COMPOSITE STRUCTURE AND ASSOCIATED MANUFACTURING PROCESS
By forming a glassy carbon film on a polycrystalline substrate through polymer resin deposition and annealing, the method addresses the challenges of surface roughness and defects in direct bonding, enabling efficient assembly of composite structures for power electronics.
Patent Information
- Application Number
- FR2022001443
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-02-18
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2042-02-18
AI Technical Summary
High-quality monocrystalline silicon carbide (c-SiC) substrates are expensive and difficult to supply in large sizes, and direct bonding of polycrystalline SiC substrates is complex due to surface roughness and residual defects, affecting the assembly of composite structures for microelectronics.
A method involving the deposition of a polymer resin with carbon-carbon bonds on a polycrystalline substrate, followed by annealing to form a glassy carbon film, which is then polished to achieve low surface roughness, enabling direct bonding with a donor substrate for thin layer transfer.
The method results in a support substrate with improved surface smoothness and electrical conductivity, facilitating the assembly of high-quality composite structures suitable for power electronics applications.
Smart Images

Figure 00000017_0000 
Figure 00000017_0001 
Figure 00000017_0002
Abstract
Description
Title of the invention: COMPOSITE STRUCTURE AND ASSOCIATED MANUFACTURING METHOD FIELD OF INVENTION
[0001] The present invention relates to the field of microelectronics and semiconductors. In particular, the invention relates to a polycrystalline substrate comprising a surface film of glassy carbon, and particularly suitable for receiving a thin film transferred from a donor substrate. The invention also relates to a method for manufacturing said support substrate and the composite structure resulting from the transfer of the thin film onto the support substrate. TECHNOLOGICAL BACKGROUND OF THE INVENTION
[0002] Silicon carbide (SiC) is increasingly used in the manufacture of high-performance power devices. However, high-quality single-crystal SiC (c-SiC) substrates for the microelectronics industry remain expensive and difficult to source in large sizes. Therefore, it is advantageous to use layer transfer solutions to create composite structures typically comprising a thin c-SiC layer (derived from a high-quality c-SiC substrate and intended to host the sensitive functional parts of the devices) on a lower-cost support substrate, for example, polycrystalline SiC (p-SiC).
[0003] A well-known thin film transfer solution is the Smart Cut® process, based on the implantation of light ions in a donor substrate (c-SiC) and on assembly, by direct bonding, at the level of a bonding interface between the donor substrate and a support substrate (for example in p-SiC).
[0004] Due to the material's hardness and polycrystalline structure, p-SiC substrates are difficult to polish and generally exhibit residual surface roughness, which complicates direct bonding. Indeed, direct bonding does not rely on adhesive substances but instead involves molecular bonds between the surfaces of the substrates being contacted: such bonding therefore requires excellent flatness as well as very low surface roughness and defects.
[0005] It is known to deposit an intermediate layer on one or both of the substrates to be assembled, said layer being easy to prepare (low roughness, in particular) for assembly by direct bonding. It should be noted that this intermediate layer must not affect the performance of the devices fabricated on the composite structure; in this case, for vertical power devices, such an intermediate layer must not affect the vertical electrical conductivity between the c-SiC thin film and the p-SiC support substrate.
[0006] It is particularly known from the prior art to use metallic intermediate layers to ensure vertical conduction in the composite structure.
[0007] Although this introduction primarily discusses the advantages of silicon carbide-based composite structures, composite structures based on other materials, which are high-performing but expensive in terms of large substrate dimensions and complex to prepare for thin-film transfer, such as SiC, may also be relevant. For example, a composite structure comprising a gallium nitride (GaN) thin film and a polycrystalline support substrate, for example aluminum nitride (AIN). SUBJECT OF THE INVENTION
[0008] The present invention proposes a solution, alternative to prior art solutions, which promotes obtaining a low surface roughness of the support substrate and enhances its electrical and thermal properties. The invention relates in particular to a polycrystalline initial substrate comprising a surface film of vitreous carbon, particularly suitable for receiving a useful layer transferred from a donor substrate. The invention also relates to a method for manufacturing said support substrate and the composite structure resulting from the transfer of the thin film onto the support substrate. BRIEF DESCRIPTION OF THE INVENTION
[0009] The present invention relates to a method for manufacturing a composite structure comprising a thin layer of a first single-crystal material disposed on a support substrate, the manufacturing method comprising the following steps: a) the provision of an initial substrate in a second polycrystalline material, b) the deposition by centrifugal coating, at least on one front face of the initial substrate, of a layer of polymer resin comprising preformed carbon-carbon bonds in three dimensions, c) the application of a first anneal at a temperature between 120°C and 180°C to the initial substrate coated with the polymer resin layer, to form a cross-linked polymer resin layer, d) the application of a second annealing at a temperature above 600°C, under a neutral atmosphere, to transform the crosslinked polymer resin layer into a vitreous carbon film.
[0010] According to advantageous features of the invention, taken alone or in any feasible combination: • the process includes, after step d), a step e) of mechanical and / or mechano-chemical polishing of the vitreous carbon film; • the polymer resin is based on coal tar, phenol formaldehyde, polyfurfuryl alcohol, polyvinyl alcohol, polyacrylonitrile, polyvinylidene chloride, and / or polystyrene; • the process includes a step f) of transferring a thin layer formed from the first single-crystal material directly onto the glassy carbon film or via an intermediate layer; • step f) implements an assembly between a donor substrate comprising the first single-crystal material, from which the thin layer will be derived, and the glassy carbon film, by direct bonding, to form a bonded assembly; • the donor substrate includes a buried fragile plane which delimits, with a front face of said substrate, the thin layer to be transferred, and step f) implements a separation of the assembly glued along the buried fragile plane, to give rise on the one hand, to a composite structure including the thin layer disposed on the glassy carbon film, itself disposed on the initial substrate, and on the other hand, the rest of the donor substrate; • the first single-crystal material is chosen from silicon carbide, gallium nitride, silicon, silicon-germanium, germanium, III-V compounds, or other semiconductor materials, or from piezoelectric materials; • the second polycrystalline material is chosen from silicon carbide, aluminum nitride, silicon, silicon-germanium, germanium, III-V compounds or other semiconductor materials, or from piezoelectric materials; • The first material and the second material are semiconductors.
[0011] The invention also relates to a composite structure comprising a thin layer of a first single-crystal material disposed on a support substrate, said support substrate including: - an initial substrate in a second polycrystalline material, - a vitreous carbon film in contact with the front surface of the initial substrate.
[0012] According to advantageous features of the invention, taken alone or in any feasible combination: • the initial substrate has a surface roughness between 100m and 200m peak-to-pit, measured by atomic force microscopy on a surface area less than or equal to 3000m x 3000m; • the vitreous carbon film has a thickness between 100nm and 4pm; • The composite structure includes an intermediate layer, between the thin layer and the glassy carbon film, chosen from silicon, carbide, silicon, carbon, tungsten or titanium; • The first single-crystal material is chosen from silicon carbide, gallium nitride, or other semiconductor materials, and the second polycrystalline material is chosen from silicon carbide, aluminum nitride, or other semiconductor materials. Brief description of the drawings
[0013] Other features and advantages of the invention will become apparent from the detailed description that follows, with reference to the accompanying figures in which:
[0014] [Fig. la]
[0015] [Fig.lb]
[0016] [Fig. le]
[0017] [Fig.ld] Figures 1a, 1b, 1e and 1d present steps of a manufacturing process for a support substrate, according to the invention;
[0018] [Fig.2] Fig.2 shows an example of the surface state of an initial substrate comprising a support substrate according to the invention;
[0019] [Fig.3] Fig.3 presents an example of the surface state of a vitreous carbon film composing a support substrate according to the invention;
[0020] [Fig.4a]
[0021] [Fig.4b]
[0022] [Fig.4c]
[0023] [Fig.4c']
[0024] [Fig.4d] Figures 4a, 4b, 4c, 4c', 4d show steps in the manufacturing process of a composite structure according to the invention.
[0025] Some figures are schematic representations which, for the sake of readability, are not to scale. In particular, the layer thicknesses along the z-axis are not to scale with respect to the lateral dimensions along the x and y axes.
[0026] The same references in the figures or in the description may be used for elements of the same nature. DETAILED DESCRIPTION OF THE INVENTION
[0027] The invention relates to a method for manufacturing a composite structure 100 comprising a thin layer 10 of a first monocrystalline material disposed on a support substrate 20, which is at least partly composed of a second polycrystalline material ([Fig. 4d]). The composite structure 100 intended allows vertical electrical conduction between the thin layer 10 and the support substrate 20, particularly for power electronics applications.
[0028] In particular, the first single-crystal material can be chosen from silicon carbide (c-SiC), gallium nitride (c-GaN), silicon, silicon-germanium, the germanium, III-V compounds, or other semiconductor materials, or even piezoelectric materials such as lithium tantalate, lithium niobate, etc. The second polycrystalline material can be chosen from silicon carbide (p-SiC), aluminum nitride (p-Ain), silicon (p-Si), or any material listed above with reference to the first material but exhibiting a polycrystalline structure or having a superficial polycrystalline layer. In composite structure 100, the first materials listed can be combined with either of the second materials mentioned above, provided, of course, that this is advantageous for the final application. Advantageously, composite structure 100 will be formed from a first and a second material with similar coefficients of thermal expansion.
[0029] In the following description, we will describe in particular the case of a first material made of c-SiC and a second material made of p-SiC. This description nevertheless applies to any other pair of first and second materials. Where certain situations require it, details will be provided for the different types of first and second materials.
[0030] The manufacturing process includes firstly a step a) of supplying an initial substrate 2 made of polycrystalline silicon carbide (p-SiC), having a front face 2a and a rear face 2b ([Fig. 1a]). The initial substrate 2 can be produced by a conventional technique such as sintering or chemical vapor deposition.
[0031] The initial substrate 2 is preferably in the form of a plate with a diameter of 100mm, 150mm, 200mm or even 300mm and a thickness typically between 300 and 800 microns.
[0032] The surface condition of the front face 2a of the initial substrate 2 is preferably chosen so that the peak-to-valley roughness (hereafter referred to as "PV roughness" in reference to "peak-to-valley" according to Anglo-Saxon terminology) is less than or equal to a few micrometers, typically less than or equal to 2 pm, 1 pm, 500 nm, 100 nm, or even 50 nm.
[0033] In the context of the present invention, roughness is measured by atomic force microscopy (AFM) over a surface area (scan area) less than or equal to 30 µm x 30 µm. The measured surface area may, for example, extend over 5 µm x 5 µm, 1 µm x 1 µm, 20 µm x 20 µm, or 30 µm x 30 µm. These areas will be referred to hereafter as PV roughness and root mean square (RMS) roughness.
[0034] It should be noted that obtaining a very good surface finish on a p-SiC substrate is complex due to the hardness of the material and the polycrystalline structure: mechanical or mechano-chemical polishing can generate the formation of scratches on the surface of the substrate and the appearance of defects (holes) due to the untimely removal of p-SiC grains from the surface.
[0035] An example of the surface condition of an initial substrate 2 is given in [Fig. 2]. Although the RMS roughness remains below Inm, a PV roughness exceeding 30 nm is observed due to the presence of scratches on the surface. Such a surface condition is likely to generate physical defects (holes) at the future interface between the substrate and the thin film of the composite structure 100: this leads to a degradation of the quality and integrity of the transferred thin film as well as the electrical conductivity of the interface.
[0036] Typically, within the framework of the present invention, the initial substrate 2 can have a PV surface roughness of up to a few micrometers, which greatly relaxes the manufacturing or supply constraints of the initial substrate 2.
[0037] The surface condition of the rear face 2b of the initial substrate 2 is not specified here. It may be similar to that of the front face 2a or more degraded, provided that it does not globally affect the curvature or the quality (defectiveness) of the initial substrate 2.
[0038] To accommodate the surface condition of the initial substrate 2, the manufacturing process according to the invention includes a step b) comprising a centrifugal coating deposition, at least on the front face 2a of the initial substrate 2, of a layer of polymer resin 3 ([Fig. 1b]). An important characteristic of this layer is that it contains preformed carbon-carbon (CC) bonds in three dimensions (3D). In this layer, the carbon-based polymer chains, which have CC bonds, are randomly dispersed in a solvent: they thus exhibit a more or less random 3D structure. The more randomly these chains are dispersed in 3D, the less graphitization will be favored and the closer a glassy state will be achieved during crosslinking.
[0039] Here, a layer of polymer resin 3 is favoured, leading to the highest possible amorphous / crystalline ratio, after crosslinking, for obtaining a glassy carbon film 30, at the end of a subsequent step d) of the process.
[0040] The polymer resin can be formed from coal tar, phenol formaldehyde, polyfurfuryl alcohol, polyvinyl alcohol, polyacrylonitrile, polyvinylidene chloride, and / or polystyrene, etc.
[0041] By way of example, known photosensitive resins, commonly used for photolithography steps in the field of microelectronics, can be used, such as commercial products:
[0042] - AZ-5214, AZ-4330, AZ-P4620 (registered trademarks) (based on l-methoxy-2-propanol acetate, diazonaphthoquinonesulfonic esters, 2-methoxy-l-propanol acetate, Cresol novolak resin),
[0043] - OCG-825 (based on ethyl-3-ethoxypropionate),
[0044] - SU-8 2000 (based on cyclopentanone, triarylsulfonium / hexafluoroantimonate salts, propylene carbonate, epoxy resin).
[0045] Epoxy resins, such as for example the Epoxy Novolac EPON product (registered trademark) offered to coat and protect various surfaces in various fields (aeronautics, marine, automotive, construction...), can also be implemented in step b) of the process according to the invention.
[0046] The centrifugal spreading carried out in step b) requires that the polymer resin solution be in viscous form.
[0047] This deposition method is particularly advantageous because the viscous solution fills the hollows (holes and scratches) present on the surface of the initial substrate 2 and therefore effectively flattens these microreliefs.
[0048] The thickness of the polymer resin layer 3 deposited in step b) can typically vary between a few hundred nanometers (e.g. 500nm) and several microns (e.g. 3 to 5 µm).
[0049] The manufacturing process then includes a step c) consisting of applying an anneal (called first anneal), with a plateau at a temperature between 120°C and 180°C, to the initial substrate 2 coated with the polymer resin layer 3 ([Fig. 1e]). The plateau can last from a few minutes (typically 30 min) to a few hours (typically 2 h). A gradual temperature increase, namely between 1°C / min and 5°C / min, from ambient temperature to the plateau is preferred, so as to gradually degas the polymer resin layer 3 and to remove the solvent and impurities initially present in the viscous solution.
[0050] Intermediate stages may also be provided in the thermal cycle of the first annealing, depending on the nature of the polymer resin.
[0051] Following the first annealing, the polymer resin layer 3' is crosslinked, and therefore solidified against the front surface 2a of the initial substrate 2. Crosslinking is characterized by the formation of bonds between the carbon chains, which will result in the solidification of the layer 3'. The arrangement, in the crosslinked polymer resin layer 3', of the polymer chains in 3 dimensions will influence the 3-dimensional orientation of the sp2-type bonding chains during the next step d) of the process.
[0052] Finally, the manufacturing process includes a step d) consisting of applying a second annealing treatment with a plateau at a temperature above 600°C, preferably above 700°C, under a neutral atmosphere, to transform the crosslinked polymer resin layer 3' into a glassy carbon film 30 ([Fig. 1d]). The plateau temperature can, for example, be 650°C, 750°C, 800°C, or even 850°C, or higher. The temperature of this plateau can reach up to approximately 1800°C, taking care to remain compatible with the nature of the second material composing the initial substrate 2.
[0053] This second annealing causes carbonization of the cross-linked layer 3'. It is essential that this carbonization gives rise to a glassy carbon structure, which exhibits sp2-type carbon-carbon (CC) atomic bonds. The structure of glassy carbon can be characterized by Raman spectroscopy, with a particular band signature (G-band), or by ellipsometry, with a specific absorption signature as is known in the literature.
[0054] The glassy carbon film 30 advantageously has 100% sp2-type CC atomic bonds; if inclusions of another phase are present in the film 30, it may be tolerated that the percentage of sp2 atomic bonds be greater than 95%, or preferably greater than 99%.
[0055] The neutral atmosphere of the second annealing is typically argon-based and / or under vacuum (i.e., at a pressure below atmospheric pressure and up to a few mbar). The second annealing is carried out with a temperature increase ranging from 5°C / min to 15°C / min, and up to 50°C / min, or even 100°C / min, from ambient temperature to the holding point. The holding point duration can vary from a few minutes (e.g., 30 min) to a few hours (e.g., 2 h).
[0056] The vitreous carbon film 30 typically has a thickness between a few hundred nanometers (typically 500-600nm) and a few micrometers (typically 1, 2, 3 or 4pm).
[0057] It is important to take into account the shrinkage that the viscous layer of polymer resin 3 (deposited in step b) of the process) will undergo during the first annealing (step c) and especially during the second annealing (step d), in order to define its sufficient initial thickness for obtaining the target thickness of the glassy carbon film 30. The shrinkage in thickness can typically be between 70% and 95%. The carbon ratio, that is, the ratio between the mass of the glassy carbon film 30 and the initial mass of the spread polymer resin layer 3, must be at least 5%, preferably greater than 50%.
[0058] The initial substrate 2 equipped with the glassy carbon film 30 corresponds to the support substrate 20 according to the present invention. Figure 3 shows an example of the surface finish of the support substrate 20 on its front face 20a, i.e., on the free face of the glassy carbon film 30. A root mean square roughness of less than or equal to 0.8 nm RMS and a peak-to-pit roughness of less than or equal to 7 nm PV can be obtained, starting from the roughnesses of the initial substrate 2 shown in Figure 2. The roughnesses are again measured by atomic force microscopy over a surface area of less than or equal to 30 µm x 30 µm.
[0059] The surface finish is significantly improved compared to surface 2a of the initial substrate 2; there is a strong absorption of scratches and other pit defects, and a roughness typically less than or equal to Inm RMS and 1Onm PV. This surface finish is particularly favorable for direct bonding with a very good interface quality.
[0060] Advantageously, the manufacturing process according to the invention includes, after step d), a step e) of mechanical and / or mechano-chemical polishing of the vitreous carbon film 30, to adjust its thickness or to further improve its surface roughness.
[0061] At the end of step e), the target is for example an RMS roughness of less than Inm, or even 0.5nm, and a PV roughness of less than 5nm.
[0062] In addition, the vitreous carbon film 30 exhibits excellent electrical conductivity characteristics, with a resistivity typically less than 6.10 3ohm.cm.
[0063] The mechanical, electrical and thermal properties of the glassy carbon film 30 make the support substrate 20 an excellent candidate for the fabrication of a composite structure 100 by transferring a thin layer 10 of single-crystal silicon carbide (c-SiC) onto said support substrate 20.
[0064] Note that these mechanical, electrical and thermal properties are also an advantage in a composite structure 100 whose support substrate 20 would include, for example, an initial substrate 2 in p-AIN and whose thin layer 10 would be, for example, in c-GaN, or other combinations of first and second materials.
[0065] Returning to the description of a SiC-based composite structure, the manufacturing process according to the invention can thus include a step f) of transferring a thin layer 10 in c-SiC onto the glassy carbon film 30.
[0066] There are various options, known from the prior art, for carrying out a thin film transfer, which will not be described exhaustively here.
[0067] According to a preferred mode, step f) of the process involves the implantation of light species according to the principle of the Smart Cut® process.
[0068] In a first phase (f1), a donor substrate 1 of single-crystal silicon carbide, from which the thin film 10 will be produced, is provided ([Fig. 4a]). The donor substrate 1 is preferably in the form of a wafer with a diameter of 100 mm, 150 mm, 200 mm, or even 300 mm (identical to or very close to that of the support substrate 20) and a thickness typically between 300 µm and 800 µm. It has a front face (la) and a back face (la). The surface roughness of the front face (la) is advantageously chosen to be less than 1 m RMS, or even less than 0.5 nm RMS, measured by atomic force microscopy (AFM) over a surface area, for example, of 20 µm x 20 µm. The donor substrate 1 can be of polytype 4H or 6H, and have n- or p-type doping, depending on the needs of the components that will be developed on and / or in the thin layer 10 of the composite structure 100.
[0069] Note that the donor substrate 1 intended to form a thin layer 10 in c-GaN can be formed from a base substrate in GaN, SiC, Si(111) or sapphire on which a single-crystal GaN epitaxy will be carried out, according to the classical processes.
[0070] A second phase f2) corresponds to the introduction of light species into the donor substrate 1 to form a fragile buried plane 11 delimiting, with a front face of the donor substrate 1, the thin layer 10 to be transferred ([Fig.4b]).
[0071] The light species are preferentially hydrogen, helium, or a co-implantation of these two species, and are implanted at a predetermined depth in the donor substrate 1, consistent with the thickness of the targeted thin layer 10. These light species will form, around the predetermined depth, microcavities distributed in a thin layer parallel to the free surface la of the donor substrate 1, i.e., parallel to the (x,y) plane in the figures. For the sake of simplicity, this thin layer is called the buried fragile layer 11.
[0072] The implantation energy of the light species is chosen to reach the determined depth. For example, hydrogen ions will be implanted at an energy between 10 keV and 250 keV, and at a dose between 5E16 / cm² and 1E17 / cm², to delimit a thin film 10 with a thickness on the order of 100 nm at 1500 nm. Note that a protective layer may be deposited on the front face of the donor substrate 1, prior to the ion implantation step. This protective layer may be composed of a material such as silicon dioxide or silicon nitride, for example. It is removed prior to the next phase.
[0073] Optionally, an intermediate layer 4 can be formed on the front face of the donor substrate 1, before or after the second phase f2) of light species introduction. This intermediate layer 4 can be made of a semiconductor material or a metallic material; for example, silicon, silicon carbide, glassy or turbostratified carbon, tungsten, titanium, etc., may be chosen. The thickness of the intermediate layer 4 is advantageously limited, typically between a few nanometers and a few tens of nanometers.
[0074] If the intermediate layer 4 is formed before phase f2), the implantation energy (and potentially the dose) of the light species will be adjusted for penetration through this additional layer. If the intermediate layer 4 is formed after phase f2), care will be taken to form this layer by applying a thermal budget lower than the bubbling thermal budget, said bubbling thermal budget corresponding to the appearance of blisters on the surface of the donor substrate 1 due to excessive growth and pressure buildup of microcavities in the buried fragile plane 11.
[0075] The transfer step f) then includes a third phase f3) of assembling the donor substrate 1, on the side of its front face la, onto the support substrate 20, on the side of its first face 20a, by molecular adhesion bonding, along a bonding interface 5 to form a bonded assembly 50 (figures 4c, 4c').
[0076] Optionally, an additional layer can also be deposited on the face to be assembled of the support substrate 20 (namely on the glassy carbon layer 30), prior to the assembly phase f3); it can be chosen to be of the same nature or of a different nature from the intermediate layer 4 mentioned for the donor substrate 1. An intermediate or additional layer 4 may possibly be deposited only on one or the other of the two substrates 1,20 to be assembled.
[0077] The objective of the intermediate layer(s) is essentially to promote the bonding energy (particularly in the temperature range below 1100°C), due to the formation of covalent bonds at lower temperatures than in the case of a direct assembly without this / these intermediate layer(s); another advantage of this / these intermediate layer(s) may be to further improve the vertical electrical conductivity of the bonding interface 5.
[0078] Returning to the description of the assembly phase f3), and as is well known, direct molecular adhesion bonding does not require an adhesive material, since bonds are established at the atomic scale between the surfaces being joined. Several types of molecular adhesion bonding exist, which differ in particular in their temperature, pressure, atmospheric conditions, or pretreatments prior to contacting the surfaces. Examples include room-temperature bonding with or without prior plasma activation of the surfaces to be joined, atomic diffusion bonding (ADB), surface-activated bonding (SAB), etc.
[0079] The assembly phase f3) may include, prior to bringing the faces la,20a to be assembled into contact, conventional sequences of chemical cleaning (for example, RCA cleaning), surface activation (for example, by oxygen or nitrogen plasma) or other surface preparations (such as scrubbing), which may promote the quality of the bonding interface 5 (low defectivity, high adhesion energy).
[0080] Finally, a fourth phase f4) includes the separation along the buried fragile plane 11, which leads to the transfer of the thin layer 10 onto the supporting substrate 20 ([Fig.4d]).
[0081] The separation along the fragile buried plane 11 is usually achieved by applying a heat treatment to the bonded assembly 50, at a temperature between 800°C and 1200°C (in the described case of a SiC-based bonded assembly 50). Of course, this temperature depends heavily on the nature of the first and second materials involved in the bonded assembly 50, as is known to those skilled in the art, and will naturally be adjusted according to the materials chosen.
[0082] Such heat treatment induces the development of cavities and microcracks in the buried brittle plane 11, and their pressurization by the light species present in gaseous form, until a fracture propagates along said brittle plane 11. Alternatively or concurrently, mechanical stress may be applied to The bonded assembly 50, particularly at the level of the buried weak plane 11, is designed to propagate or mechanically assist in propagating the fracture leading to separation. Following this separation, the composite structure 100, comprising the supporting substrate 20 and the transferred single-crystal thin film 10, is obtained on the one hand, and the remaining portion 1' of the donor substrate on the other. The level and type of doping of the thin film 10 are defined by the chosen properties of the donor substrate 1 or can be adjusted subsequently using known semiconductor layer doping techniques.
[0083] The free surface 10a of the thin film 10 is usually rough after separation: for example, it has a roughness between 5 nm and 100 nm RMS (AFM, 20 sq m x 20 sq m scan). Cleaning and / or smoothing phases can be applied to restore a good surface finish (typically, a roughness of less than a few angstroms RMS, on a 20 sq m x 20 sq m AFM scan). In particular, these phases can include a mechano-chemical smoothing treatment of the free surface of the thin film 10. A removal of between 50 nm and 300 nm effectively restores the surface finish of said layer 10. They can also include at least one heat treatment, for example at a temperature between 1300°C and 1800°C in the case of the SiC-based composite structure 100.
[0084] Such a heat treatment is applied to remove residual light species from the thin film 10 and to promote the rearrangement of its crystal lattice. It also strengthens the bonding interface 5.
[0085] The heat treatment may also include or correspond to a silicon carbide epitaxy on the thin layer 10.
[0086] The support substrate 20, and in particular the glassy carbon film 30, is perfectly compatible with the potentially very high temperature heat treatments applied during the development of the composite structure 100.
[0087] Finally, it should be noted that the transfer step f) may include a reconditioning step of the remainder 1' of the donor substrate for reuse as a donor substrate 1 for a new composite structure 100. Mechanical and / or chemical treatments, similar to those applied to the composite structure 100, may be implemented at the front face l'a of the remaining substrate 1'.
[0088] The composite structure 100 obtained comprises a thin layer 10 of monocrystalline silicon carbide disposed on the support substrate 20, said support substrate 20 including an initial substrate 2 of polycrystalline silicon carbide and a glassy carbon film 30, in contact with the front surface 2a of the initial substrate 2.
[0089] As mentioned previously with reference to the manufacturing process according to the invention, the composite structure 100 is described here in the case of a first c-SiC material and a second p-SiC material. The invention also relates to a composite structure 100 based on other pairs of first and second materials (stated non-exhaustively above), including a composite structure 100 comprising a thin layer of c-GaN and an initial substrate 2 (included in the support substrate 20) of p-AlN.
[0090] An intermediate layer 4 and / or an additional layer as referred to in the process may optionally be intercalated between the vitreous carbon film 30 and the thin layer 10.
[0091] Such a composite structure 100 is extremely robust to the high-temperature heat treatments that may be applied to manufacture components on and / or in said layer 20. The composite structure 100 according to the invention is particularly suitable for the fabrication of one (or more) high-voltage microelectronic component(s), such as, for example, Schottky diodes, MOSFET transistors, etc. More generally, it meets the requirements of power microelectronic applications, allowing excellent vertical electrical conductivity, good thermal conductivity, and providing a useful layer of high-quality single-crystal material.
[0092] Of course, the invention is not limited to the embodiments described and alternative embodiments can be made without departing from the scope of the invention as defined by the claims.
Claims
Claims
1. A method of manufacturing a composite structure (100) comprising a thin layer (10) of a first monocrystalline material arranged on a support substrate (20), the manufacturing method comprising the following steps: a) providing an initial substrate (2) of a second polycrystalline material, b) depositing by spin coating, at least on a front face (2a) of the initial substrate (2), a layer of polymer resin (3) comprising carbon-carbon bonds preformed in three dimensions, c) applying a first annealing at a temperature between 120°C and 180°C to the initial substrate (2) provided with the layer of polymer resin (3), to form a layer of crosslinked polymer resin (3'), d) applying a second annealing at a temperature above 600°C, under a neutral atmosphere,to transform the crosslinked polymer resin layer (3') into a vitreous carbon film (30) f) transferring the thin layer (10) formed from the first monocrystalline material, directly onto the vitreous carbon film (30) or via an intermediate layer (4), said transfer involving a bonding interface (5) by molecular adhesion, between one face of the vitreous carbon film (30) and one face of the thin layer (10), or between one face of the vitreous carbon film (30) and one face of an intermediate layer (4) arranged between said vitreous carbon film (30) and the thin layer (10).,
2. Manufacturing method according to the preceding claim, comprising, after step d), a step e) of mechanical and / or chemical-mechanical polishing of the vitreous carbon film (30).
3. A manufacturing method according to the preceding claim, wherein the polymer resin (3) is based on coal tar, phenol formaldehyde, polyfurfuryl alcohol, polyvinyl alcohol, polyacrylonitrile, polyvinylidene chloride, and / or polystyrene.
4. Manufacturing method according to one of the preceding claims, in which step f) implements an assembly between a donor substrate (1) comprising the first monocrystalline material, from which the thin layer (10) will be produced, and the vitreous carbon film (30), to form a bonded assembly (50).
5. Manufacturing method according to the preceding claim, in which: - the donor substrate (1) comprises a buried fragile plane (11) which delimits, with a front face (la) of said substrate (1), the thin layer (10) to be transferred, and - step f) implements a separation of the bonded assembly (50) along the buried fragile plane (11), to give rise on the one hand, to a composite structure (100) including the thin layer (10) arranged on the vitreous carbon film (30), itself arranged on the initial substrate (2), and on the other hand, the remainder of the donor substrate (1).
6. Manufacturing method according to one of the preceding claims, in which the first monocrystalline material is chosen from silicon carbide, gallium nitride, silicon, silicon-germanium, germanium, III-V compounds, or other semiconductor materials, or from piezoelectric materials.
7. Manufacturing method according to one of the preceding claims, in which the second polycrystalline material is chosen from silicon carbide, aluminum nitride, silicon, silicon-germanium, germanium, III-V compounds or other semiconductor materials, or from piezoelectric materials.
8. A manufacturing method according to one of the preceding claims, wherein the first material and the second material are semiconductors.
9. Composite structure (100) comprising a thin layer (10) of a first monocrystalline material arranged on a support substrate (20), said support substrate (20) including: - an initial substrate (2) of a second polycrystalline material, - a glassy carbon film (30), in contact with the front surface (2a) of the initial substrate (2), the composite structure (100) further comprising an interface (5) for bonding by molecular adhesion, between a face of the glassy carbon film (30) and a face of the thin layer (10) or between a face of the glassy carbon film (30) and a face of an intermediate layer (4) arranged between said glassy carbon film (30) and the thin layer (10).
10. Composite structure (100) according to the preceding claim in which the initial substrate (2) has a surface roughness of between 10m and 2pm peak-to-trough, measured by atomic force microscopy over a surface area less than or equal to 30qm x 30qm.
11. Composite structure (100) according to one of the two preceding claims- preceding, in which the glassy carbon film (30) has a thickness of between 100nm and 4pm.
12. Composite structure (100) according to the preceding claim comprising an intermediate layer (4), between the thin layer (10) and the glassy carbon film (30), chosen from silicon, silicon carbide, carbon, tungsten or titanium.
13. Composite structure (100) according to one of claims 9 to 12, in which the first monocrystalline material is chosen from silicon carbide, gallium nitride, or other semiconductor materials, and the second polycrystalline material is chosen from silicon carbide, aluminum nitride, or other semiconductor materials.