example, extrusion, injection molding, calendering, or blow molding. The molded parts generally correspond to the end products, referred to in the context of this invention as products, such as window frames, pipes, insulation material, films, or bottles. To color the PVC, masterbatches or the pigment itself are added to the compounds.

[0033] The plastic product according to the invention contains different amounts of coated pigment according to the invention depending on the intended use.

[0034] Masterbatches are typically used as "color concentrates" for coloring PVC or other plastic products. Therefore, these masterbatches have a relatively high pigment content of greater than 10 to 90 wt.%, particularly preferably 20 to 70 wt.%, of coated pigment according to the invention.

[0035] If the plastic product is already in its final use as a compound with the desired color, the contents of coated pigment according to the invention are preferably from 0.1 to 10 wt.%, particularly preferably 0.5 to 5 wt.%.

[0036] The present invention also relates to a process for producing the plastic products according to the invention, in particular compounds and masterbatches, by kneading or extruding PVC with the coated pigment according to the invention.

[0037] According to the invention, PVC is used with varying plasticizer contents. PVC with a plasticizer content of 0 to 12% is also called rigid PVC. PVC with a plasticizer content of more than 12% is also called soft PVC (Römpp Chemical Encyclopedia, online version 3.28, article last updated: December 2009, document ID: RD-16-03650).

[0038] The invention also relates to a plastic product containing from 0 to 15% by weight, preferably from 0 to 12% by weight, of plasticizer based on the amount of PVC contained in the plastic product.

[0039] Suitable plasticizers include primary and secondary plasticizers, and extenders. Primary plasticizers include phthalic acid esters, trimellitic acid esters, phosphates, and polymer plasticizers. Secondary plasticizers include adipates, azelates, decanedioic acid esters, and alkyl fatty acid esters. Extenders include aromatic hydrocarbons and chlorinated paraffins (from Römpp Chemielexikon, online version 3.2.8, article last updated: March 2006, document ID: RD-23-00480).

[0040] The present invention also relates to a plastic product, for which the term "PVC dry blend" is also used, comprising a mixture of powdered PVC, preferably rigid PVC, and a coated pigment according to the invention. Such PVC dry blends may further contain the additives required for the production of compounds (e.g., fillers, stabilizers, optionally further plasticizers, dyes, optionally further pigments). These additives may be present either in bulk alongside or already incorporated into the PVC of the dry blend. Dry blends are typically produced by intensively mixing the components described above at temperatures just below the melting point of the plastic. The products can be manufactured from the dry blends using the processing methods customary for PVC, such as extrusion, injection molding, calendering, or blow molding.

[0041] The present invention also relates to a product, for which the terms "molded part" or "finished product" are used synonymously in connection with this invention, containing at least one plastic product according to the invention. Such products include, for example, window profiles, pipes, floor coverings, insulation material, or roofing membranes.

[0042] The present invention also relates to a process for producing the coated pigments according to the invention. All processes that lead to a coating of the aforementioned compounds on inorganic pigments can be used for the coating. These include grinding, precipitating, or spraying the compounds with which the inorganic pigment is to be coated, either as a solid or as a suspension.

[0043] The preferred method according to the invention comprises at least the steps a) Providing an aqueous suspension of at least one inorganic pigment from the group consisting of iron oxides, iron oxide hydroxides, zinc ferrites, magnesium ferrites and / or manganese ferrites, b) Precipitation of the coating of hydroxides and / or oxides of magnesium and / or calcium onto the inorganic pigment by adding magnesium and / or calcium salts, preferably in dissolved form, to the suspension from step a) and then adding a precipitant from the group consisting of alkali hydroxides, alkaline earth hydroxides, or ammonia, preferably in dissolved form, to the suspension or b') Precipitation of the coating of hydroxides and / or oxides of magnesium and / or calcium onto the inorganic pigment by adding a precipitant from the group consisting of alkali hydroxides, alkaline earth hydroxides, or ammonia, preferably in dissolved form, to the suspension from step a) and then adding magnesium and / or calcium salts, preferably in dissolved form, to the suspension, whereby the coated pigment is obtained.

[0044] The preferred process for producing coated pigment according to the invention optionally additionally comprises one, two, three or four of the steps i) isolating the coated pigment, ii) washing the coated pigment, iii) drying the coated pigment, and iv) comminuting the coated pigment, preferably in the order given.

[0045] The pigments used in step a) of the preferred process are powdered pigments or pastes made from pigments derived directly from the pigment manufacturing process. Pastes are flowable, pigment-containing, aqueous suspensions.

[0046] In a further variant (step b"), the addition of the precipitant from the group of alkali metal hydroxides, alkaline earth metal hydroxides, or ammonia, preferably in dissolved form, and the magnesium and / or calcium salts, preferably in dissolved form, to a pigment suspension provided can also be carried out simultaneously. By the alternative steps b), b') or b"), the inorganic pigment is coated with hydroxides and / or oxides of magnesium and / or calcium.

[0047] The precipitants particularly preferred in the process according to the invention are sodium hydroxide and / or potassium hydroxide.

[0048] In the variants according to steps b), b') or b"), magnesium and / or calcium salts, particularly preferably their aqueous solutions, very particularly preferably magnesium sulfate, magnesium chloride, magnesium nitrate, calcium chloride, and / or calcium nitrate are preferably used.

[0049] During the precipitation of the coating of hydroxides and / or oxides of magnesium and / or calcium onto the inorganic pigment and optionally during the post-reaction, a temperature of 10 to 99°C, particularly preferably 20 to 85°C, most preferably 20 to 70°C is preferably selected.

[0050] The time during which either the precipitant or the magnesium and / or calcium salts are added to the reaction mixture can vary within wide values.

[0051] Preferably, the reaction components are mixed in steps b), b') or b"), particularly by static or dynamic mixers. For this purpose, stirrers, propellers, blades, and / or pumps are used, for example.

[0052] The reaction mixture from steps b), b') or b") is, if necessary, further mixed after the addition of the components in order to allow the precipitation of the hydroxides and / or oxides of magnesium and / or calcium onto the inorganic pigment to proceed as completely as possible. The time for the post-reaction depends on the size of the reaction batch. To check the completeness of the reaction, samples can be taken at intervals and analyzed for their magnesium and / or calcium content. If the expected magnesium and / or calcium content is reached, the reaction is complete.

[0053] After the reaction is complete, the coated inorganic pigment according to the invention is optionally separated from the reaction mixture using conventional methods, such as filtration or centrifugation. The separated solid is then optionally washed with water, preferably with demineralized water, preferably until the filtrate has a conductivity of less than or equal to 1000 µS / m, preferably less than or equal to 500 µS / m.

[0054] Calcination steps are sometimes used in processes for producing pigments. Calcination is understood to mean the thermal treatment of a solid or semi-moist pigment at temperatures greater than 600°C. This may be necessary if pigments are to be dehydrated or converted into other modifications. In the process according to the invention, a calcination step is not required. In a preferred embodiment of the process according to the invention, a calcination step is therefore excluded. In a particularly preferred embodiment of the process according to the invention, a calcination step at temperatures greater than 600°C is therefore excluded.

[0055] The coated pigments according to the invention represent an improvement over the state of the art, since plastic products and PVC products colored with the coated pigments according to the invention have high thermal stability and UV stability. Examples and methods I. Description of the measurement and testing methods used

[0056] The results of the measurements for the examples are summarized in Table 1. I.1 Zeta Potential (Isoelectric Point, IEP)

[0057] The zeta potential was determined according to ISO 13099-2 on a "Zetasizer Nano Z" from Malvern Instruments GmbH (with a He-Ne laser 633 nm). I.2 DIN pH value

[0058] The DIN pH value of pigments was measured according to EN ISO 787-9. I.3 Mg and Ca determination

[0059] The magnesium and calcium content of the pigments was measured as the content of the elements using optical emission spectrometry after excitation in inductively coupled plasma (ICP-OES: inductively coupled plasma-optical emission spectrometry). I.4 Specific BET surface area

[0060] The specific BET surface area was measured according to DIN ISO 9277. I.5 Testing of PVC stability using a Mathis oven type LTE-T from Werner Mathis AG (Mathis oven stability)

[0061] The test strips required for testing are produced on a roller mill (Servitec Polymix 150L). For this purpose, 50 g of rigid PVC compound (SorVyl DB 6668 Natural 3 / 03 PVC compound from Polymer-Chemie GmbH) and 2 g of the pigment to be tested (4 wt.%) are weighed into a polyethylene cup and thoroughly mixed with a spatula. The mixture is applied to the roller mill and rolled out at 175°C and a friction ratio of 1:1.2 to form a sheet 200 µm thick. The pigment is dispersed for 10 minutes while constantly rotating the roller.

[0062] The resulting roller skin is removed from the roller. Using guillotine shears, the strips required for the subsequent test in the Mathis furnace, measuring 50 cm in length and 2 cm in width, are prepared and clamped into the material carrier of the Mathis furnace.

[0063] In the Mathis Oven Thermal Test (Thermotester Type LTE-T, test chamber for testing the thermal stability of plastics from Werner Mathis AG, Oberhasli / Zurich, Switzerland), PVC samples are subjected to varying degrees of thermal stress, which is determined by the discrete advance of a slide out of the oven. The temperature during the test is 190°C. The material carrier containing the PVC test specimens is pushed out of the oven by 75 mm every 5 minutes (oven setting: interval time 5 minutes, advance 75 mm), with the section pushed out of the oven quickly cooling to room temperature. This results in consecutive zones on the test specimen, each 75 mm long, each of which was thermally stressed for 5 minutes longer than the zone before it. PVC decomposition begins at different times for different pigments, causing the test strip to turn darker to black at a certain zone.To assess the suitability of a pigment for stabilizing PVC, two times are specified, e.g., 35 / 45. These values ​​indicate minutes (min). The first time, in this example 35 min, is the residence time in minutes of the corresponding test specimen zone in the Mathis oven at which no discoloration of the corresponding test specimen zone is yet visible. The second time, in this example 45 min, is the residence time in minutes of the corresponding test specimen zone in the Mathis oven at which the discoloration of the corresponding test specimen zone is first maximum. As a rule, the corresponding test specimen zones are colored black after maximum discoloration. I.6 Testing of PVC stability using a Thermo Haake Rheomix 600p kneader (kneader stability)

[0064] A powdered PVC mixture consisting of 50 wt.% Vestolit B 7021 Ultra + 50 wt.% SorVyl DB 6668 Natural 3 / 03 is homogeneously mixed with the powdered pigment sample to be tested (4 wt.% based on 100% PVC composition).

[0065] The pigmented PVC mixture is manually poured into the measuring kneader (Thermo Haake Rheomix 600p with roller rotors R6) preheated to 190°C, which is equipped with a rotational rheometer. The measurement program (PolyLab Monitor) is started and records the time course of the torque applied to the roller rotors and the temperature of the sample. The pigmented PVC mixture is kneaded at 190°C and 50 rpm. To determine the suitability of the pigment for stabilizing PVC, the maximum torque is indicated on the time axis in minutes at which the highest product temperature was measured. After this maximum torque, the torque drops sharply, as the PVC gradually decomposes after this time, thereby reducing the viscosity of the kneaded product. These values ​​are compared with the corresponding value for the same, but uncoated, pigment powder.The longer the time until the stated maximum, the higher the stability of the PVC colored with the pigment. II: Examples II.1 Properties of the inorganic pigments and plastics used

[0066] Bayferrox ®< 110 pigment powder from LANXESS Deutschland GmbH: Hematite (red iron oxide, α-Fe 2 O 3 ) with a BET surface area according to DIN ISO 9277 of 13-16 m 2 < / g.

[0067] Bayferrox ®< 330 paste: Magnetite (black iron(II,III) oxide, Fe 3 O 4 ) in paste form from LANXESS Deutschland GmbH, which is dried and ground to produce Bayferrox ®< 330 powder. The powdered pigment has a BET surface area according to DIN ISO 9277 of 9-17 m 2 < / g. Alternatively, the powdered Bayferrox ®< 330 pigment can be slurried with water to the appropriate pigment concentration.

[0068] Bayferrox ®< 420 paste:Goethite (yellow iron oxide hydroxide, α-FeOOH) as a paste from LANXESS Deutschland GmbH, from which Bayferrox ®< 420 powder is produced by drying and grinding. The powdered pigment has a BET surface area according to DIN ISO 9277 of 11-15 m 2 < / g). Alternatively, the powdered pigment Bayferrox ®< 420 can be slurried with water to the appropriate pigment concentration (see examples).

[0069] Bayferrox ®< 920 paste: Goethite, α-FeOOH paste from LANXESS Deutschland GmbH, from which Bayferrox ®< 920 powder is produced by drying and grinding. The powdered pigment has a BET surface area according to DIN ISO 9277 of 11-15 m 2 < / g. Alternatively, the powdered Bayferrox ®< 920 pigment can be slurried with water to the appropriate pigment concentration (see examples).

[0070] Bayferrox ®< 943 paste:Lepidocrocite (iron oxide hydroxide, γ-FeOOH) is a paste from LANXESS Deutschland GmbH, which is dried and ground to produce Bayferrox ®< 943 powder. The powdered pigment has a BET surface area according to DIN ISO 9277 of 16-19 m 2< / g. Alternatively, the powdered Bayferrox ®< 943 pigment can be slurried with water to the appropriate pigment concentration.

[0071] Bayferrox ®< 3950 pigment powder from LANXESS Deutschland GmbH: zinc ferrite (ZnFe 2 O 4 ) with a BET surface area according to DIN ISO 9277 of 5-7 m 2 < / g.

[0072] Bayferrox ®< 645T pigment powder from LANXESS Deutschland GmbH: non-stoichiometric manganese ferrite (with <9 wt.% MnO content) with a BET surface area according to DIN ISO 9277 of 8-13 m 2 < / g.

[0073] SorVyl DB 6668 Natural 3 / 03:Rigid PVC compound from Polymerchemie (powder form, stabilized with Ca / Zn, with a bis(pentane-2,4-dionato)calcium content of less than 1 wt.%, with a softening point of >120°C, flash point of >190°C, ignition temperature of >300°C, density of 1.39 g / cm3 according to DIN EN ISO 1183-1, method A, bulk density of 0.54 g / ml according to DIN EN ISO 60, and thermal stability of greater than or equal to 25 min according to DIN EN 60811-3-2.

[0074] VESTOLIT ®< B 7021 Ultra: Homopolymer micro-S-PVC from Vestolit (powder form, K value according to DIN EN ISO 1628-2 of 70, viscosity number according to DIN EN ISO 1628-2 of 125 cm 3 < / g , bulk density according to DIN EN ISO 60 of 0.3 g / cm 3 < , sieve analysis - residue on a 0.063 mm sieve according to DIN EN ISO 1624 of < 1%, water content according to K. Fischer DIN 53 715 of ≤ 0.3%, pH value of the aqueous extract according to DIN EN ISO 1264 of 8, paste viscosity 1.5 / s of 1.8 Pa s, paste viscosity 45 / s of 2.2 Pa s). II.2 Inventive examples and comparative examples Example 1

[0075] 574 mL of a MgSO 4 solution (2.02 mol / dm 3 ) were added to a 5 dm 3 aqueous suspension of Bayferrox ® 110 (9.39 mol α-Fe 2 O 3 ) with a pH of approximately 4.5 at room temperature while stirring. Subsequently, 0.25 mol of NaOH solution (310 mL at a concentration of 7.65 mol / dm 3 ) was added dropwise over a period of 30 minutes while stirring. The suspension was stirred for a further 60 minutes. The pH of the suspension was ≥ 12. Example 2

[0076] 1148 mL of a MgSO 4 solution (2.02 mol / dm 3 as MgO) were added to a 5 dm 3 aqueous suspension of Bayferrox ® 110 (9.39 mol α-Fe 2 O 3 ) with a pH of approximately 4.5 at room temperature while stirring. Subsequently, 0.51 mol of NaOH per mol of α-Fe 2 O 3 was added dropwise over a period of 60 minutes while stirring (625 mL at a concentration of 7.65 mol / dm 3 ). The suspension was stirred for a further 60 minutes. The pH of the suspension was ≥ 12. Example 3

[0077] 162 mL of a MgSO 4 solution (2.02 mol / dm 3 as MgO) was added to a 5 dm 3 aqueous suspension of Bayferrox ® 110 (9.39 mol α-Fe 2 O 3 ) with a pH of approximately 4.5 at room temperature while stirring. Subsequently, 0.068 mol of NaOH (84 mL at a concentration of 7.65 mol / dm 3 ) was added dropwise over a period of 30 minutes while stirring. The suspension was stirred for a further 60 minutes. The pH of the suspension was ≥ 12. Example 4

[0078] To a 2.13 dm³ aqueous suspension of Bayferrox® 110 (4.01 mol α-Fe 2 O 3 ) with a pH of approximately 4.5, 5517 mL of a MgSO 4 solution (1.15 mol / dm³ as MgO) was added at room temperature with stirring. Subsequently, 3.18 mol of NaOH per mol of α-Fe 2 O 3 were added dropwise over a period of 60 minutes (using a 7.65 mol / dm³ solution). The suspension was stirred for a further 60 minutes. The pH of the suspension was ≥ 12. Example 5 (comparison example)

[0079] NaOH solution (0.06 mol, 7.65 mol / dm 3 ) was added dropwise to a 5 dm 3 aqueous suspension of Bayferrox ® 110 (9.39 mol α-Fe 2 O 3 ) with a pH of approximately 4.5 over a period of 30 minutes while stirring. The suspension was stirred for a further 60 minutes. The pH of the suspension was approximately 10. Example 6 (comparison example)

[0080] NaOH solution (0.18 mol, 7.65 mol / dm 3 ) was added dropwise over 30 minutes with stirring to 5 dm 3 of an aqueous suspension of Bayferrox ® 110 (9.39 mol α-Fe 2 O 3 ) with a pH of approx. 4.5. The suspension was stirred for a further 60 minutes. The pH of the suspension was ≥ 12. After the reaction had ended, the products from Examples 1 to 6 were filtered through a suction filter, washed until the conductivity of the filtrate was below 300 µS / cm, dried to constant weight in a drying cabinet at 180°C and ground in a Bauermeister mill (cross beater mill with a sieve insert, mesh size 1 mm). Example 7

[0081] To 7.7 kg of Bayferrox® 420 paste with a pigment content of 19.4 wt.% and a pH of 6-7, 1.12 mol of MgO from a MgSO 4 solution (1.15 mol / dm 3 as MgO) was added at 60°C with stirring. Subsequently, NaOH solution (7.7 mol / dm 3 ) was added dropwise over 15 minutes with stirring until a pH of approximately 10 was reached. Example 8

[0082] 2.24 mol of MgO from a MgSO 4 solution (1.15 mol / dm 3 as MgO) were added to 7.7 kg of Bayferrox ® 420 paste with a pigment content of 19.4 wt.% and a pH of 6-7 at 60°C while stirring. NaOH solution (7.7 mol / dm 3 ) was then added dropwise over 15 minutes while stirring until a pH of approximately 10 was reached.

[0083] After the reaction had ended, the products from Examples 7 and 8 were filtered through a Nutsche filter, washed until the conductivity of the filtrate was below 300 µS / cm, dried to constant weight in a drying cabinet at 120°C and ground on a Bauermeister mill (cross beater mill with a sieve insert, mesh size 1 mm). Example 9

[0084] To 3.29 kg of Bayferrox® 920 paste containing 130.8 g / dm 3 of pigment and a pH of 5-6, 1.65 mol of NaOH solution (7.87 mol / dm 3 ) was added while stirring at 50 °C. Subsequently, 0.82 mol of Mg from a MgSO 4 solution (2.05 mol / dm 3 as MgO) was added dropwise over 15 minutes while stirring. The pH of the suspension was approximately 10. Example 10

[0085] To 3.29 kg of Bayferrox® 920 paste containing 130.8 g / dm 3 of pigment and a pH of 5-6, 0.82 mol of Mg from a MgSO 4 solution (2.05 mol / dm 3 as MgO) was added at 50°C with stirring. Subsequently, 1.65 mol of NaOH (7.87 mol / dm 3 ) was added dropwise over 15 minutes with stirring. The pH of the suspension was approximately 10.

[0086] After the reaction had ended, the products from Examples 9 and 10 were filtered through a Nutsche filter, washed until the conductivity of the filtrate was below 500 µS / cm, dried to constant weight in a drying cabinet at 80°C and ground on a cross beater mill.

[0087] The properties of products 1 to 10 can be found in Tables 1 and 2. Examples 1 to 10 have a calcium content of 0.001 to 0.05 wt.% based on the total weight of the pigment. Example 11

[0088] 866 mL of a MgSO 4 solution (2.58 mol / dm 3 ) were added to a 4.7 dm 3 aqueous suspension of Bayferrox ® 330 paste (6.48 mol Fe 3 O 4 ) with a pH of 5.8 at 60°C while stirring. Subsequently, 0.86 mol of NaOH solution (379 g with a concentration of 7.9 mol / dm 3 ) was added dropwise over 15 minutes while stirring. The suspension was stirred for a further 60 minutes. The pH of the suspension was >11. Example 12

[0089] 2856 mL of a MgSO4 solution (2.58 mol / dm3) were added to a 2.85 dm3 aqueous suspension of Bayferrox® 330 paste (3.24 mol Fe3O4) with a pH of 5.8 at 60°C while stirring. Subsequently, 5.74 mol of NaOH solution (3000 g at a concentration of 7.9 mol / dm3) were added dropwise over 15 minutes with stirring per mol of Fe3O4. The suspension was stirred for a further 60 minutes. The pH of the suspension was > 11.

[0090] After the reaction had ended, the products from Examples 11 to 12 were filtered through a Nutsche filter, washed until the conductivity of the filtrate was below 300 µS / cm, dried to constant weight in a drying cabinet at 95°C and ground on a Bauermeister mill (cross beater mill with a sieve insert, mesh size 1 mm). Example 13

[0091] 1442 mL of a MgSO4 solution (2.58 mol / dm3) were added to a 5 dm3 aqueous suspension of Bayferrox® 3950 (6.22 mol ZnFe2O4) with a pH of approximately 7 at 60°C while stirring. Subsequently, 1.5 mol of NaOH solution (1500 g at a concentration of 7.9 mol / dm3) were added dropwise over 15 minutes with stirring per mol of ZnFe2O4. The suspension was stirred for a further 60 minutes. The pH of the suspension was > 11. Example 14

[0092] To a 2.5 dm³ aqueous suspension of Bayferrox® 3950 (3.11 mol ZnFe2O4) with a pH of approximately 7, 1443 mL of a MgSO4 solution (2.58 mol / dm³) were added at 60°C with stirring. Subsequently, 3 mol of NaOH solution (1500 g at a concentration of 7.9 mol / dm³) were added dropwise over 15 minutes with stirring per mol of ZnFe2O4. The suspension was stirred for a further 60 minutes. The pH of the suspension was > 11.

[0093] After the reaction had ended, the products from Examples 13 to 14 were filtered through a Nutsche filter, washed until the conductivity of the filtrate was below 300 µS / cm, dried to constant weight in a drying cabinet at 120°C and ground on a Bauermeister mill (cross beater mill with a sieve insert, mesh size 1 mm). Example 15

[0094] 395 mL of a MgSO 4 solution (2.83 mol / dm 3 ) were added to a 5 dm 3 aqueous suspension of Bayferrox® 645T (1500 g) with a pH of approximately 6 at 60°C while stirring. Subsequently, 2.24 mol of NaOH solution (362 g with a concentration of 7.9 mol / dm 3 ) were added dropwise over 15 min while stirring. The suspension was stirred for a further 60 min. The pH of the suspension was > 11. Example 16

[0095] To a 5 dm³ aqueous suspension of Bayferrox® 645T (1500 g) with a pH of approximately 6, 1974 mL of a MgSO4 solution (2.83 mol / dm³) were added at 60°C with stirring. Subsequently, 13.95 mol of NaOH solution (2250 g with a concentration of 7.9 mol / dm³) were added dropwise over 15 min with stirring. The suspension was stirred for a further 60 min. The pH of the suspension was > 11.

[0096] After the reaction had ended, the products from Examples 15 to 16 were filtered through a Nutsche filter, washed until the conductivity of the filtrate was below 300 µS / cm, dried to constant weight in a drying cabinet at 120°C and ground on a Bauermeister mill (cross beater mill with a sieve insert, mesh size 1 mm). Example 17

[0097] 900 mL of a MgSO 4 solution (2.48 mol / dm 3 ) were added to an 8.01 dm 3 aqueous suspension of Bayferrox ® 943 paste (16.88 mol FeOOH) with a pH of approximately 6 at room temperature while stirring. Subsequently, 0.26 mol of NaOH solution (724 g with a concentration of 7.9 mol / dm 3 ) was added dropwise over 15 minutes with stirring per mol of FeOOH. The suspension was stirred for a further 60 minutes. The pH of the suspension was > 11. Example 18

[0098] 5455 mL of a MgSO 4 solution (2.73 mol / dm 3 ) were added to an 8.01 dm 3 aqueous suspension of Bayferrox ® 943 paste (16.88 mol FeOOH) with a pH of approximately 6 at room temperature while stirring. Subsequently, 1.76 mol of NaOH solution (4800 g at a concentration of 7.9 mol / dm 3 ) were added dropwise over 15 minutes per mol of FeOOH while stirring. The suspension was stirred for a further 60 minutes. The pH of the suspension was >13.

[0099] After the reaction had ended, the products from Examples 17 to 18 were filtered through a Nutsche filter, washed until the conductivity of the filtrate was below 300 µS / cm, dried to constant weight in a drying cabinet at 120°C and ground on a Bauermeister mill (cross beater mill with a sieve insert, mesh size 1 mm). Example 19

[0100] 6476 mL of a MgSO4 solution (2.6 mol / dm3) were added to a 3.3 dm3 aqueous suspension of Bayferrox® 110 (6.26 mol Fe2O3) with a pH of approximately 4.5 at 60°C while stirring. Subsequently, 5.39 mol of NaOH solution (5440 g at a concentration of 7.9 mol / dm3) were added dropwise over 15 minutes while stirring. The suspension was stirred for a further 60 minutes. The pH of the suspension was > 13.

[0101] After the reaction had ended, the product from Example 19 was filtered through a Nutsche filter, washed until the conductivity of the filtrate was below 300 µS / cm, dried to constant weight in a drying cabinet at 180°C and ground on a Bauermeister mill (cross beater mill with a sieve insert, mesh size 1 mm).

[0102] The properties of products 11 to 19 can be found in Table 2. Examples 11 to 19 have a calcium content of 0.001 to 0.1 wt.% based on the total weight of the pigment.

Claims

1. Coated pigment comprising at least one inorganic pigment from the group of iron oxides, iron oxide hydroxides, zinc ferrites, magnesium ferrites and / or manganese ferrites, wherein the at least one inorganic pigment has been provided with a coating comprising hydroxides and / or oxides of magnesium and / or calcium, wherein the coated pigment comprises from 3.1% to 30% by weight of magnesium, or from 5.0% to 30% by weight of calcium, based on the total weight of the coated pigment.

2. Coated pigment according to Claim 1, consisting of at least one inorganic pigment from the group of iron oxides, iron oxide hydroxides, zinc ferrites, magnesium ferrites and / or manganese ferrites, wherein the at least one inorganic pigment has been provided with a coating comprising hydroxides and / or oxides of magnesium and / or calcium, preferably with a coating comprising hydroxides of magnesium and / or calcium.

3. Coated pigment according to Claim 1, comprising at least one inorganic pigment from the group of iron oxides, iron oxide hydroxides, zinc ferrites, magnesium ferrites and / or manganese ferrites, wherein the at least one inorganic pigment has been provided with a coating comprising hydroxides and / or oxides of magnesium and / or calcium, wherein the surface of a core of the inorganic pigment has been bonded directly to a surrounding layer of the hydroxides and / or oxides of magnesium and / or calcium.

4. Coated pigment according to any of Claims 1 to 3, wherein the pigment present in the coated pigment is haematite, and the coated pigment has an isoelectric point of < 7, preferably of < 6.8.

5. Coated pigment according to any of Claims 1 to 3, wherein the pigment present in the coated pigment is selected from the group of the iron oxides, iron oxide hydroxides, zinc ferrites, magnesium ferrites and / or manganese ferrites, excluding haematite, wherein the coated pigment preferably has an isoelectric point of 2 to 12.

6. Coated pigment according to any of Claims 1 to 5, wherein the coated pigment comprises from 3.5% to 25% by weight of magnesium, or from 5.5% to 25% by weight of calcium, based on the total weight of the coated pigment.

7. Plastics product comprising at least one coated pigment according to any of Claims 1 to 6, and further comprising PVC, preferably rigid PVC.

8. Plastics product comprising at least one coated pigment according to any of Claims 1 to 6 and at least one polymer as plastic, wherein at least 50% by weight, preferably at least 80% by weight, of the plastic is formed from the monomer vinyl chloride.

9. Plastics product according to Claim 7 or 8, comprising from greater than 10% to 90% by weight, preferably from 20% to 70% by weight, of coated pigment according to any of Claims 1 to 6.

10. Plastics product according to Claim 7 or 8, comprising from 0.1% to 10% by weight, preferably from 0.5% to 5% by weight, of coated pigment according to any of Claims 1 to 6.

11. Plastics product according to any of Claims 7 to 10, comprising from 0% to 15% by weight, preferably from 0% to 12% by weight, of plasticizer, based on the amount of PVC present in the plastics product.

12. Plastics product according to any of Claims 7 to 11, comprising a mixture of pulverulent PVC and coated pigment according to any of Claims 1 to 6.

13. Process for producing coated pigment according to any of Claims 1 to 6, comprising at least the steps of a) providing an aqueous suspension of at least one inorganic pigment from the group of iron oxides, iron oxide hydroxides, zinc ferrites, magnesium ferrites and / or manganese ferrites, b) precipitating the coating of hydroxides and / or oxides of magnesium and / or calcium onto the inorganic pigment by adding magnesium and / or calcium salts, preferably in dissolved form, to the suspension from step a) and then adding a precipitant from the group of alkali metal hydroxides, alkaline earth metal hydroxides, preferably in dissolved form, to the suspension or b') precipitating the coating of hydroxides and / or oxides of magnesium and / or calcium onto the inorganic pigment by adding a precipitant from the group of alkali metal hydroxides, alkaline earth metal hydroxides, preferably in dissolved form, to the suspension from step a) and then adding magnesium and / or calcium salts, preferably in dissolved form, to the suspension, to obtain the coated pigment.

14. Process for producing coated pigment according to Claim 13, additionally comprising one, two, three or four of the steps of i) isolating the coated pigment, ii) washing the coated pigment, iii) drying the coated pigment, and iv) comminuting the coated pigment, preferably in the sequence specified.

15. Process for producing coated pigment according to either of Claims 13 and 14, in which a calcination step, preferably at temperatures greater than 600°C, is ruled out.

16. Process for producing the plastics products according to any of Claims 7 to 12 by kneading or extruding PVC with the coated pigment according to any of Claims 1 to 6.

17. Process for producing the plastics product according to Claim 11 by mixing at least one coated pigment according to any of Claims 1 to 6 and pulverulent PVC, preferably by mixing the constituents just below the melting point of the plastic.

18. Use of the coated pigment according to any of Claims 1 to 6 for colouring PVC, preferably rigid PVC.

19. Product comprising at least one plastics product according to any of Claims 7 to 12.