SILOXANE-FUNCTIONALIZED SILICIC ACID

DE502021005124D1Active Publication Date: 2024-10-02WACKER CHEMIE AG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502021005124
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-05
Publication Date
2024-10-02
Estimated Expiration
2041-03-05

AI Technical Summary

Technical Problem

Existing processes for producing silicas functionalized with siloxanes often result in the presence of cyclic D-siloxanes, which are classified as very persistent and bioaccumulative, leading to regulatory limitations and environmental concerns.

Method used

A silica functionalized with a siloxane of the general formula [SiO4/2]a [R1< SiO3/2]b [R3< SiO2/2]c [R1< 3 SiO1/2]d [O1/2 R2<]e, where a, b, c, and d indices are optimized to minimize D-cycle content, ensuring the silica is essentially free of D-cycles, thereby meeting stringent regulatory requirements.

Benefits of technology

The approach effectively reduces D-cycle content to below 60 ppm, meeting regulatory standards and enhancing the environmental sustainability of silica-based products.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to silicas which are functionalized with a siloxane of the general formula (I) free of [Me 2 SiO 2 / 2 ] units and to a process for the preparation of such silicas.

[0002] Siloxanes are a technically important class of compounds used in numerous technological fields. The production of siloxanes is a key process in technical organosilicon chemistry. For example, the hydrolytic condensation of chlorosilanes according to the following reaction equation is established on an industrial scale: 2 R 3 Si-Cl + H 2 O => R 3 Si-O-SiR 3 + 2 HCl

[0003] The hydrolytic condensation of alkoxy-containing silanes and siloxanes, which are both industrially produced raw materials, is also established: R 3 Si-OR + H 2 O => R 3 Si-OH + ROH; 2 R 3 Si-OH => R 3 Si-O-SiR 3 + H 2 O

[0004] Fumed silicas are widely used additives for controlling the flow properties of adhesives, sealants, and coating materials such as paints and varnishes. They are used in particular to adjust viscosity, shear-thinning and thixotropic properties, and yield point.

[0005] Unfunctionalized silicas are typically used for non-polar, higher molecular weight systems with a high solvent content.

[0006] Hydrophobic silicas are generally used for polar, low-molecular-weight systems with low solvent content or solvent-free systems. Hydrophobicization can be achieved, for example, by functionalization with polyorganosiloxanes (e.g., polydimethylsiloxane, PDMS) or chloroalkylsilanes (especially chloromethylsilanes). The thus functionalized silicas contain mono-, di-, or trimethylsiloxy groups.

[0007] The nomenclature of polyorganosiloxanes (siloxanes for short) is based on the functionality of their units. There are four different units (building blocks): mono-, di-, tri-, and tetra-functional (M, D, T, Q). M-siloxanes act as chain ends. D-siloxanes generally serve to build linear chains and cyclic siloxanes. T- and Q-siloxanes serve to crosslink chains and build branched and hyperbranched networks.

[0008] Cyclic siloxanes can be formed during the production of siloxanes using difunctional synthetic building blocks. When silicas are then functionalized with these siloxanes, they also contain the cyclic siloxanes.

[0009] Siloxanes containing [Me 2 SiO 2 / 2 ] units form, in particular, cyclic D-siloxanes such as hexamethylcyclotrisiloxane (D3, [Me 2 SiO 2 / 2 ] 3 ), octamethylcyclotetrasiloxane (D4, [Me 2 SiO 2 / 2 ] 4 ), decamethylcyclopentasiloxane (D5 or [Me 2 SiO 2 / 2 ] 5 ) and dodecamethylcyclohexasiloxane (D6 or [Me 2 SiO 2 / 2 ] 6 ) as well as higher homologues. In the European Union, D4, D5 and D6 meet the requirements to be classified as vPvB ( English .: very persistent, very bioaccumalative), PBT ( English .: persist, bioaccumulative, toxic) and ultimately as SVHC ( English.: substances of very high concern). The REACH regulation initially stipulated a reduction of the content of these D-cycles to below 1000 ppm. In the 15th amendment to the regulation, the limit was then lowered to 250 ppm. As a result, processes have been established in which D-siloxanes with a low D-cycle content can be produced, either by distillative removal of these cycles or by targeted chemical reactions.

[0010] WO 96 / 18670 A1 describes a process for producing a substantially cycle-free polyorganosiloxane mixture, in which cycle formation is suppressed by the addition of an equilibration catalyst. The polyorganosiloxane mixtures can also be functionalized.

[0011] EP 1 580 215 B1 describes a process for the preparation of amino-functional organosiloxanes with a low D4 content.

[0012] The use of T and Q units in combination with D-siloxanes is also known. For example, US Pat. No. 4,193,885 describes the use of branched methylpolysiloxanes as heat transfer media, with the content of T and Q units preferably being less than 10 mol%.

[0013] The formation of D-cycles can be completely excluded if the use of the D building block (Me 2 SiO 2 / 2 ) is omitted.

[0014] Processes for the production of D-free siloxanes are currently limited to low-molecular TM (systems consisting only of T and M units) or QM systems and mainly concern their applications as heat transfer fluids and in cosmetics.

[0015] WO 2010 / 103103 A1 describes the use of polyorganosiloxanes as power and / or heat transfer fluids, permitting T and Q units, thus allowing both pure TM and QM systems. One of the Si-bonded residues contains at least two C atoms.

[0016] RU 2 221 826 C1 concerns, among other things, the use of TM3 [(Me)Si(OSiMe 3 ) 3 ] as a component of heat transfer fluids in mixtures with linear DM siloxanes.

[0017] WO 2016 / 124439 A1 describes the use of QM4 [Si(OSiMe 3 ) 4 ] as a heat transfer fluid.

[0018] WO 2017 / 058713 A1 describes the use of TM3 and QM4 as components of a composition for skin care applications.

[0019] Furthermore, methods for producing QM or TM systems are known.

[0020] EP 1 205 505 A2 and EP 0 495 676 A1 describe processes for the preparation of alkoxy-rich TM oligomers and polymers, respectively, which may contain Q units and unsaturated functionalities. WO 2018 / 141383 A1 describes a continuous process for the preparation of QM4, Q(VM2)4 [Si(OSi(Me)2 (C(H)=CH2))4], and TM3.

[0021] Further methods enable the generation of low-molecular-weight QM or TM systems equipped with unsaturated or amino functionalities.

[0022] JP11021289 A2 describes a process for the preparation of 3-aminopropyl-substituted TM3 and QM4, while EP 3 153 518 A1 relates to processes for the preparation of monovinylated TM3 and QM4.

[0023] An alternative process for producing TM siloxanes (including linear ones) is described in WO 2018 / 184668 A1 by silylation of alkali metal silanolates. However, this process produces stoichiometric amounts of alkali metal salts.

[0024] The functionalization of silicas with M, D, and / or T groups is well known. This typically occurs as a condensation reaction between the silanol groups of the silica and the M, D, and / or T units (R n SiX, where X is a reactive leaving group and n = 1, 2, or 3) of the siloxane or organosilane.

[0025] For example, EP 0 686 676 A1 describes a process for the silylation of silica with M-, D-, and / or T-siloxanes. The siloxane is mixed with the silica in the form of a finely atomized aerosol.

[0026] EP 0 251 176 A2 also discloses a process for producing a functionalized silica by reacting an unfunctionalized silica with diphenyldimethoxysilane and trimethylmethoxysilane.

[0027] EP 0 926 210 A1 and DE 10 2006 017 592 A1 each describe processes for hydrophobizing silicas with organomonosilanes, wherein the silica is functionalized with M, D, and / or T groups.

[0028] A disadvantage of the above-mentioned processes for functionalizing silicas is that they can contain D-cycles.

[0029] The object of the invention was to provide hydrophobic silicas that are essentially free of D-cycles.

[0030] Under essentially It should be understood that at least the detection limit for D-cycles of the analysis method used here of 60 ppm is not exceeded.

[0031] This task is solved by a silica which is reacted with a siloxane of the general formula (I) [SiO 4 / 2 ] a [R 1< SiO 3 / 2 ] b [R 3< R 1< SiO 2 / 2 ] c [R 1< 3 SiO 1 / 2 ] d [O 1 / 2 R 2< ] e (I) is functionalized, where the indices a, b, c, d, e independently take the integer values a from 0 to 100, b from 0 to 100, c from 0 to 50, d from 3 to 200, e from 0 to 50, with the proviso that the sum of a, b and c is at least 1 and for more than 50% of the siloxanes in the mixture the sum of a, b and c is ≥ 4; where R 1< independently of one another is H, amino group, unsubstituted or substituted C 1 -C 20 alkyl radical, unsubstituted or substituted C 2 -C 20 alkenyl radical, unsubstituted or substituted C 6 -C 14 aryl radical; where R 2< independently of one another is H, unsubstituted or substituted C 1 -C 20 hydrocarbon radical; where R 3< independently of one another is H, amino group, unsubstituted or substituted C 2 -C 20 alkyl radical, unsubstituted or substituted C 2 -C 20 alkenyl radical, unsubstituted or substituted C 6 -C 14 aryl radical, where substituted means that independently of one another at least one substituent from the group with OR Y< , -NR Y< 2 , -SH, -SR Y< , epoxy, -COOR Y< , -CHO, -CN, -NCO, -OCOOR Y< , -NR Y< -COOR Y< , -NR Y< -CO-NR Y< , -SiR Y< 3 and -OSiR Y< 3 is present, where RY< independently of one another is H, amino group, unsubstituted or substituted C 1 -C 20 alkyl radical, unsubstituted or substituted C 2 -C 20 alkenyl radical, unsubstituted or substituted C 6 -C 14 aryl radical.

[0032] Preferably, the indices a, b, c, d, e independently of each other the following integer values: a from 0 to 30, b from 0 to 30, c from 0 to 15, d from 3 to 60 and e from 0 to 15.

[0033] Preferably, the siloxane does not have any Q units and the index a has the value 0. In other words, the functionalized silica preferably does not have any Q groups as functionalization.

[0034] Preferably, the siloxane has no D units and the index c has the value 0. In other words, the functionalized silica preferably has no D groups as functionalization.

[0035] The D-cycle content is preferably less than 250 ppmw, particularly preferably less than 150 ppmw, and especially less than 60 ppmw. The D-cycle content can be determined using a gas chromatograph with a flame ionization detector (GC-FID). The detection limit is typically 60 ppmw (see section 8 of the measurement methods). In general, the D-cycle content should be close to or at 0 ppmw, since the siloxane used for functionalization is generally free of D-cycles, and the reaction conditions during functionalization generally do not favor the formation of D-cycles.

[0036] The functionalized silica preferably has a surface area (measured by the BET method according to DIN 66131 and 66132) of 30 to 400 m 2 < / g, particularly preferably of 40 to 300 m 2 < / g, in particular of 50 to 200 m 2 < / g.

[0037] The content of silanol groups (residual silanol content relative to the starting silica) of the functionalized silica is preferably 15 to 45% (see point 9 of the measurement methods).

[0038] The carbon content of the functionalized silica is preferably between 1 and 10% (see point 10 of the measurement methods).

[0039] Preferably, the content of volatile components at 300°C of the functionalized silica is 0.5 to 10%, particularly preferably 2 to 8%, in particular 3 to 7%.

[0040] Preferably, the volatile content of the functionalized silica at 105°C is 0.1 to 0.5%, particularly preferably 0.2 to 0.3% (see point 11 of the measurement methods).

[0041] The thickening effect of the functionalized silica is preferably 1 to 10 mPas, particularly preferably 2 to 9 mPas, in particular 3 to 8 mPas (cf. point 12 of the measurement methods).

[0042] A further aspect of the invention relates to a process for producing a functionalized silica, in particular a silica as described above, by reacting an unfunctionalized silica with a siloxane of the general formula (I) [SiO 4 / 2 ] a [R 1< SiO 3 / 2 ] b [R 3< R 1< SiO 2 / 2 ] c [R 1< 3 SiO 1 / 2 ] d [O 1 / 2 R 2< ] e (I), where the indices a, b, c, d, e independently of one another take the integer values ​​(the proviso described above applies) a from 0 to 100, b from 0 to 100, c from 0 to 50, d from 3 to 200 and e from 0 to 50, with the proviso that the sum of a, b and c is at least 1 and for more than 50% of the siloxanes in the mixture the sum of a, b and c is ≥ 4, the radicals R 1< , R 2< , R 3< are defined as above and wherein the content of alkoxy groups (R 2< ≠ H) is less than 5 mol% and the content of silanol groups (R 2< = H) is less than 500 ppm and the siloxane has a viscosity of 5 to 500000 mPa*s.

[0043] Preferably, the indices a, b, c, d, e independently take the following integer values: a from 0 to 30, b from 0 to 30, c from 0 to 15, d from 1 to 60 and e from 0 to 15, wherein the content of alkoxy groups is less than 1 wt.% and the content of silanol groups is less than 350 ppm and the siloxane has a viscosity of 60 to 10,000 mPa*s, in particular 50 to 500 mPa*s.

[0044] The viscosity (at 25°C) of the siloxane typically changes by less than 10%, especially less than 5%, over a storage period of 4 weeks at 25°C. Furthermore, the siloxane is generally hydrophobic and immiscible with water under normal conditions (25°C and 1.013 bar).

[0045] The value of the index a and / or the index c preferably has the value 0. In particular, the siloxane contains no [R 3 < R 1 < SiO 2 / 2 ] units (c = 0) and, depending on its composition, can be referred to as a TM, QTM, or QM siloxane. Siloxanes (siloxane mixtures) containing TM, QTM, and / or QM siloxanes can be collectively referred to as Q / T / M siloxanes.

[0046] In particular, the siloxane used is free of D-cycles.

[0047] The ratio of index d to index b is preferably 0.15 to 3, preferably 0.2 to 2, particularly preferably 0.3 to 1.

[0048] Examples of C 1 -C 20 -alkyl radicals, as which the radicals R1< , R2< and R 3< of the siloxane can be defined independently of each other, are: methyl, ethyl, n -propyl-, iso-propyl-, 1- n -Butyl-, 2- n -Butyl-, iso-butyl-, tert-butyl-, n-Pentyl, iso-pentyl, neo-pentyl, tert-pentyl, hexyl, like that n -Hexyl residue, heptyl residues, like that n -Heptyl radical, octyl radicals, such as the n-octyl radical and iso-octyl radicals, such as the 2,2,4-trimethylpentyl radical, nonyl radicals, such as the n -nonyl radical, decyl radicals, such as the n-decyl radical, dodecyl radicals, such as the n-dodecyl radical, and octadecyl radicals, such as the n -Octadecyl radical; Cycloalkyl radicals, such as cyclopentyl, cyclohexyl, cycloheptyl and methylcyclohexyl radicals.

[0049] Examples of C 6 -C 14 aryl radicals can be phenyl, naphthyl, anthryl and phenanthryl radicals.

[0050] Examples of aryl residues can be o -, m-, p -Tolyl residues, xylyl residues and ethylphenyl residues; and alkyl residues, such as the benzyl residue, the α - and the β -Phenylethyl radical.

[0051] Examples of C 2 -C 20 alkenyl radicals can be vinyl, allyl, 5-hexen-1-yl, E-4-hexen-1-yl, Z-4-hexen-1-yl, 2-(3-cyclohexenyl)ethyl and cyclododeca-4,8-dienyl radicals.

[0052] Examples of amino groups can be: Morpholino-(CH 2 )-, H 2 N(CH 2 ) 2 NH(CH 2 )CH(CH 3 )CH 2 -, (cyclohexyl)NH(CH 2 ) 3 -, (cyclohexyl)NH(CH 2 )-, CH 3 NH(CH 2 ) 3 -, (CH 3 ) 2 N(CH 2 ) 3 -, CH 3 CH 2 NH(CH 2 ) 3 -, (CH 3 CH 2 ) 2 N(CH 2 ) 3 -, CH 3 NH(CH 2 ) 2 NH(CH 2 ) 3 -, (CH 3 ) 2 N(CH 2 )NH(CH 2 ) 3 -, CH 3 CH 2 NH(CH 2 ) 2 NH(CH 2 ) 3 -, (CH 3CH2) 2 N(CH 2 ) 2 NH(CH 2 ) 3 .

[0053] The rest RY< is preferably independently selected from the group consisting of 3-aminopropyl, [N-(2-aminoethyl)-3-aminopropyl], methyl, ethyl, propyl, butyl, 2-butyl, tert-butyl, neo-pentyl, hexyl, vinyl, allyl, hexenyl, phenyl, benzyl, tolyl and naphthyl. In particular, RY<selected from the group consisting of methyl, ethyl, vinyl, allyl, hexenyl and phenyl.

[0054] Preferably, the C 1 -C 20 alkyl radical, the C 2 -C 20 alkenyl radical and / or the C 6 -C 14 aryl radical of the siloxane used is unsubstituted.

[0055] The rest is preferred R 2< independently of one another an unsubstituted C 1 -C 12 hydrocarbon radical, particularly preferably C 1 -C 6 hydrocarbon radical, in particular methyl or ethyl.

[0056] Preferably, the siloxane used is a substitute for polydimethylsiloxanes (formula A), where R 1< preferably independently selected from the group consisting of methyl, ethyl and phenyl. R 2< is preferably independently selected from the group consisting of H, methyl and ethyl and R 3< is preferably independently ethyl or phenyl.

[0057] According to a further embodiment, the siloxane is a substitute for vinylpolysiloxanes. In vinylpolysiloxanes, individual methyl residues per molecule are substituted by unsaturated functionalities (based on formula A). The residue R 1< is preferably independently selected from the group consisting of methyl, ethyl, phenyl, vinyl, allyl and hexenyl. R 2< is preferably independently selected from the group consisting of H, methyl and ethyl. R 3< preferably independently selected from the group consisting of ethyl, phenyl, vinyl, allyl and hexenyl.

[0058] According to a further embodiment, the siloxane is a substitute for amine oils. Based on formula A, individual methyl residues in amine oils are replaced by amino groups. The residue R 1< is preferably independently selected from the group consisting of methyl, ethyl, phenyl, 3-aminopropyl and [N-(2-aminoethyl)-3-aminopropyl].R 2< is preferably independently selected from the group consisting of H, methyl and ethyl. R 3< is preferably independently selected from the group consisting of ethyl, phenyl, 3-aminopropyl and [N-(2-aminoethyl)-3-aminopropyl].

[0059] The unfunctionalized silica preferably has a surface area of ​​50 to 400 m 2 < / g (BET method, see above).

[0060] The reaction of the unfunctionalized silica with the siloxane of the general formula (I) is preferably carried out at a temperature of 25 to 400°C, particularly preferably from 200 to 400°C, in particular from 200 to 350°C. This temperature is, in particular, the wall temperature of the reactor used.

[0061] The reaction is preferably carried out at atmospheric pressure.

[0062] The unfunctionalized silica is preferably treated with 0.5 to 5% (based on the mass of the silica) of a protic solvent or a weak base, preferably ammonia, before functionalization.

[0063] The invention further encompasses a functionalized silica which is produced by the process described and has a D-cycle content of less than 250 ppmw, preferably less than 150 ppmw, particularly preferably less than 60 ppmw.

[0064] A further aspect of the invention relates to the use of the described functionalized silicas as an additive for controlling the rheology of liquid and powder systems, in particular adhesives and sealants, toners and developers.

[0065] The siloxanes used for functionalization with an alkoxy group content [O 1 / 2 R 2< ] of less than 3 wt.% can be prepared by a process comprising the following steps: a) reacting a mixture containing at least one silicon compound from the group with R 1< 3 SiX, R 1< 3 SiOR 2< and R 1< 3 SiOSiR 1< 3 and at least one silicon compound from the group with SiX 4 , Si(OR 2< ) 4 , R 1< SiX 3 , R 1< Si(OR 2< ) 3 , R 3< R 1< SiX 2 and R 3< R 1< Si(OR 2< ) 2 , with a proportion of water which corresponds to at least 50% of the amount of alkoxy groups contained in the mixture, optionally in the presence of an alcohol and / or solvent, wherein X independently of each other is F, Cl, Br, I, tosylate, triflate or acetate and the residues R1< , R2< and R 3< are defined as described above; b) carrying out a phase separation to separate a siloxane phase; c) reacting the siloxane phase with a basic catalyst or with an acidic catalyst, wherein the reaction with the acidic catalyst takes place in the presence of at least one silicon compound from the group consisting of R 1< 3 SiOSiR 1< 3 , R 1< 3 SiX and R 1< 3 SiOH; d) separating low molecular weight constituents to obtain the siloxane.

[0066] Preferably, the mixture in step a) comprises at least one silicon compound from the group with R 1< 3 SiX, R 1< 3 SiOR 2< and R 1< 3 SiOSiR 1< 3 and at least one silicon compound from the group with SiX 4 , Si(OR 2< ) 4 , R 1< SiX 3 and R 1< Si(OR 2< ) 3-

[0067] The reaction in step a) is a cohydrolysis, which is carried out with an excess of water (relative to the amount of water required for the hydrolysis of the alkoxy functionalities present).

[0068] This variant of the procedure (cf. Fig. 1 Variant A) can be carried out in the presence of an alcohol and / or a solvent, the alcohol preferably being a mono- or dihydric C 1 -C 20 alcohol. It is particularly preferably a monohydric, unbranched C 1 -C 6 alcohol. In particular, the alcohol is selected from the group consisting of MeOH, EtOH, ethylene glycols, propylene glycols, and combinations thereof. The alcohol may optionally also be present in the solvent.

[0069] The solvent preferably comprises at least one compound from the group of alcohols, aliphatics, and aromatics, wherein the compound has 1 to 20, preferably 1 to 12, particularly preferably 1 to 9, carbon atoms. The aromatics may be substituted or unsubstituted. Preferably, they are toluene. The aliphatics are preferably acyclic compounds, in particular n- or iso-alkanes. These can exist as pure substances or as mixtures of isomers.

[0070] Phase separation serves to separate the (preliminary) siloxane obtained by cohydrolysis in step a) from an aqueous, possibly alcohol-containing, phase. For example, phase separation can be carried out using a separatory funnel or a double-column process with a coalescer.

[0071] Q / T / M siloxanes produced by cohydrolysis can have a high content of alkoxy groups. This can lead to the products not being viscosity-stable under the influence of atmospheric moisture. The alkoxy content can be reduced by further chemical treatment. The resulting siloxanes are then viscosity-stable.

[0072] In step c), the (preliminary) siloxane mixture separated from the aqueous phase is further treated under either acidic or basic catalysis. While acidic catalysis (in the presence of (functional) disiloxanes, halosilanes, or silanols) converts the alkoxy groups into -O-Si(CH 3 ) 2 R 1< functionalities, basic catalysis converts the alkoxy groups into silanols, which can either undergo condensation or be further functionalized.

[0073] In step d), low molecular weight components are separated, in particular by distillation, for example by means of distillation columns, thin-film or short-path evaporators.

[0074] The molar mass limit of the components to be separated depends on the conditions and compounds used. For example, methanol, ethanol, Si2 (Formula A, when n=1), VSi2 [H2C=C(H)Si(Me)2-O-Si(Me)2 (C(H)=CH2)], TM3, and even QM4 can be removed by distillation. A molar mass limit up to which compounds can be separated is, for example, 1000 g / mol, preferably 500 g / mol, and particularly preferably 400 g / mol (QM4 = 384.84 g / mol).

[0075] Another process variant for producing the siloxanes used includes the following steps: a) reacting a mixture containing at least one silicon compound from the group SiX 4 , Si(OR 2< ) 4 , R 1< SiX 3 , R 1< Si(OR 2< ) 3 , R 3< R 1< SiX 2 and R 3< R 1< Si(OR 2< ) 2 , with a proportion of water which corresponds to less than 50% of the amount of alkoxy groups contained in the mixture, optionally in the presence of an alcohol and / or solvent, whereinX independently of each other is F, Cl, Br, I, tosylate, triflate or acetate and the residues R1< , R2< and R 3< are defined as described above; b) reacting the reaction mixture obtained in step a) with an acidic catalyst in the presence of at least one silicon compound from the group consisting of R 1< 3 SiOSiR 1< 3 , R 1< 3 SiX and R 1< 3 SiOH; c) carrying out a phase separation to separate a siloxane phase; d) separating low molecular weight components to obtain the siloxane.

[0076] The mixture in step a) preferably comprises at least one silicon compound from the group consisting of SiX 4 , Si(OR 2< ) 4 , R 1< SiX 3 and R 1< Si(OR 2< ) 3 .

[0077] The reaction in step a) is a cohydrolysis, which is carried out with a substoichiometric amount of water and without the addition of M units. This variant (cf. Fig. 1Variant B) allows for the targeted adjustment of an average chain length in the form of oligomeric or polymeric alkoxysiloxanes. The risk of gelation can be minimized by adding substoichiometric amounts of water, but requires the chemical reduction of the alkoxy content through further treatment in step b), during which functionalities can also be incorporated.

[0078] In step b), the reaction mixture is further treated under acid catalysis. Here, too, the alkoxy groups are converted into -O-Si(CH 3 ) 2 R 1< functionalities.

[0079] With regard to the alcohol, the solvent and steps c) and d), reference can be made to the previous description.

[0080] Preferably, in both of the methods described above R 2< independently of one another an unsubstituted C 1 -C 12 hydrocarbon radical, preferably C 1 -C 6 hydrocarbon radical, particularly preferably methyl or ethyl.

[0081] It may be preferred that in the previously described variants A or B (cf. Fig. 1 ) R 1< independently of one another is methyl or phenyl, wherein between steps b) and c) or between steps c) and d) or after step d) an additional step i) is carried out in which the mixture obtained in each case in the preceding step is reacted with a basic catalyst in the presence of at least one silicon compound from the group with [R 3< Si(OR 2< ) 3 ], [R 3< R 1< Si(OR 2< ) 2 ] and [R 3< 3 Si(OR 2< )]. R 3< is a radical of the general formula (II) -R 4< -[NR 5< -R 6< -] g NR 7< 2 (II).

[0082] The remains R4< , R5< and R 7< are defined as follows: R 4< is a divalent linear or branched hydrocarbon residue with 1 to 18 C atoms. R 5< and R 7< are independently H, amino group, unsubstituted or substituted C 1 -C 20 alkyl radical, unsubstituted or substituted C 2 -C 20 alkenyl radical, unsubstituted or substituted C 6 -C 14 aryl radical. R 6< is a divalent hydrocarbon residue with 1 to 6 C atoms and the index g takes the value 0, 1, 2, 3 or 4.

[0083] The general formula (II) is a special selection from the general selection already described for R 3< (Aminoalkyl residue).

[0084] In this variant of the procedure (cf. Fig. 1 , variant D) is a further post-treatment for the introduction of amino groups.

[0085] The basic catalyst is preferably selected from the group consisting of alkali metal hydroxide, alkaline earth metal hydroxide, alkali metal alkoxide, alkaline earth metal alkoxide, alkali metal silanolate, alkaline earth metal silanolate, amines, aminoalkoxysilanes, and mixtures thereof. The amines are preferably alkylamines (e.g., triethylamine), aminosilanes, and / or aminoalkoxysilanes (e.g., aminopropylsilanes, aminoethylsilanes).

[0086] It may also be preferred that R 1< independently of one another is methyl or phenyl, wherein between steps b) and c) or between steps c) and d) or after step d) an additional step ii) is carried out in which the mixture obtained in each case in the preceding step is reacted with an acidic catalyst in the presence of at least one silicon compound from the group with R 3< 3 SiOSiR 3< 3 , R 3< 3 SiX and R 3< 3 SiOH. R 3< is independently an unsubstituted C 2 -C 20 alkyl radical, unsubstituted or substituted C 2 -C 20 alkenyl radical, unsubstituted or substituted C 6 -C 14 aryl radical. Preference is given to R 3< a vinyl, allyl or hexenyl residue.

[0087] In this variant (cf. Fig. 1 , variant C) is a post-treatment for the introduction of unsaturated, statistically distributed functionalities.

[0088] The acidic catalyst is preferably selected from the group consisting of hydrohalic acid, sulfonic acid, nitric acid, nitrous acid, sulfuric acid, organic acids, and mixtures thereof. The organic acids are preferably at least one compound from the group consisting of acetic acid, trifluoroacetic acid, formic acid, propionic acid, oxalic acid, malonic acid, succinic acid, citric acid, malic acid, adipic acid, and mixtures thereof.

[0089] The acidic and basic catalysts can each be bound to a support material or used as a liquid or gas. Examples of commercially available acidic catalysts are Tonsil (acidic alumina) or Purolite®< CT269 DR (sulfonic acid).

[0090] Preferably, the reaction is carried out in the presence of an acidic or basic catalyst until a thermodynamic equilibrium is reached and the composition of the mixture no longer changes.

[0091] The reaction in the presence of an acidic or basic catalyst can be carried out at a temperature of 20 to 200°C, preferably 50 to 150°C, particularly preferably 80 to 120°C.

[0092] Process step a) can be carried out at a temperature of -20 to 200°C, particularly preferably from 0 to 150°C, in particular from 20 to 120°C.

[0093] The process can be carried out as a batch process, a semi-batch process, or a continuous process. In principle, the process or individual process steps can be carried out independently of one another under reduced or elevated pressure. The pressure is preferably in a range from 1 to 10,000 kPa, particularly preferably in a range from 10 bar to 1,000 kPa. In particular, the process is carried out at ambient pressure.

[0094] The siloxane produced as described meets the requirements of Regulation (EC) No. 1907 / 2006 (REACH Regulation) to be classified as a polymer. Accordingly, the siloxanes have a molecular weight distribution in which no single component contains a content greater than 50%. Furthermore, they meet the so-called (3n+1) rule, according to which more than 50% of the molecules contained in the siloxane have a chain length of ≥ 4, or a chain length of at least 3 and are covalently bonded to a reactant.

[0095] The TM, QTM, and QM siloxanes possess chemical and physical properties that, while having the same viscosity at room temperature, differ significantly from the DM siloxanes in some respects (particularly with regard to chain length, low-temperature viscosity, and glass transition temperature), but are similar in other respects (refractive index, surface tension), as shown in Table 1. Table 1: *Unless otherwise stated, the measured values ​​refer to 25°C. The QTM siloxane consists of equimolar amounts of Q and T units. Measurands* DM-siloxane TM-Siloxane QTM siloxane QM-siloxane Viscosity at 25°C [mPa s] 100 100 100 100 Average chain length (determined from MN of GPC) 70 7 3-4 2-3 Viscosity at -30°C [mPa s] ∼400 ∼11.000 ∼1.400 ∼1.200 Glass transition temperature [°C] -125, 6 -79,1 -94,5 -119,1 Surface tension [mN / m] 20,5 20,1 19,8 19,1 Density [g / l] 0,963 1,026 1,015 0,941 refractive index 1,401 1,407 1,404 1,402

[0096] Depending on the choice of functional groups, the siloxanes can be used in a wide range of applications as substitutes for polydimethylsiloxanes, D-based vinyl polymers and D-based amine oils.

[0097] Polydimethylsiloxane substitutes can be used as damping medium, hydraulic oil, liquid dielectric (e.g. as transformer fluid), hydrophobic agent (particularly in the car care and textile sectors), antifoam agent, care additive (both in the personal and household care sectors), lubricant, release agent, plasticizer or heat transfer fluid in the low temperature range.

[0098] The substitutes for D-based vinyl polymers can be used for coating materials (e.g. paper coatings), as controlled-release additives, as components in the production of elastomers or as starting materials for further functionalizations via hydrosilylations and epoxidations.

[0099] The substitutes for D-based amine oils can be used in the areas of car care products, release agents, textiles, personal / household care and building protection.

[0100] Fig. 1 shows a scheme of the different process variants for the production of D-cyclene-free siloxanes. Examples Reagents

[0101] Tetrachlorosilane (CAS: 10026-04-7), trichloromethylsilane (CAS: 75-79-6), chlorotrimethylsilane (CAS: 75-77-4), trimethoxymethylsilane (CAS: 1185-55-3), tetramethoxysilane (CAS: 681-84-5), hexamethyldisiloxane (CAS: 107-46-0), 1,1,3,3-dimethyl-1,3-divinyldisiloxane (CAS: 2627-95-4), 3-aminopropyltrimethoxysilane (CAS: 13822-56-5) and N-(2-aminoethyl)-3-aminopropyltrimethoxysilane (AS1, CAS: 1760-24-3) were purchased from Sigma-Aldrich. Tonsil ®< was acquired from Clariant and Purolite ®< CT269 DR was acquired from Purolite. Measurement methods

[0102] 1) Viscosity was measured using a Stabinger SVM3000 rotational viscometer from Anton Paar at 25°C and within a temperature range of -40 to 90°C. 2) The mass-average molar mass M w , as well as the number-average molar mass M n , can be determined using size exclusion chromatography (SEC) against polydimethylsiloxane standards in toluene at 35°C, flow rate 0.7 ml / min, and detection with RI (refractive index detector) on a Meso Pore - Oligo Pore column set (Agilent, Germany) with an injection volume of 10 µl. 3) The proportion of Q, T and M units in the siloxane mixture was determined by nuclear magnetic resonance spectroscopy ( 29< Si-NMR; Bruker Avance III HD 500 ( 29< Si: 99.4 MHz) spectrometer with BBO 500 MHz S2 probe head; inverse gated pulse sequence (NS = 3000). 150 mg of Q / T / M siloxane mixture were dissolved in 500 µl of a 4*10 -2< molar solution of Cr(acac) 3 in CD 2 Cl 2 .The proportion of other functionalities was determined by correlating the 29< Si NMR data with the integrals from the 1< H NMR spectrum (1< H NMR; Bruker Avance III HD 500 (1< H: 500.2 MHz) spectrometer with BBO 500 MHz S2 probe head). 50 mg of Q / T / M siloxane mixture were dissolved in 500 µl of CD 2 Cl 2 . 4) The alkoxy content was determined by a combination of 29< Si and 1< H NMR spectroscopy (see point 3). The percentages of Q, T and M units can be determined from the 29< Si NMR spectra. Taking into account any signal overlaps (e.g. of the Si-Me units of . Me SiO 3 / 2 groups or Me3 SiO 1 / 2 groups), the relative ratios from the 29< Si NMR spectrum can be transferred to the ratios from the 1< H NMR spectrum. In this way, the relative proportion of all functionalities (Q, T, M units, alkoxy groups, unsaturated functionalities, amine functionalities, etc.) was determined. The relative proportions of the observed species are multiplied by the respective molar masses of the corresponding fragments. The individual masses determined in this way are related to the sum of all individual masses. The individual mass of the alkoxy groups in relation to the sum of all individual masses, multiplied by a factor of 100, gives the alkoxy content of the sample in weight percent. 5) The average molecular formula was determined by a combination of NMR spectroscopy (see point 3) and gel permeation chromatography (GPC, see point 2). The relative molar fractions of Q, T, and M units can be determined from the 29< Si NMR spectra.Taking into account any signal overlaps (e.g. the Si-Me units of . Me SiO 3 / 2 groups or Me3 SiO 1 / 2 groups), the relative proportions from the 29< Si NMR spectrum can be transferred to the proportions from the 1< H NMR spectrum. In this way, the relative proportion of all functionalities (Q, T, and M units, alkoxy groups, unsaturated functionalities, amine functionalities, etc.) was determined. The relative proportions thus obtained are referred to as the relative molecular formula. The relative proportions of the observed species are multiplied by the respective molecular masses of the corresponding fragments. The total mass thus obtained is referred to as the relative total mass. According to point 2, the number-average molecular mass MN of the sample to be analyzed was determined using GPC. Subsequently, the factor required to convert the relative molecular mass into the number-average molecular mass is determined. The relative proportions are multiplied by this factor. In this way, the relative molecular formula is converted into the average molecular formula.6) The content of unsaturated functionalities in the Q / T / M-based vinyl polymer substitutes is determined by the iodine value according to . Winespecified. The measurement is carried out according to DIN 53241. 7) The amine number indicates how many mmol KOH are equivalent to one gram of the substance to be determined. The amine number is determined according to DIN 16945, version 1989-03. 8) The D-cycle content is determined using a gas chromatograph with a flame ionization detector (GC-FID) (CES-Silicones Europe, April 16, 2013 (Revised Version: January 10, 2019). The detection limit is usually 60 ppmw. 9) The silanol group content can be determined by titration with 0.1 N sodium hydroxide solution in saturated saline solution (Sears et al., Anal. Chem. 1956, 12. 1981). For silicas, the sorption capacity for hydroxyl ions (OH -< ) is generally recorded. The relative sorption capacity can then be defined as the sorption capacity of the silica under investigation divided by the sorption capacity of the hydrophilic parent silica multiplied by 100.10) The carbon content is determined in an oxygen stream at temperatures > 1000°C, with the C content being determined from the combustion gases using a microprocessor (CS 530, Eltra or SC144DR, Leco). 11) The volatile content of the functionalized silica is determined at 105°C and 300°C according to DIN ISO 787 / 2. 12) The thickening effect of the functionalized silica is determined at 25°C in a polyester resin using a rotational viscometer according to DIN 53019. Examples 1 to 3: Preparation of D-cyclene-free, hydrophobic silicas by functionalization of fumed silicas with T / M-siloxane

[0103] Three pyrogenic silicas (HDK ®< V15A, HDK ®< N20, HDK ®< T30, Wacker Chemie AG) were used, the properties of which can be found in Table 2. A T / M siloxane (S250) with a viscosity of 250 mPa*s and a residual methoxy content of 0.03 wt.% was used for functionalization. Table 2: Silica and siloxane used Example No. Silica Surface area of ​​silica [m 2 / g] Mass S250 [g] 1 HDK ®< V15A 150 18 2 HDK ®< N20 200 32 3 HDK ®< T30 300 48

[0104] General experimental setup for functionalization: In a 6 L reactor (quartz glass) equipped with a stirrer, 100 g of silica were fluidized under inert gas (argon) for 15 min at 800 rpm. At the same speed, the T / M siloxane (S250) was introduced from above via a centrifugal mist nozzle (model 121, bore 0.2 mm, 30° cone, Schlick) using a gear pump (MCP-Z, Ismatec, pump head Z-1830) over a period of 15 min in a nitrogen stream against 0.6 MPa. After 15 minutes of homogenization, the reactor was heated to 300°C and maintained at this temperature for 2 h using a jacket heater. For the last 30 min of the heating period, the reactor was switched from argon blanketing to nitrogen purge (100 L / h) to expel volatile components via a riser tube.

[0105] The resulting functionalized silicas were analyzed for their carbon content, volatiles at 105°C and 300°C, as well as residual silanol content and thickening effect in polyester resin (rheological properties). The results are summarized in Table 3. Table 3: Analysis results of the functionalized silicas Example - No. Fl. fractions 105°C [%] Fl. fractions 300°C [%] C content [%] Residual silanol content [%] Thickening effect of polyester resin [mPas] 1 0 1,1 3,4 17,6 7 2 0,2 5,5 6,5 19,3 8,7 3 0,3 7,5 8,4 21,0 6,1

[0106] The rheological properties were tested by dispersing the functionalized silica in epoxy resin. After one day of storage, the viscosity of the mixture was determined at a shear rate of 0.1 s -1< and 10 s -1< and 25°C. The thixotropy index is obtained by dividing the viscosity at low shear rate by the viscosity at high shear rate. The thixotropy index was determined for two epoxy resin systems: Epoxy resin system 1: Mixture of 8 mol% of functionalized silica and 92 mol% epoxy resin (Epikote™< Resin 828 (epoxy resin based on bisphenol A and epichlorohydrin), Hexion). Epoxy resin system 2: Mixture of 8 mol% of functionalized silica (according to examples 1-3) in epoxy resin (Epikote™< Resin 828) and 4 mol% HDK®< N20 (fumed silica with a specific surface area of ​​200 m² / g) in amine hardener (Epikure™< Curing Agent MGS®< RIMH-137, Hexion), with the mixing ratio being 79 mol% epoxy resin to 21 mol% amine hardener. For comparison, a conventional, commercially available, functionalized silica (HDK ®< H17) was tested. The thixotropy indices of the functionalized silicas are shown in Table 4. Table 4: Rheological investigation Example No. Thixotropy index in epoxy resin system 1 Thixotropy index in epoxy resin system 2 1 34 48 2 42 56 3 34 54 HDK ®< H17 40 52

[0107] The silicas modified according to the invention have shear thickenings comparable to the commercial product HDK ®< H17.

[0108] No D-cycles were detected for any of the functionalized silicas according to Examples 1 to 3. Analysis of the reference silica HDK ®< H17 revealed 220 ppm D5 and 70 ppm D6. Examples 4 to 6: Preparation of D-cyclene-free, partially hydrophobic silicas by functionalization of pyrogenic silicas with T / M-siloxane

[0109] The three pyrogenic silicas HDK ®< V15A, HDK ®< N20, HDK ®< T30 (Wacker Chemie AG) were used; their properties are shown in Table 5. Functionalization was carried out using the T / M siloxane S250. Table 5: Silica and siloxane used Example No. Silica Surface area of ​​silica [m 2 / g] Mass S250 [g] 4 HDK ®< V15A 150 7,5 5 HDK ®< N20 200 13 6 HDK ®< T30 300 19,5

[0110] The experimental setup and implementation were analogous to Examples 1 to 3.

[0111] The resulting functionalized silicas were analyzed for their carbon content, volatiles at 105°C and 300°C, as well as their residual silanol content and their thickening effect in polyester resin (rheological properties). The results are summarized in Table 6. Table 6: Analysis results of the functionalized silicas Example - No. Fl. fractions 105°C [%] Fl. fractions 300°C [%] c-content [%] Residual silanol content [%] Thickening effect of polyester resin. [mPas] 4 0,3 1 1,9 35,2 3,6 5 0,3 0,8 3 29,5 5,2 6 0,4 6,4 4,4 40,3 4,8

[0112] The synthesis of the D-cyclene-free T / M siloxane S250 used for functionalization was carried out in a 4L three-neck flask equipped with a KPG stirrer, a 1L dropping funnel, and a hose connection. The flask was connected to two safety wash bottles and an exhaust gas wash bottle filled with a 25% aqueous NaOH solution. Before filling the apparatus, it was flushed with argon. A mixture of 1089 g of methanol and 592 g of hexamethyldisiloxane was placed in the flask and cooled to 0°C. At this temperature, a total of 1335 g of methyltrichlorosilane was added via the dropping funnel over a period of 4 h, and the mixture was heated to 50°C. At this temperature, 602 g of deionized water was added via the dropping funnel over a period of 3 h. The mixture was then allowed to cool to room temperature (RT) and stirred for 10 h.The siloxane phase is separated from the aqueous-methanolic phase using a separatory funnel, neutralized with a saturated sodium bicarbonate solution, and dried over sodium sulfate. After filtration (pleated filter), a large portion of the low-molecular-weight components is removed using a rotary evaporator at 80°C and 10 mbar. The resulting material is a colorless liquid with a viscosity of 64 mPa*s and a residual methoxy content of 0.03 wt.%. Subsequently, further low-molecular-weight components (especially TM3) are removed using a laboratory thin-film evaporator at 160°C and 10 mbar. The resulting product is a colorless liquid with a viscosity of 250 mPa*s and a residual methoxy content of 0.03 wt.%. Production of further D-cyclene-free siloxanes: General setup of the apparatus for cohydrolysis of halosilanes or alkoxysilanes

[0113] A 4L three-neck flask is equipped with a pressure-compensated stirrer, a 1L pressure-equalizing dropping funnel, and a hose connection. For variants A, B, and C, the flask is connected to two safety wash bottles and an exhaust gas wash bottle filled with NaOH. Inert reagents and solvents (e.g., hexamethyldisiloxane and methanol) are placed in the flask unless otherwise specified. Before filling the apparatus with the corresponding chlorosilanes, the entire apparatus is flushed with argon.

[0114] In the Figure 1 The various process variants are presented using a flow chart. The following section provides a general description of the underlying reaction setup for implementing the process variants. Variants A, B, C, and D are then explained. Choice of reactants

[0115] Halosilanes, alkoxysilanes, disiloxanes, or mixtures thereof can be used as starting materials for variant A. For variant C, at least one vinylhalosilane, vinylalkoxysilane, or vinyldisiloxane is added to this mixture. For variant B, the use of M sources is omitted during the hydrolysis. In variants A and C, an excess of water is used, relative to the amount of water required to hydrolyze all alkoxy and halogen functionalities contained in the mixture. In variant B, a deficiency of water is used.

[0116] The cohydrolyses (variants A, B, or C) can be carried out starting from chlorosilanes or methoxysilanes, or mixtures thereof. After cohydrolysis, phase separation occurs in variants A and C. The siloxane phase is then neutralized, dried over sodium sulfate for 2 hours, and isolated by filtration. In variant B, the hydrolysis product is used without further processing.

[0117] The products from variants A and B are generally characterized by a residual alkoxy content of > 3 wt.%. This can be reduced by post-treatment (paths A1, B1, B2, C1). If the residual alkoxy content is already within the desired range after variants A or C, no post-treatment is required. Post-treatment with Purolite ®< CT269 DR (in the presence of a (possibly functionalized) disiloxane; paths A1, A2, B1, B2 and C1)

[0118] A 1L one-neck flask (equipped with a reflux condenser) is charged with the siloxane to be treated, 7 wt.% Purolite®< CT269 DR (based on the initial siloxane weight), and 10 times the molar amount of hexamethyldisiloxane, 1,1,3,3-dimethyl-1,3-divinyldisiloxane, or mixtures thereof (based on the residual alkoxy content of the siloxane). The mixture is heated to 100°C for 2 h with vigorous stirring, brought to RT, and then isolated using a pleated filter (for low-viscosity siloxanes) or glass filters or glass frits with a suction flask (for high-viscosity siloxanes). For siloxanes with a high residual alkoxy content (from 15 to 30 mol%) after cohydrolysis, the catalyst content can be increased to 14 wt.%. This post-treatment can reduce the content of TM, QTM and QM cycles in the siloxanes. Post-treatment with Tonsil ®< (in the presence of a (possibly functionalized) disiloxane; pathways A1, A2, B1, B2 and C1)

[0119] A 1L three-necked flask (equipped with a reflux condenser) is charged with the siloxane to be treated, 10 wt.% Tonsil® (based on the initial siloxane weight), and 10 times the molar amount of hexamethyldisiloxane, 1,1,3,3-dimethyl-1,3-divinyldisiloxane, or mixtures thereof (based on the residual alkoxy content of the siloxane). The mixture is heated to 100°C with stirring for a total of 12 h, brought to room temperature, and then isolated using a pleated filter (for low-viscosity fluids) or a glass filter or glass frit with a suction flask (for high-viscosity fluids). Post-treatment with HCl (in the presence of a (possibly functionalized) disiloxane; paths A1, A2, B1, B2 and C1)

[0120] 600 mL of a mixture of the siloxane to be treated and 10 times the molar amount of hexamethyldisiloxane, 1,1,3,3-dimethyl-1,3-divinyldisiloxane, or mixtures thereof (based on the residual alkoxy content of the siloxane) are placed in a stainless steel autoclave (1 L total volume, equipped with analog and digital pressure sensors and a resistance jacket heater with a temperature sensor). The autoclave is sealed gas-tight, degassed (20 mbar for 3 min), and filled with 15 g of hydrogen chloride gas. The autoclave is heated to 100°C for 3 h and then brought to RT. The gas atmosphere is passed through a gas scrubber, and the gas space is purged with argon for 5 min. The siloxane phase is separated from the alcoholic phase, neutralized, dried over sodium sulfate for 2 h, and filtered. Post-treatment with KOH (Path A1)

[0121] A 1L one-neck flask (equipped with a reflux condenser) is filled with the siloxane to be treated and an equimolar amount of KOH granules (based on the residual alkoxy content of the siloxane). The mixture is heated to 100°C for 2 h with stirring and then brought to RT. The silicone phase is neutralized with hydrochloric acid (1 mol / L) and freed of adhering solids by filtration. The siloxane phase is washed with deionized water and then dried over sodium sulfate for 2 h. This post-treatment can be used in particular to reduce the cyclic content of Q / T / M siloxanes. Materials subjected to this post-treatment retain a residual hydroxyl content even after neutralization, which leads to increasing viscosities with increasing storage time. To obtain viscosity-stable materials, post-treatment with an acidic catalyst can be carried out as described.The viscosity changes in the siloxane due to this post-treatment can be significant, and in the case of TM siloxanes, restructuring is usually observed.

[0122] After each of the above-mentioned reaction steps, low molecular weight components such as methanol, ethanol, hexamethyldisiloxane, tetrakis(trimethylsiloxy)silane (QM4) and tris(trimethylsiloxy)methylsilane (TM3) can be quantitatively removed using a rotary evaporator or thin-film / short-path evaporator. Treatments with NaOMe in the presence of an aminoalkoxysilane (variant D)

[0123] In a 1L round-neck flask equipped with a reflux condenser, the siloxane to be treated is mixed with an aminoalkoxysilane and 500 ppm wt (based on the total weight) of a sodium methylate solution (20 wt% in methanol). The mixture is heated to 90°C for 2 h while stirring. The reaction is monitored by 29< Si NMR spectroscopy. Reaction sequences

[0124] After cohydrolysis (according to variant A), crude siloxanes are obtained that have a residual alkoxy content. If this is outside the desired range, it can be reduced by post-treatment using an acidic or basic catalyst (path A1). If the residual alkoxy content is already within the desired range, no post-treatment is required.

[0125] The siloxanes can be converted in subsequent steps into alkenylsiloxanes (post-treatment with an acidic catalyst using, for example, 1,1,3,3-tetramethyl-1,3-divinyldisiloxane, path A2) or aminosiloxanes (post-treatment with NaOMe in the presence of an aminoalkoxysilane). Furthermore, the incorporation of unsaturated functionalities can be coupled with the reduction of the residual alkoxy content (path C1).

[0126] After partial hydrolysis according to variant B, Q-, QT-, or T-alkoxy oligomers / polymers are obtained; M units are not used in the hydrolysis. The (alkenyl)siloxanes are produced during post-treatment with an acidic catalyst using, for example, hexamethyldisiloxane (path B1), 1,1,3,3-dimethyl-1,3-divinyldisiloxane, or mixtures thereof (path B2).

[0127] A summary of the reactants used in the examples and their weights for producing the crude siloxanes (without vinyl or amine functionalities) can be found in Table 8. Table 8: *Concentrated hydrochloric acid (32 wt%) was used as the acid. The acid and deionized water were mixed before dosing and homogenized by vigorous stirring for 5 min. Example Disposable Alcohol [g] One-way [Me 3 SiO 1 / 2 ]-Source [g] One-way [MeSiO 3 / 2 ]-Source [g] One-way [SiO 4 / 2 ]-Source [g] Disposable VE Washer [g] Temp. A and B [°C] 7 EtOH, 756 Me 3 SiCl, 254 MeSiCl 3 , 582 - 252 0; RT 8 MeOH, 1027 [Me 3 SiO 1 / 2 ] 2 , 568 MeSiCl 3 , 1281 - 577 0; 50 9 MeOH, 1001 [Me 3 Si0 1 / 2 ] 2 , 785 MeSiCl 3 , 506 SiCl 4 , 581 563 0; 50 10 MeOH, 1254 [Me 3 SiO 1 / 2 ] 2 , 983 MeSiCl 3 , 633 SiCl 4 , 727 705 0; 50 11 MeOH, 1013 [Me 3 SiO 1 / 2 ] 2 , 1064 - SiCl 4 , 958 570 0; 50 12 MeOH, 1091 [Me 3 SiO 1 / 2 ] 2 , 942 - SiCl 4 , 1084 613 0; 50 13 - [Me 3 SiO 1 / 2 ] 2 , 72 MeSi(OMe) 3 , 500 - 80 (+54g HCl)* 50 14 - - MeSi(OMe) 3 , 1500 - 245 (+15g HCl)* 50 15 MeOH, 1089 [Me 3 SiO 1 / 2 ] 2 , 592 MeSiCl 3 , 1335 - 601 0; 50 16 - MeSi(OMe) 3 , 1500 - 220 (+6g HCl)* 50 17 MeOH, 1088 [Me 3 SiO 1 / 2 ] 2 , 853 MeSiCl 3 , 550 SiCl 4 , 631 612 0; 50 18 MeOH, 1070 [Me 3 SiO 1 / 2 ] 2 , 1085 - SiCl 4 , 1022 601 0; 50

[0128] A summary of the analytical data of the siloxanes before and after post-treatment can be found in Table 9. Table 9: *For Example 19, the non-post-treated crude siloxane from Example 17 was used and reacted with HCl as catalyst according to the procedure listed above. Bsp. Viscosity of Rohsiloxane [mPa*s] Rest-Alkoxy-Containing Rohsiloxane [Gew.-%] Aftertreatment Viscosity Product [mPa*s] Residual-Alkoxy-Content [Wt.-%] 7 - - - 154 0,23 8 127,2 1,6 Purolite / Si2 1281 0,05 9 68,1 4,8 Purolite / Si2 184 0,22 10 573,5 2,8 KOH 14012 0,96 11 51,1 3,2 Purolite / Si2 187 0,33 12 1956,7 4,8 Purolite / Si2 21326 0,73 13 - - Purolite / Si2 7501 0,18 14 - - Purolite / Si2 9720 0,72 15 - - Purolite / Si2 138 0,08 16 - - Purolite / Si2 980 0,58 17 - - Tonsils / Si2 150 0,52 18 - - Purolite / Si2 80 0,19 19* - - HCl / Si2 175 <0,01

[0129] A summary of the weights and analytical data of the siloxanes after functionalization can be found in Table 10. Table 10: *The catalyst dosage of the NaOMe solution (20 wt.% in MeOH) was 500 wt. ppm (based on the total mass of base siloxane and aminosilane) Bsp. Siloxane [Example] Sample weight of siloxane [g] Reagent [g] Cat. [g] Viscosity [mPa*s] Residual alkoxy content [wt%] Iodine number Amine number [meq / g] 20 15 251 VSi 2, 14.5 Purolite, 20 179 <0,01 7,4 - 21 16 265 VSi 2 , 49.1 Purolite, 13 1081 0,04 15,4 - 22 17 300 VSi 2 , 17.1 Purolite, 21 290 0,06 6,8 - 23 18 352 VSi 2 , 40.2 Purolite, 27 145 0,82 6,6 - 24 13 738 AS1, 11.5 NaOMe* 6871 0,65 - 0,12 25 16 1296 AS1, 42.6 NaOMe* 856 1,64 - 0,28

[0130] For examples 7 to 25, the content of D-cycles was analyzed by GC-FID, with the result that no D-cycles could be detected.

Claims

1. Silica functionalized with a siloxane of the general formula (I)         [SiO4 / 2]a [R1SiO3 / 2]b [R3R1SiO2 / 2]c [R13SiO1 / 2]d [O1 / 2R2]e     (I), where the indices a, b, c, d, e each independently have integer values a from 0 to 100, b from 0 to 100, c from 0 to 50, d from 3 to 200, e from 0 to 50, with the proviso that the sum of a, b and c is at least 1 and for more than 50% of the siloxanes in the mixture the sum of a, b and c is ≥ 4; where R1 is each independently H, an amino group, unsubstituted or substituted C1-C20-alkyl radical, unsubstituted or substituted C2-C20-alkenyl radical, unsubstituted or substituted C6-C14-aryl radical; where R2 is each independently H, an unsubstituted or substituted C1-C20-hydrocarbon radical; where R3 is each independently H, an amino group, unsubstituted or substituted C2-C20-alkyl radical, unsubstituted or substituted C2-C20-alkenyl radical, unsubstituted or substituted C6-C14-aryl radical, wherein substituted signifies that independently of one another at least one substituent is present from the group of ORY, -NRY2, -SH, -SRY, epoxy, -COORY, - CHO, -CN, -NCO, -OCOORY, -NRY-COORY, -NRY-CO-NRY, - SiRY3 and -OSiRY3, where RY is each independently H, an amino group, unsubstituted or substituted C1-C20-alkyl radical, unsubstituted or substituted C2-C20-alkenyl radical, unsubstituted or substituted C6-C14-aryl radical.

2. Silica according to Claim 1, characterized in that the indices a, b, c, d, e each independently have integer values a from 0 to 30, b from 0 to 30, c from 0 to 15, d from 3 to 60, e from 0 to 15.

3. Silica according to Claim 1 or 2, characterized in that the value of the index a and / or the index c is equal to 0.

4. Silica according to any of the preceding claims, characterized in that the content of D-cycles is less than 250 ppmw, preferably less than 150 ppmw, particularly preferably less than 60 ppmw.

5. Process for producing a functionalized silica, in particular according to at least one of Claims 1 to 4, by reacting an unfunctionalized silica with a siloxane of the general formula (I)         [SiO4 / 2]a [R1SiO3 / 2]b [R3R1SiO2 / 2]c [R13SiO1 / 2]d [O1 / 2R2]e     (I), where the indices a, b, c, d, e each independently have integer values a from 0 to 100, b from 0 to 100, c from 0 to 50, d from 3 to 200, e from 0 to 50, with the proviso that the sum of a, b and c is at least 1 and for more than 50% of the siloxanes in the mixture the sum of a, b and c is ≥ 4; where R1 is each independently H, an amino group, unsubstituted or substituted C1-C20-alkyl radical, unsubstituted or substituted C2-C20-alkenyl radical, unsubstituted or substituted C6-C14-aryl radical; where R2 is each independently H, an unsubstituted or substituted C1-C20-hydrocarbon radical; where R3 is each independently H, an amino group, unsubstituted or substituted C2-C20-alkyl radical, unsubstituted or substituted C2-C20-alkenyl radical, unsubstituted or substituted C6-C14-aryl radical, wherein substituted signifies that independently of one another at least one substituent is present from the group of ORY, -NRY2, -SH, -SRY, epoxy, -COORY, - CHO, -CN, -NCO, -OCOORY, -NRY-COORY, -NRY-CO-NRY, - SiRY3 and -OSiRY3, where RY is each independently H, an amino group, unsubstituted or substituted C1-C20-alkyl radical, unsubstituted or substituted C2-C20-alkenyl radical, unsubstituted or substituted C6-C14-aryl radical; and wherein the alkoxy group content, R2 ≠ H, is less than 5 mol% and the silanol group content, R2 = H, is less than 500 ppm and the siloxane has a viscosity of 5 to 500 000 mPa*s, the viscosity being determined using a Stabinger rotational viscometer at 25°C and in a temperature range from -40 to 90°C.

6. Process according to Claim 5, characterized in that the indices a, b, c, d, e each independently have integer values a from 0 to 30, b from 0 to 30, c from 0 to 50, d from 3 to 60, e from 0 to 15.

7. Process according to Claim 5 or 6, characterized in that the value of the index a and / or the index c is 0.

8. Process according to at least one of Claims 5 to 7, characterized in that the siloxane is free from D-cycles.

9. Process according to at least one of Claims 6 to 8, characterized in that the ratio of the index d to the index b is 0.15 to 3, preferably 0.2 to 2, particularly preferably 0.3 to 1.

10. Process according to at least one of Claims 6 to 9, characterized in that R2 is each independently an unsubstituted C1-C12-hydrocarbon radical, preferably C1-C6-hydrocarbon radical, particularly preferably methyl or ethyl.

11. Process according to at least one of Claims 5 to 10, characterized in that the unfunctionalized silica has a surface area of 50 to 400 m2 / g.

12. Process according to at least one of Claims 6 to 11, characterized in that the reaction is carried out at a temperature of 25 to 400°C, particularly preferably 200 to 400°C, especially 200 to 350°C.

13. Use of the silicas according to at least one of Claims 1 to 4 or of the silicas produced according to the process according to at least one of Claims 5 to 12 as additive for controlling the rheology of liquid and pulverulent systems, particularly of adhesives and sealants, of toners and developers.