Composition comprising a thermoplastic elastomer, a polyolefin polymer, a plasticizing agent and alumina
A composition of thermoplastic elastomer, polyolefin polymer, plasticizing agent, and alumina addresses high dielectric losses and adhesion issues in flexible polymer materials, enhancing signal transmission and mechanical performance for high-frequency electronic components.
Patent Information
- Application Number
- FR2023000177
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-01-06
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-01-06
AI Technical Summary
Current flexible polymer materials used as dielectric substrates in high-frequency electronic components, such as antennas, suffer from high dielectric losses and poor adhesion with metallic layers, hindering their integration into complex, innovative devices and affecting signal transmission efficiency.
A composition comprising thermoplastic elastomer, polyolefin polymer, plasticizing agent, and alumina, with specific weight ratios, which enhances dielectric properties and adhesion with conductive inks, allowing for flexible and efficient integration into electronic components.
The composition achieves low dielectric losses and excellent adhesion, enabling effective signal transmission and mechanical performance in high-frequency applications, suitable for complex device integration.
Abstract
Description
Title of the invention: Composition comprising a thermoplastic elastomer, a polyolefin polymer, a plasticizing agent and alumina
[0001] The present invention relates to a composition comprising at least one thermoplastic elastomer, at least one polyolefin polymer, at least one plasticizing agent, alumina and optionally a filler other than alumina, according to a particular filler content(s). The present invention also relates to a method for preparing the composition as defined above, and also to a circuit comprising said composition in the form of a substrate and at least one ink. Another object of the invention is the use of the composition as defined above as a dielectric substrate for a component. Technical field
[0002] Fully organic flexible dielectric materials are attracting increasing interest in the electronics industry due to their light weight, low cost and flexibility compared to rigid devices.
[0003] Recently, the transition from wired to wireless technology has given impetus to the development of new concepts and materials suitable for wireless communication.
[0004] Currently, the wireless technology market is expanding to a multitude of applications (telecommunications for 5G, IOT, wearables, etc.) and these are moving towards higher frequencies because the lower ones are already saturated. In addition, with the proliferation of connected objects and wearables where flexibility and suppleness are becoming more crucial than ever, the electronic component must not only be able to efficiently transmit the signal but must be conformable and easily transformable to be integrated into complex unconventional geometries such as curve acquisition systems.
[0005] Nowadays, high-frequency electronic components, such as antennas, have an intrinsically different design than low-frequency components to operate at higher frequencies, not to mention the new market needs. From this point of view, the new issues that arise can be classified into two main categories: the first is related to the quality of signal transmission and the second is related to the design such as flexibility, weight reduction, transformation.
[0006] A component that is massively used in circuits and electronics is the dielectric material that can be found in antennas for example, in particular patch antennas. A dielectric substrate is sought for various properties, the main ones being relative permittivity and dielectric loss. The goal is to keep dielectric loss as low as possible, especially at high frequencies, in order to achieve greater efficiency from an energy or signal point of view.
[0007] However, at present, high-performance low-loss dielectrics are rigid and rarely, if at all, flexible. From the point of view of mechanical properties, to meet the new market needs, soft polymers or soft blends that would be the dielectric in the final system such as the antenna, could be the solution for the future because they fill the gap in the design compartment compared to rigid materials.
[0008] Thus, various flexible polymer materials have been considered as dielectric substrates to replace the rigid materials currently used, for example composites based on glass or ceramic fibers.
[0009] Although significant research has been conducted on polymer film-based materials for patch antennas, certain structural and electrical characteristics inherent in a large part of the materials studied do not allow easy and mechanically efficient integration of the antenna.
[0010] However, much research is still being done to solve the integration and also efficiency issues, so that the flexible antenna can withstand the same operating conditions as commercial antennas and can be integrated into more innovative complex devices, such as curved radar sections, sensors and target acquisition systems.
[0011] The dielectric substrate plays a key role in determining the quality of the antenna radiation. From this point of view, the development of a high-performance flexible substrate for antennas remains a challenge due to the relatively high dielectric loss factor (tan ô > 0.01) of certain flexible polymers previously studied at 1 GHz.
[0012] Different groups have worked on the development of patch antennas based on a flexible dielectric polymer.
[0013] In this context, Hage-Ali et al, in IEEE AP-S International Symposium, June 2009, Charleston, United States. P.4 (2009) developed a technical process for depositing a patch antenna array on a polydimethylsiloxane (PDMS) substrate. In another study, Baron et al (Journal of Micromechanic and Microengineering 24, 075020 (2014)) developed a microstrip patch antenna based on thermoplastic polyurethane (TPU). Unfortunately, the studies showed relatively high inherent dielectric losses at high frequencies (10 GHz and above).
[0014] Thus, polymer materials, and more generally compositions comprising polymers, today have dielectric properties which are not sufficient.
[0015] Furthermore, another disadvantage of polymer materials is their poor adhesion to a metal layer or conductive materials such as inks. This can be a critical problem, particularly in terms of the mechanical performance of a circuit such as an antenna.
[0016] There therefore remains a need to have a composition which has favorable dielectric properties, in particular low dielectric losses, but also a circuit comprising said composition in the form of a substrate, and an ink, with excellent adhesion between said substrate and said ink.
[0017] Thus, the aim of the present invention is to develop a composition having advantageous dielectric properties, in particular which has low dielectric losses, and also a circuit comprising said composition in the form of a substrate, and an ink, with excellent adhesion between said substrate and said ink. Presentation of the invention
[0018] The present invention therefore relates to a composition comprising:
[0019] a) at least one thermoplastic elastomer;
[0020] b) at least one polyolefin polymer;
[0021] c) at least one plasticizing agent;
[0022] d) alumina;
[0023] e) optionally at least one filler other than alumina,
[0024] the content of filler(s) d) + e) ranging from 10 to 25% by weight relative to the total weight of the composition.
[0025] Thanks to the composition according to the invention, advantageous dielectric properties can be obtained, in particular low dielectric losses.
[0026] The invention also relates to a process for preparing the composition according to the invention, and also a circuit comprising the composition according to the invention in the form of a substrate and at least one ink.
[0027] Another object of the invention is the use of the composition according to the invention as a dielectric substrate for a component, in particular an electronic component such as an antenna, a filter or a waveguide.
[0028] The expression “at least one” means one or more.
[0029] Unless otherwise indicated, the limits of a domain of values are included in this domain, in particular in the expressions “between” and “ranging from ... to ...”. Thermoplastic elastomer
[0030] The composition according to the invention comprises at least one thermoplastic elastomer.
[0031] By thermoplastic elastomer (TPE) is meant, in a known manner, a polymer with an intermediate structure between a thermoplastic polymer and an elastomer.
[0032] A thermoplastic elastomer consists of one or more hard (or "rigid" or "thermoplastic") segments connected to one or more soft (or "flexible" or "elastomeric") segments.
[0033] Thus, the thermoplastic elastomer(s) of the composition according to the invention comprise at least one soft block and at least one hard block.
[0034] By “soft” block (or also “flexible” or “elastomeric”), we mean a block which has a glass transition temperature (Tg) lower than ambient temperature (25°C), preferably lower than or equal to 10°C, and more preferably lower than 0°C.
[0035] By “hard” (or also “rigid” or “thermoplastic”) block is meant a block consisting of polymerized monomers and having a glass transition temperature, or a melting temperature in the case of semi-crystalline polymers, greater than or equal to 80°C, preferably varying from 80°C to 250°C, more preferably varying from 80°C to 200°C, and in particular varying from 80°C to 180°C.
[0036] Typically, each of these segments or blocks (hard or soft) contains at least more than 5, generally more than 10 basic units (polymeric units).
[0037] In the present application, when reference is made to the glass transition temperature of a thermoplastic elastomer, this is the glass transition temperature relative to the soft block (or elastomer block) (unless otherwise indicated). Indeed, in a known manner, multi-block thermoplastic elastomers comprising at least one soft block and at least one hard block have two glass transition temperature peaks (Tg, measured according to ASTM D3418), the lower temperature being relative to the soft part of the thermoplastic elastomer, and the higher temperature being relative to the hard part of the thermoplastic elastomer.
[0038] Thus, the thermoplastic elastomer(s) that can be used according to the invention preferably have a glass transition temperature (therefore a glass transition temperature of the soft block) which is less than or equal to 25°C, more preferably less than or equal to 10°C.
[0039] Also preferably, the glass transition temperature of the thermoplastic elastomers which can be used according to the invention is greater than -130°C.
[0040] These elastomers have, in their range, various molecular weights starting from low molecular weights to high molecular weights. Advantageously, said molecular weights range from 104 to 107 g / mol, preferably from 2.5* 104 to 106 g / mol, more preferably from 2.5* 104 to 2.5* 105 g / mol.
[0041] Advantageously, the thermoplastic elastomer(s) are chosen from hard block / soft block / hard block triblock elastomers.
[0042] The soft block(s) of the thermoplastic elastomer(s) that can be used according to the invention may be unsaturated soft blocks.
[0043] By unsaturated soft block, we mean that this block is derived at least in part from conjugated diene monomers.
[0044] The unsaturated soft blocks which can be used according to the invention are preferably chosen from any homopolymer of a monomer having conjugated dienes and any copolymer of a monomer having conjugated dienes with another monomer.
[0045] In particular, the unsaturated soft blocks which can be used according to the invention can be chosen from:
[0046] a) any homopolymer obtained by polymerization of a conjugated diene monomer having from 4 to 12 carbon atoms;
[0047] b) any copolymer obtained by copolymerization of one or more conjugated dienes with each other or with one or more aromatic vinyl compounds having from 8 to 20 carbon atoms;
[0048] c) a ternary copolymer obtained by copolymerization of ethylene, of an α-olefin having from 3 to 6 carbon atoms with a non-conjugated diene monomer having from 6 to 12 carbon atoms, such as for example elastomers obtained from ethylene, of propylene with a non-conjugated diene monomer of the aforementioned type such as in particular hexadiene-1,4, ethylidene norbornene, dicyclopentadiene;
[0049] d) a copolymer of isobutene and isoprene (butyl diene rubber), as well as halogenated, in particular chlorinated or brominated, versions of this type of copolymer.
[0050] Suitable conjugated dienes include, in particular, isoprene, 1,3-butadiene, piperylene, 1-methylbutadiene, 2-methylbutadiene, 2,3-dimethyl-1,3-butadiene, 2,4-dimethyl-1,3-butadiene, 1,3-pentadiene, 2-methyl-1,3-pentadiene, 3-methyl-1,3-pentadiene, 4-methyl-1,3-pentadiene, 2,3-dimethyl-1,3-pentadiene, 2,5-dimethyl-1,3-pentadiene, 2-methyl-1,4-pentadiene, 1,3-hexadiene, 2-methyl-1,3-hexadiene, 2-methyl-1,5-hexadiene, 3-methyl-1,3-hexadiene, 4-methyl-1,3-hexadiene, 5-methyl-1,3-hexadiene, 2,5-dimethyl-1,3-hexadiene, 2,5-dimethyl-2,4-hexadiene, 2-neopentyl-1,3-butadiene, 1,3-cyclopentadiene, methylcyclopentadiene, 2-methyl-1,6-heptadiene, 1,3-cyclohexadiene, l-vinyl-1,3-cyclohexadiene, and a mixture of these conjugated dienes; preferably, these conjugated dienes are selected from isoprene, butadiene and a mixture containing isoprene and / or butadiene.
[0051] It should be noted that reactive functionalities such as maleic anhydride, glycidyl methacrylate or other functionalities intended for compatibilisation or chemical reactivity can be grafted onto this unsaturated soft block.
[0052] In a particularly preferred manner in the invention, the soft block(s) are chosen from the group consisting of polyisoprenes, polybutadienes, copolymers of butadiene and isoprene, copolymers of styrene and butadiene, copolymers of ethylene and butadiene, and mixtures of these polymers, these polymers being non-hydrogenated or partially hydrogenated.
[0053] The soft block(s) of the thermoplastic elastomer(s) usable according to the invention may also be saturated soft blocks.
[0054] Generally speaking, these saturated soft blocks are obtained by hydrogenation of unsaturated soft blocks, or by simple copolymerization.
[0055] As explained previously, the thermoplastic elastomer(s) that can be used according to the invention also comprise at least one hard block.
[0056] The hard block(s) may be made from polymerized monomers of various types.
[0057] In particular, the hard block(s) may be chosen from the group consisting of polyolefins (polyethylene, polypropylene), polyurethanes, polyamides, polyesters, polyacetals, polyethers (polyethylene oxide, polyphenylene ether), polyphenylene sulfides, polyfluorinated compounds such as fluorine-ethylene-propylene (FEP), perfluoroalkoxy (PFA), and ethylene tetrafluoroethylene (ETFE), polystyrenes, polycarbonates, polysulfones, polymethylmethacrylate, polyetherimide, thermoplastic copolymers such as acrylonitrile-butadiene-styrene copolymer (ABS), and mixtures of these polymers.
[0058] Concerning polystyrenes, these are obtained from styrenic monomers.
[0059] By styrenic monomer should be understood in the present description any monomer comprising styrene, unsubstituted as substituted.Among the substituted styrenes that may be mentioned are, for example, methylstyrenes (for example, o-methylstyrene, m-methylstyrene or p-methylstyrene, alpha-methylstyrene, alpha-2-dimethylstyrene, alpha-4-dimethylstyrene or diphenylethylene), para-tert-butylstyrene, chlorostyrenes (for example, o-chlorostyrene, m-chlorostyrene, p-chlorostyrene, 2,4-dichlorostyrene, 2,6-dichlorostyrene or 2,4,6-trichlorostyrene), bromostyrenes (for example, o-bromostyrene, m-bromostyrene, p-bromostyrene, 2,4-dibromostyrene, 2,6-dibromostyrene or 2,4,6-tribromostyrene), fluorostyrenes (e.g. o-fluorostyrene, m-fluorostyrene, p-fluorostyrene, 2,4-difluorostyrene, 2,6-difluorostyrene or 2,4,6-trifluorostyrene) or para-hydroxy-styrene.
[0060] Similar to what can be done for soft blocks, reactive monomers, or functionalities can always be included, in a minority manner, in the polymer chain of the hard block.
[0061] Mention may be made, as thermoplastic elastomers which can be used according to the invention, of multiblock copolymers of ethylene and alpha-olefins where the alpha-olefin is chosen from propylene, 1-butene, 1-hexene, 1-octene, 4-methyl-1-pentene, norbornene, 1-decene, 1,5-hexadiene, ethylene or a combination of such compounds.
[0062] These multiblock copolymers of ethylene and alpha-olefins may comprise one or more hard segments comprising at least 98% by weight of ethylene, and one or more soft segments comprising less than 95% by weight, preferably less than 50% by weight of ethylene. Preferably the hard segments are present in an amount of 5 to 85% by weight.
[0063] For example, these multiblock copolymers of ethylene and alpha-olefins can be supplied by the company DOW under the Engage and Infuse range.
[0064] Advantageously, the thermoplastic elastomer(s) according to the invention are chosen from styrene / butadiene / styrene (SBS) polymers, styrene / ethylene-butylene / styrene (SEBS) polymers, styrene / ethylene / propylene / styrene (SEPS) polymers, styrene / ethylene / ethylene-propylene / styrene (SEEPS) polymers and mixtures thereof.
[0065] In a particularly preferred manner, the thermoplastic elastomer(s) according to the invention are chosen from styrene / ethylene-butylene / styrene (SEBS) polymers.
[0066] Mention may in particular be made, as an elastomer which can be used according to the invention, of the styrene / ethylene-butylene / styrene (SEBS) polymer comprising 30% by weight of styrene units relative to the total weight of the polymer sold under the name “TAIPOL 6151” by the company TSRC.
[0067] Advantageously, the content of thermoplastic elastomer(s) ranges from 20 to 40% by weight, preferably from 30 to 40% by weight, more preferably from 35 to 40% by weight relative to the total weight of the composition. Polyolefin polymer
[0068] As indicated previously, the composition according to the invention comprises at least one polyolefin polymer.
[0069] The term “polyolefin polymer” means a homopolymer or copolymer comprising one or more olefin units such as ethylene, propylene, butene-1, octene-1, butadiene, or any other alpha-olefin units.
[0070] Advantageously, the polyolefin polymer(s) are chosen from ethylene / propylene copolymers, polyethylene homopolymers, polypropylene homopolymers, and mixtures thereof, preferably from polyethylene homopolymers.
[0071] As an example of a polyolefin polymer, mention may be made of polyethylene and, in particular, low density polyethylene (LDPE), high density polyethylene (HDPE), polypropylene; ethylene / propylene copolymers.
[0072] Particularly preferably, the polyolefin polymer(s) are chosen from low density polyethylene (LDPE), high density polyethylene (HDPE) and their mixture. Even more preferably, the polyolefin polymer(s) are chosen from low density polyethylene (LDPE).
[0073] According to a particular embodiment, the content of polyolefin polymer(s) ranges from 20 to 40% by weight, preferably from 20 to 30% by weight, more preferably from 25 to 30% by weight relative to the total weight of the composition. Plasticizing agent
[0074] As indicated previously, the composition according to the invention comprises at least one plasticizing agent.
[0075] Preferably, the plasticizing agent is chosen from oils.
[0076] Thus, preferably, the plasticizing agent is an oil (or plasticizing oil or extending oil).
[0077] At room temperature (25°C), these oils are liquids (that is to say, as a reminder, a substance having the capacity to eventually take the shape of their container) as opposed in particular to resins or rubbers which are by nature solid.
[0078] Preferably, said oil is chosen from polyolefinic oils (i.e. oils resulting from the polymerization of olefins, monoolefins or diolefins), mineral oils, such as paraffinic oils, naphthenic oils (low or high viscosity), aromatic oils, and mixtures of these oils.
[0079] Mention may in particular be made, as a plasticizing agent which can be used according to the invention, of the mineral oil sold under the name “PRIMOL 352” by the company EXXON, or the mineral oil sold under the name “PIONIER M1930” by the company KLAUS DAHLEKE KG.
[0080] According to a particular embodiment, the content of plasticizing agent(s) ranges from 20 to 40% by weight, preferably from 20 to 30% by weight, more preferably from 20 to 25% by weight relative to the total weight of the composition. Charge(s)
[0081] As previously indicated, the composition comprises:
[0082] d) alumina; and
[0083] e) optionally at least one filler other than alumina,
[0084] the content of filler(s) d) + e) ranging from 10 to 25% by weight relative to the total weight of the composition.
[0085] Preferably, the composition comprises:
[0086] d) alumina; and
[0087] e) at least one filler other than alumina,
[0088] the content of filler(s) d) + e) ranging from 10 to 25% by weight relative to the total weight of the composition.
[0089] According to a particular embodiment, the content of filler(s) d) + e) ranges from 10 to 20% by weight, preferably from 15 to 20% by weight relative to the total weight of the composition.
[0090] Advantageously, the alumina content ranges from 2.5 to 17% by weight, preferably from 2.5 to 10% by weight, more preferably from 2.5 to 3.5% by weight relative to the total weight of the composition.
[0091] According to a particular embodiment, the filler(s) e) are chosen from talc, calcium carbonate, Teflon, silicate and mixtures thereof.
[0092] The content of filler(s) e) may range from 0.2 to 16% by weight, preferably from 7 to 16% by weight, more preferably from 7 to 14% by weight relative to the total weight of the composition.
[0093] According to a particular embodiment, the content of filler(s) d) + e) ranges from 10 to 20% by weight relative to the total weight of the composition, the alumina content ranges from 2.5 to 17% by weight relative to the total weight of the composition, and the content of filler(s) e) ranges from 0.2 to 16% by weight relative to the total weight of the composition. Additives
[0094] The composition according to the invention may also comprise various additional additives usually present in compositions comprising thermoplastic elastomers and polyolefin polymers, such as, for example, protective agents such as antioxidants, antiozonants, and anti-UV agents and various processing agents or other stabilizers.
[0095] According to a particularly preferred embodiment of the invention, the composition according to the invention comprises:
[0096] a) from 20 to 40% by weight of at least one thermoplastic elastomer chosen from styrene / butadiene / styrene (SBS) polymers, styrene / ethylene-butylene / styrene (SEBS) polymers, styrene / ethylene / propylene / styrene (SEPS) polymers, styrene / ethylene / ethylene-propylene / styrene (SEEPS) polymers and mixtures thereof relative to the total weight of the composition;
[0097] b) from 20 to 40% by weight of at least one polyolefin polymer chosen from ethylene / propylene copolymers, polyethylene homopolymers, polypropylene homopolymers, and mixtures thereof relative to the total weight of the composition;
[0098] c) from 20 to 40% by weight of at least one plasticizing agent relative to the total weight of the composition;
[0099] d) alumina;
[0100] e) optionally at least one filler other than alumina,
[0101] the content of filler(s) d) + e) ranging from 10 to 25% by weight relative to the total weight of the composition.
[0102] According to an even more preferred embodiment, the composition according to the invention comprises:
[0103] a) from 20 to 40% by weight of at least one thermoplastic elastomer chosen from styrene / ethylene-butylene / styrene (SEBS) polymers relative to the total weight of the composition;
[0104] b) from 20 to 40% by weight of at least one polyolefin polymer chosen from polyethylene homopolymers relative to the total weight of the composition;
[0105] c) from 20 to 40% by weight of at least one plasticizing agent relative to the total weight of the composition;
[0106] d) alumina;
[0107] e) optionally at least one filler other than alumina,
[0108] the content of filler(s) d) + e) ranging from 10 to 25% by weight relative to the total weight of the composition.
[0109] The composition according to the invention may be available in any desired form, which may be obtained in particular by injection, extrusion, 3D printing, etc. methods. Advantageously, the composition according to the invention may be available in the form of plates, granules, or even films.
[0110] The present invention also relates to a process for preparing the composition according to the invention comprising the following steps:
[0111] i) mixing said thermoplastic elastomer a) with said polyolefin polymer b), said plasticizing agent c), alumina d) and optionally said filler e);
[0112] ii) injecting into a mold or adding into an extruder die the mixture obtained at the end of step i).
[0113] The composition according to the invention can thus be prepared by mixing the constituents, then the mixture obtained can be introduced into a machine, for example a twin-screw machine. The mixture obtained can then be used for injection molding, for extrusion. The mixture obtained can also be used for 3D printing.
[0114] The present invention also relates to a circuit comprising the composition according to the invention in the form of a substrate and at least one ink.
[0115] Preferably the ink is a conductive ink.
[0116] For the purposes of the present invention, the term "conductive ink" means a composition, which may be called an EC composition, comprising at least one conductive material, for example a conductive particle. The conductive material may be chosen from conductive particles, in particular metal particles, such as silver particles, carbon nanotube particles, conductive polymers, etc.
[0117] Indeed, it is generally known that conductive inks contain conductive materials such as conductive particles, in particular metal particles, for example silver particles, as described in application US 2006 / 260493 or application WO 2010 / 089564. In these applications, it is in particular specified that the conductive particles may be present in a content which may be at least 30% by weight relative to the total weight of the composition or in a content ranging from 60 to 95% by weight relative to the total weight of the composition.
[0118] The conductive ink may have a resistivity of at least 106 Ohm.m.
[0119] The conductive ink may further comprise a binder and a solvent.
[0120] Said conductive ink can be printed on substrates by different processes (screen printing, printing). It can conduct electricity to enable the design of conductive circuits.
[0121] The circuit may be designed for a component, such as an antenna, in particular a patch antenna.
[0122] Another object of the invention is the use of the composition as a dielectric substrate for a component, in particular an electronic component such as an antenna, a filter or a waveguide.
[0123] The present invention will now be described more specifically by way of examples, which are in no way limiting of the scope of the invention. However, the examples make it possible to support specific characteristics, variations, and preferred embodiments of the invention. Examples Measurement of dielectric loss (tan ô)
[0124] The ring resonator method was used. The principle of the ring resonator is to inject a signal that will travel through the ring and the transmission coefficient S12 will be obtained as a function of the frequencies. The ring will generate a resonance at expected frequencies that depend on the diameter of the ring. Different diameters were used to generate as many measurement points. Indeed, from the peak of the resonance we can extract the values of the dielectric loss of the material.
[0125] This measurement method is well known to those skilled in the art.
[0126] In the following examples, the method of the resonator ring with coplanar waveguide was used. The dimensions are optimized according to the measurement, in particular its thickness in order to avoid losses linked to the skin effect.
[0127] Copper was used as the metal for the electrodes.
[0128] Thus, the ring resonator with coplanar copper waveguide is deposited on the composition according to the invention in the form of a plate.
[0129] Measurements of the transmission coefficient S12 can be carried out and the dielectric losses can therefore be calculated. Preparation of the compositions
[0130] The compositions as described below were prepared: the contents are expressed in % by weight in Table 1 below.
[0131] [Tables 1] Compositions Al (comp.) A2 (inv.) A3 (comp.) A4 (inv.) A5 (inv.) SEBS block copolymer (1) 36.5 36.5 - 36.5 36.5 Polyolefin polymer (2) - - 36.5 - - Polyethylene LDPE (3) 26 26 26 26 26 Plasticizer (4) 21.1 21.1 21.1 21.1 21.1 Calcium carbonate 16 13 13 7 - Silicate 0.2 0.2 0.2 0.2 0.2 Alumina - 3 3 9 16.2 Preservative(s) qs qs qs qs qs
[0132] (1) sold by the company TSRC under the trade name TAIPOL 6151 (comprising 30% by weight of styrene units),
[0133] (2) sold by the company DOW INC under the trade name INFUSE 9010,
[0134] (3) sold by the company POLIMERI EUROPA under the trade name RIBLENE MT 10R,
[0135] (4) Mineral oil sold by the company ESSO under the trade name PRIMOL 352.
[0136] The compositions as described above were first obtained by mixing the different ingredients. Then the mixture obtained was introduced into a twin-screw extruder machine. A homogeneous product was obtained. Then the mixture obtained was injected into a mold to obtain a plate. Then, the plate was cut into several pieces, and each piece was pressed and films with a thickness of about 230 qm were obtained.
[0137] Thus, compositions A1 to A5 are respectively in the form of a film. Results: measurement of dielectric loss
[0138] The measurements were carried out in the X band, i.e. at a frequency in the range from 8 to 12 GHz.
[0139] The results are collected in Table 2 below.
[0140] [Tables2] Compositions Al (comp.) A2 (inv.) A3 (comp.) A4 (inv.) A5 (inv.) tan ô 0.016 0.0006 0.03 0.006 0.002
[0141] It is clear that the compositions according to the invention A2, A4 and A5 have lower dielectric losses than those of the comparative compositions A1 and A3. Composition A2 is the one which has a significantly low dielectric loss.
[0142] By comparing the dielectric losses of the Al composition with respect to the A2 composition, it was observed that the presence of alumina had a decisive impact on the dielectric losses. Indeed, at equal loading rate, the A2 composition has a significantly lower dielectric loss than that of the comparative Al composition.
[0143] By comparing the dielectric losses of composition A3 with composition A2, it was observed that the presence of a thermoplastic elastomer according to the invention had a decisive impact on the dielectric losses. Indeed, composition A2 differs from composition A3 by the presence of a SEBS block copolymer whereas composition A3 instead comprises a polyolefin polymer. At identical contents, composition A2 has a significantly lower dielectric loss than that of comparative composition A3.
[0144] Finally, compositions A4 and A5 are compositions which have very interesting dielectric properties because the dielectric losses, which are almost similar, are lower than those of the comparative compositions Al and A3.
[0145] Thus, it clearly appears that the composition according to the invention makes it possible to obtain improved dielectric properties, with low dielectric loss. Preparation of samples
[0146] Furthermore, compositions A1 and A2 as described above were used to obtain substrates in the form of films prepared by a pressed plate. The films were prepared by pressing compositions A1 and A2, in the form of granules under 40 bars at 190°C for 5 minutes. The prepared films have a thickness of 200-400 μm.
[0147] The substrate obtained from composition Al is called substrate SL. The substrate obtained from composition A2 is called substrate S2.
[0148] Then, a conductive ink sold by the company Dupont under the trade name Intexar PE874 was applied to each of the substrates.
[0149] The ink was applied to each of the substrates S1 and S2 by screen printing. This is a printing technique consisting of passing / coating a substance through a screen, such as a stencil, placed on the substrate.
[0150] After placing the screen on the substrate, an ink coating step is carried out followed by an ink annealing step, for example at 100°C for 30 min, in order to evaporate part of the solvent contained in the ink and ensure optimal conductivity of the latter provided by the conductive ingredients.
[0151] The final printed electronic circuit comprising the ink deposited on the substrate has a configuration which depends on the screen used.
[0152] The substrate S1 on which ink has been applied is called substrate S1E. The substrate S2 on which ink has been applied is called substrate S2E. Result: adhesion test
[0153] Then, tape is placed on the ink of each of the substrates. The tape is then removed and visual observations are made in order to evaluate the effect of the removed tape on the adhesion between the substrate and the ink. The results are gathered in Table 3 below. A score is given according to a scale of values ranging from "—" to "++". The score "—" indicates that the adhesion is very poor, that is to say that the ink has been torn off the substrate, the score "++" indicates that the adhesion is very good (excellent), that is to say that the ink is still present on the substrate.
[0154] [Tables3] Samples S1E (comp.) S2E (inv.) Note ++ ++
[0155] Excellent adhesion between the substrate S2 and the ink can be observed for the substrate S2E, at the same level as for the substrate S1E between the substrate SI and the ink. Thus, the presence of alumina here does not deteriorate the adhesion of the ink to the substrate. This means here that the presence of alumina is entirely compatible with the screen printing process, and more broadly with an industrial process for applying ink to a substrate.
[0156] Thus, it clearly appears that for a circuit comprising at least one composition according to the invention, in the form of a substrate, and at least one ink, excellent adhesion can be obtained between the substrate and the ink.
Claims
Claims
1. Composition comprising: a) at least one thermoplastic elastomer; b) at least one polyolefin polymer; c) at least one plasticizing agent; d) alumina; e) optionally at least one filler other than alumina, the content of filler(s) d) + e) ranging from 10 to 25% by weight relative to the total weight of the composition.
2. Composition according to claim 1, characterized in that the thermoplastic elastomer(s) are chosen from hard block / soft block / hard block triblock elastomers.
3. Composition according to claim 1 or 2, characterized in that the thermoplastic elastomer(s) are chosen from styrene / butadiene / styrene (SBS) polymers, styrene / ethylene-butylene / styrene (SEBS) polymers, styrene / ethylene / propylene / styrene (SEPS) polymers, styrene / ethylene / ethylene-propylene / styrene (SEEPS) polymers and mixtures thereof, preferably from styrene / ethylene-butylene / styrene (SEBS) polymers.
4. Composition according to any one of the preceding claims, characterized in that the content of thermoplastic elastomer(s) ranges from 20 to 40% by weight, preferably from 30 to 40% by weight, more preferably from 35 to 40% by weight relative to the total weight of the composition.
5. Composition according to any one of the preceding claims, characterized in that the polyolefin polymer(s) are chosen from ethylene / propylene copolymers, polyethylene homopolymers, polypropylene homopolymers, and mixtures thereof, preferably from polyethylene homopolymers.
6. Composition according to any one of the preceding claims, characterized in that the content of polyolefin polymer(s) ranges from 20 to 40% by weight, preferably from 20 to 30% by weight, more preferably from 25 to 30% by weight relative to the total weight of the composition.
7. Composition according to any one of the preceding claims, characterized in that the plasticizing agent is chosen from oils.
8. Composition according to any one of the preceding claims, characterized in that the content of plasticizing agent(s) ranges from 20 to 40% by weight, preferably from 20 to 30% by weight, more preferably from 20 to 25% by weight relative to the total weight of the composition.
9. Composition according to any one of the preceding claims, characterized in that the content of filler(s) d) + e) ranges from 10 to 20% by weight, preferably from 15 to 20% by weight relative to the total weight of the composition.
10. Composition according to any one of the preceding claims, characterized in that the alumina content ranges from 2.5 to 17% by weight, preferably from 2.5 to 10% by weight, more preferably from 2.5 to 3.5% by weight relative to the total weight of the composition.
11. Composition according to any one of the preceding claims, characterized in that the filler(s) e) are chosen from talc, calcium carbonate, Teflon, silicate and mixtures thereof.
12. Composition according to any one of the preceding claims, characterized in that the content of filler(s) e) ranges from 0.2 to 16% by weight, preferably from 7 to 16% by weight, more preferably from 7 to 14% by weight relative to the total weight of the composition.
13. A process for preparing a composition as defined in any one of the preceding claims comprising the following steps: i) mixing said thermoplastic elastomer a) with said polyolefin polymer b), said plasticizing agent c), alumina d) and optionally said filler e); ii) injecting into a mold or adding into an extruder die the mixture obtained at the end of step i).
14. Circuit comprising a composition as defined in any one of claims 1 to 12, in the form of a substrate, and at least one ink.
15. Use of the composition as defined in any one of claims 1 to 12 as a dielectric substrate for a component.