SYNTHETIC CRUDE LASOMETER COMPOSITIONS IN FLOWABLE PILL FORM AND METHOD FOR THEIR PREPARATION

DE602012081173T2Active Publication Date: 2024-10-30DYNASOL ELASTOMEROS S A DE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE602012081173
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2011-03-25
Filing Date
2012-03-21
Publication Date
2024-10-30
Estimated Expiration
2032-03-21

AI Technical Summary

Technical Problem

Raw elastomeric compositions, such as SBR elastomers, tend to agglomerate and form blocks due to stickiness, making handling and storage difficult, and existing anti-blocking agents either require treatment, compromise material properties, or have limited effectiveness, which hinders their commercialization and application in free-flowing pellet form.

Method used

The use of emulsifiable inorganic fillers as anti-block agents added during the last drying stage of the elastomer polymerization process, forming raw elastomeric compositions with molecular weights between 50,000 to 400,000 Da, which are then pelletized into free-flowing form without the need for additional processing or additives, maintaining material properties and preventing agglomeration.

Benefits of technology

The approach allows for the commercialization and storage of elastomeric compositions in free-flowing pellet form for extended periods, enhancing their properties when used in applications like asphalt modification, adhesives, and rubber formulations, while reducing the quantity needed and avoiding agglomeration, thus improving handling and storage efficiency.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present invention relates to techniques used for the production, storage and application of elastomeric compositions, and more particularly, it is related to elastomeric compositions in free-flowing pellet form and the process for obtaining the same.BACKGROUND OF THE INVENTION

[0002] Synthetic elastomers, in general, are used in a variety of applications, either as such, or as modifiers of the mechanical and / or rheological properties of other polymers or materials. However, many elastomers, such as styrene-butadiene rubbers (SBR) in raw form, tend to agglomerate and form blocks, which in part gives them their usefulness in a variety of applications such as adhesives or impact modifiers, but that makes handling of the same in raw form very difficult.

[0003] For instance, the most common raw elastomers of commercial type are SBR elastomers, with styrene monomer content fluctuating from 3 to 45% w / w, with the balance being butadiene. By having the most content of butadiene, one of the properties that is immediately apparent in these materials is their stickiness, which is mainly attributed to the glass transition temperature (transition from solid to viscoelastic stage) that is less than -20o C. In particular, this stickiness is increased when the polymers are heated to temperatures above ambient temperature, and even more if pressure is applied. This phenomenon of stickiness is increased when butadiene and styrene are in a mainly random form and blocks of polystyrene are reduced.

[0004] This tackiness property makes impossible to commercialize this type of SBR elastomers in the form of free-flowing pellets, crumbs or particles, inasmuch as over time, the adherence between the particles is increased thus forming naturally blocks, phenomenon that is also known as "cold flow". Because of this fact, regardless of the polymerization process, such SBR elastomers are sold in blocks, usually weighing more than 25 kilograms.

[0005] For this reason, raw elastomers are usually commercialized in the form of big blocks and need to be further cut, milled or somehow processed to reduce them to smaller particles depending on the final application. Such processing to reduce particle size must be done on-site or at a time very close to final processing because otherwise the raw elastomer agglomerates again and form solid big blocks.

[0006] In order to maintain temporarily raw elastomers in small particles, different anti-block or partitioning agents are used in the prior art, ranging from talc or inorganic fillers to complex compounds with resins, other polymers and waxes have been used. However, the majority of these agents have at least one of the following disadvantages: a) They require some kind of treatment (heating, chemical or of some other kind) in order to be applied or after applying it to the elastomer. b) They jeopardize the properties of the elastomer in the final application by compromising tackiness, mechanical or flow properties. c) The amount required for anti-blocking activity is very high. d) The anti-blocking effect is limited in terms of temperature conditions and length of time.

[0007] Of course all of the above disadvantages impose serious applicability or economical burdens that make the majority of the anti-blocking agents unfeasible or limited in use to elastomeric compositions that have been further formulated, cross-linked or vulcanized, so that with less amount of agent the desired anti-blocking effect is achieved at least temporarily. However, when applied to virgin or raw elastomeric compositions, such agents are usually not useful in the long term so as to be able to commercialize, store and process the same in particle, crumb or pellet form.

[0008] One of the applications that are more sensitive to the above described problems is asphalt modification through elastomeric compositions.

[0009] Asphalt is a viscous, sticky and black material used as a binder in pavement mixtures for the construction of road surfaces, as well as in waterproofing. In view of the fact that asphalt is a highly impermeable, adhesive and cohesive material, able to withstand high stresses instantaneous and flow under the action of constant loads, it has ideal properties for the construction of road surfaces complying with the following functions: i) waterproof the pavement structure, making it very sensitive to moisture and effective against the penetration of water from rainfall; and, ii) providing an intimate union and cohesion between aggregates, capable of withstanding the mechanical action of disintegration caused by the loads of vehicles.

[0010] However, in its virgin state asphalt has rheological and thermomechanical properties limiting its application and usefulness life in pavements. For instance, the softening typical temperatures of virgin asphalts are in the range of 50°C to 60°C (rheological-failure temperatures or RFT). However, such temperatures can be improved with the use of polymers that allow RFT higher than 60°C, thus making asphalts more resistant to friction loss associated with rolling of vehicles.

[0011] Another interesting property is that virgin asphalts have performance degrees of the PG type of SUPERPAVE (Superior Performing Asphalt Pavements) typical for PG 64-10. The PG range can be extended to 82-22 PG grades with the help of the polymers.

[0012] Asphalts modified with polymers were developed with the intention to reduce the requirements of energy for the production, storage and application of asphalts cement in roads. The modified asphalts use polymers that can form three-dimensional networks through vulcanization, formation of crystals or entanglements of the polymer chains.

[0013] The objects pursued with the modification of asphalts with polymers are: a) Having more viscous binders at elevated temperatures in order to reduce the permanent deformation of mixtures composing the bearing layers and increasing the stiffness; b) Reducing cracking due to thermal effect at low temperatures and fatigue, thus increasing its elasticity; and c) Having a binder with best adhesive features. SBR elastomeric compositions with molecular weight (Mw) in the range from about 50,000 to 500,000 Daltons in raw form are mostly used to modify asphalts. As mentioned before, these elastomers are commercialized and stored as blocks which subsequently have to be crushed or grinded by the users on-site, thus increasing the costs in the total process of asphalt modification due to both, energy consumption, labor and time.

[0014] There have been various solutions tried in the prior art in order to solve the aforesaid problem.

[0015] One solution has been emulsifying SBR elastomers in water in order to facilitate incorporation into asphalt. However, for polymers with more than 100,000 Daltons of Mw great difficulties for emulsification have been encountered, and in addition, the high temperatures used in the modification processes of the asphalt, often higher than the evaporation temperature of water, origins flashing or sudden streams of water that can cause accidents, in addition to the oxidation of the asphalt that implies a premature aging factor, which reduces its useful life time in the application of pavement.

[0016] These emulsified elastomers have found some application in asphalt emulsions, also well known in the state of the art. These emulsions are mixtures of asphalt with emulsifiers that form a stable emulsification with water, which allows its application on cold asphalt surfaces, that is to say, at temperatures lower than 100° C.

[0017] One of these technologies is found in US Patent No. 6,136,899 wherein a specific type of SBR emulsion can be used to modify asphalt cement to greatly enhance the resistance to shoving, rutting and low temperature cracking of asphalt concretes made therewith. Such SBR emulsion is compatible with virtually all types of asphalt and the modified asphalts have extremely high levels of force ductility, tenacity and toughness. According to this patent, SBR used to modify asphalt cement in the practice of this invention is a blend of (i) a high molecular weight (Mw) styrene-butadiene rubber having an average Mw of at least about 300,000 and (ii) a low Mw styrene-butadiene rubber having an average Mw of less than about 280,000; wherein the ratio of the high Mw styrene-butadiene rubber to the low Mw styrene-butadiene rubber is within the range of about 80:20 to about 25:75, and require further features in the elastomer composition in order to work.

[0018] On the other hand, in the US Patent Serial No. 6,503,968 an asphalt modifier of styrene-butadiene-styrene block copolymer and styrene-butadiene latex is disclosed, which relates to an asphalt modifier comprising 5-30 wt % of dispersed styrene-butadiene-styrene block copolymer and 70-95 wt % of dispersed styrene-butadiene latex, which has an excellent resistance property against plastic deformation, while preventing the occurrence of crack at a low temperature. However, this technology, as mentioned before, has the disadvantage of the need of evaporating water in order to recover the elastomer and in some cases, particularly when modifying the asphalt in temperatures higher than 100° C, with the problems described above. In addition, its application require excess of polymeric latex emulsion, considering that the solids content of these materials fluctuate at levels less than 70 % solids, which impacts the final cost of operation.

[0019] An improved method for treating crumb rubber particles for use in asphalt compositions is disclosed in US Patent No. 5,927,620 which is characterized by activating the particles to enhance rheological properties thereof. A slurry of crumb rubber particles is formed by adding water thereto. The slurry is heated to a temperature of 85-90° C to release excess oils and chemicals from the particles into the slurry. The slurry is dried to produce a fine mesh rubber product with enhanced rheological properties. Such materials have the disadvantage that it is no longer a virgin material, but a cross-linked material mixed with some loads such as carbon black which is used as the main ingredient in tire formulations.

[0020] Likewise, US Patent Serial No. 6,884,831 relates to modified asphalts with partitioning agent and method for making the same, which is characterized by the addition of a partitioning agent to a polymer modifier material such as synthetic rubber to prevent re-agglomeration of the rubber. The partitioning agent is complex and includes a mixture of phenyl-formaldehide resins and waxes. Whereas reduction of time required to disperse the modifier material in asphalt and lower viscosity of the modified asphalt are reported through the use of such partitioning agent, this technology requires high temperature to incorporate the partitioning agent into the polymer and, due to the resins and waxes contained therein, its use in emulsions and the incorporation in the normal process of production of raw polymers is expensive and difficult because the additive is incompatible with water and, evidently, very difficult to emulsify, thus making the whole process more expensive due to both, energy requirements for incorporation into the polymer and further treatments and additives required at the application in asphalt.

[0021] The same disadvantages are found in US Patent Serial No. 7,371,794 and 7,847,006, which refers to the same kind of partitioning agent with phenyl formaldehyde resin and waxes, in the case of the latter with the addition of precipitated silica. As it is easily seen, the disadvantages of these additives with waxes and resins prevail, where the preferred temperatures for addition of the partitioning agent to the polymer are well above 100°C and a preheating step is necessary in order to make more fluid the resin and waxes.

[0022] Likewise, the US Patent Application Serial No. 2010 / 0187718 relates to a method for making a modified polymer, which is characterized by re-capsulating the polymer via extrusion, through the use of a cross-linking agent that is mixed with particles of synthetic rubber material to form a mixture which is then heated and delivered to an extruding machine. The extruding machine further heats the mixture and produces strands of modified polymer material which are cooled and pelletized to form small pellets of re-capsulated modified polymer. A partitioning or anti-blocking agent of the same type than described in the other patents, namely with phenyl formaldehyde resin and waxes, is added to the pellets to prevent re-agglomeration of the modified polymer.

[0023] The modifier materials or anti-block additives described in the U.S. patents mentioned above describe properties that could solve the problem of agglomeration of raw elastomer particles, but have a lot of problems in the process due to the resins and waxes contained therein, which make it difficult and expensive to apply due to the use of temperature, and problems in the drying systems during the processes of production of the elastomers, through increasing the internal pressure in the same and with the need of further additives or processing.

[0024] Furthermore, the European Patent application No. EP 0 427 339 A2 describes a composition for coating wet rubber particles during extrusion and pelletization prior to drying comprising an inorganic partitioning agent, a thickener and binder reagent, water and a water soluble anionic dispersant, and to the process for application to elastomers including those of low viscosity or high resin content to improve their processability during manufacture.

[0025] In addition, the Patent No. US 4, 207, 218 discloses a particulate rubber that is intimately and uniformly coated with an anti-cake(s) and pressed at mild temperatures to form friable rubber bales. The bales have a bulk density from about 1.3 to about two times that of the original particulate rubber and are capable of being handled as a slab and of supporting a direct load, yet break down under shear to form particles substantially similar in size and distribution to that of the original particulate rubber.

[0026] On the other hand, the Patent No. US 4, 212, 918 refers to nontacky, elastomeric shaped objects (e.g., pellets or filaments) comprising a normally tacky, uncured elastomer having an integral, porous coating of silicic or aluminic acid polymer can be prepared by bringing shaped bodies of a normally tacky, uncured elastomer latex into contact with an aqueous bath containing a soluble coagulating salt for the latex, and a silicic or aluminic acid polymer, and washing and drying the resulting coated shaped objects. The shaped objects are highly porous before washing and drying, and some porosity remains even after washing and drying.

[0027] Additionally, the Patent No. US 6, 238, 732 B1 describes a hot melt adhesive composition in pellet form. The hot melt adhesive composition is pressure sensitive, having a storage modulus, G', at 25 °C, of less than about 5×10 6< dynes / cm 2< . The pellets are coated with a pelletizing aid on the surface at a concentration preferably ranging from about 1 wt-% to about 30 wt-%. The pelletizing aid is a hot melt adhesive component or a material which does not substantially adversely affect the adhesive properties. The pellets are free-flowing and have a substantially tack free surface.

[0028] Furthermore, the application No. US 2004 / 0116578 A1 refers to a granular inorganic which is highly effective in improving the physical properties of resins and excellent in working efficiency, working atmosphere, productivity and economical efficiency, and a process for producing the filler, and resin compositions excellent in mechanical properties, surface appearance, flame retardance and anti-block properties. The filler is produced by granulating a mixture comprising inorganic filler particles having a mean particle diameter of 0.01 to 20 µm and a binder in such a way as to give an apparent density of 0.1 to 3.0 g / ml and a breakage rate of 5 to 80wt %. The resin compositions are prepared by adding the granular inorganic filler to resins.

[0029] However, none of the prior art has suggested or described raw elastomeric compositions in free-flowing pellet form that, in addition to allowing the commercialization, storage and application as particles, enhance the properties of the rubber when used in further applications, maintaining the properties of the elastomeric composition when used as modifier for asphalts, typical rubber applications or adhesives, in spite of the use of an anti-blocking or partitioning agent. Furthermore, there are not any technologies allowing the incorporation of an anti-blocking or partitioning agent without the need of further processing or the use of more additives, without compromising the properties of the elastomer in the final applications and with anti-blocking effects achieved for long storage times and high weights, thus allowing commercialization in crumb, pellet or particle form.BRIEF DESCRIPTION OF THE INVENTION OBJECTS OF THE INVENTION

[0030] Considering the defects of the prior art, it is an object of the present invention to provide raw elastomeric compositions in free-flowing pellet form that can be obtained, stored and commercialized in such form, with large periods of storage allowing keeping such form during transportation and use, without compressing thereof again and avoiding the formation of large blocks that difficult their utilization.

[0031] Moreover, it is another object of the present invention to provide raw elastomeric compositions in free-flowing pellet form such that, in addition to keep the expected properties of the raw material in the final application, enhance some properties when used in certain applications, without the need of further processes or additives.

[0032] It is a further object of the present invention to provide raw elastomeric compositions in free-flowing pellet form such that may be used in less quantities than other compositions in the prior art for the same applications.

[0033] It is another object of the present invention to provide a process for obtaining raw elastomeric compositions in free-flowing pellet form such that may be easily used in emulsified applications and produced without the need of heat and in the absence of waxes or complex additives during the production of the raw elastomeric composition, but allowing further processing with easiness in final applications such as asphalts, emulsified asphalts, adhesives or rubber forming.

[0034] It is also an object of the present invention to provide modified asphalts with enhanced mechanical properties through the addition of the raw elastomeric compositions in free-flowing pellet form, including the use in emulsified asphalts.

[0035] It is still another object of the present invention to provide an adhesive composition that keeps its adhesive properties above the minimum parameters required for applications as adhesives, in spite of being in free-flowing pellet form and not showing agglomeration.

[0036] All of the above objects are achieved through a raw elastomeric composition comprising an elastomer with molecular weight from 50,000 to 400,000 Da and an anti-block agent containing emulsifiable inorganic fillers. The process for obtaining the composition includes the step of adding the anti-block agent at the last drying stage of the raw elastomer, which anti-block agent is incorporated either as an emulsion or in solid form, without the need of pretreatment or additional heat for incorporation thereof.BRIEF DESCRIPTION OF THE DRAWINGS

[0037] The novel features of the present invention are established particularly in the appended claims. However, the invention itself together with other objects and advantages thereof will be better understood in the following detailed description of a specific embodiment, when read along with the appended figures, in which: Figure 1 is a block diagram showing the step sequence of the process for obtaining raw elastomeric compositions in free-flowing pellet form, developed according to the present invention. Figure 2 is a graphic showing the maximum temperature of rheological failure (RFT) of several specific embodiments of the claimed raw elastomeric compositions in free-flowing pellet form. Figure 3 is a graphic showing the maximum temperature of rheological failure (RFT) of another specific embodiments of the claimed raw elastomeric compositions in free-flowing pellet form. DETAILED DESCRIPTION OF THE INVENTION

[0038] In spite of the normal effect that inorganic fillers have in the properties of raw elastomeric compositions, through the use of emulsifiable inorganic fillers, the present invention provides raw elastomeric compositions in free-flowing pellet form that can be obtained, stored and commercialized in such form, with large periods of storage allowing keeping such form during transportation and use, without compressing thereof again but that, in addition to keep the expected properties of the raw material in the final application, enhance some properties when used in certain applications, without the need of further processes or additives.

[0039] According to the principles of the present invention, the raw elastomeric compositions in free-flowing pellet form comprise: a) a raw elastomer with molecular weight from 50,000 to 400,000 Da; and, b) from 2 to 8% by total weight of an anti-block agent selected from the group comprising metallic carbonates, metallic sulfates, metallic oxides, metallic hydroxides, metallic aluminosilicates, alumina, silica, talc and combinations thereof, in combination with a compatible emulsifier capable of forming emulsions of the same in water, which is selected from alkaline salts of organic 10 fatty esters with less than 20 carbon atoms. The raw elastomeric composition is formed by a process comprising at least the following steps: a) Polymerizing at least one monomer through solution polymerization in order to obtain elastomer crumbs; b) Forming an aqueous suspension of the elastomer crumbs to eliminate polymerization solvents and residues; c) Dewatering the aqueous suspension to achieve a maximum water content of 25% by weight; d) Adding from 2 to 8% of an anti-block agent comprising inorganic fillers capable of forming emulsions in water; e) Drying the dewatered suspension to achieve a maximum water content of 1%; and f) Pelletizing the elastomer to form a raw elastomeric composition in free-flowing pellets form with maximum particle size of 5.08 cm (2 inches).

[0040] As used herein, the term "raw elastomer" refers to any elastomer that has not suffered a cross-linking, vulcanization or chemical treatment after being obtained from a polymerization process.

[0041] In a preferred embodiment of the present invention, the elastomer is selected between Solution-SBR, Emulsion-SBR, SB di-block copolymers and tapered triblock copolymers, but styrene - butadiene copolymers with butadiene content higher than 60% weight / weight are particularly preferred.

[0042] The tapered triblock copolymers include, but are not limited to, elastomers and thermoplastic elastomers made from block copolymers of styrene (S), butadiene (B), and / or isoprene (I) of varying sizes and number of blocks. Examples of such elastomers and thermoplastic elastomers include (S / B-rich)-(B / S-rich)-S, (S / I-rich)-(I / S-rich)-S, (S / B)-S, (S / I)-S, (S / B)m-S and (S / I)m-S (where m is an integer), S-(S / B-rich)-(B / S-rich)-S, S-(S / I-rich)- (I / S-rich)-S, S-(B / S-rich)-(S / B-rich)-(B / S-rich)-S, S-(I / S-rich)-(S / I-rich)-(I / S-rich)-S, [S-(B / S-rich)-(S / B-rich)]n-X, [S-(I / S-rich)-(S / I-rich)]n-X, X-[S-(B / S-rich)-(S / B-rich)]n, X-[S-(I / S-rich)-(S / I-rich)]n (where X is the residue of either a coupling agent or a multifunctional initiator and n is an integer from 2 to about 30) tapered triblock copolymers as well as their hydrogenated, selectively hydrogenated, and partially hydrogenated counterparts. These tapered triblock copolymers are disclosed in US Patent Application No. 13 / 361,740.

[0043] In a particularly preferred embodiment of the invention, the compatible emulsifier is a stearate.

[0044] In a particularly preferred embodiment, the anti-block agent comprises: a) 3-9% w / w calcium hydroxide; b) 0.3-1.1% w / w talc; c) 0.5-2% w / w titanium dioxide; d) 0.3-1% w / w calcium aluminosilicate; e) 0.2-0.7% w / w potassium aluminosilicate f) 0.5-1.5% w / w magnesium sulfate; g) 75-85% w / w silica; and h) 7-11% w / w calcium stearate.

[0045] The anti-block agent can be used in powder form or as a water-based emulsion with solids content from about 5 to about 50% by weight.

[0046] The raw elastomeric compositions in free-flowing pellet form of the present invention have a maximum particle size of 2 inches; a melt flow index of 3 to 13.1 g / 10 minutes at 190°C y 2.16 Kilos and at 200°C and 5 Kilos, respectively, and require a maximum force of 15 kgf to loosen into particle form again after applying a continuous force of 2.76 kg at 50°C for 90 hours.

[0047] The process for obtaining raw elastomeric compositions in free-flowing pellet form of the present invention, as shown in Fig. 1, comprises the following steps: a) Polymerizing at least one monomer through solution polymerization in order to obtain elastomer crumbs; b) Forming an aqueous suspension of the elastomer crumbs to eliminate polymerization solvents and residues; c) Dewatering the aqueous suspension to achieve a maximum water content of 25% by weight; d) Adding from 2 to 8% of an anti-block agent comprising inorganic fillers capable of forming emulsions in water; e) Drying the dewatered suspension to achieve a maximum water content of 1%; and f) Pelletizing the elastomer to form a raw elastomeric composition in free-flowing pellets form with maximum particle size of 2 inches.

[0048] The polymerization and suspension steps of the process are well known in the prior art, and the specific conditions for polymerization and suspension will be readily known to those skilled in the art and depend on the final application of the elastomer obtained therein.

[0049] In a particularly preferred embodiment of the present invention, the dewatering stage is performed through an extrusion equipment of the type known as single screw spindle, wherein the screw cover has ribs at the lower section of the extrusion equipment partially open to eliminate the squeezed water, but without allowing pass the wet lumps of elastomer.

[0050] Likewise, the drying step may be performed through extrusion processes, wherein the anti-block additive is preferably added through the hopper of the extrusion equipment. It is particularly preferred for the drying step extrusion equipment of the single screw type having a variable configuration.

[0051] In the preferred embodiment where the extrusion process is used for the drying stage, the elastomer leaving the extruder is immediately pelletized and the obtained pellets are optionally further dried, preferably through a fluidized bed process with hot air.

[0052] In an additional embodiment of the invention, the pellets finally obtained are sprayed again with the anti-block additive in emulsified form with solids content from about 5 to about 50% by weight.

[0053] The raw elastomer composition in free-flowing pellet form of the present invention can be packed in bags or cardboard boxes of up to 1 ton and will keep its form for at least one year, featuring free-flowing at all times and without re-agglomeration.

[0054] The raw elastomer composition in free-flowing pellet form of the present invention can be used as an adhesive composition that keeps its adhesive properties above the minimum parameters required for applications as adhesives, even when it is in free-flowing pellet form and it does not agglomerate, and in spite of containing inorganic compounds. Additionally, the raw elastomer composition in free-flowing pellet form of the present invention can be used to obtain modified asphalts through the addition of 1 to 6% by weight of said raw elastomer composition in free-flowing pellet form to the asphalt. The modified asphalt thus obtained has a maximum rheological-failure temperature (RFT) of at least 90 °C. Furthermore, the raw elastomer composition in free-flowing pellet form of the present invention can be used to obtain a modified asphalt emulsion through the addition of 1 to 6% by weight of said raw elastomer composition in free-flowing pellet form to the asphalt emulsion.EXAMPLES

[0055] Using the process of the present invention, with extrusion processes for dewatering and drying, different pellets of a specific embodiment of the present invention were obtained with SBR elastomers, which were evaluated for performance without the combination of the anti-block additive, as well as with different amounts of the same. The dewatering stage for all examples was performed through an extrusion equipment of the type known as single screw spindle.

[0056] In turn, for all examples, the drying step was performed through an extrusion equipment of the single screw type having a variable configuration, and the elastomer leaving the extruder was immediately pelletized and the obtained pellets were dried through a fluidized bed process with hot air, except for Examples 1 and 3.Example 1 - Raw elastomer without anti-block agent.

[0057] The SBR elastomer was obtained as described above, with molecular weights of 109,000 Daltons and a monomer ratio 25 / 75 styrene / butadiene, but no anti-blocking agent was used for this process. The material obtained in this example was designated E1 and it was characterized and used as a reference for comparison in testing.Example 2 - Raw elastomer with anti-block agent of the present invention.

[0058] The SBR elastomer was obtained as described for Example 1, but an anti-blocking agent was incorporated to the extruder prior to the drying step. The anti-blocking agent was a mixture of calcium carbonate, magnesium sulfate, calcium oxide, calcium hydroxide, potassium aluminosilicate, calcium aluminosilicate, alumina, titanium dioxide, silica and talc, in combination with sodium estearate as compatible emulsifier. The anti-block agent was used in powder form or as a water-based emulsion and it was added in different proportions. Through this process Examples 2A, 2B and 2C were developed, using respectively 2%, 3.5% and 6% by weight (dry base) of the anti-blocking agent. The materials obtained were further characterized and tested.Example 3 - Raw elastomer without anti-block agent.

[0059] The SBR elastomer was obtained as described above, but this time with molecular weights of 240,000 Daltons and a monomer ratio 15 / 85 styrene / butadiene, but no anti-blocking agent was used for this process. The material obtained in this example was designated E3 and it was characterized and used as a reference for comparison in testing.Example 4 - Raw elastomer with anti-block agent of the present invention.

[0060] The SBR elastomer was obtained as described in Example 3, but an anti-blocking agent was incorporated to the extruder prior to the drying step. The anti-blocking agent was a mixture of calcium carbonate, magnesium sulfate, calcium oxide, alumina, titanium dioxide, silica and talc, in combination with sodium estearate as compatible emulsifier. The anti-block agent was used in powder and it was added in different proportions, but the extruder was an equipment of the single screw type having a variable configuration. Through this process Examples 4A, 4B and 4C were developed, using respectively 2%, 3.5% and 6% by weight (dry base) of the anti-blocking agent. The materials obtained were further characterized and tested.

[0061] All of the materials obtained in the examples were measured two "critical" parameters. Firstly, its adhesive properties were measured in order to verify whether the material could be used for adhesive applications or not. The results are shown for all the materials in Table 1 below: TABLE 1 - Adhesive propertiesPROPERTYSPECIFICATIONE1E2-AE-2-BE2-CBrookfield viscosity at 177°C, cP5741 maximum5289530154235507Softening temperature, °C75 minimum7575.67676.9Tension, MPa1.4 minimum1.51.41.41.4Loop Tack, kgf1.59 minimum4.084.224.314.40Peel, kgf1.81 minimum3.813.763.723.63Shear, minutes33 minimum55524844

[0062] As it can be readily seen, even though the adhesive properties are jeopardized as expected, the parameters are still above the minimum required for applications of these elastomers as adhesives in spite of the presence of the anti-block agent of the present invention, which was unexpected because the properties are usually affected greatly by inorganic fillers.

[0063] In addition, samples of the materials were subjected to a compression test. The test consisted of filling with each material of the examples a hollow cylinder of 628.3 cm3 of volume (12.5 cm height and 8 cm the diameter of the base). With the material inside the cylinder, another cylinder of 2.76 kg was put on the material and the whole system was kept at 50°C for 90 hours. After such time, the force required to divide into particles again the material after taking it from the cylinder was measured for all the materials, according to the following: TABLE 2 - Degree of force required to divide into particles the block formed in the compression testForce rangeObservation≥ 60-80 kgfThe material is totally compressed, being impossible to divide it with a hand.40-50 kgfThe material shows some compacting. It can be divided with some effort.15-30 kgfThe material takes the form of a compact cylinder, being easily divided with a hand.< 15 kgfThe material is totally flowing, being difficult that it forms a block.

[0064] The compression test simulates the storage conditions of the materials, i.e. a period of 6 months and at least 700 kg of material over the last layer of material.

[0065] The results of this compression test are shown in Table 3 below. TABLE 3 - Forces needed to loosen the materials after compression test.E1E2-AE2-BE2-CE3E4-AE4-BE4-CForce (kgf)>160>40>30<10>16030-40<15<5

[0066] According to the above, it is evident that the materials of the present invention require very little force to recover the pellet form, which is equivalent to pushing the material with the finger. Therefore, the materials obtained with the principles of the present invention can be stored and transported in pellet form without the risk of agglomeration and block forming.Example 5 - Comparison of anti-block agents

[0067] Compositions containing the SBR elastomer of Example 1 and different materials used as anti-block agents, corresponding to Examples 5A to 5O, were subjected to the compression test in order to compare their performance. The additives used were: Petrolite 01 Dispersion (E5A); micronized hydroxilated polyethylene wax (E5B), calcium stearate (E5C), industrial talc (E5D), calcium carbonate (E5E), Barbe 237 (emulsified calcium carbonate) (E5F), erucamide (E5G), crodamide (E5H), talc (E5I), gilsonites (E5J), diatomeaceous earth (E5K), Reagent A (E5L), Reagent B (E5M), Aquastab reagent

[0068] (pulverized and micronized polyethylene) (E5N) and the additive of the present invention (E5O). The results are shown in Table 4: TABLE 4 - Performance of several anti-block agents in compression testAnti-block agentConcentration of anti-block agent in the composition, %11.52345OthersE5A - Petrolite 01 Dispersion (Baker Hughes, 2003)68 kgf57 kgf40 kgfE5B - Micronized hydroxilated polyethylene wax (Baker Hughes, 2003)>50 kgf>50 kgf>50 kgfE5C - Calcium stearate (Corporacion Sierra Madre, 2005)72 kgf52 kgf36 kgf27 kgfE5D - Industrial talc ( OMYA, 2004)78 kgf50 kgfE5E - Calcium carbonate (Minstron, 2005)65 kgf42 kgfE5F - Barbe 237 (emulsified calcium carbonate) (Barbe America Inc., 2003)57 kgf40 kgfE5G - Erucamide (Croda, 2007)>150 kgf>150 kgf>150 kgfE5H - Crodamide (Croda, 2007)>150 kgf>150 kgf>150 kgfE5I - Talc (Cognis, 2007)>500 kgf>500 kgf>500 kgf (at 6%)E5J - Gilsonites (325 and 300, ER125) (American Gilsonite, 2009)>200 kgf>200 kgf>200 kgfE5K - Diatomeaceous earth (Chemtex Int. de Mex., 2006)>300 kgf>300 kgf>300 kgf>200 kgfE5L - Reagent A (Moore & Murger, 2006)67 kgf49 kgf42 kgfE5M - Reagent B (Moore & Murger, 2006)78 kgf76 kgf70 kgfE5N - Aquastab reagent (pulverized and micronized polyethylene) (Eastman, 2007)>500 kgfE5O - Additive of the present invention>120 kgf>40 kgf>30 kgf<10 kgf (E2C)

[0069] As can be seen from above, the materials of the present invention require less force to recover the pellet form after being subjected to the compression test, when compared to elastomers modified with other anti-block agents.

[0070] Now then, in order to measure the features of the materials of the present invention, the materials were tested as asphalt modifiers. The material was added to an asphalt grade AC-20, with a penetration of 60-80 1 / 10 mm at 25° C, which was heated to a temperature of 170-195° C, with a stirring of 600 rpm. TABLE 5.- Results of modified asphalt of Examples 1 and 2 SBR block (styrene-butadiene ratio 25 / 75) and SBR pellets with anti-block additive.PROPERTY TEST METHOD E1 E2-A E2-B E2-C MIXTURE WITH 2% W / W POLYMER IN ASPHALT. Elastomer dispersion time in asphalt, minutesFluorescence Microscopy with referente90809090Softening temperature, °CASTM D3657575757Penetration at 25°C, 100 g, 5 s, 1 / 10 mmASTM D554535352Brookfield viscocity at 135°CASTM D44029759759001000Torsional elastic recovery, %IRAM 683018212022MIXTURE WITH 3% W / W POLYMER IN ASPHALT .Elastomer dispersion time in asphalt, minutesFluorescence Microscopy with referente90809090Softening temperature, °CASTM D3665646564Penetration at 25°C, 100 g, 5 s, 1 / 10 mmASTM D551495151Brookfield viscocity at 135°CASTM D44021413138813881400Torsional elastic recovery, %IRAM 683020222223MIXTURE WITH 4% W / W POLYMER IN ASPHALT .Elastomer dispersion time in asphalt, minutesFluorescence Microscopy with reference110100100105Softening temperature, °CASTM D3666696666Penetration at 25°C, 100 g, 5 s, 1 / 10 mmASTM D548444844Brookfield viscocity at 135°CASTM D44021825183718621875Torsional elastic recovery, %IRAM 683021252424

[0071] As it can be seen from the results in Table 5, the additive does not affect the main thermo-mechanical properties. For example, the torsional elastic recovery at 25° C shows that the additive even slightly improves this property, and the majority of the parameters such as penetration, viscosity and dispersion time are either improved or kept as with the typical block elastomer used in the prior art without anti-blocking agent. For the particular case of viscosity, the SHRP-SUPERPAVE criterion sets that the maximum allowed viscosity at 135° C is 3000 cP, which is fulfilled in all cases.

[0072] The samples were tested also for the maximum Rheological-Failure Temperature (RFT). This is the temperature at which the ratio of complex modulus or stiffness divided by the angle of deformation of the asphalt is below or equal to 1 kPa, which is a fundamental rheological specification on modified asphalts.

[0073] The profile of RFT with different amounts of the polymer composition of the present invention is shown in Figure 2. As it is easily seen, desirable high temperatures are achieved with very low quantities of the polymer composition of the present invention, which means that not only the anti-block agent used to preserve the pellet form is not jeopardizing the properties of the asphalt, but rather such composition is improving the properties, as less amount of elastomer is required to achieve the same RFT, which for very strict applications such as airport asphalts, the RFT is set at 66°C.

[0074] The same testing was performed with Examples 3 and 4, which results are shown in Table 6 and Figure 3, and which also shows that the composition of the present invention does not affect asphalt as modifier, but it rather improves some of the properties of the modified asphalt. TABLE 6.- Results of modified asphalt of Examples 3 and 4 SBR block of 240,000 Da (styrene-butadiene ratio 15 / 85) and SBR pellets with anti-block additive.PROPERTY TEST METHOD E3 E4-A E4-B E4-C MIXTURE WITH 2% W / W POLYÍMER IN ASPHALT. Elastomer dispersion time in asphalt, minutesFluorescence Microscopy with reference1009095100Softening temperature, °CASTM D3663636364Penetration at 25°C, 100 g, 5 s, 1 / 10 mmASTM D548494848Brookfield viscocity at 135°CASTM D44021112111011121111Torsional elastic recovery, %IRAM 683029313030MIXTURE WITH 3% W / W POLYMER IN ASPHALT .Elastomer dispersion time in asphalt, minutesFluorescence Microscopy with reference110110105110Softening temperature, °CASTM D3668686968Penetration at 25°C, 100 g, 5 s, 1 / 10 mmASTM D543424140Brookfield viscocity at 135°CASTM D44021632162816091613Torsional elastic recovery, %IRAM 683034353738MIXTURE WITH 4% W / W POLYMER IN ASPHALT .Elastomer dispersion time in asphalt, minutesFluorescence Microscopy with reference120115115115Softening temperature, °CASTM D3671727271Penetration at 25°C, 100 g, 5 s, 1 / 10 mmASTM D538383837Brookfield viscocity at 135°CASTM D44022015201020132014Torsional elastic recovery, %IRAM 683036373838 Example 6 - Asphalt emulsions

[0075] The materials of the present invention were tested and compared to the traditional products used in asphalt emulsions for chip seals. The materials evaluated were EVA (E6A), butonal( E6B); SBR elastomer of Example 1 (E6C and E6D) and the materials obtained in Examples 2A and 2B (E6E and E6F).

[0076] The results are shown in Table 7. TABLE 7. Results of asphalt emulsions for chip sealsPARAMETE R METHOD SPECIFI CATION CONVENTIO NAL RAW ASPHALT CQS-65 E6A (EVA AT 3%) E6B (BUTON AL 3% SBR) E6C (E1 at 2.4% / ) E6D (E1 at 3%) E6E (E2A) E6F (E2B) EMULSION PROPERTIES 20 mesh retention, %MMMP-4-05-014Lower than 1%00000.10.20.3Discharge time in pavement, seconds300 a 600100300323520567480586SF viscosity at 50°C, secondsMMMP-4-05-00464 a 18013568160170179173179Asphalt cement content, % w / wMinimum 65%65.7676765656565Settling at 1 day, %MMMP-4-05-013Maximum 1%0.7600.20.20.30.20.3Settling at 5 days, %MMMP-4-05-013Maximum 3%0.7800.20.20.40.30.4ASPHALT RESIDUE PROPERTIES Elastic recovery by ductilometer at 10°C, %Minimum 40Not measured254340474351Elastic recovery by ductilometer at 25°C, %Minimum 50Not measured304850555257Ductility at 4°C, cmMinimum 30Not measured101414309.530Residue adherenceAustralian T230Minimum 85%70788387938894Active adherenceBoilingMinimum 90%75809093989398

[0077] As it can be seen from results of Table 7, the additive does not affect the properties of asphalt emulsions for use in chip seals, but it rather improves the adherence properties when compared to the products that are traditionally used for this purpose, even when less amount of the material of the present invention is used.

[0078] Accordingly, the present invention should not be interpreted only in the light of the examples, as many variations such as different elastomers or specific compositions of the anti-block agent used in the present invention might be apparent from the specification in full. Accordingly, the present invention shall be limited only by the scope of the appended claims.

Claims

1. A raw elastomeric composition in free-flowing pellet form comprising: a) a raw elastomer with molecular weight from 50,000 to 400,000 Da; and, b) from 2 to 8% by total weight of an anti-block agent selected from the group comprising metallic carbonates, metallic sulfates, metallic oxides, metallic hydroxides, metallic aluminosilicates, alumina, silica, talc and combinations thereof, in combination with a compatible emulsifier capable of forming emulsions of the same in water, which is selected from alkaline salts of organic 10 fatty esters with less than 20 carbon atoms; wherein the raw elastomeric composition is formed by a process comprising at least the following steps: a) Polymerizing at least one monomer through solution polymerization in order to obtain elastomer crumbs; b) Forming an aqueous suspension of the elastomer crumbs to eliminate polymerization solvents and residues; c) Dewatering the aqueous suspension to achieve a maximum water content of 25% by weight; d) Adding from 2 to 8% of an anti-block agent comprising inorganic fillers capable of forming emulsions in water; e) Drying the dewatered suspension to achieve a maximum water content of 1%; and f) Pelletizing the elastomer to form a raw elastomeric composition in free-flowing pellets form with maximum particle size of 5.08 cm (2 inches)2. The elastomeric composition of claim 1, wherein the elastomer is selected between Solution-SBR, Emulsion-SBR, SB di-block copolymers and tapered triblock copolymers.

3. The elastomeric composition of claim 2, wherein the elastomer is a styrene - butadiene copolymer with butadiene content higher than 60% weight / weight.

4. The elastomeric composition of claim 1, wherein the inorganic fillers contained in the anti-block agent are selected from the group comprising calcium carbonate, magnesium sulfate, calcium oxide, titanium dioxide, calcium hydroxide, potassium aluminosilicate, calcium aluminosilicate, alumina, silica, talc and combinations thereof.

5. The elastomeric composition of claim 4, wherein the inorganic fillers contained in the anti-block agent are selected from the group comprising magnesium sulfate, titanium dioxide, calcium hydroxide, silica, potassium aluminosilicate, calcium aluminosilicate, talc and combinations thereof.

6. The elastomeric composition of claim 1, wherein the compatible emulsifier is a stearate.

7. The elastomeric composition of claim 1, wherein the anti-block agent comprises: a) 3-9% w / w calcium hydroxide; b) 0.3-1.1% w / w talc; c) 0.5-2% w / w titanium dioxide; d) 0.3-1% w / w calcium aluminosilicate; e) 0.2-0.7% w / w potassium aluminosilicate f) 0.5-1.5% w / w magnesium sulfate; g) 75-85% w / w silica; and h) 7-11% w / w calcium stearate.

8. The elastomeric composition of claim 1, wherein the anti-block agent can be used in powder form or as a water-based emulsion with solids content from about 5 to about 50% by weight.

9. The elastomeric composition of claim 1, wherein the pellets have a maximum particle size of 5.08 cm (2 inches).

10. The elastomeric composition of claim 1, wherein it has a melt flow index of 3 to 13.1 g / 10 min.

11. A process for obtaining raw elastomeric compositions in free-flowing pellet form, comprising the steps of: a) Polymerizing at least one monomer through solution polymerization in order to obtain elastomer crumbs; b) Forming an aqueous suspension of the elastomer crumbs to eliminate polymerization solvents and residues; c) Dewatering the aqueous suspension to achieve a maximum water content of 25% by weight; d) Adding from 2 to 8% of an anti-block agent comprising inorganic fillers capable of forming emulsions in water; e) Drying the dewatered suspension to achieve a maximum water content of 1%; and f) Pelletizing the elastomer to form a raw elastomeric composition in free-flowing pellets form with maximum particle size of 5.08 cm (2 inches).

12. The process for obtaining elastomeric compositions of claim 11, wherein the dewatering stage is performed through an extrusion equipment of the type known as single screw spindle.

13. The process for obtaining elastomeric compositions of claim 11, wherein the drying step is performed through extrusion processes.

14. The process for obtaining elastomeric compositions of claim 12, wherein the drying step is performed through extrusion equipment of the single screw type having a variable configuration.

15. The process for obtaining elastomeric compositions of claim 12, wherein the elastomeric composition is additionally dried in another step through a fluidized bed process with hot air.

16. An adhesive composition comprising: a) a raw elastomer with molecular weight from 50,000 to 400,000 Da; and b) from 2 to 8% by total weight of an anti-block agent comprising inorganic fillers, capable of forming emulsions in water, wherein the Brookfield viscosity at 177°C is maximum 5741 cP, the softening temperature is at least 75 °C, Tension is at least 1.4 MPa, Loop Tack is at least 1.59 kgf, the Peel is at least 1.81 kgf, and Shear is at least 33 minutes, wherein the adhesive composition is formed by a process comprising at least the following steps: a) Polymerizing at least one monomer through solution polymerization in order to obtain elastomer crumbs; b) Forming an aqueous suspension of the elastomer crumbs to eliminate polymerization solvents and residues; c) Dewatering the aqueous suspension to achieve a maximum water content of 25% by weight; d) Adding from 2 to 8% of an anti-block agent comprising inorganic fillers capable of forming emulsions in water; e) Drying the dewatered suspension to achieve a maximum water content of 1%; and f) Pelletizing the elastomer to form an adhesive composition17. A modified asphalt emulsion of the type comprising an asphalt emulsion and an elastomer, wherein the elastomer is a raw elastomeric composition in free-flowing pellet form as claimed in claim 1.

18. The modified asphalt emulsion of claim 17, wherein in order to achieve the same adherence of the asphalt emulsion, a lower amount of the elastomeric composition is used.

19. A modified asphalt of the type comprising asphalt and an elastomer, wherein the elastomer is a raw elastomeric composition in free-flowing pellet form as claimed in claim 1.

20. The modified asphalt of claim 19, wherein the maximum rheological-failure temperature (RFT) is at least 90 °C when the modified asphalt is processed.