Heavy-duty tires for vehicles

A tire tread composition with a highly saturated diene elastomer and carbon black filler addresses the balance between wet grip, wear resistance, and rolling resistance, improving tire durability.

FR3143033B1Active Publication Date: 2024-11-29MICHELIN & CO (CIE GEN DES ESTAB MICHELIN)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
FR2022013185
Authority / Receiving Office
FR · FR
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-12-12
Publication Date
2024-11-29
Estimated Expiration
2042-12-12

AI Technical Summary

Technical Problem

Existing tires face a challenge in achieving a balance between wet grip performance, wear resistance, and rolling resistance, particularly when using highly saturated diene elastomers, as improving one property often deteriorates another.

Method used

A tire tread composition comprising a rubber mixture with a highly saturated diene elastomer random copolymer of ethylene and 1,3-butadiene, combined with a high content of carbon black filler, maintains a balance between wet grip, wear resistance, and rolling resistance.

Benefits of technology

The tire composition achieves improved wet grip performance while maintaining a good compromise between wear resistance and rolling resistance, enhancing overall tire durability.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a tire for use on a vehicle carrying heavy loads, comprising a tread whose portion intended to be in contact with the road surface is made entirely or partially of a rubber compound. This rubber compound comprises more than 50 parts per million (ppm) of a highly saturated diene elastomer, which is a random copolymer of ethylene and 1,3-butadiene containing between 55% and 65% by mole of ethylene units, and between 30% and 55% of a reinforcing filler containing carbon black at a mass percentage greater than 90% of the mass of the reinforcing filler and less than or equal to 100% of the mass of the reinforcing filler. A tire according to the invention exhibits a good compromise between wet grip, wear resistance, and rolling resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: Pneumatic tire for a vehicle carrying heavy loads

[0001] The field of the present invention is that of tires which are intended to equip vehicles transporting heavy loads and whose tread consists entirely or partly of a rubber composition reinforced with carbon black and rich in a highly saturated diene elastomer.

[0002] A tire must meet a large number of technical requirements, often contradictory, including high wear resistance, low rolling resistance, and high grip.

[0003] It is known that the grip performance of a tire can be improved by increasing the contact surface of the tread on the rolling surface. One solution consists of using a very deformable tread, in particular a very soft rubber composition which constitutes the surface of the tread intended to come into contact with the rolling surface. The use of a very soft rubber composition, although favorable for grip, can lead to a degradation of the wear resistance of the tire. Indeed, to improve wear resistance, it is known that a certain rigidity of the tread is desirable, this stiffening of the tread being able to be obtained for example by increasing the rate of reinforcing filler in the rubber compositions constituting these treads.Unfortunately, experience shows that such stiffening of the tread penalizes in a known manner, most often in a prohibitive manner, the rolling resistance properties, due to a significant increase in the hysteretic losses of the rubber composition. It is also known that a low hysteresis of the rubber composition is required to minimize rolling resistance while a dissipative rubber composition favors grip performance.

[0004] To improve the compromise between wear resistance and rolling resistance, it has been proposed in WO 2014114607 A1 to use in tire rubber compositions highly saturated diene elastomers such as copolymers of ethylene and 1,3-butadiene which contain more than 50 mol% of ethylene unit. Nevertheless, there is still a need to improve the wet grip performance of tires whose tread is made of a rubber composition comprising highly saturated diene elastomers while maintaining a good compromise between wear resistance performance and rolling resistance performance.

[0005] This objective is achieved in that the inventors have discovered that a specific rubber composition makes it possible to provide a tire having an improved compromise between wet grip performance, wear resistance and rolling resistance, in particular improved wet grip performance while maintaining a good compromise between wear resistance performance and rolling resistance performance.

[0006] Thus, an object of the invention is a tire intended to equip a vehicle carrying heavy loads which comprises a tread, the portion of which intended to be in contact with the rolling ground is made up entirely or in part of a rubber composition, which rubber composition comprises more than 50 pce of a highly saturated diene elastomer which is a random copolymer of ethylene and 1,3-butadiene which contains between 55% and 65% by mole of ethylene units, between 30 pce and 55 pce of a reinforcing filler which contains a carbon black at a mass content greater than 90% of the mass of the reinforcing filler and less than or equal to 100% of the mass of the reinforcing filler. Detailed description

[0007] Any range of values ​​designated by the expression "between a and b" represents the range of values ​​greater than "a" and less than "b" (i.e., excluding the limits a and b) while any range of values ​​designated by the expression "from a to b" means the range of values ​​from "a" to "b" (i.e., including the strict limits a and b).

[0008] The abbreviation "pce" means parts by weight per hundred parts of elastomer (of the total elastomers if several elastomers are present).

[0009] The compounds mentioned in the description may be of fossil or bio-sourced origin. In the latter case, they may be, partially or totally, derived from biomass or obtained from renewable raw materials derived from biomass. In the same way, the compounds mentioned may also come from the recycling of materials already used, that is to say they may be, partially or totally, derived from a recycling process, or obtained from raw materials themselves derived from a recycling process.

[0010] In the present invention, the term "tyre" means a pneumatic or non-pneumatic bandage. A pneumatic bandage usually comprises two beads intended to come into contact with a rim, a crown composed of at least one crown reinforcement and a tread, two sidewalls, the tire being reinforced by a carcass reinforcement anchored in the two beads. A non-pneumatic bandage, for its part, usually comprises a base, designed for example for mounting on a rigid rim, a crown reinforcement, ensuring the connection with a tread and a deformable structure, such as spokes, ribs or cells, this structure being arranged between the base and the crown. Such non-pneumatic bandages do not necessarily include a sidewall. Non-pneumatic bandages are described for example in documents WO 03 / 018332 and FR2898077. According to any one of the embodiments of the invention, the tire according to the invention is preferably a pneumatic bandage.

[0011] Unless otherwise indicated, the levels of units resulting from the insertion of a monomer into a copolymer such as the highly saturated diene elastomer useful for the purposes of the invention are expressed as a molar percentage relative to the total monomer units of the copolymer.

[0012] As is known, the expression “ethylene unit” refers to the -(CH2-CH 2)- unit resulting from the insertion of ethylene into the copolymer chain.

[0013] The highly saturated diene elastomer useful for the purposes of the invention is a random copolymer of ethylene and 1,3-butadiene, which implies that the monomer units of the copolymer distributed statistically are those resulting from the copolymerization of ethylene and 1,3-butadiene. The copolymer therefore contains ethylene units and butadiene units. In a known manner, an ethylene unit is a monomer unit of the unit -(CH2-CH2)-. Also in a known manner, a butadiene unit is a monomer unit of the unit -CH2-CH(CH=CH2)- (1,2 unit) or -CH2 -CH=CH-CH2- (1,4 unit) depending on whether the 1,3-butadiene monomer is inserted into the polymer chain during the polymerization reaction by a 2,1 or 1,4 addition. The molar ratio of ethylene units in the highly saturated diene elastomer is greater than 55% of the monomer units of the highly saturated diene elastomer and less than 65% of the monomer units of the highly saturated diene elastomer.Outside the range defining the ethylene unit content according to the invention, the performance compromise between wet grip, rolling resistance and wear resistance is not as good. For values ​​equal to or less than 55%, the wear resistance performance is reduced; for values ​​greater than or equal to 65%, the wet grip performance is reduced. The molar content of ethylene units in the highly saturated diene elastomer is preferably greater than 55% and less than or equal to 63%, more preferably greater than or equal to 58% and less than or equal to 62%, of the monomer units of the highly saturated diene elastomer.

[0014] The highly saturated diene elastomer can be obtained according to different synthesis methods known to those skilled in the art, in particular depending on the targeted microstructure of the highly saturated diene elastomer. Generally, it can be prepared by copolymerization of 1,3-butadiene and ethylene and according to methods of known synthesis, in particular in the presence of a catalytic system comprising a metallocene complex. Mention may be made in this respect of catalytic systems based on metallocene complexes, which catalytic systems are described in documents EP 1 092 731 A1, WO 2004035639 A1, WO 2007054223 A2 and WO 2007054224 A2 in the name of the Applicant. The highly saturated diene elastomer can also be prepared by a process using a preformed type catalytic system such as those described in WO 2017093654 A1, WO 2018020122 A1 and WO 2018020123 A1. Advantageously, the diene elastomer is prepared according to a semi-continuous or continuous process such as described in WO 2017103543 A1, WO 201713544 A1, WO 2018193193 A1 and WO 2018193194 A1.

[0015] The highly saturated diene elastomer preferably contains units of formula (I) or units of formula (II), unit 1,2. -CHs-CHfC^CHj- (h)

[0016] The presence of saturated 6-membered cyclic unit, 1,2-cyclohexane unit, of formula (I) in the copolymer may result from a series of very specific insertions of ethylene and 1,3-butadiene into the polymer chain during its growth. When the highly saturated diene elastomer comprises units of formula (I) or units of formula (II), the molar percentages of the units of formula (I) and the units of formula (II) in the highly saturated diene elastomer, respectively o and p, preferably satisfy the following equation (eq. 1) or equation (eq. 2), o and p being calculated on the basis of all the monomer units of the highly saturated diene elastomer. 0 < o+p < 30 (eq. 1) 0 < o+p < 25 (eq. 2)

[0017] Preferably, the highly saturated diene elastomer comprises units of formula (I) in a molar ratio greater than 0% and less than 15%, more preferably less than 10% molar, molar percentage calculated on the basis of all the monomer units of the highly saturated diene elastomer.

[0018] According to a particularly preferred embodiment, the highly saturated diene elastomer contains 1,4 units of trans configuration (1,4-trans units). When the diene elastomer contains 1,4-trans units, the 1,4-trans units represent more than 50 mol% of the 1,4 units of the highly saturated diene elastomer, preferably more than 80 mol% of the 1,4 units of the highly saturated diene elastomer.

[0019] The highly saturated diene elastomer may consist of a mixture of highly saturated diene elastomers which differ from each other by their microstructures or by their macrostructures.

[0020] The level of the highly saturated diene elastomer in the rubber composition is greater than 50 parts by weight per hundred parts of elastomer of the rubber composition (phr). It typically varies in a range from more than 50 phr up to 100 phr. Below the indicated minimum, the intended technical effect is insufficient. The greater the level of the highly saturated diene elastomer in the rubber composition, the greater the intended technical effect.

[0021] In the case where the highly saturated diene elastomer consists of a mixture of highly saturated diene elastomers which differ from each other by their microstructures or by their macrostructures, the level of the highly saturated diene elastomer in the rubber composition relates to the mixture of highly saturated diene elastomers.

[0022] The rubber composition may contain, in addition to the highly saturated diene elastomer, a second diene elastomer. A diene elastomer is understood to mean an elastomer consisting at least in part (i.e., a homopolymer or a copolymer) of diene monomer units (monomers bearing two carbon-carbon double bonds, conjugated or not). The second elastomer may be chosen from the group of highly unsaturated diene elastomers consisting of polybutadienes, polyisoprenes, butadiene copolymers, isoprene copolymers and their mixture. A highly unsaturated diene elastomer is an elastomer which contains more than 50 mol% of diene units.

[0023] The level of highly saturated diene elastomer in the rubber composition is preferably greater than 80 pce, more preferably greater than 90 pce, advantageously equal to 100 pce.

[0024] The rubber composition comprises any type of so-called reinforcing filler, known for its ability to reinforce a rubber composition, in particular usable for the manufacture of a tire tread. Such a reinforcing filler typically consists of nanoparticles whose average size (by mass) is less than one micrometer, generally less than 500 nm, most often between 20 and 200 nm, in particular and more preferably between 20 and 150 nm. The level of the reinforcing filler in the rubber composition is between 30 pce and 55 pce, preferably varies from 35 pce to 50 pce, more preferably The reinforcing filler contains more than 90% by mass to 100% by mass of a carbon black, mass percentages calculated relative to the mass of the reinforcing filler of the rubber composition. Preferably, the mass content of carbon black in the rubber composition is greater than 95% of the mass of the reinforcing filler of the rubber composition and less than or equal to 100% of the mass of the reinforcing filler of the rubber composition.When the mass content of carbon black in the rubber composition is less than 100% of the mass of the reinforcing filler of the rubber composition, the reinforcing filler may therefore comprise any type of filler other than carbon black which is also known for its ability to reinforce a rubber composition which can be used for the manufacture of tires, for example a reinforcing inorganic filler such as silica with which a coupling agent is associated in a known manner. Advantageously, the mass content of carbon black in the rubber composition is equal to 100% of the mass of the reinforcing filler of the rubber composition.

[0025] Preferably, the carbon black has a BET specific surface area greater than 90 m2 / g. More preferably, the BET specific surface area of ​​the carbon black is greater than 100 m2 / g. Preferably, the carbon black has a specific surface area less than 145 m2 / g. The BET specific surface area is typically measured according to ASTM D6556-09 [multipoint method (5 points) - gas: nitrogen - relative pressure range P / P0: 0.05 to 0.30].

[0026] Preferably, the rubber composition contains from 0 phr to less than 5 phr of plasticizer chosen from liquid plasticizers, plasticizing hydrocarbon resins and mixtures thereof. In other words, the total level of plasticizers in the rubber composition, whether liquid plasticizers, plasticizing hydrocarbon resins or mixtures thereof, preferably varies from 0 phr to less than 5 phr, more preferably from 0 phr to less than 3 phr, better still is equal to 0 phr.

[0027] A plasticizer is considered liquid when, at 23°C, it has the capacity to eventually take the shape of its container, this definition being given in contrast to plasticizing resins which are by nature solid at room temperature. Examples of liquid plasticizers include vegetable oils, mineral oils, ether, ester, phosphate, sulfonate plasticizers and their mixtures.

[0028] Plasticizing hydrocarbon resins are polymers well known to those skilled in the art, essentially based on carbon and hydrogen atoms but which may contain other types of atoms, for example oxygen, which can be used in particular as plasticizing agents or tackifying agents in polymer matrices. They are by nature at least partially miscible (i.e., compatible) at the levels used with the polymer compositions for which they are intended, so as to act as true diluting agents. They have been described for example in the work entitled "Hydrocarbon Resins" by R. Mildenberg, M. Zander and G. Collin (New York, VCH, 1997, ISBN 3-527-28617-9) whose chapter 5 is devoted to their applications, notably in pneumatic rubber (5.5. "Rubber Tires and Mechanical Goods"). As is known, these hydrocarbon resins can also be described as thermoplastic resins in the sense that they soften upon heating and can thus be molded.

[0029] Preferably, the rubber composition is free of reinforcing resin, also known as "resin cure" in English. Reinforcing resins are for example described in the document "Compounding and Vulcanization" by R. Rajesh Babu, GS Shibulal, Arup K. Chandra and Kinsuk Naskar in "Advances in Elastomers", pp 83-135, 2013, Edition Springer, as well as in document WO 0210269 A2. They are known to increase the rigidity of a rubber composition by creating a three-dimensional network in the rubber composition after curing the rubber composition. The best known are those which implement a two-component system based on a phenolic compound such as a derivative of phenol or resorcinol and a methylene donor such as hexamethylenetetramine (HMT).

[0030] The rubber composition may also comprise all or part of the usual additives normally used in elastomer compositions intended to constitute treads, such as, for example, crosslinking agents, pigments, protective agents such as anti-ozone waxes, chemical anti-ozonants, antioxidants.

[0031] The rubber composition preferably contains a vulcanization system according to any one of the embodiments of the invention. The vulcanization system typically comprises sulfur and a vulcanization accelerator.

[0032] Sulfur is typically provided in the form of molecular sulfur or a sulfur donor agent, preferably in molecular form. Sulfur in molecular form is also referred to as molecular sulfur. A sulfur donor is any compound that releases sulfur atoms, combined or not in the form of a polysulfide chain, capable of being inserted into the polysulfide chains formed during vulcanization and bridging the elastomer chains. The sulfur content in the rubber composition is preferably less than 2 phr, preferably between 0.3 and 1.5 phr.

[0033] Any compound capable of acting as a vulcanization accelerator for diene elastomers in the presence of sulfur can be used as a vulcanization accelerator (primary or secondary), in particular thiazole-type accelerators and their derivatives, sulfenamide-type accelerators for diene elastomers. primary accelerators, such as guanidines, thiurams, dithiocarbamates, dithiophosphates, thioureas and xanthates as secondary accelerators. Guanidine is understood to mean any compound containing the divalent radical -HN-C(=NH)-NH-. Guanidine is preferably diphenylguanidine. The vulcanization accelerator is used at a preferential rate of between 0.3 and 5 pce, more preferably between 0.5 and 2.5 pce.

[0034] Examples of primary accelerators include sulfenamide compounds such as N-cyclohexyl-2-benzothiazyl sulfenamide ("CBS"), N,N-dicyclohexyl-2-benzothiazyl sulfenamide ("DCBS"), N-tert-butyl-2-benzothiazyl sulfenamide ("TBBS"), and mixtures of these compounds. The primary accelerator is preferably a sulfenamide, more preferably N-cyclohexyl-2-benzothiazyl sulfenamide.

[0035] Examples of secondary accelerators that may be mentioned include thiuram polysulfides, preferably thiuram disulfides such as tetraethylthiuram disulfide, tetrabutylthiuram disulfide ("TBTD"), tetrabenzylthiuram disulfide ("TBZTD") and mixtures of these compounds. The secondary accelerator is preferably a thiuram disulfide, more preferably tetrabenzylthiuram disulfide.

[0036] The primary accelerator is preferably a sulfenamide. When the primary vulcanization accelerator is a sulfenamide, it is preferably N-cy-clohexyl-2-benzothiazyl sulfenamide.

[0037] The vulcanization accelerator is preferably a mixture of a primary accelerator and a secondary accelerator. The term "a primary accelerator" designates a single primary accelerator or a mixture of primary accelerators. Similarly, the term "a secondary accelerator" designates a single secondary accelerator or a mixture of secondary accelerators. When the vulcanization accelerator is a mixture of a primary accelerator and a secondary accelerator, the vulcanization accelerator is preferably a mixture of a sulfenamide and a thiuram disulfide or a mixture of a sulfenamide, a thiuram disulfide and a guanidine, the sulfenamide preferably being N-cyclohexyl-2-benzothiazyl sulfenamide, the thiuram disulfide preferably being tetrabenzylthiuram disulfide, the guanidine preferably being diphenylguanidine.

[0038] As is well known, the vulcanization system may also comprise vulcanization activators such as metal oxides such as zinc oxide or fatty acids such as stearic acid.

[0039] The rubber composition can be manufactured in suitable mixers, using two successive preparation phases according to a general procedure well known to those skilled in the art: a first phase of thermomechanical working or mixing (sometimes referred to as the "non-productive" phase) at high temperature, up to a maximum temperature of between 110°C and 190°C, preferably between 130°C and 180°C, followed by a second phase of mechanical working (sometimes referred to as the "productive" phase) at a lower temperature, typically below 110°C, for example between 40°C and 100°C, a finishing phase during which the sulfur or sulfur donor and the vulcanization accelerator are incorporated. For example, the first (non-productive) phase is carried out in a single thermomechanical step during which all the necessary constituents, any additional processing agents and other various additives, with the exception of the sulfur and the vulcanization accelerator, are introduced into a suitable mixer such as a conventional internal mixer. The total mixing time in this non-productive phase is preferably between 1 and 15 min. After cooling the mixture thus obtained during the first non-productive phase, the sulfur and the vulcanization accelerator are then incorporated at low temperature, generally in an external mixer such as a roller mixer, and the whole is then mixed (productive phase) for a few minutes, for example between 2 and 15 min.

[0040] When the vulcanization system comprises a primary accelerator and a secondary accelerator, the rubber composition is preferably manufactured by a process which comprises a first step, step a), during which the constituents of the rubber composition are mixed by kneading, in particular thermomechanical kneading, with the exception of the sulfur and the primary accelerator, and a second step, step b), during which the sulfur and the primary accelerator are incorporated into the kneaded mixture comprising the elastomer, the reinforcing filler and the secondary accelerator. During step a), the elastomer, the reinforcing filler and the secondary accelerator are kneaded together, typically in a suitable mixer such as a conventional internal mixer. The kneading temperature in step a) is greater than 110°C, preferably between 110°C and 190°C, advantageously greater than 130°C and less than 180°C.The temperature ranges between 110°C and 190°C and between 130°C and 180°C correspond to maximum temperature values ​​reached by the mixture kneaded in the mixer during step a). Typically, the kneading during step a) is continued until the kneaded mixture reaches the maximum kneading temperature before being extracted from the mixer. The total kneading time in step a) is preferably between 1 and 15 minutes. The mixture prepared at the end of step a) is recovered, then cooled to be able to proceed to step b), which is carried out at a lower temperature, in this case at a temperature below 110°C, preferably between 40°C and 100°C. During step b), the incorporation of sulfur and . the primary accelerator in the rubber composition is typically carried out by kneading in an external mixer such as a roller mixer, generally for a period of between 2 and 15 minutes. The kneading in step b) is carried out at a temperature below 110°C, preferably between 40°C and 100°C.

[0041] Preferably, the rubber composition is extruded to form all or part of a profile of the tire tread. Then during assembly of the tire usually comprising, radially from the outside to the inside, a tread, a crown reinforcement and a carcass reinforcement, the tread is laid radially outside the crown reinforcement. Radially means in a known manner in a radial direction relative to the axis of rotation of the tire.

[0042] The tire may be in the raw state (i.e. before the tire curing step) or in the cured state (i.e. after the tire curing step). The tire is a tire for a vehicle carrying heavy loads, in particular a tire for a heavy goods vehicle or a tire for a civil engineering vehicle, preferably a tire for a heavy goods vehicle.

[0043] In summary, the invention may be implemented according to any one of the following embodiments 1 to 22:

[0044] Mode 1: Tire intended to equip a vehicle carrying heavy loads which comprises a tread of which the portion intended to be in contact with the rolling ground is made up entirely or in part of a rubber composition, which rubber composition comprises more than 50 pce of a highly saturated diene elastomer which is a random copolymer of ethylene and 1,3-butadiene which contains between 55% and 65% by mole of ethylene units, between 30 pce and 55 pce of a reinforcing filler which contains a carbon black at a mass content greater than 90% of the mass of the reinforcing filler and less than or equal to 100% of the mass of the reinforcing filler.

[0045] Mode 2: Tire according to mode 1 in which the molar rate of ethylene units in the highly saturated diene elastomer is greater than 55% and less than or equal to 63% of the monomer units of the highly saturated diene elastomer.

[0046] Mode 3: Tire according to mode 1 or 2 in which the molar rate of ethylene units in the highly saturated diene elastomer is greater than or equal to 58% and less than or equal to 62% of the monomer units of the highly saturated diene elastomer.

[0047] Mode 4: Tire according to any one of modes 1 to 3 in which the highly saturated diene elastomer comprises units of formula (I) or units of formula (II). -CH2-CH(CH=CH2)- (11)

[0048] Mode 5: Rubber composition according to mode 4 in which the highly saturated diene elastomer comprises units of formula (I) in a molar ratio greater than 0% and less than 15%.

[0049] Mode 6: Tire according to any one of modes 1 to 5 in which the highly saturated diene elastomer contains 1,4 units of trans configuration which represent more than 50% by mole of the 1,4 units of the highly saturated diene elastomer.

[0050] Mode 7: Tire according to any one of modes 1 to 6 in which the highly saturated diene elastomer contains 1,4 units of trans configuration which represent more than 80% by mole of the 1,4 units of the highly saturated diene elastomer.

[0051] Mode 8: Tire according to any one of modes 1 to 7 in which the rate of reinforcing filler in the rubber composition varies from 35 pce to 50 pce.

[0052] Mode 9: Tire according to any one of modes 1 to 8 in which the rate of reinforcing filler in the rubber composition varies from 35 pce to 45 pce.

[0053] Mode 10: Tire according to any one of modes 1 to 9 in which the mass content of carbon black in the rubber composition is greater than 95% of the mass of the reinforcing filler and less than or equal to 100% of the mass of the reinforcing filler.

[0054] Mode 11: Tire according to any one of modes 1 to 10 in which the carbon black has a BET specific surface area greater than 90 m2 / g.

[0055] Mode 12: Tire according to any one of modes 1 to 11 in which the carbon black has a BET specific surface area greater than 100 m2 / g.

[0056] Mode 13: Tire according to any one of modes 1 to 12 in which the carbon black has a BET specific surface area of ​​less than 145 m2 / g.

[0057] Mode 14: Tire according to any one of modes 1 to 13 in which the rate of highly saturated diene elastomer in the rubber composition is greater than 80 pce.

[0058] Mode 15: Tire according to any one of modes 1 to 14 in which the level of the highly saturated diene elastomer in the rubber composition is greater than 90 pce.

[0059] Mode 16: Tire according to any one of modes 1 to 15 in which the rate of highly saturated diene elastomer in the rubber composition is equal to 100 pce.

[0060] Mode 17: Tire according to any one of modes 1 to 16 in which the rubber composition contains from 0 pce to less than 5 pce of plasticizer chosen from liquid plasticizers, plasticizing hydrocarbon resins and their mixtures.

[0061] Mode 18: Tire according to any one of modes 1 to 17 in which the rubber composition contains from 0 pce to less than 3 pce of plasticizer chosen from liquid plasticizers, plasticizing hydrocarbon resins and their mixtures.

[0062] Mode 19: Tire according to any one of modes 1 to 18 in which the rubber composition contains 0 pce of plasticizer chosen from liquid plasticizers, plasticizing hydrocarbon resins and their mixtures.

[0063] Mode 20: Tire according to any one of modes 1 to 19 in which the rubber composition is free of reinforcing resin.

[0064] Mode 21: Tire according to any one of modes 1 to 20, which tire is a tire for a heavy goods vehicle or a tire for a civil engineering vehicle.

[0065] Mode 22: Tire according to any one of modes 1 to 21, which tire is a tire for a heavy goods vehicle.

[0066] The above-mentioned characteristics of the present invention, as well as others, will be better understood upon reading the following description of several exemplary embodiments of the invention, given for illustrative and non-limiting purposes. Examples

[0067] Determination of the microstructure of elastomers by magnetic resonance nuclear (NMR) j. Ethylene and 1,3-butadiene copolymers are characterized by 1H, 13C NMR spectrometry. NMR spectra are recorded on a Brüker Avance III 500 MHz Spectrometer equipped with a BBIz-grad 5 mm broadband cryoprobe. The quantitative 1H NMR experiment uses a 30° single pulse sequence and a 5-second repetition delay between each acquisition. 64 to 256 accumulations are performed. The quantitative 13C NMR experiment uses a 30° single pulse sequence with proton decoupling and a 10-second repetition delay between each acquisition. 1024 to 10240 accumulations are performed. Two-dimensional 1H / 13C experiments are used to determine the structure of the polymers. The determination of the microstructure of copolymers is defined in the literature, according to the article by Llauro et al., Macromolecules 2001, 34, 6304-6311. NMR measurements are carried out at 25°C, with the copolymers in solution in a deuterated solvent (approximately 25 mg of elastomer in 1 mL), generally deuterated chloroform (CDCl3).

[0068] Size exclusion chromatography (SEC / RI): Size exclusion chromatography (SEC) allows the fractionation of polymer chains in a solvent according to their hydrodynamic volume. Like any chromatographic system, the technique is based on the elution of a solute (the polymer) through a column containing a stationary phase. The system is composed in this order: a solvent reservoir, a pumping system, an injector, a set of columns and detectors. The measurement chain is equipped with a Waters Alliance e2695 module and a Waters fRI410 refractometer. The mobile phase is eluted with a flow rate of 1 mL / min. The polymer is solubilized in THF at a concentration of 1 g / L. A volume of 100 pL is injected through a set of 3 AGELENT size exclusion chromatography columns (MIXED B LS). The columns are thermostated in an oven at 35°C. The stationary phase of the columns is based on a polystyrene divinylbenzene gel with controlled porosity. The polymer chains are separated according to the hydrodynamic volume they occupy when solubilized in the solvent. The larger the volume they occupy, the less accessible the pores of the columns are and the shorter their elution time. Detection is ensured by a refractometer (RI) thermostated at 35°C. Each elution volume is associated with a mass via Moore calibration (certified standard passage: standard polystyrenes from Polymer Standard Service (Mainz).The WATERS: EMPOWER software is used for data acquisition and analysis. It is then possible to determine the number-average molar masses (Mn), the mass-average molar masses (Mw) as well as the dispersity (D or Ip = Mw / Mn).

[0069] Glass transition temperature of polymers: The glass transition temperature (Tg) is measured using a differential scanning calorimeter according to ASTM D3418 (1999).

[0070] Mooney Viscosity: Mooney viscosity is measured using an oscillating consistometer as described in ASTM D1646 (1999). The measurement is carried out according to the following principle: the sample analyzed in the raw state (i.e., before curing) is molded (shaped) in a cylindrical enclosure heated to a given temperature (100°C). After 1 minute of preheating, the rotor rotates within the specimen at 2 revolutions / minute and the torque needed to maintain this movement is measured after 4 minutes of rotation. Mooney viscosity (ML) is expressed in "Mooney units" (MU, with 1 MU = 0.83 Newton.meters).

[0071] Dynamic properties: The dynamic properties are measured on a viscoanalyzer (Metravib VA4000), according to ASTM D 5992-96. The response of a sample of the vulcanized composition (cylindrical specimens 4 mm thick and 400 mm2 in cross-section), subjected to sinusoidal stress in alternating simple shear, at a frequency of 10 Hz, is recorded. For the measurements of dynamic complex shear modulus (G*) and the tanô loss factor, a strain amplitude sweep is performed from 0.1% to 100% peak-peak (forward cycle), then from 100% to 0.1% peak-peak (return cycle) at 60°C. For the forward cycle, the maximum observed tanô value, noted tanô(max), is indicated; as well as the G* modulus at 50% strain, noted G*50%. The lower the value of G* at 50%, the lower the wear resistance performance; the higher the value of tanô(max), the lower the rolling resistance performance. For the measurement of tanô(-20°C), a temperature scan is carried out, under a stress of 0.7MPa, the tanô value observed at -20°C is recorded. It is recalled that in a manner well known to those skilled in the art, the value is representative of the wet grip potential: the higher the tanô(-20°C) value, the better the wet grip performance.

[0072] Preparation of rubber compositions: The elastomer, the reinforcing filler, the secondary accelerators and the various other ingredients, with the exception of the sulfur and the primary accelerator, are successively introduced into an internal mixer with a volume of 3300 cm3 (final filling rate: approximately 70% by volume), whose initial tank temperature is approximately 50°C. Thermomechanical work (non-productive phase) is then carried out in one step, lasting a total of approximately 3 to 4 minutes, until a maximum "fall" temperature of 160°C is reached. The mixture thus obtained is recovered, cooled and then the sulfur and the primary accelerator are incorporated into an external mixer (roller mixer) at 30°C, mixing everything (productive phase) for 10 minutes. The details of the formulations of the compositions are shown in Table 1. [Tables 1] Composition pce Elastomer (1) 100 N234 (2) 40 Antiozone wax (3) 1 Antioxidant (4) 2 Stearic acid (5) 1.5 ZnO (6) 2.5 DPG (7) 0.5 TBZTD (8) 0.3 CBS (9) 0.5 Sulfur 0.5 (1) One of the elastomers E1 to E6 (2) Carbon black N234 (BET of 120 m2 / g) (3) Anti-ozone wax “VARAZON 4959” from the company Sasol Wax (4) N-(l,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine “Santoflex 6PPD” from Flexys (5) Stearin “Pristerene 4931” from Uniqema company (6) Industrial grade zinc oxide from Umicore (7) Diphenylguanidine (“Perkacit DPG” from Flexsys) (8) Tetrabenzylthiuram disulfide (“Perkacit TBZTD” from Flexsys) (9) N-cyclohexyl-2-benzothiazyl sulfenamide “Santocure CBS” from the company Flexys

[0073] The compositions thus obtained are then calendered, either in the form of plates (with a thickness ranging from 2 to 3 mm) or thin sheets of rubber, for the measurement of their physical or mechanical properties after vulcanization at 140°C (cooked state), or in the form of profiles directly usable, after cutting and / or assembly to the desired dimensions, for example as semi-finished products for tires.

[0074] The tires which contain in their tread the rubber compositions C1 to C3 respectively are not in accordance with the invention; the tires which contain in their tread the rubber compositions C4 to C6 respectively are in accordance with the invention. The compositions C1 to C3 respectively contain the elastomers E1 to E3 which contain respectively 77% of ethylene unit, 74% of ethylene unit and 68% of ethylene unit; the compositions C4 to C6 respectively contain the elastomers E4 to E6 in which the rate of ethylene units is between 55% and 65%.

[0075] The statistical copolymers of ethylene and 1,3-butadiene, elastomers E1 to E6, are synthesized according to the procedures described below in the presence of a catalytic system containing a neodymium metallocene and an organomagnesium compound according to an Mg / Nd molar ratio of 2.2. For syntheses in which the polymerization is carried out with an Mg / Nd molar ratio greater than 2.2, BOMAG is added to the polymerization medium. All reagents are obtained commercially except for the metallocene which can be prepared according to the procedure described in WO 2007054224. BOMAG butyloctylmagnesium (20% in heptane, C = 0.88 mol.L *) comes from Chemtura and is transferred and stored in a Schlenk tube under an inert atmosphere. Ethylene, N35 grade, comes from Air Liquide and is used without prior purification. The catalytic system is a preformed catalytic system. It is prepared in methylcyclohexane from a metallocene, [Me2Si(Flu)2Nd(q-BH4)2Li(THF)] at 0.0065 mol / L, a co-catalyst, butyloctylmagnesium (BOMAG) whose BOMAG / Nd molar ratio is equal to 2.2, and a preformed monomer, 1,3-butadiene whose 1,3-butadiene / Nd molar ratio is equal to 90. The medium is heated to 80°C for a period of 5 hours. It is prepared according to a preparation method in accordance with paragraph II. 1 of patent application WO 2017093654 AL

[0076] The copolymer of ethylene and 1,3-butadiene, elastomer E1, is synthesized according to the procedure described below. The polymerization of ethylene and 1,3-butadiene is carried out according to a continuous process in solution in methylcyclohexane at 100°C under 10 bar in the presence of a catalytic system (71 pmoles Nd per 100 g of monomers), the mass concentration of monomer feed in the reactor being 5.5%, the mass ratio 1,3-butadiene / ethylene being 0.4, the molar ratio active Mg / Nd being 4.4. At the desired conversion (71%) to reach an Mn of approximately 140,000 g / mol, the polymerization is stopped at the line outlet using a solution of antioxidants in methylcyclohexane (1 pce of N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine and 0.9 pce of 2,2'-methylene-bis(4-methyl-6-tertbutylphenol, pce: part by weight per hundred parts of elastomer). The copolymer is recovered by a steam distillation process called "stripping" well known to those skilled in the art, then dried on a worm machine equipped with a single screw. The copolymer contains 77% ethylene unit, 9% 1,2-unit, 6% 1,4-unit (of which more than 80% is 1,4-trans) and 8% cyclic unit (1,2-cyclohexane unit). Its transition temperature is -39°C (AT of 10°C, the AT being the temperature difference between the start of the glass transition and its end), its Mn of 137,162 g / mol (Ip 1.72), its ML (1+4) at 100°C of 63.

[0077] The copolymer of ethylene and 1,3-butadiene, elastomer E2, is synthesized according to the procedure described below. The polymerization of ethylene and 1,3-butadiene is carried out according to a continuous process in solution in methylcyclohexane at 80°C under 10 bar in the presence of a catalytic system (81 pmoles Nd per 100 g of monomers), the mass concentration of monomer feed in the reactor being 6%, the mass ratio 1,3-butadiene / ethylene being 0.5, the molar ratio active Mg / Nd being 4. At the desired conversion (71%) to reach an Mn of approximately 160,000 g / mol, the polymerization is stopped at the line outlet using a solution of antioxidants in methylcyclohexane (1 pce of N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine and 0.9 pce of 2,2'-methylene-bis(4-methyl-6-tertbutylphenol, pce: part by weight per hundred parts of elastomer). The copolymer is recovered by a steam distillation process called "stripping" well known to those skilled in the art, then dried on a worm machine equipped with a single screw. The copolymer contains 74% ethylene unit, 7% 1,2 unit, 12% 1,4 unit (of which more than 80% 1,4-trans) and 7% cyclic unit (1,2-cyclohexane unit). Its transition temperature is -44°C (AT of 7°C, the AT being the temperature difference between the beginning of the glass transition and its end), its Mn of 154,516 g / mol (Ip 1.70), its ML (1+4) at 100°C of 65.

[0078] The copolymer of ethylene and 1,3-butadiene, elastomer E3, is synthesized according to the procedure described below. The polymerization of ethylene and 1,3-butadiene is carried out according to a continuous process in solution in methylcyclohexane at 80°C under 10 bar in the presence of a catalytic system (119 pmoles Nd per 100 g of monomers), the mass concentration of monomer feed in the reactor being 7.5%, the mass ratio 1,3-butadiene / ethylene being 0.8, the molar ratio active Mg / Nd being 3.7. At the desired conversion (81%) to reach an Mn of approximately 160,000 g / mol, the polymerization is stopped at the line outlet using a solution of antioxidants in methylcyclohexane (0.8 pce of N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine and 0.7 pce of 2,2'-methylene-bis(4-methyl-6-tertbutylphenol, pce: part by weight per hundred parts of elastomer). The copolymer is recovered by a steam distillation process called "stripping" well known to those skilled in the art, then dried on a worm machine equipped with a single screw. The copolymer contains 68% ethylene unit, 15% 1,2 unit, 8.5% 1,4 unit (of which more than 80% 1,4-trans) and 8.5% cyclic unit (1,2-cyclohexane unit). Its transition temperature is - 44°C (AT of 5°C, the AT being the temperature difference between the start of the glass transition and its end), its Mn of 158 118 g / mol (Ip 1.82), its ML (1+4) at 100°C of 65.

[0079] The copolymer of ethylene and 1,3-butadiene, elastomer E4, is synthesized according to the procedure described below. The polymerization of ethylene and 1,3-butadiene is carried out according to a continuous process in solution in methylcyclohexane at 80°C under 10 bar in the presence of a catalytic system (193 pmoles Nd per 100 g of monomers), the mass concentration of monomer feed in the reactor being 8.8%, the mass ratio 1,3-butadiene / ethylene being 1.45, the molar ratio active Mg / Nd being 4. At the desired conversion (81%) to reach an Mn of 160,000 g / mol, the polymerization is stopped at the line outlet using a solution of antioxidants in methylcyclohexane (0.8 pce of N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine and 0.7 pce of 2,2'-methylene-bis(4-methyl-6-tertbutylphenol, pce: part by weight per hundred parts of elastomer). The copolymer is recovered by a steam distillation process called "stripping" well known to those skilled in the art, then dried on a screw machine equipped with a single screw. The copolymer contains 63% ethylene unit, 21% 1,2 unit, 9% 1,4 unit (of which more than 80% 1,4-trans) and 7% cyclic unit (1,2-cyclohexane unit). Its transition temperature is -42°C (AT of 6°C, the AT being the temperature difference between the beginning of the glass transition and its end), its Mn of 158,877 g / mol (Ip 1.84), its ML (1+4) at 100°C of 65.

[0080] The copolymer of ethylene and 1,3-butadiene, elastomer E5, is synthesized according to the procedure described below. The polymerization of ethylene and 1,3-butadiene is carried out according to a continuous process in solution in methylcyclohexane at 80°C under 10 bar in the presence of a catalytic system (193 pmoles Nd per 100 g of monomers), the mass concentration of monomer feed in the reactor being 8.8%, the mass ratio 1,3-butadiene / ethylene being 1.47, the molar ratio active Mg / Nd being 3.2. At the desired conversion (67%) to reach an Mn of approximately 160,000 g / mol, the polymerization is stopped at the line outlet using a solution of antioxidants in methylcyclohexane (0.8 pce of N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine and 0.7 pce of 2,2'-methylene-bis(4-methyl-6-tertbutylphenol, pce: part by weight per hundred parts of elastomer). The copolymer is recovered by a steam distillation process called "stripping" well known to those skilled in the art, then dried on a machine worm screw equipped with a single screw. The copolymer contains 62% ethylene unit, 22% 1,2 unit, 10% 1,4 unit (of which more than 80% 1,4-trans) and 6% cyclic unit (1,2-cyclohexane unit). Its transition temperature is -42°C (AT of 6°C, the AT being the temperature difference between the beginning of the glass transition and its end), its Mn of 170 231 g / mol (Ip 1.70), its ML (1+4) at 100°C of 65.

[0081] The copolymer of ethylene and 1,3-butadiene, elastomer E6, is synthesized according to the procedure described below. The polymerization of ethylene and 1,3-butadiene is carried out according to a continuous process in solution in methylcyclohexane at 80°C under 10 bar in the presence of a catalytic system (154 pmoles Nd per 100 g of monomers), the mass concentration of monomer feed in the reactor being 15.5%, the mass ratio 1,3-butadiene / ethylene being 2.9, the molar ratio active Mg / Nd being 2.2. At the desired conversion (46%) to reach an Mn of approximately 160,000 g / mol, the polymerization is stopped at the line outlet using a solution of antioxidants in methylcyclohexane (0.8 pce of N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine and 0.7 pce of 2,2'-methylene-bis(4-methyl-6-tertbutylphenol, pce: part by weight per hundred parts of elastomer). The copolymer is recovered by a steam distillation process called "stripping" well known to those skilled in the art, then dried on a worm machine equipped with a single screw. The copolymer contains 58% ethylene unit, 26.5% 1,2 unit, 11% 1,4 unit (of which more than 80% 1,4-trans) and 4.5% cyclic unit (1,2-cyclohexane unit). Its transition temperature is -41°C (AT of 6°C, the AT being the temperature difference between the beginning of the glass transition and its end), its Mn of 167,092 g / mol (Ip 1.96), its ML (1+4) at 100°C of 68.

[0082] Results: The results are shown in Table 2. The results are expressed on a base of 100 relative to a control ([value of the composition considered / value of the control composition]xl00). A value greater than 100 indicates a value higher than that of the control. Compositions C4 to C6 provide the tire with a performance compromise between wet grip, rolling resistance and wear resistance that is much better than that of compositions Cl to C3, in particular wet grip performance is greatly improved while a good compromise between wear resistance performance and rolling resistance performance is maintained. [Tables 2] Composition Cl C2 C3 C4 C5 C6 Elastomer El E2 E3 E4 E5 E6 tanô max 60°C 99 103 100 102 98 100 G*50%, 60°C 103 99 100 103 103 98 tanô -20°C, 0.7 MPa 81 79 100 110 121 124

Claims

Claims

1. A tire intended to equip a vehicle carrying heavy loads which comprises a tread, the portion of which intended to be in contact with the rolling ground is made up entirely or in part of a rubber composition, which rubber composition comprises more than 50 pce of a highly saturated diene elastomer which is a random copolymer of ethylene and 1,3-butadiene which contains between 55% and 65% by mole of ethylene units, between 30 pce and 55 pce of a reinforcing filler which contains a carbon black at a mass content greater than 90% of the mass of the reinforcing filler and less than or equal to 100% of the mass of the reinforcing filler.

2. Tire according to claim 1 wherein the molar rate of ethylene units in the highly saturated diene elastomer is greater than 55% and less than or equal to 63%, preferably greater than or equal to 58% and less than or equal to 62%, of the monomer units of the highly saturated diene elastomer.

3. A tire according to claim 1 or 2 wherein the highly saturated diene elastomer comprises units of formula (I) or units of formula (II). CrU—CH-> / ' \ çh / cw? \ / (1) -CH2-CH(CH=CH2)- (!!)

4. A tire according to any one of claims 1 to 3 wherein the highly saturated diene elastomer contains 1,4 units of trans configuration which represent more than 50 mol% of the 1,4 units of the highly saturated diene elastomer, preferably more than 80 mol% of the 1,4 units of the highly saturated diene elastomer.

5. Tire according to any one of claims 1 to 4 in which the level of reinforcing filler in the rubber composition varies from 35 pce to 50 pce, preferably from 35 pce to 45 pce.

6. A tire according to any one of claims 1 to 5 wherein the mass content of carbon black in the ca- outchouc is greater than 95% of the mass of the reinforcing filler and less than or equal to 100% of the mass of the reinforcing filler.

7. A tire according to any one of claims 1 to 6 wherein the carbon black has a BET specific surface area greater than 90 m2 / g, preferably greater than 100 m2 / g.

8. A tire according to any one of claims 1 to 7 wherein the carbon black has a BET specific surface area of ​​less than 145 m2 / g.

9. A tire according to any one of claims 1 to 8 wherein the level of highly saturated diene elastomer in the rubber composition is greater than 80 phr, preferably greater than 90 phr, more preferably is equal to 100 phr.

10. A tire according to any one of claims 1 to 9, in which the rubber composition contains from 0 pce to less than 5 pce of plasticizer chosen from liquid plasticizers, plasticizing hydrocarbon resins and their mixtures, preferably from 0 pce to less than 3 pce of plasticizer chosen from liquid plasticizers, plasticizing hydrocarbon resins and their mixtures.

11. A tire according to any one of claims 1 to 10 wherein the rubber composition contains 0 pce of plasticizer chosen from liquid plasticizers, plasticizing hydrocarbon resins and mixtures thereof.

12. A tire according to any one of claims 1 to 11 wherein the rubber composition is free of reinforcing resin.