Procedure for the determination of white pigment in a layer of paper

ES3084249T3Undetermined Publication Date: 2026-11-11FLOORING TECH LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
ES2023218573T
Authority / Receiving Office
ES · ES
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-12-20
Publication Date
2026-11-11
Estimated Expiration
2043-12-20

AI Technical Summary

Technical Problem

Existing methods for determining the white pigment content and type in paper layers used for wood-based panels are inadequate, leading to sedimentation issues, color deviations, and increased costs due to quality defects, which are not easily detected until later stages of production.

Method used

A method using Near-Infrared (NIR) spectroscopy to determine the quantity and type of white pigment in paper layers by creating a calibration model with multivariate data analysis, allowing continuous and automated monitoring of pigment content during the impregnation process.

Benefits of technology

Enables precise and continuous determination of white pigment content and type, reducing sedimentation issues, improving product quality, and enabling real-time process control, thus minimizing defects and costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000012_0000
    Figure 00000012_0000
  • Figure 00000013_0000
    Figure 00000013_0000
  • Figure 00000014_0000
    Figure 00000014_0000
Patent Text Reader

Abstract

The present invention relates to a method based on NIR spectroscopy for determining the amount of white pigment in a paper layer, in particular the amount and type of white pigment in a paper layer.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to a method for determining the white pigment in a paper layer impregnated with impregnating resin, in particular the type and quantity of white pigment or paper layer. Description

[0002] In the wood-based materials industry, impregnated papers are used extensively for surface finishing of wood-based panels. These are essentially decorative papers, overlays, and backing papers that are pressed onto wood-based panels under high pressure and high temperatures. These coated panels are then used in a wide variety of applications (furniture, interior design, laminate flooring, etc.).

[0003] Especially when using such coated wood-based panels in the furniture industry, the quality of the decorative papers used is of great importance. Even the smallest color variations in the production of front elements can lead to a negative overall impression and thus to complaints.

[0004] Decorative papers are specialty papers used for surface finishing of wood-based materials, offering a wide variety of decorative designs. In addition to typical prints of various wood textures, more elaborate prints of geometric shapes or artistic, decorative designs are available.

[0005] To ensure optimal printability, the paper used as a printing substrate must have good smoothness and dimensional stability. Furthermore, the paper should be as light a color as possible to achieve maximum brilliance. For this reason, decorative designs are preferably printed on light-colored, ideally white, papers.

[0006] An example of a method for investigating white pigments on paper substrates using infrared spectroscopy is given in US patent specification 5,795,394 A. 1

[0007] For this purpose, standard white papers or raw papers, preferably low-grammage papers for cost reasons, are first provided with a base level of white pigmentation. The white pigments are incorporated into the raw papers during the manufacturing process.

[0008] Raw papers are understood to be those papers that have not been subjected to sizing in the bulk or to impregnation of the surface with a resin or glue.

[0009] Raw papers consist essentially of pulp, pigments (preferably white pigments), fillers, and common additives. Softwood pulp, hardwood pulp, or mixtures of both can be used to produce raw papers.

[0010] A variety of inorganic compounds are used as white pigments. However, titanium dioxide remains the primary pigment, as it achieves the highest increase in opacity relative to the amount applied. Other inorganic compounds, such as barium sulfate, zinc oxide, or calcium sulfate, are sometimes added to reduce costs and / or modify the color.

[0011] To increase opacity, these white standard papers or white raw papers are treated with pigmented impregnating resins, so that their whiteness is further increased by impregnation with resins containing white pigment.

[0012] The addition of pigments to impregnating resins such as urea or melamine resin is not without its problems, as the pigments tend to sediment in the impregnation bath. For this reason, the maximum pigment dispersion that can be added to an impregnating resin is approximately 10-20% by weight, while the solids content of the dispersion is typically around 50-60% by weight. However, even highly effective dispersing agents and very fine pigment milling (particle sizes: 3 to 5 µm) used in the dispersions can only slightly reduce, but not completely prevent, the effect of sedimentation. Sedimentation not only leads to losses of the expensive titanium dioxide but also to a change in the whiteness of the paper. This effect is not visible to the naked eye at the impregnation line. Furthermore, it has been observed that once sedimentation has begun in the impregnation tank, it accelerates.

[0013] Changes in whiteness can also occur if errors happen during the formulation and mixing of the pigment-containing impregnating resin. All of this can lead to quality deviations being detected in subsequent process steps, or, even more seriously, to customer complaints (furniture manufacturers, etc.). This is less problematic for materials used in cabinet construction than for panels used to manufacture front elements. It should also be noted that customers today have significantly tightened their guidelines regarding color deviations.

[0014] The resulting disadvantages include color deviations, pigment loss, and the resulting increased costs due to increased rejects and difficult quality control.

[0015] The invention is therefore based on the technical problem of developing a method for determining the white pigmentation, or the quantity and type of white pigment, in or on paper used as a printing base, in order to eliminate quality defects attributable to this parameter. The system technology should not require increased safety standards. Furthermore, the determination should yield the lowest possible error. The determination should be performed continuously and be suitable for automated system control based on this parameter.

[0016] This problem is solved by a method having the features of claim 1.

[0017] Accordingly, a method for determining the white pigment in a paper layer, in particular the quantity and type of white pigment in a paper layer, is provided. The present method comprises the following steps: Providing several layers of paper, each containing different quantitatively defined amounts of white pigment as reference samples; recording at least one NIR spectrum of each of the reference samples using at least one NIR measuring head in a wavelength range between 900 nm and 1700 nm, preferably between 1100 nm and 1700 nm, particularly preferably between 1350 nm and 1650 nm, most preferably between 1400 nm and 1600 nm, and most advantageously between 1450 nm and 1550 nm; assigning the different quantitatively defined amounts of white pigment in the reference samples to the recorded NIR spectra of said reference samples; and creating a calibration model for the relationship between the spectral data of the NIR spectra and the corresponding quantitatively defined amounts of white pigment in the reference samples by means of a multivariate data analysis;Providing at least one sample of a paper layer containing a white pigment to be measured; recording at least one NIR spectrum of the impregnated paper layer using the at least one NIR measuring head in a wavelength range between 900 nm and 1700 nm, preferably between 1100 nm and 1700 nm, particularly preferably between 1350 nm and 1650 nm, most preferably between 1400 nm and 1600 nm, and most advantageously between 1450 nm and 1550 nm; and determining the quantitative amount of the white pigment introduced into the impregnated paper layer in the sample to be measured by comparing the NIR spectrum recorded for the sample to be measured with the calibration model created from the reference samples.

[0018] A measurement method is provided, which is not part of the invention, and which allows for the determination of the type and quantity of a white pigment in a paper layer, in particular a raw paper layer. The measurement method utilizes NIR spectroscopy, which enables the continuous determination of the white pigment contained in a paper layer.

[0019] Using this exemplary measurement method, which is not part of the invention, it is now possible to determine the content and type of white pigment in a layer of raw paper. As already defined, the term "raw paper" refers to a layer of paper that is not (yet) impregnated; i.e., a layer of paper that is not impregnated with an impregnating resin, in particular a formaldehyde resin such as melamine, urea, and / or phenol-formaldehyde resin, or other resins such as melamine ether resins, acrylic resins, or epoxy resins, and thus consists solely of bonded cellulose fibers and, if applicable, additives.

[0020] In this process, the white pigment used in the base paper layers is selected from titanium dioxide, barium sulfate, calcium sulfate, calcium carbonate and / or zinc oxide, or a mixture thereof. Titanium dioxide is the preferred white pigment.

[0021] Accordingly, in one embodiment, a base paper can be used which has a (basic) content of titanium dioxide. Typically, the amount of titanium dioxide in such a white base paper is between 20 and 40 wt%, preferably between 25 and 35 wt% (based on the total paper weight).

[0022] In the case of determining a (single) white pigment in the raw paper layer, first a first NIR spectrum is recorded for a raw paper layer without white pigment and another NIR spectrum for a raw paper layer containing a white pigment, and the quantity and type of white pigment are deduced from the difference.

[0023] To determine the combination of different white pigments in the base paper layer, a NIR spectrum is first recorded for a base paper layer containing a first white pigment (e.g., TiO₂) and another NIR spectrum for a base paper layer containing a first (e.g., TiO₂) and a second white pigment (e.g., BaSO₄ or ZnO). The difference between the values ​​for the paper with the first and second white pigments and the value for the paper with the first (single) white pigment is then calculated, from which the quantity and type of the second white pigment can be determined.

[0024] Determining the type of pigment in a layer of raw paper is important, for example, because pigments such as zinc oxide or calcium carbonate neutralize hardeners used to cure impregnating resins (with which the raw paper layers must be impregnated before further use). This can lead to under-curing of the impregnated paper layers, which cannot be readily explained without knowledge of the pigment composition.

[0025] The use of lower quality (cheaper) pigments can also lead to poorer results in terms of lightfastness or to undesirable interactions when using surface-modifying chemicals in the resin formulation.

[0026] As mentioned above, the whiteness of raw paper is insufficient or inconsistent in certain cases, making its use as a printing base impossible or disadvantageous. Therefore, it is necessary to increase the whiteness of white raw papers or standard white papers by impregnation with a white pigment-containing impregnating resin.

[0027] The amount of white pigment applied to the raw paper can also be determined (in addition to the white pigment contained in the raw paper) using NIR spectroscopy.

[0028] Accordingly, in one embodiment of the invention, a method for determining the amount of white pigment in a paper layer is also provided, wherein the white pigment to be determined is introduced into the paper layer during impregnation with an impregnating resin. The present method comprises the following steps:Impregnating several layers of paper with an impregnating resin, each containing different quantitatively defined amounts of white pigment as reference samples; recording at least one NIR spectrum of each of the reference samples using at least one NIR measuring head in a wavelength range between 900 nm and 1700 nm, preferably between 1100 nm and 1700 nm, particularly preferably between 1350 nm and 1650 nm, most preferably between 1400 nm and 1600 nm, and most advantageously between 1450 nm and 1550 nm; assigning the different quantitatively defined amounts of white pigment in the reference samples to the recorded NIR spectra of said reference samples; and creating a calibration model for the relationship between the spectral data of the NIR spectra and the corresponding quantitatively defined amounts of white pigment in the reference samples by means of a multivariate data analysis;Providing at least one sample of impregnated paper to be measured by impregnating at least one paper layer with an impregnating resin containing a white pigment; recording at least one NIR spectrum of the impregnated paper layer using the at least one NIR measuring head in a wavelength range between 900 nm and 1700 nm, preferably between 1100 nm and 1700 nm, particularly preferably between 1350 nm and 1650 nm, most preferably between 1400 nm and 1600 nm, and most advantageously between 1450 nm and 1550 nm; and determining the quantitative amount of the white pigment introduced into the impregnated paper layer in the sample to be measured by comparing the NIR spectrum recorded for the sample to be measured with the calibration model created from the reference samples.

[0029] In one embodiment, a measuring method is provided that allows for the determination of the quantity of a white pigment that is incorporated into or applied to a layer of paper along with the impregnating resin during an impregnation process. The measuring method utilizes NIR spectroscopy, which enables the continuous determination of the white pigment applied during the impregnation process.

[0030] For example, the NIR measuring head determines the sum of the white pigment already present in the raw paper and the additional white pigment introduced into the raw paper through impregnation. The difference is then calculated from this sum and the value for the unpigmented paper.

[0031] As will be explained in more detail later, calibration values ​​are created for the present process in order to establish a correlation with the spectra determined via NIR. This makes it possible to infer unknown quantities of white pigment, such as titanium dioxide, in or on the paper layer. Furthermore, this calibration enables process monitoring. This can, for example, provide quality data across the entire web width in real time and allow for rapid intervention in the event of deviations.

[0032] This method also allows for the analysis of competitor products, faster processing of complaints, and support of product development. The spectroscopic data can be used to analyze not only order volume but also order fluctuations.

[0033] In one embodiment of the present method, it is provided that the white pigment to be determined is introduced into the paper layer during a core impregnation (or pre-impregnation) of the paper layer.

[0034] The term "core impregnation" or "pre-impregnation" refers to the impregnation of the paper core, whereby the impregnating resin penetrates the paper layer. In this case, the paper layer is completely or partially saturated with the impregnating resin.

[0035] The "core impregnation" or "pre-impregnation" process in the production of impregnated materials involves applying the impregnating resin (in this case, mixed with a white pigment) to a first impregnation tank. After immersion, the resin is scraped off to a defined thickness using doctor blades or squeeze rollers. The pre-impregnated material is then dried with hot air in a suspended dryer (intermediate drying). This can be followed by surface impregnation of the pre-impregnated material and a further drying step. Each drying step reduces the water content of the paper layer, preferably to 10-20% by weight. Equipment suitable for such impregnations is known. For example, reference is made to EP 3075906 B1, which describes an impregnation plant consisting of a first impregnation station with a downstream drying station and a second impregnation station with a downstream drying station.

[0036] The determination of the amount of white pigment absorbed by the paper layer during core or pre-impregnation using NIR spectroscopy can be carried out after the first impregnation and drying step (i.e., after pre-impregnation), or after the second impregnation and drying step (i.e., after surface impregnation), the latter being preferred.

[0037] The present method requires only a single NIR measurement to determine the quantity and type of white pigment in or on the paper layer. Another advantage is that the measurement is performed on a continuous sheet of paper, meaning the paper layer is not damaged.

[0038] According to the present procedure, reference samples of paper layers are first provided, each containing different quantitatively defined amounts of white pigment and / or impregnated with an impregnating resin containing different quantitatively defined amounts of white pigment. It is essential that the reference sample is identical to the sample being measured. Thus, the impregnating resin of the reference sample should have the same composition as the impregnating resin being measured. The similarity between the sample being measured and the reference sample can be particularly important when using impregnating resins with additives such as flame retardants, fibers, or other additives.

[0039] At least one NIR spectrum is recorded from these reference samples in a wavelength range between 900 nm and 1700 nm, preferably between 1100 nm and 1700 nm, particularly preferably between 1350 nm and 1650 nm, most preferably between 1400 nm and 1600 nm, and most advantageously between 1450 nm and 1550 nm.

[0040] The known quantitative composition of the raw paper layer and / or the impregnating resin (i.e., the known white pigment content) is then assigned to the respective recorded NIR spectra of these reference samples. In other words, the different quantitatively defined amounts of white pigment in the reference samples are assigned to the recorded NIR spectra of these reference samples. A calibration model for the relationship between the spectral data of the NIR spectra of the reference samples and the corresponding parameter values ​​is created using multivariate data analysis; that is, each parameter value of the reference sample corresponds to a specific NIR spectrum of the reference sample. The calibration models created for the various parameters are stored in a suitable data repository.

[0041] Subsequently, at least one (raw) paper layer is provided with an unknown quantity of white pigment and / or impregnated with an impregnating resin containing an unknown quantity of white pigment, and the (raw) paper layer and / or impregnated paper layer is measured as a sample. For this purpose, at least one NIR spectrum of the sample to be measured is recorded using at least one NIR measuring head in a wavelength range between 900 nm and 1700 nm, preferably between 1100 nm and 1700 nm, particularly preferably between 1350 nm and 1650 nm, most preferably between 1400 nm and 1600 nm, and most advantageously between 1450 nm and 1550 nm.

[0042] The quantitative amount of white pigment contained in the (raw) paper layer and / or of white pigment introduced into the impregnated paper layer in the respective sample to be measured can then be determined by comparing the NIR spectrum recorded for the sample to be measured with the calibration model created from the reference samples.

[0043] A comparison and interpretation of the NIR spectra is best performed across the entire recorded spectral range. This is advantageously carried out using a well-established multivariate data analysis (MDA). Multivariate analysis methods typically examine several statistical variables simultaneously in a well-established manner. These methods usually reduce the number of variables contained in a dataset without diminishing the information it provides.

[0044] In this case, multivariate data analysis is performed using partial least squares regression (PLS), which allows for the creation of a suitable calibration model. The evaluation of the obtained data is preferably carried out using appropriate analysis software, such as SIMCA-P from Umetrics AB or The Unscrambler from CAMO.

[0045] In a further embodiment, it is provided that spectral data from the NIR spectral range between 1400 nm and 1600 nm, preferably between 1450 and 1550 nm and / or between 1150 and 1300 nm, are used for the creation of the calibration model, which are pretreated using suitable mathematical methods and then subjected to multivariate data analysis.

[0046] The significance of a wavelength for predicting the resin ratio from the NIR spectrum is illustrated using regression coefficients. Regions with large coefficient values ​​have a strong influence on the regression model. For example, the representation of regression coefficients in a PLS regression model for determining the quantity and type of white pigment shows that the wavelength range between 1450 nm and 1550 nm, with a maximum at 1480–1490 nm, is most important for the model calculation, as the regression coefficient values ​​are highest in this range. While other regions of the spectrum contain less information related to the NIR measurement, they nevertheless contribute to considering and minimizing other information and interfering factors (such as layer transparency, substrate surface properties, etc.).

[0047] To eliminate interfering influences (such as the surface properties of the substrate material, sample color, light scattering by solid particles or other additives, etc.), it is necessary to process the spectral data using mathematical pretreatment methods (e.g., derivative data pretreatment, standardization according to SNVT (Standard Normal Variate Transformation), multiplicative signal correction (EMSC, Extended Multiplicative Signal Correction, etc.). This removes baseline effects, which are mainly caused by the different sample colors, from the spectra, separates overlapping bands, and takes into account the dependence of light scattering at the substrate surface or at the solid particles in the coating.

[0048] From the pre-treated data, a calibration model is developed using multivariate data analysis, which includes all decors used in the calibration.

[0049] Accordingly, the comparison and interpretation of NIR spectra are preferably carried out in the spectral range between 1450 and 1550 nm using multivariate data analysis (MDA). Multivariate analysis methods typically examine several statistical variables simultaneously in a manner known per se. For this purpose, the number of variables contained in a dataset is reduced without simultaneously diminishing the information it contains.

[0050] Titanium dioxide is also preferably used alone as a white pigment to increase the whiteness of paper layers through impregnation. However, it can also be used in combination with other white pigments, particularly in combination with barium sulfate and / or zinc oxide. Preferred combinations are titanium dioxide and barium sulfate or titanium dioxide and zinc oxide. A combination of titanium dioxide, barium sulfate, and zinc oxide is also possible.

[0051] The particle size of the white pigment used in the impregnating resin is between 1 and 10 µm, preferably between 2 and 8 µm, and particularly preferably between 3 and 5 µm.

[0052] In a further embodiment of the present method, it is provided that the impregnating resin contains between 1.0 and 10.0 wt% titanium dioxide as a white pigment (based on the total amount of impregnating resin), preferably between 2.0 and 8.0 wt% titanium dioxide, and particularly preferably between 3.0 and 5.0 wt% titanium dioxide.

[0053] For this purpose, between 2 and 20 wt%, preferably between 4 and 16 wt%, and particularly preferably between 6 and 10 wt%, of a titanium dioxide dispersion with a titanium dioxide solids content of 50 wt% is added to the impregnating resin. Preferred amounts are 5, 10, or 15 wt% of an approximately 50 wt% titanium dioxide dispersion.

[0054] In another embodiment, the impregnating resin contains between 5 and 10 wt% barium sulfate and / or zinc oxide as a white pigment, alone or in combination with titanium dioxide. Accordingly, preferably 10 or 20 wt% of a dispersion with a solids content of approximately 50 wt% barium sulfate and / or zinc oxide is added to the impregnating resin.

[0055] In a further embodiment, the at least one impregnating resin containing the white pigment for the core or pre-impregnation of the paper layer is a formaldehyde resin, in particular a urea-formaldehyde resin, a melamine-formaldehyde resin or a mixture thereof, in particular preferably a urea-formaldehyde resin.

[0056] If a mixture of melamine-formaldehyde resin and urea-formaldehyde resin is used for core or pre-impregnation, the quantitative ratio of melamine-formaldehyde resin and urea-formaldehyde resin in the resin mixture used can be between 90 wt% : 10 wt% and 10 wt% : 90 wt%, preferably between 75 wt% : 25 wt% and 25 wt% : 75 wt%, and particularly preferably between 55 wt% : 45 wt% and 45 wt% : 55 wt%.

[0057] The resin application for the core or pre-impregnation of the paper layer is 80 to 100 wt%, preferably 85 to 95 wt%, particularly preferably 90 wt%.

[0058] In a further preferred embodiment, the pre-impregnated or core-impregnated paper layer is surface-impregnated with at least one further impregnating resin. The impregnating resin used for surface impregnation may also contain a white pigment. However, it is preferred if the impregnating resin used for surface impregnation does not contain a white pigment.

[0059] The impregnating resin used for surface impregnation is also a formaldehyde resin, in particular a melamine-formaldehyde resin.

[0060] The resin application for surface impregnation of the paper layer is 30 to 50 wt%, preferably 35 to 45 wt%, particularly preferably 40 wt%.

[0061] The total resin application for core impregnation and surface impregnation is therefore 110 to 150 wt%, preferably 120 to 140 wt%, particularly preferably 130 wt%.

[0062] In a further embodiment, the paper layer to be measured and / or impregnated has a paper weight between 50 and 100 g / m², preferably between 60 and 80 g / m², and in particular between 65 and 75 g / m².

[0063] In a particularly preferred embodiment, the paper layer to be impregnated consists of raw paper. The term "raw paper" refers to paper that is not (yet) impregnated; i.e., a paper layer that is not impregnated with an impregnating resin, in particular a formaldehyde resin such as melamine, urea, and / or phenol-formaldehyde resin, or other resins such as melamine ether resins, acrylic resins, or epoxy resins, and thus consists solely of bonded cellulose fibers and, optionally, additives.

[0064] As mentioned above, impregnation with a white pigment-containing impregnating resin increases the whiteness of standard white papers. Accordingly, in one embodiment, a base paper can be used for impregnation that already has a (basic) titanium dioxide content. Typically, the amount of titanium dioxide in such a white base paper is between 25 and 35 wt% (based on the total paper weight).

[0065] The present method for determining the amount of white pigment in a (raw) paper layer and / or impregnated paper layer can be carried out continuously and online in a production line, in particular in an impregnation plant.

[0066] The determination of the amount of white pigment in a (raw) paper layer is advantageously carried out upstream of an impregnation plant, e.g. at the unwinding of the paper layer before the impregnation plant or during the incoming goods inspection in the laboratory.

[0067] A system for impregnating at least one layer of paper passing through the system includes Optional paper unwinding and changing device; a first impregnation station for pre-impregnation (core impregnation) of at least one paper layer with an impregnating resin containing a white pigment; a second impregnation station for surface impregnation of the at least one pre-impregnated paper layer, wherein at least one NIR measuring head, in particular at least one NIR multi-measuring head, is provided after the second impregnation station for recording at least one NIR spectrum of the paper layer impregnated with the white pigment, and optionally a clipper and discharge table.

[0068] The NIR measuring head is preferably arranged so that the top side of the impregnated paper layer is irradiated. However, it is also generally possible to provide additional NIR measuring heads in the impregnation system for measuring the top and bottom sides of the impregnated paper layer.

[0069] The NIR measuring head can be located after core impregnation, either before or after the first dryer. Another possibility would be after the second dryer, before the clipper.

[0070] It is particularly preferred if the at least one NIR measuring head traverses the width of the paper layer and analyzes specific problem areas (e.g., in the edge or center of the sheets, etc.). Accordingly, the at least one NIR measuring head moves transversely to the direction of travel of the (pre-)impregnated paper layer. Furthermore, the measured values ​​are immediately available and allow for immediate intervention in the process. This is not readily possible with other methods.

[0071] In one embodiment of the present impregnation system, a first drying station is provided after the first impregnation station, wherein the at least one NIR measuring head is arranged after the first drying station.

[0072] In a more specific embodiment, the impregnation plant comprises impregnation troughs or impregnation immersion baths (as impregnation stations), optionally a breathing zone, a doctor blade system / pair of squeeze rollers for removing excess resin, at least one dryer (e.g. a floating dryer), optionally a grid system and an optional second dryer, at least one cooling device (e.g. a cooling roller system).

[0073] This provides a method in which the amount of white pigment in a (pre-)impregnated paper layer can be determined from an NIR spectrum using a non-contact measurement with an NIR measuring head. In an advantageous embodiment of the invention, the data obtained with the measuring head(s) are used directly for plant control or regulation.

[0074] Furthermore, in another advantageous embodiment of the invention, data storage enables improved quality control. The stored data can also advantageously contribute to the evaluation of plant trials, for example, during the commissioning of a new plant, after maintenance or repair, or for in-situ testing of new production or measurement processes. The immediate availability of the measured values ​​and the high measurement frequency allow for very close monitoring, control, and regulation of the plants.

[0075] This method enables the rapid provision of measurement data (online, preferably without disruptive delays) compared to conventional (known) measurement methods. The measurement data can be used for quality assurance, research and development, process control, process regulation, process management, etc. The measurement process does not reduce production speed or other factors. In principle, this improves production monitoring. Furthermore, downtime due to quality control and equipment adjustments is also reduced.

[0076] The advantages of the present method are manifold: Non-contact multi-parameter determination ("real time" or "real-time" measurement) with significantly reduced time delay in the evaluation of the measured parameter values; improved plant control and regulation, reduction of scrap, improvement of the quality of the products manufactured on the plant, improvement of plant availability.

[0077] The control system of the impregnation plant comprises at least one computer-aided evaluation unit (or processor unit) and a database. The evaluation unit compares the NIR spectrum measured for the product (i.e., the pressed porous coating material) with the calibration models created for each individual parameter. The parameter data determined in this way are stored in the database.

[0078] The data determined using the present spectroscopic method can be used to control the impregnation plant. The non-contact measured parameter values ​​of the NIR multi-sensor head ("actual values") can, as previously described, be used directly and in real time for controlling the plant. This is achieved, for example, by storing the measured actual values ​​in a database (e.g., a relational database) and comparing them with the target values ​​for these parameters. The resulting differences are then used to control the production line.

[0079] For the calibration and control of the impregnation plant, a computer-implemented procedure and a computer program comprising commands are provided. These commands, when executed by a computer, cause the computer to carry out the computer-implemented procedure. The computer program is stored in a memory unit of the impregnation plant's control system.

[0080] The invention is explained in more detail below using exemplary embodiments with reference to the figures. The figures show: Figure 1 NIR spectra of raw paper sheets containing titanium dioxide, of paper sheets impregnated with titanium dioxide and reference samples, Figure 2 NIR spectra of paper sheets impregnated with titanium dioxide and reference samples, and Figure 3 NIR spectra of paper sheets impregnated with titanium dioxide and zinc oxide / barium sulfate and reference samples. Example of implementation 1:

[0081] A white (raw) decorative paper (paper basis weight: 65 g / m²< ), which had a titanium dioxide content of approx. 25 wt%, was first impregnated with a urea resin (core impregnation) and then with a melamine resin (surface impregnation) (total resin application: 130 wt%, urea resin: 90 wt%, melamine resin: 40 wt%), intermediately dried and pressed onto a chipboard in a laboratory press (standard 65 g / m²< ).

[0082] Additionally, an overlay without white pigment (paper weight: < 35 g / m²) was impregnated with the same resins. The resin application was 400 wt%. The resin distribution was analogous to that of the white papers. The pigment-free overlay served as a reference sample or zero sample (overlay without TiO₂). It was pressed onto a particleboard under the same conditions.

[0083] Two further samples were then produced using the decorative paper with a basis weight of 65 g / m². For these samples, 5% and 15% wt% of a titanium dioxide dispersion (titanium dioxide content: approx. 50% wt%) were added to the urea resin used for core impregnation. The melamine resin for surface impregnation did not contain any titanium dioxide dispersion. The impregnation process was analogous to the first impregnation. The total resin application was also approx. 130% wt. These two impregnated materials were also pressed onto a particleboard panel in the laboratory press under identical conditions (Fentak 17-5% TiO₂, Fentak 17-15% TiO₂).

[0084] NIR spectra of the reference sample and the three sample samples were then recorded (see NIR spectrum of the Figure 1 As it turned out, the different titanium dioxide contents are clearly recognizable in the spectrum. Example 2:

[0085] A white decorative paper (paper weight: 65 g / m²) with a titanium dioxide content of approximately 25% was first impregnated with a urea resin (core impregnation) and then with a melamine resin (surface impregnation) (total resin application: 130 wt%, urea resin: 90 wt%, melamine resin: 40 wt%), intermediately dried, and pressed onto a particleboard in a laboratory press. This served as a reference sample or zero sample (standard 65 g / m²).

[0086] Two further samples were then produced using the decorative paper with a basis weight of 65 g / m². For these samples, 5% and 15% wt% of a titanium dioxide dispersion (titanium dioxide content: approx. 50% wt%) were added to the urea resin used for core impregnation. The melamine resin for surface impregnation did not contain any titanium dioxide dispersion. The impregnation process was analogous to the first impregnation. The total resin application was also approx. 130% wt. These two impregnated materials were also pressed onto a particleboard panel in the laboratory press under identical conditions (Fentak 17-5% TiO₂, Fentak 17-15% TiO₂).

[0087] NIR spectra of the reference sample and the two sample samples were then recorded (see NIR spectrum of the Figure 2 As it turned out, the different titanium dioxide contents are clearly recognizable in the spectrum. Example 3:

[0088] A white decorative paper (paper weight: 65 g / m²) with a titanium dioxide content of approximately 25 wt% was first impregnated with a urea resin (core impregnation) and then with a melamine resin (surface impregnation) (total resin application: 130 wt%, urea resin: 90 wt%, melamine resin: 40 wt%, moisture content: approx. 6 g / kg). Ten percent of a titanium dioxide dispersion (titanium dioxide content: approx. 50 wt%) was added to the urea resin used for core impregnation. The paper was partially dried and then pressed onto a particleboard in a laboratory press (base sample, Fen-19-10%-1).

[0089] Further samples were then produced using decorative paper with a basis weight of 65 g / m². The melamine resin used for surface impregnation again did not contain titanium dioxide dispersion. The impregnation process was analogous to the first impregnation. The resin application was also approximately 130 wt% and the moisture content approximately 6 wt%. The proportion of urea and melamine resin also remained the same. Titanium dioxide dispersions with 10 wt% and 20 wt% zinc oxide and barium sulfate, respectively, were then prepared and used analogously to the first impregnation. These four impregnating agents were also pressed onto a particleboard panel in the laboratory press under identical conditions (Fen-19-10%-Ba10%, Fen-19-10%-Ba20%, Fen-19-10%-Zn10%, Fen-19-10%-Zn20%).

[0090] NIR spectra of the one reference sample and the four sample samples were then recorded (see NIR spectrum of the Figure 3As it turned out, the different levels of zinc oxide and barium sulfate are clearly visible in the spectrum.

Claims

1. A method for determining white pigment in a paper layer impregnated with impregnating resin, in particular the amount and type of white pigment in the paper layer, comprising the steps - providing a plurality of paper layers impregnated with impregnating resin, each containing different quantitatively defined amounts of white pigment, as reference samples; - recording at least one NIR spectrum of each of the reference samples using at least one NIR measuring head in a wavelength range between 1350 nm and 1650 nm, most preferably between 1400 nm and 1600 nm, and particularly advantageously between 1450 nm and 1550 nm; - assigning the different quantitatively defined amounts of white pigment in the reference samples to the recorded NIR spectra of said reference samples; and - creating a calibration model for the relationship between the spectral data of the NIR spectra and the corresponding quantitatively defined amounts of white pigment in the reference samples using multivariate data analysis; - providing at least one sample of a paper layer containing white pigment to be measured; - recording at least one NIR spectrum of the impregnated paper layer using the at least one NIR measuring head in a wavelength range between 1350 nm and 1650 nm, most preferably between 1400 nm and 1600 nm, particularly advantageously between 1450 nm and 1550 nm; and - determining the quantitative amount of the white pigment introduced into the impregnated paper layer in the sample to be measured by comparing the NIR spectrum recorded for the sample to be measured with the calibration model created from the reference samples.

2. Method according to claim 1, characterized in that the amount of white pigment is determined in a paper layer, wherein the white pigment to be determined is introduced into the paper layer during impregnation of the paper layer with an impregnating resin, comprising the steps - impregnating a plurality of paper layers with an impregnating resin, each containing different quantitatively defined amounts of the white pigment, as reference samples; - recording at least one NIR spectrum of each of the reference samples using at least one NIR measuring head in a wavelength range between 1350 nm and 1650 nm, most preferably between 1400 nm and 1600 nm, particularly advantageously between 1450 nm and 1550 nm; - assigning the different quantitatively defined amounts of white pigment in the reference samples to the recorded NIR spectra of said reference samples; and - creating a calibration model for the relationship between the spectral data of the NIR spectra and the corresponding quantitatively defined amounts of white pigment in the reference samples using multivariate data analysis; - providing at least one sample of an impregnated paper layer to be measured by impregnating at least one paper layer with an impregnating resin containing a white pigment, - recording at least one NIR spectrum of the impregnated paper layer using the at least one NIR measuring head in a wavelength range between 1350 nm and 1650 nm, most preferably between 1400 nm and 1600 nm, particularly advantageously between 1450 nm and 1550 nm; and - determining the quantitative amount of the white pigment introduced into the impregnated paper layer in the sample to be measured by comparing the NIR spectrum recorded for the sample to be measured with the calibration model created from the reference samples.

3. Method according to one of the preceding claims, characterized in that the white pigment to be determined comprises titanium dioxide, barium sulfate, calcium sulfate, and / or zinc oxide, or a mixture thereof, in particular titanium dioxide.

4. Method according to claims 2-3, characterized in that the white pigment to be determined is introduced into the paper layer during core impregnation (or preimpregnation) of the paper layer.

5. Method according to one of claims 2-4, characterized in that the impregnating resin contains between 1.0 and 10.0 wt% (based on the total amount of impregnating resin) of titanium dioxide as a white pigment, preferably between 2.0 and 8.0 wt% of titanium dioxide, and most preferably between 3.0 and 5.0 wt% of titanium dioxide.

6. Method according to one of claims 2-5, characterized in that the impregnating resin contains between 5 and 10 wt% of barium sulfate and / or zinc oxide as a white pigment.

7. Method according to one of claims 2-6, characterized in that the at least one impregnating resin containing the white pigment is a formaldehyde resin, in particular a urea-formaldehyde resin, a melamine-formaldehyde resin, or a mixture thereof, particularly preferably a urea-formaldehyde resin.

8. Method according to one of claims 2-7, characterized in that the pre-impregnated / core-impregnated paper layer is surface-impregnated with at least one additional impregnating resin.

9. Method according to claim 8, characterized in that the impregnating resin for surface impregnation does not contain any white pigment.

10. Method according to claim 8 or 9, characterized in that the impregnating resin used for surface impregnation is a formaldehyde resin, in particular a melamine-formaldehyde resin.

11. Method according to any of the preceding claims, characterized in that the paper layer has a basis weight of between 50 and 100 g / m2, preferably between 60 and 80 g / m2, and in particular between 65 and 75 g / m2.

12. Method according to one of the preceding claims, characterized in that the determination of the amount of white pigment in the paper layer is performed continuously and online.

13. Method according to one of the preceding claims, characterized in that spectral data from the entire recorded spectral range are used to create the calibration model.

14. Method according to one of the preceding claims, characterized in that spectral data from the NIR spectral range between 1400 nm and 1600 nm, preferably between 1450 and 1550 nm, are used to create the calibration model, which data are preprocessed using suitable mathematical methods and subsequently subjected to multivariate data analysis.