METHOD FOR APPLYING A COATING TO A CONTINUOUS FIBER
Patent Information
- Application Number
- DE602018075897
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-12-26
- Filing Date
- 2018-12-20
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2038-12-20
AI Technical Summary
Existing methods for depositing coatings on continuous carbon or silicon carbide fibers, such as chemical gas infiltration (CVI), result in inhomogeneous coatings with high costs and low kinetics, leading to undesirable mechanical properties in ceramic matrix composite materials.
A process involving heating a segment of the fiber in a microwave field to form a coating from a precursor, allowing for direct and uniform heating of the fiber and precursor, enabling rapid and homogeneous coating formation, with the option to use the fiber in liquid, gas, or supercritical phases, reducing energy requirements and improving coating kinetics.
This method achieves a uniform and rapid coating formation on continuous fibers, enhancing the mechanical properties of ceramic matrix composites by reducing energy consumption and improving coating homogeneity, while allowing for continuous or semi-continuous processing.
Description
Background of the invention
[0001] The present invention relates to the general field of methods for depositing a coating on fibers, and more particularly on a continuous carbon or silicon carbide fiber from a coating precursor.
[0002] Ceramic matrix composites (CMCs), known for their good mechanical properties that make them suitable for structural elements and for maintaining these properties at high temperatures, constitute a viable alternative to traditional metal parts. Their reduced mass compared to their metal equivalents makes them the parts of choice for addressing the issues of increasing efficiency and reducing pollutant emissions from engines in the aeronautics sector.
[0003] Parts made of CMC material comprise a generally continuous fibrous reinforcement in the form of a woven textile, which is densified by a ceramic matrix. The fibrous reinforcement thus comprises long continuous fibers, generally grouped in the form of threads or strands, the orientation of which can be adapted to the main directions of stress on the part during its use. The preform intended to form the fibrous reinforcement must be woven from the strands of continuous fibers to the dimensions of the part (for example by two-dimensional or three-dimensional weaving), using a suitable loom. To produce a part made of CMC material which has improved mechanical properties, it is known to have fibers in the fiber preform which are coated with an interphase, prior to the densification of the preform.
[0004] The deposition of an interphase coating on the fibers of an already woven fiber preform by chemical vapor infiltration (CVI) is known. In addition to the high cost and low kinetics of this technique, the interphase formed on the fibers is generally not homogeneous and strong interphase thickness gradients are observed between the surface and the core of the preform, and locally between the fibers located on the surface and in the core of the yarn or strand. This inhomogeneity of the deposition within the preform has consequences on the final mechanical properties of the densified part, which is not desirable.
[0005] There is therefore a need for a method of depositing a coating on a continuous carbon or silicon carbide fiber that is rapid and forms a homogeneous coating.
[0006] US2011 / 171399 shows a method of depositing a coating by CVI / CVD on a continuous fiber from a coating precursor, the method comprising at least heating a segment of the fiber in the presence of the coating precursor in a microwave field so as to bring the surface of the segment to a temperature allowing the formation of the coating on the segment from the coating precursor. The fiber may be a silicon carbide fiber.
[0007] US6152072 shows the same process for continuous carbon fibers. US5543605 shows the same process for continuous carbon or SiC fibers. Subject matter and summary of the invention
[0008] The main aim of the present invention is therefore to overcome such drawbacks by proposing a method for depositing a coating on a continuous carbon or silicon carbide fiber from a coating precursor, the method comprising at least the heating of a segment of the fiber in the presence of the coating precursor in a microwave field so as to bring the surface of the segment to a temperature allowing the formation of the coating on the segment from the coating precursor.
[0009] A "fiber segment" herein refers to a certain length of fiber, in other words, the segment extends along the length or largest dimension of the fiber. Since a fiber may comprise several filaments, a fiber segment may comprise several filaments. In this disclosure, "surface of the segment" means the surface of each filament that composes the fiber segment, if any. Similarly, "depositing" or "forming" a coating on the fiber segment means depositing or forming the coating on the surface of each filament that composes the fiber segment, if any.
[0010] The method according to the invention is remarkable in particular by the fact that a segment of the continuous fiber is heated by direct coupling via microwaves. The inventors have in fact observed that the long carbon or silicon carbide fiber segment couples with a microwave field, which makes it possible to bring its surface to a temperature sufficient to form the coating from a coating precursor. This arrangement makes it possible to heat the fiber segment as a whole and in particular its surface, and to ensure homogeneous and rapid formation of the coating thereon. Another advantage of the method according to the invention is that the coating precursor can also couple with the microwave field, which increases its temperature and improves both the kinetics of coating formation and its homogeneity.Yet another advantage of the invention is the reduction in the energy required to form the coating, since the fiber segment is heated directly and not an entire reactor. Finally, thanks to the versatility of the process according to the invention, the fiber can be placed in the presence of the precursor in liquid phase, gas phase, or supercritical phase.
[0011] The term "microwave field" means an electromagnetic field with a frequency between several hundred MHz and several GHz. The microwave field can be characterized by its power (or amplitude) and its frequency, which a person skilled in the art can easily determine to obtain a surface temperature of the short fibers sufficient to form the coating. There are in fact a multiplicity of frequency / power couples which make it possible to obtain sufficient coupling between the fiber segment and the microwave field.
[0012] In an exemplary embodiment, the microwave field has a main frequency between 2.35 GHz and 2.55 GHz.
[0013] In an example outside the invention, during the heating step, the fiber segment may be in contact with a liquid phase of the coating precursor and the coating is formed by heating. In this configuration, the liquid phase of the precursor may couple with the microwave field, which increases its temperature, reduces heat dissipation around the fiber segment and thus improves the heating kinetics.
[0014] In an example outside the invention, during the heating step, the fiber segment may be in the presence of a gaseous phase of the coating precursor and the coating may be formed by chemical vapor infiltration. Compared to prior art methods using a gaseous precursor and CVI deposition, this exemplary embodiment of the method improves the formation kinetics and homogeneity of the coating.
[0015] In an example outside the invention, the gas phase of the coating precursor may be obtained by boiling a liquid phase of the coating precursor, the boiling resulting from contact between a hot portion of the fiber adjacent to the segment present in the microwave field and the liquid phase of the coating precursor. The portion of the fiber adjacent to the coating is, in this situation, heated by conduction from the fiber segment present in the microwave field. This technique makes it possible to form the coating on the fiber segment at a reduced pressure, equal to or slightly greater than atmospheric pressure. In addition, the wall of the reactor in which the deposition is carried out is said to be cold compared to a CVI reactor in which the reactor walls must be heated, which makes the process easier to carry out and more energy-efficient.This deposition technique can be seen as a hybrid technique between calefaction and chemical gas infiltration.
[0016] In the invention, during the heating step, the fiber segment is in the presence of a supercritical phase of the coating precursor and the coating is formed by supercritical phase chemical deposition.
[0017] In an exemplary embodiment, when heating the fiber segment, the segment may be in a first position, and the method may further comprise running the fiber so as to move the segment into a second position in which the segment is out of the microwave field. In other words, the method may comprise a step of running the continuous fiber through the microwave field. This advantageous arrangement makes it easier to form the coating over the entire length of the fiber.
[0018] In this case, the fiber scrolling can be carried out continuously or semi-continuously, depending on the deposition kinetics inherent in the variants described previously as well as the precursors involved.
[0019] In an example outside the invention, when using a liquid phase of the precursor, the fiber segment may be in contact with the liquid phase of the coating precursor when it is in the second position. This means that the fiber travels in a direction in which it plunges into the liquid phase once it has been heated. This arrangement is advantageous because it makes it possible, on the one hand, to quickly stop the formation of the deposit on the surface of the filaments constituting the fiber segment and, on the other hand, to quench the fiber segment just after the formation of the coating on the latter, which ensures homogeneity of the coating between two successive segments, and therefore across the entire continuous fiber.
[0020] In one exemplary embodiment, unwinding the fiber may include unwinding the fiber from a first mandrel and winding the fiber onto a second mandrel.
[0021] In an exemplary embodiment, the coating may be an interphase coating. The interphase has a function of weakening the composite material which promotes the deflection of any cracks reaching the interphase after having propagated in the matrix, preventing or delaying the breakage of fibers by such cracks. This interphase also makes it possible to protect the fiber from the matrix material during its formation.
[0022] In particular, the coating may comprise pyrolytic carbon (PyC), boron nitride (BN) or silicon carbide (SiC). The interphase coating may, for example, comprise Si 3 N 4 or SiBN.
[0023] In an exemplary embodiment, the fiber may be made of silicon carbide having an oxygen content of less than or equal to 1% in atomic percentage. For example, such a fiber may be a Hi-Nicalon type S fiber marketed by the Japanese company NGS.
[0024] Mentioned outside the invention is a device for implementing a method of depositing a coating on a continuous fiber from a coating precursor in the liquid phase, in the gas phase or in the supercritical phase, the device comprising a microwave generator configured to generate a microwave field, a reactor configured to be traversed by the continuous fiber and to contain the coating precursor, at least a portion of said reactor being intended to be in the microwave field of the microwave generator, and a device for running the fiber inside the reactor. The device for running the fiber may preferably be located outside the microwave field. It may be ensured that the portion of the reactor in the microwave field is present within an antinode of said field.
[0025] In one exemplary embodiment, the reactor may be substantially U-shaped. The reactor may be a tube. In this case, only a portion of a branch or vertical portion of the reactor may be present in the microwave field.
[0026] In an exemplary embodiment, in particular when the reactor has a U shape, the reactor may comprise at least one element for centering the fiber in the reactor. A centering element may be present at the inlet and / or outlet of the reactor. In a U-shaped reactor, two centering elements may be present in the reactor at the junctions between the horizontal portion and the vertical portions of the U.
[0027] In an exemplary embodiment, the unwinding device may comprise a first mandrel from which the fiber is intended to be unwound and a second mandrel onto which the fiber is intended to be wound.
[0028] In an exemplary embodiment, the microwave field can be obtained using a resonator having a resonant cavity. In this case, the only parameter to be adjusted to modulate the surface temperature of the fibers is the power supplied to the resonator, since the latter generally has a fixed resonant frequency. It is possible to ensure that the continuous fiber and the coating precursor are placed within an antinode of the microwave field, which is the case when using such a resonator and placing the fiber and the precursor in the center of its resonant cavity. Of course, other means for generating microwaves can be used. Brief description of the drawings
[0029] Other characteristics and advantages of the present invention will emerge from the description given below, with reference to the appended drawings which illustrate exemplary embodiments thereof which are not in any limiting nature. In the figures: there figure 1 shows a very schematic example of a device making it possible to implement a method according to a first embodiment, which is not according to the invention, the figure 2 shows the device of the figure 1 in a configuration making it possible to implement a method according to a second embodiment, which is not according to the invention, and the figure 3 shows a very schematic example of a device making it possible to implement a method according to a third or a fourth embodiment, the third not being according to the invention, the fourth if it is according to the invention. Detailed description of the invention
[0030] There figure 1shows a device 100, for implementing a method according to a first embodiment of said by calefaction, that is to say in which the formation of the coating is carried out in the presence of a liquid phase of a precursor of the coating. The device 100 comprises a microwave generator 110, a reactor 120, and a scrolling device 130.
[0031] The microwave generator 110 here comprises a resonator 111 provided with a resonant cavity 112, the resonator 111 is connected to a wave generator 113 by a coaxial cable 114. In operation, the resonant cavity 112 is traversed by a microwave field.
[0032] The reactor 120 may be made of a material transparent to microwaves, for example quartz. The reactor 120 here takes the form of a U-shaped tube having a horizontal part 121, a first vertical part 122 and a second vertical part 123. The second vertical part 123 of the reactor 120 is here present at least in part in the resonant cavity 112 of the resonator 111, that is to say it passes through the resonator 111.
[0033] The reactor 120 here contains a precursor of the coating 140 in liquid phase. In this example, the meniscus 141 of the precursor 140 is located above the cavity 112 of the resonator 111. In other words, the part of the reactor 120 which is present in the cavity 112 is filled with the liquid phase of the precursor 140.
[0034] The reactor 120 is here plugged at the end of the second vertical part 123 by a plug 124 pierced with a central orifice so that it can be crossed by a continuous fiber 150 made of carbon or silicon carbide. The plug 121 also plays here the role of centering element of the fiber 150 in the reactor. The plug 121 may be provided to allow the reactor 120 to be fed by the fiber 150. The reactor 120 is further provided with two centering devices 125 present respectively at the two junctions between the horizontal part 121 and the two vertical parts 122 and 123 of the reactor 120. The centering devices 124 may take the form of small rollers provided with a groove (not visible in the figures) which have the function of keeping the fiber 150 centered in the reactor 120. The centering devices 124 and 125 may have a specific shape allowing the fiber to be spread in order to improve the homogeneity of the deposition on the filaments present in the fiber, if applicable.The centering devices 124 are present inside the reactor 120. The centering devices 124 are thus also centering elements for the fiber 150 in the reactor 120.
[0035] In the illustrated example, the reactor 120 may be provided with a purge valve 126 and means (not shown) for supplying the reactor with precursor of the coating 140 and maintaining a constant level of the latter in the reactor 120.
[0036] The unwinding device 130 here comprises a first mandrel 131 from which the fiber 150 can be unwound, the first mandrel 131 can be a storage mandrel for the fiber 150 before it is coated, and a second mandrel 132 on which the fiber 150 can be wound once coated. The fiber 150 can thus circulate in the reactor 120 from the first mandrel 131 to the second mandrel 132. The centering elements 124, 125 of the fiber 150 in the reactor 120 ensure here that the fiber 150 does not touch the wall of the reactor 120 and that it is taut. The scrolling device 130 can be controlled by control means not shown, so as to scroll the fiber 150 in the device 100 continuously or semi-continuously (i.e., step by step). The scrolling device 130 can scroll the fiber 150 in the device 100 in both directions.
[0037] A first embodiment of the method, which is not according to the invention, will now be described in connection with this device 100. When the microwave generator 110 is in operation, a microwave field is created in the cavity 112. The scrolling device 130 can advance the fiber 150 in the device over a certain distance so that a segment 151 of the fiber 150 is located in the cavity 112. Under the effect of the coupling between the fiber 150 and the microwave field, the segment 151 of fiber present in an area 142 shown in dotted lines on the figure 1(this area being located inside the cavity) is heated, and in particular the surface of the heated fiber segment 151 reaches a temperature sufficient for the precursor of the coating 140 in liquid phase to vaporize locally around the fiber segment 151 and to be deposited on the fiber segment 151 by heating to form the coating. As indicated previously, a person skilled in the art knows how to choose the properties of the microwave field, in particular its frequency and / or its power, to reach the heating temperature of the precursor 140.
[0038] In the example illustrated, the scrolling device 130 scrolls the fiber 150 in the device 100 in the direction indicated by the arrows 133 and 134. More precisely, the fiber 150 scrolls here so that a segment 151 which has just passed through the microwave field continues its path inside the precursor 140 in liquid phase. This arrangement makes it possible on the one hand to quickly stop the formation of the deposit on the surface of the filaments constituting the fiber segment and on the other hand to perform a quenching of the fiber segment on which the coating has just been formed, and ensures homogeneity of formation of the coating over the entire fiber 150. Of course, it is also possible to scroll the fiber 150 in a direction opposite to that illustrated. The coated fiber 150 is then recovered at the end of the first vertical part 122 of the reactor 120 by the second mandrel 132 which can, for example, store it for later use.Alternatively, the fiber 150 thus coated can be directly used to manufacture a fiber preform, for example by weaving.
[0039] There figure 2 shows a device 200 similar to the device 100 of the figure 1 in a configuration allowing to implement a method according to a second embodiment, which is not according to the invention. In this embodiment, the segment 251 of fiber is heated by the microwave field in the presence of a gaseous phase of the precursor of the coating obtained by the boiling of a liquid phase of said precursor. Unless otherwise stated, the corresponding reference signs between the figures 1 And 2 designate identical characteristics which will not be described again.
[0040] Compared to the configuration of the device 100 shown in the figure 1, it is the location of the meniscus 241 of the precursor of the coating 240 in liquid phase which has been modified, as well as the direction of travel of the fiber 250. Indeed, the meniscus 241 is now located just below the cavity 212. In other words, the part of the reactor 220 which is present in the cavity 212 does not contain liquid phase of the precursor 240. Furthermore, as indicated, the direction of travel of the fiber 250 in the device 200 shown diagrammatically by the arrows 233 and 234 has been modified.
[0041] In this example, the meniscus 241 is positioned so that a portion of fiber that is contiguous to the segment 251 of fiber present in the microwave field is also heated by thermal conduction and allows evaporation (by boiling) of the liquid phase of the precursor of the coating 240 at an area 242 shown in dotted lines on the figure 2. The evaporated coating precursor is now present in gaseous form in the portion of the reactor 220 devoid of liquid phase 240 of coating precursor and present in the microwave field. The fiber segment 251 which is present in the microwave field is heated to a temperature sufficient for the gaseous phase precursor to be able to deposit on the fiber segment 251 and form the coating. This technique can be similar to chemical gas infiltration coupled with calefaction. As indicated previously, a person skilled in the art knows how to choose the properties of the microwave field, in particular its frequency and / or its power, to reach the appropriate temperature at the surface of the fiber segment 251 to form the coating from the coating precursor.
[0042] In this example, the direction of travel is preferably that illustrated so that sufficient precursor of the coating 240 in liquid phase is evaporated, but it is possible to travel the fiber 250 in the same direction as that illustrated in the figure 1 In this example, the coating formation can thus be carried out at a pressure in the reactor 220 of the order of atmospheric pressure or at a slightly higher pressure.
[0043] There figure 3shows a third device 300 for implementing a method according to a third embodiment, which is not according to the invention, in which the heated fiber segment is in the presence of a gaseous phase of the coating precursor, or according to a fourth embodiment, which is according to the invention, in which the heated fiber segment is in the presence of a supercritical phase of the coating precursor. The device 300 comprises, in a similar manner to the device 100, a microwave generator 310, a reactor 320 and a scrolling device 330.
[0044] The microwave generator comprises a resonator 311 provided with a resonant cavity 312, the resonator 311 is connected to a wave generator 313 by a coaxial cable 314. In operation, the resonant cavity 312 is traversed by a microwave field.
[0045] The device 300 further comprises a cylindrical reactor 320 provided with an inlet 321 and an outlet 322 for the coating precursor. The reactor 320 may be made of a material transparent to microwaves, for example quartz. At least a portion of the reactor 320 is present in the cavity 312. In the example illustrated, the inlet 321 and the outlet 322 of the reactor 320 are located on either side of the cavity 312. The reactor 320 here contains a precursor of the coating 340 in gaseous or supercritical phase which can circulate in the reactor 320 between the inlet 321 and the outlet 322 of the reactor 320. The reactor 320 further comprises two orifices 323 and 324 through which a fiber 350 can respectively enter and exit the reactor 320, the orifices 323 and 324 here being configured so as not to allow the precursor of the coating 340 to escape from the reactor 320.
[0046] The unwinding device 330 here comprises a first mandrel 331 from which the fiber 350 can be unwound, the first mandrel 331 can be a storage mandrel for the fiber 350 before it is coated, and a second mandrel 332 on which the fiber 350 can be wound once coated. The fiber 350 can thus circulate in the reactor 320 from the first mandrel 331 to the second mandrel 332. The unwinding device 330 can be controlled by control means not shown, so as to unwind the fiber 350 in the device 300 continuously or semi-continuously (i.e. step by step). The unwinding device 330 can unwind the fiber 350 in the device 200 in both directions. In the example illustrated, the fiber 350 moves from bottom to top (arrows 333 and 334), that is to say in a direction opposite to the circulation of the gaseous phase of the coating precursor in the device 300.This particular direction of movement makes it possible to further increase the coating deposition kinetics.
[0047] In this device 300, similarly to the devices 100 and 200, the segment 351 of fiber 350 present in the microwave field is heated so that its surface reaches a sufficient temperature for the gaseous or supercritical phase precursor to be deposited on the segment 351 of fiber to ensure the formation of the coating. As indicated previously, a person skilled in the art knows how to choose the properties of the microwave field, in particular its frequency and / or its power, to reach the appropriate temperature at the surface of the segment 351 of fiber to form the coating from the precursor of the coating. Depending on whether the segment 351 of fiber is in the presence of a gaseous phase or a supercritical phase of the precursor of the coating, each technique for forming the coating can be designated respectively as chemical infiltration in the gaseous phase or chemical deposition in the supercritical phase.The person skilled in the art knows how to choose the conditions, in particular temperature and pressure, of the coating precursor, to ensure the formation of the coating on the fiber segment 351. An advantage in this case is that the walls of the reactor 320 are cold in comparison with reactors used in the prior art to carry out, for example, chemical infiltration in the gas phase. Working with a cold wall offers the opportunity to overcome the standard operating conditions of a conventional CVI process, and makes it possible to achieve significantly higher deposition kinetics, up to two orders of magnitude higher.
[0048] In all the examples presented, the thickness of the coating formed on the fiber segment 151, 251, 351 depends, all other things being equal, on the residence time of the fiber segment 151, 251, 351 in the microwave field in the presence of the coating precursor.
[0049] In all of the examples presented, the coating may be an interphase coating, for example, of silicon carbide, boron nitride, or pyrolytic carbon. For example, a pyrolytic carbon interphase may be formed using a coating precursor such as an alcohol, such as ethanol, a polyalcohol, or toluene. For example, a silicon carbide interphase may be formed using a coating precursor such as methyltrichlorosilane or dimethylchlorosilane. For example, a boron nitride interphase may be formed using a coating precursor such as borazine, or a mixture of BCl 3 and NH 3 .
[0050] The devices 100, 200 and 300 have been presented as being able to accommodate a single fiber 150, 250, 350. Of course, the method can be carried out on several continuous fibers at the same time, for example by feeding the devices 100, 200 and 300 with wires or strands comprising several fibers.
[0051] The continuous fiber coated by a process according to the invention can then be used to manufacture a fiber preform, for example by weaving, which can finally be densified by a matrix. Example (not according to the invention)
[0052] A pyrocarbon interphase is deposited on continuous silicon carbide fibers by a method according to the first embodiment outside the invention, using the device 200 described above. To do this, a strand of Hi-Nicalon type S silicon carbide fibers with a diameter of 10 µm (average diameter of the filaments) is used. The precursor of the coating, ethanol in the liquid phase, is placed in the reactor 220 of the device 200 as illustrated in the figure 2. In the microwave generator used, the resonant cavity of the resonator has a natural frequency of the order of 2.45 GHz and is powered by a power of 15 W. The fiber strand passes through the device 200 at a speed of 10 mm / min. Fibers coated with a homogeneous and continuously deposited pyrocarbon interphase were obtained.
Claims
1. A process for depositing a coating on a continuous fibre (250; 350) of carbon or silicon carbide from a precursor of the coating (240; 340), the process comprising at least: heating a segment (251; 351) of the fibre in the presence of the coating precursor in a microwave field so as to bring the surface of the segment to a temperature allowing the coating to form on the segment from the coating precursor, characterized in that: the segment (351) of fibre (350) is in the presence of a supercritical phase of the precursor of the coating (340) and the coating is formed by supercritical phase chemical deposition.
2. The process as claimed in claim 1, wherein, when heating the segment (251; 351) of fibre (250; 350), the segment is in a first position, and the process further comprises running the fibre so as to move the segment to a second position in which the segment is out of the microwave field.
3. The process as claimed in claim 2, wherein the running of the fibre (250; 350) is carried out continuously or semi-continuously.
4. The process as claimed in claim 2 or 3, wherein the unwinding of the fibre (250; 350) comprises unwinding the fibre from a first mandrel (231; 331) and winding the fibre onto a second mandrel (232; 332).
5. The process as claimed in any one of claims 1 to 4, wherein the coating is an interphase coating.
6. The process as claimed in claim 5, wherein the coating comprises pyrolytic carbon, boron nitride or silicon carbide.
7. The process as claimed in any one of claims 1 to 6, wherein the fibre (250; 350) is silicon carbide having an oxygen content of less than or equal to 1 atomic percent.