Lubrication of a glassmaking mold by cold spraying of a metallic powder
The cold projection and machining of a metal powder onto glassware molds addresses inefficiencies and hazards of traditional lubrication methods, achieving a durable and efficient lubrication layer that enhances productivity and safety.
Patent Information
- Application Number
- FR2023004300
- Authority / Receiving Office
- FR · FR
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-04-28
AI Technical Summary
The existing methods for lubricating glassware molds, such as using graphitized grease or semi-complete combustion of acetylenes, are inefficient, costly, and create a hazardous working environment due to high temperatures and carbon residues, leading to productivity issues and mold degradation.
A method involving the cold projection of a metal powder onto the molding surface of glassware molds followed by machining to create a solid lubricating coating, using a high-pressure and high-temperature gas to ensure the metal powder adheres without melting, resulting in a durable and effective lubrication layer.
The method reduces the frequency of lubrication needs, enhances productivity, and minimizes environmental hazards while maintaining mold quality by providing a uniform and long-lasting lubrication without the drawbacks of traditional methods.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
Title of the invention: Lubrication of a glassware mold by cold projection of a metal powder Technical field
[0001] The present application relates generally to foundry parts in the field of glassmaking, in particular molds made of cast iron, brass, bronze (and other alloys comprising copper and tin) or steel used to make glass objects such as bottles.
[0002] The present application relates more particularly to the lubrication of the metal molding surface of these molds which comes into contact with the parison during the manufacture of glass objects during the roughing phase in order to improve the loading and unloading of the molds. STATE OF THE ART
[0003] The manufacture of a glass object, particularly hollow glass such as a bottle, is carried out in several stages.
[0004] During a first step called roughing, viscous glass is melted (at a temperature between 700°C and 1200°C) and cast in the form of a parison (drop) in a mold, called a roughing mold. The viscous glass undergoes compression in the roughing mold and is then pierced in order to bring it into contact with the walls of the roughing mold and obtain a roughing. The roughing then has a temperature which can reach 900°C, depending on the area and the thickness of the roughing.
[0005] Then, during a second stage called blowing, the blank thus formed is transferred into a finishing mold to be blown and give it its final shape. During contact between the blank and the finishing mold, a strong reduction in temperature occurs as well as an elongation of the glass. The final product is obtained after this blowing stage. It then has a temperature of around 600°C.
[0006] During the roughing stage, several loading defects may appear (bone- or banana-shaped parison, off-centering of the parison, etc.). In the case of a bottle-type object, if these defects are minimal, only a few folds appear on the body of the bottle and / or on the shoulder. However, if the off-centering is too great, the parison cannot penetrate to the bottom of the roughing mold. The pressing against the walls of the roughing mold will therefore be degraded, which can lead to the formation of defects at the rings (neck of the bottle), and therefore the rejection of the bottle.
[0007] It has therefore been proposed to lubricate the molding surface of the rough molds, that is to say the surface which comes into contact with the parison, by regularly depositing a lubricant on this surface. The lubricant generally includes a graphite-filled grease to allow the parison to penetrate the blank mold and facilitate demolding of the blank.
[0008] However, this lubrication operation must be repeated very regularly to be effective, typically every twenty minutes, which reduces the productivity of the molding process. Furthermore, it is generally carried out manually by the operators: however, the temperature around the roughing mold is very high, which creates a difficult working environment for the operators, the roughing molds themselves being at a temperature of around 500 °C. In addition, fouling of the mold and the production machine can occur due to the presence of carbon residues due to the use of graphite grease. Due to the successive openings and closings of the mold to allow lubrication, the temperature of the mold is also heterogeneous, which destabilizes the molding process.Finally, since the lubrication of the molds is not controlled (and is therefore not uniform over the entire molding surface of the rough mold), localized wear by abrasion can appear and the lubricant can decompose under the effect of high temperatures.
[0009] It has also been proposed to replace lubrication with semi-complete combustion of acetylenes. However, this combustion requires a constant presence of combustible projection gas on site which is expensive. EXPOSED
[0010] An aim of the present application is to remedy the aforementioned drawbacks.
[0011] To this end, the invention relates, according to a first aspect, to a method for lubricating a molding surface of a glassware mold comprising the following steps: - cold projection of a solid metal powder onto the molding surface of the glassware mold so as to obtain a solid deposit; and - machining of the solid deposit to obtain a lubricating coating.
[0012] According to particular embodiments of the invention, the lubrication method also has one or more of the following characteristics, taken in isolation or in any technically possible combination(s): - the metal powder is projected using a projection gas subjected to a pressure greater than thirty bars, for example between forty bars and seventy bars, for example approximately fifty bars; - the metal powder is projected using a projection gas heated to a temperature greater than or equal to 750°C, in particular greater than or equal to 900°C, for example between 990°C and 1010°C; - during the projection step, a projection distance, corresponding to a distance between a metal powder projection nozzle and the surface of molding, is between 15 millimeters and 30 millimeters, preferably equal to approximately 20 millimeters; - during the projection step, a speed of movement of a nozzle for projection of the metal powder during projection is between 500 millimeters per second (mm / s) and 1000 millimeters per second (mm / s), for example equal to approximately 800 millimeters per second (mm / s); - the projection step is carried out for a sufficient time to obtain a solid deposit having a thickness of between 0.3 millimeters and 3 millimeters, preferably between 0.5 millimeters and 1 millimeter; and - an injection flow rate of the metal powder into the projection gas is between 5.936 and 17.808 cmVmin, preferably between 8.904 and 14.840 cmVmin, for example of the order of 11.872 cmVmin.
[0013] The invention also relates, according to a second aspect, to a metal powder for lubricating a glassware mold in accordance with a lubrication method according to the first aspect.
[0014] According to particular embodiments of the invention, the metal powder has one or more of the following characteristics, taken in isolation or in any technically possible combination(s): - said metal powder comprises and is advantageously essentially made up of, by mass relative to the total mass of the powder: • between 90 and 97%, for example 95%, of NiCr powder, and • between 3 and 10%, for example 5%, of titanium dioxide powder,
[0015] the nickel content in the NiCr powder being between 40 and 50% by mass and the chromium content being between 50% and 60% by mass, relative to the total mass of the NiCr powder; - a particle size of the NiCr powder is between 10 and 40 micrometers and a particle size of the titanium dioxide powder is between 5 and 40 micrometers; - said metal powder comprises and is advantageously essentially made up of, by mass relative to the total mass of the powder: • between 60 and 70%, preferably between 62 and 68%, of copper; • between 7 and 17%, preferably between 10 and 15%, of nickel; • between 5 and 15%, preferably between 8 and 12%, of aluminum; • between 5 and 15%, preferably between 8 and 12%, of zinc; and - a particle size of the metal powder is greater than or equal to 15 microns and less than or equal to 45 microns.
[0016] The invention also relates, according to a third aspect, to a glassware mold comprising: - a molding surface; and - a lubricating coating covering all or part of the molding surface and comprising a metal alloy resulting from the cold projection of a metal powder onto the molding surface in accordance with a lubrication method according to the first aspect.
[0017] According to particular embodiments of the invention, the glassware mold also has one or more of the following characteristics, taken in isolation or in any technically possible combination(s): - the metal powder is mainly made up of nickel, chromium and titanium dioxide; - the casting surface comprises at least one of the following materials: graphite cast iron with a lamellar, vermicular or spheroidal micrographitic structure, a copper and tin-based alloy such as bronze, iron-carbon steel, refractory steel or stainless steel, brass; - the lubricating coating is obtained by cold projection of a metallic powder according to the second aspect.
[0018] Finally, the invention has as its objects, according to a fourth and a fifth aspect, a machine for lubricating a glassware mold, comprising a support configured to receive a glassware mold having a molding surface and a projection nozzle configured to cold project a metal powder in the solid state onto the molding surface so as to obtain a solid deposit, and an installation comprising a lubrication machine according to the fourth aspect and a machining station configured to machine the solid deposit and obtain a lubricating coating. DESCRIPTION OF FIGURES
[0019] Other characteristics, aims and advantages will emerge from the following description, which is purely illustrative and non-limiting, and which must be read in conjunction with the appended drawings in which: [Fig.l] schematically illustrates an example of an installation for the lubrication of a glassware mold according to one embodiment;
[0020] [Fig. 2] is a flowchart illustrating steps of a method of lubricating a glassware mold according to one embodiment; [Fig. 3] is a schematic sectional view of a glassware mold including a lubricating coating according to one embodiment; [Fig.4] is a schematic view showing a drop of parison on the free surface of a glass mold type substrate;
[0021] [Fig.5] is a curve illustrating the viscosity of the glass composing the parison drop of [Fig.4] as a function of temperature.
[0022] Throughout the figures, similar elements bear identical references. DETAILED DESCRIPTION
[0023] With reference to [Fig. 1], the present application relates to the lubrication of all or part of the molding surface 2 of a glassware mold 1. The glassware mold 1 may in particular comprise a blank mold 1 configured to receive a drop of glass (parison) and form a blank. The molding surface 2 corresponds to the surface of the mold 1 likely to come into contact with the parison during the molding process. The molding surface 2 may in particular comprise at least one of the following materials: graphite cast iron with a lamellar, vermicular or spheroidal micrographitic structure, bronze (and other alloys comprising copper and tin), steel of the iron-carbon steel type, refractory steel or stainless steel, brass. Preferably, the glassware mold 1 is integrally formed from the same constituent material as the molding surface 2.
[0024] In order to lubricate the molding surface 2 of a glassware mold 1, it is proposed to cold-project and at a very high speed, by a projection gas 3 under high pressure transporting it, a metal powder 4 onto all or part of the molding surface 2.
[0025] Cold and high-pressure projection, known by its English name of “cold spray”, makes it possible to obtain a deposit density very close to the theoretical density of the solid metallic material constituting the powder, without heating the molding surface 2 during the deposition, which avoids modifying the metallurgical quality of the molding surface 2 and of the solid deposit 5. It also makes it possible to obtain large thicknesses of deposits (up to several millimeters) with low roughness and a material yield of more than 90%, as well as high interparticle cohesion. In addition, the implementation of this cold projection does not require a prior step of preparing the molding surface 2 or masking the mold 1 to be treated. LUBRICATION PLANT 9
[0026] An installation 9 intended for this lubrication of all or part of the molding surface 2 of a glassware mold 1 is shown in [Fig.l]. This installation 9 comprises a lubrication machine 10 and a machining station 11.
[0027] The lubrication machine 10 is configured to cold spray the metal powder 4, in solid form, onto the molding surface 2 of the mold 1. For this purpose, it comprises a spray nozzle 7, preferably made of ceramic, comprising: - a system for heating and pressurizing a projection gas 3, typically nitrogen or helium, in a pressurization chamber 12; - a powder dispenser 13 for supplying the metal powder 4; - an injection system 18 for injecting the metal powder 4 into the gas of projection 3 downstream of the pressurization chamber 12 so that it is not heated by the lubrication machine 10 and therefore remains in the solid state; - a transport system 19 for transporting the metal powder 4 from the powder distributor 13 to the injection system 18 by means of a carrier gas (typically identical to the projection gas 3); - a convergent-divergent nozzle 8 placed downstream of the injection system 18 and configured to accelerate the projection gas 3 when it transports the metal powder 4, the divergent part of the nozzle 8 forming a deposition tube 14; and - a cooling system 15 which may comprise a conduit which surrounds the deposition tube 14 in order to cool the projection gas 3, which transports the metal powder 4, by conduction by circulating a cooling fluid around the deposition tube 14; the cooling fluid may in particular comprise distilled water at a temperature lower than the temperature of the projection gas 3, typically at a temperature between 8 and 20°C.
[0028] The lubrication machine 10 further comprises a support 17 configured to fix the glassware mold 1 relative to the projection nozzle and actuators configured to move the projection nozzle 7 relative to the molding surface 2 in the three spatial directions. These actuators can move the projection nozzle 7, the support 17 on which the mold 1 is mounted or both the projection nozzle 7 and the support 17. The actuators are configured to move the nozzle relative to the molding surface 2 at a speed of between 600 millimeters per second (mm / s) and 1000 millimeters per second (mm / s), for example of the order of 800 millimeters per second (mm / s) (to within 5%). The actuators are further configured to shift the impact zone by a distance of between 0.5 millimeters and two millimeters (no projection between two adjacent cords), for example of the order of one millimeter (to within 10%).
[0029] The heating system is configured to heat the projection gas 3 to a temperature greater than or equal to 750°C, in particular greater than or equal to 900°C, for example between 990°C and 1010°C. The projection gas 3 is furthermore pressurized in the pressurization chamber to a pressure greater than or equal to thirty-five bars, preferably between forty bars and seventy bars, for example of the order of fifty bars.
[0030] The projection nozzle 7 can be controlled by a remote control station 16, placed near the lubrication machine 10 or remotely.
[0031] The machining station 11 comprises a support configured to receive the mold 1 coated with the solid deposit 5 and a machining tool, such as a milling machine, configured to machine the solid deposit 5 and obtain the lubricating coating 6. The machining tool can be handled by an operator or mounted on the installation 8 and controlled by a machining station. remote control, for example the same control station 16 of the projection nozzle 7. LUBRICATION METHOD 100
[0032] A method 100 for lubricating the molding surface 2, implemented by the lubrication installation 9, is shown in [Fig. 2]. It comprises the following steps: - cold projection 110 of a metal powder 4 in the solid state onto the molding surface 2 of the glassware mold 1 so as to obtain a solid deposit 5; and - machining 120 of the solid deposit 5 so as to obtain a lubricating coating 6 ([Fig.3]).
[0033] The method 100 can be applied to the entire molding surface 2 of the mold 1 or to only part of this surface 2.
[0034] During the projection step 110, a high-temperature (typically nitrogen or helium) and high-pressure projection gas 3 is used to propel the metal powder 4 at a supersonic speed (greater than 300 m / s) onto the molding surface 2 in order to create a solid deposit 5 intended to form the lubricating coating 6 by impact of the metal powder 4 on the molding surface 2, the impact force ensuring the quality of the deposit. In the present application, the deposit is said to be “solid” insofar as the grains of the metal powder 4 remain in the solid state throughout the projection and adhesion step 110 to the molding surface 2, as opposed to processes during which the temperature of the metal powder 4 exceeds its melting temperature so that all or part of the powder 4 melts at some point during the process 100.When the metal powder 4 comes into contact at high speed with the molding surface 2, it mechanically adheres to the molding surface 2 by plastic deformation with strong adhesion, which makes it possible to avoid defects linked to high temperatures such as oxidation, residual stresses, phase transformations, etc. The solid deposit 5 is then integral with the molding surface 2, that is to say that it can only be separated from the molding surface 2 by being completely or partially damaged.
[0035] The projection step 110 is said to be cold insofar as the metal powder 4 is not heated before or during deposition, other than by its contact with the projection gas 3 or the molding surface 2.
[0036] During the projection step 110, the projection gas 3 is heated and pressurized in order to ensure that the metal powder 4 is projected at a projection speed (speed of the metal powder 4 at the outlet of the nozzle 7) capable of allowing the plastic deformation of the metal powder 4 during its impact against the contact surface. It will be noted that the gas is heated and pressurized before injecting the solid powder into the gas and its projection onto the molding surface 2 in order to ensure that the metal powder 4 remains in the solid state. For this purpose, said projection speed is greater than or equal to the critical speed of the metal powder 4. This speed critical corresponds to the speed from which the attachment (adhesion) of the solid deposit 5 is possible: when the impact speed is lower than the critical speed of the material, then the particles of metal powder 4 do not deform plastically and can rebound and / or erode the molding surface 2. The critical speed depends on the nature of the material and the grain size of the metal powder 4. The critical speed is for example higher in the case of a metal powder 4 comprising a hard material, such as a titanium dioxide-based material (above 1250 m / s), than in the case of a metal powder 4 comprising a ductile material, such as a copper-based material (of the order of 600 m / s). An equation E1 making it possible to determine the critical speed of a material has been highlighted by T. Schmidt, F. Gartner, H. Assadi, H. Kreye, “Development of a generalized parameter window for cold spray deposition”, Acta Mater.54 (2006) 729-742 ; . https: / / doi.Org / 10.1016 / j.actamat.2005.10.005) : where: or is the breaking stress of the material; p is the density of the material to be characterized; T; is the initial temperature of the material to be characterized; Tm is the melting temperature of the material to be characterized; cp is the specific heat; Tr is a reference temperature equal to 293 K; and Fi and F2 are calibration coefficients used to recalibrate the calculated value to measured speed values.
[0037] The pressure applied to the projection gas 3 is therefore chosen so as to exceed the critical speed of the metal powder 4 used for the solid deposition 5. A pressure greater than or equal to thirty-five bars, preferably greater than or equal to forty bars, for example equal to fifty bars, is suitable for most metal powders which can be used in the lubrication of a glassware mold 1.
[0038] Furthermore, the temperature to which the projection gas 3 is heated is typically greater than or equal to 750°C, in particular greater than or equal to 900°C, for example between 990°C and 1010°C. This heating temperature is advantageously at least 300°C below the melting temperature of the constituent of the metal powder 4 with the lowest melting temperature and for example between 300 and 700°C below this melting temperature.
[0039] If necessary, the projection gas 3 can further be accelerated by the configuration of the projection nozzle 7 (modification of the gas passage section, for example in a convergent-divergent nozzle 8, etc.).
[0040] For a nickel-chromium based powder as described below, the critical speed is for example of the order of 574 m / s.
[0041] If necessary, the projection gas 3 can be cooled downstream of the injection point of the metal powder 4 into the gas in order to ensure that the metal powder 4 remains solid without reducing the projection speed of the powder.
[0042] The projection step 110 is carried out so as to obtain a solid deposit 5 whose thickness is sufficient to allow machining of the solid deposit 5 and obtaining of the lubricating coating 6. This thickness of the solid deposit 5 is typically between 0.3 millimeters and 3 millimeters, preferably between 0.5 millimeters and 1 millimeter. The thickness of the coating 6 (after machining) can thus be between 0.1 millimeters and 1.5 millimeters.
[0043] For this purpose, the molding surface 2 is moved relative to the lubrication machine 10 during the projection step 110 in order to carry out a deposit on all or part of the molding surface 2. The projection nozzle 7 can be moved while the glassware mold 1 is fixed, or alternatively the glassware mold 1 can be moved while the projection nozzle 7 is fixed, or both the projection nozzle 7 and the glassware mold 1 are moved. The relative movement speed and the number of passes over a given surface determine the thickness of the deposit. For example, the relative displacement speed of the projection nozzle 7 and the molding surface 2 of the glassware mold 1 may be between 600 millimeters per second (mm / s) and 1000 millimeters per second (mm / s), for example of the order of 800 millimeters per second (mm / s) (to within 5%).
[0044] The flow rate of supply of the metal powder 4 by the distributor 13 is between 5.936 and 17.808 cmVmin, preferably between 8.904 and 14.840 cmVmin, for example of the order of 11.872 cmVmin. The metal powder 4 thus supplied is entirely transported by the carrier gas to the injection system 18, so that this supply flow rate also constitutes a flow rate of injection of the metal powder 4 into the projection gas 3 by the injection system 18. For this purpose, the flow rate of carrier gas is typically between 3 and 6 cubic meters per hour (m3 / h), for example of the order of 4.5 cubic meters per hour (m3 / h).
[0045] The size (width of the bead) of the solid deposit 5 is preferably between 0.5 millimeters and two millimeters, for example of the order of one millimeter (to within 10%). This size depends on the distance between the outlet of the projection nozzle 7 of the lubrication machine 10 and the molding surface 2 and on the outlet diameter of the projection nozzle 7. In order to obtain the aforementioned solid deposit size, said distance is typically between fifteen millimeters and sixty millimeters, for example of the order of twenty millimeters (to within 10%) for an outlet diameter of the projection nozzle 7 of between two and ten millimeters, for example of the order of six millimeters.
[0046] The projection pitch (distance between the centers of two solid deposit cords 5 adjacent) is between 0.5 millimeters and two millimeters, for example of the order of one millimeter (to within 10%). It is preferably substantially equal to the size of the solid deposit 5.
[0047] After machining, the porosity of the coating 6 can be between 0.2% and 15%, knowing that the lower the porosity of the coating 6, the closer the behavior (in terms of sliding of the parison) of the lubricating coating 6 is to the behavior of a graphite grease. This porosity is a function of the parameters of projection used during step 110. It is evaluated as follows: - a color image of the coating 6 is obtained with a Leica DMi8 C optical microscope using x5 magnification and the automatic exposure parameters of the microscope; - this image is then binarized using the ImageJ software (version 1.53f51), this binarization comprising the following steps: converting the image to 8-bit grayscale using the software's ad hoc function, then conversion to black and white using the software's automatic thresholding function (Yen method) (thresholding function defining the gray intensity establishing the threshold between pixels converted to white and those converted to black); finally, the surface fraction of black pixels compared to the rest of the image is calculated (equation E2), this surface fraction being assimilated to the porosity rate:
[0048] %porosity= # (E2) METAL POWDER 4
[0049] The metal powder 4 preferably comprises 75% by mass or more of spherical grains, relative to the total mass of the powder.
[0050] Laser granulometry is measured according to ISO 13320:2019.
[0051] The diameter of the grains of the powder is advantageously between 10 and 50 pm, in particular between 12 and 45 pm, and preferably has a D50 value between 20 and 30 pm.
[0052] The melting temperature of the powder compounds is typically higher than the parison temperature - which can reach 1100°C - in order to avoid thermal degradation of the lubricant coating 6 during molding. Preferably, the melting temperature of the powder component having the lowest melting temperature is 300°C higher than the parison temperature.
[0053] The “packed density” is evaluated according to the bases of the NF EN ISO 3923 standard (2018) on “Metal powders - Determination of apparent density after tamping”. Typically, a 25 cm3 volume test tube and a KERN SEAL balance with a maximum capacity of 6000 g and a resolution of 0.1 g are used. The tamping is stopped after 3000 strokes.
[0054] The "true density" is evaluated according to the basis of the standard NF EN ISO 8130-2 (2011) relating to "Powders for coating - Determination of the density using a gas pycnometer (reference method)". A helium pycnometer (Quantachrome Upyc 1200 e) with a 10 cm3 cell is used. The mass of the powder is measured with a balance, for example METTLER TOLEDO AB 104 with a maximum capacity of 110 g and a resolution of 0.1 mg.
[0055] The packed density of the metal powder is typically between 3 and 7 g / cm3
[0056] The true density is typically between 6 and 10 g / cm3, preferably with a low standard deviation, for example 0.001. Metal powders having such a true density in fact make it possible to obtain a denser solid deposit 5.
[0057] For the purposes of the present invention, a powder is “essentially composed” of a compound A when the powder comprises at least 99% by mass of the compound A, relative to the total mass of the powder.
[0058] The metal powder 4 comprises a first so-called “matrix” powder, to enable its adhesion to the molding surface 2. This first matrix powder gives the coated mold improved thermomechanical and / or heat diffusion properties.
[0059] The metal powder 4 also comprises, in addition to the matrix powder, a lubricating powder, to facilitate the penetration of the parison into the glassware mold 1 and facilitate the demolding of the blank.
[0060] The metal powder 4 has a lubricating powder content of 3% to 10% by mass, typically 5% by mass, relative to the total mass of the metal powder 4.
[0061] The metal powder 4 is advantageously obtained by simple mixing of the matrix powder and the lubricating powder. A person skilled in the art will be able to determine the duration, type and intensity of stirring necessary to obtain a homogeneous lubricating metal powder.
[0062] Lubricating powder
[0063] The lubricating powder may comprise or consist of a metal oxide in powder form. Preferably, the lubricating powder comprises or consists essentially of titanium oxide (denoted TiO2).
[0064] The lubricating powder advantageously comprises at least 95% by mass, very advantageously at least 98% by mass of spherical grains, relative to the total weight lubricating powder.
[0065] The tamped density of the lubricating powder is typically between 0.8 and 1.8 g / cm3, in particular between 1.0 and 1.5 g / cm3. The true density of the lubricating powder is typically between 3.5 and 4.5 g / cm3, in particular between 3.8 and 4.2 g / cm3.
[0066] The particle size of the lubricating powder is advantageously between 5 and 40 μm. The D50 value of the lubricating powder is typically between 15 and 20 μm.
[0067] Matrix powder comprising a NiCr alloy
[0068] According to a first embodiment, the matrix powder comprises or is essentially made up of an alloy of nickel and chromium (called nickel-chromium alloy and denoted NiCr). A coating comprising NiCr gives the mold thermomechanical protection. In particular, a coating comprising NiCr gives the mold better abrasion resistance, which is particularly useful in the case of molds for borosilicate glass.
[0069] The Nickel content in the NiCr alloy is advantageously between 40% and 85% by mass, preferably between 45 and 80% by mass, relative to the total mass of the NiCr alloy, the remainder being essentially made up of chromium.
[0070] For example, the nickel content in the NiCr alloy is between 40 and 50% by mass, while the chromium content is between 50% and 60% by mass, relative to the total mass of the NiCr alloy.
[0071] The particle size of the NiCr matrix powder is advantageously between 10 and 40 μm. The D50 value of the NiCr powder is typically between 20 and 30 μm.
[0072] The tapped density of the NiCr matrix powder is typically between 4 and 5 g / cm3, in particular between 4.3 and 4.8 g / cm3. The true density of the NiCr matrix powder is typically between 7.5 and 8.5 g / cm3, in particular between 7.6 and 8.0 g / cm3.
[0073] According to an example of implementation of this first embodiment, the metal powder 4 comprises or is essentially made up of: - 90 to 97% by mass, for example 95% by mass, of NiCr; and - 3 to 10% by mass, in particular 5% by mass, of titanium dioxide.
[0074] According to this example, the metal powder 4 can be obtained by mixing the NiCr powder with the titanium dioxide powder for 15 to 24 hours to obtain a homogeneous powder, for example for 17h30, then the mixture is placed in a hermetic enclosure until use. In order to improve the homogeneity of the deposit, the mixture can be placed under an inert atmosphere in the hermetic enclosure.
[0075] Matrix powder comprising a cupronickel type alloy
[0076] According to a second embodiment, the matrix powder comprises or is essentially It is primarily made of an alloy of copper, nickel, aluminum and zinc, which for the sake of simplification will be called "cupronickel" in the following. A coating comprising a so-called "cupronickel" alloy gives the mold better heat diffusion properties, which allows the glass to be cooled more evenly upon contact with the coated mold. Such a coating is particularly advantageous in the case of molds for soda-lime glass.
[0077] According to this second embodiment, the matrix powder comprises or is essentially constituted of a powder of an alloy comprising, by mass relative to the total mass of the alloy: between 60 and 70%, preferably between 62 and 68%, of copper; between 7 and 17%, preferably between 10 and 15%, of nickel; between 5 and 15%, preferably between 8 and 12%, of aluminum; between 5 and 15%, preferably between 8 and 12%, of zinc; the possible complement preferably being essentially made up of chromium, manganese and / or iron.
[0078] Typically, the complement represents at most 3% by mass relative to the total mass of the alloy. Preferably, the complement comprises, by mass relative to the total mass of the alloy: at most 1% chromium; not more than 1% manganese; and not more than 1% iron.
[0079] The tapped density of the “cupronickel” matrix powder is typically between 1 and 6 g / cm3, in particular between 4.5 and 5.5 g / cm3. The true density of the “cupronickel” matrix powder is typically between 4 and 9 g / cm3, in particular between 7.5 and 9.0 g / cm3.
[0080] The particle size of the “cupronickel” matrix powder is advantageously between 15 and 45 μm. The D50 value of the “cupronickel” powder is typically between 20 and 30 μm.
[0081] According to an example of implementation of this second embodiment, the metal powder 4 then comprises or is essentially made up of: - 90 to 97% by mass, for example 95% by mass, of cupronickel; and - 3 to 10% by mass, in particular 5% by mass, of titanium dioxide.
[0082] According to this example, the metal powder 4 can be obtained by mixing the cupronickel powder with the titanium dioxide powder for 15 to 24 hours to obtain a homogeneous powder, for example for 17h30, then the mixture is placed in a hermetic enclosure until use. In order to improve the homogeneity of the deposit, the mixture can be placed under an inert atmosphere in the hermetic enclosure.
[0083] EXAMPLE OF CARRYING OUT THE LUBRICATION OF A MOLD 1 GLASSWARE
[0084] An example of carrying out the lubrication of a glassware mold 1 will now be described, with reference to [Fig.4]. I - Materials and methods
[0085] Preparation of metal powder 4
[0086] The metal powder 4 is obtained by mixing a matrix powder of NiCr with a lubricating powder of TiO2, in the following proportions:
[0087] - 95% by mass of NiCr powder comprising 50% by mass of nickel and 50% by mass of mass of chromium (i.e., in the total powder, 47.5% by mass of nickel and 47.5% by mass of chromium); and - 5% by mass of titanium dioxide powder.
[0088] These powders are mixed for 17.5 hours to obtain a homogeneous metal powder 4, which is placed in a hermetic enclosure until use.
[0089] The NiCr powder used consists of an alloy comprising approximately 50% by mass of Nickel and approximately 50% by mass of Chromium. It is marketed by SANDVIK OSPREY.
[0090] The melting temperature of the NiCr compound is 1345°C.
[0091] The NiCr powder comprises at least 75% by mass, advantageously at least 80% by mass of spherical grains, relative to the total weight of the NiCr powder.
[0092] The average value of the packed density after three measurements is 4.7 g / cm3.
[0093] The powder test sample for the measurement of the true density was 30.8561 g. The The average true density value after five measurements was 7.71 g / cm3 with a standard deviation of 0.001.
[0094] Three measurements were carried out to determine the parameters D10, D50 and D90 (laser granulometry). The average of these parameters is as follows: -D10= 14.7 pm; - D50 = 26.1 pm; and - D90 = 44.0 pm.
[0095] The TiO2 powder used is marketed by Saint Gobain, under the name “TiO 2 anastase nanostructured powder”.
[0096] The TiO2 powder comprises at least 95% by mass, advantageously at least 98% by mass of spherical grains, relative to the total weight of the TiO2 powder. The surface appearance of the grains is very smooth. At least 80% by weight of the grains have internal porosities, relative to the total weight of the TiO2 powder.
[0097] The average value of the packed density after three measurements is 1.2 g / cm3.
[0098] The true density was measured under the same conditions as for the NiCr compound, with a powder sample of 7.3359 g. The average true density value after five measurements was 4.16 g / cm3 with a standard deviation of 0.002.
[0099]
[0100]
[0101]
[0102]
[0103]
[0104]
[0105] The laser granulometry was carried out under the same conditions as for the NiCr compound: the average of these parameters is as follows: - D10 = 8.80 pm; - D50 = 17.8 pm; and - D90 = 33.9 pm. Preparation of plates representative of the molding surface of a glassware mold Four flat plates 22 are prepared. Each plate 22 has a free surface 21 representative of the molding surface 2 of a glass mold 1 and intended to receive a drop of glass. The four plates 22 are made of graphite cast iron with a lamellar micrographitic structure of the same composition. A first of these plates 22 is untreated, that is to say that neither the lubricating coating 6 nor even a conventional lubricant such as graphite-loaded grease is applied to its free surface 21. A second of these plates 22 has its free surface 21 coated with a conventional lubricant comprising a graphite-loaded grease. This grease, of the KleenMold® brand, comprises: - the following solid particles: calcium (Ca), sulfur (S), carbon (C), oxygen (O) and calcium carbonate (CaCO3), and - the following binders: sulfur (S), silicon (Si) and chlorine (Cl). A third of the plates 22 has its free surface 21 covered with a first lubricating coating 6 obtained according to the lubrication method 100 of the present disclosure, with the following parameters: - 7 ceramic Laval type projection nozzle (convergent divergent) with an outlet diameter of 6 mm; - projection gas 3: nitrogen; - temperature and pressure of the gas in the pressurization chamber 12: 1000°C, 50 bars; - cooling fluid: distilled water; - distance between the outlet of the projection nozzle 7 and the impact zone on the molding surface 2: 20 mm; - speed of movement of the projection nozzle 3: 800 mm / s; - metal powder 4: consisting of nickel-chromium and titanium dioxide, as described above, at room temperature (20°C); - flow rate of supply of metal powder 4 by distributor 13: 11.872 cmVmin; - carrier gas flow rate: 4.5 m3 / h; - thickness of solid deposit 5: 0.5 mm; - thickness of the lubricating coating after machining of the solid deposit: 0.2 mm; - porosity of the coating (after machining of the solid deposit 5): approximately 1.3%; - adhesion of the lubricating coating 6 (after machining of the solid deposit 5): between 35 MPa and 45 MPa.
[0106] A fourth of the plates 22 has its free surface 21 covered with a bonding sub-layer, itself coated with a second lubricating coating 6 obtained according to the lubrication method 100 of the present disclosure.
[0107] The bonding undercoat is obtained by cold spraying of a powder consisting essentially of a NiCr alloy comprising approximately 80% by mass of Nickel and approximately 20% by mass of Chromium, with the following parameters: - Laval type ceramic projection nozzle (convergent divergent) with an outlet diameter of 6 mm; - projection gas: helium; - temperature and pressure of the gas in the pressurization chamber 12: 750°C, 42 bars; - cooling fluid: distilled water; - distance between the outlet of the projection nozzle and the impact zone on the molding surface: 30 mm; - speed of movement of the projection nozzle: 800 mm / s; - powder supply flow rate: 8.904 cmVmin; - carrier gas flow rate: 3 mVh; - thickness of the solid deposit: between 250 and 350 pm.
[0108] The solid deposit 5 intended to form the second lubricating coating 6 is obtained with the following parameters: - 7 ceramic Laval type projection nozzle (convergent divergent) with an outlet diameter of 6 mm; - projection gas 3: nitrogen; - temperature and pressure of the gas in the pressurization chamber 12: 1000°C, 50 bars; - cooling fluid: distilled water; - distance between the outlet of the projection nozzle 7 and the impact zone on the molding surface 2: 20 mm; - speed of movement of the projection nozzle 3: 800 mm / s; - metal powder 4: consisting of nickel-chromium and titanium dioxide, as described above, at room temperature (20°C); - flow rate of supply of metal powder 4 by distributor 13: 11.872 cmVmin; - carrier gas flow rate: 4.5 m3 / h; - thickness of solid deposit 5: 1 mm.
[0109] The solid deposit 5 was then machined so as to obtain a thickness of lubricating coating 6, including the adhesion sub-layer, equal to approximately 1 mm. The porosity of the second lubricating coating (excluding the adhesion sub-layer) was measured at approximately 7.6%. II - Implementation
[0110] The four plates 22 are tested. For this purpose, each plate 22 is placed on a support, the free surface 21 of this plate 22 being oriented horizontally on the support, and a drop of glass 20a, 20b, 20c, 20d is applied to the free surface 21 of the plate 22 while the plate 22 is heated: - a first drop of glass 20a is applied to the free surface 21 of the first plate 22, - a second drop of glass 20b is applied to the free surface 21 of the second plate 22, - a third drop of glass 20c is applied to the free surface 21 of the third plate 22, and - a fourth drop of glass 20d is applied to the free surface 21 of the fourth plate 22.
[0111] The temperature of each plate 22 is measured between 440°C and 450°C during the deposition of the glass drop 20a, 20b, 20c, 20d on the plate 22.
[0112] The glass making up the drops 20a, 20b, 20c, 20d is the same for the four plates 22. It has the following composition (the contents are expressed as a mass percentage): B2O3: 0.66% Na2O: 18.9% MgO: 3.14% A12O3:1.87% SiO2: 69.7% SO3:0.15% K2O: 0.06% CaO: 5.24% TiO2: 0.025% Cr2O3: < 0.020% Fe2O3: 0.072% ZrO2:0.021% BaO: < 0.02% PbO: 0.014%.
[0113] For all elements except boron, the content was determined by quantitative analysis of the glass by X-ray fluorescence spectrometry (XRF). For this purpose, a first glass sample was first obtained by grinding and making molten beads which were dissolved in a flow of lithium tetraborate. The sample was then analyzed using a BRUKER S4 Pioneer sequential wavelength dispersive spectrometer.
[0114] For boron, the content was determined by plasma excitation atomic emission spectrometry. For this purpose, a second glass sample was obtained by acid solution after alkaline fusion and removal of interfering cations. The sample was then analyzed using a Varian Vista MPX plasma excitation atomic emission spectrometer.
[0115] From the element contents thus obtained, the oxide contents were deduced by calculation.
[0116] The glass making up the drops 20a, 20b, 20c, 20d also has the following physical parameters: - coefficient of thermal expansion (between 20°C and 300°C): 9.9x10 6+0.1x106 K1; - glass transition temperature: 513±6°C; - softening temperature (Littleton point): 676±4°C; - working temperature: 967+3°C; - density: 2.484+0.003 g / cm3.
[0117] Finally, the said glass has the viscosity curve illustrated in [Fig.5]. These parameters and this curve are determined by applying the ISO 7884 standard.
[0118] The pouring temperature of the glass drops (parison) 20a, 20b, 20c, 20d is measured between 1050°C and 1200°C during their contact with the free surface 21 of the plate 22. Its flow speed is approximately 4 m / s. The diameter of each glass drop 20a, 20b, 20c is approximately 7 mm and its mass is 0.38+0.04 g. III - Results
[0119] The geometric properties of the drops 20a, 20b, 20c, 20d obtained are measured in order to determine the capacity of the lubricating coating 6 to improve sliding and / or promote the detachment of the drop 20 on the free surface 21 of the plate 22.
[0120] For this purpose, each glass drop 20a, 20b, 20c, 20d is filmed using a high acquisition frequency camera in order to determine its geometric characteristics between 0 and 3 seconds after impact (i.e. while the drop is liquid, before it solidifies) and to deduce therefrom the capacity of the lubricating coating to allow the sliding and / or detachment of the drop 20a, 20b, 20c, 20d on the free surface 21 of the plate 22.
[0121] The measurements are carried out by image processing and polynomial interpolation of the drop shape 20a, 20b, 20c, 20d on the four plates 22.
[0122] The average measurements (obtained after measurements taken on three hundred images and related to the initial diameter d0 of the drop during the fall, before impact) are as follows: First drop 20a (plate without lubricant or lubricant coating 6) Second drop 20b (plate coated with a conventional lubricant) Third drop 20c (plate with lubricant coating 6 (NiCr-TiO2) having an average porosity of 1.3%) Fourth drop 20d (plate with lubricant coating 6 (NiCr-TiO2) having an average porosity of 7.6%) Drop diameter at the interface with plate 22 (dsut / do) 1.15 1.25 1.16 0.90 Maximum drop diameter (dmax / d0 ) 1.24 1.24 1.24 1.12 Maximum drop height (hmax / d0) 0.60 0.55 0.55 0.65 Drop wetting angle (0) 125 ° 115 ° 130° 145 °
[0123] The wetting angle 0 of a drop 20a, 20b, 20c, 20d corresponds to the angle formed between the tangent to the free surface 21 of the plate 22 and the tangent to the surface of the drop 20a, 20b, 20c, 20d at the interface between the drop 20a, 20b, 20c, 20d and the free surface 21 of the plate 22.
[0124] Thus, all of the measured geometric parameters show that the wetting of a drop of glass on the free surface 21, when it is coated with the lubricating coating 6 of the plate 22, is reduced in comparison with the wetting of a substantially identical drop of glass on the free surface of a conventionally lubricated plate 22. ally (graphited grease) or untreated.
[0125] The lubricating coating 6 therefore reduces the adhesion of the parison to the molding surface 2 and facilitates its detachment and its penetration (sliding) into the glassware mold 1 and the demolding of the blank. Thus, it is possible to reduce the lubrication frequency of the mold 1, or even to do without any new lubrication of the mold 1, without harming the lubrication performance of the mold 1. Lubrication costs can thus be reduced, and the production rate increased.
Claims
Claims
1. A method of lubricating (100) a molding surface (2) of a glassware mold (1) comprising the following steps: - cold spraying (110) of a metal powder (4) in the solid state onto the molding surface (2) of the glassware mold (1) so as to obtain a solid deposit (5); and - machining (120) the solid deposit (5) so as to obtain a lubricating coating (6).
2. Lubrication method (100) according to claim 1, in which the metal powder (4) is projected using a projection gas (3) subjected to a pressure greater than thirty bars, for example between forty bars and seventy bars, for example approximately fifty bars.
3. Lubrication method (100) according to one of claims 1 or 2, in which the metal powder (4) is projected using a projection gas (3) heated to a temperature greater than or equal to 750°C, in particular greater than or equal to 900°C, for example between 990°C and 1010°C.
4. Lubrication method (100) according to one of claims 1 to 3, wherein during the projection step (110), a projection distance, corresponding to a distance between a projection nozzle (7) of the metal powder (4) and the molding surface (2), is between 15 millimeters and 30 millimeters, preferably equal to approximately 20 millimeters.
5. Lubrication method (100) according to one of claims 1 to 4, wherein during the projection step (110), a speed of movement of a projection nozzle (7) of the metal powder (4) during the projection is between 500 millimeters per second (mm / s) and 1000 millimeters per second (mm / s), for example equal to approximately 800 millimeters per second (mm / s).
6. Lubrication method (100) according to one of claims 1 to 5, in which the projection step (110) is carried out for a sufficient time to obtain a solid deposit (5) having a thickness of between 0.3 millimeters and 3 millimeters, preferably between 0.5 millimeters and 1 millimeter.
7. Lubrication method (100) according to one of claims 1 to 6, in which an injection flow rate of the metal powder (4) into the gas of projection (3) is between 5.936 and 17.808 cmVmin, preferably between 8.904 and 14.840 cmVmin, for example of the order of 11.872 cm3 / min.
8. Lubrication method (100) according to one of claims 1 to 7, wherein said metal powder (4) comprises and advantageously consists essentially of, by mass relative to the total mass of the powder: - between 90 and 97%, for example 95%, of NiCr powder; and - between 3 and 10%, for example 5%, of titanium dioxide powder, the nickel content in the NiCr powder being between 40 and 50% by mass and the chromium content being between 50% and 60% by mass, relative to the total mass of the NiCr powder.
9. A lubrication method (100) according to claim 8, wherein a particle size of the NiCr powder is between 10 and 40 micrometers and a particle size of the titanium dioxide powder is between 5 and 40 micrometers.
10. Lubrication method (100) according to one of claims 1 to 7, in which said metal powder (4) comprises and is advantageously essentially composed of, by mass relative to the total mass of the powder: • between 60 and 70%, preferably between 62 and 68%, of copper; • between 7 and 17%, preferably between 10 and 15%, of nickel; • between 5 and 15%, preferably between 8 and 12%, of aluminum; • between 5 and 15%, preferably between 8 and 12%, of zinc
11. A lubrication method (100) according to claim 10, wherein a particle size of the metal powder (4) is greater than or equal to 15 microns and less than or equal to 45 microns.
12. Glassware mold (1) comprising: - a molding surface (2); and - a lubricating coating (6) covering all or part of the molding surface (2) and comprising a metal alloy resulting from the cold projection of a metal powder (4) onto the molding surface (2) in accordance with a lubrication method (100) according to one of claims 1 to 7.
13. A glassware mold (1) according to claim 12, wherein the metal powder (4) consists essentially of nickel, chromium and titanium dioxide.
14. Glassware mold (1) according to one of claims 12 and 13, wherein the molding surface (2) comprises at least one of the following materials: graphite cast iron with a lamellar, vermicular or spheroidal micrographitic structure, a copper and tin-based alloy such as bronze, iron-carbon steel, refractory steel or stainless steel, brass.
15. Glassware mold (1) according to one of claims 12 to 14, in which the lubricating coating (6) is obtained by cold spraying: * either a metal powder comprising and advantageously being essentially constituted of, by mass relative to the total mass of the powder: - between 90 and 97%, for example 95%, of NiCr powder; and - between 3 and 10%, for example 5%, of titanium dioxide powder, the nickel content in the NiCr powder being between 40 and 50% by mass and the chromium content being between 50% and 60% by mass, relative to the total mass of the NiCr powder and a particle size of the NiCr powder is between 10 and 40 micrometers and a particle size of the titanium dioxide powder is between 5 and 40 micrometers;* either a metal powder (4) comprising and advantageously being essentially constituted of, by mass relative to the total mass of the powder: - between 60 and 70%, preferably between 62 and 68%, of copper; - between 7 and 17%, preferably between 10 and 15%, of nickel; - between 5 and 15%, preferably between 8 and 12%, of aluminum; - between 5 and 15%, preferably between 8 and 12%, of zinc, a particle size of the metal powder (4) possibly being greater than or equal to 15 microns and less than or equal to 45 microns.;
16. Lubrication machine (10) for a glassware mold (1) comprising: - a support (17) configured to receive a glassware mold (1) having a molding surface (2); and - a projection nozzle (7) configured to cold project a metal powder (4) in the solid state onto the molding surface (2) so as to obtain a solid deposit (5).
17. Installation comprising a lubrication machine (10) according to the re- claim 16 and a machining station (11) configured to machine the solid deposit (5) and obtain a lubricating coating (6).
Citation Information
Patent Citations
Laser recharging powder, associated manufacturing method and mould
EP3834960A1
Method for depositing a coating on a bore of a mechanical part by cold spray method
EP4001460A1
Glass working tools mfr. - by chromaluminisation of nickel, iron or copper (SW201276)
FR2311639A1
Spray system for glass moulds
GB2132188A
Wear-resistant and low-friction coatings and articles coated therewith