USE OF POLYOLETHERS FOR THE PRODUCTION OF POROUS PLASTIC COATINGS
Patent Information
- Application Number
- DE502018015302
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-08-30
- Filing Date
- 2018-08-02
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2038-08-02
AI Technical Summary
Current surfactants used in producing porous polyurethane coatings, such as ammonium stearate, face issues like water susceptibility, foam instability, and migration, leading to undesirable properties like flocculation, gelling, and surface defects, particularly in contact with lime-containing water, and require additional surfactants for stability.
The use of polyol ethers as additives in aqueous polymer dispersions for producing porous polymer coatings, which enables efficient foaming, stable foam formation, and improved hydrolysis stability, reducing the need for additional surfactants and enhancing mechanical and haptic properties.
Polyol ethers provide a fine and homogeneous cell structure, increased foam stability, and improved air permeability, preventing drying defects and reducing the complexity of formulations, while maintaining stability across a wide pH range and avoiding migration in the dried film.
Description
[0001] The present invention lies in the field of plastic coatings, artificial leather and polyol ethers.
[0002] It particularly concerns the production of porous polymer coatings, preferably porous polyurethane coatings, using polyol ethers as additives.
[0003] Textiles coated with plastics, such as artificial leather, usually consist of a textile substrate onto which a porous polymer layer is laminated, which in turn is covered with a top layer or topcoat.
[0004] The porous polymer layer preferably has pores in the micrometer range, is air-permeable and therefore breathable (i.e., permeable to water vapor), but water-resistant. This porous polymer layer is often porous polyurethane. Currently, porous polyurethane layers are mostly produced using a coagulation process that employs DMF as a solvent. However, due to environmental concerns, this production method is increasingly criticized and should therefore be gradually replaced by other, more environmentally friendly technologies. One such technology is based on aqueous polyurethane dispersions, so-called PUDs. These typically consist of polyurethane microparticles dispersed in water, with a solids content usually ranging from 30 to 60 wt%.To produce a porous polyurethane layer, these PUDs are mechanically foamed, coated onto a substrate (layer thicknesses typically between 300 and 2000 µm), and then dried at elevated temperatures. During this drying step, the water contained in the PUD system evaporates, resulting in the formation of a film of polyurethane particles. To further increase the mechanical strength of the film, hydrophilic (poly)isocyanates can be added to the PUD system during the manufacturing process. These isocyanates react with free OH residues present on the surface of the polyurethane particles during the drying step, leading to additional cross-linking of the polyurethane film.
[0005] Both the mechanical and haptic properties of PUD coatings produced in this way are largely determined by the cell structure of the porous polyurethane film. Furthermore, the cell structure of the porous polyurethane film influences the air permeability or breathability of the material. Particularly good properties are achieved with the finest possible, homogeneously distributed cells. To influence the cell structure during the manufacturing process described above, it is common practice to add surfactants to the PUD system before or during mechanical foaming. These surfactants ensure that sufficient quantities of air are incorporated into the PUD system during the foaming process. They also directly influence the morphology of the resulting air bubbles. The stability of the air bubbles is also significantly affected by the type of surfactant used.This is particularly important during the drying of foamed PUD coatings, as it prevents drying defects such as cell coarsening or drying cracks.
[0006] The prior art discloses a number of ionic and nonionic surfactants that can be used to produce porous, PUD-based textile composite materials. Anionic surfactants based on ammonium stearate are particularly preferred; see, for example, US 2015 / 0284902 A1 or US 2006 / 0079635 A1.
[0007] However, the use of ammonium stearate comes with several disadvantages. Firstly, ammonium stearate is susceptible to hard water. In polymer dispersions containing calcium ions, insoluble calcium soaps can form, leading to flocculation or gelation of the polymer dispersion. Furthermore, synthetic leather made with ammonium stearate has the disadvantage that calcium soaps can form on the surface when in contact with hard water, appearing as white spots. This is particularly undesirable with dark-colored leather. In addition, ammonium stearate exhibits a relatively high degree of migration in the dried polyurethane film. Especially in contact with water, this can result in an unpleasant smearing film on the surface of the synthetic leather coating.Another disadvantage of ammonium stearate is that it usually needs to be used in combination with other surfactants to achieve sufficient foam stability; sulfosuccinamates, for example, are described in the prior art. These additional components increase the complexity of the application.
[0008] The use of polyol esters for the production of porous plastic coatings, particularly porous polyurethane coatings, was already described in the still unpublished European patent application 16180041.2. It was demonstrated therein that such polyol esters allow for the efficient foaming of aqueous polymer dispersions without exhibiting the disadvantages listed in the prior art. However, a disadvantage of these polyol esters can be their insufficient hydrolysis stability in aqueous polymer dispersions, especially at high pH values. The object of the present invention was therefore to provide a further class of surfactants that also allows for the efficient foaming of aqueous polymer dispersions but is additionally characterized by increased hydrolysis stability. Surprisingly, it was found that the use of polyol ethers enables the solution of this object.
[0009] The present invention therefore relates to the use of polyol ethers as additives in aqueous polymer dispersions for the production of porous polymer coatings, preferably for the production of porous polyurethane coatings.
[0010] The porous polymer layer (i.e., the porous polymer coating) to be produced according to the invention preferably has pores in the micrometer range, wherein the mean cell size is preferably less than 150 µm, more preferably less than 120 µm, particularly preferably less than 100 µm, and most preferably less than 75 µm. The preferred layer thickness is in the range of 10–10,000 µm, preferably 50–5,000 µm, more preferably 75–3,000 µm, and particularly 100–2,500 µm.
[0011] The use of polyol ethers according to the invention surprisingly has many advantages.
[0012] It enables efficient foaming of the polymer dispersion. The foams produced in this way are characterized by an exceptionally fine pore structure with a particularly homogeneous cell distribution, which in turn has a very beneficial effect on the mechanical and haptic properties of the porous polymer coating produced on the basis of these foams. Furthermore, this can improve the air permeability or breathability of the coating.
[0013] A further advantage of the polyol ethers used according to the invention is that they enable the production of particularly stable foams. This has a beneficial effect on their processability. Furthermore, the increased foam stability has the advantage that drying defects such as cell coarsening or drying cracks can be avoided during the drying process. In addition, the improved foam stability allows for faster drying of the foams, which offers process-related advantages from both an ecological and an economic perspective.
[0014] Another advantage of the polyol ethers to be used according to the invention is that they are no longer migratory in the dried polymer film, in particular polyurethane film, especially when additional (hydrophilic) (poly) isocyanates or melamine-based crosslinkers are added to the system during drying.
[0015] An additional advantage of the polyol ethers used according to the invention is that they can lead to an increase in the viscosity of the foamed, undried dispersion. This, in turn, can have a beneficial effect on the processability of the foam. Furthermore, this may eliminate the need for additional thickening agents to adjust the foam viscosity, or allow for a reduction in their concentration, which offers economic advantages.
[0016] Another advantage of the polyol ethers used according to the invention is that they are not very susceptible or not at all susceptible to hard water.
[0017] A further advantage of the polyol ethers used according to the invention is that they provide sufficient stabilization of foams based on aqueous polymer dispersions even without the use of additional surfactants. This reduces the complexity for the user when formulating a suitable foam formulation.
[0018] A further advantage of the polyol ethers according to the invention is that they are characterized by excellent hydrolysis stability over a wide pH range.
[0019] For the purposes of the present invention, the term polyol ether also includes their alkoxylated adducts, which can be obtained by reacting a polyol ether with alkylene oxides such as ethylene, propylene and / or butylene oxide.
[0020] For the purposes of the present invention, the term polyol ether also includes polyol ester-polyol ether hybrid structures produced by O-alkylation of polyol esters (for the term polyol ester, see in particular the still unpublished European patent application 16180041.2) or by esterification of polyol ethers.
[0021] For the purposes of this entire invention, the term "polyol ether" also includes its ionic derivatives, preferably the phosphorylated and sulfated derivatives, in particular phosphorylated polyol ethers. These polyol ether derivatives, especially phosphorylated polyol ethers, are preferred polyol ethers according to the invention. They are described in more detail below.
[0022] The polyol ethers used according to the invention can be produced, in particular, by the O-alkylation of polyols or by the O-alkylation of hydroxy alkanes or hydroxy alkenes. This is generally known and described in detail in the technical literature (see, for example, Römpp or Ullmann's Encyclopedia of Industrial Chemistry "Acylation and Alkylation" and the literature cited therein). It is known that the formation of a carbon-oxygen bond to yield a corresponding polyol ether can be achieved by reacting a polyol with an acylating agent. Suitable alkylating agents include olefins, alkyl halides (Williamson ether synthesis), alcohols, ethers, epoxides, aldehydes, ketones, thiols, diazo compounds, sulfonic acid esters, and related compounds. Typical catalysts used when employing olefins as alkylating agents include, for example, H₂SO₄, acidic ion exchangers, phosphoric acid, and zeolites.In the Williamson ether synthesis, alcohols or polyols are first converted to their alcoholates by reaction with, for example, sodium or potassium, or sodium or potassium hydride, and then reacted with an alkyl halide as an alkylating agent. When using epoxides as alkylating agents, acids, Lewis acids, bases, and Lewis bases can be used as catalysts.
[0023] The invention is further described below by way of example, without being limited to these exemplary embodiments. Where ranges, general formulas, or compound classes are specified below, these are intended to include not only the corresponding ranges or groups of compounds explicitly mentioned, but also all sub-ranges and subgroups of compounds that can be obtained by extracting individual values (ranges) or compounds. Unless otherwise stated, percentages are given as weight percent. Where parameters determined by measurement are specified below, the measurements were carried out at a temperature of 25 °C and a pressure of 101,325 Pa, unless otherwise stated.
[0024] Within the scope of the present invention, such polyol ethers can be used which are obtainable by reacting a polyol with at least one linear or branched, saturated or unsaturated, primary or secondary alcohol or corresponding mixtures. This corresponds to one embodiment of the invention. Such polyol ethers are known per se and are described, for example, in WO2012082157 A2.
[0025] Furthermore, within the scope of the present invention, such polyol ethers can be used which are obtainable by reacting a polyol with at least one linear or branched alkyl or alkenyl halide or linear or branched alkyl or alkenyl sulfonic acid ester, such as tosylates, mesylates, triflates or nonaflates, or mixtures of such substances. This also corresponds to an embodiment of the invention. Such polyol ethers are also known per se.
[0026] Furthermore, within the scope of the present invention, such polyol ethers can be used which are obtainable by reacting a polyol with at least one linear or branched alkyl or alkenyl oxirane, thiirane, or aziridine, or mixtures of such substances. This also corresponds to an embodiment of the invention. Such polyol ethers are also known per se.
[0027] Furthermore, within the scope of the present invention, polyethers obtainable by reacting linear or branched, saturated or unsaturated, primary or secondary alcohols with glycidol or epichlorohydrin or glycerol carbonate, or mixtures of these substances, are preferably used. This also corresponds to a preferred embodiment of the invention. Such polyol ethers are also known per se.
[0028] Preferred polyols used for the production of the polyol ethers according to the invention are selected from the group of C3-C8 polyols and their oligomers. Particularly preferred polyols include 1,3-propanediol, propylene glycol, glycerol, trimethylolethane, trimethylolpropane, sorbitan, sorbitol, isosorbide, erythritol, threitol, pentaerythritol, arabitol, xylitol, ribitol, fucitol, mannitol, galactitol, iditol, inositol, volemitol, and glucose. Glycerol is especially preferred. Preferred polyol oligomers are oligomers of C3-C8 polyols with 1-20, preferably 2-10, and particularly preferably 2.5-8 repeating units. Particularly preferred are diglycerol, triglycerol, tetraglycerol, pentraglycerol, dierythritol, trierythritol, tetraerytritol, di-(trimethylolpropane), tri-(trimethylolpropane), and di- and oligosaccharides. Sorbitan and oligo- and / or polyglycerols are especially preferred.In particular, mixtures of different polyols can be used.
[0029] The term "polyglycerol" as used in the present invention refers to a polyglycerol which may also contain glycerol. Therefore, when calculating quantities, masses, and the like, the glycerol content must be taken into account. Polyglycerols as used in the present invention thus also include mixtures containing at least one glycerol oligomer and glycerol. Glycerol oligomers are understood to encompass all corresponding structures, e.g., linear, branched, and cyclic compounds. The same applies to the term "polyglycerol ether" as used in the present invention.
[0030] If linear or branched alkyl or alkenyl halides are used to produce the polyol ethers, halides corresponding to the general formula RX are particularly preferred, where X is a halogen atom, preferably a chlorine atom, more preferably a bromine atom, and more preferably an iodine atom, and where R is a linear or branched, saturated or unsaturated hydrocarbon residue with 4 to 40 carbon atoms, preferably 8 to 22, and particularly preferably with 10 to 18 carbon atoms. Particularly preferred are alkyl halides selected from 1-chlorooctane, 1-chlorodecane, 1-chlorodecane, 1-chlorotetradecane, 1-chlorohexadecane, 1-chlorooctadecane, 1-chloroicosane, 1-chlorodocosane and mixtures thereof, wherein 1-chlorohexadecane and 1-chlorooctadecane and mixtures of these two substances are particularly preferred.
[0031] Particularly preferred are alkyl halides selected from 1-bromooctane, 1-bromodecane, 1-bromododecane, 1-bromotetradecane, 1-bromohexadecane, 1-bromooctadecane, 1-bromeicosane, 1-bromodocosane and mixtures thereof, wherein 1-bromohexadecane and 1-bromooctadecane and mixtures of these two substances are particularly preferred.
[0032] Also particularly preferred are alkyl halides selected from 1-lodoctane, 1-loddecane, 1-loddodecane, 1-lodtetradecane, 1-lodhexadecane, 1-lodoctadecane, 1-lodeicosane, 1-loddocosane and mixtures thereof, wherein 1-lodhexadecane and 1-lodooctadecane and mixtures of these two substances are particularly preferred.
[0033] Also particularly preferred are alkyl halides selected from 2-chlorooctane, 2-chlorodecane, 2-chlorodecane, 2-chlorotetradecane, 2-chlorohexadecane, 2-chlorooctadecane, 2-chloroicosane, 2-chlorodocosane and mixtures thereof, wherein 2-chlorohexadecane and 2-chlorooctadecane and mixtures of these two substances are particularly preferred.
[0034] Also particularly preferred are alkyl halides selected from 2-bromooctane, 2-bromodecane, 2-bromododecane, 2-bromotetradecane, 2-bromohexadecane, 2-bromooctadecane, 2-bromeicosane, 2-bromodocosane and mixtures thereof, wherein 2-bromohexadecane and 2-bromooctadecane and mixtures of these two substances are particularly preferred.
[0035] Also particularly preferred are alkyl halides selected from 2-lodoctane, 2-loddecane, 2-loddodecane, 2-lodtetradecane, 2-lodhexadecane, 2-lodoctadecane, 2-lodeicosane, 2-loddocosane and mixtures thereof, wherein 2-lodhexadecane and 2-lodooctadecane and mixtures of these two substances are particularly preferred.
[0036] If alkyl epoxides are used to produce the polyol ethers, alkyl epoxides corresponding to general formula 1 are particularly preferred. wherein R' are independently identical or different monovalent aliphatic, saturated or unsaturated hydrocarbon residues with 2 to 38 carbon atoms, preferably 6 to 20, particularly preferably with 8 to 18 carbon atoms or hydrogen, provided that at least one of the residues is a hydrocarbon residue. Alkyl epoxides in which exactly one of the residues R' is a hydrocarbon residue and the other is hydrogen are particularly preferred. Epoxides derived from C6-C24 alpha-olefins are most particularly preferred.
[0037] If alkyl glycidyl ethers are used to produce the polyol ethers, they are preferably selected from the group of linear or branched, saturated or unsaturated alkyl alcohols with 4 to 40 carbon atoms, preferably 8 to 22, and particularly preferably with 10 to 18 carbon atoms. Particularly preferred are alkyl glycidyl ethers selected from octyl glycidyl ether, decyl glycidyl ether, dodecyl glycidyl ether, tetradecyl glycidyl ether, hexadecyl glycidyl ether, octadecyl glycidyl ether, eicosyl glycidyl ether, docosyl glycidyl ether, and mixtures thereof, with hexadecyl glycidyl ether and octadecyl glycidyl ether, as well as mixtures of these two substances, being particularly preferred. In a particularly preferred embodiment of the present invention, the polyol ethers are selected from the group of sorbitan ethers and / or polyglycerol ethers.Particularly preferred are polyglycerol hexadecyl ethers, polyglycerol octadecyl ethers, and mixtures of these two substances. Very preferred are polyglycerol hydroxyhexadecyl ethers and polyglycerol hydroxyoctadecyl ethers, and mixtures of these substances. Even more preferred are polyglycerol (1-hydroxyhexadecyl) ethers, polyglycerol (2-hydroxyhexadecyl) ethers, polyglycerol (1-hydroxyoctadecyl) ethers, and polyglycerol (2-hydroxyoctadecyl) ethers, and mixtures of these substances.
[0038] Particularly preferred are polyglycerol ethers which correspond to the general formula 2: M a D b T c Formula 2 where M = [C 3 H 5 (OR") 2 O 1 / 2 ] D = [C 3 H 5 (OR") 1 O 2 / 2 ] T = [C 3 H 5 O 3 / 2 ] a = 1 to 10, preferably 2 to 3, particularly preferably 2 b = 0 to 10, preferably greater than 0 to 5, particularly preferably 1 to 4, c = 0 to 3, preferably 0 wherein the residues R" are independently of one another identical or different monovalent aliphatic, saturated or unsaturated hydrocarbon residues with 2 to 38 C atoms, preferably 6 to 20, particularly preferably with 8 to 18 carbon atoms or H, provided that at least one of the residues R" is a hydrocarbon residue which may also bear substituents, in particular hydroxyl groups.
[0039] Even more preferred are polyglycerol ethers, which correspond to the general formula 3: M x D y T z Formula 3 where x = 1 to 10, preferably 2 to 3, particularly preferably 2, y = 0 to 10, preferably greater than 0 to 5, particularly preferably 1 to 4, z = 0 to 3, preferably greater than 0 to 2, particularly preferably 0, provided that at least one residue R" is not hydrogen, and furthermore R" as defined above.
[0040] Polyglycerol ethers of general formula 4 are also preferred: where k = 1 to 10, preferably 2 to 3, particularly preferably 2, m = 0 to 10, preferably greater than 0 to 5, particularly preferably 1 to 3, provided that at least one residue R" is not hydrogen, furthermore R" as defined above, and that the sum k + m is greater than zero and the fragments with the indices k and m are statistically distributed.
[0041] Statistical distributions are structured block-wise with any number of blocks and any sequence or randomized distribution. They can also be structured alternately or form a gradient over the chain; in particular, they can also form all mixed forms, in which groups of different distributions may follow one another. Specific implementations can lead to restrictions being imposed on the statistical distributions. For all regions not affected by the restriction, the statistical distribution remains unchanged.
[0042] Preferably, the polyglycerol ethers that can be used according to the invention have no more than 6, more preferably no more than 5, and more preferably no more than 4 hydrocarbon residues of the form R", as described above.
[0043] Structurally, polyol ethers can be characterized by wet chemical parameters such as their hydroxyl number. Suitable methods for determining the hydroxyl number include those according to DGF CV 17 a (53), Ph. Eur. 2.5.3 Method A, and DIN 53240. Suitable methods for determining the acid number include those according to DGF CV 2, DIN EN ISO 2114, Ph. Eur. 2.5.1, ISO 3682, and ASTM D 974. Suitable methods for determining the saponification number include those according to DGF CV 3, DIN EN ISO 3681, and Ph. Eur. 2.5.6.
[0044] Suitable methods for determining the epoxy oxygen content are in particular those according to R. Kaiser "Quantitative Determination of Organic Functional Groups: Methods of Analysis in Chemistry", Akad. Verlagsgesellschaft, 1966 and RR Jay, Anal. Chem. 1964, 36 (3), 667-668.
[0045] Suitable methods for determining the melting point are in particular those according to DIN 53181 , DIN EN ISO 3416 , DGF C-IV 3a and Ph.Eur.2.2.14.
[0046] According to the invention, it is preferred and corresponds to a particularly preferred embodiment of the invention if a polyglycerol with a mean degree of condensation of 1–20, preferably 2–10, and particularly preferably 2.5–8, is used to produce the polyglycerol ether. The mean degree of condensation N can be determined here based on the OH number ( OHZ , in mg KOH / g) of the polyglycerol and is linked to this according to: N = 112200 − 18 ⋅ OHZ 75 ⋅ OHZ − 56100
[0047] The OH number of the polyglycerol can be determined as described above. Consequently, polyglycerols with an OH number of 1829 to 824, particularly preferably 1352 to 888, and especially preferably 1244 to 920 mg KOH / g, are particularly preferred for the production of the polyglycerol ethers according to the invention.
[0048] The polyglycerol used can be provided by various conventional methods, such as polymerization of glycidol (e.g., base-catalyzed), polymerization of epichlorohydrin (e.g., in the presence of equimolar amounts of a base such as NaOH), or polycondensation of glycerol. This is known from the literature.
[0049] It has already been clarified that the term "polyol ethers" within the meaning of the present invention also includes their ionic derivatives, preferably the phosphorylated and sulfated derivatives, and in particular phosphorylated polyol ethers. Phosphorylated polyol ethers are obtained by reacting the polyol ethers with a phosphorylation reagent and optional, preferably mandatory, subsequent neutralization (see in particular *Industrial Applications of Surfactants. II. Preparation and Industrial Applications of Phosphate Esters*, edited by Dr. Dr. Karsa, Royal Society of Chemistry, Cambridge, 1990). Preferred phosphorylation reagents within the meaning of this invention are phosphorus oxychloride, phosphorus pentoxide (P₄O₁₀), and, most preferably, polyphosphoric acid.The term phosphorylated polyol ethers, within the meaning of the entire present invention, also covers partially phosphorylated polyol ethers, and likewise the term sulfated polyol ethers, within the meaning of the entire present invention, also covers partially sulfated polyol ethers.
[0050] Furthermore, ionic derivatives of the polyol ethers can also be obtained in accordance with the present invention by reacting the polyethers with di- or tricarboxylic acid or corresponding cyclic anhydrides and optional, preferably mandatory, neutralization.
[0051] Furthermore, ionic derivatives of the polyol ethers can also be obtained in accordance with the present invention by reacting the polyethers with unsaturated di- or tricarboxylic acids or corresponding cyclic anhydrides and subsequent sulfonation as well as optional, preferably mandatory, neutralization.
[0052] The term neutralization, as used in the present invention, also encompasses partial neutralization. Conventional bases can be used for neutralization, including partial neutralization. These include water-soluble metal hydroxides, such as barium, strontium, calcium, and thallium(I) hydroxides, and preferably alkali metal hydroxides, which dissociate into free metal and hydroxide ions in aqueous solutions, particularly NaOH and KOH. This also includes anhydrobases that react with water to form hydroxide ions, such as barium oxide, strontium oxide, calcium oxide, lithium oxide, silver oxide, and ammonia. In addition to these aforementioned alkalis, solid substances that also react alkaline when dissolved in water, but without possessing HO- (in the solid compound), can also be used as bases. These include, for example...Amines such as mono-, di- and trialkylamines, which can also be functionalized alkyl groups such as in amidamines, mono-, di- and trialkanolamines, mono-, di- and triaminoalkylamines and e.g. the salts of weak acids such as potassium cyanide, potassium carbonate, sodium carbonate, trisodium phosphate etc.
[0053] Particularly preferred polyol ethers within the meaning of this invention are phosphorylated sorbitan ethers and / or phosphorylated polyglycerol ethers, especially phosphorylated polyglycerol ethers. In particular, a phosphorylated and neutralized polyglycerol hexadecyl ether, a phosphorylated and neutralized polyglycerol octadecyl ether, or a mixture of these substances are preferred.
[0054] A particularly preferred embodiment of this invention provides for the use of polyol ethers of formula 2, 3 and / or 4, as previously described, with the additional requirement that these are (at least partially) phosphorylated, such that these polyol ethers of formula 2, 3 and / or 4 bear, in particular as residue R" at least one residue (R‴O)₂P(O)⁻, wherein the residues R‴ are independently of one another cations, preferably Na⁺, K⁺ or NH₄⁺, or ammonium ions of mono-, di- and trialkylamines, which may also be functionalized alkyl residues such as, for example, amidamines, of mono-, di- and trialkanolamines, of mono-, di- and triaminoalkylamines or H or Rʺʺ-O⁻, wherein Rʺʺ is a monovalent aliphatic, saturated or unsaturated hydrocarbon residue with 3 to 39 C atoms, preferably 7 to 22, particularly preferably with 9 to 18 carbon atoms or a polyol residue.
[0055] Of the sulfated polyol ethers, those that can be obtained by reacting the polyol ethers with sulfur trioxide or sulfonic acid are particularly preferred. Sulfated sorbitan ethers and / or sulfated polyglycerol ethers are especially favored.
[0056] In a particularly preferred embodiment of the present invention, polyol ethers are not used pure, but in mixtures with at least one co-surfactant as additives in aqueous polymer dispersions. Preferred co-surfactants according to the invention are, for example, fatty acid amides, alkyl alkoxylates such as fatty alcohol ethoxylates, nonylphenol ethoxylates, ethylene oxide-propylene oxide block copolymers, betaines such as amidopropyl betaines, amine oxides, quaternary ammonium surfactants, or amphoacetates. Furthermore, the co-surfactant can be a silicone-based surfactant, such as trisiloxane surfactants or polyether siloxanes.
[0057] Particularly preferred co-surfactants are ionic, and preferably anionic, co-surfactants. Preferred anionic co-surfactants include ammonium and / or alkali salts of fatty acids, alkyl sulfates, alkyl ether sulfates, alkyl sulfonates, alkylbenzenesulfonates, alkyl phosphates, alkyl sulfosuccinates, alkyl sulfosuccinamates, and alkyl sarcosinates. Alkyl sulfates with 12-20 carbon atoms are particularly preferred, more preferably with 14-18 carbon atoms, and even more preferably with more than 16-18 carbon atoms. In the case of ammonium and / or alkali salts of fatty acids, it is preferred that they contain less than 25 wt% stearate salts, and in particular, are free of stearate salts.
[0058] When using co-surfactants, it is particularly preferred if the proportion of co-surfactant relative to the total amount of polyol ether plus co-surfactant is in the range of 0.1 - 50 wt.%, preferably in the range of 0.2 - 40 wt.%, more preferably in the range of 0.5 - 30 wt.%, and even more preferably in the range of 1 - 25 wt.%.
[0059] As previously described, an object of the present invention is the use of polyol ethers as additives in aqueous polymer dispersions for the production of porous polymer coatings. The polymer dispersions are preferably selected from the group consisting of aqueous polystyrene dispersions, polybutadiene dispersions, poly(meth)acrylate dispersions, polyvinyl ester dispersions, and polyurethane dispersions. The solids content of these dispersions is preferably in the range of 20–70 wt.%, more preferably in the range of 25–65 wt.%. The use of polyol ethers as additives in aqueous polyurethane dispersions is particularly preferred according to the invention. Polyurethane dispersions based on polyester, polyesteramide, polycarbonate, polyacetal, and polyether polyols are especially preferred.
[0060] The concentration of the polyol ethers according to the invention in aqueous polymer dispersions is preferably in the range of 0.2 - 10 wt.%, particularly preferably in the range of 0.4 - 7.5 wt.%, and especially preferably in the range of 0.5 - 5 wt.% based on the total weight of the dispersion.
[0061] The polyol ethers can be added to the aqueous dispersion either pure or diluted in a suitable solvent. Preferred solvents are selected from water, propylene glycol, dipropylene glycol, polypropylene glycol, butyldiglycol, butyltriglycol, ethylene glycol, diethylene glycol, polyethylene glycol, polyalkylene glycols based on EO, PO, BO and / or SO, as well as mixtures of these substances. In the case of aqueous dilutions or mixtures of the polyol ethers according to the invention, it can be advantageous to add hydrotropic compounds to the mixture to improve the formulation properties (viscosity, homogeneity, etc.). Hydrotropic compounds are water-soluble organic compounds consisting of a hydrophilic and a hydrophobic part, but which are too low in molecular weight to exhibit surfactant properties. They lead to an improvement in solubility and / or...the solubility properties of organic, in particular hydrophobic, organic substances in aqueous formulations. The term hydrotropic compounds is known to those skilled in the art. Within the scope of the present invention, alkali and ammonium toluenesulfonates, alkali and ammonium xylenesulfonates, alkali and ammonium naphthalenesulfonates, alkali and ammonium cumenesulfonates, and phenol alkoxylates, in particular phenol ethoxylates with up to 6 alkoxylate units, are preferred as hydrotropic compounds.
[0062] In addition to the polyol ethers according to the invention, the aqueous polymer dispersions may contain further additives such as fillers, organic and inorganic pigments, matting agents, stabilizers such as hydrolysis or UV stabilizers, antioxidants, absorbers, crosslinkers, leveling additives, thickeners or possibly other co-surfactants, as described above.
[0063] The polyol ethers according to the invention are preferably used in aqueous polymer dispersions as foaming aids or foam stabilizers to foam the dispersions. However, they can also be used as drying aids, leveling agents, wetting agents, and rheology additives.
[0064] Since, as described above, the polyol ethers lead to a significant improvement in porous polymer coatings produced from aqueous polymer dispersions, aqueous polymer dispersions containing at least one of the polyol ethers according to the invention, as previously described in detail, are also the subject of the present invention.
[0065] Another object of the present invention is porous polymer layers produced from aqueous polymer dispersions, obtained using the polyol ethers according to the invention as additives, as previously described in detail.
[0066] Preferably, the porous polymer coatings according to the invention can be produced by a process comprising the steps a) Providing a mixture containing an aqueous polymer dispersion as described above, at least one of the polyol ethers according to the invention, and optionally further additives. b) Foaming the mixture into a homogeneous, fine-celled foam. c) Optionally adding at least one thickener to adjust the viscosity of the wet foam. d) Applying a coating of the foamed polymer dispersion to a suitable substrate. e) Drying the coating.
[0067] With regard to preferred embodiments, in particular with regard to the polyol ethers and aqueous polymer dispersions that can preferably be used in the process, reference is made to the preceding description and also to the previously mentioned preferred embodiments, in particular as described in claims 2-11.
[0068] It is clarified that the process steps of the method according to the invention, as described above, are not subject to a fixed temporal sequence. For example, process step c) can be carried out simultaneously with process step a).
[0069] It is a preferred embodiment of the present invention if, in process step b), the aqueous polymer dispersion is foamed by applying high shear forces. The foaming can be carried out using shear units familiar to those skilled in the art, such as dispersants, dissolvers, Hansa mixers, or Oakes mixers.
[0070] Furthermore, it is preferred that the wet foam produced at the end of process step c) has a viscosity of at least 3, preferably at least 5, more preferably at least 7.5, and even more preferably at least 10 Pa s. The viscosity of the foam can be determined, for example, using a Brookfield viscometer, model LVTD, equipped with an LV-4 spindle. Corresponding measurement methods for determining the wet foam viscosity are known to those skilled in the art.
[0071] As described above, additional thickeners can be added to the system for adjusting the wet foam viscosity.
[0072] Preferred thickeners that can advantageously be used within the scope of the invention are selected from the class of associative thickeners. Associative thickeners are substances that produce a thickening effect by association with the surfaces of the particles contained in the polymer dispersions. The term is familiar to those skilled in the art. Preferred associative thickeners are selected from polyurethane thickeners, hydrophobically modified polyacrylate thickeners, hydrophobically modified polyether thickeners, and hydrophobically modified cellulose ethers. Polyurethane thickeners are particularly preferred. Furthermore, within the scope of the present invention, it is preferred that the concentration of the thickeners, based on the total composition of the dispersion, is in the range of 0.01–10 wt.%, more preferably in the range of 0.05–5 wt.%, and most preferably in the range of 0.1–3 wt.%.
[0073] Within the scope of the present invention, it is further preferred that in process step d) coatings of the foamed polymer dispersion with a layer thickness of 10–10,000 µm, preferably 50–5,000 µm, more preferably 75–3,000 µm, and even more preferably 100–2,500 µm, are produced. These coatings of the foamed polymer dispersion can be produced by methods familiar to those skilled in the art, such as applying them with a doctor blade. Both direct and indirect coating processes (so-called transfer coating) can be used.
[0074] Furthermore, within the scope of the present invention, it is preferred if, in process step e), the drying of the foamed and coated polymer dispersion takes place at elevated temperatures. According to the invention, drying temperatures of at least 50 °C, preferably 60 °C, and more preferably at least 70 °C are preferred. It is also possible to dry the foamed and coated polymer dispersions in multiple stages at different temperatures to avoid the occurrence of drying defects. Corresponding drying techniques are widespread in industry and known to those skilled in the art.
[0075] As already described, process steps c) - e) can be carried out using common methods known to those skilled in the art. An overview of these methods is given, for example, in "Coated and laminated Textiles" (Walter Fung, CR-Press, 2002).
[0076] Within the scope of the present invention, porous polymer coatings containing polyol ethers are particularly preferred, which have a mean cell size of less than 250 µm, preferably less than 150 µm, particularly preferably less than 100 µm, and most preferably less than 75 µm. The mean cell size can preferably be determined microscopically, preferably by electron microscopy. For this purpose, a cross-section of the porous polymer coating is viewed using a microscope with sufficient magnification, and the size of at least 25 cells is determined. To obtain sufficient statistical data from this evaluation method, the magnification of the microscope should preferably be selected such that at least 10 x 10 cells are within the field of view. The mean cell size is then calculated as the arithmetic mean of the viewed cells or cell sizes. This method of cell size determination using microscopy is familiar to those skilled in the art.
[0077] The porous polymer layers (or polymer coatings) containing polyol ethers according to the invention can be used, for example, in the textile industry, e.g., for artificial leather materials, in the building and construction industry, in the electronics industry, e.g., for foamed seals, in the sports industry, e.g., for the production of sports mats, or in the automotive industry. Examples
[0078] Substances: Impranil®< DLU: aliphatic polycarbonate ester polyether polyurethane dispersion from Covestro Stokal®< STA: ammonium stearate (approx. 30% in H₂O) from Bozetto Stokal®< SR: talc-based sodium sulfosuccinamate (approx. 35% in H₂O) from Bozetto Tego®< Viscoplus 3030: polyurethane-based associative thickener from Evonik Industries AG.
[0079] Viscosity measurements: All viscosity measurements were performed using a Brookfield LVTD viscometer equipped with an LV-4 spindle, at a constant rotation speed of 12 rpm. For the viscosity measurements, the samples were placed in a 100 ml glass container into which the measuring spindle was immersed. The measurement was always delayed until the viscometer displayed a constant reading. Example 1A: Synthesis of polyglyceryl hydroxystearyl ethers
[0080] A mixture of commercially available polyglycerol-3 (Spiga Nord, hydroxyl value 1124 mg KOH / g, 52.5 g, 0.219 mol, 1.0 equiv.) and sodium methoxide (1.96 g of a 25% solution in methanol, 0.009 mol, 0.04 equiv.) was heated to 180 °C within 2 h under stirring and nitrate injection at 15 mbar, and the methanol was distilled off. After reaching 180 °C, the vacuum was broken, and then 1,2-epoxyoctadecane (CAS RN 7390-81-0, 85%, 97.0 g, 0.361 mol, 1.65 equiv.), heated to 80 °C, was slowly added dropwise over 1 h. The mixture was stirred for a further 4 h at 180 °C until an epoxy oxygen content of 0.16% was reached. The mixture was then cooled to 90 °C and the phases separated. 5.6 g of unreacted polyglycerol (lower phase) and 113 g of polyglyceryl hydroxyalkyl ether (upper phase, melting point = 71.5 °C, hydroxyl value = 387 mg KOH / g, acid value = 0.4 mg KOH / g, epoxy oxygen content = 0.06%) were obtained. Example 1B: Phosphorylation of Polyglyceryl hydroxystearyl ether
[0081] A mixture of a polyglyceryl hydroxyalkyl ether (97.62 g, obtained as described in Example 1A) and polyphosphoric acid (115% H₃PO₄, 2.38 g) was heated to 80 °C for 4 h with stirring. The mixture then had an acid number of 27.6 mg KOH / g. Subsequently, 45% aqueous KOH solution (9.77 g) was added at 80 °C and stirred for a further 30 min at 80 °C. The mixture then had an acid number of 1.3 mg KOH / g. Example 1C: Synthesis of a polyglyceryl hydroxystearyl ether stearate
[0082] A mixture of a polyglyceryl hydroxyalkyl ether (150 g, obtained as described in Example 1A) and stearic acid (44.3 g, 0.156 mol) was heated to 240 °C for 3 h with stirring and introduction of nitrogen, and stirred at 240 °C until an acid number of ≤1 mg KOH / g was reached. 186 g of polyglyceryl hydroxystearyl ether stearate was obtained (hydroxyl number = 264 mg KOH / g, acid number = 0.6 mg KOH / g, saponification number 44 mg KOH / g). Example 2A: Synthesis of Polyglyceryl hydroxystearyl ether
[0083] A mixture of commercially available polyglycerol-3 (Spiga Nord, hydroxyl value 1124 mg KOH / g, 52.6 g, 0.219 mol, 1.0 equiv.) and concentrated sulfuric acid (0.36 g) was heated to 100 °C within 1 h under stirring and nitrogen introduction at 15 mbar. After reaching 100 °C, the vacuum was broken, and then 1,2-epoxyoctadecane (CAS RN 7390-81-0, 85%, 97.1 g, 0.362 mol, 1.65 equiv.), preheated to 80 °C, was slowly added dropwise over 1 h. The mixture was stirred for a further 4 h at 100 °C until an epoxy oxygen content of 0.01% was reached. The mixture was then cooled to 90 °C and the phases separated. 22.8 g of unreacted polyglycerol (lower phase) and 113.8 g of polyglyceryl hydroxystearyl ether (upper phase, melting point = 49.5 °C, hydroxyl value = 268 mg KOH / g, acid value = 0.6 mg KOH / g, epoxy oxygen content = 0.01%) were obtained. Example 2B: Phosphorylation of Polyglyceryl hydroxystearyl ether
[0084] A mixture of a polyglyceryl hydroxyalkyl ether (98.81 g) obtained as described in Example 2A and polyphosphoric acid (115% H₃PO₄, 1.19 g) was heated to 80 °C for 4 h with stirring. The mixture then had an acid number of 12 mg KOH / g. Subsequently, 45% aqueous KOH solution (2.67 g) was added at 80 °C and stirred for a further 30 min at 80 °C. The mixture then had an acid number of 1.0 mg KOH / g. Example 2C: Synthesis of potassium- Polyglyceryl hydroxystearyl ether -Succinate
[0085] A Polyglyceryl hydroxyalkyl ether (300 g) obtained as described in Example 2A was heated to 80 °C and, while stirring, succinic anhydride (9.15 g) was added portionwise over 1 h. The mixture was stirred for a further 2 h at 80 °C until an acid number of 19.2 mg KOH / g was reached. Subsequently, 12.90 g of a 45% aqueous KOH solution was added and the mixture was stirred for a further 15 min. The potassium- obtained Polyglyceryl hydroxystearyl ether-Succinate had an acid number of 8.0 mg KOH / g. Example 3: Formulation and blending of surfactants according to the invention
[0086] The surfactants according to the invention from example 1 AC and 2 AC were blended according to the compositions listed in Tables 1 and 2 and then homogenized at 80 °C: Table 1: Composition of the surfactant mixtures used below Surfactant 1 Surfactant 2 Surfactant 3 Polyglycerol hydroxystearyl ether (from Example 1A) 19,7 g --- --- Phosphorylated polyglycerol hydroxystearyl ether (from Example 1B) --- 21,3 g --- Polyglycerol hydroxystearyl ether stearate (from Example 1 C) --- --- 19,7 g Cetearyl sulfate 1,6 g --- 1,6 g Water 59,1 g 59,1 g 59,1 g Propylene glycol 6,25 g 6,25 g 6,25 g Table 2: Composition of the surfactant mixtures used below Surfactant 4 Surfactant 5 Surfactant 6 Polyglycerol hydroxystearyl ether (from Example 2A) 19,7 g --- --- Phosphorylated polyglycerol hydroxystearyl ether (from Example 2B) --- 21,3 g --- Potassium- Polyglyceryl hydroxystearyl ether -Succinate (from Example 2 C) --- --- 21,3 g Cetearyl sulfate 1,6 g --- --- Water 59,1 g 59,1 g 59,1 g Propylene glycol 6,25 g 6,25 g 6,25 g Example 4:
[0087] 150 g of the Impranil®< DLU dispersion were placed in a 500 ml plastic beaker and stirred for 3 minutes at 800 rpm using a VMA Getzmann dissolver equipped with a 6 cm diameter dissolver disc. During this time, the surfactant was slowly added using a syringe. The exact compositions of the samples are listed in Tables 3 and 4.
[0088] To foam the mixtures, the shear rate was then increased to 2000 rpm, ensuring that the dissolver disc was always immersed in the dispersion sufficiently to form a proper vortex. At this speed, the mixtures were foamed to a volume of approximately 425 ml. The shearing time required for this is also noted in Tables 3 and 4. The shear rate was then reduced to 1000 rpm; Tego® Viscoplus 3030 was added using a syringe and sheared again for 15 minutes. In this step, the dissolver disc was immersed in the mixtures to such a depth that no further air was introduced into the system, while the entire volume remained in motion.
[0089] In all cases, fine, homogeneous foams were obtained at the end of this foaming process. It was noteworthy that the foams produced with the surfactants 1-6 according to the invention exhibited a higher viscosity despite a lower thickener concentration (see Tables 3 and 4). The foams were coated onto a siliconized polyester film using a film-drawing machine (type AB3220 from TQC) equipped with a box doctor blade (blade thickness = 800 µm) and then dried for 10 minutes at 60 °C and for a further 5 minutes at 120 °C.
[0090] Compared to sample 1, the dried samples 2-7 according to the invention were characterized by a more homogeneous macroscopic appearance and a more velvety feel. The cell structure of the dried samples was evaluated using scanning electron microscopy. In the case of the comparison sample 1, an average cell size of approximately 120 µm was observed, while samples 2 and 3 according to the invention exhibited a significantly finer cell size of approximately 55 µm. Table 3: Overview of the foams produced in Example 4 Sample 1 Sample 2 Sample 3 Sample 4 Impranil®< DLU 150 g 150 g 150 g 150 g Stokal ®< STA 2,4 g Stokal ®< SR 1,8 g Surfactant 1 4 g Surfactant 2 4 g Surfactant 3 4 g Tego® Viscoplus 3030 0,7 g 0,2 g 0,2 g 0,2 g Scherdauer 3 min 4.5 min 4 min 3.5 min Foam viscosity 14 Pa s 21 Pa s 18.5 Pa s 19 Pa s Cell size End foam approx. 120 µm approx. 55 µm approx. 55 µm Approx. 55 µm Table 4: Overview of the foams produced in Example 4 Sample 5 Sample 6 Sample 7 Impranil®< DLU 150 g 150 g 150 g Surfactant 4 4 g Surfactant 5 4 g Surfactant 6 4 g Tego® Viscoplus 3030 0,2 g 0,2 g 0,2 g Scherdauer 4 min 4 min 4.5 min Foam viscosity 17 Pa s 20.5 Pa s 19 Pa s Cell size End foam approx. 55 µm approx. 55 µm approx. 55 µm Example 5:
[0091] The compositions listed in Tables 3 and 4 were foamed analogously to the method described in Example 4 and coated onto a siliconized polyester film using a box doctor blade (blade thickness = 800 µm). However, the samples were dried this time for only 5 minutes at 90 °C and for 3 minutes at 120 °C. It was observed that the control sample 1 exhibited significant defects (drying cracks) after drying, while the samples 2-7 according to the invention dried without defects despite the shortened, more intense drying conditions.
[0092] Additionally, a coating with a doctor blade thickness of 2000 µm was produced on all samples. This coating was dried for 10 min at 60 °C, for 10 min at 90 °C, and for 10 min at 120 °C. Here too, samples 2–7, which contained the surfactants according to the invention, dried without defects, while the control sample showed significant drying cracks 1.
Claims
1. Use of polyol ethers as additives in aqueous polymer dispersions for production of porous polymer coatings, wherein the polyol ethers are obtainable by the reaction of a polyol with at least one alkyl halide or alkylene halide, at least one primary or secondary alcohol or else at least one alkyl- or alkenyloxirane, thiirane or aziridine, or obtainable by the reaction of primary or secondary alcohols with glycidol, epichlorohydrin and / or glycerol carbonate, wherein the polyols are selected from the group of the C3-C8 polyols and oligomers thereof.
2. Use according to Claim 1, wherein the polyol ethers are obtainable by the reaction of a polyol with at least one alkyl halide.
3. Use according to Claim 1 or 2, wherein the polyols are propane-1,3-diol, propylene glycol, glycerol, trimethylolethane, trimethylolpropane, sorbitan, sorbitol, isosorbide, erythritol, threitol, pentaerythritol, arabitol, xylitol, ribitol, fucitol, mannitol, galactitol, iditol, inositol, volemitol and glucose, especially glycerol, and wherein preferred polyol oligomers are the oligomers of C3-C8 polyols having 1-20, preferably 2-10 and more preferably 2.5-8 repeat units, particular preference being given here to diglycerol, triglycerol, tetraglycerol, pentaglycerol, dierythritol, trierythritol, tetraerythritol, di(trimethylolpropane), tri(trimethylolpropane) and di- and oligosaccharides, especially sorbitan and oligo- and / or polyglycerols.
4. Use according to any of Claims 1 to 3, characterized in that the alkyl halide conforms to the general formula R-X where X is a halogen atom, preferably a chlorine atom, and where R is a linear or branched, saturated or unsaturated hydrocarbon radical having 4 to 40 carbon atoms, preferably 8 to 22 and more preferably 10 to 18 carbon atoms, and wherein preferred alkyl halides are selected from 1-chlorohexadecane, 1-chlorooctadecane, 2-chlorohexadecane, 2-chlorooctadecane, 1-bromohexadecane, 1-bromooctadecane, 2-bromohexadecane, 2-bromooctadecane, 1-iodohexadecane, 1-iodooctadecane, 2-iodohexadecane and / or 2-iodooctadecane, particular preference being given to mixtures of at least two alkyl chlorides.
5. Use according to any of Claims 1 to 4, characterized in that the alkyl epoxide conforms to the general formula 1: where R' are independently identical or different monovalent aliphatic saturated or unsaturated hydrocarbon radicals having 2 to 38 carbon atoms, preferably 6 to 20, more preferably having 8 to 18 carbon atoms, or H, with the proviso that at least one of the radicals is a hydrocarbon radical, particular preference here being given to alkyl epoxides in which exactly one of the radicals is a hydrocarbon radical, especially preferably epoxides that derive from C6-C24 alpha-olefins.
6. Use according to one of Claims 1 to 5, characterized in that the polyol ethers used include those that are selected from the group of the sorbitan ethers and / or polyglycerol ethers, preferably polyglycerol ethers, preferably those polyglycerol ethers which conform to the general formula 2: MaDbTc Formula 2 where M = [C3H5(OR")2O1 / 2] D = [C3H5(OR")1O2 / 2] T = [C3H5O3 / 2] a = 1 to 10, preferably 2 to 3, more preferably 2, b = 0 to 10, preferably greater than 0 to 5, especially preferably 1 to 4, c = 0 to 3, preferably 0, where the R' ' radicals are independently identical or different monovalent aliphatic saturated or unsaturated hydrocarbon radicals having 2 to 38 carbon atoms, preferably 6 to 20, more preferably having 8 to 18 carbon atoms, or H, with the proviso that at least one of the R'' radicals is a hydrocarbon radical, and / or conform to the general formula 3: MxDyTz Formula 3 where x = 1 to 10, preferably 2 to 3, especially preferably 2, y = 0 to 10, preferably greater than 0 to 5, especially preferably 1 to 4, z = 0 to 3, preferably greater than 0 to 2, especially preferably 0, with the proviso that at least one R' ' radical is not hydrogen, still R'' as defined above, and / or conform to the general formula 4: where k = 1 to 10, preferably 2 to 3, especially preferably 2, m = 0 to 10, preferably greater than 0 to 5, especially preferably 1 to 3, with the proviso that at least one of the R" radicals is not hydrogen, still R'' as defined above, and that the sum total of k + m is greater than zero and the fragments having the indices k and m are distributed statistically.
7. Use according to Claim 6, characterized in that the polyol ethers of the formula 2, 3 and / or 4 have been phosphorylated, especially bear at least one (R‴O)2P(O)- radical as the R" radical, where the R‴ radicals are independently cations, preferably Na+, K+ or NH4+, or ammonium ions of mono-, di- and trialkylamines, which may also be functionalized alkyl radicals as, for example, in the case of amide amines, of mono-, di- and trialkanolamines, of mono-, di- and triaminoalkylamines, or H or Rʺʺ-O-, where Rʺʺ is a monovalent aliphatic saturated or unsaturated hydrocarbon radical having 3 to 39 carbon atoms, preferably 7 to 22, more preferably having 9 to 18 carbon atoms, or a polyol radical.
8. Use according to any of Claims 1 to 7, characterized in that the polyol ethers are used in a blend with at least one ionic, preferably anionic, co-surfactant as additives in aqueous polymer dispersions, preferred ionic co-surfactants being the ammonium and alkali metal salts of fatty acids, alkyl sulfates, alkyl ether sulfates, alkylsulfonates, alkylbenzenesulfonates, alkyl phosphates, alkyl sulfosuccinates, alkyl sulfosuccinamates and alkyl sarcosinates, preference being given especially to alkyl sulfates having 12-20 carbon atoms, further preferably having 14-18 carbon atoms, even more preferably having more than 16-18 carbon atoms, with the proviso that the proportion of ionic co-surfactant based on the total amount of polyol ether plus co-surfactant is preferably in the range of 0.1-50% by weight, preferably in the range of 0.2-40% by weight, more preferably in the range of 0.5-30% by weight, even more preferably in the range of 1-25% by weight.
9. Use according to any of Claims 1 to 8, characterized in that the aqueous polymer dispersions are selected from the group of aqueous polystyrene dispersions, polybutadiene dispersions, poly(meth)acrylate dispersions, polyvinyl ester dispersions and polyurethane dispersions, especially polyurethane dispersions, where the solids content of these dispersions is preferably in the range of 20-70% by weight, more preferably in the range of 25-65% by weight.
10. Use according to any of Claims 1 to 9, characterized in that the use concentration of the polyol ethers in the aqueous polymer dispersion is in the range of 0.2-10% by weight, more preferably of 0.4-7.5% by weight, especially of 0.5-5% by weight, based on the total weight of the dispersion.
11. Use according to any of Claims 1 to 10, characterized in that the polyol ethers serve as foaming aids or foam stabilizers for foaming of the aqueous polymer dispersions, and as a drying aid, levelling additive, wetting agent and / or rheology additive.
12. Process for producing a porous polymer coating, preferably porous polyurethane coating, using polyol ethers as additives in aqueous polymer dispersions, comprising the steps of a) providing a mixture comprising an aqueous polymer dispersion, at least one polyol ether according to any of Claims 1 to 11, preferably comprising sorbitan ethers and / or polyglycerol ethers, and optionally further additives, b) foaming the mixture to give a preferably homogeneous, fine-cell foam, c) optionally adding at least one thickener to establish the desired viscosity of the wet foam, d) applying a coating of the foamed polymer dispersion to a suitable carrier, e) drying the coating.
13. Porous polymer coating, preferably porous polyurethane coating, obtainable by the use of polyol ethers, preferably comprising sorbitan ethers and / or polyglycerol ethers, as additives in aqueous polymer dispersions in the production of such polymer coatings, obtainable by a process according to Claim 12, with the proviso that the porous polymer coating preferably has a mean cell size less than 150 µm, preferably less than 120 µm, especially preferably less than 100 µm, most preferably less than 75 µm, where cell size is determined by the method specified in the description.