Obtaining surface protection layers by additive manufacturing
A filament composition for additive manufacturing addresses adhesion and warping issues by using polyolefins and styrene-based copolymers, enabling flexible and removable protective layers on various surfaces.
Patent Information
- Application Number
- FR2021008109
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-07-26
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2041-07-26
AI Technical Summary
Current additive manufacturing methods face challenges in achieving temporary surface protection layers with good adhesion to various surfaces at room temperature, while avoiding warping and buckling effects.
A filament composition comprising polyolefins with specific density, fluidity, hardness, and flexural modulus, combined with styrene-based copolymers and additives, is used for additive manufacturing to form protective layers with good adhesion and peelability.
The solution provides flexible, adherent, and easily removable protective layers that prevent warping and buckling, suitable for diverse surfaces including plastics, metals, and complex shapes.
Abstract
Description
Title of the invention: Obtaining surface protection layers by additive manufacturing Field of invention
[0001] The invention relates to the field of surface protection. More specifically, the invention relates to the composition of a filament for additive manufacturing, capable of being used to form a surface protection film. The invention also relates to a method for coating the surface of an object, by additive manufacturing, using such a filament. The invention also relates to an object coated with a surface protection film deposited by additive manufacturing. State of the art
[0002] Currently, in the surface protection industry, films are manufactured by extrusion or co-extrusion. These films are then coated with glue and finally calendered onto smooth, flat plates. These plates with the protective film can be used as they are or transformed by cutting, folding, stamping, thermoforming to obtain, for example, sinks, bathtubs, refrigerators, etc. There are also liquid protection solutions, such as spray-applied varnishes or other coating techniques.
[0003] The Fused Filament Fabrication (FFF) or Fused Deposition Modeling (FDM) technique is described in US Patent No. 5,121,329. This technique falls into the category of multi-layer additive manufacturing and has the particularity of using an extrusion system as a dispensing head. In fact, a filament of solid materials and of a diameter adapted to the printer is melted here at 1°C above its solidification point. The resulting fluid is deposited on the plate and solidifies on contact with it. In this way, the material is deposited in multi-layers following a pre-drawn model. The last layer deposited must be solidified before depositing the next one and the new layer must adhere to the previous one. The deposit thickness is defined by the space between the plate and the dispensing head. The latter is moved in the z axis to control the thickness.The pattern is obtained by moving the plate in the xy axes. A CAD / CAM (computer-aided design / computer-aided manufacturing) system controls these movements to follow the pre-recorded pattern. Now, extrusion temperatures can be well above the solidification point depending on the materials. For good print quality, the first layer of molten filament must adhere to the print plate. For this, the plate is usually heated or covered with a bonding solution. De- . Placements can also vary depending on the printer. The aforementioned patent specifies that the filaments can be made from beeswax, thermoplastic resins, metals, or even metal alloys. The primary qualities of these materials are that they can melt at a predefined temperature and solidify quickly without creating distortions.
[0004] DFF is mainly used to manufacture 3D articles for various applications such as automotive, aeronautics, medical etc. Polylactic acid (PLA) is the most common material for DFF printing because it has a low melting point (150°C-160°C°) and therefore involves low energy consumption. Its mechanical properties are also highly demanded for rigid and solid articles.
[0005] There is work on the deposition of adhesive or surface functionalization layers by DFF. Patent application WO2021 / 028795 proposes the use, for DFF printing, of pressure-sensitive adhesive (PSA)-based filament to permanently adhere two surfaces. The PSAs in question are (meth)acrylate polymers with a Tg<20°C and low hardness. This document highlights the fact that PSAs cannot be used as such in DFF. Their overly sticky surface is in fact not compatible with the filament delivery system. A layer of polyolefin must be deposited on the surface of the filament to make the filament non-sticky. The printer used has a screw in its extrusion head to mix the resulting filament. The use of PSA-based filaments is also described in applications EP-A-3 680 301 and WO 2020 / 127348. Patent application WO2020 / 114963 describes the functionalization of a film by DFF.This film is then placed on the surface of a 3D object to modify its surface and also provide protection.
[0006] Due to their high flexibility and shock absorption capacity, thermoplastic elastomers (TPEs) have appeared in DFF manufacturing to create flexible objects. Shoes, sports equipment, automotive / aeronautical parts, toys, and cases for phones and tablets are all produced using additive manufacturing. However, printing TPEs using DFF is not as straightforward as printing very rigid materials. The most rigid and high-density TPEs are often very crystalline and apolar, which leads to warping and delamination between layers. For low-density and very flexible TPEs, the filament cannot function as a piston and bends instead of pushing the molten material through the extrusion head.To avoid this problem, it is therefore recommended to use a low extrusion speed and to use a printer where the motor and the extruder are connected in "direct drive" or a printer combining "direct drive" and "Bowden" (extruders of the "direct drive" and "Bowden" type are commonly used for DFF printing). TPEs can also lack . hardness and prevent the spools from unwinding properly or be damaged by the teeth of the filament delivery system. These impacts cause material shortages that are found in the printed product. This phenomenon is called buckling (in English, "buckling effect"). Patent application WO 2021 / 037593 proposes cooling all filament before entering the extrusion head to impose sufficient hardness and rigidity during printing.
[0007] Polyolefins such as polyethylene and polypropylene are the largest volume materials produced by the plastics industry. In general, they have a low density and are light and flexible. For manufacturing via DFF, however, polyolefins suffer from their crystalline and apolar character which limits their interlayer adhesion and generates distortions. As it solidifies, the material accumulates stress which it compensates for by contracting. Several patents have proposed to remedy this problem, for example by adding a certain percentage of amorphous polyolefin polymers. Amorphous polymers do not accumulate stress as they solidify and are less sensitive to temperature change during the process. However, they have a low flexural modulus, which is insufficient for most 3D articles.Patent application WO 2020 / 096718 proposes an additive manufacturing process which consists in depositing successive layers of a thermoplastic material comprising an olefin block copolymer. It is shown that manufacturing using a low or very low density polyethylene does not work. Patent application WO 2020 / 028013 proposes an additive manufacturing process using a mixture of high density polyethylene and a second thermoplastic polymer selected from a low density polyethylene in a ratio (1.5 / 1 to 20 / 1). Patent application WO 2018 / 144141 proposes a composition for additive manufacturing comprising a thermoplastic polymer and an inorganic additive capable of reducing the specific heat of the composition (generated by the thermoplastic polymer). Patent application GB 2 515 348 proposes an additive manufacturing process using a polymer of variable stiffness, in particular a polymer with a Tg <10 °C.The biggest challenge with polymers with such low Tg is that they deform under their own weight at room temperature and therefore during printing. To solve this problem, the proposed solution is to place the 3D printer in a cooling chamber, so the polymer remains solidified and resistant during printing.
[0008] The state of the art summarized above shows that there is currently no satisfactory solution to address the issues of temporary surface protection by additive manufacturing. There is therefore a need to be able to have compositions or filaments which make it possible to obtain, by additive manufacturing, in particular by DFF, temporary surface protection layers or films having, among other things:
[0009] - good adhesion to all types of surfaces at room temperature, without having use of a hook solution;
[0010] - and good peelability, while being free from warping and buckling. It is with these specifications in mind that the present invention was made. Summary of the invention
[0011] According to a first aspect, the invention relates to a filament composition for additive manufacturing by fused filament deposition, which comprises:
[0012] a) from 60 to 100% by mass of a polyolefin or a mixture of polyolefins having (i) a density, measured according to ISO 1183 or ASTMD792, between 0.85 and 0.92 g / cm3, (ii) a melt flow index, measured according to ASTM D1238 (190°C / 2.16 kg) between 5.0 and 20.0 g / lOmin, (iii) a Shore A hardness, measured according to ISO 48-4:2018, between 70 and 90, and (iv) a flexural modulus, measured according to ISO-178 or ASTM D790, greater than 10 MPa;
[0013] b) from 0 to 40% by mass of a compound chosen from a styrene-ethylene-butylene-styrene copolymer, a styrene-butadiene-styrene copolymer, a styrene-isoprene-styrene copolymer, a styrene-isoprene-butadiene-styrene copolymer, a styrene-isobutylene-styrene copolymer, a styrene-ethylene-propylene-styrene copolymer, a styrene-ethylene-ethylene-propylene-styrene copolymer, an ethylene-styrene copolymer, a copolymer of ethylene and vinyl acetate, an ethylene and acrylic derivative copolymer and mixtures of these compounds0;
[0014] c) from 0 to 15% by mass of at least one tackifying resin0;
[0015] d) from 0 to 10% by mass of at least one additive chosen from matting agents, slip agents, colorants, UV stabilizers, UV barriers, antioxidants, anti-blocking agents and mixtures thereof;
[0016] the sum of a), b), c) and d) is equal to 100%.
[0017] The filament obtained from the mixture a), b), c) and d) has the following properties: (i) a density, measured according to ISO1183 or ASTMD792, between 0.85 and 1.10 g / cm3, (ii) a melt flow index, measured according to ASTM D1238 (190°C / 2.16 kg) between 5.0 and 20.0 g / lOmin, (iii) a Shore A hardness, measured according to ISO 48-4:2018, between 70 and 90, and (iv) a flexural modulus, measured according to ISO-178 or ASTM D790, greater than lOMPa.
[0018] According to another aspect, the invention relates to a method for coating, by additive manufacturing by fused deposition, the surface of an object or an article with at least two protective layers, said method comprising the following steps:
[0019] (i) heating and extruding a filament as defined below through a nozzle for form an extradite,
[0020] (ii) dispensing the extrudate through the nozzle while moving the nozzle so as to have a horizontal movement between the surface and the nozzle in a predetermined pattern to form a first protective layer on the surface of the object or article,
[0021] (iii) raising the nozzle along the z axis and repeating step (ii) to form at least one additional layer.
[0022] According to another aspect, the invention relates to an object or article coated with at least two protective layers by implementing the aforementioned method. Description of the invention
[0023] A first aspect of the invention relates to a filament composition for additive manufacturing by fused filament deposition, which comprises:
[0024] a) from 60 to 100% by mass of a polyolefin or a mixture of polyolefins having (i) a density, measured according to ISO 1183 or ASTMD792, between 0.85 and 0.92 g / cm3, (ii) a melt flow index, measured according to ASTM D1238 (190°C / 2.16 kg) between 5.0 and 20.0 g / lOmin, (iii) a Shore A hardness, measured according to ISO 48-4:2018, between 70 and 90, and (iv) a flexural modulus, measured according to ISO-178 or ASTM D790, greater than lOMPa;
[0025] b) from 0 to 40% by mass of a compound chosen from a styrene-ethylene-butylene-styrene copolymer, a styrene-butadiene-styrene copolymer, a styrene-isoprene-styrene copolymer, a styrene-isoprene-butadiene-styrene copolymer, a styrene-isobutylene-styrene copolymer, a styrene-ethylene-propylene-styrene copolymer, a styrene-ethylene-ethylene-propylene-styrene copolymer, an ethylene-styrene copolymer, a copolymer of ethylene and vinyl acetate, an ethylene and acrylic derivative copolymer and mixtures of these compounds0;
[0026] c) from 0 to 15% by mass of at least one tackifying resin0;
[0027] d) from 0 to 10% by mass of at least one additive chosen from matting agents, slip agents, colorants, UV stabilizers, UV barriers, antioxidants, anti-blocking agents and mixtures thereof;
[0028] the sum of a), b), c) and d) is equal to 100%.
[0029] For all practical purposes, it is specified here that the expression “the sum of a), b), c) and d) is equal to 100%" means that in all circumstances the cumulative quantities of a), b), c) and d) must be equal to 100%. Thus, for example, if the quantity of a) is 70%, the cumulative quantities of b), c) and d) must be equal to 30%. In this case, the quantity of b) can therefore be at most equal to 30% (no c) or d) in the filament composition).
[0030] The filament obtained from the mixture a), b), c) and d) has the following properties: (i) a density, measured according to the ISO1183 or ASTMD792 standard, between 0.85 and 1.10 g / cm3 , (ii) a melt flow index, measured according to ASTM D1238 (190°C / 2.16kg) between 5.0 and 20.0 g / lOmin, (iii) a Shore A hardness, measured according to ISO 48-4:2018, between 70 and 90, and (iv) a flexural modulus, measured according to ISO-178 or ASTM D790, greater than lOMPa.
[0031] In the present description, the expression "between x and y" must be interpreted as including the limits of the range considered (i.e., x and y).
[0032] The different embodiments and / or preferred variants of the invention can be combined.
[0033] In certain embodiments, the polyolefin a) is selected from a radical polyethylene (PEr), a linear polyethylene (linear PE), a polypropylene (PP), a copolymer of ethylene and propylene (EPM), an ethylene-propylene-diene copolymer (EPDM), advantageously from a linear polyethylene and a copolymer of ethylene and propylene. A "polyolefin blend" comprises, for the purposes of the present invention, either a blend of several polyolefins of the same type (for example, a blend of two linear PEs), or of one or more polyolefin(s) of a first type with one or more polyolefin(s) of one or more other types (for example, a blend of linear PE and PP). The polyolefin (taken individually) or the polyolefin blend a) must meet the above-mentioned criteria, namely:
[0034] - a density, measured according to ISO 1183 or ASTMD792, between 0.85 and 0.92 g / cm3;
[0035] - a fluidity index, measured according to ASTM D1238 (190°C / 2.16 kg) between 5.0 and 20.0 g / lOmin;
[0036] - a Shore A hardness, measured according to ISO 48-4:2018, between 70 and 90; and
[0037] - a flexural modulus, measured according to ISO-178 or ASTM D790, greater than 10 MPa.
[0038] In other words, when component a) is a mixture of polyolefins, it is the mixture as such which must meet the abovementioned criteria.
[0039] In some embodiments, the linear PE is a copolymer of ethylene and a C3-C8 olefin monomer, such as propene, butene, hexene, methylpentene, or octene.
[0040] In some embodiments, the EPM has a propylene content of between 25 and 60% by mass.
[0041] In some embodiments, the EPDM has a propylene content in the range of 25 to 60% by mass and a diene content, such as 1,4-hexadiene or ethylidiene norbornene, of less than or equal to 6% by mass.
[0042] In certain embodiments, the PEr, the linear PE, the EPM and the EPDM are indifferently of metallocene or Ziegler-Natta catalysis.
[0043] As polyolefins that can be used in the context of the invention, mention may be made of the resins of the QUEO range marketed by the company Boréalis, the resins of the Engage range marketed by the company DOW, the resins of the Exact range marketed by the company ExxonMobil or even the resins of the Vistamaxx Performance range marketed by the company ExxonMobil.
[0044] Compound b) is selected from a styrene-ethylene-butylene-styrene copolymer (SEBS), a styrene-butadiene-styrene copolymer (SBS), a styrene-isoprene-styrene copolymer (SIS), a styrene-isoprene-butadiene-styrene copolymer (SIBS), a styrene-isobutylene-styrene copolymer (SiBS), a styrene-ethylene-propylene-styrene copolymer (SEPS), a styrene-ethylene-ethylene-propylene-styrene copolymer (SEEPS), an ethylene-styrene copolymer (ES), an ethylene-vinyl acetate copolymer (EVA), an ethylene-acrylic derivative copolymer (EDA) and mixtures of these compounds. For the purposes of the present invention, the term "mixture of these compounds" means a mixture of several copolymers of the same type, or of one or more copolymer(s) of a first type with one or more copolymer(s) of one or more other types.
[0045] In some embodiments, compound b) is selected from a styrene-ethylene-butylene-styrene (SEBS) copolymer, a styrene-butadiene-styrene (SBS) copolymer, a styrene-ethylene-propylene-styrene (SEPS) copolymer, a styrene-ethylene-ethylene-propylene-styrene (SEEPS) copolymer, an ethylene-styrene (ES) copolymer, an ethylene vinyl acetate (EVA) copolymer, and mixtures of these compounds.
[0046] In some embodiments, the SEBS, SBS, SIS, SIBS, SiBS, SEPS and SEEPS each independently have a styrene content of less than or equal to 50% by mass, preferably between 5 and 45% by mass.
[0047] In some embodiments, the SEBS, SBS, SIS, SIBS, SiBS, SEPS and SEEPS each independently have a SEB, SB, SI, SIB, SiB, SEP and SEEP diblock content of less than or equal to 70% by mass.
[0048] In some embodiments, the ES have a styrene content between 5 and 85% by mass. In some embodiments, the ES have a melt flow index, measured according to ASTM DI238 (190°C / 2.16 kg), between 0.1 and 40 g / 10 min.
[0049] In certain embodiments, the EVAs have a vinyl acetate content of less than or equal to 80% by weight, and a melt flow index, measured according to ASTM D1238 (190°C / 2.16 kg), between 0.1 and 40 g / 10 min.
[0050] In certain embodiments, the EDAs preferably have a level of acrylic derivative, such as for example butyl acrylate and / or (meth)acrylic acid, such as for example butyl acrylate and / or (meth)acrylic acid, less than or equal to 40% by mass.
[0051] In certain embodiments, component a) is a mixture of polyolefin(s) as defined above, for example a linear PE and / or an EPM, and a copolymer as defined above, for example a copolymer chosen from a SEBS, an SBS, a SEPS, a SEEPS, an ES, an EVA and mixtures thereof.
[0052] As compound b) capable of being used in the context of the invention, mention may be made of the products of the Kraton range marketed by the company Kraton Polymers, the products of the SEPTON™ and HYBRAR™ ranges marketed by the company Kuraray.
[0053] In certain embodiments, the at least one tackifying resin c) is a thermoplastic resin, of low molecular weight, natural or synthetic, or non-hydrogenated, hydrogenated totally or partially or in a mixture, in particular in C5 or C9 or a mixture of C5 / C9, a cyclic diolefin (C5)2, or even a derivative of rosin (polymerized, hydrogenated, esterified or even disproportionated rosin).
[0054] In certain embodiments, the at least one additive d) is chosen from matting agents, antioxidant agents (primary or secondary) and anti-aging agents. In certain embodiments, the matting agents are either matting agents incompatible with PEs, for example acrylic grafted polyethylenes or polyethylene salts, or anti-blocking agents, for example silica and its derivatives, talc and its derivatives, mica and its derivatives. In certain embodiments, the anti-aging agents are sterically hindered amines also called HALS (from the English "Hindered Amine Light Stabilizers"). In the context of the invention, it is possible to use several additives of the same type.
[0055] In certain embodiments, the filament according to the invention is free of compound b) and therefore comprises:
[0056] al) from 75 to 100% by mass of a polyolefin or a mixture of polyolefins having (i) a density, measured according to ISO 1183 or ASTMD792, between 0.85 and 0.92 g / cm3, (ii) a melt flow index, measured according to ASTM D1238 (190°C / 2.16 kg) between 5.0 and 20.0 g / lOmin, (iii) a Shore A hardness, measured according to ISO 48-4:2018, between 70 and 90, and (iv) a flexural modulus, measured according to ISO-178 or ASTM D790, greater than lOMPa;
[0057] bl) from O to 15% by mass of at least one tackifying resin0;
[0058] cl) from 0 to 10% by mass of at least one additive chosen from matting agents, slip agents, colorants, UV stabilizers, UV barriers, antioxidants, anti-blocking agents and mixtures thereof;
[0059] the sum of a1), b1) and c1) is equal to 100% (and the polyolefin or the mixture of polyolefins a1) are as defined above for component a), the tackifying resin b1) is as defined above for the tackifying resin c), and the additives c1) are as defined above for the additives d)).
[0060] The filament obtained from the mixture a1), b1) and c1) has the following properties: (i) a density, measured according to ISO 1183 or ASTMD792, between 0.85 and 0.92 g / cm3, (ii) a melt flow index, measured according to ASTM D1238 (190°C / 2.16 kg) between 5.0 and 20.0 g / lOmin, (iii) a Shore A hardness, measured according to ISO 48-4:2018, between 70 and 90, and (iv) a flexural modulus, measured according to ISO-178 or ASTM D790, greater than lOMPa.
[0061] The filaments in accordance with the invention can be prepared according to methods known to those skilled in the art.
[0062] In some embodiments, the filaments have a diameter of between about 1.50 mm and about 3.50 mm, for example a diameter equal to 1.75 mm, 2.85 mm or 3.25 mm depending on the 3D printer used.
[0063] The filaments according to the invention can be used to coat (and temporarily protect) the surface of objects or articles manufactured using the fused filament deposition additive manufacturing technique.
[0064] Another aspect of the invention thus relates to a method for coating, by additive manufacturing by fused deposition, the surface of an object or an article with at least two protective layers, said method comprising the following steps:
[0065] (i) heating and extruding a composition as defined above through a nozzle to form an extrudate,
[0066] (ii) dispensing the extrudate through the nozzle while moving the nozzle so as to have a horizontal movement between the surface and the nozzle in a predetermined pattern to form a first layer on the surface of the object or article,
[0067] (iii) raising the nozzle along the z axis and repeating step (ii) to form at least one additional layer.
[0068] In some embodiments, step (iii) is repeated up to 10 times, for example 1 time, 2 times, 3 times, 4 times, 5 times, 6 times, 7 times, 8 times, 9 times or 10 times. In some embodiments, step (iii) is repeated three times. It is understood that when performing step (iii) for the first time, the "first" additional layer is deposited on the first layer formed in step (ii). When step (iii) is repeated each additional layer is deposited on the layer immediately previously formed.
[0069] In some embodiments, each of the layers formed by additive manufacturing has a thickness of between 40 micrometers and 500 micrometers, for example between 40 micrometers and 200 micrometers, between 50 micrometers and 200 micrometers, or between 50 micrometers and 100 micrometers. In some embodiments, each of the formed layers has the same thickness. In some embodiments, at least two of the formed layers have a thickness distinct from each other.
[0070] The assembly of layers deposited on the surface of an object or article to be protected forms a temporary protective film. This temporary protective film has a peeling force, measured at a peeling speed of 300 mm / min, of between 0.1 and 300 N / m, preferably between 0.1 and 150 N / m, more preferably between 0.5 and 100 N / m.
[0071] The deposition of the various (temporary) protective layers on the surface of an object or article is carried out with a 3D printer by molten filament deposition. This printer has its motor and its extrusion head connected in “direct drive”. The filament is heated by the extrusion head to a temperature between approximately 185°C and approximately 230°C and deposited on a plate at room temperature. The diameter of the outlet nozzle of the extrusion head is typically 0.4 mm, but other diameters are possible depending on the nature of the object or article to be protected. The first layer is generally deposited at low speed (for example 10 mm / sec) until a thickness of between 40 and 500 μm is obtained. For the following layer(s), the deposition speed is increased (for example 20 mm / sec) to obtain a layer thickness of between 40 and 300 μm.
[0072] The implementation of the aforementioned method makes it possible to protect different objects or manufactured articles due to the formation of at least two layers on their surface. This protection is temporary because the layers formed can be easily removed without leaving undesirable residues on the surface in question.
[0073] Thus, another aspect of the invention relates to an object or manufactured article coated with at least two protective layers by implementing the fused filament deposition method described above. In certain embodiments, the object or article is coated with two to twelve protective layers, preferably with two to five protective layers.
[0074] In certain embodiments, the surface of the object or manufactured article is a plastic surface, in particular a surface in the form of plates (for example PMMA, PC, PVC, etc.), a pre-coated surface (for example a pre-lacquered, glued surface, etc.), a laminate, a wooden surface, a plastic profile, a bare metal (aluminum, stainless steel).
[0075] The filament compositions according to the invention make it possible to form, by additive manufacturing by fused filament deposition, protective layers on the surface of objects which combine high flexibility, good adhesion to the surface, good peelability, while avoiding buckling effects during printing. Those skilled in the art will understand that depending on the nature of the filament formed from the composition according to the invention, one or more types of surface (as defined above) may be protected.
[0076] The implementation of the invention makes it possible to deposit at least two layers of thick protection(s) directly onto the surface to be protected by following more or less complex surface models. Thanks to the DFF technique and its modeling systems, it is possible to protect curved, structured, rough surfaces and 3D objects, in particular luxury products (watches, jewelry, etc.) requiring great complexity and precision on the area to be protected.
[0077] The invention is illustrated by the following examples, given purely for illustrative purposes. Example 1
[0078] Different compositions were tested for their ability to be produced in the form of filaments (spinning). When filaments have been formed, these are wound into a reel. The unwinding and rewinding capacity of the reels was evaluated (winding). The results are shown in Table 1.
[0079] [Tables 1] Composition Type Density (g / cm3) Melt Flow Index (g / 10min, 190°C / 2.16k g) Hardness (Shore A) Flexural Modulus (MPa) Spinning Winding ENGAGE™ 8842 Linear PE 0.857 1 54 4.5 NO - QUEO™ 0201 Linear PE 0.902 1.1 93 72 NO - Versaflex™ MD6649 SEBS 0.920 17 37 - NO - Vistamaxx™ 6202 PP 0.862 9.1 64 13 NO - Versaflex™ MD6741 SEBS 0.910 4.5 49 - YES NO QUEO™ 8210 Linear PE 0.883 10 84 24 YES YES Exact™ 0210 Linear PE 0.902 10 88 65 YES YES QUEO™ 7007 Linear PE 0.870 6.6 71 8 YES YES Exact™ 0210 / Kraton™ G1657M 80 / 20 PE / SE BS 0.902 7.7 79 YES YES QUEO™ 8210 / Vistamaxx PE / PP 0.879 9.2 65 - YES YES ™ 6202 80 / 20
[0080] The first four compositions in the table could not be spun. Of the other compositions, which could be spun, all the filaments formed could be unwound and rewound into a reel, with the exception of those obtained from Versaflex™ MD6741 because they were too sticky. Example 2
[0081] The filaments that successfully passed the winding test were subjected to a printing test. Printing was carried out with a Volumic Stream 30 Dual MK2 printer. For each filament tested, the extrusion head temperature was optimized between 185°C and 230°C. The print bed temperature was adjusted between 25 and 90°C. The first layer was deposited at a slower speed of 10 mm / sec to form a layer thickness between 100-200 pm. For the second layer, the deposition speed was increased to 20 mm / sec and the layer thickness was between 100-200 pm. 2 cm x 12 cm strips were thus formed. The filaments were evaluated on their print adhesion to the surface without adhesion primer and on good filling of the printed strip.
[0082] Filaments based on QUEO™ 7007 and based on the QUEO™ 8210 / Vistamaxx™ 6202 mixture were not compatible with the fused filament printing process. The resulting filaments were too flexible to be inserted into the delivery system and act as a piston in the printer.
[0083] Printing with Exact™ 0210, QUEO™ 8210 and Exact™ 0210 / Kraton™ G1657M based filaments gave good surface adhesion and filling. Example 3
[0084] Tapes were printed on different types of surfaces (metals, pre-lacquered, plastics, glass, etc.) and tested as a protective layer. For each type of surface, one test was carried out on the surface at room temperature and another on the surface heated by a plate at 90°C. To pass the test successfully, the tapes must adhere to the surface, be easily peelable and have good mechanical strength. These characteristics were evaluated manually and by measuring the peeling forces at a peeling speed of 300 mm / min. The manual peel test consists of removing the applied film by hand. This test is considered negative in cases where the film: (i) peels off prematurely, (ii) shows strong deformation, (iii) breaks during peeling, (iv) damages the surface to be protected or (v) shows too high adhesion. The peeling forces are measured using a dynamometer.Peeling forces should be between 0.1 and 300 N / m. to meet the needs of surface protection.
[0085] Some examples are shown in Table 2.
[0086] [Tables2] Printed composition Surface to be protected Manual peel test Peel force (at 300mm / min, in N / m) (surface at 25°C) QUEO 8210 Stainless steel (Ra*=2.5) + + 0.7 Aluminum GB + + 1.6 Bare glass + + 1.5 Pre-painted + + 1.6 PMMA + + 0.5 Polycarbonate + + 1.6 Exact 0210 Stainless steel (Ra=2.5) + - Aluminum GB + - Bare Glass - Pre-painted - - PMMA + - Polycarbonate + + 8.5 Exact 0210 / KratonR G1657M 80 / 20 Stainless Steel (Ra=2.5) + - Aluminum GB + - Bare Glass + + 1.0 Pre-painted + + 1.6 PMMA + + 8.6 Polycarbonate + + 17
[0087] 1 Ra = surface roughness, measured according to ISO 13565-2
[0088] + + Good hold and peelability of the printed film on the surface at room temperature
[0089] + Good hold and peelability of the printed film on the surface at 90°C but not at tem room temperature
[0090] - Premature detachment, deformation or rupture of the film, damage to the surface or too large
[0091] adhesion
[0092] - - Non-printable on the surface
[0093] QUEO 8210™ based filaments are printable at room temperature on all surfaces tested and the film obtained offers good hold and peelability.
[0094] Filaments based on the Exact 0210™ / Kraton™ G1657M blend are printable at room temperature on all tested surfaces. For glass, pre-painted, PMMA and polycarbonate surfaces, the resulting film offers good hold and peelability.
[0095] Filaments based on Exact 0210™ can be printed on stainless steel, aluminum and polycarbonate surfaces.
Claims
Claims
1. A filament composition for additive manufacturing by fused filament deposition, which comprises: (a) from 60 to 100% by mass of a polyolefin or a mixture of polyolefins having (i) a density, measured according to ISO 1183, between 0.85 and 0.92 g / cm3, (ii) a melt flow index, measured according to ASTM DI238 (190°C / 2.16 kg) between 5.0 and 20.0 g / 10 min, (iii) a Shore A hardness, measured according to ISO 48-4:2018, between 70 and 90, and (iv) a flexural modulus, measured according to ISO-178, greater than 1000Pa; b) from 0 to 40% by mass of a compound selected from a styrene-ethylene-butylene-styrene copolymer, a styrene-butadiene-styrene copolymer, a styrene-isoprene-styrene copolymer, a styrene-isoprene-butadiene-styrene copolymer, a styrene-isobutylene-styrene copolymer, a styrene-ethylene-propylene-styrene copolymer, a styrene-ethylene-ethylene-propylene-styrene copolymer, an ethylene-styrene copolymer, an ethylene and vinyl acetate copolymer, an ethylene-acrylic derivative copolymer and mixtures of these compounds; c) from 0 to 15% by mass of at least one tackifying resin; d) from 0 to 10% by mass of at least one additive chosen from matting agents, slip agents, colorants, UV stabilizers, UV barriers, antioxidants, anti-blocking agents and mixtures thereof; the sum of a), b), c) and d) is equal to 100%.
2. A composition according to claim 1, which comprises: al) from 75 to 100% by mass of a polyolefin or a mixture of polyolefins having (i) a density, measured according to ISO 1183, between 0.85 and 0.92 g / cm3, (ii) a melt flow index, measured according to ASTM DI238 (190°C / 2.16 kg) between 5.0 and 20.0 g / 10 min, (iii) a Shore A hardness, measured according to ISO 48-4:2018, between 70 and 90, and (iv) a flexural modulus, measured according to ISO-178, greater than 1000Pa; bl) from 0 to 15% by mass of at least one tackifying resin; cl) from 0 to 10% by mass of at least one additive chosen from matting agents, slip agents, colorants, UV stabilizers, UV barriers, antioxidants, anti-blocking agents and their mixtures; the sum of al), bl) and cl) is equal to 100%.
3. A composition according to claim 1 or claim 2, wherein said polyolefin is selected from a radical polyethylene, a linear polyethylene, a polypropylene, a copolymer of ethylene and propylene, and an ethylene-propylene-diene copolymer.
4. A composition according to claim 3, wherein said polyolefin is a linear polyethylene or a copolymer of ethylene and propylene.
5. Composition according to any one of claims 1 to 4, in which compound b) is chosen from a styrene-ethylene-butylene-styrene copolymer, a styrene-butadiene-styrene copolymer, a styrene-ethylene-propylene-styrene copolymer, a styrene-ethylene-ethylene-propylene-styrene copolymer, an ethylene-styrene copolymer, a copolymer of ethylene and vinyl acetate, and mixtures of these compounds.
6. Filament obtained by melting the composition according to claim 1, which has (i) a density, measured according to ISO 1183, between 0.85 and 1.10 g / cm3, (ii) a melt flow index, measured according to ASTM DI238 (190°C / 2.16 kg) between 5.0 and 20.0 g / 10 min, (iii) a Shore A hardness, measured according to ISO 48-4:2018, between 70 and 90, and (iv) a flexural modulus, measured according to ISO-178, greater than 1000 Pa.
7. Filament obtained by melting the composition according to claim 2, which has (i) a density, measured according to ISO 1183, between 0.85 and 0.92 g / cm3, (ii) a melt index, measured according to ASTM DI238 (190°C / 2.16 kg) between 5.0 and 20.0 g / 10 min, (iii) a Shore A hardness, measured according to ISO 48-4:2018, between 70 and 90, and (iv) a flexural modulus, measured according to ISO-178, greater than 1000 Pa.
8. A method for coating, by additive manufacturing by fused deposition, the surface of an object or article with at least two protective layers, said method comprising the following steps: (i) heating and extruding a composition as defined in any one of claims 1 to 5 through a nozzle to form an extrudate, (ii) dispensing the extrudate through the nozzle while moving the nozzle so as to have a horizontal displacement between the surface and the nozzle according to a predetermined pattern to form a first layer on the surface of the object or article, (iii) raising the nozzle and repeating step (ii) to form at least one additional layer.
9. The method of claim 8, wherein step (iii) is repeated one to ten times.
10. A method according to claim 8 or claim 9, wherein each formed layer has a thickness of between 40 micrometers and 500 micrometers.
11. The method of claim 10, wherein each of the formed layers has the same thickness.
12. The method of claim 10, wherein at least two of the formed layers have a thickness distinct from each other.
13. Manufactured object or article coated with at least two protective layers, said object or article being obtained by implementing the method according to any one of claims 8 to 12.
14. An object or article according to claim 13, which is coated with two to twelve protective layers, preferably with two to five protective layers.
15. An object or article according to any one of claims 13 to 14, wherein each protective layer has a thickness of between 40 micrometers and 500 micrometers, preferably between 40 micrometers and 200 micrometers.