CROSS-CUTTING SILYL-TERMINATED POLYMER COMPOSITION AND SUBSTRATE ASSEMBLY PROCESS IMPLEMENTING IT

A crosslinkable adhesive composition with hydrolyzable alkoxysilane groups addresses sagging and safety issues in polyurethane-based adhesives, providing a uniform, strong, and heat-resistant joint at lower temperatures and ambient humidity, enhancing assembly efficiency and safety.

FR3125053B1Active Publication Date: 2024-11-01BOSTIK SA(FR)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
FR2021007429
Authority / Receiving Office
FR · FR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-07-08
Publication Date
2024-11-01
Estimated Expiration
2041-07-08

AI Technical Summary

Technical Problem

Existing semi-structural adhesives face issues such as sagging, high crosslinking time, and the need for controlled humidity and temperature conditions, particularly in the assembly of automobile parts, due to the use of polyurethane-based adhesives with alkoxysilane terminals, which also pose safety risks from volatile diisocyanates and emit carbon dioxide.

Method used

A crosslinkable adhesive composition comprising a polymer with hydrolyzable alkoxysilane groups, tackifying resin, fumed silica, and a crosslinking catalyst, which can be applied at lower temperatures and ambient humidity, forming a uniform and strong adhesive joint with improved heat resistance and mechanical strength.

Benefits of technology

The composition significantly reduces sagging, shortens crosslinking time, and enhances the adhesive joint's cohesion and heat resistance, allowing for efficient assembly without the need for controlled humidity or high temperatures, while being safer and more productive.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

1) A crosslinkable adhesive composition comprising: - at least one polymer (A) comprising a hydrolyzable alkoxysilane group; - at least one tackifying resin (B); - at least one fumed silica (C), preferably hydrophobic; and - at least one crosslinking catalyst (D). 2) Use of said composition for the semi-structural bonding of two substrates. 3) A method for bonding two substrates comprising: - melting said composition by heating to a temperature of 30 to 130°C, then - deposition on a surface of a first substrate, then - crosslinking it by heating to a temperature of 15 to 200°C and bringing said surface into contact with a surface of a second substrate.
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: CROSSLINKABLE COMPOSITION OF SILYL-TERMINATED POLYMER AND METHOD FOR ASSEMBLING SUBSTRATES USING IT FIELD OF THE INVENTION

[0001] The present invention relates to a novel crosslinkable adhesive composition based on a polymer comprising at least one hydrolyzable alkoxysilane group. It also relates to its use as a semi-structural adhesive for the assembly of two substrates. Finally, it relates to a method for assembling two substrates by bonding, which comprises the deposition of said composition, in particular in the form of a bead, on a surface of one of the two substrates to be assembled. TECHNICAL BACKGROUND

[0002] In many industrial fields, adhesives are used for the semi-structural assembly of the most diverse substrates. Semi-structural assembly is understood to mean an assembly of two substrates in which the adhesive joint is capable of withstanding shear stresses in a range from 2 to 8 MPa.

[0003] For example, in automobile construction, adhesives play a major role in the manufacture and assembly of various equipment intended for cars, as well as in the fixing of said equipment or various elements on the chassis, with a view to covering the bodywork to form the passenger compartment. This may therefore involve the interior trim of the doors, the roof, the floor, the trunk or even the assembly of the seats or windshields. Other elements such as filters, such as the air filter, are also fixed by means of adhesives, near the engine.

[0004] Thus, all kinds of substrates can be assembled together using semi-structural adhesives, and / or fixed to the metal chassis of cars, on automated production lines.

[0005] Hot melt adhesives are commonly used for this type of application.

[0006] Hot melt adhesives are solvent-free adhesives which are solid or highly viscous at room temperature and which are applied, in the molten state, at a temperature ranging from 150°C to 210°C, to the substrate to be fixed and / or joined. After cooling, the adhesive returns to the solid state and thus forms, at the end of a physical process, a cohesive adhesive joint which secures the two substrates to be joined. Said adhesive joint can thus withstand shear stresses in a range ranging from approximately 2 to 8 MPa. Hot melt adhesives are generally in the form of compositions which comprise a thermoplastic polymer and possibly actually a tackifying resin and a plasticizer.

[0007] For the purpose of forming an assembly, hot-melt adhesives are often deposited in the form of a bead on a surface of a first substrate. Such a bead is obtained by extruding the adhesive hot through a die connected either to a cartridge handled by an operator, or to a reservoir (in the case of robotic application on an assembly line). The bead can thus be positioned precisely on the surface of the first substrate, at the desired location for assembly with a surface of a second substrate. The diameter of the bead can also be adjusted in a range ranging for example from 2 mm to 2 cm, depending on the desired quantity for coating, for the purpose of forming the adhesive joint.

[0008] The disadvantage of hot-melt adhesives is, however, that, due to the very presence of a thermoplastic polymer in the adhesive joint, the latter has, in the final assembly and the article containing it, a heat resistance which, during the lifetime of the assembly, may prove insufficient depending on the temperature and stress conditions to which said assembly is exposed. Another disadvantage of hot-melt adhesives is also their very high application temperature, as defined above.

[0009] This is the reason why reactive (or crosslinkable) hot-melt adhesives have been developed and are commonly used in various industrial fields, including the field of semi-structural assembly and / or the field of automobile construction.

[0010] Crosslinkable hot-melt adhesives are also solid or very viscous at room temperature, and applied hot to a substrate. After cooling, such an adhesive therefore also regains its solid form, thus giving an initial cohesion to the adhesive joint which is often referred to in the art by the English term “green strength”. In addition, the cohesion of said joint is considerably reinforced under the effect of a chemical crosslinking reaction which takes place in the presence of moisture present in the ambient air and / or on the surface of the substrates to be assembled. Before crosslinking, the constituent composition of the adhesive joint remains thermoplastic and can be re-melted and re-solidified.After crosslinking, the polymer chains included in the adhesive composition are chemically bonded to each other to form a three-dimensional network, with the consequence that the adhesive joint is no longer thermoplastic but in an irreversible solid form.

[0011] Such a crosslinked adhesive composition thus gives the adhesive joint a final cohesion and a heat resistance which are significantly improved compared to a non-reactive hot-melt adhesive.

[0012] Reactive hot melt adhesives are generally moisture curing polyurethane hot melt adhesives, also referred to as HMPUR (for Hot Melt Polyurethane). The reactive part of the corresponding composition consists of an isocyanate-terminated polyurethane prepolymer that reacts with moisture, such that the polymer chains are linked by a urea bond to form a three-dimensional network. Isocyanate-terminated polyurethane prepolymers are conventionally prepared by reacting diols with excess diisocyanates. These HMPURs can be conveniently processed in the form of beads, and have the advantages of a high crosslinking speed, excellent mechanical properties for the adhesive joint after crosslinking and adhesion to a wide variety of substrates.

[0013] These HMPURs, however, have a drawback linked to the presence, in the adhesive composition, of significant residual quantities of the more volatile diisocyanates, which are used in the preparation of the polyurethane prepolymer with isocyanate ends. In the application temperature range (typically around 90-100 °C), the unreacted monomeric diisocyanates contained in the adhesive composition have a considerable vapor pressure and can be released in gaseous form. These diisocyanate vapors can be toxic, in particular irritant, so that safety measures must be taken in the industrial process for implementing the HMPUR. In addition to this toxicity problem, the HMPURs emit carbon dioxide during the crosslinking reaction. The formation of carbon dioxide in amorphous adhesives can lead to the formation of bubbles in the adhesive joint during crosslinking.

[0014] Reactive hot-melt adhesive compositions comprising a polymer comprising at least one hydrolyzable alkoxysilane group have been developed as an alternative to HMPURs. Mention may thus be made of adhesive compositions based on silane-modified polymers (MS Polymers or MS Polymers for "Modified Silane Polymers" in English) with a high filler content, well known in the field of adhesives, which are used for the bonding assembly of a wide variety of objects. MS polymers are polymers whose main chain is a polyether, such as a poly(oxypropylene), and which comprise at least one, preferably two silyl (or alkoxysilane) terminal groups.

[0015] The adhesive joints obtained from such adhesive compositions therefore result from a crosslinking reaction of the polymer chains, via the alkoxysilane terminal group, in the presence of atmospheric humidity or humidity present on the surface of the substrates. These joints thus comprise a three-dimensional polymer network in which the polymer chains are linked by siloxane bonds and allow, due to their cohesion, the obtaining of a solid assembly. These joints are also advantageously temperature resistant.

[0016] Adhesive compositions based on polyurethane (or polyether) with alkoxysilane termination which are described in particular by the three Bostik patent applications: WO 09 / 106699, EP2336208 and WO 2020 / 128200. These adhesive compositions, free of solvent and water, are implemented by coating on a support layer at a temperature between 50 and 150°C, with a view to preparing self-adhesive supports, usable in particular for the manufacture of labels which can be conveniently fixed, thanks to the adhesive seal formed, on all kinds of substrates.

[0017] However, if the implementation of these latter adhesive compositions does not present any risk linked to possible contact with diisocyanate monomers, its use as a semi-structural adhesive comes up against a major drawback linked to a particularly significant risk of sagging.

[0018] Indeed, it may happen that either the first surface on which the bead of glue is initially deposited, or the two substrates just after they come into contact, are in a non-horizontal position, in particular a vertical position, even though the crosslinking of the glue is not complete. This has the effect of exposing either said bead or the non-crosslinked adhesive joint which binds the two substrates in the assembly to the force of gravity. This consequently results in a risk of deformation or fining or even sagging (also referred to in English as "sagging" or "slump"), under the action of the stress resulting from said force.

[0019] Such a change in shape of the bead (or of the non-crosslinked adhesive joint) is designated in the remainder of this text by the general term "run". It can thus result in a variation in the thickness of the adhesive during crosslinking between the 2 substrates, and therefore inhomogeneity, in particular dimensional, of the adhesive joint which firmly bonds the 2 substrates in the final assembly obtained after complete crosslinking. This inhomogeneity of the adhesive joint is particularly likely to affect its mechanical properties.

[0020] An aim of the present invention is thus to limit and / or eliminate the running (or fining) of polyurethane (or polyether)-based adhesive compositions with alkoxysilane endings, in particular as described by the aforementioned Bostik SA application WO 2020 / 128200.

[0021] Furthermore, due to a high crosslinking time at room temperature, it is generally necessary to implement these compositions hot and in the presence of humidity, which may lead to the need, when it is desired to assemble substrates on an automated line, to provide humidity and temperature-controlled chambers on the line.

[0022] Another aim of the present invention is thus to propose a crosslinkable adhesive composition based on a polymer comprising at least one hydrolyzable alkoxysilane group, which allows the assembly of 2 substrates, by a crosslinking reaction. which does not require relative humidity control and / or which is carried out at a lower temperature, in particular at a temperature below 50°C, and even at room temperature.

[0023] Another aim of the present invention is to provide a crosslinkable adhesive composition based on a polymer comprising at least one hydrolyzable alkoxysilane group, which crosslinks at ambient temperature and / or humidity in a reduced time.

[0024] Another object of the invention is that the adhesive joint which is formed by the crosslinking and which ensures the assembly of the 2 substrates, has improved heat resistance.

[0025] Another object of the invention is that said adhesive seal has improved mechanical resistance.

[0026] Another object of the invention is that the thickness of said adhesive seal is more uniform or homogeneous.

[0027] It has now been found that these objects can be achieved in whole or in part by means of the adhesive composition, its use as a semi-structural adhesive, and the method of joining two substrates which are described below. DESCRIPTION OF THE INVENTION Crosslinkable adhesive composition:

[0028] The present invention therefore relates firstly to a crosslinkable adhesive composition, characterized in that it comprises:

[0029] - at least one polymer (A) comprising a hydrolyzable alkoxysilane group;

[0030] - at least one tackifying resin (B);

[0031] - at least one pyrogenic silica (C); and

[0032] - at least one crosslinking catalyst (D).

[0033] It has now been found that the sagging of said adhesive composition is considerably lowered compared to polyurethane (or polyether)-based adhesive compositions with alkoxysilane terminations, which are described in particular in WO 2020 / 128200. It can thus advantageously lead to the deposition of said composition on a surface of a first substrate, even at a high grammage, and in particular in the form of a bead, which leads, after crosslinking and contact with a second substrate, to an assembly whose adhesive joint is homogeneous and of uniform thickness.

[0034] Furthermore, the crosslinking time of said crosslinkable composition is also significantly reduced at ambient temperature and humidity, compared to the compositions of WO 2020 / 128200. This crosslinking time can advantageously be further reduced when the crosslinking is carried out using a temperature and humidity controlled chamber; which is particularly favorable to increasing the productivity of the assembly manufacturing, for example when this is carried out on the assembly lines of car manufacturers.

[0035] Furthermore, said adhesive composition can be applied in a temperature range from 30°C to 130°C, preferably from 90°C to 130°C, i.e. at a lower application temperature than that of a hot-melt adhesive.

[0036] Furthermore, in addition to the advantages stated above for the implementation of the crosslinkable adhesive composition, the adhesive joint formed between the 2 substrates in the assembly offers, due to the presence of the three-dimensional network formed by the crosslinking, a largely improved heat resistance compared to the non-reactive hot-melt adhesives known from the prior art. Finally, said adhesive joint has, compared to the compositions of WO 2020 / 128200, improved properties of cohesion and adhesion to the substrates. These properties are quantified by measurements of tensile breaking stress on the adhesive joint alone and of shear breaking stress on the adhesive joint joining 2 substrates in an assembly. Polymer (A):

[0037] For the purposes of the present invention, the term “polymer (A) comprising a hydrolyzable alkoxysilane group” means a polymer which comprises at least one, and preferably at least two, hydrolyzable groups of formula (I):

[0038] -Si(R4)p(OR5)3 p (I)

[0039] in which:

[0040] - R4 represents a linear or branched alkyl radical comprising from 1 to 4 carbon atoms, with the possibility that when there are several R4 radicals, the latter are identical or different; - R5 represents a linear or branched alkyl radical comprising from 1 to 4 carbon atoms, with the possibility that when there are several R5 radicals, the latter are identical or different, with the possibility that two OR5 groups can be engaged in the same cycle; and - p is an integer equal to 0, 1 or 2, preferably equal to 0 or 1.

[0041] The hydrolyzable alkoxysilane group is preferably positioned at the end of said polymer. However, positioning in the middle of the chain is not excluded. The polymer (A) is not crosslinked before application of the adhesive composition. The adhesive composition is applied under conditions allowing its crosslinking.

[0042] The polymer (A) is therefore a silylated polymer which is generally in the form of a more or less viscous liquid. Preferably, the polymer (A) has a viscosity ranging from 10 to 200 Pa.s, preferably ranging from 20 to 175 Pa.s, said viscosity being for example measured according to a Brookfield type method at 23°C and 50% relative humidity (needle S28).

[0043] The polymer (A) preferably comprises two groups of formula (I), but it may also comprise from three to six groups of formula (I).

[0044] Preferably, the polymer(s) (A) have a number-average molecular mass (Mn) ranging from 500 to 50,000 g / mol, more preferably ranging from 700 to 20,000 g / mol. The number-average molecular mass (Mn) of the polymers can be calculated or measured by methods well known to those skilled in the art, for example by NMR and size exclusion chromatography using polystyrene-type standards.

[0045] According to one embodiment of the invention, the polymer (A) corresponds to one of the formulas (II), (III) or (IV): T 4 h po—r—sf(R

[0046]

[0047] in which: R4, R5 and p have the same meaning as in formula (I) described above, P represents a saturated or unsaturated, linear or branched polymeric radical optionally comprising one or more heteroatoms, such as oxygen, nitrogen, sulfur, silicon, and preferably having a number-average molecular mass (Mn) ranging from 100 g / mol to 48600 g / mol, more particularly from 300 g / mol to 18600 g / mol or from 500 g / mol to 12600 g / mol, R1 represents a divalent hydrocarbon radical comprising from 5 to 15 carbon atoms which may be aromatic or aliphatic, linear, branched or cyclic, R3 represents a linear or branched divalent alkylene radical comprising from 1 to 6 carbon atoms, preferably from 1 to 3 carbon atoms, X represents a divalent radical chosen from -NH-, -NR7- or -S-, R7 represents a linear or branched alkyl radical comprising from 1 to 20 carbon atoms and which may also comprise one or more heteroatoms, and f is an integer ranging from 1 to 6, preferably ranging from 2 to 5, preferably from 2 to 4, more preferably ranging from 2 to 3.

[0048] Preferably, in formulas (II), (III) and / or (IV) above, P represents a polymeric radical chosen in a non-limiting manner from polyethers, polycarbonates, polyesters, polyolefins, polyacrylates, polyether polyurethanes, polyester polyurethanes, polyolefin polyurethanes, polyacrylate polyurethanes, polycarbonate polyurethanes, polyether / polyester block polyurethanes.

[0049] For example, document EP 2468783 describes silylated polymers of formula (II) in which P represents a polymer radical with polyurethane / polyester / polyether blocks.

[0050] According to one embodiment, the silylated polymers are chosen from silylated polyurethanes, silylated polyethers, and mixtures thereof.

[0051] According to a particular embodiment, the silylated polymer (A) corresponds to one of the formulas (II'), (III') or (IV'): -R—w-ç— o—fh-o— e— mh- o—R^o—ç—^hr— ■ ■ rï lnnj„ rï - OGOO

[0052] (II') 4' 2 4 S (R"Q)3_p(E —R—O— R—Q— R—S1(R

[0053] (III)

[0054] (IV')

[0055] in which:

[0056] - R1, R3, R4, R5, X, R7 and p have the same meaning as in formulas (II), (III) and (IV) described above, - R2 represents a saturated or unsaturated, linear or branched divalent hydrocarbon radical optionally comprising one or more heteroatoms, such as oxygen, nitrogen, sulfur, silicon, and preferably having a number-average molecular mass (Mn) ranging from 100 g / mol to 48,600 g / mol, more particularly from 300 g / mol to 18,600 g / mol or from 500 g / mol to 12,600 g / mol, and - n is an integer greater than or equal to 0.

[0057] In the silylated polymers of formulae (II'), (III') or (IV') defined above, when the radical R2 comprises one or more heteroatoms, said heteroatoms are not present at the end of the chain. In other words, the free valences of the divalent radical R2 linked to the oxygen atoms adjacent to the silylated polymer each come from a carbon atom. Thus, the main chain of the radical R2 is terminated by a carbon atom at each of the two ends, said carbon atom then having a free valence.

[0058] According to one embodiment, the silylated polymers (A) are obtained from polyols chosen from polyether polyols, polyester polyols, polycarbonate polyols, polyacrylate polyols, polysiloxane polyols and polyolefin polyols and mixtures thereof, and more preferably from diols chosen from polyether diols, polyester diols, polycarbonate diols, polyacrylate diols, polysiloxane diols, polyolefin diols and mixtures thereof. In the case of the polymers of formulae (II'), (III') or (IV') described above, such diols may be represented by the formula H0-R2-OH where R2 has the same meaning as in formulae (II'), (III') or (IV').

[0059] For example, among the radicals of type R2 which may be present in formulas (II'), (III') or (IV'), we may cite the following divalent radicals whose formulas below show the 2 free valences:

[0060] - derivative of a polypropylene glycol:

[0061] - derivative of a polyester diol:

[0062] - derivative of a polybutadiene diol:

[0063] - derivative of a polyacrylate diol:

[0064] - derivative of a polysiloxane diol:

[0065] In the above formulas, the meaning of the radicals and indices is as follows:

[0066] - q represents an integer such that the number-average molecular mass of the radical R2 ranges from 100 g / mol to 48600 g / mol, preferably from 300 g / mol to 18600 g / mol, more preferably from 500 g / mol to 12600 g / mol,

[0067] - r and s represent zero or a non-zero integer such as the average molecular mass in number (Mn) of the radical R2 ranges from 100 g / mol to 48600 g / mol, preferably from 300 g / mol to 18600 g / mol, more preferably from 500 g / mol to 12600 g / mol, it being understood that the sum r+s is different from zero,

[0068] - Q1 represents a linear or divalent aromatic or aliphatic alkylene radical or branched, saturated or unsaturated, preferably having from 1 to 18 carbon atoms, more preferably from 1 to 8 carbon atoms,

[0069] - Q2 represents a linear or branched divalent alkylene radical having preferably from 2 to 36 carbon atoms, more preferably from 1 to 8 carbon atoms,

[0070] - Q3, Q4, Q5, Q6, Q7 and Q8, represent, independently of each other, an atom of hydrogen or an alkyl, alkenyl or aromatic radical, preferably having from 1 to 12 carbon atoms, preferably from 2 to 12 carbon atoms, more preferably from 2 to 8 carbon atoms.

[0071] According to the embodiment of the composition according to the invention, the silylated polymer (A) is such that the radical R2 which appears in the formulas (II'), (III') and (IV') represents a polyether radical, preferably a poly(oxyalkylene) radical, and even more preferably a radical derived from a polypropylene glycol corresponding to the formula indicated above.

[0072] According to one embodiment, R1 is chosen from one of the following divalent radicals whose formulas below show the 2 free valences:

[0073] a) the divalent radical derived from isophorone diisocyanate (IPDI): ch3 ch2— CH3J 1 ch3

[0074] b) the divalent radical derived from dicyclohexylmethane diisocyanate (H12MDI) x / '■ * S

[0075] c) the divalent radical derived from toluene diisocyanate (TDI)

[0076] d) divalent radicals derived from the 4,4' and 2,4'- isomers of diphenylmethane dii- socyanate (MDI)

[0077] e) the divalent radical derived from hexamethylene diisocyanate (HDI) -(CH2)6-

[0078] f) the divalent radical derived from m-xylylene diisocyanate (m-XDI)

[0079] The polymers of formula (II) or (II') can be obtained according to a process described in documents EP 2336208 and WO 2009 / 106699. Those skilled in the art will be able to adapt the manufacturing process described in these two documents in the case of the use of different types of polyols. Among the polymers corresponding to formula (II), mention may be made of:

[0080] - GENIOSIL® STP-E10 (available from WACKER): polyether comprising two groups (I) of dimethoxy type (n equal to 0, p equal to 1 and R4 and R5 represent a methyl group) having a number-average molecular mass of 8889 g / mol where R3 represents a methyl group; - GENIOSIL® STP-E30 (available from WACKER): with a number-average molecular weight of 14493 g / mol, it is a polypropylene glycol with 2 end groups consisting of a dimethoxy(methyl)silylmethylcarbamate, i.e. in formula (II1): n equal to 0; p equal to 1; R4 and R5 represent a methyl group and R3 represents a methyl group; - SPUR+® 1050MM (available from MOMENTIVE): polyurethane comprising two groups (I) of the trimethoxy type (n different from 0, p equal to 0 and R5 represents a methyl group) having a mo mass number average lecular of 16393 g / mol where R3 represents an n-propyl group; - SPUR+® Y-19116 (available from MOMENTIVE): polyurethane comprising two groups (I) of the trimethoxy type (n different from 0 and R5 represents a methyl group) having a number-average molecular mass ranging from 15000 to 17000 g / mol g / mol where R3 represents an n-propyl group; - DESMOSEAL® S XP 2636 (available from BAYER): polyurethane comprising two groups (I) of the trimethoxy type (n different from 0, p equal to 0 and R5 represents a methyl group) having a number-average molecular mass of 15038 g / mol where R3 represents an n-propylene group.

[0081] The polymers of formula (III) or (III') can be obtained by hydrosilylation of polyether diallyl ether according to a process described for example in document EP 1829928. Among the polymers corresponding to formula (III), mention may be made of:

[0082] - the MS SAX® 350 polymer (available from KANEKA) corresponding to a polyether comprising two groups (I) of dimethoxy type (p equal to 1 and R4 and R5 represent a methyl group) having a number-average molecular mass ranging from 14000 to 16000 g / mol;

[0083] - the MS SAX® 260 polymer (available from KANEKA) corresponding to a polyether comprising two groups (I) of dimethoxy type (p equal to 1, R4 and R5 represent a methyl group) having a number-average molecular mass of 16000 to 18000 g / mol where R3 represents an ethyl group;

[0084] - the MS S303H polymer (available from KANEKA) corresponding to a polyether comprising two dimethoxy-type groups (I) (p is equal to 1 and R4 represents a methyl group) having a number-average molecular mass of approximately 22,000 g / mol.

[0085] The polymers of formula (IV) or (IV') can for example be obtained by reaction of polyol(s) with one or more diisocyanate(s) followed by a reaction with aminosilanes or mercaptosilanes. A process for preparing polymers of formula (IV) or (IV') is described in document EP 2 583 988. Those skilled in the art will be able to adapt the manufacturing process described in this document in the case of the use of different types of polyols.

[0086] According to a preferred embodiment of the invention, the adhesive composition comprises at least one silylated polymer (A) of formula (II) and / or (II') or at least one silylated polymer (A) of formula (III) and / or (III').

[0087] According to a very particularly preferred embodiment of the invention, the polymer (A) is a silylated polymer of formula (II') in which n equals 0, R2 is a radical divalent derived from a polyether, preferably from a poly(oxyalkylene) diol, and even more particularly from a polypropylene glycol.

[0088] Tackifying resin (B):

[0089] The crosslinkable adhesive composition according to the invention also comprises at least one tackifying resin (B).

[0090] Said resin may be any resin compatible with the silylated polymer(s) (A).

[0091] The term "compatible tackifying resin" is intended to mean a tackifying resin which, when mixed in proportions 50% / 50% with the polymer(s) (A), gives a substantially homogeneous mixture.

[0092] The resins (B) are advantageously chosen from:

[0093] - (i) resins obtained by polymerization of terpenic hydrocarbons and phenols, in the presence of Friedel-Crafts catalysts;

[0094] - (ii) resins obtained by a process comprising polymerization alpha-methyl styrene, said process also including reaction with phenols;

[0095] - (iii) rosins of natural or modified origin, (such as for example rosin extracted from pine gum, wood rosin extracted from the roots of the tree and their derivatives hydrogenated, dimerized, polymerized or esterified by monoalcohols or polyols, such as glycerol or pentaerythritol);

[0096] - (iv) resins obtained by hydrogenation, polymerization or copolymerization (with an aromatic hydrocarbon) of mixtures of unsaturated aliphatic hydrocarbons having about 5, 9 or 10 carbon atoms derived from petroleum fractions;

[0097] - (v) terpene resins, (which generally result from the polymerization terpene hydrocarbons - such as monoterpene (or pinene) - in the presence of Friedel-Crafts catalysts);

[0098] - (vi) copolymers based on natural terpenes, (such as, for example, styrene / terpene, alpha-methyl styrene / terpene and vinyl toluene / terpene); or

[0099] - (vii) acrylic resins having a viscosity at 100°C of less than 100 Pa.s;

[0100] as well as among the mixtures of these resins.

[0101] Such resins are commercially available and among those of type (i), (ii), (iii) and (iv) defined above, the following products may be mentioned:

[0102] - resins of type (i): Dertophene® 1510 available from the company DRT having a number average molecular weight (Mn) of approximately 870 Da; Dertophene® H150 available from the same company having a number average molecular weight (Mn) of approximately 630 Da; Sylvarez® TP 95 available from Arizona Chemical Company having a number average molecular weight (Mn) of approximately 1200 Da;

[0103] - type (ii) resins: Cleartack® W100 available from Cray Valley, which is obtained by polymerization of alpha-methyl styrene without the action of phenols, with a number-average molecular weight (Mn) of 900 Da; Sylvarez® 510 which is also available from the Arizona Chemical Company with a number-average molecular weight (Mn) of approximately 1740 Da, the process for obtaining which also includes the addition of phenols;

[0104] - resins of type (iii): Sylvalite® RE 100 which is an ester of rosin and pentae- rethritol available from Arizona Chemical Company and with a number-average molecular weight (Mn) of approximately 1700 Da;

[0105] - type (iv) resins: Picco® AR100 available from Eastman and number-average molecular mass (Mn) of approximately 550 g / mol.

[0106] According to a preferred variant, a resin chosen from those of type (i) or (iv) is used as resin (B). Fumed silica (C):

[0107] Fumed silica (also called "fumed silica" in English) is in the form of very fine silica particles (of the order of a nanometer), with a very low apparent density and a very high specific surface area. Fumed silica can be obtained by pyrolysis, in the presence of hydrogen and oxygen, of silicon compounds, such as silicon tetrachloride, itself prepared from silicon and chlorine.

[0108] Fumed silica is initially hydrophilic, due to the presence of silanol groups (Si-OH) on the surface of its constituent particles. It can be made hydrophobic by reaction of these silanol groups with different reagents, generally a silicone oil, such as PolyDiMethylSiloxane (PDMS).

[0109] Preferably, the fumed silica (C) is a hydrophobic fumed silica.

[0110] According to one embodiment, the hydrophobic fumed silica (C) is obtained by treating a fumed silica with a PolyDiMethylSiloxane.

[0111] According to one embodiment, the fumed silica (C) has a BET specific surface area of ​​at least 10 m2 / g, preferably ranging from 50 to 400 m2 / g, even more preferably from 80 to 290 m2 / g. The BET specific surface area is measured, in a manner well known to those skilled in the art, by determining an adsorption isotherm based on the Brunauer, Emmett and Teller (BET) method, for example according to the ISO 9277 standard of September 2010.

[0112] According to another embodiment, the fumed silica (C) is obtained by a compaction treatment, for example from a roller compactor or from the process described by patent EP 0 280 851. The apparent density is quantified by a measurement of the packed apparent density, measured according to the ISO 787 / 11 standard of August 1983, which is generally within a range from 50 to 200 g / 1-

[0113] Such pyrogenic silicas, particularly hydrophobic ones, are commercially available, such as the products in the AEROSIL® range from the company EVONIK.

[0114] As an example of hydrophobic fumed silica (C), we can notably cite AEROSIL® R202, the BET specific surface area of ​​which is 100+20 m2 / g, the bulk density of approximately 60 g / l, and which is made hydrophobic by treatment with PolyDiMethylSiloxane. The constituent particles of AEROSIL® R202 have a size of approximately 16 nm. Crosslinking catalyst (D):

[0115] The crosslinking catalyst (D) that can be used in the composition according to the invention can be any catalyst known to those skilled in the art for the condensation of silanol. Examples of such catalysts that may be mentioned are organic titanium derivatives such as titanium acetyl acetonate (commercially available under the name TYZOR® AA75 from the company DuPont), aluminum such as aluminum chelate (commercially available under the name K-KAT® 5218 from the company King Industries), amines such as 1,8-diazobicyclo (5.4.0) undecene-7 or DBU.

[0116] Silsesquioxane resin (E):

[0117] In addition to ingredients (A), (B), (C) and (D), the crosslinkable adhesive composition according to the invention may also optionally comprise a silsesquioxane resin (E).

[0118] According to a preferred variant of the invention, the crosslinkable adhesive composition according to the invention comprises at least one such silsesquioxane resin.

[0119] Silsesquioxane resins are organic silicon compounds that can adopt a polyhedral structure or a polymeric structure, with Si-O-Si bonds. They generally have the following general formula:

[0120] [RSiO3 / 2]t

[0121] in which R, of identical or different nature, represents an organic radical, and t is an integer which can vary from 6 to 12, preferably t equals 6, 8, 10 or 12.

[0122] According to one embodiment, the silsesquioxane (E) has a polyhedral structure (or POSS for “Polyhedral Oligomeric Silsesquioxane” in English).

[0123] Preferably, the silsesquioxane (E) corresponds to the following general formula (V): R' \ / " HAS

[0124] (V)

[0125] in which each of R'1 to R'8 represents, independently of one another, a group chosen from:

[0126] - a hydrogen atom, - a radical chosen from the group consisting of a linear or branched C1-C4 alkoxy radical, a linear or branched alkyl radical comprising from 1 to 30 carbon atoms, an alkenyl radical comprising from 2 to 30 carbon atoms, an aromatic radical comprising from 6 to 30 carbon atoms, an allyl radical comprising from 3 to 30 carbon atoms, an aliphatic cyclic radical comprising from 3 to 30 carbon atoms, an acyl radical comprising from 1 to 30 carbon atoms, and - a group -OSiR'9R'10 in which R'9 and R'10 each represent, independently of one another, a hydrogen atom or a radical chosen from the group consisting of linear or branched C1-C4 alkyls, linear or branched C1-C4 alkoxys, C2-C4 alkenyls, a phenyl, a C3-C6 allyl radical, a C3-C8 cyclic aliphatic radical, and a C1-C4 acyl radical;

[0127] provided:

[0128] - that at least one radical among the radicals R'1 to R'8 is a C1-C4 alkoxy radical; and - that at least one radical among the radicals R'1 to R'8 is a phenyl radical.

[0129] Silsesquioxanes are known compounds which are described in particular in application WO 2008 / 107331. Some are also commercially available, such as the DOW product marketed under the name: DOW CORNING® 3074 and DOW CORNING® 3037 (CAS number = 68957-04-0). Other additives:

[0130] The crosslinkable adhesive composition according to the invention may also comprise one or more additives chosen from the group consisting of moisture absorbers, plasticizers, antioxidants, pigments, dyes, adhesion promoters, UV stabilizers, flame retardant additives or even fillers such as than carbonate fillers, for example calcium carbonate type.

[0131] The moisture absorber (or desiccant) may be, for example, chosen from hydrolyzable, non-polymeric alkoxysilane derivatives with a molecular mass of less than 500 g / mol, preferably chosen from trimethoxysilane and trimethoxysilane derivatives. Such an agent may typically extend the shelf life of the composition during storage and transport before use. Examples include gamma-metacryloxypropyltrimethoxysilane (for example available under the trade name SILQUEST ® A-174 from MOMENTIVE), methacryloxymethyltrimethoxysilane (for example available under the name GENIOSIL ® XL33 from WACKER), vinyltrimethoxysilane, risooctyltrimethoxysilane, or phenyltrimethoxysilane.

[0132] When present, the moisture absorber may for example represent from 0.1% to 3% by weight or from 1% to 2% by weight relative to the total weight of the composition according to the invention.

[0133] The composition according to the invention may also comprise a plasticizing agent.

[0134] As an example of a plasticizing agent that can be used, any plasticizing agent usually used in the field of adhesives can be used, such as, for example, phthalates, benzoates, trimethylolpropane esters, trimethylolethane esters, trimethylolmethane esters, glycerol esters, pentaerythritol esters, naphthenic mineral oils, adipates, cyclohexanedicar-boxylates, paraffinic oils, natural oils (optionally epoxidized), polypropylenes, polybutylenes, hydrogenated polyisoprenes, and mixtures thereof.

[0135] Among the phthalates, we can for example cite diisononyl phthalate, di-isobutyl phthalate, dioctyl phthalate, dicyclohexyl phthalate, diisooctyl phthalate, diiso-dodecyl phthalate, dibenzyl phthalate or butylbenzyl phthalate.

[0136] Among the benzoates, we can for example cite: neopentyl glycol dibenzoate (for example available under the name UNIPLEX ® 512 from LANXESS), dipropylene glycol dibenzoate (for example available under the name BENZOFLEX ® 9-88SG from EASTMAN), a mixture of diethylene glycol dibenzoate and dipropylene glycol dibenzoate (for example available under the name K-FLEX ® 850 S from KALAMA CHEMICAL), or a mixture of diethylene glycol dibenzoate, dipropylene glycol dibenzoate and triethylene glycol dibenzoate (for example available under the name BENZOFLEX ® 2088 from EASTMAN).

[0137] Among the pentaerythritol esters, we can for example cite pentaerythritol tetravalerate (for example available under the name PEVALEN™ from the company PESTORP).

[0138] Among the cyclohexanedicarboxylates, we can for example cite diisononyl 1,2-cyclohexanedicarboxylate (e.g. available under the name HEXAMOLL DINCH ® from BASF) and the l,4-bis(2-ethylhexyl)-l,4-cyclohexanedicarboxylate (e.g. available as DEHCH from CONNECT CHEMICALS).

[0139] The total content of plasticizer(s) in the composition according to the invention may range from 0% to 30% by weight, preferably from 1% to 30% by weight, or even for example from 1% to 15% by weight relative to the total weight of said composition.

[0140] The composition according to the invention may also comprise an antioxidant (also designated by the term UV stabilizing agent).

[0141] Antioxidants are compounds that may be introduced to protect the composition from degradation resulting from a reaction with oxygen that is likely to form by the action of heat or light. These compounds may include primary antioxidants that scavenge free radicals. Primary antioxidants may be used alone or in combination with other secondary antioxidants or UV stabilizers.

[0142] Examples include IRGANOX ® 1010, IRGANOX ® B561, IRGANOX ® 245, IRGANOX ® 1076, IRGAFOS ® 168 marketed by BASF.

[0143] An amount of antioxidant ranging from 0.1% to 3%, preferably from 1% to 3% by weight, based on the total weight of the composition according to the invention is generally used.

[0144] According to one embodiment, the crosslinkable adhesive composition according to the invention comprises:

[0145] - from 3% to 90% by weight, preferably from 5% to 80% by weight, preferentially from 10% to 70% by weight, advantageously from 20% to 60% by weight of at least one polymer (A) comprising a hydrolyzable alkoxysilane group;

[0146] - from 15% to 80% by weight, preferably from 20% to 70%, preferentially from 25% to 70%, in particular from 30% to 60%, advantageously from 40% to 60% by weight of at least one tackifying resin (B);

[0147] - from 1 to 10% by weight, preferably from 2 to 8%, advantageously from 2 to 6% of the fumed silica (C); and

[0148] - from 0.01% to 10% by weight, preferably from 0.01% to 5%, preferentially from 0.05% to 4%, advantageously from 0.1% to 3%, in particular from 0.5% to 2%, of crosslinking catalyst (D);

[0149] these percentages by weight being indicated on the basis of the total weight of said composition.

[0150] When, according to a preferred variant of the invention, the crosslinkable adhesive composition further comprises a silsesquioxane resin (E), the amount thereof may vary from 0.1 to 20% by weight, preferably from 1% to 20% by weight, preferentially from 2% to 15% by weight, advantageously from 3% to 12% by weight, based on the weight total of said composition.

[0151] The crosslinkable adhesive composition according to the invention can be prepared by a process which comprises:

[0152] - a mixing step, protected from air, preferably under an inert atmosphere, of the polymer (A), tackifying resin (B), and, where appropriate, other optional additives, to form a part (PA); then

[0153] - a step of mixing the crosslinking catalyst (D) with, when it is present, the silsesquioxane resin (E); to form a part (PB); then

[0154] - a step of incorporating the pyrogenic silica (C) into the part (PA), at a temperature temperature between 50 and 180°C, preferably between 100 and 150°C, until a homogeneous mixture is obtained (PC); and finally

[0155] - a step of mixing (PC) with (PB).

[0156] Use of the crosslinkable adhesive composition:

[0157] The present invention also relates to the use of the crosslinkable adhesive composition, as defined above, for the semi-structural assembly of two substrates.

[0158] Semi-structural assembly is understood to mean an assembly of two substrates in which the adhesive joint is capable of resisting shear stresses in a range from 2 to 8 MPa.

[0159] The substrates concerned are very varied and are notably chosen from:

[0160] - metals (such as aluminum or steel) and composites, possibly coated with paint (such as those used in the automotive industry);

[0161] - cardboard, textiles, leather, glass;

[0162] - thermoplastic polymers, such as:

[0163] - polyolefins (for example PolyEthylene or PolyPropylene) having even actually received a preliminary surface treatment, such as a primer, plasma treatment, or corona treatment;

[0164] - Acrylonitrile-Butadiene-Styrene (or ABS);

[0165] - Styrene-AcryloNitrile (SAN);

[0166] - polyvinyl chloride (PVC);

[0167] - polycarbonate;

[0168] - poly(methyl methacrylate) (PMMA); or

[0169] - polyesters.

[0170] According to a preferred variant, the use of the crosslinkable adhesive composition is implemented in the fields of electronics, construction, manufacturing of means of transport, preferably in the automotive, railway, aerospace and naval industries. It can also be used for the assembly of two substrates outdoors, due to its resistance to variable climatic conditions. Assembly process:

[0171] The present invention also relates to a method for assembling 2 substrates comprising:

[0172] - a step (i) of melting the adhesive composition as defined previously, by heating to a temperature between 30 and 130°C, then

[0173] - a step (ii) of depositing said composition on a surface of a first substrate, Then

[0174] - a step (iii) comprising:

[0175] - a step (iiil) of crosslinking said composition by heating at a temperature temperature ranging from 15°C to 200°C; and

[0176] - a step (iii2) of bringing said surface into contact with a surface of a second substrate.

[0177] The first substrate and the second substrate may be different or of the same chemical nature, and are as defined above.

[0178] The melting step (i) is advantageously carried out in a temperature range which is lower than that of hot melt adhesives, which is generally 150°C to 210°C.

[0179] According to a first embodiment of step (ii), which is more particularly preferred, the deposition of the composition is carried out in the form of a bead. The diameter of such a bead is generally within a range from 0.1 mm to 2 cm. Such a bead can be obtained by extrusion of the hot adhesive composition through a die connected either to a cartridge handled by an operator, or to a reservoir in the case of a robotic application on an assembly line. Such an application is particularly advantageous in the industrial fields mentioned above for the use of the composition.The reduction, or even the elimination, of the fining of the crosslinkable adhesive composition according to the invention advantageously makes it possible to apply it in the said form of a bead on substrates inclined relative to a horizontal plane, and to form after the crosslinking step (iiil) an adhesive joint whose thickness and mechanical properties are advantageously uniform.

[0180] According to a 2nd embodiment of step (ii), the deposition of the composition is carried out in the form of a layer with a thickness of between 0.1 mm and 2 cm, preferably between 1 mm and 10 mm. Such a layer can be obtained by spraying, by extrusion (for example by means of a die, such as a lip nozzle), by coating (for example by means of rollers or scrapers).

[0181] Step (iiil) of crosslinking the adhesive composition according to the invention is carried out by heating said composition to a temperature ranging from 15°C to 200°C.

[0182] According to a first variant of this embodiment, said step (iiil) is implemented operates at a temperature ranging from 15°C to 45°C, preferably at room temperature and in the presence of humidity from the surrounding atmosphere. Such crosslinking conditions are particularly advantageous since they allow for an industrial crosslinking process that does not require the presence of an oven. They also allow the second substrate to be chosen from heat-sensitive substrates such as PolyEthylene, PolyPropylene, foams or textiles.

[0183] According to a second variant of this embodiment, said step (iiil) is carried out at a temperature ranging from 90°C to 160°C, even more preferably from 120°C to 140°C and in the presence of an absolute humidity ranging from 10 to 200 g of water per m3 of gas (in particular air), preferably from 20 to 60 g / m3, even more preferably from 40 to 50 g / m3. Such crosslinking conditions are for example obtained by means of ovens (or chambers) placed on automated assembly lines.

[0184] This crosslinking step (iiil) has the effect in particular of creating - between the polymer chains with a hydrolyzable alkoxysilane terminal group of the adhesive composition and under the action of atmospheric humidity - siloxane type bonds which lead to the formation of a three-dimensional polymer network.

[0185] In the assembly method according to the invention, steps (i), (ii) and (iii) are implemented sequentially.

[0186] As regards steps (iiil) and (iii2) included in step (iii), they can be carried out in any order and even simultaneously.

[0187] Thus, according to a first embodiment of step (iii), step (iii11) of crosslinking the composition is carried out until the reaction is complete. It is then followed by step (iii2) of bringing into contact (or "displaying") the second substrate. This embodiment is particularly advantageous in the case where the second substrate is chosen from heat-sensitive substrates such as those mentioned above.

[0188] According to a 2nd embodiment of step (iii), the display step (iii2) is carried out simultaneously with the crosslinking step (iiil), even though the crosslinking reaction is not yet complete. In this case, said crosslinking reaction is continued and completed, after the display of the 2nd substrate.

[0189] According to a 3rd embodiment of step (iii), step (iii2) of displaying the second substrate is carried out first, then is followed by step (iii11) of crosslinking the adhesive composition comprised between the 2 surfaces of the substrates thus brought into contact.

[0190] Finally, according to a 4th embodiment of step (iii), step (iiil) of crosslinking the composition is carried out partially before step (iii2) of bringing into contact (or "displaying") the 2nd substrate. In this case, said crosslinking reaction (iiil) is continued and completed, after the display of the 2nd substrate.

[0191] The present invention finally relates to an assembly product comprising at least two substrates bonded by the adhesive composition as defined above, in the crosslinked state.

[0192] The invention is now described in the following exemplary embodiments which are given purely for illustrative purposes and cannot be interpreted to limit its scope.

[0193] Example A (comparative according to WO 2020 / 128200):

[0194] Heat-crosslinkable adhesive composition based on GENIOSIL® STP-E30

[0195] AL Preparation of the composition:

[0196] The composition shown in Table 1 is prepared by first introducing the Picco® AR100 tackifying resin into a glass reactor under vacuum and heated to approximately 160°C. Then, once the resin is well melted, the GENIOSIL® STP-E30 is added.

[0197] The mixture is stirred under vacuum for 15 minutes, then cooled to 70°C. The catalyst (K-KAT® 5218) and the silsesquioxane DOW CORNING® 3074 are then introduced. The mixture is kept under vacuum and stirred for a further 10 minutes.

[0198] A2. Measurement of creep (or sagging):

[0199] The composition thus prepared is deposited on a cardboard substrate using a manual gun in the form of a bead of diameter 5 mm, at a temperature of 120°C.

[0200] The cord is crosslinked in a vertical position at a temperature of 140°C and in the presence of an absolute humidity of 50 g / m3, for a time of 1 minute.

[0201] We then measure the distance over which the cord has flowed, between its initial position and its furthest final position.

[0202] The result obtained is reported in Table 1.

[0203] A3. Measurement of crosslinking time at room temperature:

[0204] The composition prepared in Al is applied at 120°C, so as to fill a mold corresponding to a type H2 test piece, as defined by standard NF T46-002, the thickness of which is 4 mm and the central part of which has a rectangular section of 4 x 2 mm over a length of 25 mm.

[0205] Said mold is left at room temperature and the behavior of the composition is observed.

[0206] The time required for complete crosslinking is reported in Table 1.

[0207] A4. Measurement of stress and elongation at break of the adhesive joint by test traction:

[0208] The principle of the measurement consists of stretching in a tensile machine, the movable jaw of which moves at a constant speed equal to 100 mm / minute, a test piece of type H2, as defined above, consisting of the composition crosslinked adhesive and to record, at the moment when the rupture of the test piece occurs, the stress applied (in MPa) as well as the elongation of the test piece or elongation (in %).

[0209] The results of the measurements obtained are shown in Table 1.

[0210] A5. Measurement of the breaking stress of the adhesive joint on Poly- support Propvlene (PP) by shear test:

[0211] Two parallelepiped PP test pieces of length 100 mm, width 25 mm and thickness 2.5 mm are used.

[0212] The adhesive composition, packaged in a cartridge, is applied at 120°C in the form of a bead with a diameter of approximately 5 mm, which is deposited on an overlap zone located at the end of a first test piece, 25 mm wide and 12.5 mm long.

[0213] One end of the 2nd test piece is then pressed onto said zone, such that the 2 test pieces being in the extension of one another, their two free ends are located symmetrically with respect to the overlap zone, and that, by using a wedge system and removing the excess adhesive using a spatula, the adhesive layer resulting from the crushing of the bead in the overlap zone has a thickness of 800 μm.

[0214] The adhesive composition is allowed to crosslink in the assembly thus obtained for 24 hours, under standard conditions (23°C and in the presence of an absolute humidity of 10 g of water per m3).

[0215] The assembly is then subjected to a shear test using a dynamometer operating at a speed of 10 mm / minute until the two specimens separate and the assembly breaks.

[0216] The test is repeated 3 times and the average shear stresses corresponding to the failure of the assembly are reported in Table 1.

[0217] A6. Temperature resistance test of the adhesive seal:

[0218] A6.1: Prior preparation of a PET support layer coated with the crosslinked composition, at a weight of 60 g / m2:

[0219] A rectangular sheet of PolyEthyleneTetrafluoroethylene (PET) with a thickness of 50 μm and dimensions of 20 cm by 40 cm is used as the support layer.

[0220] The composition obtained at point AL is preheated to a temperature close to 100°C and introduced into a cartridge from which a bead is extruded which is deposited near the edge of the sheet parallel to its width.

[0221] The composition contained in this bead is then distributed over the entire surface of the sheet, so as to obtain a uniform layer of substantially constant thickness. For this, a film puller (also called a film-mograph) is used which is moved from the edge of the sheet to the opposite edge. This deposits a composition layer corresponding to a weight of 60 g / m2, which represents approximately a thickness of the order of 60 pm.

[0222] The PET sheet thus coated is then placed in an oven at 120°C and under a humid atmosphere (50 g / m3 of absolute humidity) for 5 minutes to crosslink the composition, then laminated onto a protective non-stick layer (or “release liner”) consisting of a sheet of rectangular silicone film of the same dimensions.

[0223] The three-layer obtained is subjected to the test described below.

[0224] A6.2: Static shear resistance time at 125°C of the adhesive joint:

[0225] The heat resistance of the adhesive joint made of the crosslinked adhesive composition is evaluated by a test which determines the resistance time of said adhesive joint to static shear at 125°C. Reference is made for this test to FIN AT method No. 8. The principle is as follows.

[0226] A test piece in the form of a rectangular strip (25 mm x 75 mm) is cut from the three-layer obtained previously and is stored at room temperature (23°C, 50% humidity) for 24 hours.

[0227] After removing all of the protective anti-adhesive layer, a square portion of 25 mm on each side located at the end of the adhesive strip is fixed to a glass plate.

[0228] The test plate thus obtained is introduced, by means of a suitable support, in a substantially vertical position into an oven at 125°C, the unglued part of the 50 mm long strip being located below the plate. After thermal balancing, the remaining free part of the strip is connected to a mass of 1 kg, the entire device always remaining in the oven at 125°C for the duration of the test.

[0229] Under the effect of this mass, the adhesive joint which ensures the fixing of the strip on the plate is subjected to a shear stress. To better control this stress, the test plate is in fact placed so as to make an angle of 2° with respect to the vertical.

[0230] The time after which the strip detaches from the plate following the rupture of the glue joint under the effect of this stress is noted.

[0231] The result, expressed in hours, is shown in Table 1.

[0232] Examples 1 and 2: Adhesive compositions crosslinkable at room temperature based on GENIOSIL® STP-E30

[0233] The preparation of the composition of Example A is repeated as indicated in point A1, except that, after adding the catalyst and the silsesquioxane and then stirring for 10 minutes, the AEROSIL® R202 is introduced, and stirring is carried out again for approximately 10 minutes.

[0234] The measurement of the finishing, the crosslinking time at room temperature, and than the tensile and shear tests, as indicated in points A2, A3, A4 and A5. The results indicated in Table 1 are obtained. It is observed that:

[0235] - the sagging of the composition of examples 1 and 2 is, compared to example A, significantly lowered, or even removed;

[0236] - for example 2: the crosslinking time at room temperature of the com position is, compared to example A, considerably reduced (by more than a factor of 3), and the tensile breaking stress of the adhesive joint is significantly increased;

[0237] - the cohesion of the adhesive joint of examples 1 and 2 in the assembly of PP substrates, evaluated by the shear breaking stress, is, unlike example A, of an order of magnitude representative of a semi-structural adhesive. For reference, the corresponding value determined for the PolyAmide hot melt adhesive marketed by Bostik SA as a semi-structural adhesive under the name HM4229, is 6 MPa.

[0238] The preparation of the self-adhesive PET support layer is also repeated, as indicated in point A6.1., except that the coated PET sheet is left at room temperature and humidity (approximately 23°C and 10 g / m3 in absolute humidity) for 7 hours for crosslinking, before being laminated onto the protective release layer. The resulting trilayer is then subjected to the test described in point A6.2, which leads to the results indicated in Table 1.

[0239] For the adhesive joint of examples 1 and 2, shear strength values ​​at 125°C are observed which demonstrate a cohesion at temperature much higher than that of example A. Furthermore, such cohesion can advantageously be obtained at ambient temperature and humidity, without using an oven (or stove) as for example A.

[0240] [Tables 1] Ingredient Content in % wt / wt Example A Example 1 Example 2 (A) GENIOSIL® STP-E30 42.4 40.84 40.19 (B) Picco® AR100 51.6 49.71 48.94 (C) AEROSIL® R202 - 3.5 5.0 (D) K-KAT ® 5218 1 0.98 0.98 (E) DOW CORNING® 3074 5 4.97 4.89 Sagging (cm) 5 1 0 Curing time at room temperature (hours) 24 ND 7 Adhesive joint tensile test: - stress at break (MPa) - elongation at break (%) 0.16 326 ND ND 0.39 300 Adhesive joint shear test: - stress at break (MPa) * 4 5 Shear strength time at 125°C of the adhesive joint (hours) 24 70 40

[0241] ND = Not Determined

[0242] *: lower than sensitivity

[0243] of the force sensor

Claims

Claims

1. Crosslinkable adhesive composition, characterized in that it comprises: - at least one polymer (A) comprising a hydrolyzable alkoxysilane group; - at least one tackifying resin (B); - at least one pyrogenic silica (C); - at least one crosslinking catalyst (D), and - a silsesquioxane resin (E).

2. Adhesive composition according to claim 1, characterized in that the polymer (A) comprises at least one, and preferably at least two, hydrolyzable groups of formula (I): -Si(R4)p(OR5)3_p (I) in which: - R4 represents a linear or branched alkyl radical comprising from 1 to 4 carbon atoms, with the possibility that when there are several R4 radicals, the latter are identical or different; - R5 represents a linear or branched alkyl radical comprising from 1 to 4 carbon atoms, with the possibility that when there are several R5 radicals, the latter are identical or different, with the possibility that two OR5 groups can be engaged in the same cycle; and - p is an integer equal to 0, 1 or 2, preferably equal to 0 or 1.

3. Adhesive composition according to one of claims 1 or 2, characterized in that the pyrogenic silica (C) is hydrophobic.

4. Adhesive composition according to claim 3, characterized in that the hydrophobic fumed silica (C) is obtained by treatment of a fumed silica with a PolyDiMethylSiloxane.

5. Adhesive composition according to one of claims 1 to 4, characterized in that the pyrogenic silica (C) has a BET specific surface area of ​​at least 10 m2 / g, preferably ranging from 50 to 400 m2 / g.

6. Adhesive composition according to one of claims 1 to 5, characterized in that it comprises: - from 3% to 90% by weight of at least one polymer (A); - from 15% to 80% by weight of at least one tackifying resin (B); - from 1 to 10% by weight of fumed silica (C); - from 0.01% to 10% by weight of crosslinking catalyst (D); and - from 0.1 to 20% by weight of silsesquioxane resin (E); these percentages by weight being indicated on the basis of the total weight of said composition.

7. Use of the crosslinkable adhesive composition, as defined in one of claims 1 to 6, for the semi-structural assembly of two substrates.

8. Use according to claim 7 in the fields of electronics, construction, manufacturing of means of transport, preferably in the automotive, railway, aerospace and naval industries.

9. Method for assembling 2 substrates comprising: - a step (i) of melting the adhesive composition, as defined in one of claims 1 to 6, by heating to a temperature between 30 and 130°C, then - a step (ii) of depositing said composition on a surface of a first substrate, then - a step (iii) comprising: - a step (iii11) of crosslinking said composition by heating to a temperature ranging from 15°C to 200°C; and - a step (iii2) of bringing said surface into contact with a surface of a second substrate.

10. A method according to claim 9, characterized in that in step (ii) the composition is deposited on the surface of the first substrate in the form of a bead.

11. Method according to claim 9, characterized in that in step (ii) the composition is deposited on the surface of the first substrate in the form of a layer with a thickness of between 0.1 mm and 2 cm.

12. Method according to one of claims 9 to 11, characterized in that the crosslinking step (iiil) is carried out at a temperature ranging from 15°C to 45°C, preferably at room temperature and in the presence of humidity from the surrounding atmosphere.

13. Method according to one of claims 9 to 11, characterized in that the crosslinking step (iiil) is carried out at a temperature ranging from 90°C to 160°C and in the presence of an absolute humidity ranging from 10 to 200 g of water per m3 of gas, preferably from 20 to 60 g / m3.

14. An assembly product comprising at least two substrates bonded by the adhesive composition as defined in one of claims 1 to 6.