Copolymers containing polydimethylsiloxane (PDMS) portions

A triblock copolymer synthesized from PDMS and polyamide with controlled reactions at elevated temperatures addresses the complexity and cost issues of silicone elastomers, providing stable and reversible mechanical properties for medical adhesives.

FR3149011A1Pending Publication Date: 2024-11-29INST POLYTECHN DE BORDEAUX +4
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
FR2023005083
Authority / Receiving Office
FR · FR
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-23
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing silicone elastomers used in medical adhesives are complex to manufacture, expensive, and have unstable mechanical properties due to irreversible cross-linking, making them unsuitable for practical applications.

Method used

A triblock copolymer is synthesized by reacting polydimethylsiloxane (PDMS) with terminal amine groups and a molar excess of isocyanate, followed by a polyamide with amine terminal groups at elevated temperatures, creating a reversible solid-liquid transition for improved mechanical stability and ease of processing.

Benefits of technology

The process results in copolymers with stable mechanical properties and a reversible melting temperature, allowing for practical use under hot melt conditions and easy reprocessing, reducing manufacturing complexity and cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000045_0000
    Figure 00000045_0000
  • Figure 00000045_0001
    Figure 00000045_0001
  • Figure 00000046_0000
    Figure 00000046_0000
Patent Text Reader

Abstract

Copolymers containing polydimethylsiloxane (PDMS) parts The present invention relates to a process for the synthesis of a triblock copolymer comprising the following steps: (1) reaction between (A) a polydimethylsiloxane (PDMS) comprising at least two amine terminal groups, i.e. primary amine (-NH2) and / or secondary amine (-NH(alkyl)) groups, and (B) a molar excess, relative to all molecules of type (A), of a molecule comprising at least two isocyanate (-N=C=O) groups, in order to obtain a prepolymer terminated by isocyanate groups; (2) reaction between the prepolymer obtained in step (1) and a polyamide comprising an amine terminal group (-NH2), the number of moles of polyamide comprising an amine terminal group (-NH2) being at least equivalent to the number of moles of isocyanate (-N=C=O) groups in the prepolymer obtained in step (1). The present invention also relates to a triblock copolymer thus obtained and the use thereof in dressings.
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: Copolymers containing polydimethylsiloxane (PDMS) parts Technical field

[0001] The present invention relates to novel copolymers containing polydimethylsiloxane (PDMS) parts, the use of such copolymers in adhesive products intended to be applied to the skin, wounds, appendages and / or mucous membranes, and dressings comprising an elastomeric matrix obtained from such copolymers. Prior art

[0002] Silicone elastomers are used in many fields (automotive, medical devices, childcare, optics, cosmetics, etc.). In the field of adhesives, silicone elastomers are particularly interesting in a medical context, particularly in their application to the skin, wounds, appendages or mucous membranes. They are "soft" adhesives, which are not aggressive on the skin in the sense that they are well tolerated, while exhibiting good resistance over time. They are also repositionable, atraumatic upon removal and therefore well tolerated by the skin, in particular fragile skin such as peri-wound skin. These adhesives can be applied, removed and then reapplied, without leaving residue or causing redness. Silicones can be used at the edge of dressings or in direct contact with the wound to be treated.

[0003] However, the manufacturing processes for silicone elastomers are quite complex: whether they are obtained by hot or cold vulcanization, their manufacturing process must comply with very precise temperature and humidity conditions. In addition, due to the nature of the components used in their composition and the process for obtaining them, silicone elastomers are expensive.

[0004] In the general context of adhesive copolymers containing polydimethylsiloxane (PDMS) parts, not limited to medical-type adhesive applications such as in dressings, among the prior technologies using polysiloxanes linked to other polymer segments via isocyanate or amide groups, mention may be made of: - applications US 2006 / 194937 and US 2006 / 036055 which describe polydimethyl-siloxane (PDMS) terminated by amino (bisaminomethyl) groups, reacted with diisocyanates; - applications US 2013 / 225768 and US 2007 / 148475 which describe a technology comprising the reaction of a PDMS diamine with diethyl oxalate, the product resulting from this reaction can then be reacted with diamines such as ethylenediamine. - US patent 6,090,902 which describes poly(ethylene-butylene) with groups in the terminal position carrying an isocyanate residue, obtained with methacryloyl isocyanate, the resulting polymer then being reacted with a PDMS carrying a methacryl group, in the presence of 2-ethylhexyl acrylate; - application US 2021 / 0009880 which describes polyolefin-polydiorganosiloxane copolymers, the synthesis route used involving the preparation of polyethylene with -SiMe2H groups in the terminal position, which can react with Si-OH groups carried in the terminal position by PDMS;

[0005] - application WO 2014 / 123775 which describes polysiloxane-polyamide copolymers whose bond is achieved by polymerization of diacids and diamines (such as hexamethylenediamine (HDMA) and adipic acid for Nylon 6,6) with the incorporation at the end of the reaction of undecylenic acid (UDA), introducing a C=C double bond which can react with a -SiH group of a siloxane; - application CN109384930 which describes a polyamide block copolymer based on a linear aliphatic chain (abbreviated in English) and polysiloxane; - application KR20170032726 which describes a polyamideimide-polydimethylsiloxane-polyamideimide (PAI-PDMS-PAI) triblock copolymer: _ O । s C> H il / 1 \ I h H PAt-'N-^-Of-SU * ' I ( 14 I PAi ^11 HJH ? H ' | j - V (b)

[0006] - application KR20160146250) which describes polymers as follows:

[0007] The present invention aims to develop specific copolymers whose manufacturing process is simple and inexpensive. The compatibility of the precursors is a relevant element for an efficient synthesis of the polymers. With regard to the copolymer product obtained, at the same time as a melting temperature which allows a use lisation under practical "hot melt" conditions with an appropriate solid-liquid transition temperature, copolymers with a fully reversible melting temperature and stable mechanical properties over time are required, instability in these properties being generally indicative of reactions such as additional crosslinks that occur after the initial synthesis of the copolymer.

[0008] The present invention relates not only to specific copolymers but also to an elastomeric matrix obtained from such copolymers. Finally, the present invention relates to a dressing comprising such an elastomeric matrix.

[0009] <Exposé de l’invention>

[0010] Thus, according to a first aspect, the present invention therefore relates to a method synthesis of a triblock copolymer comprising the following steps: (1) reaction between (A) a polydimethylsiloxane (PDMS) comprising at least two amine terminal groups, either primary amine (-NH2) and / or secondary amine (-NH(alkyl)) groups, and (B) a molar excess, relative to all molecules of type (A), of a molecule comprising at least two isocyanate groups (-N=C=O), in order to obtain a prepolymer terminated by isocyanate groups; (2) reaction between the prepolymer obtained in step (1) and a polyamide comprising an amine terminal group (-NH2), the number of moles of polyamide comprising an amine terminal group (-NH2) being at least equivalent to the number of moles of isocyanate groups (-N=C=O) in the prepolymer obtained in step (1).

[0011] According to a particular characteristic of the invention, step (2) is carried out at a minimum temperature Tf of at least 100°C, preferably at least 130°C.

[0012] According to a particular characteristic of the invention, in the process for synthesizing a triblock copolymer: - in step (1), a reaction is carried out, preferably at a temperature of at least 25°C and at most 50°C, between at least one polydimethylsiloxane of formula (A) [Chem. 1] ngU wri3 rlgU Ung ngU V113 H v / wwh Rz Ri Ri ^R2 (HAS) and at least one diisocyanate of formula (B): [Chem. 2] (B) with a molar ratio (B) / (A) > 1, to obtain a prepolymer terminated by isocyanate groups of formula (C): [Chem. 3] (C) in which - x represents an integer greater than or equal to 10; - n represents an integer greater than or equal to 1; - R1 and R2 represent saturated, linear or branched hydrocarbon groups; and - Li represents a saturated, linear or branched, cyclic or acyclic hydrocarbon group, or an unsaturated, linear or branched hydrocarbon group, comprising at least one double bond and / or at least one aromatic ring; and in step (2), a reaction is carried out between the prepolymer (C) obtained in step (1) and a semi-crystalline polyamide with a melting temperature Tf and comprising an amine terminal group (-NH2), of formula (D): [Chem. 4] (D) with a molar ratio (D) / (C) of more than 0 and less than 4, preferably (D) / (C) being approximately or equal to 2, at a reaction temperature T > Tf, to obtain the triblock copolymer of formula (E): [Chem. 5] (E) in which - y and z represent numbers between 0 and 100; - Tf represents a temperature greater than or equal to 100°C.

[0013] Preferably in the execution of a synthesis method according to the invention, a polydimethylsiloxane (PDMS) used in step (1) comprises at least least two primary amine terminal groups (-NH2), and preferably comprises terminal groups -(CH2)3NH2 and / or -(CH2)—(CH)CH3-(CH2)NH2, and / or RI may be chosen from the following groups, the symbol * indicating a branch point: (Rl-1) [Chem. 6] * —CH2-CH2-CH2 —* (R 1-2) [Chem. 7] CH3 I * —CH2 —CH —CH2—*

[0014] Preferably in the execution of a synthesis method according to the invention, the polydimethylsiloxane (PDMS) used in step (1) comprises at least two secondary amine end groups, preferably -NH(ethyl) or -NH(methyl) groups and / or R2 can be chosen from the following groups, the symbol * indicating a branch point: (R2-1 [Chem. 8]) * —H (R2-2) [Chem. 9] * —CH3 (R2-3) [Chem. 10] * — CH2 ~ CH3

[0015] Preferably in the execution of a synthesis method according to the invention, the polydimethylsiloxane (PDMS) used comprises at least two amine terminal groups, has a number-average molecular mass (Mn) of at least 500 g.mol1 and at most 150,000 g.mol *, preferably at least 800 g.mol1 and at most 50000 g.mol *, and / or the number of units x is at least 10 and at most 900.

[0016] Preferably in the execution of a synthesis process according to the invention, the molecule comprising at least two isocyanate groups (-N=C=O) is chosen from alkyl diisocyanates, aromatic diisocyanates or alicyclic diisocyanates.

[0017]

[0018]

[0019]

[0020] Preferably in the execution of a synthesis method according to the invention, L1 is a hydrocarbon structure such that at least 4 and at most 12 carbon atoms separate the two branching points by the shortest route, and preferably L1 is chosen from the following groups, the symbol * indicating a carbon atom forming part of the structure L1 and also being a branching point: (Ll-1) [Chem. 11] (Ll-2) [Chem. 12] (Ll-3) [Chem. 13] (Ll-4) [Chem. 14] (Ll-5) [Chem. 15] Preferably in the execution of a synthesis method according to the invention, the molecule comprising at least two isocyanate groups (-N=C=O) is an alkyl diisocyanate with the isocyanate groups in the terminal position, and preferably hexamethylene diisocyanate. Preferably in the execution of a synthesis method according to the invention, in step (1), the quantity used of the molecule comprising at least two isocyanate groups (-N=C=O) corresponds to a value (n+1) in number of moles, n being the number of moles of polydimethylsiloxane (PDMS) comprising at least two amine terminal groups (-NH2). Preferably in the execution of a synthesis process according to the invention, the polyamide comprising an amine terminal group (-NH2) used in step (2) is chosen from: a copolymer polyamide containing units of 6 and 11 carbon atoms, preferably a copolymer between 6-aminohexanoic acid and 11-aminoundecanoic acid and / or between caprolactam and 11-aminoundecanoic acid.

[0021] According to a second aspect, the present invention relates to a triblock copolymer obtained according to the process of the invention. A copolymer according to the present invention may also be a triblock copolymer having the following structure: [Chem. 16] PA in which: - each group (LDI'-LDF) corresponds to an alkyl, aromatic or alicyclic group, and preferably is a hydrocarbon structure such that at least 4 and at most 12 carbon atoms separate the two branching points by the shortest route, and preferably chosen from groups (L1-1) to (L1-5); - each group R1 corresponds to H, Me or Et; - polydimethylsiloxane (PDMS) is connected to -NR1- groups by reaction of a terminal -(CH2)3NH2 and / or -(CH2)—(CH)CH3-(CH2)NH2 bond of a starting PDMS; - PA denotes a polyamide.

[0022] According to a third aspect, the present invention relates to the use of a triblock copolymer according to the present invention in adhesive products intended to be applied to the skin, wounds, appendages and / or mucous membranes.

[0023] According to a third aspect, the present invention relates to a dressing comprising an elastomeric matrix obtained from the triblock copolymer according to the present invention. Preferably, in a dressing according to the present invention, the elastomeric matrix has through holes. In preferred dressings according to the present invention, the elastomeric matrix further contains one or more active ingredients for treating a wound, the active ingredients being selected from the group consisting of: antibacterials, antiseptics, painkillers, anti-inflammatories, healing-promoting active ingredients, and anesthetics. In preferred dressings according to the present invention, the elastomeric matrix obtained from the triblock copolymer is present in the form of an adhesive border allowing the dressing to be fixed to the skin surrounding a wound to be treated.In preferred dressings according to the present invention, the elastomeric matrix obtained. from the triblock copolymer is present in the form of a film having a thickness of at least 20 pm and at most 50 pm.

[0024] <Brève description des dessins>

[0025] [Fig-1] [Fig.l] represents a triblock synthesis diagram SC-b-PDMSurea-b-SC according to the present invention. [Fig.2] [Fig.2] represents the structure (A) and DSC analysis (B) of the polyamide used. [Fig.3] [Fig.3] represents the structures and DSC analyses of the polyethylenes used: PENH2 (A), PENH.hexyie (B) and P^ (C). [Fig.4] [Fig.4] represents thermograms of urea prepolymers: cooling (A) and heating (B) cycles. [Fig.5] [Fig.5] represents a study of the rheological properties of urea prepolymer 1 as a function of temperature. [Fig.6] [Fig.6] represents the rheological properties of urea prepolymers during a heating cycle. [Fig.7] [Fig.7] represents the thermograms of PENH2, urea prepolymer and PE-b-PDMSurea-b-PE triblock system: cooling (A) and heating (B) cycles. [Fig.8] [Fig.8] represents the rheological properties of the system PE-b-PDMSurea-b-PE before (A) and after addition of PE (B) during a heating cycle.

[0026] [Fig.9] [Fig.9] represents the thermograms of PANH2, urea prepolymer and of the PA-b-PDMSurea-b-PA triblock system: cooling (A) and heating (B) cycles. [Fig. 10] [Fig. 10] represents the rheological properties of the system PA-b-PDMSurea-b-PA before (A) and after addition of PA (B) during a heating cycle. [Fig. 11] [Fig. 11] represents a reaction scheme of the polyaddition of PDMS endNH2On HDI. [Fig. 12] [Fig. 12] represents a reaction scheme of the polyaddition of PA6-11 on the prepolymer PDMSurea- [Fig. 13] [Fig. 13] represents a DSC thermogram of the prepolymer PDMSurea [Fig. 14] [Fig. 14] represents a DSC thermogram of the triblock PA-b-PDMSurea-b-PA. [Fig. 15] [Fig. 15] represents the moduli G' and G" of PA-b-PDMSurea-b-PA as a function of temperature during a heating cycle. [Fig. 16] [Fig. 16] represents the stress curve as a function of the elongation of the PA-b-PDMSurea-b-PA system. [Fig. 17] [Fig. 17] represents a reaction scheme of the two-step synthesis of PA-b-PDMSureeth-b-PA. [Fig. 18] [Fig. 18] represents a DSC thermogram of a PA-b-PDMSurea eth-b-PA triblock. [Fig. 19] [Fig. 19] represents the rheological properties of the PA-b-PDMSurea eth-b-PA system during the second heating cycle. [Fig.20] [Fig.20] represents a reaction scheme of the two-step synthesis of PA-b-PDMSurea / urea eth-b-PA. [Fig.21] [Fig.21] represents the storage moduli of urea / ethyl urea prepolymers as a function of the urea fraction at room temperature. [Fig.22] [Fig.22] represents the evolution of G' as a function of the urea fraction at 25 °C (A); sol / liq transition temperature as a function of the urea fraction (B). [Fig.23] [Fig.23] represents a stress curve as a function of strain (A), maximum elongation (B) and elastic moduli as a function of the % of urea group (C) of the PA-b-PDMSurea / ureaeth--b-PA systems.

[0027] <Description des modes de réalisation>

[0028] The triblock copolymers according to the present invention comprise a polydimethylsiloxane (PDMS), linked by isocyanate-derived zones to a polyamide. In the context of the present invention, for the preparation of such copolymers, the compatibility of the PDMS and polyamide precursors is a relevant element for an efficient synthesis of the polymers. The polyamide part can strongly influence the final mechanical properties of the material (high elastic modulus, very low deformation under stress).Along with the issue of final mechanical properties, it is noted that a goal is also to prepare copolymers containing a polysiloxane block (such as PDMS) and semi-crystalline blocks, so that the semi-crystalline nodules are physical crosslinking nodes, which can be reversibly formed and destroyed by applying suitable temperature ramps, thus allowing reversible transition from an "elastic solid" state to a "viscous liquid" state. Preferably, the semi-crystalline blocks will have a melting temperature that is within the target temperature range of at least 100 °C and at most 140 °C.In this context, it has been observed by the inventors that some products obtained from PDMS precursors having hydroxyl groups along the chain and terminal epoxide groups, transformed into a copolymer by reaction with a secondary diamine such as NN-dimethyl-1,6-hexanediamine, are not satisfactory in an industrial context because the liquid-solid transition of the materials is not reversible. It seems that a parasitic reaction leads to the chemical (i.e. irreversible) crosslinking of the materials. Thus, after a storage time of a few weeks, the materials can no longer be melted in the form of a viscous liquid. They can no longer be easily solubilized in a solvent either. The inventors postulate that the pendant hydroxyl groups are involved in a . parasitic reaction leading to crosslinking of the PDMS phase, in particular with residual epoxy groups, or even with the terminal ester functions of the polyamide (PA).

[0029] According to the present invention, a PDMS terminated by amine functions is first reacted with a diisocyanate spacer, a preferred example of diisocyanate being hexamethylene diisocyanate. The ratio between reactants is chosen so that the PDMSurea prepolymers are terminated by isocyanate functions. The second synthesis step then consists of adding the monofunctional semi-crystalline polymer, terminated by an NH2 function, which will be able to react with the terminal isocyanate functions of PDMS prepolymers, to lead to the formation of SC-b-PDMSurea-b-SC triblock copolymers, where SC = semi-crystalline. The approach is described in [Fig. 1].

[0030] It is considered that the potential advantages of this approach are multiple: 1. Urea functional groups are known to develop strong hydrogen bonds (NH 2 O). Their presence along the PDMS chain should allow the development of intra-chain physical interactions within the PDMS phase, which in turn should make it more cohesive. This should improve the mechanical properties of the material, in particular its strain rates at break. 2. The urea functions are polar and should therefore allow good reactive compatibilization to be observed between the PDMSurea prepolymers and the polyamide, PA.

[0031] In a particularly preferred embodiment of the present invention, the polyamide (PA) part used in the preparation of the copolymer of the invention is a PA6 / n copolymer containing mixed 6-carbon and 11-carbon units. A polymer of this type is commercially available, supplied by ARKEMA under the trade name APOLYA, with proportions of PA6 and PAn of approximately 0.3 and 0.7 respectively (by mass) with a molar mass Mn = 2500 g.mol A terminated at one end by a primary amine function and at the other by a methyl ester function (see [Fig.2], part A).

[0032] According to one aspect, the present invention relates to a triblock copolymer having the following structure: (PA)-(NH-CO-NH)-(LDI1)-[(PDMS urea)n(PDMS urea alkyl)m ]-(LDIl)-(NH-CO-NH)-(PA) in which: PA represents a polyamide block; NH-CO-NH represents a urea bond; LDI1 represents a linking group (or “linker”) that can be derived from a part of a diisocyanate chain; the part -[(PDMS urea)n(PDMS urea alkyl)m]- represents an entity comprising n PDMS groups integrated into the copolymer by urea groups and m PDMS groups integrated into the copolymer by urea alkyl groups, n and m being integers and the PDMS urea and PDMS urea alkyl groups being present in separate blocks or mixing in the chain constituting the part -[(PDMS urea)n(PDMS urea alkyl)m]- ; the elements (PDMS urea) having repeating units represented by the formula -[(LDI2)-(NH-CO-NH)-(LSX1)-(PDMS)-(LSX1)-(NH-CO-NH)-(LDI2)]-in which: LDI2 represents a linker that can be derived from a diisocyanate chain portion; NH-CO-NH represents a urea linkage; LSX1 represents a linker between the urea group and the silicon atom at the end of the poly(dimethyl)siloxane (PDMS) chain; the elements [(PDMS urea alkyl) having repeating units represented by the formula -[(LDI2)-(NH-CO-NR)-(LSX2)-(PDMS)-(LSX2)-(NH-CO-NR)-(LDI2)]-in which: LDI2 represents a linker derivable from a diisocyanate chain portion; NH-CO-NR represents an alkyl urea linkage, R being an alkyl group of at least 2 carbon atoms, preferably ethyl; LSX2 represents a linker between the urea group and the silicon atom at the end of the poly(dimethyl)siloxane (PDMS) chain.

[0033] According to the aspect of the invention cited above, preferably the combined linker elements LDI1-LDI2, LSX1 and LSX2 each correspond to an alkyl, aromatic or alicyclic group, and preferably to a hydrocarbon structure such that at least 4 and at most 12 carbon atoms separate the two branching points by the shortest route, and preferably the linkers LDI1-LDI2, LSX1 and LSX2 correspond to a group L1 chosen from the following groups, the symbol * indicating a carbon atom forming part of the structure L1 and also a branching point: (Ll-1) [Chem. 17] (Ll-2) [Chem. 18] (Ll-4) [Chem. 20] (Ll-5) [Chem. 21] According to this aspect, the polydimethylsiloxane(s) (PDMS) present, at one or more units in the overall structure of the copolymer, have for each PDMS unit (used during the synthesis) a number-average molecular mass (Mn) of at least 500 g.mol1 and at most 150,000 g.mol ', preferably at least 800 g.mol1 and at most 50,000 g.mol *, and / or the number of units x is at least 10 and at most 900.

[0034] <Matrice élastomérique>

[0035] According to one aspect, the present invention relates to an elastomeric matrix obtained from the triblock copolymers according to the invention as described above. In particular, the elastomeric matrix can be obtained by hot physical transformation according to methods well known to those skilled in the art.

[0036] The elastomeric matrices thus obtained can be used in various devices, such as, for example, dressings. In order to produce dressings, the matrix according to the invention will preferably be formed in a thin layer.

[0037] According to a preferred embodiment of the invention, the matrix has through holes. The through holes can be made by perforation or by punching the matrix previously formed in a thin layer.

[0038] Alternatively, the dies in accordance with the invention may be manufactured by hot casting a polymer composition as described above onto a plate etched with the selected pattern to form through holes, followed by a cooling step and finally a demolding step.

[0039] The production of adhesive dressings generally meets complex specifications in order to reconcile contradictory characteristics. The main criteria to be checked for such a dressing are essentially to have good breathability while avoiding the risk of leaks, and to be impermeable to liquids and bacteria while being breathable (i.e. permeable to water vapor). Preferably, the dressing will maintain its cohesion when removed once loaded with exudates, and will preferably be easy to manufacture. The dressing must also be easy to apply and remain in place for as long as possible without damaging the peri-wound skin. Preferably, it will not impair wound healing when removed. Finally, the dressing must fit the patient's morphology.

[0040] The elastomeric matrix is ​​preferably thin, so as to better fit the shapes of the body and follow movements without risking detachment. The adhesive support is advantageously conformable. Generally speaking, the elastomeric matrices in accordance with the invention have a thickness of between 15 μm and 2 mm.

[0041] The elastomeric matrix will preferably be impermeable to external fluids and pathogenic microorganisms while ensuring permeability to water vapor, so as to avoid both contact of the wound with external liquids and bacteria and maceration of the wound.

[0042] The elastomeric matrix is ​​preferably adhesive so as to hold the dressing in place.

[0043] The matrix may contain active ingredients having a favorable role in the treatment of the wound. Among the substances capable of being used in the context of the present invention as active ingredients, the following may be mentioned, as examples: - antibacterials such as silver derivatives such as silver or other metal salts (e.g. silver sulfate, chloride or nitrate and silver sulfadiazine), silver or other metal complexes (e.g. silver zeolites such as alphasan, or ceramics), metrodinazole, neomycin, Polymyxin B, penicillins (Amoxycillin), clavulanic acid, tetracyclines, Minocycline, chlortetracycline, aminoglycosides, Amikacin, Gentamycin or probiotics; - antiseptics such as chlorhexidine, triclosan, biguanide, hexamidine, thymol, Lugol, Povidone iodine, Benzalkonium and Benzethonium Chloride; - painkillers such as Paracetamol, Codeine, Dextropropoxyphene, Tramadol, Morphine and its derivatives, Corticosteroids and derivatives; - anti-inflammatory drugs such as glucocorticoids, non-steroidal anti-inflammatory drugs, aspirin, ibuprofen, ketoprofen, flurbiprofen, diclofenac, aceclofenac, ketorolac, meloxicam, piroxicam, tenoxicam, naproxen, indomethacin, naproxcinod, nimesulide, celecoxib, etoricoxib, parecoxib, rofecoxib, valdecoxib, phenylbutazone, niflumic acid, mefenamic acid; - active ingredients that promote healing such as Retinol, Vitamin A, Vitamin E, N-acetyl-hydroxyproline, Centella Asiatica extracts, papain, essential oils of thyme, niaouli, rosemary and sage, hyaluronic acid, polysulfated oligosaccharides and their salts (in particular synthetic sulfated oligosaccharides having 1 to 4 sugar units such as the potassium salt of octasulfated sucrose or the silver salt of octasulfated sucrose), sucralfate, Allantoin, urea, metformin, enzymes (e.g. proteolytics such as streptokinase, triestin or collagenase), peptides or protease inhibitors; - anesthetics such as benzocaine, lidocaine, dibucaine, pramoxine hydrochloride, bupivacaine, mepivacaine, prilocaine, or etidocaine.

[0044] In the context of the present invention, it is possible to envisage matrices which are easy to handle, repositionable, allow painless removal when applied to the skin, mucous membranes or appendages, and have satisfactory durability over time.

[0045] <pansements>

[0046] The present invention also relates to a dressing comprising the elastomeric matrix obtained from triblock copolymers according to the invention.

[0047] According to a preferred embodiment of the invention, the present application aims to cover an absorbent dressing comprising an elastomeric matrix in the form of an adhesive border which can take the form of a "sidewalk", and allowing the dressing to be fixed to the skin surrounding the wound. These dressings, in particular when used for the treatment of particularly painful chronic wounds, are advantageously conformable and thin in order to limit the tensions that the dressing can generate on the surface of the skin. According to a preferred embodiment of the invention, the adhesive absorbent dressing comprises the assembly of an absorbent layer and the elastomeric matrix forming the sidewalk of the absorbent dressing, which is respectful of the fragile and sensitive peri-wound skin.

[0048] According to a preferred embodiment of the invention, the present application aims to cover an absorbent dressing comprising an absorbent layer coated with an elastomeric matrix in the form of a perforated coating. The through holes allow the passage of exudates towards the absorbent layer. The elastomeric matrix is ​​present over the entire surface of the dressing in contact with the skin. Advantageously, this type of dressing does not adhere to wet wounds but adheres to the peri-wound skin, thus allowing removal without trauma or pain. Among the known dressings of this type, the products marketed by the company Molnlycke under the brand Mepilex®, can be cited.

[0049] According to a preferred embodiment of the invention, the present application aims to cover a self-supporting interface dressing comprising an elastomeric matrix in the form of a thin layer having through holes for allow exudates to pass through. The thickness of such a dressing is preferably between 0.4 and 2 mm. In order to protect the matrix from the external environment, the interface dressing may be covered, preferably on each of its faces, with a temporary protective film which will be removed before use by the user. Among the known dressings of this type, the products marketed by URGO Laboratories under the UrgoTul® brand, can be mentioned.

[0050] According to a preferred embodiment of the invention, the present invention aims to cover a dressing composed of an elastomeric matrix in the form of a thin transparent adhesive film. The thickness of such a dressing is preferably between 20 and 50 μm. The transparency allows visual inspection of the area to be treated. These films are semi-permeable, they are permeable to gas exchanges, and are impermeable to liquids and bacteria. They provide mechanical protection against the phenomena of rubbing, friction and shearing. Among the known dressings of this type, the products marketed by the company Smith & Nephew under the brand Opsite®, or by the company 3M under the brand Tegaderm® or by Laboratoires URGO under the brand Optiskin®, can be cited.

[0051] According to a preferred embodiment of the invention, the present invention aims to cover a dressing composed of an elastomeric matrix in the form of a flexible gel plate having through holes. These dressings, in particular when used in the treatment of hypertrophic or keloid scars, are advantageously self-adhesive and conformable in order to adapt to each scar. Among the known dressings of this type, the products marketed by the company Smith & Nephew under the brand Cica-care®, can be cited.

[0052] In the present invention, the term “dressing” means any medical device of the dressing type comprising at least one elastomeric matrix. In particular, the invention applies to dressings used for the treatment of wounds, the treatment of scars and cosmetic patches.

[0053] <exemples>

[0054] <Réactifs>

[0055] All raw materials used are commercially available. The characteristics of all products are set out in Table 1 below.

[0056] <a) Polymères semi-cristallins>

[0057] Two semi-crystalline polymers were used, a polyamide and a polyethylene. These polymers differ in many aspects. For example, polyethylene has an inert structure while polyamide has many amide functions on its chain. Being semi-crystalline and each having melting temperatures between 100 and 130°C, they are potentially promising candidates for the preparation of thermoplastic elastomers.

[0058] Regarding the question of possible incompatibility between polymer components, polyethylene does not show strong incompatibility with PDMS, polyethylene having a lower solubility parameter than polyamide with a value ôPE = 16 MPa1 / 2.

[0059] <polyamide>

[0060] The PA6 / nest copolymer is supplied by ARKEMA under the trade name APOLYA. The proportions of PA6 and PAn were determined by analysis H NMR and are 21 wt% and 79 wt%, respectively. This low molar mass copolymer (Mn = 2500 g.mol ') is terminated at one end by a primary amine function and at the other by a methyl ester function ([Fig.2], part A). It has melting temperatures, Tf ~130°C, and crystallization temperatures, Tf ~105°C, which were measured by DSC ([Fig.2], part B).

[0061] <Polyéthylène>

[0062] The polyethylene is obtained from Activation. More precisely, these are three types of monofunctional polyethylenes with low molar masses which differ in their terminal functions. The first is an iodinated terminated polyethylene (PEO) with a molar mass defined by SEC (Mw = 1039 g.mol ') • This polyethylene is the precursor for obtaining the two other primary amine (PENH2) and secondary amine (PENH hexyl) terminated polyethylenes with molar masses, defined from the PEb substrate, of 929 and 1013 g.mol respectively *.

[0063] In DSC, these polyethylenes exhibit bimodal melting peaks as shown in [Fig. 3]. For low molar masses, the presence of bimodal peaks seems to be linked to two crystal sizes due to a fraction of non-functional polyethylene (C. Soulié-Ziakovic, Macromolecules, 2015, 48, pp. 3257-3268).

[0064] <b) PDMS>

[0065] The PDMS used were supplied by Gelest, Genesee Polymers and ABCR. The exact molar masses were systematically calculated from the 'H NMR data using trichlorobenzene as an internal standard. These products were used without further treatment.

[0066] <PDMS amines primaires pendantes>

[0067] These PDMS will be denoted PDMSgraftNH2- Their chemical formula is represented below. A polymer having a molar mass of Mn -50000 g.mol1 with 6 to 7% of aminopropylmethylsiloxane unit (trade name AMS-163 at Gelest) was used. [Chem. 22]

[0068]

[0069]

[0070]

[0071] <PDMS terminé amines primaires> These PDMS will be denoted PDMSendNH2- Their chemical formula (PDMS terminated at each end by an aminopropyl group) is represented below. A polymer with a molar mass of Mn -5000 g.mol1 was used (trade name DMS-A21 from Gelest and AB 109371 from ABCR). [Chem. 23] ÇH3 ^H3 ^H3 H2NCH2CH2CH2—O^"^~"O4'^"CH2CH2CH2NH2 ch3 \ch3 / n ch3 <PDMS terminé amines secondaires> These PDMS will be noted PDMSendNH- Their chemical formula (PDMS terminated at each end by an N-ethylaminoisobutyl group) is represented below. A polymer with a molar mass of Mn -2500 g.mol1 to 3500 g.mol1 was used (trade name DMS-A214 at Gelest). [Chem. 24]

[0072] <Techniques d’analyse et caractérisation>

[0073] <a) Résonance magnétique nucléaire (RMN)>

[0074] Due to various solubilization conditions, the NMR analysis parameters are separated according to the products concerned. • PDMS blocks: H NMR on Bruker Avance 400 spectrometer in deuterated chloroform at 25°C. • Products containing polyamide: H NMR on Bruker Avance 400 spectrometer in a mixture of deuterated chloroform and anhydrous trifluoroacetic acid at 25°C (6:1). • Products containing polyethylene: H NMR on Bruker Ascend 400 Prodigy spectrometer in deuterated chloroform at 70°C.

[0075] The spectra are processed and analyzed using the Topspin software provided by Bruker.

[0076] <b) Calorimétrie différentielle à balayage (DSC)>

[0077] Thermograms of the samples are obtained using the DSC Q100 device marketed by TA® instruments, equipped with a liquid nitrogen refrigeration system. Samples with masses between 5 and 10 mg are introduced into sealed aluminum capsules and then analyzed using the following procedure: - Equilibrium at -150°C - 1st heating up to 150°C with a ramp of 10°C / min - Isothermal 1 min at 150°C - Temperature reduction to -150°C at 10°C / min - Isothermal 1 min at -150°C - 2nd heating up to 200°C with a ramp of 10°C / min The glass transition, crystallization and melting temperatures are determined after erasing the thermal history of the materials during the first heating.

[0078] <c) Rhéologie>

[0079] Rheological measurements were carried out on the Anton Paar MCR rheometer. Measurements were made with a 8 mm diameter plane-plane geometry for solid or particularly viscous samples. For the less viscous samples, a 25 mm diameter cone-plane geometry was preferred. Two types of measurements were carried out: - A frequency sweep: measurement of the elastic modulus (G') and the loss modulus (G”) as a function of the shear rate at constant angular frequency at 25°C - A temperature scan: measurement of G' and G' ' as a function of temperature (ramp of 3.6 °C / min) at a constant shear rate and at an angular frequency of 10 rad / s. During these measurements, the sample was placed on the low geometry at 150 °C. The first analysis is carried out when cooling from 150 to 25 °C. The second analysis corresponds to heating the sample from 25 to 150 °C.

[0080] <d) Test de traction>

[0081] Tensile tests were performed on an MTS QTest 25 at room temperature. Measurements were made on dogbone-shaped samples approximately 40 mm long, 4 mm wide and 1 mm thick. Deformations were applied at a speed of 5 mm / min.

[0082] <e) Diffraction et diffusion des rayons X (DRX)>

[0083] The DRX material analyses were carried out in a partner laboratory, the CRPP, on a Xeuss 2.0 device marketed by Xenocs. This device delivers a beam with an energy of 8 keV. The data are collected on a DECTRIS PILATUS-300k detector placed at different distances from the sample, thus giving access to the angle range 0.03° to 50° (0.025 nm 1 to 34.5 nm1).

[0084] Table 1 below summarizes the commercially available semi-crystalline polymers and PDMS polymers experimentally explored by the present inventors in the preparation of polymers according to the present invention and comparative polymers.

[0085] [Tables 1] Names Denominations Trade Names (Supplier) Molar masses (g.mol1) (Supplier data) Polyamide 6-11 PA6_n APOLYA (Arkema) 2500 Mono-terminated iodine polyethylene PEj PE-I (Activation) 1039 Mono-terminated amine polyethylene PEnh2 pe-nh2 (Activation) 929 Mono-terminated N-hexyl polyethylene । |ie\y|e PE-NH-hexyl (Activation) 1013 Epoxypropoxypropyl terminated polydimethylsiloxane PDMSend epoxy 1000 DMS-E12 (Gelest) 1000-1400 PDMSend epoxy 5000 DMS-E21 (Gelest) GP504 (Genesee Polymers) 4500-5500 Epoxypropoxypropyl mono-terminated polydimethylsiloxane PDMSend mono epoxy MCR-E11 (Gelest) 5000 Copolymer (6-7% aminopropyl-methylsiloxane)-dimethylsiloxane PDMSgraft NH2 AMS-163 (Gelest) 50000 Aminopropyl terminated polydimethylsiloxane PDMSend NH2 DMS-A21 (Gelest) AB 109371 (Gelest) 5000 Polydimethylsiloxane terminated N-ethylaminoisobutyl PDMSend NH DMS-A214 (Gelest) 2500-3000

[0086] Table 1 presents a summary of the data concerning the commercial products used.

[0087] <Réacteurs>

[0088] The various reactions were carried out in glass reactors composed of a glass tube or flask and a mechanical stirrer made of glass or Teflon under nitrogen flow. A Radleys 6 Plus carousel was also used to run up to 6 reactions in parallel.

[0089] <Chimie isocyanate-amine>

[0090] <Systèmes triblocs SC-b-PDMSurée-b-SC>

[0091] The synthesis of these triblock copolymers is carried out in two stages ([Fig.l]): 1. Prepolymer synthesis: reaction between PDMSendNH2 and hexamethylene diisocyanate with excess diisocyanate to obtain isocyanate-terminated prepolymers. 2. Addition of the semi-crystalline polymer terminated by a primary amine.

[0092] <i) Prépolymère PDMSurée>

[0093] The primary objective in the synthesis of this type of prepolymer was to observe the reactivity between the isocyanate and the primary amine located at the end of a PDMS chain. Several materials with a molecular mass gradient were prepared to observe the influence of chain length on thermal and rheological properties.

[0094] <Synthèse>

[0095] To do this, three materials were synthesized in order to obtain prepolymers terminated by amines. These materials differ in the ratio r = [isocyanate] / [NH2], thus the quantities of material introduced are stated in Table 2 below. For these syntheses, a PDMSendNH2 supplied by ABCR (AB 109371) and having a molar mass of 5800 g.mol1 was used. The reactions were carried out in the carousel at room temperature under mechanical stirring.

[0096] [Tables2] Sample m hdi g Dl PDMSend NH2 g ra DPnb Mnc theoretical kg.mol1 Conversion NH2d % (NMR) 1 0.066 2.42 0.95 39 120 90 2 0.048 1.83 0.90 19 60 86 3 0.050 2.05 0.85 12.3 40 83

[0097] Table 2 presents data relating to the synthesis of PDMSurea prepolymers terminated with primary amines [Math. 1] = = UZ 4îatheorique = Mhdï x + MpDMSend NH2 X ™ = 100 x (1 -

[0098] As soon as the two precursors are brought into contact by mechanical stirring, it is possible to observe a significant increase in viscosity. Thus, due to an almost instantaneous reaction, kinetic monitoring could not be carried out. The products obtained are transparent elastic solids that can be shaped.

[0099] 'H NMR analysis allowed the measurement of the conversion rate of the amine functions. According to the results obtained by analyzing the evolution of the intensity of the peak corresponding to the alpha protons of the NH2 group, it can be concluded that there is a total reaction between the isocyanates and the primary amines (NH2 conversion -100 xr). The remaining amines in the systems correspond to the chain ends of the synthesized prepolymers.

[0100] As expected, the reactive compatibility between the two precursors allows a total conversion with reaction conditions of time and temperature perfectly compatible with a reactive extrusion process. Therefore, it is possible to imagine the synthesis of urea prepolymers with primary amine or isocyanate terminations and having various concentrations in urea function using PDMSendNH2 of various molar masses.

[0101] Urea prepolymer synthesis tests were carried out with a lower molecular weight PDMSendNH2 precursor (AB 109370 with Mn = 3200 g.mol '). This change in precursor leads to an increase in the concentration of functional groups. The high reactivity then leads to the production of solid materials in a liquid PDMS phase.

[0102] <Caractérisation>

[0103] <dsc>

[0104] The thermal phase transitions of the materials presented in Table 2 were analyzed by DSC. These materials were obtained from the same precursors introduced in varying proportions in order to obtain three distinct molar masses.

[0105] The thermal cycles are described in the experimental part. [Fig.4], part B, represents the 2nd heating cycles of the three samples. In all cases, a first inflection point is observed, around -120 °C, characteristic of the glass transition of PDMS (Tg PDMS). Only sample 3 shows an exothermic peak and an endothermic peak, between -80 and -40 °C, corresponding to the crystallization and melting of PDMS. While the prepolymers obtained by the epoxy-amine route did not show any other thermal transition than that mentioned above, the DSC analyses of the urea prepolymers systematically show an endothermic peak around 20 °C. This peak can then be attributed to a melting in a phase constituted by the stacking of the urea groups. The inflection points relating to the Tg as well as the crystallization of the urea phase are observable during cooling ([Fig.4], part A).

[0106] The values ​​of Tg (PDMS), Tf (urea) and AHf(urea) are reported in Table 3 for all samples. For clarity, the fusion enthalpies of the urea groups have been reduced to one mole of urea and expressed in kJ.mol *.

[0107] [Tables3] Sample r = [isocyanate] / [amine] T PDMS °C Tt Urea °C AHf Urea J.g1 AHf Urea kJ.mol1 1 0.95 -123.55 20.15 0.85 5.36 2 0.90 -123.29 19.64 0.82 5.44 3 0.85 -123.64 19.25 0.76 5.35 PDMS end NH2 / -123.36 / / /

[0108] Table 3 presents characteristics of the thermal phase transitions of the urea prepolymers and the PDMSendNH2 precursor measured by DSC.

[0109] The glass transition temperatures of the PDMS obtained are identical and have a value of -123.5 °C for all the synthesized prepolymers. This value is equal to that of the precursor PDMSendNH2- Thus, the introduction of urea groups by reaction of the isocyanate HDI on the PDMSendNH2 does not influence the glass transition temperature of the PDMS phase. In the same way, the Tg of the PDMS is not impacted by the chain length of the “decorated” PDMS with identical values ​​for the three synthesized materials.

[0110] Finally, the fusion enthalpies, AHf, of the urea phases were measured. Samples 1 (r = 0.95), 2 (r = 0.90) and 3 (r = 0.85) have melting temperatures of 20.15, 19.64 and 19.25 °C respectively. A slight decrease in Tf is observed with decreasing urea concentration. Consistently, the fusion enthalpy values ​​change from 0.85 to 0.76 Jg 1 between samples 1 and 3. Once reduced to enthalpy values ​​in kJ.mol *, all samples have identical values ​​of 5.4 kJ.mol *. [YES]<Propriétés rhéologiques>

[0112] Preliminarily, the linearity domain of the urea prepolymers was measured by performing a shear rate scan at constant temperature and angular frequency. Thus, all the mechanical properties presented here were obtained in plane-plane mode (8 mm diameter geometry) with a shear rate, y = 5% and an angular frequency, co = 10 rad.s '. G' and G” were analyzed during a cooling cycle from 150 to 25 °C and heating from 25 to 150 °C (1.3 °C / min).

[0113] [Fig.5] represents the storage (G') and loss (G”) moduli of sample 1. The sample was placed on the geometry at 150 °C, at this temperature the material is a viscous liquid. The mechanical properties are first measured during cooling, we can then observe a transition from a liquid state (G' < G”) to a solid state (G' > G”) at a temperature of 69 °C (G' = G”). During heating, this transition temperature is measured at 89 °C. This hysteresis between the heating cycle and the cooling cycle is consistent with the difference between the crystallization temperature and the melting temperature of the urea domains measured in DSC. A slight increase in the G' modulus is observed around 80 °C, this can reflect an incomplete conversion during the reaction or a slippage of the sample in the geometry.

[0114] The drastic drop in modulus G' observed during heating to a temperature of approximately 110 °C cannot be fully explained. It only reflects a significant drop in viscosity in this temperature range. At these modulus values, of the order of Pa, the analysis comes up against the limits of the apparatus. This phenomenon is also present during cooling with a drastic increase in G' at approximately 80 °C.

[0115] At 25 °C, sample 1 behaves like an elastic solid with modulus values ​​G' = 230 kPa and G” = 62 kPa. These values ​​are relatively low and are consistent with the macroscopic appearance (“soft” materials).

[0116] The comparison of the mechanical properties of the three urea prepolymers of variable molar mass is presented in [Fig.6]. Only the heating cycles are represented. The hysteresis phenomenon described for sample 1, between heating and cooling, was observed for all the materials studied.

[0117] The three synthesized urea prepolymers exhibit similar behavior: "soft" elastic solid at room temperature and viscous liquid at a temperature above the transition temperature (TsoWiq). However, these phase change temperatures are a function of the chain length. Sample 1 (Mn theoretic ~ 120 kg.mol ') exhibits a transition at 89 °C, sample 2 at 56 °C (Mn theoretic = 60 kg.mol ') and sample 3 at 47 °C (Mntheoretical = 40 kg.mol '). Similarly, the values ​​of G' and G” vary according to the molar mass. All the data obtained are summarized in Table 4.

[0118] [Tables4] Theoretical sample kg.mol1 Tsol / liq cooling °C TsOl / |iq heating °C G' T = 35 °C kPa G” T = 35 °C kPa 1 120 69 89 160 38 2 60 42 56 69 35 3 40 37 47 21 13

[0119] Table 4 presents a summary of the rheological properties of urea prepolymers.

[0120] Increasing the molar mass of the synthesized urea prepolymers, from 40 to 120 kg.mol, has two effects on the rheological properties. The first is an increase in the storage (21 to 160 kPa at 35 °C) and loss (13 to 38 kPa at 35 °C) moduli. The second is an increase in the solid / liquid transition temperature (47 to 89 °C during heating). The increase in chain length results in an increase in entanglement and in the urea group concentration as seen in thermal analysis (DSC). Thus, the length of the prepolymer can strongly influence the intra- and inter-chain interactions and therefore the mechanical properties.

[0121] <conclusion>

[0122] These first attempts at synthesizing urea prepolymers are of great interest due to their synthesis conditions (short time and room temperature) and their mechanical strength. The materials obtained are flexible and reprocessable. However, the sol / liq transition temperatures are relatively close to room temperature. Thus, the addition of a crystalline polymer to these urea “decorated” PDMS systems appears to be an appropriate solution for obtaining thermally stable, reprocessable flexible materials.

[0123] <ii) Triblocs PE-b-PDMSurée-b-PE (Exemples Comparatifs PE)>

[0124] The production of PE-b-PDMSurea-b-PE (PE = polyethylene) triblock systems is made possible by the presence of functional groups at each end of the PDMSurea prepolymer.

[0125] <Synthèse>

[0126] In order to facilitate the comparison between the PE-b-PDMSurea-b-PE and PA-b-PDMSurea-b-PA systems, the prepolymer used is identical and has the characteristics set out in Table 5 below. The molar mass of the PDMSendNH2 used is 5827 g.molA

[0127] [Tables5] Urea prepolymer (PDMSurea) Termination Isocyanate r = [amine] / [isocyanate] 0.95 Mn theoretical [kg.mola] 120

[0128] Table 5 presents characteristics of the PDMSurea prepolymer used for the synthesis of SC-b-PDMSurea-b-SC triblocks

[0129] The addition of a semi-crystalline polymer to the prepolymer is described in the 2nd step of the synthesis scheme of [Fig.l]. The prepolymer being terminated at each end by an isocyanate function, it can therefore react directly with a polyethylene mono-functionalized by a primary amine. The quantity of polyethylene to be reacted with the prepolymer is calculated by considering a conversion of 100% of the primary amines during the synthesis of the isocyanate-terminated prepolymer. The polyethylene is then added in a ratio [1:1] with the isocyanate functions present at each end of the PDMSurea prepolymer according to the following equation (1): [Math. 2] = 2 x (1)

[0130] Experimentally, the prepolymer is preheated in a flask to 150°C to be in a molten state. Polyethylene, which has a melting temperature of approximately 100°C, is then added to the reaction medium. The quantities of material introduced for the synthesis of the PE-b-PDMSurea-b-PE system are shown in Table 6:

[0131] [Tableauxô] Sample PDMSurea PENH2 mass g theoretical kg.mol1 mass g Mn % by weight PE-b-PDMSurea-b-PE 2.288 120 0.032 929 1.4

[0132] Table 6 presents experimental data of the synthesis of the PE-b-PDMSurea-b-PE system

[0133] As with the synthesis of the urea prepolymer, the kinetics of this reaction could not be studied. Thus, the reaction time was determined from visual observations. First, the polyethylene melts in the PDMS phase. A two-phase system is then initially observed with a transparent, low-viscosity phase on the edges of the balloon (PDMSurea) and a more viscous, opaque phase around the mechanical stirring blade. Within a few minutes, the system homogenizes with a single opaque and more viscous phase. The material obtained after one hour at 150 °C (overestimation of the reaction time) is a slightly translucent white "soft" elastic solid. This can be shaped and reshaped by placing it in a silicone mold in an oven at 150 °C.

[0134] Confirmation of the creation of a covalent bond between the prepolymer and the polyethylene could not be carried out due to the superposition of peaks during the NMR analysis. Similarly, the difference in molar masses between the prepolymer and the triblocks was not observed in size exclusion chromatography due to a small mass difference of the order of a percent. Nevertheless, visual observations during the synthesis as well as dispersion tests of non-functionalized polyethylene in the urea prepolymer seem to indicate the obtaining of the PE-b-PDMS^-b-PE triblock system.

[0135] For this reaction, it is necessary to note the low mass proportion of polyethylene. With the available precursors, the increase in this mass fraction can only be done by reducing the molar mass of the prepolymer (increase in the number of chain ends for a given mass).

[0136] <Caractérisation>

[0137] <dsc>

[0138] The phase transitions of the PE-b-PDMSurea-b-PE system were analyzed by DSC. For clarity, the obtained thermogram is compared with those of the urea prepolymer and PENH2 in [Fig.7].

[0139] The Tg values ​​of PDMS can be identified during the heating cycle in [Fig.7], part B. These glass transition temperatures are thus not influenced by the addition of polyethylene with values ​​of -123.4 °C for the urea prepolymer and -123.3 °C for the triblocks. On the contrary, the melting temperatures of the urea and polyethylene domains are modified. Indeed, when PE is added, Tf (urea) decreases and goes from 20 to 14 °C and Tf (PE) increases from 97 to 114 °C. The enthalpy of fusion of polyethylene, AHfPE = 1.03 J / g1, allows access to the crystallinity rate of the polyethylene phase, / PE = 36%. This value is much lower than that of PENH2 alone, which is 80%. All these results seem to indicate the presence of a phase where urea and polyethylene groups coexist. X-ray diffraction analysis is a technique that can confirm this conclusion.

[0140] <Propriétés rhéologiques>

[0141] To facilitate comparison between the different systems, the conditions for measuring the moduli G' and G” of the triblock systems with urea prepolymers are identical to the conditions set for the urea prepolymers. That is, a shear rate, y = 5% and an angular frequency, co = 10 rad.s 1 with a cooling ramp and heating of 1.3°C.min '.

[0142] [Fig.8] shows the storage (G') and loss (G”) moduli during a heating cycle of the PE-b-PDMSurea-b-PE triblock system before (urea prepolymer) and after addition of polyethylene.

[0143] With the addition of polyethylene at each end of the prepolymer, the sol / liq transition temperature increases from 53 to 58 °C. Similarly, the G' modulus increases from 73 to 90 kPa. Thus, the mechanical and thermal properties of the material are only slightly improved by the presence of the semi-crystalline polyethylene polymer. This result is explained by the low mass proportion of PE in the system (1.4%) and by the melting temperature of PE close to 100 °C.

[0144] <conclusion>

[0145] The synthesis of PE-b-PDMSurea-b-PE triblocks is of interest due to the problem of having synthesis conditions suitable for industrial processes. The materials obtained are flexible and reprocessable. However, the low thermal stability of the system is a barrier to its use.

[0146] <iii) Triblocs PA-b-PDMSurée-b-PA>

[0147] The polyamide 6 / 11 used here has a molar mass of 2500 g.mol1 while polyethylene has a molar mass of less than 1000 g.mol '. Thus, for the use of the same prepolymer, the mass fraction of semi-crystalline polymer is multiplied by approximately 2.5 in the case of the polyamide supplied by Arkema. In addition, the melting temperature of this polyamide is much higher than that of polyethylene with a Tf = 130 °C.

[0148] <Synthèse>

[0149] For the synthesis of the PA-b-PDMSurea-b-PA triblock system, the urea prepolymer used is identical to that used during the synthesis of PE-b-PDMSurea-b-PE. Its characteristics are listed in Table 7. The addition of the polyamide to PDMSurea is carried out in the same way as for polyethylene and corresponds to the second step shown in [Fig.l]. The prepolymer is heated to 150 °C with mechanical stirring, the polyamide is then added through the neck of the flask and the reaction is continued until a homogeneous mass is obtained. The material obtained is an opaque elastic solid with a non-adherent surface; it can be shaped into a bar or film in an oven at 150 °C.

[0150] As a reminder, the quantity of polyamide to be reacted with the prepolymer is calculated by considering a 100% conversion of the primary amines during the synthesis of the isocyanate-terminated prepolymer. The quantities of material used in this synthesis are given in Table 7. The mass proportion of semi-crystalline polymer is here 4.1%.

[0151] [Tables?] Sample PDMSurea PAnh2 theoretical mass g kg.mol1 mass g Mn % by weight PA-b-PDMSurea-b-PA 2.312 120 0.098 2500 4.1

[0152] Table 7 presents experimental data of the synthesis of the PA-b-PDMS^-b-PA system

[0153] As previously for the systems containing urea groups, the reaction kinetics could not be studied due to the superposition of the urea and isocyanate peaks with those of the polyamide in NMR analysis. The reaction was monitored using visual observation such as the transition from a two-phase system with a dense and opaque phase around the stirring blade and a transparent phase to a homogeneous system. The creation of a covalent bond between the prepolymer and the polyamide could be observed during a DOS Y experiment. This experiment showed a difference in diffusion index between the prepolymer and the PA-b-PDMSurea-b-PA triblocks.

[0154] <Caractérisation>

[0155] <dsc>

[0156] The phase transitions of the PA-b-PDMSurea-b-PA system were analyzed by DSC. For clarity, the obtained thermogram is compared with those of the urea prepolymer and PA^n in [Fig.9].

[0157] As shown by the thermograms in [Fig.9], part B, obtained during the second heating cycle, the glass transition temperature is unchanged upon addition of the polyamide, with values ​​of -123.4 °C for the prepolymer and -123.9 °C for the PA-b-PDMSurea-b-PA triblocks. Unlike the prepolymer and the system containing polyethylene, the system with polyamide no longer exhibits an endothermic peak around 15-20 °C (urea domains). This can be explained by a greater interaction between the amide groups of the polyamide and the ureas contained in the PDMS chain.

[0158] Finally, thermal analysis by DSC makes it possible to observe the presence of an endothermic peak corresponding to the melting of the crystalline phase of the polyamide. This temperature is 130 °C for the polyamide alone and 131 °C for the triblock system. The enthalpy of fusion of the polyamide, AHfPA = 1.23 J / g1, allows access to the crystallinity rate of the polyethylene phase, / PA = 10.5%. This value is lower than that of PAnh2 alone, which is 19%. Again, these results seem to indicate the presence of a phase where the urea groups and the polyamide coexist.

[0159] <Propriétés rhéologiques>

[0160] The conservation (G') and loss (G”) modules of the system PA-b-PDMSurea-b-PA, over a temperature range of 25 to 150 °C, are shown in [Fig.10], part B and compared with those of the urea prepolymer ([Fig.10], part A).

[0161] The rheological analysis firstly allows the observation of a significant increase in the sol / liq transition temperature between the prepolymer and the triblock system with respective values ​​of 53 and 82 °C. The G' modulus also increases significantly with the addition of the polyamide, going from 70 kPa for the urea prepolymer to a value of 330 kPa. This increase was expected with the addition of a higher mass proportion than with the addition of polyethylene (4.1% and 1.4%). These semi-crystalline polymers creating "hard" nodules within the final material naturally increase the elastic moduli. Finally, the PA-b-PDMS„rpP-b-PA triblock material exhibits good thermal resistance with a slight decrease in mechanical properties up to a temperature close to 80 °C.

[0162] <conclusion>

[0163] Compared to the use of polyethylene with respect to the prepolymer, the impact of polyamide is very promising. Indeed, its use combined with a PDMS “decorated” with urea functions allows the production of reprocessable elastic solid materials with properties better corresponding to those sought in the context of the present invention. Indeed, these materials are at the same time flexible, elastic and meltable at a relatively high temperature.

[0164] <iv) Montée en échelle du système Triblocs PA-b-PDMSurée-b-PA>

[0165] Until now, the synthesis of the materials has been carried out from a quantity of precursors of the order of 2 to 5 grams. The aim here is to verify the potential for scaling up the synthesis of the PA-b-PDMSurea-b-PA system. To do this, the synthesis was carried out from 50 g of PDMSendNH2-

[0166] <Synthèse>

[0167] As seen previously, the synthesis of this type of triblock is carried out in two stages. First, a prepolymer containing urea groups is synthesized. This is terminated at each end by an isocyanate function in order to be able to react in the second stage with the mono-functionalized polyamide with a primary amine.

[0168] <lère étape : synthèse du prépolymère PDMSurée>

[0169] The synthesis of the prepolymer is carried out from hexamethylene diisocyanate (HDI) and a PDMS terminated at each end by a primary amine function. This PDMSendNH2 is not identical to that used in the synthesis of the systems presented in sub-parts i, ii and iii. This is a new batch ordered from ABCR (AB 109371) which has a molar mass of 47200 g.mol1 (analyzed by NMR). The difference in molar mass with the previous batch leads to a change in the concentration of urea group, here, it is an increase with the decrease in molar mass (5800 to 4700 g.mol '). This difference explains the gap between the properties of the PA-b-PDMSurea-b-PA system presented in subsection iii and those presented below.

[0170] For the synthesis of the PDMSurea prepolymer ([Fig. 11]), the ratio [NH2] / [NCO] is 0.95. Thus, the theoretical molar mass of the prepolymer is 93,000 g.mol *.

[0171] Experimentally, 50 g of PDMSendNH2 were placed in a 100 mL three-necked flask under nitrogen flow at room temperature. The addition of the diisocyanate is done directly into the PDMS using a syringe under vigorous mechanical stirring. During certain scale-up tests, non-homogeneous products with viscosity gradients were observed. Considering that this is probably due to the significant reactivity between primary amines and isocyanates, a small volume of THF was added to the diisocyanate, in order to reduce this reactivity, this volume not representing more than 5% by mass of precursors. Thus, a gradual addition of the THF / HDI solution (-50 / 50 by volume) allows a “controlled” reaction. The solidification is of the order of a minute and mechanical stirring is then no longer efficient. The medium is then placed at a temperature of 150°C to melt, lower the viscosity of the product and ensure maximum conversion..

[0172] The conversion of primary amines into urea is finally monitored by 'H NMR. This analysis allows the elimination of the THF introduced earlier to be observed.

[0173] <2nd step: Addition of the polyamide>

[0174] Since the reaction mixture was already placed at a temperature above the Tm of the polyamide used (Tm = 130 °C), the addition of the PA could be done directly with stirring. The medium became opaque and whitened in a few minutes. The product could then be shaped to obtain films of approximately 0.5 and 1 mm thickness. This shaping was carried out in a silicone mold by allowing the product to flow at a temperature of 150 °C.

[0175] <conclusion>

[0176] When switching from a synthesis of 2 to 50 g of the copolymer PA-b-PDMSurea-b-PA, the high reactivity of the system causes a sudden solidification which was controlled with the use of a small amount of solvent (less than 5% by weight). However, this solvent disappears very quickly (confirmation by NMR). The reaction times, of the order of one minute to ten minutes, are short. A protocol for monitoring the 2nd stage of the reaction will have to be developed to obtain a more precise reaction time. This experiment confirms that scaling up is easy and could be considered in particular in reactive extrusion.

[0177] <Caractérisation>

[0178] The mechanical properties of the material were studied by rheology and tensile testing, the thermal properties by DSC.

[0179] <dsc>

[0180] The measurements presented were carried out between -75 and 150°C. The thermograms presented correspond to the second heating of the material.

[0181] The DSC analysis of the isocyanate-terminated PDMS prepolymer is shown in [Fig. 13]. The characteristic melting temperature of the urea groups of the prepolymer, around 25 °C, can be observed.

[0182] After the 2nd synthesis step, the addition of the polyamide, the melting temperature of the PA can be observed at 130°C ([Fig. 14]).

[0183] <Propriétés rhéologiques>

[0184] For rheology analyses, the material is placed at room temperature and directly melted at 150 °C to adapt to the 8 mm plane-plane geometry. After analysis of the moduli during cooling, the storage and loss moduli are measured during heating from 25 to 150 °C with a ramp of 1.3 °C.min 1 (y = 5% and co = 10 rad.s ') and presented in [Fig.15].

[0185] The sol / liq phase transition temperature is measured at approximately 116 °C. At 25 °C, the storage modulus has a value of 412 kPa. These two results are, as expected, higher than those obtained during syntheses with a PDMS endnh2 precursor of greater molar mass. Indeed, the increase in the concentration of urea group leads to an increase in inter- and intra-molecular hydrogen interactions and therefore an increase in the moduli and thermal stability.

[0186] The absence of an increase in modulus at high temperature suggests a complete reaction during balloon synthesis. This result is also in agreement with the macroscopic appearance of the material, which does not have a "sticky" appearance.

[0187] <Test de traction>

[0188] The measurements of the modulus of elasticity (E') and the elongation at break could be carried out by tensile test. To do this, a constant speed deformation was applied to 6 samples cut with a die in the shape of a "dogbone". The results obtained are reproducible and only the measurement with the greatest elongation at break is shown in [Fig. 16].

[0189] The tensile analysis of the PA-b-PDMSurea-b-PA system shows a typical behavior of a low-strain elastic solid. It is therefore possible to determine a value of the modulus of elasticity, E' = 108 kPa, from the linear domain. The material has an elongation at break of 44%.

[0190] <v) Systèmes triblocs PA-b-PDMSurée éth.-b-PA>

[0191] PA-b-PDMSurea-b-PA systems show strong potential, but nevertheless it is still possible to try to improve the mechanical properties of the designed systems by playing on the nature of the bonds created between the PDMS and the spacer. Replacing the PDMSendNH2 with a PDMSendNH thus makes it possible to obtain ethylated urea groups and to reduce inter and intramolecular interactions by crowding the group.

[0192] <Synthèse>

[0193] In the following, polyamide 6-11 is used as a semi-crystalline polymer. The reaction scheme of the two-step synthesis of PA-b-PDMSureeth-b-PA is shown in [Fig. 17].

[0194] The PDMSendNH used here is supplied by Gelest (DMS-A214) and has a molar mass of 1900 g.mol *.

[0195] The experimental conditions for the synthesis of this type of triblocks are identical to those presented during the synthesis of the systems PA-b-PDMSurea-b-PA. The total quantities of material used are listed in Table 8.

[0196] [Tables8] Sample r = (nNH / n NCo) m hdi g •H PDMSend NHg m pa6-ii g wt% PA 6-11 PA-b-PDMSurea eth.-b-PA 0.95 0.3371 3.5924 0.5737 12.7

[0197] Table 8 presents experimental data of the synthesis of the PA-b-PDMSurea eth.-b-PA system

[0198] The first stage of synthesis consists of synthesizing an ethylated urea prepolymer terminated at each end by an isocyanate function. 'H NMR analysis makes it possible to observe the total conversion of the primary amines and to control the presence of isocyanates at the end of the chains. When the product obtained has solidified and is homogeneous, the reaction is considered complete and the product is then heated to 150 °C to be able to introduce the polyamide.

[0199] The polyamide is added directly to the reaction medium with stirring. The medium quickly becomes opaque and whitens. The white material obtained exhibits mechanical behavior at the boundary between liquid and solid and particularly strong adhesion to glass or metal. It is important to note the high mass fraction of polyamide of 12.7% by weight. This difference is linked to the low molar mass of the precursor PDMSendNH-

[0200] <Caractérisation>

[0201] <dsc>

[0202] The thermal analysis by DSC of the material PA-b-PDMSureeth-b-PA is shown in [Fig. 18]. In this figure is shown the cooling cycle followed by the second heating cycle.

[0203] In this thermogram, the glass transition temperature of PDMS can be observed at a temperature of -120 °C. This temperature is close to the reference value of the PDMS used in this study (-123.5 °C). An analysis of the PDMSendNH precursor will allow conclusions to be drawn regarding the difference in Tg values.

[0204] The endothermic melting peak and the exothermic crystallization peak of the polyamide are indeed present at temperatures of 129 (TfPA) and 108°C (TcPA). These values ​​are consistent with the expected and already observed values. From the melting enthalpy value, AHfPA = 3.71 Jg ', it is possible to access the crystallinity rate of the polyamide phase, / PA = 12.2%. This rate is higher than that obtained on the PA-b-PDMSurea-b-PA systems ( / PA = 10.5%) and therefore closer to the crystallinity of PA alone ( / PA = 19.0%). This result indicates a more marked phase separation with the use of ethylated urea group.

[0205] Unlike systems containing urea groups, no melting peak is observed around 15-20 °C. Nevertheless, the presence of a low inflection point between 0 and 50 °C may provide information on a state transition of the ethylated urea phase.

[0206] <Propriétés rhéologiques>

[0207] The storage (G') and loss (G”) moduli, during the second heating cycle, of the PA-b-PDMSurea eth.-b-PA system, over a temperature range from 25 to 150 °C, are shown in [Fig.19].

[0208] At a temperature of 25 °C, the storage and loss moduli have respective values ​​of 84 and 77 kPa. These two values ​​are particularly close and explain the behavior observed at the end of the synthesis. Although G' is greater than G”, the material does not show the behavior of a classic solid. At low stress frequency, the material appears close to a viscous liquid (partial flow in the pillbox), whereas at high stress frequency, the material behaves like a solid.

[0209] The sol / liq transition temperature here is 107°C but does not in any way reflect a change of state with a very small delta between G' and G' over the entire temperature range studied.

[0210] <conclusion>

[0211] The introduction of ethylated urea type bonds has made it possible to obtain materials with strong adhesion properties. In addition, these bonds can reduce the interactions between the “decorated” PDMS chains compared to urea bonds.

[0212] <vi) Systèmes triblocs PA-b-PDMSurée / uréeéth.-b-PA>

[0213] According to the results obtained on the PA-b-PDMSurea-b-PA and PA-b-PDMSurea eth.-b-PA systems and due to similar reaction conditions, it is quite possible to imagine synthesizing materials with intermediate properties with a mixture of urea and ethyl urea groups. In these materials, cohesion can be ensured by the urea bonds and adhesion properties by the ethyl urea bonds.

[0214] <Synthèse>

[0215] For this part on PA-b-PDMSurea / urea eth.-b-PA triblock copolymers, four materials were synthesized with varying ratios in urea / ethyl urea function. The precursors used for these syntheses are a PDMSendNH2 with a molar mass of 4728 g.mol *, a PDMSendNH with a molar mass of 1887 g.mol1 and hexamethylene diisocyanate (HDI). The reaction scheme for this type of reaction allowing the production of PA-b-PDMSurea / urea eth.-b-PA systems is presented in [Fig.20]. The experimental parameters concerning these syntheses are stated in Table 9. Sample 1 (100% by weight urea) corresponds to the sample presented in the scale-up part of the PA-b-PDMSurea-b-PA system. For all syntheses, the ratio I* (iLmines / HiSOCyanates) 0.95.

[0216] [Tables9] Sample m hdi gm PDMSend NHg m PDMSend NH2g % by weight3 PDMSend NH % by weightb PDMSend NH2 -Mn theoretical kg.mol1 % by weight PA6-n 1 1.885 0 50.351 0 100 93 5.8 2 0.155 0.747 2.259 25 75 80 7.7 3 0.180 1.203 1.801 40 60 72 8.5 4 0.219 1.698 1.670 50 50 66 9.3

[0217] Table 9 presents data relating to the synthesis of PA-b-PDMSurea / urea eth.-b-PA system "% by weight PDMSNH nipDMS NH , b% by weight PDMS Nh2 nipDMS NH2 = nipDMS NH2 + nipDMS NH = nipDMS NH2 + OlpDMS NH

[0219] The two synthesis steps proceed in a similar manner to those presented so far in the section on isocyanate-amine chemistry.

[0220] Once formed into a film by flow in an oven at 150 °C, the materials show strong macroscopic differences ([Fig.23]). While samples 1 and 2 are white in color, sample 3 is slightly translucent. Sample 4 is relatively close to transparency. These observations provide information on the dimensions of the polyamide nodules within the material.

[0221] The second difference concerns the adhesion properties of the materials. Adhesion is greatly increased with the increase in the fraction of ethyl urea group.

[0222] <Caractérisation>

[0223] <dsc>

[0224] [TableauxlO] Sample % theoretical urea kg.mol1 T PDMS °C Tt PA(,.h °C AHf PA(,.h J.g1 % by weight PA6.n % 1 100 93 -123.4 127.9 1.91 5.8 14 2 75 80 -122.98 128.9 2.01 7.7 11 3 60 72 -122.65 129.1 2.69 8.5 13 4 50 66 -122.3 127.6 3.10 9.3 14

[0225] Table 10 presents characteristics of the thermal phase transitions of the PA-b-PDMSurea / Urea eth.-b-PA systems measured by DSC.

[0226] The glass transition temperatures of PDMS measured for the 4 materials are very close with values ​​ranging from -123.4 °C for the sample with 100% urea group and -122.3 °C for 50% urea. Generally, a slight increase is observed with the increase in the ethylated urea fraction. The analysis of the PDMSendNH precursor will allow to conclude on the difference in Tg values.

[0227] The melting temperatures of polyamide are very close and contained between 127.6 and 129.1 °C. These values ​​depending on the analysis of the thermograms will be considered as identical. Finally, the melting enthalpy values ​​of the crystalline phase of the polyamide allow the calculation of the crystallinity rate. These rates are between 11 and 14% but it is impossible to conclude on the differences without analyzing the dimensions and the separation of the phases by a technique such as DRX.

[0228] <Propriétés rhéologiques>

[0229] The storage (G') and loss (G”) moduli of the 4 materials as well as their 4 associated prepolymers were obtained by rheological analyses.

[0230] First of all, the behavior of the prepolymers should be noted. Surprisingly, the prepolymers corresponding to materials 1 and 4 appear as solids (G' > G”) at room temperature, while prepolymers 2 and 3 are liquids (G' < G”). The G' values ​​for all the prepolymers are shown in [Fig. 21] and summarized in Table 11.

[0231] After addition of the polyamide, these four elastic solid materials exhibit a decrease in the storage moduli with increasing fraction of ethylated urea group ([Fig.22], part A). Indeed, G' goes from 410 kPa for 100% urea to a value of 74 kPa for 50% urea. This is explained by the reduction of inter- and intramolecular hydrogen interactions.

[0232] For the same reason, a decrease in the sol / liq transition temperature is observed, from 117 to 83 °C, with the decrease in the urea fraction ([Fig.22]).

[0233] [Tableauxll] Sample % urea Prepolymer PDMS urea / urea eth. PA-b-PDMSurea / urea eth.-b-PA G' 25°C kPa G” 25°C kPa G' 25°C kPa G” 25°C kPa TA sol / liq °C 1 100 73 40 410 94 117 2 75 0.2 2 321 75 115 3 60 2 6.5 283 92 135 4 50 23 24 74 47 83

[0234] Table 11 provides a summary of the rheological properties of PDMSurea / urea eth. prepolymers and PA-b-PDMSurea / Urea eth.-b-PA systems.

[0235] <Test de traction>

[0236] The measurements of the modulus of elasticity (E') and the elongation at break of the 4 materials were obtained by tensile testing. For each material, 6 dogbone-shaped specimens were analyzed. The stress-deformation curves were obtained during deformation at a constant speed (5 mm / min). The results obtained are reproducible and presented in [Fig.23].

[0237] The tensile analysis of the PA-b-PDMSurea / ureaeth--b-PA systems shows a typical behavior of an elastic solid at low deformation. It is therefore possible to determine the values ​​of the modulus of elasticity from the linear domains. In [Fig.23], part C, a linear relationship can be observed between the modulus of elasticity and the rate of urea groups. By going from 100% urea to 50%, the modulus E' changes from a value of 108 to 7 kPa. The introduction of 50% ethylated urea makes it possible to reduce the modulus of elasticity by a factor greater than 10. Similarly, [Fig.23], part B, shows the relationship between Xmax and the urea rate. Thus, the maximum elongation at break increases from 44 to 95% between 100 and 50% urea (factor 2). These two results are consistent with the modification of hydrogen interactions induced by the presence of hindered urea groups. The summary of the results is shown in Table 12.

[0238] [Tablesl2] Sample % urea E' kPa X max % 1 100 108 44 2 75 80 53 3 60 30 62 4 50 7 95

[0239] Table 12 provides a summary of the mechanical properties of the PA-b-PDMSurea / uæe eth.-b-PA systems.

[0240] <conclusion>

[0241] The synthesis of PA-b-PDMSurea / ureaeth--b-PA systems did not show any difference with the synthesis of PA-b-PDMSurea-b-PA systems. The reaction times remain in the order of one minute to ten minutes at temperature and pressure conditions compatible with industrial processes.

[0242] The partial replacement of the PDMSendNH2 precursor by a PDMSendNH precursor allows the production of flexible and reprocessable materials with a wide range of properties. Indeed, the introduction of this new precursor leads to the creation of hindered urea groups within the final material. Thus, the reduction of intra and intermolecular interactions allows a reduction of the storage moduli E' and G' in parallel with an increase in the elongation at break.

[0243] Finally, these materials have interesting adhesion properties, the presence of ethyl urea group leading to an increase in these properties.< / conclusion> < / dsc> < / conclusion> < / dsc> < / dsc> < / conclusion> < / conclusion> < / dsc> < / conclusion> < / dsc> < / conclusion> < / dsc> < / polyamide> < / exemples> < / pansements>

Claims

Claims

1. A method for synthesizing a triblock copolymer comprising the following steps: (1) reaction between (A) a polydimethylsiloxane (PDMS) comprising at least two amine end groups, either primary amine (-NH2) and / or secondary amine (-NH(alkyl)) groups, and (B) a molar excess, relative to all the molecules of type (A), of a molecule comprising at least two isocyanate groups (-N=C=O), in order to obtain a prepolymer terminated by isocyanate groups; (2) reaction between the prepolymer obtained in step (1) and a polyamide comprising an amine end group (-NH2), the number of moles of polyamide comprising an amine end group (-NH2) being at least equivalent to the number of moles of isocyanate groups (-N=C=O) in the prepolymer obtained in step (1).

2. A process for synthesizing a triblock copolymer according to claim 1, step (2) being carried out at a minimum temperature Tf of at least 100°C, preferably at least 130°C.

3. Process for the synthesis of a triblock copolymer according to claim 1 or 2 in which: - in step (1), a reaction is carried out, preferably at a temperature of at least 25 °C and at most 50 °C, between at least one polydimethylsiloxane of formula (A) [Chem. 1] h3c ch3 h3c ch3 h3c ch3 HUWWH .N R2^ ^oT ^R2 'x (A) and at least one diisocyanate of formula (B): [Chem. 2] O=C = NN=C=O (B) with a molar ratio (B) / (A) > 1, to obtain a prepolymer terminated by isocyanate groups of formula (C): [Chem. 3] O 0 0 O J n (C) in which - x represents an integer greater than or equal to 10; - n represents an integer greater than or equal to 1; - R1 and R2 represent saturated, linear or branched hydrocarbon groups; and - Li represents a saturated, linear or branched, cyclic or acyclic hydrocarbon group, or an unsaturated, linear or branched hydrocarbon group, comprising at least one double bond and / or at least one aromatic ring; and in step (2), a reaction is carried out between the prepolymer (C) obtained in step (1) and a semi-crystalline polyamide with a melting temperature Tf and comprising an amine terminal group (-NH2), of formula (D): [Chem. 4] (D) with a molar ratio (D) / (C) of more than 0 and less than 4, preferably (D) / (C) being approximately or equal to 2, at a reaction temperature T > Tf, to obtain the triblock copolymer of formula (E): [Chem. 5] (E) in which - y and z represent numbers between 0 and 100; - Tf represents a temperature greater than or equal to 100°C.

4. A synthesis method according to any one of claims 1 to 3 wherein a polydimethylsiloxane (PDMS) used in step (1) comprises at least two primary amine end groups (-NH2), and preferably comprises -(CH2)3NH2 and / or -(CH2 )—(CH)CH3-(CH2)NH2 end groups, and / or RI may be selected from the following groups, the symbol * indicating a branch point: (Rl-1) [Chem. 6] * — CH2-CH2-CH2 — * (Rl-2) [Chem. 7] CH 'O 1 * — CH2 —CH —CH2—*

5. A synthesis process according to any one of claims 1 to 3 wherein a polydimethylsiloxane (PDMS) used in step (1) comprises at least two secondary amine end groups, preferably -NH(ethyl) or -NH(methyl) groups and / or R2 may be selected from the following groups, the symbol * indicating a branch point: (R2-1 [Chem. 8]) * —H (R2-2) [Chem. 9] * —CH3 (R2-3) [Chem. 10] *—ch2—ch3

6. A synthesis method according to any one of claims 1 to 3, wherein the polydimethylsiloxane (PDMS) used, comprising at least two amine end groups, has a number-average molecular weight (Mn) of at least 500 g.mol1 and at most 150,000 g.mol *, preferably at least 800 g.mol1 and at most 50,000 g.mol *, and / or the number of units x is at least 10 and at most 900.

7. A synthesis process according to any one of claims 1 to 6, wherein the molecule comprising at least two isocyanate groups (-N=C=O) is chosen from alkyl diisocyanates, aromatic diisocyanates or alicyclic diisocyanates.

8. A preparation process according to any one of claims 3 to 7, wherein L1 is a hydrocarbon structure such that at least 4 and at most 12 carbon atoms separate the two branch points by

9.

10.

11. the shortest route, and preferably L1 is chosen from the following groups, the symbol * indicating a carbon atom forming part of the L1 structure and also being a branch point: (Ll-1) [Chem. 11] (Ll-2) [Chem. 12] (Ll-3) [Chem. 13] (Ll-4) [Chem. 14] (Ll-5) [Chem. 15] Synthesis method according to claim 7, wherein the molecule comprising at least two isocyanate groups (-N=C=O) is an alkyl diisocyanate whose isocyanate groups are in the terminal position, and preferably hexamethylene diisocyanate. Synthesis method according to any one of claims 1 to 9, wherein, in step (1), the quantity used of the molecule comprising at least two isocyanate groups (-N=C=O) corresponds to a value (n+1) in number of moles, n being the number of moles of polydimethylsiloxane (PDMS) comprising at least two amine terminal groups (-NH2). Synthesis process according to claim 1 or 2, in which the polyamide comprising an amine terminal group (-NH2) used in step (2) is chosen from: a copolymer polyamide containing units of 6 and 11 carbon atoms, preferably a copolymer between 6-aminohexanoic acid and 11-aminoundecanoic acid and / or between caprolactam and 11-aminoundecanoic acid.

12. Triblock copolymer obtained according to the process of any one of claims 1 to 11.

13. Triblock copolymer having the following structure: [Chem. 16] PA HtL ÎJ r ? Il U , S ï h pdms ]—mr' [] in which: - each group (LDI1-LDI2) corresponds to an alkyl, aromatic or alicyclic group, and preferably to a group as defined in claim 8; - each group R1 corresponds to H, Me or Et; - the polydimethylsiloxane (PDMS) is connected to -NR1- groups by reaction of a terminal -(CH2)3NH2 and / or -(CH2)—(CH)CH3-(CH2)NH2 bond of a starting PDMS; - PA denotes a polyamide.

14. Use of a triblock copolymer according to one of claims 12 or 13 in adhesive products intended to be applied to the skin, wounds, appendages and / or mucous membranes.

15. Dressing comprising an elastomeric matrix obtained from the triblock copolymer according to one of claims 12 or 13.

16. A dressing according to claim 15, wherein the elastomeric matrix has through holes.

17. A dressing according to claim 15 or 16, wherein the elastomeric matrix further contains one or more active ingredients for treating a wound, the active ingredients being selected from the group consisting of: antibacterials, antiseptics, painkillers, anti-inflammatories, healing-promoting active ingredients, and anesthetics.

18. A dressing according to any one of claims 15 to 17, wherein the elastomeric matrix obtained from the triblock copolymer is present in the form of an adhesive border allowing the dressing to be fixed to the skin surrounding a wound to be treated.

19. A dressing according to any one of claims 15 to 18, wherein the elastomeric matrix obtained from the triblock copolymer is present in the form of a film having a thickness of at least 20 pm and at most 50 pm.

Citation Information

Patent Citations

  • Aliphatic linear chain polyamide and polysiloxane segmented copolymer and preparation method thereof

    CN109384930A

  • Ceramic sol nanohybrid materials using polydimethylsiloxane-polyamideimide copolymers and manufacturing method thereof

    KR1020160146250A

  • Micro / Nano hybrid materials using a Polydimethylsiloxane-Polyamideimide tri-block copolymer and method of manufacturing the same

    KR1020170032726A

  • Organopolysiloxane / polyurea / polyurethane block copolymers

    US20060036055A1

  • Method for the production of organopolysiloxane copolymers and use thereof

    US20060194937A1