Multilayer structure for creating a floor covering
A multilayer floor covering with a low-load bonding layer and reinforcing frames addresses imbalance and weight issues, ensuring balanced installation and effective acoustic insulation.
Patent Information
- Application Number
- FR2022014502
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-12-26
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-12-26
AI Technical Summary
Existing multilayer floor coverings face issues with imbalance, increased weight, and degraded acoustic insulation due to excessive thickness or material loading, leading to logistical and environmental challenges, especially in large surface installations.
A multilayer structure with a bonding layer having a low load rate and specific plasticizer content, combined with reinforcing frames, balances the structure without increasing thickness, maintaining acoustic insulation and puncture resistance, and reducing weight.
The structure achieves balanced installation, reduced weight, and improved environmental impact while maintaining acoustic insulation and puncture resistance, suitable for large surfaces without adhesives.
Smart Images

Figure 00000015_0000 
Figure 00000015_0001 
Figure 00000015_0002
Abstract
Description
Title of the invention: Multilayer structure for the production of a floor covering technical field
[0001] The present invention relates to a multilayer structure with acoustic insulation properties, without coupling means and presented in tiles, strips, for the creation of a floor covering in semi-free installation using a tack or double-sided adhesive, or even in glued installation, or presented in rolls for the creation of a floor covering in free installation. Previous art
[0002] A multilayer structure without coupling means, presented in slabs, blades, or rolls, for the production of a floor covering with acoustic insulation properties, is known from the prior art.
[0003] This multilayer structure comprises successively, that is to say from the top down: - a top wear layer made of plasticized PVC, and having a thickness between 0.3 and 2 mm; - a compact, plasticized PVC backing layer, i.e. non-foamed, obtained not by coating, but rather by calendering, pressing or extrusion, the backing layer is plasticized and with a filler content greater than 130 PCR (percent parts of resin), or even greater than 150 PCR; - a foamed underlayer made of plasticized and filled PVC.
[0004] In order to facilitate installation and improve the dimensional stability of this type of floor covering, it is known that the backing layer includes a reinforcing structure, such as a glass veil coated with a gelled PVC plastisol on both sides and placed in contact with the wear layer.
[0005] To facilitate installation, particularly loose-lay installation, the structure must be balanced. To achieve this, it is known to add weights to the PVC backing layer or to increase its thickness to a thickness greater than 2 mm. However, an excessive increase in the thickness of the backing layer can degrade the acoustic insulation performance of the structure. Conversely, increasing the thickness of the foamed underlay reduces its resistance to indentation.
[0006] Moreover, for surfaces larger than 30 m2, or even larger than 50 m2, the installation of this type of roll-up flooring still requires the use of glue to ensure that it stays in place.
[0007] The resulting disadvantage is that the total thickness of the structure becomes too important, especially if the thickness is greater than 6 mm, which results in an excessive weight, on the order of 6 to 10 kg / m2, and therefore logistical difficulties and environmental impact problems.
[0008] Document EP3505342 describes the implementation of a second reinforced layer with a second reinforcing mesh, which stiffens the structure and creates a so-called "bimetallic" effect, contributing to the weight-bearing effect of the slab, thus facilitating its installation. However, this type of structure does not allow the use of recycled PVC materials in its composition.
[0009] Another disadvantage of the prior art is encountered when the top wear layer is transparent, with 20 to 50 PCR of plasticizer, and a zero filler rate, or even less than 5% by weight of the top layer.
[0010] In this situation, the small amount of load causes, during the manufacture of the structure, a shrinkage of the wear layer which generates the phenomenon well known to those skilled in the art under the English term "curving", or incurvation in French, in which the periphery of the multilayer structure rises up, which creates an imbalance.
[0011] Another disadvantage of the prior art is encountered when the PVC foamed underlayer has a plasticizer content of between 20 and 60 PCR, and a filler content of less than 130 PCR, or even less than 100 PCR.
[0012] In this situation, the difference in load rate with the reverse layer causes, during the manufacture of the structure, a shrinkage of the foamed underlayer which generates the phenomenon of curvature in French, contributing to the imbalance. Description of the invention
[0013] One of the aims of the invention is therefore to propose a multilayer structure for the production of a floor covering, which is balanced, suitable for loose laying in the case of rolls, and without coupling means, with sufficient rigidity to withstand the passage of heavy loads, while exhibiting acoustic attenuation greater than 15 dB or even 19 dB according to NF EN ISO 717-2 May 2013 and NF EN ISO 10140-3 July 2021 and a walking sound level less than 65 according to NF EN 16205 August 2013 / NF EN 16205 / IN1 May 2018 / NF S 31-074.
[0014] To this end, a multilayer structure has been developed for the production of a floor covering without coupling means and comprising successively, i.e. from top to bottom: - a top wear layer of PVC comprising 20 to 50 PCR of plasticizer (PCR means percent parts of resin), and having a thickness of between 0.3 and 2 mm, preferably between 0.5 and 1 mm; - a first reinforcing frame; - a layer of plasticized PVC adhesive allowing the reinforcing frame to be bonded to a backing layer; - said reverse layer, which is made of compact PVC and includes 40 to 60 PCR of plasticizer, and a loading rate greater than 130 PCR, or even greater than 150 PCR, or even greater than 200 PCR and up to 250 PCR; - a foamed underlayer made of plasticized and filled PVC.
[0015] According to the invention, the backing layer has a thickness of between 0.4 and 2 mm, preferably between 0.6 and 1.5 mm, and the gluing layer comprises 20 to 50 PCR of plasticizer and a filler rate of less than 5% by weight of the gluing layer and has a thickness of between 0.05 and 0.5 mm, preferably between 0.1 and 0.3 mm.
[0016] The presence of the adhesive layer according to the invention makes it possible to balance the structure, without requiring an increase in the thickness of the reverse layer of filled PVC.
[0017] In practice, the presence of the bonding layer according to the invention, which is plasticized and which includes a low charge rate, makes it possible to generate the phenomenon of inverse curvature of the wear layer, well known to those skilled in the art under the English term "doming" in which the edges of the structure lower (or the center rises), creating an inverse imbalance which therefore compensates and rebalances the structure.
[0018] Given the low load-bearing capacity of the adhesive layer, it has a lower surface mass than the backing layer, which is loaded and therefore heavier. In other words, the invention allows the structure to be rebalanced, resulting in a lower weight compared to the known solution of increasing the thickness of the backing layer, while preserving the acoustic performance and puncture resistance of the structure.
[0019] The high plasticizer content in the backing layer increases the flexibility of the structure. The presence of the bonding layer according to the invention therefore also makes it possible to stiffen the multilayer structure with a minimum of material, in order to facilitate installation, reduce weight compared to the prior art, and consequently reduce the environmental impact.
[0020] In a particular embodiment, the upper wear layer is transparent and comprises 30 to 50 PCR of plasticizer, with a filler rate of zero or even less than 5% by weight of the upper layer, and the multilayer structure includes a decorative layer positioned under the upper wear layer.
[0021] In a particular embodiment, the upper wear layer has a chamfer on its upper face and on at least one edge of the roller or slab or blade, preferably on all four edges. The presence of a chamfer may This can lead to a decrease in the structure's traffic resistance performance, generating a "split zone" where the structure detaches. This effect is limited by the characteristics of the multilayer structure according to the invention.
[0022] The decorative layer can, for example, be in the form of a layer of ink printed on a lower face of the wear layer, or on a top face coated with the first reinforcing reinforcement, or on a top face of a decorative film positioned under the wear layer.
[0023] In this configuration, the low load rate in the upper wear layer of plasticized PVC causes the phenomenon of "curving" or incurvation tending to unbalance the multilayer structure, compensated by the bonding layer.
[0024] According to another embodiment, the wear layer can be in the form of a layer of pressed granules, such that the wear layer itself forms the decoration. The granules can be of any desired color, as is well known in the prior art.
[0025] The layer of pressed granules is obtained from plasticized and filled PVC. Generally, the filling ratio of the pressed granules is well below 130 PCR, preferably below 100 PCR or even 80 PCR, in order to provide good scratch resistance. The layer of pressed granules thus tends to generate a "curving" phenomenon that tends to unbalance the multilayer structure, which is compensated for by the adhesive layer.
[0026] Advantageously, the multilayer structure includes a second reinforcing reinforcement, embedded in the surface of the reverse layer and also linked to a lower face of the first reinforcing reinforcement by the bonding layer.
[0027] Alternatively, the multilayer structure comprises a second reinforcing reinforcement, embedded on the reverse side of the back layer, on the surface of the sublayer so as to produce a bimetallic effect. This is, for example, directly bonded to the sublayer during the manufacturing of the structure by coating the PVC plastisol sublayer onto the second reinforcing reinforcement and then allowing it to gel.
[0028] This second reinforcement makes it possible to improve the rigidity of the multilayer structure, and in particular to improve the resistance test to the rolling chair.
[0029] The bonding layer is, for example, a layer of plastisol, preferably a PVC plastisol. This makes it possible in particular to simplify the manufacturing process of the multilayer structure by depositing a PVC plastisol by coating on the first reinforcement or on the surface of the back layer, then bringing into contact the assembly formed by the wear layer, the first reinforcing reinforcement and the back layer and gelling the plastisol so as to obtain the bonding layer and bind the whole.
[0030] Preferably, the foamed underlayer has a thickness of between 1 and 3mm, preferably between 1.5 and 2.2mm.
[0031] The total thickness of the multilayer structure is generally between 3.5 and 6mm, preferably between 4 and 5mm.
[0032] A method for obtaining the multilayer structure according to the invention may also include the following steps: - coating and gelling of a PVC plastisol on both sides of a glass veil in order to obtain a decorative layer and a compact bonding layer, on both sides of the glass veil; - printing a design onto the decorative layer; - coating and gelling of a top wear layer from a PVC plastisol on the decorative layer; - coating and gelling of the adhesive layer on the compact bonding layer from a PVC plastisol; - obtaining by calendering, extrusion or pressing and hot lamination of the PVC back layer on the bonding layer, the back layer having a reinforcing grid completely embedded on its surface opposite the bonding layer; - coating and gelling of the foamed underlayer on the reverse layer from a PVC plastisol.
[0033] According to another embodiment, the bonding layer can also be made from a lower impregnation layer of plastisol, such as a gelled PVC plastisol, and a glass veil comprising the first reinforcing mesh. In this situation, the decorative layer can be printed onto a top layer of plastisol, such as a PVC plastisol, coated onto the glass veil and then gelled.
[0034] According to particular embodiments, the first and / or second reinforcing structure is in the form of a glass veil, a glass grid, or a glass grid and glass veil complex, in particular to satisfy tests of resistance to the passage of heavy loads and punching. Brief description of the drawings
[0035] Other features and advantages of the invention will become clear from the description given below, by way of example and not limitation, with reference to the accompanying figures in which:
[0036] [Fig-1] is a schematic cross-sectional representation of one embodiment of the multilayer structure of the invention.
[0037] [Fig.2] is a schematic cross-sectional representation of another embodiment of the multilayer structure of the invention incorporating a printed decorative layer.
[0038] [Fig.3] is a schematic cross-sectional representation similar to that of [Fig.2], the decorative layer being printed on a polymer film.
[0039] [Fig.4] is a schematic representation, in cross-section similar to that of [Fig.2], the decorative layer being printed on a glass sail coated on both sides with a PVC plastisol.
[0040] [Fig.5] is a schematic representation, in cross-section similar to that of [Fig.1], the structure incorporating a second reinforcing reinforcement embedded in the surface of the reverse layer and linked to the first reinforcement by a bonding layer.
[0041] [Fig.6] is a schematic representation, in cross-section similar to that of [Fig.1], the structure incorporating a second reinforcing reinforcement embedded in the reverse face of the reverse layer.
[0042] [Fig.7] is a schematic representation, in cross-section similar to that of [Fig.5], the multilayer structure incorporating a decorative layer, for example conforming to that of [Fig.4], Detailed description of the invention
[0043] The invention relates to a multilayer structure (1) with acoustic insulation properties, without coupling means and presented in tiles, strips, for the creation of a floor covering in semi-free installation using a tack or double-sided adhesive, or even in glued installation, or presented in rolls, for the creation of a floor covering in free installation.
[0044] The multilayer structure (1) according to the invention can have any shape, in particular in panel, slab or blade, and can be wound on itself or on a mandrel to be presented in roll form.
[0045] When presented in roll form, the multilayer structure exhibits a flexibility that allows it to comply with ISO 24344:2008. In this standard, flexibility is defined as the ability of a floor covering or a layer of a floor covering to be wound around a 20 mm core without cracking or splitting. Thus, the multilayer structure according to the invention, as tested in this way, would not exhibit any breaks, splits, cracks, or other permanent defects.
[0046] With reference to [Fig.1], the multilayer structure (1) comprises successively, from top to bottom, an upper wear layer (2) of plasticized PVC, a first reinforcing frame (3), a bonding layer (4) of plasticized PVC allowing the reinforcing frame (3) to be linked to a back layer (5), a compact back layer (5) of plasticized and filled PVC, and a foamed underlayer (6) of plasticized PVC intended to form the last layer of the structure, in particular for the purpose of being in contact with the ground.
[0047] The upper wear layer (2) provides slip resistance, wear resistance, and ease of cleaning. It comprises 20 to 50 PCR of plasticizer and has a thickness of between 0.3 and 2 mm, preferably between 0.5 and 1 mm.
[0048] The upper wear layer (2) can be obtained by extrusion, by calendering, by by pressing, or by coating and then gelling a plastisol. The upper wear layer (2) may be coated with a varnish without departing from the scope of the invention, such as a polyurethane or urethane acrylate-based varnish. The upper wear layer (2) may be varnished and / or textured to improve stain and scratch resistance.
[0049] The upper wear layer (2) can also serve as a decorative layer, in particular if it is obtained from a dyed plastisol or by pressing dyed granules.
[0050] The bonding layer (4) comprises 20 to 50 PCR of plasticizer and a filler content of less than 5% by weight of the bonding layer, and has a thickness of between 0.05 and 0.5 mm, preferably between 0.1 and 0.3 mm. The bonding layer (4) is preferably obtained by coating or is hot-laminated after being obtained by calendering or extrusion. The bonding layer (4) can be related to the top wear layer (2) in terms of composition and properties, and thus allows the structure to be balanced by counteracting the curvature generated by the top wear layer (2), with a low weight compared to the backing layer (5) (at equivalent thickness).
[0051] Preferably, the upper wear layer (2) and the bonding layer (4) are obtained from plasticized PVC and have the same plasticizer content.
[0052] Preferably, and with reference to [Fig.2], the upper wear layer (2) is transparent or translucent so that a decorative layer (7) is visible through the upper wear layer (2).
[0053] In this configuration, the upper wear layer (2) comprises 30 to 50 PCR of plasticizer, and a filler rate of zero, or even less than 5% by weight of the upper wear layer (2), and the decorative layer (7) can be printed on a lower face of the upper wear layer (2), or on a top face coated with the reinforcing reinforcement, or on a polymer film (8) such as a PVC film, see [Fig.3], printed by any known technique and positioned under the upper wear layer (2).
[0054] The first reinforcing armature (3) can be a glass grid, a glass fiber veil.
[0055] In order to combine the advantages of the different existing solutions, the reinforcement includes a glass veil, which is complexed with the glass grid by means of a binder, preferably by lamination.
[0056] In order to bond the glass veil to the glass grid without complicating the manufacturing process or unduly increasing the structure's weight, the binder comprises an acrylic adhesive, or ethylene-vinyl acetate ("EVA"), or a plastisol such as a PVC plastisol. Preferably, the binder is arranged in a thin layer, at a density of between 5 and 35 g / m², or preferably between 10 g / m² and 30 g / m².
[0057] For example, the glass veil comprises glass fibers approximately 1 Opm in diameter and 10 mm in length, randomly distributed and bonded together by a modified polyvinyl alcohol.
[0058] Glass veil generally has a surface mass between 30 g / m² and 100 g / m². The tensile strength of a reinforcing veil is generally chosen to be between 100 N / 50mm and 400 N / 50mm in the longitudinal and transverse directions, measured according to the ISO 1924 / 2 method.
[0059] The strands of a glass grid according to the invention are, for example, obtained from glass fibers and are preferably spaced between 1 mm and 5 mm apart, preferably between 2 mm and 4 mm, depending on the longitudinal and transverse dimensions, and have a linear density between 20 g / m and 110 g / m, advantageously between 35 g / m and 70 g / m. A glass grid generally has a thickness between 0.1 mm and 1 mm and a surface density between 30 g / m² and 150 g / m², preferably between 45 g / m² and 110 g / m². The tensile strength of a reinforcing grid according to the invention is advantageously between 400 N / 50 mm and 1000 N / 50 mm in the longitudinal and transverse directions.
[0060] The first reinforcing armature (3) improves the dimensional stability of the multilayer structure (1) as well as its resistance to punching shear. The multilayer structure according to the invention can claim U4P3 classification according to the UPEC standard.
[0061] The first reinforcing mesh (3) can be bonded to the decorative layer (7) and the backing layer (5) by any means, including thermolamination, cold bonding, hot bonding, extrusion of the layer(s) onto the first reinforcing mesh (3), application of hot-melt adhesive powder, or using double-sided adhesive. If the first reinforcing mesh (3) is bonded by thermolamination, it directly penetrates the thickness of the backing layer (5) and the decorative layer (7), which then impregnate the first reinforcing mesh (3).
[0062] According to a particular embodiment, see [Fig.4], the first reinforcing frame (3) is a glass veil impregnated on its lower face with a bonding layer in the form of a gelled plastisol (9), such as a PVC plastisol, and on its upper face with a plastisol, such as a PVC plastisol, gelled and printed with a decorative layer (7).
[0063] The reverse layer (5) is made of compact plasticized polyvinyl chloride, i.e., which is not foamed.
[0064] The backing layer (5) has a thickness of between 0.4 and 2 mm, preferably between 0.6 and 1.5 mm, and is calendered, pressed, or extruded. Generally, a calendered backing layer (4) is preferred because it is easier to incorporate recycled material into its composition with this manufacturing technique, without degrading the decoration or the appearance of the multilayer structure (1). The backing layer (5) comprises between 40 and 60 PCR, preferably between 50 and 55 PCR of plasticizer and a loading rate greater than 130 PCR, preferably greater than 150 PCR, more preferably greater than 200 PCR and up to 250 PCR.
[0065] With reference to [Fig.5], the multilayer structure (1) preferably includes a second reinforcing frame (10) to increase rigidity and improve dimensional stability and taking the form of a glass veil, a glass grid, or a glass grid and glass veil complex.
[0066] The second reinforcing frame (10) is embedded in the surface of the back layer (4) so as to limit the deformation of the decorative layer (7), and is linked to an underside face of the first reinforcing frame (3) by the adhesive layer (4), in particular in the form of a plastisol, preferably a PVC plastisol.
[0067] Alternatively and with reference to [Fig.6], the second reinforcing armature (10) is embedded in the reverse face of the reverse layer (5) so as to produce a bimetallic effect.
[0068] The back layer (5), preferably calendered, filled and plasticized, increases the mass and flexibility of the structure, in combination with the bonding layer (4) which stiffens the structure, the stability of the structure is improved and its installation is facilitated.
[0069] With reference to [Fig.7], the multilayer structure according to [Fig.5] can incorporate a decorative layer conforming to that of [Fig.4].
[0070] The plasticizers used in the multilayer structure (1) are of all well-known types, such as Diisononyl Phthalate (DINP), Diisodecyl Phthalate (DIDP), 2-Ethylhexyl Diphenyl Phosphate (DPO), Dioctyl Terephthalate (DOTP), 1,2-Cyclohexane dicarboxylic acid diisononyl ester (DINCH), plasticizers from the benzoate family, plasticizers from the adipate family, plasticizers marketed under the PEVALEN® brand by Perstorp, epoxy soybean oil (HSE), octyl epoxy stearate (ESO), totally or partially bio-based plasticizers such as, for example, the plasticizers in the polysorb® exelD 37 range marketed by Roquette Pharma, plasticizers from The Citrofol® range marketed by Jungbunzlauer International AG, or the Soft-n-safe® range of plasticizers marketed by Danisco. Liquid plasticizers can be used alone or in mixtures.
[0071] The fillers used in each layer of the structure may be calcium carbonate, clay, silica, kaolin, or talc. Preferably, the material should be powdered to prevent degradation of the filler during the mixing of the PVC masterbatch used to form the layers, but the use of fibers may be considered. The fillers may be used alone or in mixtures.
[0072] Preferably, the foamed underlayer (6) has a thickness between 1 and 3mm, preferably between 1.5 and 2.2mm.
[0073] The total thickness of the multilayer structure is generally between 3.5 and 6mm, preferably between 4 and 5mm.
[0074] Tests were carried out by the Applicant on the following multilayer structure (1), according to the invention, and comprising from top to bottom: - 0.01 mm acrylic varnish (not shown); - wear layer (2) of 0.65mm plasticized PVC, obtained by coating with a plastisol; - bonding layer (9) of 0.6mm and decorative layer (7) printed of 0.2 mm, on either side of a glass veil (3), obtained by coating with a plastisol; - 0.2mm bonding layer (4), obtained by coating with a plastisol; - calendered back layer (5) of 0.6mm with glass grid on the surface opposite the bonding layer; - foamed underlayer (6) of 2.09 mm, obtained by coating with a plastisol.
[0075] The coating is in the form of strips 1250 mm by 245 mm long. The calendered backing layer comprises approximately 30% recycled material by weight.
[0076] Total thickness: 4.35 mm, surface mass of 3785 g / m2.
[0077] [Tables 1] Technical Specifications Characteristics Units Surface mass g / m2 Total thickness mm Wear layer thickness mm Backing layer thickness mm Sub-layer thickness mm Indentation 2h30 mm Initial curvature mm Curvature 6h80°C mm Curvature 72h80°C mm Curvature at 23°C mm Acoustic insulation 19dB at 23.2°C Walkable sound
[0078] The above values are values measured according to the following standards: Total thickness: NF EN ISO 24346 April 2012 Layer thicknesses: NF EN ISO 24340 April 2012 Weight / Surface mass: ISO 23997 December 2007 Bending at 6 hours at 80°C: NF EN ISO 23999 August 2018 Bending at 80°C for 72 hours: NF EN ISO 23999 August 2018 Curvature monitoring at 23° for 1 month: NF EN ISO 23999 August 2018 Residual static punching shear (Building): ISO 24343-1 June 2007. Acoustic attenuation: NF EN ISO 717-2 May 2013 and NF EN ISO 10140-3 July 2021. Sound at walking less than 65 according to NF EN 16205 August 2013 / NF EN 16205 / IN1 May 2018 / NFS 31-074.
[0079] It follows from the above that the invention does indeed provide a multilayer structure (1) for the production of a floor covering, which is balanced and stable and which has satisfactory sound insulation performance when glued down, while reducing the environmental impact.
Claims
Claims
1. Multilayer structure (1) for producing a floor covering, the multilayer structure (1) is devoid of coupling means and successively comprises: - an upper wear layer (2) made of PVC comprising 20 to 50 PCR of plasticizer, and having a thickness of between 0.3 and 2 mm, preferably between 0.5 and 1 mm; - a first reinforcing frame (3); - a bonding layer (4) made of plasticized PVC for bonding the reinforcing frame (3) to a backing layer (5); - said backing layer (5), which is made of compact PVC and comprising 40 to 60 PCR of plasticizer, and a loading rate greater than 130 PCR, or even greater than 150 PCR, or even greater than 200 PCR and up to 250 PCR; - a foamed underlayer (6) made of plasticized and loaded PVC;characterized in that the backing layer (5) has a thickness of between 0.4 and 2 mm, and in that the bonding layer (4) comprises from 20 to 50 PCR of plasticizer and a filler rate of less than 5% by weight of the bonding layer (4) and has a thickness of between 0.05 and 0.5 mm.;
2. Multilayer structure (1) according to claim 1, characterized in that the upper wear layer (2) is transparent, comprises 30 to 50 PCR of plasticizer, and a filler rate of less than 5% by weight of the upper layer (2), and in that the multilayer structure (1) comprises a decorative layer (7) positioned under the upper wear layer (2).
3. Multilayer structure (1) according to claim 2, characterized in that the decorative layer (7) is a layer of ink printed on a lower face of the upper wear layer (2), or on an upper coated face of the first reinforcing frame (3), or on an upper face of a decorative film positioned under the upper wear layer (2).
4. Multi-layer structure (1) according to claim 1, characterized in that the upper wear layer (2) is a layer of pressed granules.
5. Multilayer structure (1) according to one of the preceding claims, characterized in that it comprises a second reinforcing frame (10) in the form of a glass veil, a grid of glass, or a complex glass grid and glass veil.
6. Multilayer structure (1) according to one of the preceding claims, characterized in that it comprises a second reinforcing frame (10), embedded in the surface of the backing layer (5), and bonded to a lower face of the first reinforcing frame by the bonding layer.
7. Multilayer structure (1) according to one of claims 1 to 5, characterized in that it comprises a second reinforcing frame (10), embedded on the reverse face of the reverse layer (5), on the surface of the underlayer.
8. Multilayer structure (1) according to one of the preceding claims, characterized in that the sub-layer (6) has a thickness of between 1 and 3 mm.
9. Multilayer structure (1) according to one of the preceding claims, characterized in that the bonding layer (4) is a layer of plastisol, such as a PVC plastisol.
10. Multilayer structure (1) according to one of the preceding claims, characterized in that the backing layer (5) has a thickness of between 0.6 mm and 1.5 mm.
11. Multilayer structure (1) according to one of the preceding claims, characterized in that the first and / or the second reinforcing frame (9) is a glass veil, a glass grid, or a glass grid and glass veil complex.