Surface treatment of a glass mold by cold spraying of a metallic powder
Cold spraying metal powder on glassware molds addresses thermal conductivity and wear issues by creating a durable coating that enhances both thermal efficiency and abrasion resistance, reducing mold replacement costs.
Patent Information
- Application Number
- FR2023004301
- Authority / Receiving Office
- FR · FR
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-04-28
AI Technical Summary
Existing glassware molds face issues with excessive thermal conductivity costs and rapid wear due to abrasion and corrosion, necessitating expensive materials like copper-tin alloys and inefficient resurfacing techniques that do not effectively treat the entire molding surface.
A method involving cold spraying of metal powder onto the molding surface of glassware molds to create a solid deposit, followed by machining to form a coating, using specific metal powders and conditions to enhance thermal conductivity and abrasion resistance.
The method improves thermal conductivity and reduces mold wear, extending the lifespan and reducing replacement frequency while maintaining the structural integrity of the molds.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
Title of the invention: Surface treatment of a glassware mold by cold projection of a metal powder Field of invention
[0001] The present application relates generally to foundry parts in the field of glassmaking, in particular molds made of cast iron, brass, bronze (and other alloys comprising copper and tin) or steel used to make glass objects such as bottles.
[0002] The present application relates more particularly to the surface treatment of the metal molding surface of these molds which comes into contact with the parison during the manufacture of glass objects during the roughing and finishing phase in order to improve the thermal and / or mechanical properties of the molds. State of the art
[0003] The manufacture of a glass object, particularly hollow glass such as a bottle, is carried out in several stages.
[0004] During a first step called roughing, viscous glass is melted (at a temperature between 700°C and 1200°C) and cast in the form of a parison (drop) in a mold, called a roughing mold. The viscous glass undergoes compression in the roughing mold and is then pierced in order to bring it into contact with the walls of the roughing mold and obtain a roughing. The roughing then has a temperature which can reach 900°C, depending on the area and the thickness of the roughing.
[0005] Then, during a second stage called finishing, the blank thus formed is transferred into a finishing mold to be blown and give it its final shape. During contact between the blank and the finishing mold, a strong reduction in temperature occurs as well as an elongation of the glass. The final product is obtained after this blowing stage. It then has a temperature of around 600°C.
[0006] Glassware molds thus have several functions.
[0007] First of all, glass molds have a thermal function by allowing the glass to cool. It is necessary that, upon leaving the blank mold, the blank is sufficiently cooled to retain its shape. To this end, the blank should remain in the blank mold for a sufficient time to allow the dissipation of a quantity of heat allowing the glass to reach the desired viscosity. It is easy to understand that this quantity of heat increases with the weight of the blank, which, at constant thermal conductivity, normally leads to an extension of the residence time in the blank mold. Added to this is the fact that, during the finishing step, the molding surface of the mold will heat up via the heat transfer between the core of the blank and its surface. To avoid both the cooling time in the blank mold becoming excessive and incompatible with an industrial production rate and the surface temperature of the finishing mold becoming excessive and leading to a modification of its structure, it is therefore advisable to carefully choose the mold material so that it has sufficient thermal conductivity.
[0008] For bulky objects such as bottles of sparkling wine and champagne, molds made of copper and tin alloys, particularly bronze, which have good thermal conductivity, have been proposed. However, these molds are very expensive.
[0009] It is therefore desirable to have glass molds which, while exhibiting good thermal conductivity, are less expensive than molds made of copper and tin alloy.
[0010] Then, glassware molds have a geometric function since they give the article its final shape. This function is however undermined by problems of mold wear. These molds, most often made of cast iron, bronze (and other alloys including copper and tin), or steel (in particular iron-carbon steels, stainless steels, refractory steels), tend to wear quickly, particularly in areas such as the joint plane (or seam), the bottom, the ring or even the neck of the mold, due to a phenomenon of abrasion and / or corrosion due to the presence of silica in the glass. In order to avoid having to change the entire mold, techniques of recharging with a torch, by Plasma Transferred Arc (PTA) or by laser have been proposed, during which a layer of metal alloy is fused onto the surface of a mold, at the edges.The mold thus obtained is then machined after cooling in order to obtain the desired geometry.
[0011] However, known reloading techniques are not entirely satisfactory, insofar as they only allow the edges to be treated and not the entire molding surface. Indeed, treating the entire molding surface with these known techniques induces a high risk of cracking of the mold. Known reloading techniques therefore do not completely prevent wear of the molds, which, as a result, must be regularly replaced.
[0012] It is therefore desirable to have new reloading techniques allowing the entire molding surface to be treated. Exposed
[0013] An aim of the present application is to remedy at least in part the aforementioned drawbacks.
[0014] To this end, the invention relates, according to a first aspect, to a method of surface treatment for treating a molding surface of a glassware mold, the surface treatment method comprising the following steps: - cold projection of a solid metal powder onto the molding surface of the glassware mold so as to obtain a solid deposit; and - machining of the solid deposit to obtain a coating.
[0015] According to particular embodiments of the invention, the surface treatment method also has one or more of the following characteristics, taken in isolation or in any technically possible combination(s): - the metal powder is projected using a projection gas subjected to a pressure greater than thirty bars, for example between forty bars and seventy bars, for example around fifty bars; - the metal powder is projected using a projection gas heated to a temperature greater than or equal to 750°C, in particular greater than or equal to 900°C, for example between 990°C and 1010°C; - during the projection step, a projection distance, corresponding to a distance between a nozzle for projection of the metal powder and the molding surface, is between 15 millimeters and 60 millimeters, preferably between 15 and 35 millimeters, for example equal to approximately 20 millimeters or approximately 30 millimeters; - during the projection step, a speed of movement of a nozzle for projection of the metal powder during projection is between 500 millimeters per second and 1000 millimeters per second, for example equal to approximately 800 millimeters per second; - the projection step is carried out for a sufficient time to obtain a solid deposit having a thickness of between 0.3 millimeters and 3 millimeters, preferably between 0.5 millimeters and 1 millimeter; - an injection flow rate of the metal powder into the projection gas is between 5.936 and 17.808 cmVmin, preferably between 8.904 and 14.840 cmVmin, for example of the order of 11.872 cmVmin; - the coating has better mechanical resistance than the casting surface, in particular better abrasion resistance; - the metal powder comprises and advantageously consists essentially of NiCr powder; - the glass mold is a mold for borosilicate glass or a mold made of a copper and tin alloy, for example bronze; - the coating has a thermal conductivity higher than that of the molding surface; - the metal powder comprises and is advantageously essentially consisting of, in mass relative to the total mass of the powder: • between 60 and 70%, preferably between 62 and 68%, of copper; • between 7 and 17%, preferably between 10 and 15%, of nickel; • between 5 and 15%, preferably between 8 and 12%, of aluminum; • between 5 and 15%, preferably between 8 and 12%, of zinc; - the glass mold is a mold for soda-lime glasses; and - the glassware mold is made of graphite cast iron with a micrographitic structure mellar, vermicular or spheroidal, in iron-carbon steel, refractory steel or stainless steel.
[0016] The invention also relates, according to a second aspect, to a metal powder for the surface treatment of a glassware mold in accordance with a surface treatment method according to the first aspect.
[0017] According to particular embodiments of the invention, the metal powder has one or more of the following characteristics, taken in isolation or in any technically possible combination(s): - said metal powder comprises and advantageously consists essentially of NiCr powder; - the nickel content in the NiCr powder is between 40 and 50% by mass and the chromium content is between 50% and 60% by mass, relative to the total mass of the NiCr powder; - the nickel content in the NiCr powder is between 55 and 85% by mass and the chromium content is between 15% and 45% by mass, relative to the total mass of the NiCr powder; - a particle size of NiCr powder is between 10 and 40 micrometers; - said metal powder comprises and is advantageously essentially made up of, by mass relative to the total mass of the powder: • between 60 and 70%, preferably between 62 and 68%, of copper; • between 7 and 17%, preferably between 10 and 15%, of nickel; • between 5 and 15%, preferably between 8 and 12%, of aluminum; • between 5 and 15%, preferably between 8 and 12%, of zinc. - a particle size of the metal powder is greater than or equal to 15 microns and less than or equal to 45 microns.
[0018] The invention also relates, according to a third aspect, to a glassware mold comprising: - a molding surface; and - a coating covering all or part of the molding surface and comprising a metal alloy resulting from the cold projection of a powder metal on the casting surface in accordance with a surface treatment method according to the first aspect.
[0019] According to particular embodiments of the invention, the glassware mold also has one or more of the following characteristics, taken in isolation or in any technically possible combination(s): - the metal powder is made up mainly of nickel and chromium; - the molding surface comprises at least one of the following materials: graphite cast iron with a lamellar, vermicular or spheroidal micrographitic structure, a copper-tin based alloy such as bronze, iron-carbon steel, refractory steel or stainless steel, brass; - the coating is obtained by cold projection of a metallic powder according to the second aspect.
[0020] Finally, the invention has as its subject matter, according to a fourth and a fifth aspect, a machine for surface treatment of a glassware mold, comprising a support configured to receive a glassware mold having a molding surface and a projection nozzle configured to cold project a metal powder in the solid state onto the molding surface so as to obtain a solid deposit, and an installation comprising a surface treatment machine according to the fourth aspect and a machining station configured to machine the solid deposit and obtain a coating. Description of figures
[0021] Other characteristics, aims and advantages will emerge from the following description, which is purely illustrative and non-limiting and is given with reference to the appended drawings, in which: - [Fig.l] schematically illustrates an example of an installation for the surface treatment of a glassware mold conforming to a method of rea lization; - [Fig.2] is a flowchart illustrating steps of a method of surface treatment of a glassware mold according to one embodiment; - [Fig.3] is a schematic sectional view of a glassware mold comprising a coating according to one embodiment;
[0022] Throughout the figures, similar elements bear identical references. Detailed description
[0023] With reference to [Fig.l], the present application relates to the surface treatment of all or part of the molding surface 2 of a glassware mold 1. The glassware mold 1 may in particular comprise a blank mold 1 configured to receive a drop of glass (parison) and form a blank. The molding surface 2 corresponds to the surface of the mold 1 likely to come into contact with the parison during the molding process. The molding surface 2 may in particular comprise at least one of the following materials: graphite cast iron with a lamellar, vermicular or spheroidal micrographitic structure, bronze (and other alloys comprising copper and tin), steel of the iron-carbon steel type, refractory steel or stainless steel, brass. Preferably, the glassware mold 1 is integrally formed from the same constituent material as the molding surface 2.
[0024] In order to treat the molding surface 2 of a glassware mold 1, it is proposed to cold-project and at a very high speed, by a projection gas 3 under high pressure transporting it, a metal powder 4 onto all or part of the molding surface 2.
[0025] Cold and high-pressure projection, known by its English name of “cold spray”, makes it possible to obtain a deposit density very close to the theoretical density of the solid metallic material constituting the powder, without heating the molding surface 2 during the deposition, which avoids modifying the metallurgical quality of the molding surface 2 and of the solid deposit 5. It also makes it possible to obtain large thicknesses of deposits (up to several millimeters) with low roughness and a material yield of more than 90%, as well as high interparticle cohesion. In addition, the implementation of this cold projection does not require a prior step of preparing the molding surface 2 or masking the mold 1 to be treated. SURFACE TREATMENT FACILITY 9
[0026] An installation 9 intended for this treatment of all or part of the molding surface 2 of a glassware mold 1 is shown in [Fig.l]. This installation 9 comprises a surface treatment machine 10 and a machining station 11.
[0027] The surface treatment machine 10 is configured to cold spray the metal powder 4, in solid form, onto the molding surface 2 of the mold 1. For this purpose, it comprises a spray nozzle 7, preferably made of ceramic, comprising: - a system for heating and pressurizing a projection gas 3, typically nitrogen or helium, in a pressurization chamber 12; - a powder dispenser 13 for supplying the metal powder 4; - an injection system 18 for injecting the metal powder 4 into the projection gas 3 downstream of the pressurization chamber 12 so that it is not heated by the surface treatment machine 10 and therefore remains in the solid state; - a transport system 19 for transporting the metal powder 4 from the powder distributor 13 to the injection system 18 by means of a carrier gas (typically identical to the projection gas 3); - a convergent-divergent nozzle 8 placed downstream of the injection system 18 and configured to accelerate the projection gas 3 when it transports the metal powder 4, the diverging part of the nozzle 8 forming a deposition tube 14; and - a cooling system 15 which may comprise a conduit which surrounds the deposition tube 14 in order to cool the projection gas 3, which transports the metal powder 4, by conduction by circulating a cooling fluid around the deposition tube 14; the cooling fluid may in particular comprise distilled water at a temperature lower than the temperature of the projection gas 3, typically at a temperature between 8 and 20°C.
[0028] The projection nozzle 7 has an outlet diameter (at the free end of the deposition tube 14) of between two and ten millimeters, for example of the order of six millimeters.
[0029] The surface treatment machine 10 further comprises a support 17 configured to fix the glassware mold 1 relative to the projection nozzle and actuators (not shown) configured to move the projection nozzle 7 relative to the molding surface 2 in the three spatial directions. These actuators can move the projection nozzle 7, the support 17 on which the mold 1 is mounted or both the projection nozzle 7 and the support 17. The actuators are configured to move the nozzle 7 relative to the molding surface 2 at a speed of between 600 millimeters per second (mm / s) and 1000 millimeters per second (mm / s), for example of the order of 800 millimeters per second (mm / s) (to within 5%). The actuators are further configured to shift the impact zone by a distance of between 0.5 millimeters and two millimeters (no projection between two adjacent cords), for example of the order of one millimeter (to within 10%).
[0030] The heating system is configured to heat the projection gas 3 to a temperature greater than or equal to 750°C, in particular greater than or equal to 900°C, for example between 990°C and 1010°C. The projection gas 3 is furthermore pressurized in the pressurization chamber to a pressure greater than or equal to thirty-five bars, preferably between forty bars and seventy bars, for example of the order of fifty bars.
[0031] The projection nozzle 7 can be controlled by a remote control station 16, placed near the surface treatment machine 10 or remotely.
[0032] The machining station 11 comprises a support configured to receive the mold 1 coated with the solid deposit 5 and a machining tool, such as a milling machine, configured to machine the solid deposit 5 and obtain the coating 6. The machining tool can be handled by an operator or mounted on the installation 8 and controlled by a remote control station, for example the same control station 16 of the projection nozzle 7. SURFACE TREATMENT PROCESS 100
[0033] A method 100 for treating the molding surface 2, implemented by the surface treatment installation 9, is shown in [Fig.2]. It includes the following steps: - cold projection 110 of a metal powder 4 in the solid state onto the molding surface 2 of the glassware mold 1 so as to obtain a solid deposit 5; and - machining 120 of the solid deposit 5 so as to obtain a coating 6 ([Fig.3]).
[0034] The method 100 can be applied to the entire molding surface 2 of the mold 1 or to only a part of this surface 2.
[0035] During the projection step 110, a high-temperature (typically nitrogen or helium) and high-pressure projection gas 3 is used to propel the metal powder 4 at a supersonic speed (greater than 300 m / s) onto the molding surface 2 in order to create a solid deposit 5 intended to form the coating 6 by impact of the metal powder 4 on the molding surface 2, the impact force ensuring the quality of the deposit. In the present application, the deposit is said to be “solid” insofar as the grains of the metal powder 4 remain in the solid state throughout the projection and adhesion step 110 to the molding surface 2, as opposed to processes during which the temperature of the metal powder 4 exceeds its melting temperature so that all or part of the powder 4 melts at some point during the process.When the metal powder 4 comes into contact at high speed with the molding surface 2, it mechanically adheres to the molding surface 2 by plastic deformation with strong adhesion, which makes it possible to avoid defects linked to high temperatures such as oxidation, residual stresses, phase transformations, etc. The solid deposit 5 is then integral with the molding surface 2, that is to say that it can only be separated from the molding surface 2 by being completely or partially damaged.
[0036] The projection step 110 is said to be cold insofar as the metal powder 4 is not heated before or during deposition, other than by its contact with the projection gas 3 or the molding surface 2.
[0037] During the projection step 110, the projection gas 3 is heated and pressurized in order to ensure that the metal powder 4 is projected at a projection speed (speed of the metal powder 4 at the outlet of the nozzle 7) capable of allowing the plastic deformation of the metal powder 4 during its impact against the contact surface. It will be noted that the gas is heated and pressurized before injection of the solid powder into the gas and its projection onto the molding surface 2 in order to ensure that the metal powder 4 remains in the solid state. For this purpose, said projection speed is greater than or equal to the critical speed of the metal powder 4. This critical speed corresponds to the speed from which the attachment (adhesion) of the solid deposit 5 is possible: when the impact speed is lower than the critical speed of the material, then the particles of metal powder 4 do not deform plastically. and can rebound and / or erode the molding surface 2. The critical speed depends on the nature of the material and the grain size of the metal powder 4. The critical speed is for example higher in the case of a metal powder 4 comprising a hard material, such as a titanium dioxide-based material (above 1250 m / s), than in the case of a metal powder 4 comprising a ductile material, such as a copper-based material (of the order of 600 m / s). An equation E1 for determining the critical speed of a material has been demonstrated by T. Schmidt, F. Gartner, H. Assadi, H. Kreye, “Development of a generalized parameter window for cold spray deposition”, Acta Mater. 54 (2006) 729-742; https: / / doi.Org / 10.1016 / j.actamat.2005.10.005) : where: or is the breaking stress of the material; p is the density of the material to be characterized; T; is the initial temperature of the material to be characterized; Tm is the melting temperature of the material to be characterized; cp is the specific heat; Tr is a reference temperature equal to 293 K; and Fi and F2 are calibration coefficients used to recalibrate the calculated value to measured speed values.
[0038] The pressure applied to the projection gas 3 is therefore chosen so as to exceed the critical speed of the metal powder 4 used for the solid deposition 5. A pressure greater than or equal to thirty-five bars, preferably greater than or equal to forty bars, for example equal to fifty bars, is suitable for most metal powders which can be used in the surface treatment of a glassware mold.
[0039] Furthermore, the temperature to which the projection gas 3 is heated is typically greater than or equal to 750°C, in particular greater than or equal to 900°C, for example between 990°C and 1010°C. This heating temperature is advantageously at least 300°C below the melting temperature of the constituent of the metal powder 4 with the lowest melting temperature and for example between 300 and 700°C below this melting temperature.
[0040] If necessary, the projection gas 3 can further be accelerated by the configuration of the projection nozzle 7 (modification of the gas passage section, for example in a convergent-divergent nozzle 8, etc.).
[0041] For a nickel-chromium based powder as described below, the critical speed is for example of the order of 574 m / s.
[0042] If necessary, the projection gas 3 can be cooled downstream of the point of injection of the metal powder 4 into the gas in order to ensure that the metal powder 4 remains solid without reducing the projection speed of the powder.
[0043] The projection step 110 is carried out so as to obtain a solid deposit 5 whose thickness is sufficient to allow machining of the solid deposit 5 and obtaining of the coating 6. This thickness of the solid deposit 5 is typically between 0.3 millimeters and 3 millimeters, preferably between 0.5 millimeters and 1 millimeter. The thickness of the coating 6 (after machining) can thus be between 0.1 millimeters and 1.5 millimeters.
[0044] For this purpose, the molding surface 2 is moved relative to the surface treatment machine 10 during the projection step 110 in order to carry out a deposit on all or part of the molding surface 2. The projection nozzle 7 can be moved while the glassware mold 1 is fixed, or alternatively the glassware mold 1 can be moved while the projection nozzle 7 is fixed, or both the projection nozzle 7 and the glassware mold 1 are moved. The relative movement speed and the number of passes over a given surface determine the thickness of the deposit. For example, the relative displacement speed of the projection nozzle 7 and the molding surface 2 of the glassware mold 1 may be between 600 millimeters per second (mm / s) and 1000 millimeters per second (mm / s), for example of the order of 800 millimeters per second (mm / s) (to within 5%).
[0045] The flow rate of supply of the metal powder 4 by the distributor 13 is between 5.936 and 17.808 cmVmin, preferably between 8.904 and 14.840 cmVmin, for example of the order of 11.872 cmVmin. The metal powder 4 thus supplied is entirely transported by the carrier gas to the injection system 18, so that this supply flow rate also constitutes a flow rate of injection of the metal powder 4 into the projection gas 3 by the injection system 18. For this purpose, the flow rate of carrier gas is typically between 3 and 6 cubic meters per hour (m3 / h), for example of the order of 4.5 cubic meters per hour (m3 / h).
[0046] The size (width of the bead) of the solid deposit 5 is preferably between 0.5 millimeters and two millimeters, for example of the order of one millimeter (to within 10%). This size depends on the distance between the outlet of the projection nozzle 7 of the surface treatment machine 10 and the molding surface 2 and on the outlet diameter of the projection nozzle 7. In order to obtain the aforementioned solid deposit size, said distance is typically between fifteen millimeters and sixty millimeters, preferably between fifteen millimeters and thirty-five millimeters, for example equal to approximately twenty millimeters or approximately thirty millimeters, for an outlet diameter of the projection nozzle 7 of between two and ten millimeters, for example of the order of six millimeters.
[0047] The projection pitch (distance between the centers of two adjacent solid deposit beads 5) is between 0.5 millimeters and two millimeters, for example of the order of one millimeter (to within 10%). It is preferably substantially equal to the size of the solid deposit 5. METAL POWDER 4
[0048] The metal powder 4 preferably comprises 75% by mass or more, advantageously at least 80% by mass, of spherical grains, relative to the total mass of the powder.
[0049] Laser granulometry is measured according to ISO 13320:2019.
[0050] The diameter of the grains of the powder is advantageously between 10 and 50 pm, in particular between 12 and 45 pm, and preferably has a D50 value between 20 and 30 pm.
[0051] The melting temperature of the powder compounds is typically higher than the parison temperature - which can reach 1100°C - in order to avoid thermal degradation of the coating 6 during molding. Preferably, the melting temperature of the powder component having the lowest melting temperature is 300°C higher than the parison temperature.
[0052] The “packed density” is evaluated according to the basis of the NF EN ISO 3923 (2018) standard relating to “Metal powders - Determination of the apparent density after tamping”. Typically, a test tube with a volume of 25 cm3 and a KERN SEAL balance with a maximum capacity of 6000 g and a resolution of 0.1 g are used. The tamping is stopped after 3000 strokes.
[0053] The "true density" is evaluated according to the basis of the standard NF EN ISO 8130-2 (2011) relating to "Powders for coating - Determination of the density using a gas pycnometer (reference method)". A helium pycnometer (Quantachrome Upyc 1200 e) with a 10 cm3 cell is used. The mass of the powder is measured with a balance, for example METTLER TOLEDO AB 104 with a maximum capacity of 110 g and a resolution of 0.1 mg.
[0054] The packed density of the metal powder is typically between 3 and 7 g / cm3
[0055] The true density is typically between 6 and 10 g / cm3, preferably with a low standard deviation, for example 0.001. Metal powders having such a true density in fact make it possible to obtain a denser solid deposit 5.
[0056] For the purposes of the present invention, a powder is “essentially composed” of a compound A when the powder comprises at least 99% by mass of the compound A, relative to the total mass of the powder.
[0057] Metal powder comprising a NiCr alloy
[0058] According to a first embodiment, the metal powder 4 comprises or is essentially made up of an alloy of nickel and chromium (called nickel-chromium alloy and denoted NiCr). This makes it possible to obtain a coating 6 comprising NiCr which gives to the mold 1 thermomechanical protection. In particular, a coating 6 comprising NiCr gives the mold 1 better abrasion resistance, which is particularly useful in the case of molds for borosilicate glasses and in the case of molds made of copper and tin alloy. Indeed, borosilicate glasses are particularly abrasive and generally lead to premature wear of the molds. As for molds made of copper and tin alloy, they have good thermal conductivity and are generally very expensive, so that it is advantageous to lose a little of the thermal conductivity of the mold if this allows it to be preserved for a longer time.
[0059] Thus, according to an advantageous variant of this first embodiment, the glassware mold 1 is a mold for borosilicate glass or a mold made of a copper and tin alloy, for example bronze.
[0060] The nickel content in the NiCr alloy is advantageously between 40% and 85% by mass, preferably between 45 and 80% by mass, relative to the total mass of the NiCr alloy, the remainder being essentially made up of chromium.
[0061] According to a first variant, the nickel content in the NiCr alloy is between 40 and 50% by mass, while the chromium content is between 50% and 60% by mass, relative to the total mass of the NiCr alloy. For example, the nickel content in the NiCr alloy is substantially equal to 50% by mass, the chromium content also being substantially equal to 50% by mass, relative to the total mass of the NiCr alloy. According to a second variant, the nickel content in the NiCr alloy is approximately 80% by mass, while the chromium content is approximately 20% by mass, relative to the total mass of the NiCr alloy.
[0062] The particle size of the NiCr powder is advantageously between 10 and 50 pm. The D50 value of the NiCr powder is typically between 20 and 30 pm, preferably between 25 and 27 pm, for example substantially equal to 26.1 pm. The D10 value of the NiCr powder is typically between 10 and 20 pm, preferably between 14 and 16 pm, for example substantially equal to 14.7 pm. The D90 value of the NiCr powder is typically between 40 and 50 pm, preferably between 43 and 45 pm, for example substantially equal to 44.0 pm.
[0063] The packed density of the NiCr powder is typically between 4 and 5 g / cm3, in particular between 4.3 and 4.8 g / cm3, for example of the order of 4.7 g / cm3. The true density of the NiCr powder is typically between 7.5 and 8.5 g / cm3, in particular between 7.6 and 8.0 g / cm3, for example of the order of 7.71 g / cm3.
[0064] Metal powder comprising a cupronickel type alloy
[0065] According to a second embodiment, the metal powder 4 comprises or is essentially made up of an alloy of copper, nickel, aluminum and zinc, which for the sake of for simplification will be called "cupronickel" in the following. This makes it possible to obtain a coating 6 comprising a so-called "cupronickel" alloy which gives the mold better thermal conductivity, which allows the glass to be cooled more homogeneously during contact with the coated mold. Such a coating is particularly advantageous in the case of molds for soda-lime glasses.
[0066] Thus, according to an advantageous variant of this first embodiment, the glassware mold 1 is a mold for soda-lime glasses. The material of the mold 1 is typically a cast iron, for example a graphite cast iron with a lamellar, vermicular or spheroidal micrographitic structure, an iron-carbon steel, a refractory steel or a stainless steel.
[0067] According to this second embodiment, the metal powder 4 comprises or is essentially constituted of a powder of an alloy comprising, by mass relative to the total mass of the alloy: • between 60 and 70%, preferably between 62 and 68%, of copper; • between 7 and 17%, preferably between 10 and 15%, of nickel; • between 5 and 15%, preferably between 8 and 12%, of aluminum; • between 5 and 15%, preferably between 8 and 12%, of zinc; • the possible complement preferably being essentially made up of chromium, manganese and / or iron.
[0068] Typically, the complement represents at most 3% by mass relative to the total mass of the alloy. Preferably, the complement comprises, by mass relative to the total mass of the alloy: • at most 1% chromium; • not more than 1% manganese; and • at most 1% iron.
[0069] The packed density of the “cupronickel” powder is typically between 1 and 6 g / cm3, in particular between 4.5 and 5.5 g / cm3. The true density of the powder of "cupronickel" is typically between 4 and 9 g / cm3, especially between 7.5 and 9.0 g / cm3.
[0070] The particle size of the “cupronickel” powder is advantageously between 15 and 45 μm. The D50 value of the “cupronickel” powder is typically between 20 and 30 μm. ADVANTAGES OF THE INVENTION
[0071] Thus, thanks to the invention described above, it is possible to improve both the abrasion resistance and the thermal conductivity of the glassware mold 1. It is therefore possible to reduce the frequency of replacement of the glassware molds, by completely coating their molding surface with a coating having good abrasion resistance, such as a NiCr coating, or to use for the molding of large volumes of glass or soda-lime glass from less expensive molds whose molding surface is simply coated with a coating having good thermal conductivity, such as a "cupronickel" alloy coating.
[0072] The costs of purchasing and replacing molds can thus be reduced.
Claims
Claims
1. Surface treatment method (100) for treating a molding surface (2) of a glassware mold (1), the surface treatment method (100) comprising the following steps: - cold spraying (110) of a metal powder (4) in the solid state onto the molding surface (2) of the glassware mold (1) so as to obtain a solid deposit (5); and - machining (120) of the solid deposit (5) so as to obtain a coating (6).
2. Surface treatment method (100) according to claim 1, in which the metal powder (4) is projected using a projection gas (3) subjected to a pressure greater than thirty bars, for example between forty bars and seventy bars, for example approximately fifty bars.
3. Surface treatment method (100) according to one of claims 1 or 2, in which the metal powder (4) is projected using a projection gas (3) heated to a temperature greater than or equal to 750°C, in particular greater than or equal to 900°C, for example between 990°C and 1010°C.
4. Surface treatment method (100) according to one of claims 1 to 3, wherein during the projection step (110), a projection distance, corresponding to a distance between a projection nozzle (7) of the metal powder (4) and the molding surface (2), is between 15 millimeters and 60 millimeters, preferably between 15 and 35 millimeters, for example equal to approximately 20 millimeters or approximately 30 millimeters.
5. Surface treatment method (100) according to one of claims 1 to 4, wherein during the projection step (110), a speed of movement of a projection nozzle (7) of the metal powder (4) during the projection is between 500 millimeters per second (mm / s) and 1000 millimeters per second (mm / s), for example equal to approximately 800 millimeters per second (mm / s).
6. Surface treatment method (100) according to one of claims 1 to 5, in which the projection step (110) is carried out for a sufficient time to obtain a solid deposit (5) having a thickness between 0.3 millimeters and 3 millimeters, preferably between 0.5 millimeters and 1 millimeter.
7. Surface treatment method (100) according to one of claims 1 to 6, in which an injection flow rate of the metal powder (4) into the projection gas (3) is between 5.936 and 17.808 cmVmin, preferably between 8.904 and 14.840 cmVmin, for example of the order of 11.872 cmVmin.
8. Surface treatment method (100) according to one of claims 1 to 7, wherein the coating (6) has better mechanical resistance than the molding surface (2), in particular better abrasion resistance.
9. Surface treatment method (100) according to one of claims 1 to 7, wherein the coating (6) has a thermal conductivity greater than that of the molding surface (2).
10. Surface treatment method (100) according to one of claims 1 to 9, in which the metal powder (4) comprises and advantageously consists essentially of NiCr powder.
11. Surface treatment method (100) according to one of claims 1 to 9, in which the metal powder (4) comprises and advantageously consists essentially of, by mass relative to the total mass of the powder: • between 60 and 70%, preferably between 62 and 68%, of copper; • between 7 and 17%, preferably between 10 and 15%, of nickel; • between 5 and 15%, preferably between 8 and 12%, of aluminum; • between 5 and 15%, preferably between 8 and 12%, of zinc.
12. Glassware mold (1) comprising: - a molding surface (2); and - a coating (6) covering all or part of the molding surface (2) and comprising a metal alloy resulting from the cold projection of a metal powder (4) onto the molding surface (2) in accordance with a surface treatment method (100) according to one of claims 1 to 9.
13. A glassware mold (1) according to claim 12, wherein the powder metallic (4) is made up mainly of nickel and chromium.
14. Glassware mold (1) according to one of claims 12 and 13, wherein the molding surface (2) comprises at least one of the following materials: graphite cast iron with a lamellar, vermicular or spheroidal micrographitic structure, a copper and tin-based alloy such as bronze, iron-carbon steel, refractory steel or stainless steel, brass.
15. Glassware mold (1) according to one of claims 12 to 14, in which the coating (6) is obtained by cold spraying of a metal powder comprising and advantageously being essentially constituted of NiCr powder or of a metal powder comprising and advantageously being essentially constituted of, by mass relative to the total mass of the powder: • between 60 and 70%, preferably between 62 and 68%, of copper; • between 7 and 17%, preferably between 10 and 15%, of nickel; • between 5 and 15%, preferably between 8 and 12%, of aluminum; • between 5 and 15%, preferably between 8 and 12%, of zinc.
16. Surface treatment machine (10) for a glassware mold (1) comprising: - a support (17) configured to receive a glassware mold (1) having a molding surface (2); and - a projection nozzle (7) configured to cold project a metal powder (4) in the solid state onto the molding surface (2) so as to obtain a solid deposit (5).
17. Installation comprising a surface treatment machine (10) according to claim 16 and a machining station (11) configured to machine the solid deposit (5) and obtain a coating (6).
Citation Information
Patent Citations
Method for refilling a mold for glas using powder laser buildup
EP2540433A1
Laser recharging powder, associated manufacturing method and mould
EP3834960A1
Glass working tools mfr. - by chromaluminisation of nickel, iron or copper (SW201276)
FR2311639A1
Powder for cold spray, method for manufacturing macromolecular coating film, and macromolecular coating film
US20170152601A1