METHOD FOR PRODUCING A COVER SUBSTRATE, METHOD FOR PRODUCING A HERMETICALLY ENCLOSED OPTOELECTRONIC COMPONENT AND HERMETICALLY ENCLOSED OPTOELECTRONIC COMPONENT

DE502022002083D1Active Publication Date: 2024-11-21FRAUNHOFER GESELLSCHAFT ZUR FORDERUNG DER ANGEWANDTEN FORSCHUNG EV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE502022002083
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-02-19
Filing Date
2022-02-18
Publication Date
2024-11-21
Estimated Expiration
2042-02-18

AI Technical Summary

Technical Problem

Current methods for producing hermetically sealed optical or optoelectronic components, such as blue and green laser diodes, face challenges in ensuring long service life and maintaining beam quality due to exposure to water vapor and volatile organic compounds, and require effective heat dissipation and manufacturing processes that are costly and complex.

Method used

A method involving the use of a molded substrate with a glass cover substrate formed through glass flow processes to create optically neutral window areas, allowing for hermetic sealing of sensitive components with improved heat dissipation and reduced manufacturing costs, using a single homogeneous glass material for the cover substrate and employing techniques like anodic bonding and glass flow processes to achieve high planarity and parallelism of the window surfaces.

Benefits of technology

The method results in hermetically sealed optoelectronic components with extended service life and improved beam quality, reduced optical errors, and lower manufacturing costs, while preventing clouding and damage to laser facets by minimizing exposure to harmful substances and enhancing heat dissipation.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

Technical area

[0001] The present invention relates to a method for producing a cover substrate, such as for producing a cover substrate for housing (= accommodating in a housing) one or a plurality of optical or optoelectronic components, wherein a cover substrate formed during the manufacturing method forms the cover substrate with at least one cover element. The present invention further relates to a method for producing a hermetically packaged optical or optoelectronic component, wherein the production can be carried out individually (at the individual substrate level) or at the wafer level. The present invention further relates to a hermetically packaged optical or optoelectronic component that is manufactured or housed using this manufacturing method.

[0002] For example, a packaging concept for optical or optoelectronic components, such as LEDs or laser diodes, is provided, wherein the manufacturing process can be carried out at wafer level and / or single substrate level in order to package the optoelectronic components with a lid substrate with optically passive (= optically neutral), lateral window regions. Technical background

[0003] Currently, blue and green laser diodes, for example, are finding increasingly broad applications. The use of blue laser diodes as a crucial component in the readout of high-density optical storage media, such as Blu-ray, is established and widespread. Meanwhile, a wide range of other applications for high-performance blue and green laser diodes are emerging, such as as RGB sources in mobile image and video projection (projectors). Both green and blue laser diodes should always be hermetically packaged (housed) in a housing. It is possible to encapsulate such laser diodes using a packaging technology with special TO headers (e.g., TO 38) with an integrated optical window and copper heat sink.

[0004] In addition to the consumer applications mentioned above, there is also a need in the field of medical and industrial spectroscopy for hermetically encapsulated semiconductor-based light sources with particularly good heat dissipation and organic-free housing in order to guarantee the required long lifetimes.

[0005] DE 25 24 731 A1 relates to a method for producing an article made of glass with at least one curved part.

[0006] WO 2019 / 020708 A1 relates to a MEMS mirror arrangement and to a method for producing a MEMS mirror arrangement.

[0007] The object underlying the present invention is therefore to provide an improved method for producing a cover substrate, e.g., for encapsulating optoelectronic (radiation-emitting or radiation-sensitive) components, and further to provide an improved method for producing a hermetically packaged optoelectronic component, whereby correspondingly packaged optoelectronic components with improved properties can be created.

[0008] This problem is solved by the subject matter of the independent patent claims.

[0009] Specific embodiments, implementations and further developments of the present application are defined in the dependent patent claims. Overview of the inventive concept (= method and device)

[0010] The present invention is based on the finding that, using the manufacturing methods shown, a cover substrate with glass cover elements for the packaging of optoelectronic components can be obtained and provided, wherein the cover elements have very thin optical (= optically neutral) glass window surfaces (for lateral radiation) on the sides. The optical refractive power of very thin optical glass windows is so low that (often) no optically flat surface is required to produce a glass cover for the packaging of optoelectronic (radiation-emitting or radiation-sensitive) components (semiconductor components). These thin-walled window surfaces are optically passive or optically neutral (= have no optical effect). In particular, planarity is not required if the changes in the thickness of the window are sufficiently small.Since (relevant) laser diodes essentially always exhibit a variation in their angular distribution (divergence component) of the emission, even small changes do not play a (significant) role in the optical properties of the package. If the radiation emitted by the semiconductor emitters (or the radiation received by the semiconductor receivers) needs to be collimated, focused, or redirected, this is done by additional optical components mounted either inside the sealed package or outside on a so-called optical bench.

[0011] A further finding of the present invention is that such a cover substrate for an improved, packaged, optoelectronic (radiation-emitting or radiation-receiving) component (semiconductor component) can be manufactured particularly advantageously at the wafer level with significantly simplified effort. If a mold substrate is used to form cover substrates using a glass flow process, optically largely neutral window regions can be formed in a cover substrate, which can then be used to hermetically seal sensitive radiation sources or radiation receivers.

[0012] A mold substrate is, for example, a substrate with a shape, contour or topography, such as a topographically structured substrate.

[0013] According to exemplary embodiments, such a lid substrate (= shaped cover substrate) for an improved, packaged optoelectronic component can thus be manufactured particularly advantageously at the wafer level with significantly simplified effort, because, for example, only one (single) glass material is used. Furthermore, if a mold substrate is used to form lid substrates by glass flow processes, a large number of glass caps with similarly shaped, optically neutral window regions can be formed in one lid substrate, whereby sensitive optoelectronic components, e.g., sensitive radiation sources or receiving elements, can subsequently be hermetically sealed. If required by assembly technology, these shaped glass lid substrates can also be separated, and the caps can be used for individual encapsulation on specific carrier substrates, both at the wafer and at the individual substrate level.

[0014] This allows the packaged optoelectronic (radiation-emitting and / or radiation-sensitive) components (semiconductor components) to have a long service life while maintaining consistently good beam and power quality. In particular, clouding of the outlet window and damage to the laser facets can be reduced or prevented, as the exposure to water vapor and / or volatile organic components under the influence of the extremely intense and high-energy laser radiation can be reduced or prevented. Heat dissipation from the package can also be improved. Furthermore, low manufacturing costs can be achieved due to relatively low manufacturing effort. Short description of the drawings and figures

[0015] Preferred embodiments of the present invention are explained in more detail below with reference to the accompanying drawings and figures. They show: Fig. 1 shows a schematic flow diagram of the manufacturing method according to the invention according to one embodiment; Figs. 2-6 show exemplary basic flow diagrams of the manufacturing method according to the invention according to further embodiments; Fig. 7 shows a schematic flow diagram of the method according to the invention for producing a hermetically packaged, optoelectronic component according to a further embodiment; Figs. 8-10 show exemplary basic flow diagrams of the method according to the invention for producing a hermetically packaged, optoelectronic component according to further embodiments; and Figs. 11-16 show exemplary embodiments for a hermetically packaged, optoelectronic component according to further embodiments, which are each produced, for example, using the manufacturing method described here.

[0016] Before exemplary embodiments of the present invention are explained in more detail below with reference to the drawings, it is pointed out that identical, functionally equivalent or equivalent elements, objects, functional blocks and / or method steps in the different figures are provided with the same reference numerals, so that the description of these elements, objects, functional blocks and / or method steps (with the same reference numerals) shown in different exemplary embodiments is interchangeable or can be applied to one another. Detailed description of the figures and embodiments

[0017] In the following description, the description of an element made of a semiconductor material means that the element comprises a semiconductor material, i.e., is formed at least partially or entirely from the semiconductor material. In the following description, the description of an element made of a glass material means that the element comprises a glass material, i.e., is formed at least partially or entirely from the glass material.

[0018] It is understood that when an element is described as being "connected" or "coupled" to another element, it may be directly connected or coupled to the other element, or intervening elements may be present. Conversely, when an element is described as being "directly connected" or "coupled" to another element, no intervening elements are present. Other terms used to describe the relationship between elements should be interpreted similarly (e.g., "between" versus "directly between," "adjacent" versus "directly adjacent," etc.).

[0019] To simplify the description of the various embodiments, at least some of the figures have a Cartesian coordinate system x, y, z, where the directions x, y, z are arranged orthogonally to one another. In the embodiments, the xy plane corresponds to the main surface area of ​​a carrier or substrate (= reference plane = xy plane), where the vertical upward direction relative to the reference plane (xy plane) corresponds to the "+z" direction, and the vertical downward direction relative to the reference plane (xy plane) corresponds to the "-z" direction. In the following description, the term "lateral" means a direction parallel to the x and / or y direction, i.e., parallel to the xy plane, where the term "vertical" indicates a direction parallel to the + / -z direction.

[0020] In the context of this description, terms and / or text passages placed in brackets are to be understood as examples of further explanations, exemplary embodiments, additions and / or exemplary alternatives (to the preceding term or the preceding text passage).

[0021] Fig. 1 shows, by way of example, a basic flow diagram of the manufacturing method 100 according to the invention according to an embodiment. Thus, the flow diagram of Fig. 1For example, a method 100 for producing a cover substrate for housing one or a plurality of optical or optoelectronic components (semiconductor components), wherein the formed cover substrate then forms the cover substrate with the at least one cover element for housing the optoelectronic component. An optoelectronic component (semiconductor component) is, for example, a radiation-emitting and / or radiation-sensitive semiconductor component, such as an optoelectronic transmitting component and / or receiving component.

[0022] Since the method according to the invention for producing a cover substrate for housing one or more optical / optoelectronic components, e.g., at the wafer level, uses a mold substrate comprising a semiconductor material, which is formed, for example, as a preprocessed silicon wafer, the term "silicon mold substrate" or "silicon wafer" will also be used below. However, it should be clear that the use of silicon as the material for the mold substrate (semiconductor wafer) is only exemplary; depending on the application or manufacturing process, other suitably processable materials or semiconductor materials can also be used for the mold substrate.

[0023] Referring to the method 100 of Fig. 1Now, at step 120, a mold substrate and a cover substrate that are bonded to each other are provided, wherein a surface area of ​​the mold substrate and / or the cover substrate is structured (formed) to form (at least) a closed cavity between the cover substrate and the mold substrate.

[0024] According to one embodiment, the mold substrate can be formed as a semiconductor substrate (semiconductor wafer or silicon wafer) and the cover substrate as a glass substrate or glass wafer. According to one embodiment, the mold substrate and the cover substrate are hermetically bonded or joined to each other, which can be achieved, for example, with an anodic bonding process or another joining process. Furthermore, a surface region of the mold substrate and / or the cover substrate is provided with a recess or several recesses (recesses) to form the sealed cavity between the cover substrate and the mold substrate.

[0025] The cover substrate comprises, for example, a single homogeneous material or glass material in order to form the shaped cover substrate as a lid substrate or glass caps in the following manufacturing steps.

[0026] The mold substrate is, for example, a substrate with a shape, contour, or topography, such as a topographically structured substrate. The mold substrate can be formed, for example, as a semiconductor wafer, e.g., a silicon wafer, wherein the surface structuring or the topography of the mold substrate can be obtained very precisely by means of semiconductor processing steps (e.g., silicon processing steps). Such semiconductor processing processes, such as, for example, photolithographic processes with wet or dry etching processes, are technically extremely well mastered. Furthermore, mechanical surface processing methods, e.g., for CNC milling, can also be used to form the structure in the mold substrate. Furthermore, in addition to semiconductor materials, such as, for example, Si, SiGe, other materials, such as, for example, AlN, SiC, high-melting glass (e.g.,Schott AF 32) are used for the mold substrate, which are suitable for a photolithographic or mechanical surface treatment process for forming the structure in the mold substrate and are also sufficiently temperature-stable during the annealing processes (temperature treatment processes) during the process for producing the lid substrate.

[0027] In a (subsequent) step 130, the cover substrate and the mold substrate are then tempered, i.e., subjected to a temperature treatment or heated (warmed), to reduce the viscosity of the glass material of the cover substrate. Furthermore, in a step 140, an overpressure is provided in the (at least one) sealed cavity(ies) relative to the surrounding atmosphere in order to effect, based on the reduced viscosity of the glass material of the cover substrate and the overpressure in the sealed cavity relative to the surrounding atmosphere, a defined bulging, e.g., blowing out or deformation, of the glass material of the cover substrate, starting from the sealed cavity and reaching a stop surface of a stop element spaced apart from the cover substrate.The defined bulging of the glass material due to the overpressure in the sealed cavity and the reduced viscosity of the glass material can also be referred to as blowing out or deformation of the glass material. The defined bulging of the glass material of the cover substrate thus results in a shaped cover substrate with (at least) one lid element (= bulging or deformation). The resulting bulging or deformation of the shaped cover substrate (= lid substrate) is therefore referred to as the lid element.

[0028] Due to the defined curvature of the glass material of the cover substrate, side surfaces with high planarity (small changes in the thickness of the side windows) are obtained in the resulting cover element of the formed cover substrate, so that "optically passive" side windows are obtained in the respective cover elements of the formed cover substrate. Optical window surfaces are considered to be, for example, those regions of the cover wafer whose wall thickness homogeneity across the area illuminated by the beam does not differ by more than 15% or 10%. The wall thickness of the optically passive (= neutral) side windows in the respective cover elements, i.e., in the optically irradiated area of ​​the cover elements, is made so thin and uniform, for example, using the manufacturing process described, that the optical influence on the beam divergence is negligible, i.e., for example, a divergence of less than 0.5° or even less than 0.3°.For this purpose, the wall thickness of the side windows in this area is designed to be no thicker than 200 µm, 120 µm, or 60 µm, for example, in a thickness range between 5 and 200 µm, between 5 and 120 µm, or between 5 and 60 µm. In the context of this description, the divergence of the transmitted and / or received radiation refers to the widening or radiation angle of the incident or outgoing radiation, e.g., a laser beam and / or LED radiation.

[0029] An important difference between optically thin side windows and a lens is that a window is as optically neutral as possible or only acts like a very long focal length lens (= lens with a long focal length). The latter case can be tolerated for lasers (as light sources) because, on the one hand, the emission angles of the lasers themselves have a range of variation and, on the other hand, optical lenses are required and adjusted for beam shaping anyway. As long as the refractive power is low and the window is as homogeneous as possible, higher-order optical errors (coma, spherical aberration, etc.) can remain below a critical limit. In this way, it can be achieved that the wavefronts do not exceed a wavefront deformation of approximately 150 nm RMS due to the summed non-global Zernicke coefficients (global: lateral, tilt, global focus; non-global, e.g., coma, spherical aberration, etc.).With the current manufacturing technology, this can be achieved by making the window thinner, which reduces its optical power and, due to the manufacturing process, by making the inner and outer surfaces of the window more similar. Both effects lead to significantly reduced optical errors.

[0030] According to one embodiment, a high level of surface planarity and a high level of parallelism of the inner and outer surfaces of the lateral sidewall regions of the cover element of the formed cover substrate are achieved in the step of annealing and providing an overpressure.

[0031] In a subsequent step 150, the stop element and the molded substrate are removed from the molded cover substrate, whereby the molded cover substrate now forms the lid substrate with the at least one lid element. As the following explanations will show, the lid substrate can be used to package one or a plurality of optical or optoelectronic components.

[0032] As already mentioned above, according to one embodiment, the cover substrate comprises a single homogeneous material, such as a glass material, in order to form the molded cover substrate, i.e., the lid substrate or the glass cap, from a single surrounding material. Thus, the individual lid elements are also formed integrally (in one piece) from a single homogeneous material, e.g., the glass material.

[0033] In this context, reference is also made to the Fig. 2-6and the associated description of the basic flow diagrams of possible implementations of the manufacturing method 100 according to the invention, in which these method steps are shown or implemented.

[0034] According to one embodiment, step 120 of providing the mold substrate and the cover substrate, which are connected to one another, can comprise the following steps (substeps). Thus, first, in a step 110, the mold substrate, e.g., a silicon wafer, with the structured surface region (provided with depressions or recesses) is provided. Furthermore, the cover substrate, e.g., a glass wafer, is provided.

[0035] In step 112, the cover substrate is arranged on the structured surface area of ​​the mold substrate, wherein the cover substrate comprises a glass material. For example, the surface area of ​​the cover substrate that abuts (i.e., lies opposite) the mold substrate can be flat or planar (i.e., without recesses or depressions).

[0036] In a step 114, the cover substrate is then connected or joined to the mold substrate, e.g., hermetically connected by anodic bonding or another joining technique, to form at least one sealed cavity (or a plurality of sealed cavities) between the cover substrate and the mold substrate. The recess(es) arranged in the mold substrate then each form the at least one sealed cavity between the cover substrate and the mold substrate.

[0037] According to a further embodiment, step 110 of providing the mold substrate and the cover substrate may further comprise the following steps or substeps. For example, in step 112-1, the mold substrate, e.g., a silicon wafer, may be provided. In step 114-1, the cover substrate, e.g., a glass wafer having a structured (= recessed) surface area, may be arranged or positioned on the mold substrate. For example, the surface area of ​​the mold substrate that abuts or lies opposite the cover substrate may have a flat or planar shape.

[0038] In step 114, the cover substrate is again connected or joined to the mold substrate, e.g., hermetically connected by anodic bonding or by a joining process, to form the at least one sealed cavity or the plurality of sealed cavities between the cover substrate and the mold substrate. The at least one sealed cavity is thus formed, for example, by the recess(es) or structure(s) arranged in the cover substrate.

[0039] According to a further alternative embodiment, both the mold substrate and the cover substrate can have a structured surface region provided with recesses to jointly form the at least one sealed cavity between the cover substrate and the mold substrate. For example, during the (aligned) arrangement of the cover substrate on the mold substrate, the recess provided in the cover substrate and the mold substrate can be aligned with each other in order to then form the sealed cavity(ies) between the cover substrate and the mold substrate during the joining step, e.g., hermetic joining by anodic bonding.

[0040] According to one embodiment of the method, the (hermetic) bonding of the cover substrate to the mold substrate is carried out in an atmosphere with a defined atmospheric ambient pressure in order to enclose a defined atmospheric pressure in the closed cavities. In this context, reference is also made, for example, to the Fig. 2-6 and the associated description.

[0041] According to one embodiment of the method, the cover substrate and / or the mold substrate are configured to form the closed cavity with a plurality of closed cavity regions between the cover substrate and the mold substrate, wherein the closed cavity regions are arranged fluidically separated from one another. According to a further embodiment, gas exchange channels are further provided between the cavity regions closed from the ambient atmosphere in order to fluidically connect them to one another in order to maintain a common defined atmospheric pressure in the connected cavity regions relative to the ambient atmosphere. In this context, reference is also made, for example, to the Fig. 2-6 and the corresponding description.

[0042] According to one embodiment of the method 100, the step of tempering and providing an overpressure is carried out as a glass flow process, for example, in a vacuum furnace, in order to maintain a defined atmospheric overpressure in the closed cavity relative to the surrounding atmosphere. In this context, reference is also made, for example, to the Fig. 2-6 and the corresponding description.

[0043] According to one embodiment, the method 100 further comprises the following steps: cooling the stop element, the mold substrate, and the molded cover substrate, and subsequently removing the mold substrate by means of an etching process, e.g., by means of a semiconductor etching process or a silicon etching process of the semiconductor material or the silicon material of the mold substrate. In this context, reference is also made, for example, to the Fig. 2-6 and the corresponding description.

[0044] According to one embodiment, the method further comprises the following step: subsequently removing the stop element by means of an etching process. In this context, reference is also made, for example, to the Fig. 2-6 with associated description.

[0045] According to one embodiment of the method, the cover substrate is bulged or blown out during the step of annealing and providing an overpressure in the region of the closed cavity up to a height that is predetermined by the vertical distance of the stop surface ("flat stop surface") to the cover substrate. In this context, reference is also made, for example, to the Fig. 2-6 and the corresponding description.

[0046] According to one embodiment of the method 100, the region of the stop surface of the stop element opposite the cavity or the cavity regions is formed flat and parallel to the main surface region of the cover substrate (parallel to the reference plane) in order to form a flat cover region of the cover element during the step of annealing and providing an overpressure. In this context, reference is also made, for example, to the Fig. 2-6 and the corresponding description.

[0047] According to one embodiment of the method, during cooling of the molded cover substrate in a temperature range above 650 °C, e.g., between 650 °C and 950 °C or between 650 °C and 750 °C, an atmospheric overpressure is created in the closed cavities relative to the surrounding atmosphere in order to generate an (e.g., convex) curvature of the side wall regions (= side windows = "optically passive" side windows) of the cover element of the molded cover substrate outward.

[0048] According to one embodiment of the method 100, the step of annealing and providing an overpressure is carried out in a vacuum furnace, wherein the atmospheric overpressure in the sealed cavities relative to the surrounding atmosphere is maintained by a reduced atmospheric pressure in the vacuum furnace. In this context, reference is also made, for example, to the Fig. 2-6 and the corresponding description.

[0049] According to one embodiment of the method, during cooling of the molded cover substrate in a temperature range above 650 °C, e.g., between 650 °C and 950 °C or between 650 °C and 750 °C, an atmospheric negative pressure is created in the closed cavities relative to the surrounding atmosphere in order to produce a (concave) curvature of the side wall regions (= side windows) of the cover element of the molded cover substrate inwards.

[0050] According to one embodiment of the method 100, the step of annealing and providing an overpressure is carried out in a vacuum furnace, wherein the atmospheric negative pressure in the sealed cavities relative to the surrounding atmosphere is maintained by an increased atmospheric pressure in the vacuum furnace. In this context, reference is made, for example, to the Fig. 2-6 and the corresponding description.

[0051] According to one embodiment of the method 100, the stop element (= chuck) is designed as a reusable tool and has a non-stick coating for the glass material of the cover substrate at least on the region of the stop surface opposite the cavity or on an entire stop surface. In this context, reference is also made, for example, to the Fig. 2-6 and the corresponding description.

[0052] The stop element can, for example, comprise or consist of a semiconductor material, such as silicon, and have an at least partially or completely flat (plane) stop surface opposite the cover substrate. In addition to a semiconductor component, the stop element can also comprise or consist of other materials, such as silicon carbide (SiC), graphite, or aluminum nitride (AlN).

[0053] The flat stop surface in this process 100 can be used as a reusable tool (see also Fig. 6 ) can be used multiple times. Several materials are in principle suitable for the production of such a stop surface, including temperature-resistant steels and ceramics (e.g. SiC, glassy carbon or others), especially if these stop surfaces are additionally provided with a coating, e.g. graphite or boron nitride (BN), which prevents the glass mass from sticking. By applying such a repellent protective layer, a process according to Figures 1 to 6 Such a stop surface can also be made of silicon.

[0054] According to one embodiment, the method 100 further comprises the step of applying, such as depositing, a metallization as a coherent frame structure (= a sealing frame) on connection regions at non-bulged regions (= base regions) of the formed cover substrate (= the lid substrate). In this context, reference is also made, for example, to the Fig. 2-6 and the corresponding description.

[0055] According to one embodiment of the method, the cover substrate can have a partially formed recess (= partially thinned area) in the first main surface area. This partially formed recess can be provided, for example, to make the base area of ​​the cover elements of the formed cover substrate (which is not curved during the blow-out process) as thin as possible. In this context, reference is also made, for example, to the Fig. 2aand the corresponding description.

[0056] According to one embodiment of the method 100, an anti-reflection coating is applied or deposited on a region (ceiling region and / or sidewall region) of the cover element of the formed cover substrate. In this context, reference is also made, for example, to the Fig. 2-6 and the corresponding description.

[0057] In the following, some further technical explanations of the various steps of the manufacturing method 100 described above, as well as the elements and structures mentioned, are presented by way of example. Unless otherwise stated, these following explanations are applicable to all exemplary embodiments and are to be viewed as alternative or additional embodiments of individual method steps or individual elements or structures.

[0058] Within the scope of the present description, the mold substrate is provided, for example, with a topographically structured surface region (first main surface region). This means that a surface region (the first main surface region) of the mold substrate has one or more depressions. The surface region of the mold substrate can have the depressions over its entire lateral extent up to a few millimeters at or in front of the edge in order to maintain the cavities and / or gas exchange channels during the hermetic bonding of the mold substrate to the cover substrate. The mold substrate can therefore have a negative topography.

[0059] Furthermore, first recesses (cavity regions) in the mold substrate can be provided to form cavities or bulges for an optoelectronic (radiation-emitting or radiation-receiving) component in the cover substrate by blowing out during the glass flow process. Furthermore, adjacent second cavity regions can be configured to form a cavity for a dicing lane or to serve to expose the electrical connection pads in the housing during subsequent process steps.

[0060] According to the present description, an inversion or inverted arrangement of these functional units is also possible. Thus, a cavity region or a depression according to the present description can be a surface or trench structure recessed relative to the substrate surface, which was introduced into the mold substrate by an etching process. Basic geometries for the cavity regions can depend on the required cap geometry (cover substrate geometry) and are essentially freely selectable. Thus, square, rectangular, trapezoidal, and linearly elongated shapes with possibly not necessarily rectangular corners, as well as other shapes with linear edge sections, are possible. Furthermore, circular or ellipsoidal basic shapes are also possible.

[0061] In the context of the present description, tempering (see step 130) refers to a temperature treatment, for example, a time-controlled, homogeneous heating or cooling, wherein this tempering step is carried out, for example, in a defined, controllable pressure environment, i.e., under defined ambient pressure conditions. According to one embodiment, tempering step 130 can be carried out in a temperature range above 650°C, e.g., between 650°C and 955°C or between 650°C and 750°C.

[0062] A glass material within the meaning of the present description is, for example, an amorphous inorganic material whose viscosity decreases with increasing temperature (e.g. continuously).

[0063] In the illustrated manufacturing method 100, a cover substrate (molded cover substrate) is produced with one or more cover elements. The cover element has a lateral and an upper sidewall region, which can also function as optical window regions. These optical window regions allow beam coupling and / or beam coupling from lateral to vertical to the carrier substrate.

[0064] According to the illustrated manufacturing method 100, the cover substrate, which can also be referred to as a cap or lid wafer, is manufactured with the lateral, optically passive window surfaces made of glass, for example, for a variety of packages. The lateral, optically passive window surfaces can thus be formed, for example, vertically (= extending vertically) to the original main surface area of ​​the cover substrate.

[0065] The method described is essentially based on so-called glass flow techniques. In the embodiments, the glass material of the cover substrate can be Borofloat® glass or another glass such as Schott AF32, Corning Eagle XG, Hoya SD2. The coefficient of thermal expansion (CTE) of the glass materials is selected, for example, to match the semiconductor material used, since both the production of the cover wafer (cover substrate) and the bonding of the cover wafer take place on the semiconductor material of the mold substrate, for example, on a silicon substrate. Excessive differences in the coefficient of thermal expansion could otherwise lead to very large thermomechanical stresses or to the destruction of the elements involved if the CTE of the glass material of the cover substrate is not (e.g.within a tolerance range of less than 1%, 5%, or 10%) to the CTE of the semiconductor material of the molding substrate. "Adapted" means, for example, that the CTE of the glass material in embodiments does not deviate from the CTE of the semiconductor material by more than 1-2 ppm / K. In the embodiments, the CTE of the glass material deviates from the CTE of the semiconductor material by, for example, less than 0.5 ppm / K.

[0066] The cover substrate 20 has a thickness of, for example, 100 µm to 1500 µm or 300 µm to 800 µm. This allows a thickness of the window elements 24-1, i.e., the areas of the window elements 24-1 effective for light transmission, of 20 µm to 1200 µm or 20 µm to 300 µm. A window thickness of 20 µm to 300 µm is provided, for example, for optical transmission windows 24-1. The vertical distance h between the (flat) stop surface 40-1 of the stop element 40 and the (undeformed) cover substrate 20 is, for example, 1.2 mm to 10 mm.

[0067] A possible process sequence for the production of these lid wafers with optical window surfaces is shown below, for example, using the Figures 2-6These lid wafers, i.e. the lid substrates, can be manufactured with integrated vertical, convex or concave optical window surfaces. Optical window surfaces are considered to be, for example, areas of the lid wafer whose wall thickness homogeneity across the area illuminated by the beam does not differ by more than 15% and / or whose surfaces have a roughness of less than 50 nm. Optical window surfaces can have very different geometric shapes: vertically flat, vertically concave, vertically convex, uniaxially inclined, rotationally symmetrically inclined and, if necessary, with an offset, and plane-parallel to the base plane of the lid wafer. The optical window surfaces serve for beam coupling and / or beam extraction for at least one radiation or light-emitting component and optionally for one or more photodetectors.For example, several optical side windows can be provided in the same cover element on different sides in order to allow, for example, lateral beam decoupling and / or beam coupling in different directions.

[0068] In the different embodiments (e.g. the process sequences shown below in Fig. 2-6 ) of method 100, the lid elements (= glass lids) are formed through a tempering process. The geometry achieved at the end of the process is influenced by four variables: the enclosed gas volume, the temperature profile, the pressure in the furnace, and the distance from the stop.

[0069] In one possible (simple) implementation of the process sequence, the pressure in the furnace is constant throughout, with the pressure trapped in the cavity being at least temporarily greater than the pressure in the furnace. The furnace temperature should follow a profile consisting of a heating phase, a processing phase, and a cooling phase. The temperature of the processing phase should be above the softening temperature of the glass so that the pressure of the trapped gas can inflate the cavity. If the pressure inside the cavity is always greater than the pressure in the furnace, the wall surface will become convex. If, on the other hand, the process is conducted in such a way that the pressure in the inflated cavity approaches the furnace pressure (equilibrium state), cooling the furnace can reverse the pressure so that the pressure in the furnace is greater than that inside the cavity.This leads to a deformation of the convex surface, allowing a flat, almost plane wall to be achieved, at least in some areas. However, geometric control is significantly increased by inflating against a stop. In extreme cases, it is even possible to achieve a convex cross-section of the wall. Apart from the described effect of temperature change, such a reversal of the pressure conditions can also be achieved by changing the, for example, regulated, furnace pressure.

[0070] Another way to influence the geometry of the cap (the lid element) is to move the stop during annealing. If the glass is first inflated to a spherical shape before the stop is brought into contact with the substrate by reducing the distance, the cavity lid is created with a very uniform thickness. If the distance between the substrate and the stop is increased again after the glass has come into contact with it, this leads to an elongation of the walls. The initially convex cross-section of the walls is thereby flattened. If the distance is further increased, the cross-section in the area of ​​the walls constricts, giving them a convex cross-section.

[0071] The combination of mechanical movement with the previously described pressure and temperature changes enables the targeted influence of the cap geometry and in particular the wall cross-section.

[0072] In the different embodiments (e.g. the process sequences shown below in Fig. 2-6 ) of the method 100, it is provided that in steps 110 and 112 the mold substrate and the cover substrate are provided and the same are anodically bonded.

[0073] According to one embodiment, the method 100 with regard to providing 110 the mold substrate may comprise the following steps: providing a semiconductor wafer with a passivation layer on a surface (= first main surface region), lithographing the passivation layer such that the resist layer is removed on the surface where the depressions and gas channels are provided, etching the passivation layer on the surface of the semiconductor wafer with regard to the lithographed regions, removing the resist layer, etching the exposed semiconductor material such that a thickness of the semiconductor wafer is reduced perpendicular to the lithographed regions of the surface in order to structure the surface region and thus provide depressions, e.g. cavities and gas channels, and completely removing the passivation layer.

[0074] This allows, for example, the mold substrate to be manufactured and provided with a suitably structured surface area. For example, the semiconductor wafer is a silicon wafer. The semiconductor wafer can be coated with an etch-resistant passivation, for example, made of LP nitride (LP = low pressure) in an LP-CVD process (LP-CVD = low pressure chemical vapor deposition). Lithography is then performed. The passivation is opened by plasma etching. The lithographed areas can be processed by plasma-assisted gas-phase etching, for example, anisotropic high-rate etching or isotropic wet etching, so that the surface of the semiconductor wafer is etched with respect to the lithographed areas. Finally, the passivation layer is completely removed, for example, by selective etching.

[0075] According to one embodiment of the first method, the method comprises the following step during the arrangement 112 and connection 114 of the cover substrate: surface anodic bonding of the recessed surface region of the mold substrate to the overlying surface region of the cover substrate. A glass wafer suitable as a cover substrate can, for example, comprise (consist of) Pyrex, Borofloat®<33, or similar glass materials with a low CTE. Such glass materials can be characterized by their particularly good suitability for use in glass flow processes.

[0076] According to one embodiment, the overpressure for bulging the glass material of the cover substrate can be achieved by enclosing an increased gas pressure in the closed cavities 30 between the cover substrate 20 and the mold substrate 10 in order to maintain the overpressure in the cavities 30 relative to the ambient atmosphere. For example, the bonding process 114 of the cover substrate 20 and the mold substrate 10 can be performed in a defined atmosphere to enclose such a high, defined gas pressure in the cavities and channel structures 30 that the subsequent process of bulging the glass material of the cover substrate can also be performed at normal ambient pressure or a corresponding (reduced) negative pressure of the ambient atmosphere.An enclosed gas pressure in the cavities 30 can therefore be provided in order to effect or (at least) assist the blowing out of the glass material by means of a pressure difference.

[0077] Alternatively or additionally, the atmospheric overpressure in the closed cavities 30 relative to the ambient atmosphere can also be maintained in a so-called negative pressure furnace, in that the negative pressure furnace provides the ambient atmosphere for the manufacturing process with an atmospheric negative pressure (relative to the set gas pressure in the cavities 30).

[0078] In the following, the Fig. 2-6 exemplary process sequences or process flows for the implementation of the Fig. 1 The basic manufacturing process 100 shown in FIG. Fig. 2-6 the drawing plane extends parallel to the xz-plane.

[0079] All process alternatives of method 100 described below are based on the fundamental concept that a cover substrate for housing one or a plurality of optical (optoelectronic) components is produced using a hot-viscous glass flow process, wherein the formed cover substrate forms the cover substrate with the at least one optically neutral cover element. The cover element has an optically neutral (passive) side window (= glass window).Hermetically sealed cavities between the cover substrate and the mold substrate are used to achieve a defined bulging of the glass material of the cover substrate during annealing of the cover substrate and the mold substrate. This bulging action reduces the viscosity of the glass material of the cover substrate and creates an overpressure in the sealed cavity relative to the surrounding atmosphere. This creates the molded cover substrate with the cover element or bulge. This cover element with the optically passive glass window can then be used to package optoelectronic components, such as radiation-emitting and / or radiation-receiving components.

[0080] Fig. 2now shows an exemplary flow diagram 100-1 of the manufacturing method 100 according to the invention for producing a cover substrate which can be used, for example, for housing one or a plurality of optical or optoelectronic components. The window elements can thus be formed, for example, as erected side windows.

[0081] In step 110, the mold substrate 10, e.g., a semiconductor or silicon wafer, is first provided with the structured surface region 10-1, i.e., the mold substrate 10 is provided with at least one depression or recess 12. Furthermore, the cover substrate 20, e.g., a glass wafer, is provided.

[0082] According to one embodiment, the mold substrate 10 can be formed as a semiconductor substrate (semiconductor wafer or silicon wafer) and the cover substrate 20 as a glass substrate or glass wafer. The mold substrate 10 is, for example, a molded substrate with a shape, contour, or topography, such as a topographically structured substrate. The mold substrate can be formed, for example, as a semiconductor wafer, e.g., a silicon wafer, wherein the surface structuring or topography of the mold substrate can be obtained extremely precisely using semiconductor processing steps or silicon processing steps. The cover substrate 20 comprises, for example, a single homogeneous material or glass material in order to form the molded cover substrate 20 as a lid substrate or glass cap in one piece with the subsequent manufacturing steps.

[0083] In a step 112, the cover substrate 20 is arranged in alignment with the structured surface region 10-1 of the mold substrate 10. For example, the second main surface region 20-2 of the cover substrate 20, which abuts the mold substrate 10, ie, the raised regions of the structured surface region 10-1 of the mold substrate 10, can be flat or planar and thus formed without recesses or depressions.

[0084] In a step 114, the cover substrate 20 is then connected or joined to the mold substrate 10, e.g., hermetically bonded by anodic bonding, to form at least one sealed cavity 30 between the cover substrate 20 and the mold substrate 10. The recess 12 arranged in the mold substrate 10, or the recesses 12 arranged in the mold substrate 10, then each form the at least one sealed cavity 30 between the cover substrate 20 and the mold substrate 10.

[0085] According to one embodiment of the flowchart 100-1 of the method 100, the (hermetic) bonding 114 of the cover substrate 20 to the mold substrate 10 is performed in an atmosphere with a defined atmospheric ambient pressure in order to enclose a defined atmospheric pressure in the closed cavities 30.

[0086] In preparation for the actual manufacturing process, the mold substrate 10, e.g., a silicon mold substrate, is provided with one-sided cavities and channel structures 12 (= recesses or depressions). The glass wafer 20 is aligned with the mold substrate 10 and bonded, for example, anodically, in a defined atmosphere to confine a (defined) gas pressure in the cavities and channel structures 30.

[0087] According to one embodiment of the flow diagram 100-1 of the method 100, the cover substrate 20 and / or the mold substrate 10 are configured to form the closed cavity 30 with a plurality of closed cavity regions 30 between the cover substrate 20 and the mold substrate 10, wherein the closed cavity regions 30 are arranged fluidically separated from one another, or wherein gas exchange channels 30-1 are further provided between the cavity regions 30 closed from the ambient atmosphere in order to fluidically connect them to one another in order to maintain a common defined atmospheric pressure in the connected cavity regions 30.

[0088] In step 120, the mold substrate 10 and the cover substrate 20, which are bonded to one another, are provided, wherein the surface region 10-1 of the mold substrate 10 is structured (formed with recesses or channel structures 12) to form the at least one closed cavity 30 between the cover substrate 20 and the mold substrate 10. In step 120, for example, an anodically bonded glass-silicon cover substrate 10, 20 is obtained or provided.

[0089] In a (subsequent) step 130, the cover substrate 20 and the mold substrate 10 are now tempered, i.e., subjected to a temperature treatment or heated (warmed), in order to reduce the viscosity of the glass material of the cover substrate 20. Furthermore, in a step 140, an overpressure is provided in the (at least one) sealed cavity or cavities 30 relative to the surrounding atmosphere in order to effect, based on the reduced viscosity of the glass material of the cover substrate 20 and the overpressure in the sealed cavity 30 relative to the surrounding atmosphere, a defined bulging, e.g., blowing out or deformation, of the glass material of the cover substrate 20, starting from the sealed cavity 30 up to a stop surface 40-1 of a stop element 40 spaced apart from the cover substrate 20.The defined bulging of the glass material of the cover substrate 20 due to the overpressure in the closed cavity 30 and the reduced viscosity of the glass material can also be referred to as blowing out or deformation of the glass material. The defined bulging of the glass material of the cover substrate 20 thus results in a shaped cover substrate 20' with (at least) one cover element 24 (= bulging or deformation). The resulting bulging or deformation of the shaped cover substrate (= cover substrate) 20' is thus referred to as the cover element 24. According to one embodiment, the annealing step 130 can be carried out in a temperature range above 650°C, e.g., between 650°C and 955°C or between 650°C and 750°C.

[0090] Furthermore, the defined bulging of the cover substrate 20 causes or forms the side windows 24-1 on the cover element 24. The side region of the cover element 24 is also referred to as an (optically passive or neutral) window element or optically passive glass window 24-1 (= lateral window element).

[0091] According to one embodiment of the flow diagram 100-1 of the method 100, the step of tempering 130 and providing 140 an overpressure is carried out as a glass flow process in a vacuum furnace 50 in order to obtain a defined atmospheric overpressure in the closed cavity 30 compared to the surrounding atmosphere. According to one embodiment of the flow diagram 100-1 of the method 100, the cover substrate 20 is bulged or blown out in the step of tempering 130 and providing 140 an overpressure in the region of the closed cavity 30 up to a height h which is predetermined by the vertical distance of the stop surface 40-1 of the stop 40 to the first main surface region 20-1 of the cover substrate 20.

[0092] According to one embodiment of the flowchart 100-1 of the method 100, the region of the stop surface 40-1 of the stop element 40 opposite the cavity 30 or the cavity regions 30 is flat and parallel to the main surface region 20-1 of the cover substrate 20 (= parallel to the reference plane) in order to form a flat cover region 24-2 of the cover element 24 during the step of annealing 130 and providing 140 an overpressure. According to one embodiment, the stop element 40 can be designed as a reusable tool.

[0093] The glass flow process 130, 140 can thus be carried out in a pressure-controlled furnace 50. The glass wafer (cover substrate) 20 is blown out in the region of the cavities 30 up to the height h, which can be determined by a stop surface 40-1 of the stop element 40. The stop 40 and thus the stop surface 40-1 are designed to be flat, for example. After the glass flow process 130, 140, the cover substrate 20' is cooled and removed from the furnace 50, for example. After the glass flow process 130, 140, the wafers 10, 20' are cooled in the blown-out state.

[0094] According to one embodiment of the flowchart 100-1 of the method 100, in a step 142, the cooling of the molded cover substrate 20' can be carried out in a defined manner in order to produce a convex or a concave curvature of the side wall regions (side windows) 24-1 of the cover element 24 of the molded cover substrate 20'.

[0095] In a subsequent step 150, the stop element 40 and the molded substrate 10 are removed from the molded cover substrate 20', whereby the molded cover substrate 20' now forms the lid substrate 20' with the at least one lid element 24. The lid substrate 20' can be used, for example, for housing one or a plurality of optical or optoelectronic components.

[0096] According to one embodiment, the flowchart 100-1 of the method 100 may further include the step 142 of cooling the stop element 40, the mold substrate 10 and the molded cover substrate 20', wherein the mold substrate 10 is then removed in step 150 by means of an etching process, e.g., a silicon or semiconductor etching process of the silicon or semiconductor material of the mold substrate.

[0097] According to one embodiment, the step 150 of removing the stop element 40 is also carried out by means of an etching process, e.g., by means of a silicon or semiconductor etching process of the silicon or semiconductor material of the stop 40.

[0098] Since the cover substrate 20 according to one embodiment comprises a single homogeneous material, e.g., a glass material, the shaped cover substrate 20', ie, the lid substrate or the glass cap, is also formed integrally with the at least one lid element 24 and from a single homogeneous material, e.g., the glass material.

[0099] In step 150, for example, a glass cover substrate 20' with the side windows 24-1 of the glass caps 24 is obtained after the removal of the silicon from both sides of the mold substrate 10 and the stop element 50. The side windows 24-1 can be circumferential or segmented.

[0100] In an (optional) subsequent step 160, the process flow 100-1 of the method 100 may further comprise applying or depositing a metallization 60 as a (continuous) frame structure or as a sealing frame on connection regions 62 on the second main surface region 20-2 on non-bulged regions (base regions) 24-3 of the lid elements 24 of the formed cover substrate (the lid substrate) 20'.

[0101] According to one embodiment, at step 160, an anti-reflective coating 64 may further be applied or deposited on an inside and / or outside region, e.g., inside and / or outside of the ceiling region 24-2 and / or sidewall region 24-1, of the lid element 24 of the molded cover substrate 20'.

[0102] In the optional step 160, sealing frames 60 and / or optional anti-reflective coatings 64 can thus be deposited on the cover substrate 20'. This glass cover substrate 20' can then be used to hermetically seal optical structures at the wafer level, as will be explained below.

[0103] In an (optional) subsequent step 170, the process sequence 100-1 of the method 100 may further include singulating the formed cover substrate 20' to obtain singulated cover elements 24'. The singulation 170 of the glass cover substrate 20' may be performed, for example, by sawing or laser separation. With the singulated caps 24', optical assemblies can be hermetically sealed at the individual substrate level or at the wafer level by individual encapsulation, as will be explained below.

[0104] In the following, some process steps of process flow 100-1 of method 100 of Fig. 2 summarized again.

[0105] Fig. 2shows a flowchart 100-1 which, based on steps 110 to 170, illustrates a first process sequence 100-1 for producing a cover substrate 20'. The cover substrate 20' resulting from the manufacturing method 100-1 has, after the process sequence, for example, an optically passive (neutral) side window 24-1 which is an integral component of the cover element 24 (cap) and allows lateral beam decoupling and / or beam coupling. For example, a plurality of lateral (side) side windows 24-1 (e.g. with a vertical extension) can also be provided, which are an integral component of the cover element 24 (cap) of the cover substrate 20' and allow lateral beam decoupling or beam coupling in different directions, e.g. in different directions parallel to the reference plane (xy plane). For example, a vertical (upper) side window 24-2 (e.g.with lateral extension) may be provided, which is an integral part of the cover element 24 (cap) of the cover substrate 20' and allows a vertical beam coupling or beam coupling, e.g. perpendicular to the reference plane (xy plane).

[0106] The process flow 100-1 of Fig. 2thus comprises as a step 110 of providing the mold substrate with a structured (provided with depressions) surface area, wherein the mold substrate comprises a semiconductor material, such as e.g. silicon, or consists of the semiconductor material, e.g. silicon. This is followed by arranging the unstructured cover substrate on the structured surface area of ​​the mold substrate. The cover substrate comprises a glass material or consists of a glass material. When arranging the cover substrate on the mold substrate, the structured surface of the mold substrate is arranged so as to at least partially overlap a surface of the cover substrate and when connecting the cover substrate to the mold substrate, e.g. anodically bonded or hermetically joined. In this case, the structured surface of the mold substrate is bonded to the surface of the cover substrate, e.g.gas-tight connected to a defined enclosed internal atmosphere in the recesses (cavities).

[0107] This is followed, for example, by annealing 130 the bonded substrates 10, 20 in a vacuum furnace such that the enclosed pressure in relation to the furnace pressure causes the glass material of the cover substrate to blow out in the region of the recesses. The temperatures are selected such that the viscosity of the glass material is significantly reduced and the glass material in the window area can expand in a well-controlled manner but does not melt.

[0108] To assist the blowing process, a pressure difference, e.g., can be established between the interior spaces or cavities located between the substrates and the ambient atmosphere in the furnace. A trapped gas pressure in the interior spaces can be provided to effect or (at least) assist the blowing out of the glass material through a pressure difference. This allows the process to be performed in a single annealing step. The existing pressure difference between the trapped gas pressure in the recessed interior spaces and the controlled vacuum (negative pressure) of the furnace atmosphere supports the entire flow process.

[0109] During the glass flow process, the flow front stops at the stop surface 40-1 of the stop element 40 at an adjustable distance h in the vacuum furnace, wherein the stop element 40 with the stop surface 40-1, for example, has a silicon wafer or consists of a silicon wafer. The flow process with the stop surface 40-1 at a static distance is therefore based on the reduced viscosity of the glass material of the cover substrate 20 and the overpressure in the closed cavity 30 compared to the surrounding atmosphere, wherein the bulging (blowing out / deformation) of the glass material of the cover substrate 20 is effected, starting from the closed cavity 30 up to the stop surface 40-1 of the stop element 40, which is spaced apart from the cover substrate 20, in order to obtain the shaped cover substrate 20' with (at least) one cover element (= bulge) 24.

[0110] During the glass flow process 130, 140, the joined substrates are cooled under a reproducible temperature and pressure ramp and finally the cover substrate 20' with the mold substrate and, for example, the stop element 40 is removed from the furnace 50.

[0111] Then, a removal 150 of the stop element 40 and the mold substrate 10 takes place in order to obtain the structured cover substrate 20' obtained from the cover substrate 20 by the blow-out process. The removal 150 can mean a separation or a selective etching of the semiconductor material of the mold substrate 10 and / or the stop element 40 by means of an etching process (silicon or semiconductor etching process of the silicon or semiconductor material), e.g. in hot potassium hydroxide solution. In this way, an effective method for producing a cover substrate 20' for encapsulating radiation-emitting components is provided, since the cover substrate 20', which is obtained by the method 100 as described in Fig. 2-6described schematically, comprises an (optically passive) output window 24-1 which is formed by means of the window component (cover element) 24.

[0112] In one embodiment of the method 100 for producing a cover substrate 20', the resulting cover substrate 20' has, for example, a side window 24-1, which is an integral component of the cap (the cover element) 24 and allows lateral (= side) beam extraction. For example, multiple side windows 24-1 can also be provided, which are an integral component of the cap 24 and allow lateral beam extraction in different directions, e.g., each in a different direction.

[0113] In the optional step 160, the metallization 60 can further be applied (deposited) as a (continuous) frame structure (a sealing frame) on connecting regions 62 on the second main surface region 20-2 at the non-bulged regions (base regions) 62 of the molded cover substrate (lid substrate) 20'. In the optional step 160, an anti-reflection coating 64 can further be applied or deposited on a region (ceiling region and / or sidewall region) of the lid element 24 of the molded cover substrate 20'. In a further optional step 170, the molded cover substrate 20' can be singulated to obtain singulated lid elements 24'.

[0114] The manufacturing method 100 described above with the exemplary process flow of Fig. 2is a very effective and simple procedure for installing side windows on side areas 24-1 of the respective cover element 24.

[0115] Regarding the Fig. 2 The manufacturing process 100 shown by means of the flow chart 100-1 will now be described in Fig. 2a a further alternative embodiment of the cover substrate 20 with a partially formed recess (= partially thinned out) 20-3 in the first main surface region 20-1 of the cover substrate 20 is shown.

[0116] This region-wise recess 20-3 can now be provided, for example, in order to make the (non-bulged) base region 24-3 of the cover elements 24 of the shaped cover substrate (= cover substrate) 20' as thin as possible, that is to say in order to make the base region 24-3 as thin or flat as possible, at least adjacent to the lateral beam exit region 24-1. This can ensure that, during (subsequent) packaging of an optical component (transmitting and / or receiving component) arranged on a component substrate, the required installation height of the optical component above the component substrate plane is as low as possible. This can ensure that, in the optoelectronic component, this component (e.g., a laser emitter or a photodiode) does not require additional effort, e.g.needs to be mounted elevated on a submount to avoid a collision of the transmitting or receiving radiation of the optical component with an otherwise elevated glass base.

[0117] According to this exemplary embodiment, the base region 24-3 of the cover element 24 can be formed (relatively) flat, at least in the direction of the lateral beam passage of the transmitting or receiving radiation of the optoelectronic component, in order to avoid the need to build the optoelectronic component on an additional elevation, e.g. on a (raised) submount, on the component substrate, so that the transmitting and / or receiving radiation of the optoelectronic component 1 does not collide with the base region (glass base) 24-3 of the cover element or is disturbed by it.

[0118] For this purpose, the glass material of the cover substrate 20 is already placed on the mold substrate 10 with a thinned area 20-3 on the upper side (= on the first main surface area) 20-1, wherein this thinning 20-3 extends at least in the beam coupling-out direction into the frame area of ​​the cover element (the glass cap) 24 or, for example, up to the separation area of ​​the cover substrate 20'.

[0119] This thinning 20-3 can also extend into the area of ​​the window surface 24-1 still to be blown out, which, after the bulging process, is arranged vertically, for example, in order to create a particularly thin-walled window element with a low optical effect in the beam passage area, for example. Furthermore, due to the flat base area 24-3, the thin-walled window element has a large beam passage area without the need to blow the glass cap (the cover substrate) 20 out particularly high during the blowing-out process.

[0120] Fig. 2a shows, by way of example, such a cover substrate provided with thinning regions 20-3 in the step 110 of providing and further after passing through the manufacturing method 100 in the steps 160, 170, wherein the reduced thickness of the base region 24-3 of the cover substrate 20' is clearly shown.

[0121] The provision of these thinning regions 20-3 in the cover substrate is equally applicable to the different process sequences of the manufacturing method 100 shown below, wherein the thinning regions 20-3 of the cover substrate 20 are provided there in order to obtain a targeted, thin configuration of the resulting cover element 24 in the desired sidewall regions and the resulting (improved) optical properties.

[0122] Fig. 3 now shows a further exemplary basic flow diagram 100-2 of the inventive manufacturing method 100 according to a further embodiment. The following essentially describes differences or different method steps of the flow diagram 100-2 of Fig. 3 compared to flowchart 100-1 of Fig. 2 Therefore, the above description of the Fig. 1 and 2accordingly to the following description of the embodiment of Fig. 3 be applied, whereby in the following description, the differences, such as different (= alternative and / or additional) process steps and / or elements, to the process flow 100-1 of Fig. 2 and the resulting technical effects are described.

[0123] Fig. 3 100-2 shows an exemplary flow diagram of the inventive manufacturing method 100 for producing a cover substrate, which can be used, for example, for housing one or a plurality of optical or optoelectronic components. The window elements can thus be formed, for example, as raised, convex (outwardly curved) side windows.

[0124] In step 110, the mold substrate 10, e.g., a semiconductor or silicon wafer, is first provided with the structured surface region 10-1, i.e., the mold substrate 10 is provided with at least one depression or recess 12. Furthermore, the cover substrate 20, e.g., a glass wafer, is provided.

[0125] In a step 112, the cover substrate 20 is arranged in alignment with the structured surface region 10-1 of the mold substrate 10. For example, the second main surface region 20-2 of the cover substrate 20, which abuts the mold substrate 10, ie, the raised regions of the structured surface region 10-1 of the mold substrate 10, can be flat or planar and thus formed without recesses or depressions.

[0126] In a step 114, the cover substrate 20 is then connected or joined to the mold substrate 10, e.g., hermetically bonded by anodic bonding, to form at least one sealed cavity 30 between the cover substrate 20 and the mold substrate 10. The recess 12 arranged in the mold substrate 10, or the recesses 12 arranged in the mold substrate 10, then each form the at least one sealed cavity 30 between the cover substrate 20 and the mold substrate 10.

[0127] According to one embodiment of the flowchart 100-2 of the method 100, the (hermetic) bonding 114 of the cover substrate 20 to the mold substrate 10 is performed in an atmosphere with a defined atmospheric ambient pressure in order to enclose a defined atmospheric pressure in the closed cavities 30.

[0128] In preparation for the actual manufacturing process, the mold substrate 10, e.g., a silicon mold substrate, is provided with one-sided cavities and channel structures 12 (= recesses or depressions). The glass wafer 20 is aligned with the mold substrate 10 and bonded, for example, anodically, in a defined atmosphere to confine a (defined) gas pressure in the cavities and channel structures 30.

[0129] In step 120, the mold substrate 10 and the cover substrate 20, which are bonded to one another, are provided, wherein the surface region 10-1 of the mold substrate 10 is structured (formed with recesses or channel structures 12) to form the at least one closed cavity 30 between the cover substrate 20 and the mold substrate 10. In step 120, for example, an anodically bonded glass-silicon cover substrate 10, 20 is obtained or provided.

[0130] In a (subsequent) step 130, the cover substrate 20 and the mold substrate 10 are now tempered, i.e., subjected to a temperature treatment or heated (warmed), in order to reduce the viscosity of the glass material of the cover substrate 20. Furthermore, in a step 140, an overpressure is provided in the (at least one) sealed cavity or cavities 30 relative to the surrounding atmosphere in order to effect, based on the reduced viscosity of the glass material of the cover substrate 20 and the overpressure in the sealed cavity 30 relative to the surrounding atmosphere, a defined bulging, e.g., blowing out or deformation, of the glass material of the cover substrate 20, starting from the sealed cavity 30 up to a stop surface 40-1 of a stop element 40 spaced apart from the cover substrate 20.The defined bulging of the glass material of the cover substrate 20 due to the overpressure in the closed cavity 30 and the reduced viscosity of the glass material can also be referred to as blowing out or deformation of the glass material. The defined bulging of the glass material of the cover substrate 20 thus results in a shaped cover substrate 20' with (at least) one cover element 24 (= bulging or deformation). The resulting bulging or deformation of the shaped cover substrate (= cover substrate) 20' is thus referred to as the cover element 24. According to one embodiment, the annealing step 130 can be carried out in a temperature range above 650°C, e.g., between 650°C and 955°C or between 650°C and 750°C.

[0131] Furthermore, the defined bulging of the cover substrate 20 causes or forms the side windows 24-1 on the cover element 24. The side region of the cover element 24 is also referred to as an (optically passive) window element or optically passive glass window 24-1.

[0132] According to an embodiment of the flow diagram 100-2 of the method 100, the step of tempering 130 and providing 140 an overpressure is carried out as a glass flow process in a vacuum furnace 50 in order to obtain a defined atmospheric overpressure in the closed cavity 30 compared to the surrounding atmosphere.

[0133] According to one embodiment of the flow diagram 100-2 of the method 100, the cover substrate 20 is bulged or blown out during the step of annealing 130 and providing 140 an overpressure in the region of the closed cavity 30 up to a height h which is predetermined by the vertical distance of the stop surface 40-1 of the stop 40 to the first main surface region 20-1 of the cover substrate 20.

[0134] According to one embodiment of the flow diagram 100-2 of the method 100, the region of the stop surface 40-1 of the stop element 40 opposite the cavity 30 or the cavity regions 30 is flat and parallel to the main surface region 20-1 of the cover substrate 20 (= parallel to the reference plane) in order to form a flat cover region 24-2 of the cover element 24 in the step of annealing 130 and providing 140 an overpressure.

[0135] According to one embodiment of the flow diagram 100-2 of the method 100, in a step 142 of (defined) cooling of the molded cover substrate 20' in a temperature range above 650°C, e.g., between 650°C and 955°C or between 650°C and 750°C, an atmospheric overpressure can be effected in the closed cavities 30 relative to the surrounding atmosphere in order to produce a convex curvature of the side wall regions (side windows) 24-1 of the cover element 24 of the molded cover substrate 20' outwards. According to one embodiment of the method, the step of annealing 130 and providing 140 an overpressure can be carried out in a vacuum furnace 50, wherein the atmospheric overpressure in the closed cavities 30 relative to the surrounding atmosphere is maintained by a reduced atmospheric pressure in the vacuum furnace 50.

[0136] In a subsequent step 150, the stop element 40 and the molded substrate 10 are removed from the molded cover substrate 20', whereby the molded cover substrate 20' now forms the lid substrate 20' with the at least one lid element 24. The lid substrate 20' can be used, for example, for housing one or a plurality of optical or optoelectronic components.

[0137] According to one embodiment, the flowchart 100-2 of the method 100 may further include the step 142 of cooling the stop element 40, the mold substrate 10 and the molded cover substrate 20', wherein the mold substrate 10 is then removed in step 150 by means of an etching process, e.g., a silicon or semiconductor etching process of the silicon or semiconductor material of the mold substrate.

[0138] In an (optional) subsequent step 160, the process flow 100-2 of the method 100 may further comprise applying or depositing a metallization 60 as a (continuous) frame structure or as a sealing frame on connection regions 62 on the second main surface region 20-2 on non-bulged regions (base regions) 24-3 of the lid elements 24 of the formed cover substrate (the lid substrate) 20'.

[0139] According to one embodiment, at step 160, an anti-reflective coating 64 may further be applied or deposited on an inside and / or outside region, e.g., inside and / or outside of the ceiling region 24-2 and / or sidewall region 24-1, of the lid element 24 of the molded cover substrate 20'.

[0140] In an (optional) subsequent step 170, the process sequence 100-2 of the method 100 may further include singulating the formed cover substrate 20' to obtain singulated cover elements 24'. The singulation 170 of the glass cover substrate 20' may be performed, for example, by sawing or laser separation. With the singulated caps 24', optical assemblies can be hermetically sealed at the individual substrate level or at the wafer level by individual encapsulation, as will be explained below.

[0141] In the following, some process steps of process flow 100-2 of method 100 of Fig. 3 summarized again.

[0142] Fig. 3100-2 shows a flowchart 100-2 illustrating a first process sequence 100-2 for producing a cover substrate 20' based on steps 110 to 170. The cover substrate 20' resulting from the manufacturing method 100-2 has, for example, (at least) an optically passive side window 24-1 after the process sequence, which is an integral part of the cover element 24 (cap) and allows lateral beam coupling and / or beam extraction.

[0143] The process flow 100-2 of Fig. 3Thus, as a step 110, the process comprises providing the mold substrate with a structured (depression-provided) surface region, wherein the mold substrate comprises a semiconductor material, such as silicon, or consists of the semiconductor material, e.g. silicon. This is followed by arranging the unstructured cover substrate on the structured surface region of the mold substrate. The cover substrate comprises a glass material or consists of a glass material. When arranging the cover substrate on the mold substrate, the structured surface of the mold substrate is arranged to at least partially overlap a surface of the cover substrate, and when connecting the cover substrate to the mold substrate, the structured surface of the mold substrate is bonded, e.g., anodically or hermetically. In this case, the structured surface of the mold substrate is bonded to the surface of the cover substrate, e.g.,gas-tight connected to a defined enclosed internal atmosphere in the recesses (cavities).

[0144] This is followed, for example, by annealing 130 the bonded substrates 10, 20 in a vacuum oven such that blowing out of the glass material of the cover substrate in the region of the recesses is caused by the enclosed pressure in relation to the oven pressure.

[0145] During the glass flow process, the flow front is stopped at the stop surface 40-1 of the stop element 40 at an adjustable distance h in the vacuum furnace, wherein the stop element 40 with the stop surface 40-1, for example, has a silicon wafer or consists of a silicon wafer.

[0146] During the glass flow process 130, 140, the bonded substrates are cooled under a reproducible temperature and pressure ramp to create the convex window shape. Finally, the cover substrate 20', along with the mold substrate and, for example, the stop element 40, is removed from the furnace 50.

[0147] Then, the stop element 40 and the mold substrate 10 are removed 150 to obtain the structured cover substrate 20' obtained from the cover substrate 20 by the blow-out process.

[0148] Fig. 4 100-3 now shows an exemplary flow diagram of the inventive manufacturing method 100 for producing a cover substrate, which can be used, for example, for housing one or a plurality of optical or optoelectronic components. The window elements can thus be formed, for example, as raised, concave (inwardly curved) side windows.

[0149] In step 110, the mold substrate 10, e.g., a semiconductor or silicon wafer, is first provided with the structured surface region 10-1, i.e., the mold substrate 10 is provided with at least one depression or recess 12. Furthermore, the cover substrate 20, e.g., a glass wafer, is provided.

[0150] In a step 112, the cover substrate 20 is arranged in alignment with the structured surface region 10-1 of the mold substrate 10. For example, the second main surface region 20-2 of the cover substrate 20, which abuts the mold substrate 10, ie, the raised regions of the structured surface region 10-1 of the mold substrate 10, can be flat or planar and thus formed without recesses or depressions.

[0151] In a step 114, the cover substrate 20 is then connected or joined to the mold substrate 10, e.g., hermetically bonded by anodic bonding, to form at least one sealed cavity 30 between the cover substrate 20 and the mold substrate 10. The recess 12 arranged in the mold substrate 10, or the recesses 12 arranged in the mold substrate 10, then each form the at least one sealed cavity 30 between the cover substrate 20 and the mold substrate 10.

[0152] According to one embodiment of the flowchart 100-3 of the method 100, the (hermetic) bonding 114 of the cover substrate 20 to the mold substrate 10 is performed in an atmosphere with a defined atmospheric ambient pressure in order to enclose a defined atmospheric pressure in the closed cavities 30.

[0153] In preparation for the actual manufacturing process, the mold substrate 10, e.g., a silicon mold substrate, is provided with one-sided cavities and channel structures 12 (= recesses or depressions). The glass wafer 20 is aligned with the mold substrate 10 and bonded, for example, anodically, in a defined atmosphere to confine a (defined) gas pressure in the cavities and channel structures 30.

[0154] In step 120, the mold substrate 10 and the cover substrate 20, which are bonded to one another, are provided, wherein the surface region 10-1 of the mold substrate 10 is structured (formed with recesses or channel structures 12) to form the at least one closed cavity 30 between the cover substrate 20 and the mold substrate 10. In step 120, for example, an anodically bonded glass-silicon cover substrate 10, 20 is obtained or provided.

[0155] In a (subsequent) step 130, the cover substrate 20 and the mold substrate 10 are now tempered, i.e., subjected to a temperature treatment or heated (warmed), in order to reduce the viscosity of the glass material of the cover substrate 20. Furthermore, in a step 140, an overpressure is provided in the (at least one) sealed cavity or cavities 30 relative to the surrounding atmosphere in order to effect, based on the reduced viscosity of the glass material of the cover substrate 20 and the overpressure in the sealed cavity 30 relative to the surrounding atmosphere, a defined bulging, e.g., blowing out or deformation, of the glass material of the cover substrate 20, starting from the sealed cavity 30 up to a stop surface 40-1 of a stop element 40 spaced apart from the cover substrate 20.The defined bulging of the glass material of the cover substrate 20 due to the overpressure in the closed cavity 30 and the reduced viscosity of the glass material can also be referred to as blowing out or deformation of the glass material. The defined bulging of the glass material of the cover substrate 20 thus results in a shaped cover substrate 20' with (at least) one cover element 24 (= bulging or deformation). The resulting bulging or deformation of the shaped cover substrate (= cover substrate) 20' is thus referred to as the cover element 24. According to one embodiment, the annealing step 130 can be carried out in a temperature range above 650°C, e.g., between 650°C and 955°C or between 650°C and 750°C.

[0156] Furthermore, the defined bulging of the cover substrate 20 causes or forms the side windows 24-1 on the cover element 24. The side region of the cover element 24 is also referred to as an (optically passive) window element or optically passive glass window 24-1.

[0157] According to an embodiment of the flow diagram 100-3 of the method 100, the step of tempering 130 and providing 140 an overpressure is carried out as a glass flow process in a vacuum furnace 50 in order to obtain a defined atmospheric overpressure in the closed cavity 30 compared to the surrounding atmosphere.

[0158] According to one embodiment of the flow diagram 100-3 of the method 100, the cover substrate 20 is bulged or blown out during the step of annealing 130 and providing 140 an overpressure in the region of the closed cavity 30 up to a height h which is predetermined by the vertical distance of the stop surface 40-1 of the stop 40 to the first main surface region 20-1 of the cover substrate 20.

[0159] According to an embodiment of the flow diagram 1003 of the method 100, the region of the stop surface 40-1 of the stop element 40 opposite the cavity 30 or the cavity regions 30 is flat and parallel to the main surface region 20-1 of the cover substrate 20 (= parallel to the reference plane) in order to form a flat cover region 24-2 of the cover element 24 in the step of annealing 130 and providing 140 an overpressure.

[0160] According to a further embodiment of the flow diagram 100-3 of the method 100, in step 142 of (defined) cooling of the molded cover substrate 20' in a temperature range above 650°C, e.g., between 650°C and 955°C or between 650°C and 750°C, an atmospheric negative pressure can be brought about in the closed cavities 30 relative to the surrounding atmosphere in order to produce a concave curvature of the side wall regions (side windows) 24-1 of the cover element 24 of the molded cover substrate 20' inwards. According to one embodiment of the method 100-3, the step of annealing 130 and providing 140 the overpressure in the vacuum furnace 50 is carried out, wherein furthermore the atmospheric negative pressure P in the closed cavities 30 relative to the surrounding atmosphere is maintained by an increased atmospheric pressure in the vacuum furnace 50.

[0161] In a subsequent step 150, the stop element 40 and the molded substrate 10 are removed from the molded cover substrate 20', whereby the molded cover substrate 20' now forms the lid substrate 20' with the at least one lid element 24. The lid substrate 20' can be used, for example, for housing one or a plurality of optical or optoelectronic components.

[0162] According to one embodiment, the flowchart 100-3 of the method 100 may further include the step 142 of cooling the stop element 40, the mold substrate 10 and the molded cover substrate 20', wherein the mold substrate 10 is then removed in step 150 by means of an etching process, e.g., a silicon or semiconductor etching process of the silicon or semiconductor material of the mold substrate.

[0163] In an (optional) subsequent step 160, the process flow 100-3 of the method 100 may further comprise applying or depositing a metallization 60 as a (continuous) frame structure or as a sealing frame on connection regions 62 on the second main surface region 20-2 on non-bulged regions (base regions) 24-3 of the lid elements 24 of the formed cover substrate (the lid substrate) 20'.

[0164] According to one embodiment, at step 160, an anti-reflective coating 64 may further be applied or deposited on an inside and / or outside region, e.g., inside and / or outside of the ceiling region 24-2 and / or sidewall region 24-1, of the lid element 24 of the molded cover substrate 20'.

[0165] In an (optional) subsequent step 170, the process sequence 100-3 of the method 100 may further include singulating the formed cover substrate 20' to obtain singulated cover elements 24'. The singulation 170 of the glass cover substrate 20' may be performed, for example, by sawing or laser separation. With the singulated caps 24', optical assemblies can be hermetically sealed at the individual substrate level or at the wafer level by individual encapsulation, as will be explained below.

[0166] In the following, some process steps of process flow 100-3 of method 100 of Fig. 4 summarized again.

[0167] Fig. 4100-3 shows a flowchart 100-3 illustrating, based on steps 110 to 170, a first process sequence 100-3 for producing a cover substrate 20'. The cover substrate 20' resulting from the manufacturing method 100-3 has, for example, (at least) an optically passive side window 24-1 after the process sequence, which is an integral part of the cover element 24 (cap) and allows lateral beam coupling and / or beam extraction.

[0168] The process flow 100-3 of Fig. 4Thus, as a step 110, the process comprises providing the mold substrate with a structured (depression-provided) surface region, wherein the mold substrate comprises a semiconductor material, such as silicon, or consists of the semiconductor material, e.g. silicon. This is followed by arranging the unstructured cover substrate on the structured surface region of the mold substrate. The cover substrate comprises a glass material or consists of a glass material. When arranging the cover substrate on the mold substrate, the structured surface of the mold substrate is arranged to at least partially overlap a surface of the cover substrate, and when connecting the cover substrate to the mold substrate, the structured surface of the mold substrate is bonded, e.g., anodically or hermetically. In this case, the structured surface of the mold substrate is bonded to the surface of the cover substrate, e.g.,gas-tight connected to a defined enclosed internal atmosphere in the recesses (cavities).

[0169] This is followed, for example, by annealing 130 the bonded substrates 10, 20 in a vacuum oven such that blowing out of the glass material of the cover substrate in the region of the recesses is caused by the enclosed pressure in relation to the oven pressure.

[0170] During the glass flow process, the flow front is stopped at the stop surface 40-1 of the stop element 40 at an adjustable distance h in the vacuum furnace, wherein the stop element 40 with the stop surface 40-1, for example, has a silicon wafer or consists of a silicon wafer.

[0171] During the glass flow process 130, 140, the bonded substrates are cooled under a reproducible temperature and pressure ramp to create the concave window shape. Finally, the cover substrate 20', along with the mold substrate and, for example, the stop element 40, is removed from the furnace 50.

[0172] Then, the stop element 40 and the mold substrate 10 are removed 150 to obtain the structured cover substrate 20' obtained from the cover substrate 20 by the blow-out process.

[0173] Fig. 5 now shows an exemplary flow diagram 100-4 of the inventive manufacturing method 100 for producing a lid substrate 20` with a reusable stop element 40 or with a reusable stop surface 40.

[0174] In step 110, the mold substrate 10, e.g., a semiconductor or silicon wafer, is first provided with the structured surface region 10-1, i.e., the mold substrate 10 is provided with at least one depression or recess 12. Furthermore, the cover substrate 20, e.g., a glass wafer, is provided.

[0175] In a step 112, the cover substrate 20 is arranged in alignment with the structured surface region 10-1 of the mold substrate 10. For example, the second main surface region 20-2 of the cover substrate 20, which abuts the mold substrate 10, ie, the raised regions of the structured surface region 10-1 of the mold substrate 10, can be flat or planar and thus formed without recesses or depressions.

[0176] In a step 114, the cover substrate 20 is then connected or joined to the mold substrate 10, e.g., hermetically bonded by anodic bonding, to form at least one sealed cavity 30 between the cover substrate 20 and the mold substrate 10. The recess 12 arranged in the mold substrate 10, or the recesses 12 arranged in the mold substrate 10, then each form the at least one sealed cavity 30 between the cover substrate 20 and the mold substrate 10.

[0177] In step 120, the mold substrate 10 and the cover substrate 20, which are bonded to one another, are provided, wherein the surface region 10-1 of the mold substrate 10 is structured (formed with recesses or channel structures 12) to form the at least one closed cavity 30 between the cover substrate 20 and the mold substrate 10. In step 120, for example, an anodically bonded glass-silicon cover substrate 10, 20 is obtained or provided.

[0178] In a (subsequent) step 130, the cover substrate 20 and the mold substrate 10 are now tempered, i.e., subjected to a temperature treatment or heated (warmed), in order to reduce the viscosity of the glass material of the cover substrate 20. Furthermore, in a step 140, an overpressure is provided in the (at least one) sealed cavity or cavities 30 relative to the surrounding atmosphere in order to effect, based on the reduced viscosity of the glass material of the cover substrate 20 and the overpressure in the sealed cavity 30 relative to the surrounding atmosphere, a defined bulging, e.g., blowing out or deformation, of the glass material of the cover substrate 20, starting from the sealed cavity 30 up to a stop surface 40-1 of a stop element 40 spaced apart from the cover substrate 20. According to one embodiment, the annealing step 130 may be carried out in a temperature range above 650°C, e.g.between 650°C and 955°C or between 650°C and 750°C.

[0179] According to an embodiment of the flow diagram 100-4 of the method 100, the step of tempering 130 and providing 140 an overpressure is carried out as a glass flow process in a vacuum furnace 50 in order to obtain a defined atmospheric overpressure in the closed cavity 30 compared to the surrounding atmosphere.

[0180] According to one embodiment of the flow diagram 100-4 of the method 100, the cover substrate 20 is bulged or blown out during the step of annealing 130 and providing 140 an overpressure in the region of the closed cavity 30 up to a height h which is predetermined by the vertical distance of the stop surface 40-1 of the stop 40 to the first main surface region 20-1 of the cover substrate 20.

[0181] According to one embodiment of the flow diagram 100-4 of the method 100, the region of the stop surface 40-1 of the stop element 40 opposite the cavity 30 or the cavity regions 30 is flat and parallel to the main surface region 20-1 of the cover substrate 20 (= parallel to the reference plane) in order to form a flat cover region 24-2 of the cover element 24 in the step of annealing 130 and providing 140 an overpressure.

[0182] According to one embodiment, the stop element 40 can be designed as a reusable tool and have a non-stick coating 42 (as or on the stop surface 40) for the glass material of the cover substrate 20 at least on the region 40-1 of the stop surface 40 opposite the cavity 30 or on the entire stop surface 40.

[0183] In a subsequent step 150, the reusable stop element 40 and the molded substrate 10 are removed from the molded cover substrate 20', whereby the molded cover substrate 20' now forms the lid substrate 20' with the at least one lid element 24. The lid substrate 20' can be used, for example, for housing one or a plurality of optical or optoelectronic components.

[0184] According to one embodiment, the flow diagram 100-4 of the method 100 may further comprise the step 142 of cooling the stop element 40, the mold substrate 10 and the molded cover substrate 20', wherein in step 150 (only) the mold substrate 10 is then removed by means of an etching process, e.g., a silicon or semiconductor etching process of the silicon or semiconductor material of the mold substrate.

[0185] In an (optional) subsequent step 160, the process flow 100-4 of the method 100 may further comprise applying or depositing a metallization 60 as a (continuous) frame structure or as a sealing frame on connection regions 62 on the second main surface region 20-2 on non-bulged regions (base regions) 24-3 of the lid elements 24 of the formed cover substrate (the lid substrate) 20'.

[0186] According to one embodiment, at step 160, an anti-reflective coating 64 may further be applied or deposited on an inside and / or outside region, e.g., inside and / or outside of the ceiling region 24-2 and / or sidewall region 24-1, of the lid element 24 of the molded cover substrate 20'.

[0187] In an (optional) subsequent step 170, the process sequence 100-4 of the method 100 may further include singulating the formed cover substrate 20' to obtain singulated cover elements 24'. The singulation 170 of the glass cover substrate 20' may be performed, for example, by sawing or laser separation. With the singulated caps 24', optical assemblies can be hermetically sealed at the individual substrate level or at the wafer level by individual encapsulation, as will be explained below.

[0188] In the following, some process steps of process flow 100-4 of method 100 of Fig. 5 summarized again.

[0189] Fig. 5100-4 shows a flowchart 100-4 illustrating a process sequence 100-4 for producing a cover substrate 20' based on steps 110 to 170. The cover substrate 20' resulting from the manufacturing method 100-4 has, for example, (at least) an optically passive side window 24-1 after the process sequence, which is an integral part of the cover element 24 (cap) and allows lateral beam coupling and / or beam extraction.

[0190] The process flow 100-4 of Fig. 5Thus, as a step 110, it comprises providing the mold substrate with a structured (depression-provided) surface region, wherein the mold substrate comprises a semiconductor material, such as silicon, or consists of the semiconductor material, e.g. silicon. This is followed by arranging the unstructured cover substrate on the structured surface region of the mold substrate. The cover substrate comprises a glass material or consists of a glass material. When arranging the cover substrate on the mold substrate, the structured surface of the mold substrate is arranged to at least partially overlap a surface of the cover substrate and, when connecting the cover substrate to the mold substrate, is e.g. anodically bonded or hermetically joined.

[0191] This is followed, for example, by annealing 130 the bonded substrates 10, 20 in a vacuum oven such that blowing out of the glass material of the cover substrate in the region of the recesses is caused by the enclosed pressure in relation to the oven pressure.

[0192] During the glass flow process, the flow front is stopped at the stop surface 42 (at the first main surface area 40-1) of the stop element 40 at an adjustable distance h in the vacuum furnace. The stop element 40 with the stop surface 42 comprises, for example, a silicon wafer or consists of a silicon wafer. The stop tool 40 or only the stop surface 42 of the stop tool 40 comprises or consists of a high-melting material, such as silicon, metal, ceramic, or glass ceramic with a glass-repellent protective layer, for example based on boron nitride, carbon, etc., in order to make the stop tool 40 or the stop surface 42 reusable.

[0193] According to one embodiment, a silicon wafer 40 can be coated with a glass-repellent layer 42 on the first main surface region 40-1 to obtain the stop surface 42. Thus, a semiconductor wafer 40 with a glass-repellent passivation layer 42 on a surface 40-1 can be provided.

[0194] For reusable stop elements or stop surfaces, a (selectable or complex) negative molding process can also be provided, for example, to transfer these high-quality shapes into the upper window of the cover element through the glass flow process. This allows for 100% shape transfer (from the stop surface to the upper window of the cover element) for (at least not too fine) structures. For example, flat lenses or holographic structures can be transferred from the stop surface to the upper window 24-2 of the cover element 24.

[0195] During the glass flow process 130, 140, the bonded substrates are cooled under a reproducible temperature and pressure ramp to create the concave window shape. Finally, the cover substrate 20', along with the mold substrate and, for example, the stop element 40, is removed from the furnace 50.

[0196] Then, the reusable stop element 40 and the mold substrate 10 are removed 150 to obtain the structured cover substrate 20' obtained from the cover substrate 20 by the blow-out process.

[0197] In summary, it can be stated that the Fig. 2 - 5 illustrate possible and optional sub-steps and process sequences of the method 100 for producing a cover substrate 20', as described in the Fig. 1 This was described in Fig. 2 - 5The substeps and process sequences illustrated are to be viewed only as examples and may vary in other embodiments. Possible process sequences are illustrated for how the production of the cover wafer 20', i.e., the cover substrate 20', with the vertical, convex or concave, optically passive window surfaces 24-1, 24-2 can proceed. The method 100 is essentially based on so-called glass flow techniques. In a preparatory step, a silicon wafer 40, i.e., a stop surface 40, is coated with a glass-repellent layer 42.

[0198] The special cover substrate 20' is, for example, a prerequisite for producing improved packaged radiation-emitting components 1' using the method 200 described below. The above substeps and process sequences are to be considered only as examples and may have variations in other embodiments. A possible process sequence is shown for how the production of these cover wafers, i.e., the cover substrates, with the window surfaces 24-1, 24-2 can proceed.

[0199] Fig. 6 now shows a further basic process flow 100-5 of the inventive manufacturing method 100 according to a further embodiment. The following essentially describes differences or different process steps of the flow diagram 100-5 of Fig. 6 compared to flowcharts 100-1, 100-2, 100-3, 100-4 of the Fig. 2 to 5 Therefore, the above description of the Fig. 1 to 5accordingly to the following description of the embodiment of Fig. 6 applied, whereby the following description focuses primarily on differences, such as different (= alternative and / or additional) process steps and / or elements, compared to the previous process sequences and the resulting technical effects.

[0200] In step 110, the mold substrate 10, e.g., a semiconductor or silicon wafer, is first provided with the structured surface region 10-1, i.e., the mold substrate 10 is provided with at least one depression or recess 12. Furthermore, the cover substrate 20, e.g., a glass wafer, is provided. The cover substrate 20 comprises a glass material.

[0201] In a step 112, the cover substrate 20 is arranged (aligned) on the structured surface region 10-1 of the mold substrate 10. In a step 114, the cover substrate 20 is then hermetically bonded to the mold substrate 10, e.g., by anodic bonding (e.g., in a defined atmosphere), to form at least one sealed cavity 30 or a plurality of sub-cavities 30 between the cover substrate 20 and the mold substrate 10. The (hermetic) bonding 114 of the cover substrate 20 to the mold substrate 10 can be performed in an atmosphere with a defined atmospheric ambient pressure in order to contain a defined atmospheric pressure in the sealed cavities 30.The cover substrate 20 and / or the mold substrate 10 are configured to form the closed cavity 30 with one or a plurality of closed cavity regions 30 between the cover substrate 20 and the mold substrate 10, wherein the closed cavity regions 30 are arranged fluidically separated from one another, or wherein gas exchange channels 30-1 can further be provided between the cavity regions 30 closed from the ambient atmosphere in order to fluidically connect them to one another in order to maintain a common defined atmospheric pressure in the connected cavity regions 30.

[0202] In step 120, the mold substrate 10 and the cover substrate 20, which are (firmly) connected to each other, are provided, wherein the surface region 10-1 of the mold substrate 10 is structured (formed with depressions or channel structures 12).

[0203] In the (subsequent) step 130, the cover substrate 20 and the mold substrate 10 are now tempered, i.e., subjected to a temperature treatment or heated (warmed), to reduce the viscosity of the glass material of the cover substrate 20. Furthermore, in a step 140, an overpressure is provided in the (at least one) sealed cavity or cavities 30 relative to the surrounding atmosphere to cause a defined bulging, e.g., blowing out or deformation, of the glass material of the cover substrate 20. By the defined bulging of the glass material of the cover substrate 20, a shaped cover substrate 20' with (at least) one cover element 24 is thus obtained, wherein the bulges or deformations, ie the blown-out regions, then form the side wall regions 24-1 and the base regions 24-3 of the resulting cover elements 24.

[0204] According to one embodiment of the flow diagram 100-5 of the method 100, the step of annealing 130 and providing 140 an overpressure is carried out as a glass flow process in a vacuum furnace 50 in order to obtain a defined atmospheric overpressure in the closed cavity 30 relative to the surrounding atmosphere. According to one embodiment of the flow diagram 100-5 of the method 100, the cover substrate 20 is bulged or blown out during the step of annealing 130 and providing 140 an overpressure in the region of the closed cavity 30 up to a height h, which is predetermined by the vertical distance of the stop surface 40-1 of the stop 40 from the first main surface region 20-1 of the cover substrate 20.

[0205] According to one embodiment of the flow diagram 100-5 of the method 100, the region of the stop surface 40-1 of the stop element 40 opposite the cavity 30 or the cavity regions 30 is flat and parallel to the main surface region 20-1 of the cover substrate 20 in order to form a flat base region 24-3 of the cover element 24 during the step of annealing 130 and providing 140 an overpressure. The glass flow process 130, 140 can therefore be carried out in a pressure-controlled furnace (e.g., in a vacuum furnace) 50. The glass wafer (cover substrate) 20 is blown out in the region of the cavities 30 up to the height h, which can be determined by a stop surface 40-1 of the stop element 40.

[0206] In the case of Fig. 6In the further process sequence 100-5 of the manufacturing method 100 shown, the frames (side wall regions 24-1 and base regions 24-3) of the cover elements 24 are blown out or blown out. This essentially results in an inversion of the glass cap (cavity facing upwards = z-direction). With this procedure, it can be ensured that the cover shape is not impaired by the glass flow process. The cover substrate 20 is anodically bonded to the mold substrate 10, and the circumferential channel structures or trench structures 12 in the mold substrate 10 are blown out, forming the cavity(ies) 30 with the distance h.

[0207] Fig. 2 - 6 illustrate possible and optional sub-steps and process sequences of the method 100 for producing a cover substrate 20', as described in the Fig. 1 This was described in Fig. 2 - 6The substeps and process sequences illustrated are to be viewed only as examples and may vary in other embodiments. Possible process sequences are illustrated for how the production of the cover wafer 20', i.e., the cover substrate 20', with the optically neutral window surfaces 24-1 can proceed. The method 100 is essentially based on so-called glass flow techniques. In a preparatory step, a silicon wafer 40, i.e., a stop surface 40-1, is coated with a glass-repellent layer.

[0208] The special cover substrate 20' is, for example, a prerequisite for producing improved packaged radiation-emitting components 1' using the method 200 described below. The above substeps and process sequences are to be considered only as examples and may have variations in other embodiments. A possible process sequence is shown for how the production of these cover wafers, i.e., the cover substrates, with the optical window surfaces 24-1 can proceed.

[0209] With regard to the above-mentioned Fig. 2-6The process sequences shown can thus be summarized as follows: in process sequences 100-1, 100-2, 100-3 and 100-4, when the glass material of the cover substrate is bulged (step 140), the side windows 24-1 and the cover regions 24-2 are bulged (blown out or deformed), while in process sequence 100-5, when the glass material of the cover substrate 20 is bulged, the side windows 24-1 and the base regions 24-3 are bulged to obtain the shaped cover substrate 20' with the cover elements 24'.

[0210] According to one embodiment of the method, in the step of annealing 130 and providing an overpressure 140, either the side windows 24-1 and the cover region 24-2 (in the processes 100-1, 100-2, 100-3, 100-4) or the side windows 24-1 and the base regions 24-3 (in the process 100-5) are bulged with the glass material of the cover substrate 20, starting from the closed cavity 30 up to the spaced-apart stop surface 40-1 of the stop element 40.

[0211] Fig. 7 now shows, for example, a schematic flow diagram of a method 200 according to the invention for producing a hermetically packaged, optical or optoelectronic component 1' according to a further embodiment.

[0212] Before the following embodiments are explained in more detail with reference to the drawings, it is pointed out again that identical, functionally equivalent or equivalent elements, objects, functional blocks and / or method steps in the different figures are provided with the same reference numerals, so that the description of these elements, objects, functional blocks and / or method steps shown in different embodiments is interchangeable or can be applied to one another.

[0213] In the method 200 for producing a hermetically packaged optical component, e.g., an optoelectronic transmitting and / or receiving component, the following steps are now performed. Thus, first, in step 210, the method 100 described above is performed with the exemplary process sequences 100-1, 100-2, 100-3, 100-4, 100-5 for producing a shaped cover substrate (= structured lid substrate) 20'. The shaped cover substrate 20' can have a single or isolated lid element 24' or can also have a plurality or a multiplicity of lid elements 24 (e.g., a lid wafer at the wafer level).

[0214] Furthermore, in step 220, a component substrate 2 with at least one optoelectronic component 1 (= transmitting and / or receiving component) arranged thereon is provided. According to one embodiment, a component substrate 2 can be provided with a single optoelectronic component 1 or as a component wafer 2 with a plurality of optoelectronic components 1 arranged thereon.

[0215] According to one embodiment, for example, step 210 of performing the method 100 can be performed at the wafer level, wherein a plurality of optical components 1 are arranged on the component substrate 2 (component wafer), and wherein the formed cover substrate 20' (cover wafer) has a plurality of cover elements 24. In this context, reference is also made, for example, to the Fig. 8 - 10 and the corresponding description.

[0216] According to one embodiment, step 230 of method 200 further comprises, for example, a step of connecting or hermetically connecting the component substrate 2 and the formed cover substrate 20' along an intermediate connecting region 60, 61, such as a bond frame. In this context, reference is also made, for example, to the Fig. 8 - 10 and the corresponding description.

[0217] According to an embodiment of the method 20, the connection region 60 on the second main surface region 20-2 has, for example, a metallization in order to form a frame structure, e.g. a continuous frame structure, on non-bulged regions 24-3 (= base regions) of the formed cover substrate 20', wherein the method 200 further comprises, for example, a step 230 of connecting the formed cover substrate 20' and the component substrate 2 by means of a bonding frame 60. The bonding frame 60 can, for example, have a metallic solder material 66. In this context, reference is also made, for example, to the Fig. 8 - 10 and the corresponding description.

[0218] According to one embodiment, step 230 of method 200 further comprises, for example, a step of connecting the component substrate 2 and the cover substrate 20' by means of laser direct welding, laser soldering, eutectic solder bonding, thermocompression bonding, glass frit bonding, reactive nano-metal layer soldering (RMS) or induction soldering along the connection region 62. In this context, reference is also made, for example, to the Fig. 8 - 10 and the corresponding description.

[0219] According to one embodiment, the method 200 further comprises, for example, the steps of singulating 170 the formed cover substrate 20' to obtain singulated cover elements 24', and (hermetically) connecting 230 the singulated cover element 24' to a component substrate 2 to obtain the packaged optical component 1'. In this context, reference is also made, for example, to the Fig. 8 - 10and the corresponding description.

[0220] According to one embodiment, the method 200 further comprises, for example, the steps of (hermetically) connecting 230 the formed cover substrate 20' with the plurality of cover elements 24 to the component substrate 2, which has a plurality of optoelectronic components 1, in order to obtain a plurality of packaged optical components 1' (at wafer level), and further the step of singulating 240 the plurality of packaged optical components 1' in order to obtain singulated, hermetically packaged optical components 1'. The step of singulating 240 can be carried out, for example, by sawing or by laser separation. In this context, reference is also made, for example, to the Fig. 8 - 10 and the corresponding description.

[0221] According to one embodiment, the method 200 further comprises, for example, the steps of singulating the shaped cover substrate 20' to obtain singulated cover elements 24', singulating the component substrate 2 to obtain singulated components 1 on the singulated component substrates 2', and (hermetically) connecting 230 each of the singulated cover element 24' to the singulated component 1 to obtain a packaged optical component 1'. In this context, reference is also made, for example, to the Fig. 8 - 10 and the corresponding description.

[0222] In the method 200 for producing a packaged radiation-emitting component 1, which can be carried out, for example, at wafer level, it is also provided according to one embodiment that the arrangement and hermetic bonding 230 of the substrates 2, 20', i.e., the component substrate 2 and the molded cover substrate 20', takes place under a predetermined atmosphere. This ensures that the housing 2, 20' or its interior volume (cavity) 32 is completely free of organic substances or water vapor, so that the lifetime of the optoelectronic components 1, such as light-emitting diodes or laser diodes, is not impaired.

[0223] The cavity 32 contains, for example, dry air (= reactive atmosphere), nitrogen, or another type of inert atmosphere. However, a negative pressure or even a complete vacuum can also be set in principle and, in addition, can be maintained for long periods by introducing special getter layers 4. A reduced atmospheric pressure (negative pressure) in the cavity 32 of approximately 100 Torr, 50 Torr, 5 Torr, or 1 Torr, or lower pressure values, can be considered a vacuum. The cavity 32 can also be hermetically sealed against the penetration of water vapor. In this context, reference is also made, for example, to the Fig. 8 - 10 and the corresponding description.

[0224] In some embodiments, the packaged optoelectronic (radiation-emitting or radiation-sensitive) component 1 is designed such that the component substrate 2 serves as a housing base and as a bearing surface for the radiation-emitting component 1, wherein the cover substrate 20' cooperates with the housing base 2 to hermetically seal the cavity 32 of the housing 5. In this context, reference is also made, for example, to the Fig. 8 - 10 and the corresponding description.

[0225] In some embodiments, the packaged radiation-emitting component 1' is designed such that the housing base 2 (component substrate) is formed as a base wafer comprising a plurality of housing base elements 2' and / or the cover substrate 20' is formed as a cover wafer comprising a plurality of cover elements 24. In this context, reference is also made, for example, to the Fig. 8 - 10 and the corresponding description.

[0226] In some embodiments, the packaged radiation-emitting component 1' is designed such that an intermediate carrier 6 for the radiation-emitting component 1 is arranged between the component substrate 2 and the radiation-emitting component 1, so that the component substrate 2 carries the radiation-emitting component 1 indirectly (via the intermediate carrier 6). In this context, reference is also made, for example, to the Fig. 8 - 10 and the corresponding description.

[0227] In some embodiments, the packaged radiation-emitting component 1' is designed such that the component substrate 2 and the cover substrate 20' are fastened to one another by means of a bonding frame 60, 61 comprising a metallic solder material 66. The bonding frame 60, 61 can bond the opposing metallizations 60, 61 to the cover substrate 20' (on the second main surface region 20-2) and the component substrate 2 (on the first main surface region 2-1) with the solder material 66 in between, which establishes a mechanical and electrical connection between the metallizations 60, 61. In this context, reference is also made, for example, to the Fig. 8 - 10 and the corresponding description.

[0228] In some embodiments, the packaged radiation-emitting component 1' is designed such that a conductor track 7 for electrically connecting the radiation-emitting component 1 is arranged on the side of the component substrate 2, and the conductor track 7 is led out of the cavity 32, e.g., laterally, between the cover substrate 20' and the component substrate 2. In this context, reference is also made, for example, to the Fig. 8 - 10 and the corresponding description.

[0229] In some embodiments, the packaged radiation-emitting component 1' is designed such that a conductor track 7 for electrically connecting the radiation-emitting component 1 is arranged on the component substrate 2, and the conductor track 7 is led downwards through the component substrate 2 out of the cavity 32. For this purpose, for example, a TSV and / or TGV arrangement 7-1 (Through silicon vias (TSV) or Through Glass Via (TGV)) can be used. In this context, reference is also made, for example, to the Fig. 8 - 10 and the corresponding description.

[0230] In some embodiments, the packaged radiation-emitting component 1' is designed such that an optical bench 8 with one or more additional optical elements 8-1, e.g. discrete lens elements, is arranged in front of the optical output coupling window (optical side window) 24-1 on the component substrate 2, so that the optical output coupling window 24-1 is arranged between the optical bench 8 with the additional optical element 8-1 and the radiation-emitting component 1. In this context, reference is also made, for example, to the Fig. 8 - 10 and the corresponding description.

[0231] In some embodiments, the packaged radiation-emitting component 1 is designed such that the optical bench 8 with the additional optical elements 8-1, e.g. lenses, prisms, mirrors, apertures, etc., is arranged on the component substrate 2 and is located in the radiation direction of the radiation-emitting component 2. In this context, reference is also made, for example, to the Fig. 8 - 10 and the corresponding description.

[0232] In some embodiments, the packaged radiation-emitting component 1 is designed such that it further comprises an element (conversion element) 9 which is effective for a light color conversion of the emitted light, so that the optical output coupling window 24-1 is arranged between the effective element 9 and the radiation-emitting component 1.

[0233] In some embodiments, the packaged radiation-emitting component 1 is designed such that the cavity 32 has a reactive atmosphere and / or the cavity 32 contains exclusively inorganic substances. The cavity 32 can also be hermetically sealed against the penetration of water vapor. This can ensure or at least support long-term operation of, for example, blue and green laser diodes.

[0234] In some embodiments, the packaged radiation-emitting component 1 is designed such that an electronic driver circuit 3 is arranged in the cavity. The electronic driver circuit 3 can, for example, be integrated into the component substrate 2.

[0235] In some embodiments, radiation-emitting components and photodetectors are located in the same cavities of the cover substrate.

[0236] In some embodiments, radiation-emitting components and photodetectors are located in adjacent cavities of the cover substrate, configured such that the component substrate forms a common housing base. According to embodiments, no optical decoupling between adjacent cavities is required. In some embodiments, the packaged optoelectronic component 1 comprises a detector element and an emitter element in a housing 5.

[0237] According to the above statements, the manufacturing method 200 for the hermetic packaging of an optoelectronic component 1 enables various embodiments and configurations of the resulting, hermetically packaged, optoelectronic component 1', for example: A packaging of individual laser diodes 1 (or generally individual optoelectronic components 1) on a submount 6 in a hermetically sealed housing 5, created by bonding a cover 20' with at least one lateral optically neutral window surface 24-1.

[0238] A capping of individual laser diodes 1 directly on the substrate 2 in a hermetically sealed housing 5, created by bonding a cover 20' with at least one lateral optically neutral window surface 24-1.

[0239] A packaging of individual laser diodes 1 and individual passive optical elements in a hermetically sealed housing 5, created by bonding a cover 20' with at least one lateral window surface 24-1.

[0240] A capping of one or more laser diodes 1 with "fast focus collimation" by a common cylindrical lens (top or side) within the hermetically sealed housing, optionally with one further lens each or a common multiple cylindrical lens 8 for slow axis collimation outside the hermetic housing 5.

[0241] A casing of one or more laser diodes 1 with beam collimation by individual collecting lenses within the hermetically sealed housing (top or side), optionally with one further lens each or a common multiple collecting lens 8 for further beam collimation outside the hermetic housing 5, optionally with an optical structure for beam superposition and optionally for static beam deflection.

[0242] A casing of one or more laser diodes 1 with beam collimation by individual collecting lenses within the hermetically sealed housing (top or side), optionally with one further lens each or a common multiple collecting lens 8 for further beam collimation outside the hermetic housing 5, optionally with an optical structure for beam superposition and optionally for static beam deflection.

[0243] A packaging of laser diodes on a submount with electronic driver circuitry within the hermetic housing.

[0244] A housing of one or more laser diodes 1 with or without a submount, with or without fast-axis collimation, and a light color conversion by an externally arranged phosphor body, which is fixed as a molded body or dispensed and cured as phosphor bound in a polymer (epoxy or silicone matrix). The optically active components arranged externally (= outside the housing 5) can be soldered or fixed by adhesive, because organic outgassing does not cause clouding in the beam exit.

[0245] A capping of at least one semiconductor-based light source 1 and at least one photodetector 1-2 in the hermetically sealed housing 5 created by bonding (= method 200) a glass cover 20' produced according to the aforementioned method 100, e.g. with an optically neutral window surface pointing away from the substrate 2.

[0246] The components 1 arranged in the cavity 32 and the encapsulation 20' itself can be joined, for example, by metallic joining methods such as soldering, eutectic AuSn soldering, etc., to avoid organic outgassing in the housing 5. Fluxes do not need to be used.

[0247] In the following, the Fig. 8 - 10 exemplary process sequences or process flows for the implementation of the Fig. 7 The basic manufacturing process 200 shown in FIG. Fig. 8 - 10 the drawing plane extends again parallel to the xz-plane.

[0248] All process alternatives to method 200 described below are based on the fundamental concept that first the shaped cover substrate 20', i.e., the structured lid substrate with one or a plurality of lid elements 24, is produced using the above method 100. Furthermore, a component substrate 2, on which one or a plurality of optoelectronic components 1 are arranged, is provided (step 220). In a step 230, the shaped cover substrate 20' and the component of the substrate 1 are connected to one another, e.g., hermetically connected / bonded, in order to hermetically package the optical component 1, i.e., to accommodate it in a housing that is hermetically sealed against the ambient atmosphere or environmental influences.A fluidically tight, mechanical connection (encapsulation) of the component substrate 2 and the molded cover substrate 20' is considered to be a hermetic or hermetically sealed housing.

[0249] Fig. 8 now shows a first exemplary basic flow diagram 200-1 of the inventive method 200 for producing a hermetically packaged optical component 1' according to a further embodiment. In particular, Fig. 8a sequence of the encapsulation process 200-1 with optically neutral side windows 24-1 at wafer level up to the wafer singulation according to an embodiment in a variant with the vertical lateral window surface 24-1, wherein the optically neutral coupling-out windows (side windows) 24-1 have a 90° orientation to the carrier substrate plane (xy plane), and wherein the radiation-emitting component 1 has, for example, a radiation direction or main radiation direction (in the case of a diverging or widening beam) substantially parallel to the carrier substrate plane (xy plane).

[0250] In the method 200 for producing a hermetically packaged optical component, e.g., an optoelectronic transmitting and / or receiving component, the following steps are now carried out. First, the method 100 described above is carried out with the exemplary process sequences 100-1, 100-2, 100-3, 100-4, 100-5 for producing a shaped cover substrate (= structured lid substrate) 20'. The shaped cover substrate 20' can have a plurality or multiplicity of lid elements 24. Furthermore, in step 220, a component substrate 2, e.g., as a component wafer, with a plurality of optoelectronic components 1 arranged thereon is provided. In this case, an optoelectronic component 1 can be assigned to each lid element 24.In the step of (hermetically) connecting 230 the shaped cover substrate 20' with the plurality of cover elements 24 to the component substrate 2, which in turn has a plurality of optoelectronic components 1, a plurality of packaged optical components 1' (at wafer level) is thus obtained.

[0251] The step of connecting the component substrate 2 and the formed cover substrate 20' can be performed, for example, along an intermediate connection region 60, such as a bond frame. The connection region 60 can have a metallization to form a frame structure, e.g., a continuous frame structure, on non-bulged regions 24-3 (= base regions) of the formed cover substrate 20'. The bond frame 60 can, for example, have a metallic solder material 66.

[0252] The step of connecting 230 the device substrate 2 and the cover substrate 20' may also be performed by means of laser direct welding, laser soldering, eutectic solder bonding, thermocompression bonding, glass frit bonding, reactive nano-metal layer soldering (RMS) or induction soldering along the connection region 60.

[0253] Furthermore, a dicing step 240 of the plurality of packaged optical components 1' is performed along a dicing line DL to obtain singulated, hermetically packaged optical components 1'. The dicing step 240 can be performed, for example, by sawing or laser separation.

[0254] The method 200 for producing a packaged radiation-emitting component 1 can, for example, be carried out at wafer level, wherein the arrangement and hermetic bonding 230 of the substrates 2, 20', i.e., the component substrate 2 and the molded cover substrate 20', takes place under the predetermined atmosphere. This ensures that the housing 2, 20' or its internal volume 32 is completely free of organic substances or water vapor, so that the lifetime of the optoelectronic components 1, such as light-emitting diodes or laser diodes, is not impaired. The cavity 32 contains, for example, dry air (= reactive atmosphere), nitrogen, or another type of inert atmosphere, but a negative pressure or even a complete vacuum can also be set in principle and, in addition, can be maintained over long periods of time by introducing special getter layers 4.A vacuum can be considered a reduced atmospheric pressure (negative pressure) in the cavity 32 of approximately 100 Torr, 50 Torr, 5 Torr, or 1 Torr, or lower. The cavity 32 can also be hermetically sealed against the ingress of water vapor.

[0255] Furthermore, an intermediate carrier 6 for the radiation-emitting component 1 can be arranged between the component substrate 2 and the radiation-emitting component 1, so that the component substrate 2 supports the radiation-emitting component 1 indirectly (= via the intermediate carrier 6). In the embodiments, the packaged radiation-emitting component 1' is designed such that a conductor track 7 for electrically connecting the radiation-emitting component 1 is arranged on the component substrate 2 side, and the conductor track 7 is led out of the cavity 32, e.g., laterally, and / or downwardly, between the cover substrate 20' and the component substrate 2. For this purpose, for example, a TSV and / or TGV arrangement 7-1 (through silicon vias (TSV) or through glass via (TGV)) can be used.

[0256] In the exemplary flow diagram 200-1 of the method 200 according to the invention for producing a hermetically packaged optical component 1' of Fig. 8 A sequence of a capping process with flat side windows at wafer level up to wafer separation is shown in an exemplary variant with a lens 11 positioned in the housing 5. During the capping process, one or more laser diodes with a Fast-focus collimation (fast focus collimation) by a common cylindrical lens (collimation lens) 11 within the hermetically sealed housing 5. This lens 11 is, for example, soldered to the component substrate 2 to prevent organic outgassing in the vicinity of the laser diode.

[0257] Fig. 8a and 8bnow show a further exemplary embodiment of the flow diagram 200-1 of the inventive method 200 for producing a hermetically packaged optical component 1' according to a further embodiment. In particular, Fig. 8a the use of a shaped cover substrate (= structured lid substrate) 20' with concave side windows 24-1 in the wafer-level encapsulation process 200. Fig. 8b shows the use of a molded cover substrate 20' with convex side windows 24-1, 24-2 in the wafer-level encapsulation process 200.

[0258] The above description of the process flow 200-1 with the sequence of the capping process 200-1 in Fig. 8 is equally and accordingly also on the use of concave side windows 24-1 in Fig. 8a (where the optical output window has a concave window geometry with 90° alignment to the carrier substrate plane) and convex side windows 24-1 in Fig. 8b (where the optical output window has a convex window geometry with 90° alignment to the carrier substrate plane).

[0259] This also applies to the following description of further process sequences 200 with the sequence of the capping process 200-#, ie the description is equally and accordingly also applicable to the use of flat vertical, concave or convex side windows 24-1.

[0260] Fig. 9 now shows a further exemplary basic flow diagram 200-2 of the inventive method 200 for producing a hermetically packaged optical component 1' according to a further embodiment. In particular, Fig. 9 a sequence of the encapsulation process 200-2 with optically neutral side windows 24-1 at wafer level up to the wafer singulation according to an embodiment in a variant in which the radiation-emitting component 1 has, for example, a radiation direction or main radiation direction (in the case of an expanding beam) substantially parallel to the carrier substrate plane (xy plane).

[0261] Fig. 9 shows a sequence of a capping process with convex side windows at the wafer level up to wafer singulation. The description is also applicable to the use of flat, vertical, or concave side windows 24-1. The carrier substrate 2 is equipped with an optical bench 8-1. Lenses 11 are mounted within the hermetic housing 5, for example, by soldering, and additional optical elements 8-1 are mounted on an open optical bench 8, for example, by adhesive.

[0262] In the method 200 for producing a hermetically packaged optical component, e.g., an optoelectronic transmitting and / or receiving component, the following steps are now performed. First, the method 100 described above is performed with the exemplary process sequences 100-1 ... 100-5 for producing a shaped cover substrate (= structured lid substrate) 20'. The shaped cover substrate 20' can have a plurality or multiplicity of lid elements 24. Furthermore, in step 220, a component substrate 2, e.g., as a component wafer, with a plurality of optoelectronic components 1 arranged thereon is provided. In this case, an optoelectronic component 1 can be assigned to each lid element 24.In the step of (hermetically) connecting 230 the shaped cover substrate 20' with the plurality of cover elements 24 to the component substrate 2, which in turn has a plurality of optoelectronic components 1, a plurality of packaged optical components 1' (at wafer level) is thus obtained (= . Fig. 9a ).

[0263] Furthermore, a step of singulating 240 the plurality of packaged optical components 1' is performed to obtain singulated, hermetically packaged optical components 1'. The singulating step 240 can be performed, for example, by sawing or laser separation.

[0264] In the step of separating 240, as in Fig. 9b is shown, an intermediate region 20'-1 of the cover substrate 20' is separated, for example by sawing or laser separation on the separation line DL and at Fig. 9c removed from the arrangement. When arranging Fig. 9c Thus, the optoelectronic components 1 are each individually hermetically housed on the component substrate 2 with a cover element 24'.

[0265] As in Fig. 9d-f As shown by way of example, the step of singulating 240 the plurality of packaged optoelectronic components 1' can be divided into different sub-process sequences. According to one embodiment, the packaged radiation-emitting component 1' can now be designed such that an optical bench 8 with the additional optical element 8-1 is arranged upstream of the optically neutral output window (optical side window) 24-1 on the component substrate 2, so that the optically neutral output window 24-1 is arranged between the optical bench 8 and the radiation-emitting component (optoelectronic component) 1. 1. Alternative - Process sequence according to Fig. 9a - b - c - d - f : As in Fig. 9d As shown by way of example, the packaged optoelectronic components 1' can be separated in order to obtain the separated, hermetically packaged optoelectronic components 1'. According to the first alternative, (at least) one optical bench 8 is arranged on the separated component substrates 2' in front of the output window 24-1, ie outside the housing 5 with the radiation-emitting component (optoelectronic component) 1. Thus, the Fig. 9f The arrangement of the individual, hermetically packaged optical components 1' with the upstream optical bench 8 on the component substrate 8 is obtained. 2. Alternative - Process sequence according to Fig. 9a - b - c - e - f : As in Fig. 9c As shown by way of example, the individually packaged optoelectronic components 1' are obtained on the common component substrate 2. According to the second alternative, (at least) one optical bench 8 with the additional optical element 8-1 is arranged on the component substrate 2 in front of the output window 24-1, ie outside the housing 5 with the radiation-emitting component (optoelectronic component) 1, as shown in Fig. 9e As shown in Fig. 9f As shown by way of example, the packaged optoelectronic components 1' are now separated to obtain the separated, hermetically packaged optoelectronic components 1'. Thus, the Fig. 9f illustrated arrangement of the isolated, hermetically packaged optical components 1' with the upstream optical bench 8 with the additional optical element 8-1 on the component substrate 8.

[0266] The Fig. 9a-f show a sequence of a capping process with optically neutral side windows 24-1 at wafer level up to wafer separation. The carrier substrate 2 is equipped with an optical bench 8 with the additional optical element 8-1. Joining processes with high temperature requirements are first performed on the carrier substrate. Capping is carried out at wafer level with a glass cap wafer. The standard procedure is carried out from Fig. 9a-c , whereby a branching of the process sequence by substrate separation in Fig. 9a-b-c-e-f (1st alternative) or Fig. 9a-b-cd-f (2nd alternative). Here, the process flow branches: The sequence abcdf shows the optics assembly on the optical bench 8 in the case of upstream wafer singulation, while the sequence abcef shows the optics assembly on the optical bench 8 in the case of downstream wafer singulation. In addition to the semiconductor emitters 1, monitor diodes for monitoring the laser power, lenses, or other optical elements are optionally mounted within the hermetic housing 5, e.g., soldered on. This also applies if the caps are applied individually but are all hermetically joined to the carrier substrate together in a single joining process step.

[0267] The optical functions required for beam collimation and beam combination can be integrated or arranged on an open, connected optical bench 8 outside the hermetic housing 5.

[0268] Fig. 9f thus shows a distributed arrangement of the optical elements 8, 11, with some of the optical functions being constructed within the hermetically sealed housing 5 as the lens elements 11. For this purpose, organic-free joining techniques based on soft solder are preferably used. Other necessary optical elements 8-1 are constructed on the connected optical bench 8.

[0269] Fig. 9a-f further shows, by way of example, an embodiment in which the component substrate 2, in this case, for example, a silicon carrier chip, was lowered in the region of the optics 8 (optical bench) by etching by a lowering height "Δz" in order to thereby create more vertical installation space for the optics 8. The optics 8 can be arranged as the optical bench 8 on the component substrate 2 by means of adhesive bonds. As shown in Fig. 9f As shown, the plane of the optical bench 8 is located on a different, (vertically) lower height plane than the mounting plane for the laser diodes 1 or the sealing frame 3 (= 60, 61, 66).

[0270] According to further embodiments, the plane of the optical bench 8 with the additional optical element 8-1 can also be located on a different, vertically higher height plane than the mounting plane for the laser diodes 1 or the sealing frame 3. A raised mounting plane can also be formed in the carrier wafer (e.g., as a mesa structure).

[0271] In the capping process of Fig. 9 can (according to Fig. 8 and 8a-b ) a shaped cover substrate (= structured lid substrate) 20' or a shaped cover substrate 20' with concave or flat, vertical side windows 24-1 can be used.

[0272] Fig. 9a-f show how the optical functions required for beam collimation and beam combination are fundamentally integrated on an open, connected optical bench outside the hermetic housing.

[0273] Fig. 10 now shows a further exemplary basic flow diagram 200-3 of the inventive method 200 for producing a hermetically packaged optical component 1' according to a further embodiment. In particular, Fig. 10 a sequence of the encapsulation process 200-3 with optically neutral side windows 24-1 at wafer level up to the wafer singulation according to an embodiment, wherein the optically neutral coupling-out windows (side windows) 24-1 have, for example, a 90° (vertical) alignment to the carrier substrate plane (xy plane), and wherein the radiation-emitting component 1 has, for example, a radiation direction or main radiation direction (in the case of a diverging beam) substantially parallel to the carrier substrate plane (xy plane).

[0274] Fig. 10 shows a sequence of a capping process with convex side windows at the wafer level up to wafer separation. The carrier substrate 2 is equipped with an optical bench 8-1. Lenses 11 are soldered within the hermetic housing, for example, and additional optical elements 8-1 are mounted on the open optical bench 8, for example, using adhesive.

[0275] In the method 200 with the flow diagram 200-3 for producing a hermetically packaged optical component, e.g., an optoelectronic transmitting and / or receiving component, the following steps are now carried out. Thus, first, the method 100 described above with the exemplary process sequences 100-1 ... 100-5 for producing a shaped cover substrate (= structured lid substrate) 20' is carried out, wherein the shaped cover substrate 20' is singulated to obtain singulated lid elements 24' and to provide them for the subsequent bonding step. Thus, the shaped cover substrate 20' can each have a singulated lid element 24'. Furthermore, in step 220, a component substrate 2, e.g., as a component wafer, with a plurality of optoelectronic components 1 arranged thereon is provided.In this case, a single cover element 24' can be assigned to each optoelectronic component 1 on the component substrate 2 (component wafer). In the (hermetic) bonding step 230, the single cover elements 24' of the formed cover substrate 20' are bonded to the component substrate 2, which has a plurality of optoelectronic components 1, in order to hermetically package the optoelectronic components and thus obtain a plurality of packaged optical components 1' on the component substrate 2.

[0276] Furthermore, a step of singulating 240 of the plurality of packaged optical components 1' is performed to obtain singulated, hermetically packaged optical components 1'. The singulating step 240 can be performed, for example, along the singulation line DL by sawing or by laser separation.

[0277] In process flow 200-3 of Fig. 10 Thus, the optoelectronic components 1 are individually capped with the individual cover elements 24', whereby, compared to the process sequence 200-4, Fig. 9 a removal of a central portion 20'-1 of the lid substrate 20' is not required. As with Fig. 10c As shown by way of example, the individually housed optoelectronic components 1' are obtained on the common component substrate 2.

[0278] As in Fig. 10d-f As shown by way of example, the step of singulating 240 the plurality of packaged optoelectronic components 1' can be divided into different sub-process sequences. According to one exemplary embodiment, the packaged radiation-emitting component 1' can now be designed such that an optical bench 8 with the additional optical element 8-1 is arranged upstream of the optical output window (optical side window) 24-1 on the component substrate 2, so that the optical output window 24-1 is arranged between the optical bench 8 and the radiation-emitting component (optoelectronic component) 1.

[0279] The above description of the process flow 200-2 with regard to Figures 8d-f is the same with the different alternatives and accordingly also the process flow 200-3 in the Figuren 10d-f applicable.

[0280] The Fig. 10a-f shows a sequence of a capping process with optically neutral side windows 24-1 at wafer level up to wafer separation. The carrier substrate 2 is equipped with an optical bench 8. Joining processes with high temperature requirements are first performed on the carrier substrate. Capping is carried out at wafer level using individual glass caps. The standard procedure is carried out from Fig. 10a-c , whereby a branching of the process sequence by substrate separation in Fig. 10a-b-c-e-f (1st alternative) or Fig. 10a-b-c-d-f (2nd alternative). Here, the process flow branches: The sequence abcdf shows the optics assembly on the optical bench 8 in the case of upstream wafer singulation, while the sequence abcef shows the optics assembly on the optical bench 8 in the case of downstream wafer singulation. Optionally, in addition to the semiconductor emitters 1, monitor diodes 1-2 for monitoring the laser power, lenses 11, or other optical elements are mounted within the hermetic housing 24' (= 5), e.g., soldered on. Additional optical elements 8-1 are mounted on the open optical bench using adhesive. This also applies if the caps are applied individually, but are all hermetically joined to the carrier substrate together in one joining process step.

[0281] In the capping process of Fig. 10 Cover elements 24' with convex side windows 24- can be used. Likewise, cover elements 24` with concave or flat side windows 24-1 can also be used.

[0282] Fig. 10a-f show a distributed arrangement of optical elements, with some of the optical functions installed within the hermetically sealed housing under the glass cover. For this purpose, organic-free joining techniques based on soft solder are used, for example. Other necessary optical elements are mounted on the connected optical bench.

[0283] Embodiments thus describe a method 200 for the hermetically sealed packaging of radiation-emitting and radiation-detecting components 1, for example laser diodes or LEDs and PIN diodes, APD, SPAD, silicon photomultiplier, which can be referred to as WLP-IVA (wafer level packages - with integrated vertical optical apertures). The optical window region 24-1, which allows beam coupling from lateral to vertical to the carrier substrate 2', can be particularly advantageous. Window regions with a reflective mirror coating 65, within the meaning of the present description, are flat and curved surfaces inclined to the ground plane of the cover substrate 20'. Lenses 8, 11 within the meaning of the present description are passively imaging elements, e.g., uniaxial cylindrical lenses, rotationally symmetrical converging lenses, and freeform lenses.

[0284] The assembly of the laser diodes 1 and, if applicable, further optical elements and photodetectors 1-2 can be carried out, for example, on a semiconductor wafer as a substrate, for example a silicon wafer, and the encapsulation process can be carried out for all components mounted up to this step on the substrate together by bonding a cover substrate with window areas, usually with a similar arrangement. If additional optical elements 8-1 are to be mounted on an optical bench 8, this step preferably takes place after separating the cover substrate, whereby the areas of the optical bench become freely accessible for assembly. For reasons of system technology, increasing yield, and also to keep heat input low, individual encapsulation can be realized by placing and sealing individual (pre-measured) glass covers.The optical bench 8 thus remains exposed and can be directly populated with additional optical elements 8-1. Only then, for both process variants, does the carrier substrate undergo separation or singulation into individual chips, or more precisely, individual components.

[0285] Alternatively, the laser diodes can be mounted on a single piece of an already singulated semiconductor wafer, referred to here as a single substrate, for example a sawn-out chip from a carrier wafer, and the encapsulation process for the mounted components on the single substrate can be carried out by bonding a glass cover with at least one optical window that has already been singulated from a cover substrate.

[0286] According to one embodiment, a hermetically packaged optical component 1' manufactured using the present manufacturing method 100, 200 comprises an optical component 1 arranged on the component substrate 2', and a molded cover substrate 20' providing a hermetically sealed cover for the optical component 1, within which the optical component 1 is packaged, wherein the molded cover substrate 20' has a cover element 24' with a (laterally flat, inwardly curved or outwardly curved) sidewall region 24-1 between a base region 24-3 and a ceiling region 24-2.

[0287] According to one embodiment of the hermetically packaged optical component 1', the side wall region 24-1 and / or the ceiling region 24-2 of the cover element 24' of the molded cover substrate 20 comprises a material that is permeable to the transmitting or receiving radiation of the optical component 1, and is provided for coupling in and / or out electromagnetic radiation.

[0288] According to one embodiment of the hermetically packaged optical component 1', the hermetically sealed cover 2', 24' (with the cavity 32) has a reactive atmosphere and / or the cavity 32 contains exclusively inorganic substances, und / oder wherein the hermetically sealed cover 2`, 24` (cavity 32) is hermetically sealed against the penetration of water vapor.

[0289] The packaged optoelectronic component 1' can accordingly be created according to the method 200 for producing a packaged optoelectronic component 1' at wafer level with the following steps: producing a cover substrate, providing a component substrate in the form of a wafer with a multiplicity of radiation-emitting components, arranging the substrates on top of one another such that the substrates are connected along an intermediate connecting frame, and singulating the packaged radiation-emitting components.

[0290] Accordingly, exemplary embodiments of the present invention describe a method and a connection technology for the hermetically sealed packaging of radiation-emitting and / or radiation-receiving components 1, for example laser diodes or LEDs, which can be referred to as WLP-IVA (wafer level packages - with integrated vertical optical apertures). The optical (optically neutral) window region 24-1 can be particularly advantageous and, for example, also allows a beam to be coupled out lateral to the carrier substrate 2'. The optical window region 24-1 is characterized in the sense of the invention by a slight influence on the beam propagation, so that any divergence additionally impressed on the beam as it passes through the window 24-1 is in the range of less than + / - 0.5 ° or less than + / - 1.0 °.

[0291] The beam aberration through window 24-1 does not result in a shift in the focus position as the only error, although this resulting error currently contributes the largest portion of the error. However, the other errors that occur also scale with the refractive power of the window, so that a sufficiently thin window becomes (approximately) error-free. Another (important) fact, however, is that the inner and outer surfaces of window 24-1 become increasingly identical as the starting material for the window 24-1 becomes thinner.

[0292] For this purpose, the cover substrate 20 can have a thickness of 100 µm to 1500 µm or 300 µm to 800 µm, in order to achieve a thickness of the window elements 24-1, ie, the areas of the window elements 24-1 effective for light transmission, of 20 µm to 1200 µm or 20 µm to 300 µm. A window thickness of 20 µm to 300 µm is provided, for example, for optical transmission windows 24-1.

[0293] Aberrations are deviations from the ideal optical image produced by an optical system that result in a blurred or distorted image. As long as aberrations cause a wavefront deformation of less than 100 nm or less than 150 nm (RMS = root-mean-square standard deviation) (the sum of all aberrations), they can be considered negligible.

[0294] The assembly of the optoelectronic component 1, e.g., laser diodes, and possibly other optical elements can be carried out, for example, on a semiconductor wafer 2' as a substrate, for example, a silicon wafer, and the encapsulation process can be carried out for all mounted components on the substrate together by bonding a (common) cover substrate 20' with window regions 24-1. Only then does the separation or singulation into individual chips, more precisely into individual packages, take place.

[0295] According to one embodiment, a wafer arrangement having a plurality of housed radiation-emitting components with the following features is provided: a component substrate in the form of a wafer, which is designed as a common component substrate for the radiation-emitting components arranged thereon, and a common cover substrate, which has the cover substrates for the radiation-emitting components, wherein the substrates are arranged one next to the other such that the cover substrate and the component substrate are connected along an intermediate bond frame.

[0296] Alternatively, the assembly of the optoelectronic component 1, e.g., laser diodes, can be carried out on a single piece of an already singulated semiconductor wafer, referred to here as a single substrate, for example, a sawn-out chip 2' from a silicon wafer, and the encapsulation process for the assembled components on the single substrate can be carried out by bonding a glass cover with an optical window that has already been singulated from a cover substrate.

[0297] Fig. 11a-b now show a further exemplary embodiment of a hermetically packaged optoelectronic component 1' according to an embodiment, which is produced, for example, using the method 200 described above.

[0298] As in Fig. 11a-b As shown by way of example, the hermetically packaged optoelectronic component 1', which is produced, for example, using the manufacturing method 200, has an optical component 1 arranged on the singulated component substrate 2', and furthermore a shaped cover substrate 20' or singulated lid element 24', which provides a hermetically sealed cover or housing for the optical component 1. The optical component 1 is housed within the housing. The shaped cover substrate 20' can have a (curved) lid element 24' with a (vertically planar, inwardly or outwardly) curved sidewall region 24-1 between a ceiling region 24-2 and a base region 24-3. In Fig. 11a-b an outwardly curved (convex) side wall region 24-1 is shown.

[0299] According to one embodiment, the side wall region 24-1 and / or the ceiling region 24-2 of the cover element 24' of the molded cover substrate 20' comprises a material that is permeable to the transmitting or receiving radiation of the optoelectronic component 1 and is provided for coupling in and / or out of electromagnetic radiation (the transmitting or receiving radiation).

[0300] According to one embodiment, the hermetically sealed cover 24' with the cavity 32 has a reactive atmosphere and / or the cavity 32 contains exclusively inorganic substances. According to one embodiment, the hermetically sealed cover 24' with the cavity 32 is hermetically sealed against the penetration of water vapor. Fig. 11a-b In the embodiment shown, a hermetically sealed area is produced with sealing, for example, on a height level, wherein a variant with optical bench 8 with the additional optical element 8-1 at the surface level of the carrier wafer 2' is shown as an example.

[0301] Fig. 11a-b show an embodiment in which, by way of example, a lowered optical bench 8 is arranged on the singulated component substrate 2' for mounting passive optical components 8, 26. The plane of the optical bench 8 with the additional optical element 8-1 can be at a different height than the mounting plane for the components 1, such as laser diodes, or the sealing frame. The component substrate can be lowered in the region of the optics 8 (optical bench), e.g., by etching, by a lowering height "Δz". A raised mounting plane can also be formed in the carrier wafer 2', e.g., in the form of a mesa structure.

[0302] For example, no adhesives are used inside the glass cover 24'. Outside, lenses, prisms, mirrors, apertures, etc., e.g., as part of the optical bench, are preferably assembled with UV adhesive. Multiple optical elements 8-1 (lenses, prisms, mirrors, apertures, etc.) can also be on the same optical bench 8.

[0303] This arrangement with lateral vias 7-2 can be used for one or more components 1, e.g., laser diodes, and can be arranged to produce beams L 1 that are parallel to the axis or intersect at a point. In addition, the active components 1 can also be electrically contacted using flip-chip technology.

[0304] The arrangement is obtained by assembly, capping, and singulation at the wafer level. Optical bench on the same substrate for mounting passive optical components. The plane of the optical bench can be at a different height than the mounting plane for the laser diodes or the sealing frame. No adhesives are used inside the glass lid. Outside, lenses, prisms, mirrors, apertures, etc. are assembled, preferably / for example, with UV adhesive. Of course, several optical elements can be mounted on the same optical bench. This arrangement can be used for one or more laser diodes, arranged to produce beams parallel to the axis or beams that intersect at a point.

[0305] Fig. 11b shows, for example, an embodiment in which a hermetically packaged optoelectronic component 1' is produced from individual carrier substrates 2' and individual glass caps 24' at the individual substrate level.

[0306] Fig. 11a-b Thus, they show an embodiment in which the component substrate 2', e.g., a silicon carrier chip, has been lowered by etching in the area of ​​the optics 8-1, thereby creating more vertical installation space for the optics 8-1. The optics 8-1 are arranged on the optical bench 8, for example, by means of adhesive bonds.

[0307] Fig. 11a-b show a further embodiment in which additional electronic components can also be integrated into the laser housing, i.e., into the cavity 32, which is advantageous for some applications. Specifically, these can be, for example, (at least) an additional photodiode 1-2 for monitoring the power of the radiation-emitting component 1, for example, a laser, or driver circuits 25 for the radiation-emitting components 1. Fig. 11a-b a driver IC 25 and such a monitor photodiode 1-2 are shown in the cavity. Fig. 11a-b thus show an embodiment in which an electronic driver circuit 25 is arranged in the cavity 32.

[0308] In the following description of further embodiments of the hermetically packaged, optoelectronic component 1', the respective differences (= alternative and / or additional elements) compared to the arrangement of Fig. 11a-b and the resulting technical effects are described. Therefore, the above description of the Fig. 11a-b can also be applied accordingly to the following description of the further embodiments.

[0309] Further exemplary embodiments for a hermetically packaged optoelectronic component 1', which is produced, for example, using a method 200 described above, will now be described below.

[0310] In the following description of the exemplary embodiments of the hermetically packaged optoelectronic component, differences (= alternative and / or additional elements) compared to the other arrangements are essentially presented and the resulting technical effects are described. Therefore, the description of one exemplary embodiment of the hermetically packaged optoelectronic component can also be applied accordingly to the description of the other exemplary embodiments.

[0311] Fig. 12 shows an embodiment in which, for example, a lateral beam coupling of the optoelectronic component 1, e.g., a laser diode, takes place into a phosphor converter 27 to generate a different light color and resolve the laser coherence. If the lasers 1 are constructed so that they radiate upwards, the phosphor converter would be applied as an upwardly covering layer, and the outer housing 24' would be correspondingly equipped with an upper window opening 24-2.

[0312] Fig. 12 shows an embodiment with a light conversion element (conversion medium) 27, which can be mounted in the cavity 32 formed by the cover substrate 24' and the component substrate 2' when using a short-wave laser diode as a radiation-emitting (optoelectronic) component 1. The conversion medium 27 can, for example, be applied outside the hermetically sealed laser housing 2', 24' as an additional epoxy resin containing corresponding phosphors. The housed radiation-emitting component 1' according to Fig. 12 is thus designed such that it has an element 27 effective for a light color conversion of the emitted light L1, so that the optical output window 24-1 is arranged between the effective element 27 and the radiation-emitting component 1.

[0313] As in Fig. 12 As further illustrated by way of example, an outer cap or housing 28 can be provided for the hermetically packaged optoelectronic component 1', wherein the housing 28 is arranged on the substrate 2' and surrounds the hermetically packaged optoelectronic component 1' and, except for an optical exit window 28-1, the light conversion element 27. The outer cap 28 is provided, for example, to provide further protection and / or hermetic shielding of the entire hermetically packaged optoelectronic component 1' from the environment.

[0314] Fig. 13 now shows a further exemplary embodiment for a hermetically packaged optoelectronic component 1' according to an embodiment, wherein the arrangement 1' has a first lens 11 within the hermetically sealed region 32.

[0315] This lens 11 is soldered, for example, to prevent organic outgassing in the vicinity of the optoelectronic component 1, e.g., a laser diode. The carrier substrate 2' has hermetic lateral feedthroughs 7-2, which can be used, for example, for laser contacting via wire bonds or flip-chip connection techniques.

[0316] The packaged radiation-emitting component 1' is thus, as shown in the Fig. 13 is illustrated, is designed such that an optical bench 8 is arranged upstream of the optical output window 24-1 on the component substrate 2', so that the optical output window 24-1 is arranged between the optical bench 8 and the radiation-emitting component 1. In the embodiments shown, the housed radiation-emitting component 1' is designed such that the optical bench 8 is arranged on the component substrate 2' and is located in the emission direction of the radiation-emitting component 1.

[0317] Fig. 14 now shows a further exemplary embodiment of a hermetically packaged, optoelectronic component 1' according to an embodiment, wherein the packaged radiation-emitting component 1' is designed such that a conductor track 7 for electrically connecting the radiation-emitting component 1 is arranged on the side of the component substrate 2, and the conductor track 7 is led downwards through the component substrate 2 out of the cavity 30. For this purpose, for example, a TSV and / or TGV arrangement 7-1 (through silicon vias (TSV) or through glass via (TGV)) can be used. This arrangement can be used both for laser contacting through wire ribbons and through flip-chip connection techniques.

[0318] Fig. 15 now shows a further exemplary embodiment for a hermetically packaged, optoelectronic component 1' according to an embodiment, wherein the upper side wall 24-2 of the cover element 24' has a material that is permeable to the transmitting or receiving radiation of the optical component 1 and is provided for coupling in and / or out electromagnetic radiation L1.

[0319] The upper window surface 24-2 (ceiling window) is therefore provided for coupling and / or decoupling, wherein the radiation-emitting component 1 has, for example, a radiation direction or main radiation direction (in the case of a diverging beam) with the coupled-out light beam L 1 substantially perpendicular to the carrier substrate plane (xy plane). Fig. 15 the glass caps 24' (independent of the geometry of the side windows 24-1) also enable the optical coupling or coupling upwards or away from the carrier substrate 2` (e.g. vertically).

[0320] Fig. 15 shows a device 1' based on a carrier substrate with hermetic, electrical feedthroughs 7-2 through the substrate 2' (through silicon vias TSV). The contact surfaces 7 on the underside of the carrier substrate 2' enable further processing as an SMD component. Several laser diodes 1 can be constructed in parallel adjacent to one another beneath a glass cap. The glass caps 24' also enable (regardless of the side window geometry) optical coupling or coupling upwards or away from the carrier substrate 2'.

[0321] According to Fig. 14 and 15An embodiment with an advantageous configuration of the electrical contact 7, 7-2 is shown. For a particularly compact construction of the laser diode housing 2`, 24', i.e. of the housed optoelectronic component 1', the electrical connections can be led through the component substrate 2' in the form of vertical feedthroughs 7-2. On the rear side, the necessary connection pads 7 can be provided, as shown in the Fig. 14 and 15 shown, be provided with a solderable metallization. If these connection areas 7 are designed to be particularly surface-intensive, these areas are also suitable for ensuring the heat dissipation of the housing. Otherwise, in the embodiment according to Fig. 14 and 15The cover substrate 20', i.e., the glass cover 24', and the component substrate 2', in this case, for example, a silicon chip, are again connected to one another by means of a bonding frame 3, thus providing a hermetic cavity 3 for the optoelectronic component 1, in this case, for example, a laser diode. The optical surfaces, for example, are again provided with an anti-reflective coating 64 (ARC = Anti-Reflex Coating).

[0322] Fig. 16 now shows a further exemplary embodiment of a hermetically packaged, optoelectronic component 1' according to an embodiment, which is manufactured, for example, using a method 200 described above. According to an embodiment of the hermetically packaged, optoelectronic component 1', the cover substrate 20' can optionally be formed such that the upper side wall 24-2 of the cover element 24' comprises a material permeable to the transmitted or received radiation of the optical component 1 and is provided for coupling in and / or out electromagnetic radiation L1.

[0323] The packaged optoelectronic component 1' comprises, for example, a radiation-emitting semiconductor component 1, such as an optoelectronic transmitting component, and a radiation-sensitive semiconductor component 1-2, such as an optoelectronic receiving component or a photodiode. The radiation-emitting component 1A has, for example, a radiation direction or main radiation direction (in the case of a diverging beam) with the decoupled light beam L 1 pointing away from the carrier substrate plane (xy plane).

[0324] Fig. 16 thus shows an embodiment in which additional electronic components are integrated into the housing 24' for the laser 1, i.e., into the cavity 32. This is suitable for applications when, for example, one or more additional photodiodes 1-2 are to be provided to monitor the power of the radiation-emitting component 1, for example, the laser 1, or the driver circuits for the radiation-emitting components 1. The radiation reflected by the object 70 can be detected by the receiving element 1-2. The optical surfaces of the window element 24-2, for example, are again provided with an anti-reflection coating 64 (ARC = Anti-Reflex Coating).

[0325] In the Fig. 16 The driver IC 25 with the transmitting element 1 and the monitor photodiode 1-2 are shown in the cavity 32. In the Fig. 16 In the embodiment shown, the electronic driver circuit 25 is arranged as part of the transmitting element 1 in the cavity 32 of the cover element 24'.

[0326] Fig. 16 thus shows a "top-looking" arrangement 1', e.g., for a proximity sensor with emission and reception of reflected radiation L1 at an object 70 through the upper glass surface 24-2 (possibly with coating layers 64). The side walls 24-1 of the cap 24 are part of the housing but are not used for an optical function. The component 1' can be manufactured using one of the presented capping processes.

[0327] The Fig. 11 -16show embodiments in which several optoelectronic (e.g. radiation-emitting) components can be formed in the same housing. This is an example of an embodiment for the assembly of several laser diodes in one housing, e.g. an RGB laser source. The three radiation-emitting components 1, for example, are each mechanically connected to the component substrate 2' via intermediate carriers. This achieves favorable heat dissipation. The radiation-emitting components 1 are each electrically connected by means of conductor tracks 7 and lateral feedthroughs 7-2, which are led out of the cavity 30 through a hermetically sealed bonding frame. It can be advantageous to place the respective optical components for beam processing outside the hermetically sealed housing 5 and in front of the optical window, i.e. the optical surfaces. These optical components can be, for example, cylindrical lenses or other types of lenses.Then these optical components can also include substances that are undesirable in the hermetically sealed cavity, such as organic substances.

[0328] Although some aspects of the present disclosure have been described as features in the context of an apparatus, it is to be understood that such a description may also be considered a description of corresponding method features. Although some aspects have been described as features in the context of a method, it is to be understood that such a description may also be considered a description of corresponding features of an apparatus or the functionality of an apparatus. Some or all of the method steps may be performed by (or using) a hardware apparatus, such as a microprocessor, a programmable computer, or electronic circuitry. In some embodiments, some or more of the method steps may be performed by such an apparatus.Depending on particular implementation requirements, embodiments of the invention may be implemented in hardware or in software, or at least partially in hardware or at least partially in software.

[0329] In the foregoing detailed description, various features have been grouped together in examples in order to streamline the disclosure. This manner of disclosure should not be interpreted as an intention that the claimed examples include more features than are expressly recited in each claim.

[0330] Although specific embodiments have been shown and described herein, it will be apparent to one skilled in the art that a variety of alternative and / or equivalent implementations may be substituted for the specific embodiments shown and illustrated therein without departing from the scope of the present application. This application text is intended to cover all adaptations and variations of the specific embodiments described and discussed herein. Therefore, the scope of the present application is limited only by the language of the claims.

Claims

1. A method (100), comprising: - providing (120) a mold substrate and a cover substrate that are connected to each other, wherein a surface region of the mold substrate and / or of the cover substrate is structured so as to form an enclosed cavity between the cover substrate and the mold substrate, - tempering (130) the cover substrate and the mold substrate so as to decrease the viscosity of the glass material of the cover substrate, and providing (140) an overpressure in the enclosed cavity compared to the surrounding atmosphere so as to cause, on the basis of the decreased viscosity of the glass material of the cover substrate and the overpressure in the enclosed cavity compared to the surrounding atmosphere, bulging of the glass material of the cover substrate starting from the enclosed cavity up to a stop area, spaced apart from the cover substrate, of a stop element so as to obtain a molded cover substrate with a cap element; and - removing the stop element and the mold substrate from the molded cover substrate.

2. The method according to claim 1 for manufacturing a cap substrate for housing one or a plurality of optical devices, wherein the molded cover substrate forms the cap substrate with the one cap element.

3. The method according to claim 1 or 2, wherein the cover substrate comprises a single homogenous material so as to form the molded cover substrate from this single homogenous material.

4. The method according to any of the preceding claims, wherein the step of providing a mold substrate and a cover substrate comprises: - providing a mold substrate with a structured surface region - arranging a cover substrate on the structured surface region of the mold substrate, wherein the cover substrate comprises a glass material, and - connecting the cover substrate to the mold substrate so as to form the enclosed cavity between the cover substrate and the mold substrate, or wherein the step of providing a mold substrate and a cover substrate comprises: - providing a mold substrate; - arranging a cover substrate with a structured surface region on the mold substrate, wherein the cover substrate comprises a glass material, and - connecting the cover substrate to the mold substrate so as to form the enclosed cavity between the cover substrate and the mold substrate.

5. The method according to any of the preceding claims, wherein connecting the cover substrate to the mold substrate is carried out in an atmosphere with a defined atmospheric ambient pressure so as to enclose a defined atmospheric pressure in the enclosed cavities.

6. The method according to any of the preceding claims, wherein the step of tempering and providing an overpressure is performed as glass flow process in a negativepressure oven to obtain in the enclosed cavity a defined atmospheric overpressure compared to the surrounding atmosphere.

7. The method according to any of the preceding claims, wherein, in the step of tempering and providing an overpressure, the cover substrate is bulged-out in the region of the enclosed cavity up to a height specified by the distance of the stop area to the cover substrate.

8. The method according to any of the preceding claims, wherein, in cooling the molded cover substrate in the temperature range of above 650°C, an atmospheric overpressure is caused in the enclosed cavities compared to the surrounding atmosphere so as to generate a bulging of the sidewall regions of the cap element of the molded cover substrate towards the outside.

9. The method according to any of claims 1 to 7, wherein, in cooling the molded cover substrate in a temperature range above 650°C, an atmospheric negative pressure in the enclosed cavities compared to the surrounding atmosphere is caused so as to generate a bulging of the side wall regions of the cap element of the molded cover substrate towards the inside.

10. The method according to any of the preceding claims, wherein, in the step of tempering (130) and providing an overpressure (140), the side windows (24-1) and the cap region (24-2) or the side windows (24-1) and the socket regions (24-3) are bulged-out with the glass material of the cover substrate (20) starting from the enclosed cavity (30) up to the spaced-apart stop area (40-1) of the stop element 40.

11. A method (200) for manufacturing a hermetically housed optical device, comprising: performing the method (100) for manufacturing a molded cover substrate according to any of the preceding claims, providing (220) a device substrate with an optical device arranged thereon, and connecting (230) the molded cover substrate with the device substrate so as to house the optical device.

12. The method according to claim 11, further comprising: performing the method for manufacturing housed optical devices on the wafer level, wherein a plurality of optical devices are arranged on the device substrate, and wherein the molded cover substrate comprises a plurality of cap elements.

13. A hermetically housed optical device manufactured with the manufacturing method according to claims 11 or 12, comprising: an optical element arranged on the device substrate; and a molded integral cover substrate providing a hermetically sealed cover for the optical device, within which the optical device is housed, wherein the molded cover substrate comprises a cap element with a bulged sidewall region between a socket region and a ceiling region.

14. The hermetically housed optical device according to claim 13, wherein the sidewall region and / or the ceiling region of the integral cap element of the molded cover substrate comprises a material that is permeable for transmission and / or reception radiation of the optical device, and for coupling and / or decoupling electromagnetic radiation.

15. The housed radiation-emitting device according to claim 13 or 14, wherein the hermetically sealed cover comprises a reactive atmosphere and / or the cavity exclusively contains inorganic substances, and / or wherein the hermetically sealed cover is hermetically sealed against the introduction of water vapor.