Main catalyst for preparing poly(4-methyl-1-pentene) and use of main catalyst

GB2629722APending Publication Date: 2024-11-06PETROCHINA CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
GB2024010538
Authority / Receiving Office
GB · GB
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-08-11
Publication Date
2024-11-06

AI Technical Summary

Technical Problem

When preparing poly(4-methyl-1-pentene), it is difficult for existing catalysts to simultaneously achieve high molecular weight, narrow molecular weight distribution, and high isotacticity, which limits its application in high-end fields.

Method used

Using a non-bridged bisimide hafnium complex as the main catalyst, a combination of triphenylcarbonium tetrakis(pentafluorobenzene)borate and alkyl aluminum as the activator, through specific reaction steps and optimization of conditions, A catalyst with high catalytic activity and selectivity is prepared to realize the homopolymerization reaction of poly(4-methyl-1-pentene).

Benefits of technology

The obtained poly(4-methyl-1-pentene) has high molecular weight, narrow molecular weight distribution and high isotacticity, which significantly improves its mechanical properties and thermal stability, and expands its application prospects in high-end fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

The present application provides a main catalyst for preparing poly(4-methyl-1-pentene) and a use of the main catalyst. The main catalyst for preparing poly(4-methyl-1-pentene) of the present application has a structure represented by formula I. In the formula I, R1 is selected from hydrogen or phenyl, and when R1 is selected from phenyl, R1 is fused with a benzene ring in the formula I to form an anthracene ring; and R2 is selected from methyl or isopropyl. When the main catalyst of the present application is used in a catalytic system to catalyze homopolymerization of 4-methyl-1-pentene, the catalyst exhibits high catalytic activity, and the prepared poly(4-methyl-1-pentene) has high molecular weight, narrow molecular weight distribution and high isotacticity, and thus has broad market application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

A main catalyst for preparing poly (4-methyl-1-pentene) and its application

[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on September 8, 2022, with application number 202211099369.3 and application name “A main catalyst for the preparation of poly(4-methyl-1-pentene) and its application”, the entire contents of which are incorporated by reference into this application. Technical Field

[0002] The embodiments of the present application relate to the technical field of olefin polymerization, and in particular to a main catalyst for preparing poly(4-methyl-1-pentene) and its application. Background Art

[0003] Poly(4-methylpentene-1) (PMP) is a crystalline resin with a stereoregular structure. Its unique structure provides excellent chemical resistance, mechanical properties, processability, electrical insulation, low dielectric properties, optical properties, breathability, and easy stripping properties. Therefore, poly(4-methylpentene-1) has important applications in fiber materials, release materials, high-end medical materials, and electronic materials.

[0004] Poly(4-methyl-1-pentene) is mainly prepared by homopolymerization of 4-methyl-1-pentene monomer catalyzed by a catalyst. Currently, there are three types of catalyst systems used to catalyze the polymerization of 4-methyl-1-pentene monomer: Ziegler-Natta catalysts, metallocene catalysts, and late transition metal nickel palladium catalysts.

[0005] Ziegler-Natta catalysts can effectively catalyze the polymerization of 4-methyl-1-pentene to produce highly isotactic crystalline polymers. Furthermore, the stereoregularity of the product can be adjusted by adding an external electron donor, so that the isotacticity of the polymer is greater than 95% and the melting temperature reaches above 230°C. However, Ziegler-Natta catalysts have multiple active centers, and the molecular weight distribution of the resulting polymer is very wide, typically greater than 10. The low molecular weight portion has poor mechanical properties, limiting its application in high-end fields.

[0006] Metallocene catalysts can also catalyze the polymerization of 4-methyl-1-pentene, but the structure of the metallocene catalyst has a significant impact on the isotacticity of the poly(4-methyl-1-pentene). Currently reported C2-symmetric titanocene / zirconium catalysts can catalyze the polymerization of 4-methyl-1-pentene, with the polymer's isotacticity exceeding 90%. Because the metallocene catalysts have a single metal active center, the resulting poly(4-methyl-1-pentene) has a narrow molecular weight distribution, typically less than 3. However, the metallocene catalysts have significant steric hindrance, making it difficult for the heavily hindered 4-methyl-1-pentene monomer to insert. Consequently, the metallocene catalysts have low activity in catalyzing 4-methyl-1-pentene, making it difficult to produce polymers with a molecular weight exceeding 100,000.

[0007] Late transition metal nickel palladium catalysts have poor stereo control when used in the polymerization of 4-methyl-1-pentene, and high-regularity poly (4-methyl-1-pentene) cannot be obtained. In addition, late transition metal nickel palladium catalysts have a chain walking process during the catalytic polymerization process, resulting in complex product branching. The result is a non-crystalline polymer that is difficult to have practical commercial use.

[0008] Therefore, it is of great significance to develop a catalytic system that can prepare poly(4-methyl-1-pentene) with high molecular weight, high isotacticity and narrow molecular weight.

[0009] Summary of the Invention

[0010] The present application provides a main catalyst for preparing poly(4-methyl-1-pentene) and a preparation method thereof. The main catalyst has high catalytic activity in the polymerization reaction of 4-methyl-1-pentene, and the poly(4-methyl-1-pentene) obtained by catalysis has the advantages of high molecular weight, narrow molecular weight distribution, and high isotacticity.

[0011] The present application also provides a catalyst for preparing poly(4-methyl-1-pentene), which is obtained by compounding the above-mentioned main catalyst and an activator. Since the catalyst includes the above-mentioned main catalyst, it has high catalytic activity, and the poly(4-methyl-1-pentene) prepared by catalysis has the advantages of high molecular weight, narrow molecular weight distribution, and high isotacticity.

[0012] The present application also provides a method for preparing poly(4-methyl-1-pentene), which uses the above-mentioned catalyst to catalyze the homopolymerization reaction of 4-methyl-1-pentene monomer to prepare poly(4-methyl-1-pentene). Therefore, the poly(4-methyl-1-pentene) prepared by this method has the advantages of high molecular weight, narrow molecular weight distribution, and high isotacticity.

[0013] In a first aspect, the present application provides a main catalyst for preparing poly(4-methyl-1-pentene), wherein the main catalyst has a structure shown in Formula I:

[0014] In formula I, R1 is selected from hydrogen or phenyl. When R1 is selected from phenyl, R1 is fused with the naphthalene ring in formula I to form an anthracene ring; R2 is selected from methyl or isopropyl.

[0015] The compound shown in Formula I is a non-bridged imine-amino hafnium complex. The complex has a small steric hindrance, which is conducive to the coordination insertion of the large steric hindrance 4-methyl-1-pentene monomer, enabling the catalyst to obtain high catalytic activity and obtain high molecular weight poly (4-methyl-1-pentene). At the same time, the single metal active center of the complex can make the catalyst have higher selectivity, which is conducive to obtaining a narrow molecular weight distribution and highly isotactic poly (4-methyl-1-pentene).

[0016] The inventors have found that when R2 is selected from isopropyl, the main catalyst exhibits higher catalytic activity, and the poly(4-methyl-1-pentene) obtained by catalysis has a narrower molecular weight and higher isotacticity.

[0017] The second aspect of the present application provides a method for preparing the above-mentioned main catalyst for preparing poly(4-methyl-1-pentene). The preparation route of the method is as follows:

[0018] The specific steps include: 1) reacting methylglyoxal with 2,6-diisopropylaniline to obtain intermediate A; 2) reacting intermediate A with α-naphthylamine or α-anthrylamine to obtain intermediate B; 3) reacting intermediate B with a phenyl lithium compound substituted with R2 to obtain intermediate C; 4) reacting intermediate C with alkyl lithium and hafnium tetrahalide in sequence to obtain intermediate D; 5) reacting intermediate D with methyl magnesium halide to obtain the main catalyst shown in formula I.

[0019] In steps 1) and 2), arylamine compounds are used to condense the aldehyde group and carbonyl group in methylglyoxal to obtain an asymmetric aryl-substituted diimine intermediate B. In step 3), a phenyllithium compound substituted with R2 is used as a nucleophilic reagent to perform nucleophilic addition on intermediate B to obtain a bridgehead-substituted imine-amine intermediate C, which is the ligand of the main catalyst. In step 4), alkyllithium removes the proton on the secondary amine, which then reacts with hafnium tetrahalide to obtain an imine-amine hafnium halide intermediate D. In step 5), intermediate D is subjected to a Grignard reaction with methylmagnesium halide to obtain the main catalyst shown in Formula I.

[0020] The alkyl lithium in step 4) is preferably n-butyl lithium, the hafnium tetrahalide is preferably hafnium tetrachloride, and the methyl magnesium halide in step 5) is preferably methyl magnesium bromide.

[0021] The selection of specific reaction conditions from step 1) to step 5) is a conventional method for those skilled in the art having a basic understanding of organic synthesis and will not be described in detail here.

[0022] The third aspect of the present application provides a catalyst for preparing poly(4-methyl-1-pentene), which includes the main catalyst and activator provided in the first aspect of the present application.

[0023] Since the catalyst includes the main catalyst provided in the first aspect of the present application, it has high catalytic activity, and the poly(4-methyl-1-pentene) prepared by catalysis has the advantages of high molecular weight, narrow molecular weight distribution, and high isotacticity.

[0024] Furthermore, the activator of the present application is selected from a combination of triphenylcarbonium tetrakis(pentafluorophenyl)borate and an alkylaluminum. In consideration of factors such as catalyst activity, selectivity, and cost, the alkylaluminum compound in the combination is preferably at least one of trimethylaluminum, triethylaluminum, and triisobutylaluminum.

[0025] In addition, through experimental exploration of the molar ratio of triphenylcarbonium tetrakis(pentafluorobenzene)borate and alkylaluminum in the composition, as well as the molar ratio of the main catalyst and the co-catalyst, it was found that when the molar ratio of triphenylcarbonium tetrakis(pentafluorobenzene)borate and alkylaluminum in the composition is 1:(50~300), and the molar ratio of the main catalyst and the activator is 1:(1~5), the catalyst has higher catalytic activity, and the prepared polymer has a higher molecular weight, a narrower molecular weight distribution and a higher isotacticity.

[0026] The fourth aspect of the present application provides a method for preparing poly(4-methyl-1-pentene), which comprises: using the catalyst provided in the third aspect of the present application to catalyze a homopolymerization reaction of 4-methyl-1-pentene monomer to obtain the poly(4-methyl-1-pentene).

[0027] The catalyst of the present application has high catalytic activity and high selectivity in the homopolymerization reaction of 4-methyl-1-pentene. The prepared poly(4-methyl-1-pentene) has a high molecular weight, a narrow molecular weight distribution and a high isotacticity, exhibits better mechanical properties and thermal stability, and has a broader market application prospect.

[0028] In the above homopolymerization reaction, the molar ratio of 4-methyl-1-pentene monomer to catalyst, the temperature of the homopolymerization reaction, the solvent and other conditions can be optimized to obtain poly(4-methyl-1-pentene) with a higher molecular weight, a narrower molecular weight distribution and a higher isotacticity.

[0029] After optimization experiments, it was found that the molar ratio of 4-methyl-1-pentene monomer to catalyst is preferably (100-400,000):1, and more preferably (10,000-100,000):1; the temperature of the homopolymerization reaction is 20-60°C; and the solvent of the homopolymerization reaction is preferably one or more of 1,2-dichloroethane, chloroform, chlorobenzene, toluene, benzene, and xylene.

[0030] By controlling factors such as the molar ratio of 4-methyl-1-pentene monomer to catalyst, polymerization temperature, and polymerization solvent in the homopolymerization reaction, the prepared poly(4-methyl-1-pentene) can have a weight-average molecular weight of ≥500,000, preferably 500,000 to 1,630,000; a molecular weight distribution index of ≤4, preferably 2.0 to 4.0; an isotacticity of ≥95%; and a melting temperature of ≥230°C, preferably 230 to 240°C.

[0031] Compared with the prior art, this application has at least the following beneficial effects:

[0032] 1) The main catalyst provided in this application is a non-bridged imine-amine complex, which has a small steric hindrance, which is conducive to the coordination insertion of the large steric hindrance 4-methyl-1-pentene monomer, enabling the catalyst to obtain high catalytic activity and obtain high molecular weight poly (4-methyl-1-pentene). At the same time, the single metal active center of the complex can make the catalyst have higher selectivity, which is conducive to obtaining narrow molecular distribution and high isotacticity poly (4-methyl-1-pentene).

[0033] 2) The main catalyst of the present application is applied to the catalytic system to catalyze the polymerization of 4-methyl-1-pentene monomer. The poly(4-methyl-1-pentene) obtained by polymerization has high molecular weight, narrow molecular weight distribution, high isotacticity, and high melting temperature. Therefore, the obtained polymer has better mechanical properties and thermal stability, and has broader application prospects.

[0034] 3) The poly(4-methyl-1-pentene) preparation method provided in this application has the advantages of mild reaction conditions and high efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, a brief introduction will be given below to the drawings required for use in the embodiments or the description of the prior art. It is obvious that the drawings described below are some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.

[0036] Figure 1 is a graph showing the structure of poly (4-methyl-1-pentene) prepared in Example 1. 13 C NMR spectrum;

[0037] FIG2 is a DSC curve diagram of poly(4-methyl-1-pentene) prepared in Example 1;

[0038] FIG3 is a GPC curve of poly(4-methyl-1-pentene) prepared in Example 1. DETAILED DESCRIPTION

[0039] To make the purpose, technical solutions, and advantages of the embodiments of this application more clear, the technical solutions in the embodiments of this application will be clearly and completely described below in conjunction with the drawings in the embodiments of this application. Obviously, the described embodiments are part of the embodiments of this application, not all of the embodiments. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.

[0040] The main catalyst for preparing poly(4-methyl-1-pentene) provided in the present application and its application are further described in detail below with reference to specific examples.

[0041] It should be noted that, in the following examples, unless otherwise specified, the raw materials used can be obtained by commercial purchase or conventional methods, and the experimental methods without specific conditions are conventional methods and conventional conditions well known in the art.

[0042] The catalytic activity of the catalysts in the following examples and comparative examples is calculated as follows: catalytic activity = mass of poly(4-methyl-1-pentene) (g) / (amount of main catalyst added (mol) × reaction time (h)).

[0043] The weight average molecular weight and molecular weight distribution index of the poly(4-methyl-1-pentene) prepared in the following examples and comparative examples were measured by GPC.

[0044] The melting temperatures of the poly(4-methyl-1-pentene) prepared in the following examples and comparative examples were all measured using DSC thermal analysis.

[0045] The isotacticity of the poly (4-methyl-1-pentene) prepared in the following examples and comparative examples is adopted 13 C NMR was used for determination.

[0046] Example 1

[0047] The preparation process of the main catalyst, catalyst and poly (4-methyl-1-pentene) of this embodiment is as follows:

[0048] 1) Preparation of main catalyst P1

[0049] The preparation route is as follows:

[0050] The preparation steps include:

[0051] a. Add 0.79 g (11 mmol) of S1 (methylglyoxal), 50 mL of ethanol, and a catalytic amount of formic acid to a reaction flask and mix well. Then, slowly add 1.77 g (10 mmol) of 2,6-diisopropylaniline dropwise to the reaction flask. After the addition is complete, stir and react for 12 hours. The reaction system is concentrated to remove the solvent, and the concentrate is purified by silica gel column chromatography (eluent: a mixed solvent of n-hexane and ethyl acetate in a volume ratio of 50:1) to obtain compound S2 with a yield of 93%;

[0052] b. Dissolve 0.93 g (4 mmol) of compound S2 in 50 mL of toluene, then slowly add dropwise 0.72 g (5 mmol) of α-naphthylamine and a catalytic amount of p-toluenesulfonic acid, heat to reflux, react for 12 h, cool, and concentrate to remove the solvent. The concentrate is purified by column chromatography (eluent: a mixed solvent of n-hexane and ethyl acetate in a volume ratio of 50:1) to obtain compound S3 in an 89% yield.

[0053] c. At -40°C, 1.78 g (5 mmol) of compound S3 was dissolved in anhydrous ether, and a solution of 0.76 g (6 mmol) of 2-isopropylphenyllithium in ether was slowly added dropwise. After the addition was complete, the reaction system was naturally warmed to room temperature and allowed to react overnight. After TLC analysis, a saturated solution of ammonium chloride was added to the reaction system to quench the reaction. The mixture was extracted three times with anhydrous ether, and the ether phase was collected and washed with saturated brine, dried over anhydrous sodium sulfate, filtered, and concentrated to obtain a concentrate. The concentrate was recrystallized from ethanol to obtain ligand L1 with a yield of 90%.

[0054] The characterization data of ligand L1 are:

[0055] 1 H NMR (CD3Cl, 400MHz): δ (ppm) 8.44 (d, 1H, Nap-H), 8.12-8.08 (d, 3H, Nap-H), 7.97 (d, 1H, Nap-H), 7.70-6.87 (m, 9H, Ar-H), 6.71 (s, 1H, CNH), 4.26 (s ,1H,NCH),3.67(sept,2H,CH(CH3)2),2.94(sept,1H,CH(CH3)2),1.78(d,6H,CH(CH3)2),1.19(d,6H,CH(CH3)2),1.13(s,3H,C-CH3),1.01(d,3H, CH(CH3)2),0.93(d,3H,CH(CH3)2).

[0056] Anal.Calcd for C 34 H40 N2:C,85.67;H,8.46;N,5.88;Found:C,85.73;H,8.45;N,5.82

[0057] d. Under nitrogen atmosphere, 0.93 g (2 mmol) of compound S4 was added to a dry Schlenk bottle, and 20 mL of toluene was added to dissolve it. At -50 ° C, n-butyl lithium solution (1.5 mL, 1.6 M) was added dropwise to the Schlenk bottle. After the addition was complete, the temperature was naturally raised to room temperature. After the reaction was completed, the solvent was drained to precipitate a yellow powder, which was washed three times with n-hexane. After the n-hexane was drained, a yellow lithium salt ligand was obtained. The yellow ligand lithium salt was dissolved in toluene and transferred to the reaction bottle. HfCl4 0.71 g (2.2 mmol) of toluene suspension was also added to the reaction flask, and then the temperature was raised to 120 ° C for 6 hours, naturally cooled to room temperature, and then placed in a low-temperature bath to cool to -40 ° C. MeMgBr (2.5 mL, 3 M) was then slowly dripped into the reaction system. After the addition was completed, the temperature was naturally raised to room temperature and stirred for 6 hours. The precipitate was filtered to remove the precipitate, and then the precipitate was washed three times with toluene. The filtrate was combined and the solvent in the filtrate was distilled off under reduced pressure to obtain a solid. The solid was washed three times with n-hexane and dried to obtain the main catalyst P1 as a yellow solid with a yield of 64%.

[0058] The characterization data of the main catalyst P1 are:

[0059] 1 H NMR(C6D6,400MHz): δ(ppm)8.52(d,1H,Nap-H),8.26(d,1H,Nap-H),7.94(d,1H,Nap-H),7.73(d,1H,Nap-H),7 .35-6.97(m,9H,Ar-H),4.42(s,1H,NCH),3.78(sept,1H,CH(CH3)2),3.02(sept,1H,CH(CH3)2),2.89(sept,1 H,CH(CH3)2),1.35(d,3H,CH(CH3)2),1.31(d,3H,CH(CH3)2),1.21(d,3H,CH(CH3)2),1.17(s,3H,C-CH3),1.1 2(d,3H,CH(CH3)2),0.97(s,3H,Hf-CH3),0.73(d,3H,CH(CH3)2),0.66(s,3H,Hf-CH3),0.34(d,3H,CH(CH3)2).

[0060] MS-EI (m / z): 684.3 (M + ).

[0061] Anal.Calcd for C36 H 44 N2Hf:C,63.28;H,6.49;N,4.10;Found:C,63.32;H,6.44;N,4.03.

[0062] 2) Preparation of Catalyst C1-3

[0063] Compound P1 was used as the main catalyst, a composition of triphenylcarbonium tetrakis(pentafluorobenzene)borate and triisobutylaluminum (molar ratio of 1:67) was used as the activator, and the activator was marked as A3. The main catalyst P1 and the activator A3 were compounded in a molar ratio of 1:1.5 to obtain catalyst C1-3.

[0064] 3) Preparation of poly(4-methyl-1-pentene)

[0065] The specific steps include: continuously evacuating a Schlenk flask equipped with a magnetic stirrer and drying it with an infrared lamp for two hours. After natural cooling, the atmosphere is replaced with nitrogen three times to atmospheric pressure. Then, 7 mL of toluene and 3 mL of 4-methyl-1-pentene monomer are sequentially added to the Schlenk flask, and stirred at 40°C in a water bath for half an hour. Subsequently, 1 μmol of catalyst C1-3 (the molar ratio of 4-methyl-1-pentene monomer to catalyst C1-3 is 24,000:1) is added to the system to initiate polymerization. After polymerization for 5 minutes, a 10% hydrochloric acid-containing ethanol solution is added to terminate the polymerization. The polymerization system is filtered, washed three times with ethanol, and vacuum-dried to constant weight to obtain poly(4-methyl-1-pentene).

[0066] Calculation shows that the catalytic activity of catalyst C1-3 in the above homopolymerization reaction is 14.5 kg polymer / (mmol Hf·h).

[0067] The data of poly (4-methyl-1-pentene) prepared in Example 1 are characterized. FIG1 is a graph showing the data of poly (4-methyl-1-pentene) prepared in Example 1. 13 C NMR graph; FIG2 is a DSC curve graph of the poly(4-methyl-1-pentene) prepared in Example 1; FIG3 is a GPC curve graph of the poly(4-methyl-1-pentene) prepared in Example 1. Analysis of FIG1 to FIG3 shows that the poly(4-methyl-1-pentene) prepared in Example 1 has a weight-average molecular weight of 705 kg / mol, a molecular weight distribution index of 2.3, a melting temperature of 238°C, and an isotacticity of 98%.

[0068] Example 2

[0069] The main catalyst and catalyst preparation of this embodiment are consistent with those of Example 1;

[0070] The preparation steps of poly(4-methyl-1-pentene) in this example are basically the same as those in Example 1, except that the polymerization temperature is changed from 40°C to 20°C.

[0071] The catalytic activity of catalyst C1-3 in this example is 3.1 kg polymer / (mmol Hf·h). The prepared poly(4-methyl-1-pentene) has a weight-average molecular weight of 733 kg / mol, a molecular weight distribution index of 4.0, a melting temperature of 240° C., and an isotacticity of >99%.

[0072] Example 3

[0073] The main catalyst and catalyst preparation of this embodiment are consistent with those of Example 1;

[0074] The preparation steps of poly(4-methyl-1-pentene) in this example are basically the same as those in Example 1, except that the polymerization temperature is changed from 40°C to 60°C.

[0075] The catalytic activity of catalyst C1-3 in this example is 6.5 kg polymer / (mmol Hf·h). The weight-average molecular weight of the prepared poly(4-methyl-1-pentene) is 821 kg / mol, the molecular weight distribution index is 2.0, the melting temperature is 237° C., and the isotacticity is 97%.

[0076] Example 4

[0077] The preparation of the catalyst and the catalyst were the same as those in Example 1.

[0078] The preparation steps of poly(4-methyl-1-pentene) in this example are basically the same as those in Example 1, except that 0.0125 mL of 4-methyl-1-pentene monomer is added to the homopolymerization reaction (the molar ratio of 4-methyl-1-pentene monomer to catalyst C1-3 is 100:1).

[0079] The catalytic activity of catalyst C1-3 in this example is 4.8 kg polymer / (mmol Hf·h). The weight-average molecular weight of the prepared poly(4-methyl-1-pentene) is 501 kg / mol, the molecular weight distribution index is 2.0, the melting temperature is 239° C., and the isotacticity is 99%.

[0080] Example 5

[0081] The main catalyst and catalyst preparation of this embodiment are consistent with those of Example 1;

[0082] The preparation steps of poly(4-methyl-1-pentene) in this example are basically the same as those in Example 1, except that 0.125 mL of 4-methyl-1-pentene monomer is added to the homopolymerization reaction (the molar ratio of 4-methyl-1-pentene monomer to catalyst C1-3 is 1000:1).

[0083] The catalytic activity of catalyst C1-3 in this example is 13.8 kg polymer / (mmol Hf·h). The weight-average molecular weight of the prepared poly(4-methyl-1-pentene) is 538 kg / mol, the molecular weight distribution index is 2.2, the melting temperature is 239° C., and the isotacticity is 99%.

[0084] Example 6

[0085] The main catalyst and catalyst preparation of this embodiment are consistent with those of Example 1;

[0086] The preparation steps of poly(4-methyl-1-pentene) in this example are basically the same as those in Example 1, except that 1 mL of 4-methyl-1-pentene monomer is added to the homopolymerization reaction (the molar ratio of 4-methyl-1-pentene monomer to catalyst C1-3 is 8000:1).

[0087] The catalytic activity of catalyst C1-3 in this example is 9.2 kg polymer / (mmol Hf·h). The weight-average molecular weight of the prepared poly(4-methyl-1-pentene) is 686 kg / mol, the molecular weight distribution index is 2.3, the melting temperature is 238° C., and the isotacticity is 98%.

[0088] Example 7

[0089] The main catalyst and catalyst preparation of this embodiment are consistent with those of Example 1;

[0090] The preparation steps of poly(4-methyl-1-pentene) in this example are basically the same as those in Example 1, except that 5 mL of 4-methyl-1-pentene monomer is added to the homopolymerization reaction (the molar ratio of 4-methyl-1-pentene monomer to catalyst C1-3 is 40,000:1).

[0091] The catalytic activity of catalyst C1-3 in this example is 29.6 kg polymer / (mmol Hf·h). The weight-average molecular weight of the prepared poly(4-methyl-1-pentene) is 830 kg / mol, the molecular weight distribution index is 2.7, the melting temperature is 238° C., and the isotacticity is 98%.

[0092] Example 8

[0093] The main catalyst and catalyst preparation of this embodiment are consistent with those of Example 1;

[0094] The preparation steps of poly(4-methyl-1-pentene) in this example are basically the same as those in Example 1, except that the polymerization solvent is replaced by benzene from toluene.

[0095] The catalytic activity of catalyst C1-3 in this example is 8.3 kg polymer / (mmol Hf·h). The weight-average molecular weight of the prepared poly(4-methyl-1-pentene) is 811 kg / mol, the molecular weight distribution index is 2.7, the melting temperature is 238° C., and the isotacticity is 98%.

[0096] Example 9

[0097] The main catalyst and catalyst preparation of this embodiment are consistent with those of Example 1;

[0098] The preparation steps of poly(4-methyl-1-pentene) in this example are basically the same as those in Example 1, except that the polymerization solvent is replaced by xylene from toluene.

[0099] The catalytic activity of catalyst C1-3 in this example is 10.5 kg polymer / (mmol Hf·h). The prepared poly(4-methyl-1-pentene) has a weight-average molecular weight of 785 kg / mol, a molecular weight distribution index of 2.7, a melting temperature of 238° C., and an isotacticity of 98%.

[0100] Example 10

[0101] The main catalyst and catalyst preparation of this embodiment are consistent with those of Example 1;

[0102] The preparation steps of poly(4-methyl-1-pentene) in this example are basically the same as those in Example 1, except that the polymerization solvent is replaced by 1,2-dichloroethane from toluene.

[0103] The catalytic activity of catalyst C1-3 in this example is 12.1 kg polymer / (mmol Hf·h). The weight-average molecular weight of the prepared poly(4-methyl-1-pentene) is 738 kg / mol, the molecular weight distribution index is 2.6, the melting temperature is 237°C, and the isotacticity is 97%.

[0104] Example 11

[0105] The main catalyst and catalyst preparation of this embodiment are consistent with those of Example 1;

[0106] The preparation steps of poly(4-methyl-1-pentene) in this example are basically the same as those in Example 1, except that the polymerization solvent is replaced by chloroform from toluene.

[0107] The catalytic activity of catalyst C1-3 in this example is 9.8 kg polymer / (mmol Hf·h). The weight-average molecular weight of the prepared poly(4-methyl-1-pentene) is 765 kg / mol, the molecular weight distribution index is 2.6, the melting temperature is 237°C, and the isotacticity is 97%.

[0108] Example 12

[0109] The main catalyst and catalyst preparation of this embodiment are consistent with those of Example 1;

[0110] The preparation steps of poly(4-methyl-1-pentene) in this example are basically the same as those in Example 1, except that the polymerization solvent is replaced by chlorobenzene from toluene.

[0111] The catalytic activity of catalyst C1-3 in this example is 10.9 kg polymer / (mmol Hf·h). The weight-average molecular weight of the prepared poly(4-methyl-1-pentene) is 857 kg / mol, the molecular weight distribution index is 2.7, the melting temperature is 238° C., and the isotacticity is 98%.

[0112] Example 13

[0113] The main catalyst and catalyst preparation of this embodiment are consistent with those of Example 1;

[0114] The preparation steps of poly(4-methyl-1-pentene) in this example are basically the same as those in Example 1, except that the polymerization solvent is replaced from toluene with a mixed solvent of toluene and benzene in a volume ratio of 1:1.

[0115] The catalytic activity of catalyst C1-3 in this example is 7.8 kg polymer / (mmol Hf·h). The weight-average molecular weight of the prepared poly(4-methyl-1-pentene) is 778 kg / mol, the molecular weight distribution index is 2.7, the melting temperature is 238° C., and the isotacticity is 98%.

[0116] Example 14

[0117] The main catalyst and catalyst preparation of this embodiment are consistent with those of Example 1;

[0118] The preparation steps of poly(4-methyl-1-pentene) in this example are basically the same as those in Example 1, except that the polymerization solvent is replaced from toluene with a mixed solvent of toluene and xylene in a volume ratio of 1:1.

[0119] In the homopolymerization reaction of this example, the catalytic activity of catalyst C1-3 was 8.7 kg polymer / (mmol Hf·h). The prepared poly(4-methyl-1-pentene) had a weight-average molecular weight of 749 kg / mol, a molecular weight distribution index of 2.7, a melting temperature of 238° C., and an isotacticity of 98%.

[0120] Example 15

[0121] The main catalyst and catalyst preparation of this embodiment are consistent with those of Example 1;

[0122] The preparation steps of poly(4-methyl-1-pentene) in this example are basically the same as those in Example 1, except that the polymerization solvent is replaced from toluene with a mixed solvent of 1,2-dichloroethane and chloroform in a volume ratio of 1:1.

[0123] The catalytic activity of catalyst C1-3 in this example is 7.1 kg polymer / (mmol Hf·h). The weight-average molecular weight of the prepared poly(4-methyl-1-pentene) is 794 kg / mol, the molecular weight distribution index is 2.6, the melting temperature is 237° C., and the isotacticity is 97%.

[0124] Example 16

[0125] The main catalyst and catalyst preparation of this embodiment are consistent with those of Example 1;

[0126] The preparation steps of poly(4-methyl-1-pentene) in this example are basically the same as those in Example 1, except that the polymerization solvent is replaced from toluene with a mixed solvent of chlorobenzene and benzene in a volume ratio of 1:1.

[0127] The catalytic activity of catalyst C1-3 in this example is 8.1 kg polymer / (mmol Hf·h). The weight-average molecular weight of the prepared poly(4-methyl-1-pentene) is 843 kg / mol, the molecular weight distribution index is 2.7, the melting temperature is 238° C., and the isotacticity is 98%.

[0128] Example 17

[0129] The main catalyst of this embodiment is consistent with that of embodiment 1;

[0130] The catalyst of this embodiment is obtained by compounding the main catalyst P1 and the activator A3 in a molar ratio of 1:1. The obtained catalyst is marked as catalyst C1-7;

[0131] The preparation steps of poly(4-methyl-1-pentene) in this example are basically the same as those in Example 1, except that catalyst C1-3 is replaced by catalyst C1-7.

[0132] The catalytic activity of catalyst C1-7 in this example is 6.8 kg polymer / (mmol Hf·h). The weight-average molecular weight of the prepared poly(4-methyl-1-pentene) is 688 kg / mol, the molecular weight distribution index is 2.5, the melting temperature is 238° C., and the isotacticity is 98%.

[0133] Example 18

[0134] The main catalyst of this embodiment is consistent with that of embodiment 1;

[0135] The catalyst of this embodiment is obtained by compounding the main catalyst P1 and the activator A3 in a molar ratio of 1:3. The obtained catalyst is marked as catalyst C1-8;

[0136] The preparation steps of poly(4-methyl-1-pentene) in this example are basically the same as those in Example 1, except that catalyst C1-3 is replaced by catalyst C1-8.

[0137] The catalytic activity of catalyst C1-8 in this example is 7.2 kg polymer / (mmol Hf·h). The weight-average molecular weight of the prepared poly(4-methyl-1-pentene) is 744 kg / mol, the molecular weight distribution index is 2.6, the melting temperature is 238° C., and the isotacticity is 98%.

[0138] Example 19

[0139] The main catalyst of this embodiment is consistent with that of embodiment 1;

[0140] The catalyst of this embodiment is obtained by compounding the main catalyst P1 and the activator A3 in a molar ratio of 1:5. The obtained catalyst is marked as catalyst C1-9;

[0141] The preparation steps of poly(4-methyl-1-pentene) in this example are basically the same as those in Example 1, except that catalyst C1-3 is replaced by catalyst C1-9.

[0142] The catalytic activity of catalyst C1-9 in this example is 8.8 kg polymer / (mmol Hf·h). The weight-average molecular weight of the prepared poly(4-methyl-1-pentene) is 798 kg / mol, the molecular weight distribution index is 2.7, the melting temperature is 238° C., and the isotacticity is 98%.

[0143] Example 20

[0144] The main catalyst of this embodiment is consistent with that of embodiment 1;

[0145] The catalyst of this embodiment uses compound P1 as the main catalyst and a composition of triphenylcarbonium tetrakis(pentafluorobenzene)borate and triisobutylaluminum (molar ratio of 1:50) as the activator. The activator is marked as A4. The main catalyst P1 and the activator A4 are compounded in a mass ratio of 1:1.5 to obtain catalyst C1-4.

[0146] The preparation steps of poly(4-methyl-1-pentene) in this example are basically the same as those in Example 1, except that catalyst C1-3 is replaced by catalyst C1-4.

[0147] The catalytic activity of catalyst C1-4 in this example is 8.3 kg polymer / (mmol Hf·h). The prepared poly(4-methyl-1-pentene) has a weight-average molecular weight of 667 kg / mol, a molecular weight distribution index of 2.8, a melting temperature of 238° C., and an isotacticity of 98%.

[0148] Example 21

[0149] The main catalyst of this embodiment is consistent with that of embodiment 1;

[0150] The catalyst of this embodiment uses compound P1 as the main catalyst and a composition of triphenylcarbonium tetrakis(pentafluorobenzene)borate and triisobutylaluminum (molar ratio of 1:150) as the activator. The activator is marked as A5. The main catalyst P1 and the activator A5 are compounded in a mass ratio of 1:1.5 to obtain catalyst C1-5.

[0151] The preparation steps of poly(4-methyl-1-pentene) in this example are basically the same as those in Example 1, except that catalyst C1-3 is replaced by catalyst C1-5.

[0152] The catalytic activity of catalyst C1-5 in this example is 8.9 kg polymer / (mmol Hf·h). The weight-average molecular weight of the prepared poly(4-methyl-1-pentene) is 601 kg / mol, the molecular weight distribution index is 3.0, the melting temperature is 238° C., and the isotacticity is 98%.

[0153] Example 22

[0154] The main catalyst of this embodiment is consistent with that of embodiment 1;

[0155] The catalyst of this embodiment uses compound P1 as the main catalyst and a composition of triphenylcarbonium tetrakis(pentafluorobenzene)borate and triisobutylaluminum (molar ratio of 1:300) as the activator. The activator is marked as A6. The main catalyst P1 and the activator A6 are compounded in a mass ratio of 1:1.5 to obtain catalyst C1-6.

[0156] The preparation steps of poly(4-methyl-1-pentene) in this example are basically the same as those in Example 1, except that catalyst C1-3 is replaced by catalyst C1-6.

[0157] The catalytic activity of catalyst C1-6 in this example is 7.4 kg polymer / (mmol Hf·h). The weight-average molecular weight of the prepared poly(4-methyl-1-pentene) is 519 kg / mol, the molecular weight distribution index is 3.5, the melting temperature is 238° C., and the isotacticity is 98%.

[0158] Example 23

[0159] The main catalyst of this embodiment is consistent with that of embodiment 1;

[0160] The catalyst of this embodiment uses compound P1 as the main catalyst and a composition of triphenylcarbonium tetrakis(pentafluorophenyl)borate and trimethylaluminum (molar ratio of 1:67) as the activator. The activator is marked as A1. The main catalyst P1 and the activator A1 are compounded in a mass ratio of 1:1.5 to obtain catalyst C1-1.

[0161] The preparation steps of poly(4-methyl-1-pentene) in this example are basically the same as those in Example 1, except that catalyst C1-3 is replaced by catalyst C1-1.

[0162] The catalytic activity of catalyst C1-1 in this example is 7.8 kg polymer / (mmol Hf·h). The weight-average molecular weight of the prepared poly(4-methyl-1-pentene) is 556 kg / mol, the molecular weight distribution index is 3.0, the melting temperature is 238° C., and the isotacticity is 98%.

[0163] Example 24

[0164] The main catalyst of this embodiment is consistent with that of embodiment 1;

[0165] The catalyst of this embodiment uses compound P1 as the main catalyst and a composition of triphenylcarbonium tetrakis(pentafluorobenzene)borate and triethylaluminum (molar ratio of 1:67) as the activator. The activator is marked as A2. The main catalyst P1 and the activator A2 are compounded in a mass ratio of 1:1.5 to obtain catalyst C1-2.

[0166] The preparation steps of poly(4-methyl-1-pentene) in this example are basically the same as those in Example 1, except that catalyst C1-3 is replaced by catalyst C1-2.

[0167] The catalytic activity of catalyst C1-2 in this example is 9.4 kg polymer / (mmol Hf·h). The weight-average molecular weight of the prepared poly(4-methyl-1-pentene) is 618 kg / mol, the molecular weight distribution index is 2.8, the melting temperature is 238° C., and the isotacticity is 98%.

[0168] Example 25

[0169] The preparation process of the main catalyst, catalyst and poly (4-methyl-1-pentene) of this embodiment is as follows:

[0170] 1) Preparation of main catalyst P2

[0171] The structural formula of the main catalyst P2 is as follows:

[0172] The preparation steps of the main catalyst P2 are basically the same as the preparation steps of the main catalyst P1 recorded in Example 1, except that the 2-isopropylbenzene lithium in step c is replaced by methylbenzene lithium, the product of step c is ligand L2, the yield of step c is 91%, and the yield of step d is 68%.

[0173] The structural formula of ligand L2 is as follows:

[0174] The characterization data of ligand L2 are:

[0175] 1 H NMR(CD3Cl,400MHz): δ(ppm)8.24(d,1H,Nap-H),8.19-8.16(d,3H,Nap-H),8.00(d,1H,Nap-H),7.63-7.08(m,9H,Ar-H),6.80(s,1H,CNH),4.01(s,1H,NC H),3.77(sept,2H,CH(CH3)2),3.01(sept,1H,CH(CH3)2),2.96(d,3H,C(CH3)2).1.78(d,6H,CH(CH3)2),1.19(d,6H,CH(CH3)2),1.01(d,3H,CH(CH3)2).

[0176] Anal.Calcd for C 32 H 36 N2:C,85.67;H,8.09;N,6.24;Found:C,85.73;H,8.05;N,6.20.

[0177] The characterization data of the main catalyst P2 are:

[0178] 1H NMR(C6D6,400MHz): δ(ppm)8.42(d,1H,Nap-H),8.18(d,1H,Nap-H),8.05(d,1H,Nap-H),7.76(d, 1H,Nap-H),7.41-6.99(m,9H,Ar-H),4.12(s,1H,NCH),3.12(sept,1H,CH(CH3)2),2.93(sept,1H ,CH(CH3)2),2.37(s,3H,C-CH3),2.01(s,3H,NC-CH3),1.33(d,3H,CH(CH3)2),1.21(d,3H,CH(CH 3)2),1.13(d,3H,CH(CH3)2),0.90(s,3H,Hf-CH3),0.87(d,3H,CH(CH3)2),0.78(s,3H,Hf-CH3).

[0179] MS-EI(m / z):656.27(M + ).

[0180] Anal.Calcd for C 34 H 40 N2Hf:C,62.33;H,6.15;N,4.28;Found:C,62.40;H,6.12;N,4.25.

[0181] 2) Preparation of Catalyst C2-3

[0182] Compound P2 was used as the main catalyst, and the main catalyst P2 and the activator A3 were compounded in a molar ratio of 1:1.5 to obtain catalyst C2-3.

[0183] 3) Preparation of poly(4-methyl-1-pentene)

[0184] The specific steps are basically the same as those in Example 1, except that catalyst C1-3 is replaced by catalyst C2-3.

[0185] The catalytic activity of catalyst C2-3 in this example is 0.6 kg polymer / (mmol Hf·h). The weight-average molecular weight of the prepared poly(4-methyl-1-pentene) is 1634 kg / mol, the molecular weight distribution index is 4.0, the melting temperature is 231°C, and the isotacticity is 95%.

[0186] Example 26

[0187] The preparation process of the main catalyst, catalyst and poly (4-methyl-1-pentene) of this embodiment is as follows:

[0188] 1) Preparation of main catalyst P3

[0189] The structural formula of the main catalyst P3 is as follows:

[0190] The preparation steps of the main catalyst P3 are basically the same as the preparation steps of the main catalyst P1 described in Example 1, except that the naphthylamine in step b is replaced by anthracenamine.

[0191] The ligand obtained in step c is L3, the yield in step c is 87%, and the yield in step d is 59%.

[0192] The structural formula of ligand L3 is as follows:

[0193] The characterization data of ligand L3 are:

[0194] 1 H NMR(C6D6,400MHz): δ(ppm)8.49(d,2H,An-H),8.21(d,2H,An-H),8.13(d,1H,An-H), 7.68(d,1H,An-H),7.49-6.95(m,10H,Ar-H),6.02(s,1H,CNH),4.17(s,1H,NCH),3.42 (sept,2H,CH(CH3)2),2.81(sept,1H,CH(CH3)2),1.79-1.71(d,6H,CH(CH3)2),1.23( d,6H,CH(CH3)2),1.06(s,3H,C-CH3),1.02(d,3H,CH(CH3)2),0.91(d,3H,CH(CH3)2).

[0195] Anal.Calcd for C 38 H 42 N2:C,86.64;H,8.04;N,5.32;Found:C,86.70;H,8.07;N,5.35.

[0196] The characterization data of the main catalyst P3 are:

[0197] 1H NMR (CD3Cl, 400MHz): δ (ppm) 8.58 (d, 1H, An-H), 8.41 (d, 1H, An-H), 8.13 (d, 1H, An-H), 8.02 (d, 1H, An-H), 7.64 (d, 1H,An-H),7.49-6.84(m,10H,Ar-H),4.18(s,1H,NCH),3.16(sept,1H,CH(CH3)2),2.96(sept,1H,CH(CH3)2),2.84 (sept,1H,CH(CH3)2),1.37(d,3H,CH(CH3)2),1.32(d,3H,CH(CH3)2),1.20(d,3H,CH(CH3)2),1.15(s,3H,C-CH3), 1.11(d,3H,CH(CH3)2),0.90(s,3H,Hf-CH3),0.76(d,3H,CH(CH3)2),0.62(s,3H,Hf-CH3),0.29(d,3H,CH(CH3)2).

[0198] MS-EI(m / z):732.31(M + ).

[0199] Anal.Calcd for C 40 H 46 N2Hf:C,65.52;H,6.32;N,3.82;Found:C,65.59;H,6.29;N,3.80.

[0200] 2) Preparation of Catalyst C3-3

[0201] Using compound P3 as the main catalyst, the main catalyst P3 and the activator A3 were compounded in a molar ratio of 1:1.5 to obtain the catalyst system C3-3.

[0202] 3) Preparation of poly(4-methyl-1-pentene)

[0203] The specific steps are basically the same as those in Example 1, except that catalyst C1-3 is replaced by catalyst C3-3.

[0204] The catalytic activity of catalyst C3-3 in this example is 8.3 kg polymer / (mmol Hf·h). The weight-average molecular weight of the prepared poly(4-methyl-1-pentene) is 637 kg / mol, the molecular weight distribution index is 3.0, the melting temperature is 236°C, and the isotacticity is 97%.

[0205] Example 27

[0206] The preparation process of the main catalyst, catalyst and poly (4-methyl-1-pentene) of this embodiment is as follows:

[0207] 1) Preparation of main catalyst P4

[0208] The structural formula of the main catalyst P4 is as follows:

[0209] The preparation steps of the main catalyst P4 are basically the same as those of the main catalyst P3 recorded in Example 26, except that the 2-isopropylbenzene lithium in step c is replaced by methylbenzene lithium, and the product obtained in step c is ligand L4. The yield of step c is 89%, and the yield of step d is 61%.

[0210] The structural formula of ligand L4 is as follows:

[0211] The characterization data of ligand L4 are:

[0212] 1 H NMR (CD3Cl, 400MHz): δ (ppm) 8.47 (d, 2H, An-H), 8.19 (d, 2H, An-H), 8.09 (d, 1H ,An-H),7.46(d,1H,An-H),7.40-6.65(m,10H,Ar-H),6.17(s,1H,CNH),3.99(s ,1H,NCH),3.18(sept,2H,CH(CH3)2),2.41(s,3H,C-CH3),1.56-1.53(d,6H,C H(CH3)2),1.01(s,3H,C-CH3),0.97(d,3H,CH(CH3)2),0.87(d,3H,CH(CH3)2).

[0213] Anal.Calcd for C 36 H 38 N2:C,86.70;H,7.68;N,5.62;Found:C,86.74;H,7.66;N,5.59.

[0214] The characterization data of the main catalyst P4 are:

[0215] 1H NMR(C6D6,400MHz): δ(ppm)8.51(d,1H,An-H),8.38(d,1H,An-H),8.15(d,1H,An-H),7.98(d,1H,An- H),7.57(d,1H,An-H),7.45-6.96(m,10H,Ar-H),4.11(s,1H,NCH),3.21(sept,1H,CH(CH3)2),3.01( sept,1H,CH(CH3)2),2.41(s,3H,C-CH3),2.17(s,3H,NC-CH3),1.37(d,3H,CH(CH3)2),1.28(d,3H,C H(CH3)2),1.13(d,3H,CH(CH3)2),0.86(s,3H,Hf-CH3),0.81(d,3H,CH(CH3)2),0.71(s,3H,Hf-CH3).

[0216] MS-EI(m / z):706.28(M + ).

[0217] Anal.Calcd for C 38 H 42 N2Hf:C,64.72;H,6.00;N,3.97;Found:C,64.80;H,6.04;N,4.02.

[0218] 2) Preparation of Catalyst C4-3

[0219] Compound P4 was used as the main catalyst, and the main catalyst P4 and the activator A3 were compounded in a molar ratio of 1:1.5 to obtain the catalyst system C4-3.

[0220] 3) Preparation of poly(4-methyl-1-pentene)

[0221] The specific steps are basically the same as those in Example 1, except that catalyst C1-3 is replaced by catalyst C4-3.

[0222] In this example, the catalytic activity of C4-3 was 0.4 kg polymer / (mmol Hf·h), and the prepared poly(4-methyl-1-pentene) had a weight-average molecular weight of 1084 kg / mol, a molecular weight distribution index of 3.8, a melting temperature of 230°C, and an isotacticity of 95%.

[0223] Example 28

[0224] The main catalyst of this embodiment is consistent with that of embodiment 1;

[0225] The catalyst of this embodiment uses compound P1 as the main catalyst and a composition of triphenylcarbonium tetrakis(pentafluorobenzene)borate and triisobutylaluminum (molar ratio of 1:25) as the activator. The activator is marked as A4. The main catalyst P1 and the activator A4 are compounded in a mass ratio of 1:1.5 to obtain catalyst C1-10.

[0226] The preparation steps of poly(4-methyl-1-pentene) in this example are basically the same as those in Example 1, except that catalyst C1-3 is replaced by catalyst C1-10.

[0227] The catalytic activity of catalyst C1-10 in this example is 9.5 kg polymer / (mmol Hf·h). The weight-average molecular weight of the prepared poly(4-methyl-1-pentene) is 345 kg / mol, the molecular weight distribution index is 2.4, the melting temperature is 238°C, and the isotacticity is 98%.

[0228] Example 29

[0229] The main catalyst of this embodiment is consistent with that of embodiment 1;

[0230] The catalyst of this embodiment uses compound P1 as the main catalyst and a composition of triphenylcarbonium tetrakis(pentafluorobenzene)borate and triisobutylaluminum (molar ratio of 1:450) as the activator. The activator is marked as A6. The main catalyst P1 and the activator A6 are compounded in a mass ratio of 1:1.5 to obtain catalyst C1-11.

[0231] The preparation steps of poly(4-methyl-1-pentene) in this example are basically the same as those in Example 1, except that catalyst C1-3 is replaced by catalyst C1-11.

[0232] The catalytic activity of catalyst C1-11 in this example is 6.9 kg polymer / (mmol Hf·h). The weight-average molecular weight of the prepared poly(4-methyl-1-pentene) is 402 kg / mol, the molecular weight distribution index is 4.0, the melting temperature is 239° C., and the isotacticity is 98%.

[0233] Example 30

[0234] The main catalyst of this embodiment is consistent with that of embodiment 1;

[0235] The catalyst of this embodiment is obtained by compounding the main catalyst P1 and the activator A3 in a molar ratio of 2:1. The obtained catalyst is marked as catalyst C1-12;

[0236] The preparation steps of poly(4-methyl-1-pentene) in this example are basically the same as those in Example 1, except that catalyst C1-3 is replaced by catalyst C1-12.

[0237] The catalytic activity of catalyst C1-12 in this example is 2.9 kg polymer / (mmol Hf·h). The weight-average molecular weight of the prepared poly(4-methyl-1-pentene) is 348 kg / mol, the molecular weight distribution index is 2.3, the melting temperature is 238°C, and the isotacticity is 98%.

[0238] Example 31

[0239] The main catalyst of this embodiment is consistent with that of embodiment 1;

[0240] The catalyst of this embodiment is obtained by compounding the main catalyst P1 and the activator A3 in a molar ratio of 1:7. The obtained catalyst is marked as catalyst C1-13;

[0241] The preparation steps of poly(4-methyl-1-pentene) in this example are basically the same as those in Example 1, except that catalyst C1-3 is replaced by catalyst C1-13.

[0242] The catalytic activity of catalyst C1-13 in this example is 9.9 kg polymer / (mmol Hf·h). The weight-average molecular weight of the prepared poly(4-methyl-1-pentene) is 301 kg / mol, the molecular weight distribution index is 3.0, the melting temperature is 238°C, and the isotacticity is 98%.

[0243] Example 32

[0244] The preparation of the catalyst and the catalyst were the same as those in Example 1.

[0245] The preparation steps of poly(4-methyl-1-pentene) in this example are basically the same as those in Example 1, except that 0.025 mL of 4-methyl-1-pentene monomer is added to the homopolymerization reaction (the molar ratio of 4-methyl-1-pentene monomer to catalyst C1-3 is 200:1).

[0246] The catalytic activity of catalyst C1-3 in this example is 0.6 kg polymer / (mmol Hf·h). The prepared poly(4-methyl-1-pentene) has a weight-average molecular weight of 324 kg / mol, a molecular weight distribution index of 2.0, a melting temperature of 234° C., and an isotacticity of 98%.

[0247] Example 33

[0248] The main catalyst and catalyst preparation of this embodiment are consistent with those of Example 1;

[0249] The preparation steps of poly(4-methyl-1-pentene) in this example are basically the same as those in Example 1, except that 7.5 mL of 4-methyl-1-pentene monomer is added to the homopolymerization reaction (the molar ratio of 4-methyl-1-pentene monomer to catalyst C1-3 is 60,000:1).

[0250] The catalytic activity of catalyst C1-3 in this example is 27.4 kg polymer / (mmol Hf·h). The weight-average molecular weight of the prepared poly(4-methyl-1-pentene) is 940 kg / mol, the molecular weight distribution index is 2.9, the melting temperature is 238° C., and the isotacticity is 97%.

[0251] Comparative Example 1

[0252] In this comparative example, a Ziegler-Natta catalyst (commercially available, with the product model CS-2) was used to catalyze the homopolymerization of 4-methyl-1-pentene. The specific steps are as follows:

[0253] A Schlenk flask equipped with a magnetic stirrer was continuously evacuated and dried using an infrared lamp for two hours. After natural cooling, the atmosphere was replaced with nitrogen three times to atmospheric pressure. 7 mL of toluene, 3 mL of 4-methyl-1-pentene, and 500 μmol of triethylaluminum were added sequentially, stirred, and the mixture was kept constant at 40°C in a water bath for half an hour. 20 mg of Ziegler-Natta catalyst was added to the reaction system and timed. After polymerization reached 2 hours, the reaction flask was opened and 10% hydrochloric acid-containing ethanol solution was added to terminate the polymerization. The mixture was stirred for 3 hours, filtered, washed three times with ethanol, and dried under vacuum to constant weight to obtain poly(4-methyl-1-pentene).

[0254] The catalytic activity of the Ziegler-Natta catalyst in this comparative example was 275 g polymer / (mmol Ti·h). The prepared poly(4-methyl-1-pentene) had a weight-average molecular weight of 1004 kg / mol, a molecular weight distribution index of 13.7, a melting temperature of 237° C., and an isotacticity of 96%.

[0255] Comparative Example 2

[0256] In this comparative example, a zirconocene catalyst was used to catalyze the homopolymerization of 4-methyl-1-pentene. The structural formula of the zirconocene catalyst is as follows:

[0257] The above catalyst can be prepared by referring to the method described in J. Mol. Catal. A 1996, 112: 37.

[0258] The specific steps of the homopolymerization reaction of this comparative example are as follows: a Schlenk flask equipped with a magnetic stirrer is continuously evacuated and dried with an infrared lamp for two hours. After natural cooling, the nitrogen is replaced three times to normal pressure. 7mL of toluene, 3mL of 4-methyl-1-pentene, and 20mmol of methylaluminoxane (MAO) are added in sequence, stirred, and the temperature is kept at 40°C in a water bath for half an hour. 10μmol of zirconocene catalyst is added to the reaction system and the reaction is timed. After polymerization reaches 7 hours, the reaction flask is opened and an ethanol solution acidified with 10% hydrochloric acid is added to terminate the polymerization. After stirring for 3 hours, the mixture is filtered, washed three times with ethanol, and vacuum dried to constant weight to obtain poly(4-methyl-1-pentene).

[0259] The catalytic activity of the zirconocene catalyst in this comparative example is 10.9 g polymer / (mmol Zr·h), and the prepared poly(4-methyl-1-pentene) has a weight-average molecular weight of 17 kg / mol, a molecular weight distribution index of 2.9, a melting temperature of 214° C., and an isotacticity of 90%.

[0260] Comparative Example 3

[0261] This comparative example uses a late transition metal nickel catalyst to catalyze the homopolymerization of 4-methyl-1-pentene. The structural formula of the catalyst is as follows:

[0262] The above catalyst can be prepared by the method described in Macromolecules 2000, 33, 2320.

[0263] The concrete steps of the homopolymerization of this comparative example are: the Schlenk bottle equipped with a magnetic stirrer is continuously vacuumized and dried with an infrared lamp for two hours. After natural cooling, the nitrogen is replaced three times to normal pressure. 7mL of toluene, 3mL of 4-methyl-1-pentene and 2.5mmol of diethylaluminum chloride are added successively, stirred, and the mixture is thermostated to 40 ℃ for half an hour with a water bath. 10μmol of a late transition metal nickel catalyst is added in the reaction system and timed. After polymerization reaches 1h, the reaction flask is opened and the ethanolic solution acidified with 10% hydrochloric acid is added to terminate the polymerization. After stirring for 3h, the mixture is filtered, washed with ethanol three times, and vacuum-dried to constant weight to obtain poly-(4-methyl-1-pentene).

[0264] The catalytic activity of the late transition metal nickel catalyst in this comparative example is 105 g polymer / (mmol Ni·h). The prepared poly(4-methyl-1-pentene) has a weight-average molecular weight of 175 kg / mol, a molecular weight distribution index of 1.5, no melting point, and is an atactic polymer with an isotacticity of less than 10%.

[0265] For the convenience of comparison, the catalytic activities of the catalysts prepared in the above examples and comparative examples and the weight average molecular weight, molecular weight distribution index, melting temperature and isotacticity of the prepared poly (4-methyl-1-pentene) are listed in Table 1.

[0266] In Table 1, M in the catalyst activity units of Examples 1 to 33 is Hf, in Comparative Example 1, M is Ti, in Comparative Example 2, M is Zr, and in Comparative Example 3, M is Ni.

[0267] Table 1

[0268] As can be seen from Table 1, the poly(4-methyl-1-pentene) obtained by using the imine-amine hafnium type catalyst of the present application has higher catalytic activity and a narrower molecular weight distribution than that of the Ziegler-Natta catalyst. It exhibits higher catalytic activity than the zirconocene catalyst, and the prepared poly(4-methyl-1-pentene) has a higher molecular weight and isotacticity. It exhibits higher catalytic activity than the late transition metal nickel catalyst, and the prepared polymer (4-methyl-1-pentene) has a higher isotacticity.

[0269] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some or all of the technical features therein. These modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application.

Claims

1. A main catalyst for preparing poly(4-methyl-l-pentene), wherein the main catalyst has a structure represented by Formula I:5 in which, Ri is selected from hydrogen or phenyl, and when Ri is selected from phenyl, Ri is fused with naphthalene ring in Formula I to form an anthracene ring; and R2 is selected from methyl or isopropyl.

2. A preparation method of the main catalyst for preparing poly(4-methyl-1-pentene) according to claim 1, comprising the following steps:1) reacting methyl glyoxal with 2,6-diisopropylaniline to obtain an intermediate A;2) reacting the intermediate A with a-naphthylamine or a-anthramine to obtain an intermediate B;3) reacting the intermediate B with a 2-position R2-displaced phenyl lithium15 compound to obtain an intermediate C;4) reacting the intermediate C with alkyl lithium and hafnium tetrahalide in sequence to obtain an intermediate D;5) reacting the intermediate D with methylmagnesium halide to obtain the main catalyst represented by Formula I.

3. The preparation method of the main catalyst for preparing poly(4-methyl-l-pentene) according to claim 2, wherein the alkyl lithium in step 4) is n-butyllithium; and / or,the hafnium tetrahalide in step 4) is hafnium tetrachloride; and / orthe methylmagnesium halide in step 5) is methylmagnesium bromide.

4. A catalyst for preparing poly(4-methyl-l-pentene), wherein the catalyst comprises an activator and the main catalyst according to claim 1.

5. The catalyst according to claim 4, wherein the activator is selected from a composition of trityl tetrakis (pentafluorophenyl) borate and alkyl aluminum.

6. The catalyst according to claim 5, wherein a molar ratio of the trityl tetrakis (pentafluorophenyl) borate to the alkyl aluminum in the composition is 1: (50-300).

7. The catalyst according to any one of claims 4-6, wherein a molar ratio of the main catalyst to the activator is 1: (1-5).

8. A preparation method of poly(4-methyl-l -pentene), wherein the preparation method comprises:catalyzing homopolymerization of 4-methyl-1 -pentene monomer using the catalyst according to any one of claims 5-7 to obtain the poly (4-methyl-l-pentene).

9. The preparation method according to claim 8, wherein a molar ratio of the 4-methyl-l -pentene monomer to the catalyst is (100-400,000):1.

10. The preparation method according to claim 9, wherein the molar ratio of the 4-methyl-l-pentene monomer to the catalyst is (10,000-100,000):1.

11. The preparation method according to any one of claims 8-10, wherein a temperature of the homopolymerization is 20-60°C.

12. The preparation method according to any one of claims 8-11, wherein the poly(4-methyl-l-pentene) has a weight average molecular weight of > 500,000, amolecular weight distribution index of < 4, an isotacticity of > 95% and a melting temperature of > 230°C.

13. The preparation method according to claim 12, wherein the poly(4-methyl-l-pentene) has the weight average molecular weight of 500,000 to 1,630,000, the 5   molecular weight distribution index of 2.0-4.0, the isotacticity of > 95% and the meltingtemperature of 230-240°C.

Citation Information

Patent Citations

  • Preparation method and application of amido-imine nickel vinyl polymerization catalyst

    CN102250152A

  • Ligand compound, transition metal compound, and catalyst composition comprising same

    CN113272310A

  • Pyridine amine hafnium compound as well as preparation method and application thereof

    CN113527351A

  • Pyridine amino hafnium compound as well as preparation method and application thereof

    CN113527352A

  • Substituted pyridyl amine ligands, complexes and catalysts therefrom; processes for producing polyolefins therewith

    WO2002038628A2