AQUEOUS DISPERSION OF POLYORGANOSILOXANE HYBRID RESIN.

IT202600041410T2Active Publication Date: 2026-10-07EVONIK OPERATIONS GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
IT502026000041410
Authority / Receiving Office
IT · IT
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-04-01
Filing Date
2020-03-17
Publication Date
2026-10-07
Estimated Expiration
2040-03-17
Patent Text Reader

Abstract

The invention relates to an aqueous polyorganosiloxane hybrid resin dispersion comprising - at least one polyorganosiloxane hybrid resin, - at least one emulsifier based on partially hydrolyzed polyvinyl acetates, - wherein it has a solids content of 30.0 wt.% - 70.0 wt.%, preferably 45.0 wt.% - 55.0 wt.%, based on the polyorganosiloxane hybrid resin dispersion and the residual solvent content is < 6.0 wt.%, preferably < 2.5 wt.%, particularly preferably < 1.0 wt.%, based on the polyorganosiloxane hybrid resin dispersion.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to aqueous polyorganosiloxane hybrid resin dispersions, their manufacturing process and use.

[0002] Pure silicone resins, also known as polyorganosiloxanes, are known for their thermal and weather stability. They are used for impregnation of concrete, in high-temperature-resistant coatings, and in weather-resistant exterior coatings. To increase the durability of polyorganosiloxanes, they are modified with other polymers. The chemical bonding of the silicone resins with these polymers occurs in an early stage of the manufacturing process.

[0003] Well-known organically modified polyorganosiloxane resins, hereinafter referred to as polyorganosiloxane hybrid resins, include silicone alkyd resins, silicone polyester resins, silicone-epoxy hybrid resins, silicone polyurethane resins, and silicone polyacrylate resins. These resins combine the positive properties of pure silicone resins, such as temperature resistance, weather resistance, and low surface tension, with the positive properties of, for example, polyesters, such as low thermoplasticity, high elasticity, and good pigment wetting.

[0004] The properties of silicone polyester resins prove particularly advantageous in the decorative coating of thermally stressed household appliances such as toasters, basking lamp housings, fan heaters, and cookers, as well as in the external coating of deep fryers, pots, and pans. Coatings of household items must also be detergent-resistant. This means they must withstand the now-common cleaning process in dishwashers, in the presence of surfactant-containing and highly alkaline detergents, without sustained damage. The detergent resistance of a coating is generally determined by the coating formulation, but especially by the resin used.

[0005] The properties of epoxy resins can also be combined with those of silicone resins. These silicone-epoxy hybrid resins, compared to pure silicone resins, are characterized by improved metal adhesion and corrosion protection, as well as better resistance to chemicals. Typical applications include exhaust coatings, but also coating systems for ceramic substrates such as all types of stoneware or concrete. Such coating systems are also used in the maritime sector, for example, for coating ship hulls, marine underwater and above-sea installations, and port facilities.

[0006] Polyorganosiloxane hybrid resins are typically supplied in an organic solvent, such as aromatic hydrocarbons, esters, ethers, or ketones, e.g., xylene, toluene, Solvesso, and methoxypropyl, ethyl, and butyl acetate. The advantages of solvent-based formulations lie in their ease of application, good flow properties, and the formation of an initial film on the substrate. The polyorganosiloxane hybrid resin films can be physically dried, reactively cured as a two-component system, or baked on. Room-temperature curing systems are also available.

[0007] However, solvent-based systems have toxicological and environmental disadvantages. The high content of flammable and sometimes harmful solvents is increasingly being assessed critically from the perspectives of occupational safety, health, and environmental protection. Furthermore, the use of solvents is increasingly subject to legal regulations worldwide. In many cases, environmental labels (Blue Angel, Nordic Swan, etc.) or industry standards along the value chain (RAL, IKEA, etc.) also require the complete elimination or drastic reduction of solvents.

[0008] Therefore, the search is consistently on for low-solvent or completely solvent-free systems. Numerous solutions for pure silicone resins, so-called polyorganosiloxanes, are described in the state of the art.

[0009] EP 098 940 describes a process in which a liquid oligomeric siloxane is emulsified with polyvinyl alcohol or a cellulose ether, and the liquid oligoorganosiloxane then condenses within this emulsion to form a highly viscous or solid polyorganosiloxane. The disadvantages of this process include the additional technological effort required, as the synthesis of the liquid oligomeric siloxane demands a different technology than the synthesis of polymeric organosiloxanes, and the condensation within the emulsion is difficult to control.

[0010] DE 21 58 348 describes a process for producing emulsions based on highly viscous siloxanes that can be crosslinked to form rubbers. In this process, a highly diluted preemulsion containing at least 150% water and at least 80% emulsifier (based on the siloxane content) is prepared, and this emulsion is then concentrated by distilling off a solvent / water mixture. This process requires a comparatively high amount of emulsifier, which is undesirable in many applications due to the significant alteration of the application profile and also increases costs. The maximum siloxane content is 45%, and 5 to 7% solvent remains in the emulsion.

[0011] DE 44 15 322 A1 describes a process for producing aqueous silicone resin emulsions using a polymeric organosilicon compound dissolved in an organic solvent such as toluene. After adding an emulsifier mixture consisting of an ethoxylated triglyceride and an ethoxylated tridecyl alcohol and water to the polymeric organosilicon compound, and achieving a homogeneous, non-flowing mixture, the organic solvent is separated as a solvent / water mixture. Subsequently, the amount of water required to achieve the desired final concentration, as well as any known additives, are homogeneously incorporated. This document provides no indication that this process is suitable for resins other than the polyorganosiloxanes described, such as polyorganosiloxane hybrid resins.

[0012] Further information from the prior art includes WO 2015 / 091901, which describes an aqueous dispersion of silicone-modified polyester resins. However, due to the process described in the document, the residual solvent content of the aqueous dispersion, relative to the solids content of the silicone-modified polyester resin in the dispersion, cannot be less than 6 wt%. This disadvantage was demonstrated in the comparative example.

[0013] The present invention was therefore based on the objective of providing an aqueous polyorganosiloxane hybrid resin dispersion that can be used in various coatings without significantly impairing the other coating properties and the utility for the respective application, and that the residual solvent content in relation to the solids content is lower than is known in the prior art.

[0014] Surprisingly, the problem could be solved by an aqueous polyorganosiloxane hybrid resin dispersion according to claim 1.

[0015] Surprisingly, it was found that the dispersion according to the invention has a residual solvent content of < 6.0 wt.%, preferably < 2.5 wt.%, particularly preferably < 1.0 wt.%, based on the polyorganosiloxane hybrid resin dispersion at a solids content of 30.0 wt.% - 70.0 wt.%, preferably 45.0 wt.% - 55.0 wt.%, based on the polyorganosiloxane hybrid resin dispersion.

[0016] The solid content selected according to the invention is particularly advantageous because it reflects the user's wishes regarding storage stability, quantity used and freedom in formulation and application.

[0017] In a comparative example, it was demonstrated that dispersions produced according to the process in WO 2015 / 091901 achieve a maximum residual solvent content of 6 wt.% with a solids content of 30.0 wt.% based on the polyorganosiloxane hybrid resin dispersion. If the solids content is increased, the residual solvent content in the dispersion also increases.

[0018] According to the invention, the solid content consists of polyorganosiloxane hybrid resin and emulsifier.

[0019] For the purposes of this invention, solvents and solvents are used synonymously.

[0020] Another advantage of the invention is the aspect of occupational safety. Even when using products containing small amounts of flammable solvent, some basic occupational safety measures are necessary. The flash point is an important factor for taking precautions. To avoid fire and explosion hazards, solvent-based products with a high flash point are preferred over those with a low flash point.

[0021] Surprisingly, it was found that the dispersion according to the invention contributes to occupational safety. This is because the lower the residual solvent content in the dispersion, the higher the flash point.

[0022] Preferably, the polyorganosiloxane hybrid resin dispersion according to the invention has a flash point of > 30.0°C, preferably > 60.0°C and particularly preferably > 90.0°C, according to the method described in this application.

[0023] In principle, experts distinguish between secondary and primary aqueous polymer dispersions. Secondary dispersions are produced from polymers that are manufactured conventionally and then, in a subsequent step, converted from solution or melt into aqueous dispersion. Primary dispersions, on the other hand, are those in which the polymer is directly produced in a dispersed distribution within the aqueous dispersion medium in the presence of an emulsifier. All manufacturing processes essentially share the characteristic that monomers are used in the polymer structure or that this structure is formed exclusively from such monomers.

[0024] EP 0 008 090 A1 describes a process for producing a water-miscible silicone-polyester resin, in which the stable dispersion is based on the use of an "acidified" polyester during the production of the silicone-polyester resin. Besides the very complex process, there is also the risk of the polyester being broken down back into its original form (acid ester hydrolysis) due to the acid numbers of 25–110 required in this process.

[0025] The requirements for a reduction in solvent emissions can be met with the aqueous polyorganosiloxane hybrid resin dispersion according to the invention.

[0026] Preferably, the polyorganosiloxane hybrid resin is a polyorganosiloxane modified with an organic polymer.

[0027] The polyorganosiloxane hybrid resin is particularly preferably a reaction product of a composition containing Component A) 5 to 95 parts by weight, preferably 10 to 70 parts by weight of one or more polyorganosiloxanes of the general formula R a Si(OR') b O (4-ab / 2) formula (I) with 0 <a<2, 0<b<2 und a+b<4, optional Komponente B) 0 - 20 Gew.-Teile, bevorzugt 1 -10 Gew.-Teile eines oder mehrerer linearer und / oder verzweigter Polyorganosiloxane der Formel          R"O-[R"' 2 Si-O] n -     Formel (II) Komponente C) 5 bis 95 Gew.-Teile, bevorzugt 30 bis 90 Gew.-Teile eines organischen Polymers, where R a , R', R" and R'" each independently represent an alkyl group with 1 to 8 C atoms or an aromatic group with 6 to 20 C atoms, and n represents a number in the range of 4 to 250.

[0028] The polyorganosiloxane hybrid resins can be produced in a known manner. Common processes can be found in DE 10 2013 218976 A1, DE 10 2013 218981 A1, US 3,154,597, or US 3,170,962. Those skilled in the art will be familiar with further literature, such as "Silicone resins and their combination" by Wernfried Heilen, Chapter 2.2 Silicone combination resins / silicone resin hybrids, 2015, or "High Silicones and Silicone-Modified Materials strength Silicone-Urethane Copolymers: Synthesis and Properties," Chapter 26, pp. 395-407.

[0029] For example, either a polyorganosiloxane is reacted with a hydroxy group-containing organic polymer, or the organic polymer is produced in the presence of the polyorganosiloxane by suitable monomers, or an organic polymer with alkoxysilane functionality is produced by hydrolysis / condensation or equilibration with alkoxysilane monomers or siloxane oligomers.

[0030] Preferably, the polyorganosiloxane is a linear, simply or multiply branched Si-OH or SiOR 3< functional polyorganosiloxane.

[0031] Polyorganosiloxanes are also referred to in the literature as siloxane oligomers, alkoxy-functional methyl, phenyl and methyl / phenyl siloxanes, hydroxy-functional methyl, phenyl and methyl / phenyl silicone resins or silanols.

[0032] Alkoxy-functional methyl, phenyl, and also methyl / phenyl siloxane oligomers are available from ShinEtsu, among others under the trade names KC-89S, KR-500, X 40-9225, X 40-9246, X 40-9250, KR-401N, X-40-9227, KR-510, KR-9218, KR-213.

[0033] Methoxy-functional methyl, phenyl, and methyl / phenyl siloxanes are available from Dow Corning under the trade names Dow Corning® US-CF 2403 Resin, US-CF 2405 Resin, 3037 Intermediate, 3074 Intermediate, and RSN-5314 Intermediate. Silanol-functional methyl / phenyl resins are marketed under the trade names RSN-0409 HS Resin, RSN-0431 HS Resin, RSN-0804 Resin, RSN-0805 Resin, RSN-0806 Resin, RSN-0808 Resin, and RSN-0840 Resin.

[0034] Alkoxy-functional methyl / phenyl, phenyl and methyl silicone resins, which are also offered hydrolyzed to the corresponding silanol, are available under the trade name SILRES® from Wacker Chemie, such as with the additional designations REN 50, REN 60, REN 80, KX, HK 46, MSE 100 or SY 300, IC 836, REN 168, SY 409, IC 232, SY 231, IC 368, IC 678.

[0035] The production of such silicone resins has long been known in the literature (see W. Noll - Chemie und Technologie der Silicone, Wiley-VCH Verlag GmbH & Co. KGaA, Weinheim, 1960) and is also described in the German patent DE 34 12 648.

[0036] Preferably, the organic polymer is polyepoxides, polyesters, polyacrylates and / or methacrylates and copolymers thereof, polyurethanes, cellulose derivatives, polysulfones, polyethersulfones, polyphenylene sulfides and oxides, polyamides, polyamide-imide, polyimides, polyethers, aromatic and aliphatic glycidyl-functional polymers, oligomers, phenoxy resins, polycarbonates, ketone formalaldehyde resins, polyvinyl resins selected from polyvinyl alcohol, polyglycerols, polyvinyl acetate, their (partial) hydrolysates and derivatives, phenolic resins, fluoropolymers, alkyd resins and mixtures thereof.

[0037] Preferably, polyesters are used, selected from the reaction products of aromatic and / or aliphatic and / or cycloaliphatic monocarboxylic acids and / or dicarboxylic acids and / or polycarboxylic acids as well as their anhydrides and / or esters with linear and / or branched, aliphatic and / or cycloaliphatic and / or aromatic diols and / or polyols. Examples of common carboxylic acids are phthalic acid, phthalic anhydride, dimethyl terephthalate, isophthalic acid, terephthalic acid, 1,4-cyclohexanedicarboxylic acid, succinic acid, succinic anhydrides, sebacic acid, maleic acid, maleic anhydride, fumaric acid, methyltetrahydrophthalic acid, methyltetrahydrophthalic anhydride, methylhexahydrophthalic acid, methylhexahydrophthalic anhydride, hexahydrophthalic acid, tetrahydrophthalic acid, dodecanedioic acid, adipic acid, azelaic acid, isononanic acid, 2-ethylhexanoic acid, pyromellitic acid, pyromellitic dianhydride, and trimellitic acid.and / or trimellitic anhydride. Examples of common diols and / or polyols are ethylene glycol, 1,2- and / or 1,3-propanediol, diethylene, dipropylene, triethylene, tetraethylene glycol, 1,2- and / or 1,4-butanediol, 1,3-butylethylpropanediol, 1,3-methylpropanediol, 1,5-pentanediol, cyclohexanedimethyl, glycerol, hexanediol, neopentyl glycol, trimethylolethane, trimethylolpropane and / or pentaerythritol, as well as bisphenol A, B, C, F, norbornylene glycol, 1,4-benzyldimethanol and benzyldimethyl, and 2,4-dimethyl-2-ethylhexane-1,3-diol.

[0038] Epoxy resins with at least two 1,2-epoxy groups per molecule are preferably used. Examples of suitable epoxy resins are aliphatic or aromatic epoxides: Eponex® and EPON® resins from Hexion, Epalloy® resins from Emerald Performance Materials Company, Epotec® resins from Aditya Birla Chemicals, Denacol® resins from Nagase ChemteX, Araldite® resins from Huntsman, Beckopox® from Allnex, and VORAFORCE® resins from Dow Chemical Company.

[0039] The various fragments of the siloxane chains specified in formula (I) and formula (II) can be statistically distributed. Statistical distributions can be block-based with any number of blocks and any sequence, or subject to a randomized distribution; they can also be alternating or form a gradient along the chain; in particular, they can also form any combination thereof.

[0040] The index numbers and value ranges of the specified indices presented here can be understood as mean values ​​of the possible statistical distribution of the actual existing structures and / or their mixtures. This also applies to structural formulas that are reproduced exactly as such, such as formula (I).

[0041] In the context of this invention, the term "poly" encompasses not only compounds with at least three repeating units of one or more monomers in the molecule, but also, in particular, compositions of compounds that exhibit a molecular weight distribution and have an average molecular weight of at least 200 g / mol. This definition takes into account the fact that, in the relevant field of technology, it is common practice to refer to such compounds as polymers, even if they do not appear to meet a polymer definition analogous to OECD or REACH directives.

[0042] Unless otherwise stated, percentages are given as weight percentages.

[0043] If measured values ​​are given below, these measurements were carried out under standard conditions (25 °C and 1013 mbar), unless otherwise stated.

[0044] Unless otherwise stated, where average values ​​are given below, they are weight averages.

[0045] The organic polymer preferably contains hydroxyl groups and / or acidic hydrogens.

[0046] Preferably, the emulsifiers are partially hydrolyzed polyvinyl acetates with a degree of alcoholysis between 10% and 99% (mol / mol), preferably between 50% and 95% (mol / mol), and particularly preferably between 70% and 90% (mol / mol).

[0047] Preferably, the partially hydrolyzed polyvinyl acetates have a viscosity, measured in a 4% aqueous polyvinyl acetate solution at 20°C according to DIN 53015, of 1 - 50 mPa s, preferably 1 - 40 mPa s and particularly preferably 1 - 30 mPa s.

[0048] Preferably, the emulsifier does not contain any bound silane.

[0049] It is also conceivable to use the emulsifiers according to the invention together with other emulsifiers, such as anionic, cationic, or non-ionic emulsifiers. If several emulsifiers are used, they are referred to as an emulsifier system in the present invention.

[0050] Preferably, the weight ratio of polyorganosiloxane hybrid resin to emulsifier or emulsifier system is between 5 and 50, more preferably between 7 and 40, and particularly preferably between 10 and 30.

[0051] If necessary, the polyorganosiloxane hybrid resin dispersion preferably comprises further additives selected from defoamers, deaerators, rheology additives, preservatives, substrate wetting agents, crosslinkers, drying aids, catalysts, antioxidants, skin-preventing agents, anti-segregation agents, thickeners, coalescing agents, film-forming aids, fillers, pigments and / or dispersing agents.

[0052] Preferably, the pigments are organic, inorganic, or carbon black. Examples of inorganic pigments include iron oxides, chromium oxides, and titanium oxides. Suitable organic pigments include azo pigments, metal complex pigments, anthraquinoid pigments, phthalocyanine pigments, and polycyclic pigments, particularly those of the thioindigo, quinacridone, dioxazine, pyrrolopyrrole, napthalenetetracarboxylic acid, perylene, isoamidolin(one), flavanthrone, pyranthrone, or isoviolanthrone series. Carbon blacks such as gas blacks, flame blacks, or furnace blacks can be used. These carbon blacks may be further oxidized and / or pearled.

[0053] Optionally, further additives can be added. An additive is defined as any component that positively influences the properties of the dispersion according to the invention. One or more additives can be added independently of one another. Some additives that can be used for the dispersion according to the invention are listed below. This list is not exhaustive: Wetting and dispersing additives are particularly advantageous. A large number of wetting and dispersing additives are available on the market that can be used for the dispersions according to the invention. These dispersing additives are derived, for example, from polymer classes well known in the prior art, such as styrene-maleic anhydride copolymers, acrylates, polyethers (e.g., styrene oxide polyethers), polyesters, amino polyesters, polyurethanes, and amino polyethers.The additives can have different topologies, for example, linear, branched, comb-like, or star-shaped. Typically, network and dispersing additives have a heterogeneous structure, which is divided into a binding group and a stabilizing side chain.

[0054] In addition to pigments, fillers can also be used in the dispersions according to the invention. Suitable fillers are, for example, those based on kaolin, talc, mica, other silicates, quartz, cristobalite, wollastonite, perlite, diatomaceous earth, fiber fillers, aluminum hydroxide, barium sulfate, glass, or calcium carbonate.

[0055] The use of a defoamer or deaerator can be advantageous for actively reducing the amount of air introduced during processing or manufacturing. Examples include those based on mineral or vegetable oils, or on polyethersiloxanes, some of which contain particulate components such as silica. Other additives include binders, colorants, surface additives, compatibilizers, wetting and spreading agents, crosslinking agents, rheology additives, thickeners, UV stabilizers, and preservatives.

[0056] Preferably, fungicides, bactericides, pesticides, algicides and / or herbicides are used as preservatives.

[0057] Preferably, the mean volume-weighted diameter of the polyorganosiloxane hybrid resin particles is between 0.1 and 10.0 µm, more preferably between 0.1 and 2.0 µm, particularly preferably between 0.2 and 1.0 µm, and most preferably between 0.2 and 0.7 µm, measured according to ISO 13320:2009. For the present invention, the mean volume-weighted diameter of the particles was determined using a Coulter LS 13320 instrument from Beckman Coulter.

[0058] Preferably, the polyorganosiloxane hybrid resin dispersion has a solids content of 30.0 wt.% - 70.0 wt.%, preferably 45.0 wt.% - 55.0 wt.%, based on the dispersion.

[0059] Another object of the invention is a process for producing aqueous polyorganosiloxane hybrid resin dispersion comprising the steps a. Emulsifying a polyorganosiloxane hybrid resin solution containing an organic solvent with an emulsifier solution comprising at least one emulsifier based on partially hydrolyzed polyvinyl acetates and b. separating the solvent.

[0060] Preferably, water is added in step a). This allows, for example, the solids content to be determined in this step or at least to be set within a desired solids content range.

[0061] Preferably, the solids content for the aqueous polyorganosiloxane hybrid resin dispersion can be adjusted after step b).

[0062] Particularly preferably, in step a) a desired solids content range can be specified and in step b) the solids content of the aqueous polyorganosiloxane hybrid resin dispersion according to the invention can be adjusted.

[0063] The method according to the invention thus enables an elegant manufacturing method with which the solids content can be predetermined at the outset. Fine-tuning can be carried out subsequently if necessary.

[0064] Preferably, partially hydrolyzed polyvinyl acetates with a degree of alcoholysis between 10% and 99% (mol / mol), preferably between 50% and 95% (mol / mol), and particularly preferably between 70% and 90% (mol / mol) are used.

[0065] Preferably, the emulsifier does not contain any bound silane.

[0066] Preferably, the partially hydrolyzed polyvinyl acetates have a viscosity, measured in a 4% aqueous polyvinyl acetate solution at 20°C according to DIN 53015, of 1 - 50 mPa s, preferably 1 - 40 mPa s and particularly preferably 1 - 30 mPa s.

[0067] Such emulsifiers are available, for example, under the brand names Mowiol, Elvanol or Poval (Kuraray), Gohsenol (Nippon Gohsei), Selvol (Sekisui), and Polyviol (Wacker).

[0068] Preferably, further emulsifiers selected from the group of anionic, cationic, zwitterionic or non-ionic emulsifiers may be used.

[0069] The polyorganosiloxane hybrid resin used preferably consists of reaction products of a composition containing Component A) 5 to 95 parts by weight, preferably 10 to 70 parts by weight of one or more polyorganosiloxanes of the general formula R a Si(OR') b O (4-ab / 2) formula (I) with 0 <a<2, 0<b<2 und a+b<4, optional Komponente B) 0 - 20 Gew.-Teile, bevorzugt 1 -10 Gew.-Teile eines oder mehrerer linearer und / oder verzweigter Polyorganosiloxane der Formel          R"O-[R"' 2 Si-O] n -     Formel (II) Komponente C) 5 bis 95 Gew.-Teile, bevorzugt 30 bis 90 Gew.-Teile eines organischen Polymers, where R a , R', R" and R'" each independently represent an alkyl group with 1 to 8 C atoms or an aromatic group with 6 to 20 C atoms, and n represents a number in the range of 4 to 250.

[0070] Preferably, the polyorganosiloxane is a linear, singly or multiply branched Si-OH or SiOR3< functional polyorganosiloxane. Commercially available polyorganosiloxanes are described above.

[0071] Preferably, the organic polymer is polyepoxides, polyesters, polyacrylates and / or methacrylates and copolymers thereof, polyurethanes, cellulose derivatives, polysulfones, polyethersulfones, polyphenylene sulfides and oxides, polyamides, polyamide-imide, polyimides, polyethers, aromatic and aliphatic glycidyl-functional polymers, oligomers, phenoxy resins, polycarbonates, ketone formalaldehyde resins, polyvinyl resins selected from polyvinyl alcohol, polyglycerols, polyvinyl acetate, their (partial) hydrolysates and derivatives, phenolic resins, fluoropolymers, alkyd resins and mixtures thereof.

[0072] Particularly preferably, the organic polymer is an organic polymer containing hydroxyl groups, preferably selected from the group consisting of polyepoxides, polyesters, polyacrylates, polymethacrylates, polyurethanes and cellulose derivatives.

[0073] Preferably, polyesters are used, selected from the reaction products of aromatic and / or aliphatic and / or cycloaliphatic monocarboxylic acids and / or dicarboxylic acids and / or polycarboxylic acids as well as their anhydrides and / or esters with linear and / or branched, aliphatic and / or cycloaliphatic and / or aromatic diols and / or polyols. Examples of common carboxylic acids are phthalic acid, phthalic anhydride, dimethyl terephthalate, isophthalic acid, terephthalic acid, 1,4-cyclohexanedicarboxylic acid, succinic acid, succinic anhydrides, sebacic acid, maleic acid, maleic anhydride, fumaric acid, methyltetrahydrophthalic acid, methyltetrahydrophthalic anhydride, methylhexahydrophthalic acid, methylhexahydrophthalic anhydride, hexahydrophthalic acid, tetrahydrophthalic acid, dodecanedioic acid, adipic acid, azelaic acid, isononanic acid, 2-ethylhexanoic acid, pyromellitic acid, pyromellitic dianhydride, and trimellitic acid.and / or trimellitic anhydride. Examples of common diols and / or polyols are ethylene glycol, 1,2- and / or 1,3-propanediol, diethylene, dipropylene, triethylene, tetraethylene glycol, 1,2- and / or 1,4-butanediol, 1,3-butylethylpropanediol, 1,3-methylpropanediol, 1,5-pentanediol, cyclohexanedimethyl, glycerol, hexanediol, neopentyl glycol, trimethylolethane, trimethylolpropane and / or pentaerythritol, as well as bisphenol A, B, C, F, norbornylene glycol, 1,4-benzyldimethanol and benzyldimethyl, and 2,4-dimethyl-2-ethylhexane-1,3-diol.

[0074] Epoxy resins with at least two 1,2-epoxy groups per molecule are preferably used. Examples of suitable epoxy resins are aliphatic or aromatic epoxides: Eponex® and EPON® resins from Hexion, Epalloy® resins from Emerald Performance Materials Company, Epotec® resins from Aditya Birla Chemicals, Denacol® resins from Nagase ChemteX, Araldite® resins from Huntsman, Beckopox® from Allnex, and VORAFORCE® resins from Dow Chemical Company.

[0075] Preferably, the solvent is an organic solvent or mixtures thereof that were used in the manufacture of the polyorganosiloxane hybrid resin.

[0076] Preferably, the solvent can also be a semi-organic solvent.

[0077] Preferably, a solvent from the group of ketones selected from methyl ethyl ketone, acetone, methyl isobutyl ketone, diethyl ketone, methyl propyl ketone, cyclohexanone, or methylcyclohexanone; esters selected from ethyl acetate, butyl acetate, ethyl propionate, isobutyl acetate, or tert-butyl acetate; carbonates, for example, dialkyl carbonates or cyclic carbonates such as ethylene, propylene, or glycerol carbonate; aromatic hydrocarbons, for example, xylene; cyclic hydrocarbons, for example, cyclohexane; crown ethers or ethers such as dibutyl ether; ester ethers, for example, methoxypropyl acetate; siloxanes, for example, hexamethyldisiloxane, octamethylcyclotetrasiloxane, or decamethylcyclopentasiloxane; or organometallic germanium compounds, for example, tetramethylgermanium, are used. It is conceivable to use other solvents known to those skilled in the art or mixtures of different solvents.

[0078] Particularly preferably, the organic solvent or mixtures thereof has a boiling point range of 50°C - 150°C, preferably 90°C - 120°C, at normal pressure or 1013 mbar.

[0079] Preferably, the solvent is separated by distillation at reduced pressure with or without stripping gas, by steam distillation, by means of a (diffusion) membrane process or a thin-film evaporator.

[0080] Preferably, the polyorganosiloxane hybrid resin solution has a polyorganosiloxane hybrid resin concentration of 40.0 wt.% - 95.0 wt.%, preferably 60.0 wt.% - 70.0 wt.%, based on the polyorganosiloxane hybrid resin solution.

[0081] Preferably an aqueous emulsifier solution or an aqueous emulsifier system solution is used, wherein its concentration is between 5 - 40 wt.%, preferably 10 - 30 wt.%, particularly preferably 15 - 25 wt.% based on the emulsifier solution.

[0082] The process according to the invention differs from the process according to WO 2015 / 091901 in that the solvent removal takes place in the presence of the emulsifier solution. It was surprising that the solvent could be significantly removed from the polyorganosiloxane hybrid resin. Regardless of the initial solvent concentration of the polyorganosiloxane hybrid resin, low residual solvent concentrations could be generated without impairing the stability and thus the processability of the polyorganosiloxane hybrid resin dispersion.

[0083] The process according to WO 2015 / 091901 describes, in the first step, the removal of the solvent from a silicone-polyester hybrid resin, in the second step the homogenization of the still processable resin with a concentrated emulsifier solution, and in the third step the dispersion by adding water to produce the dispersion. The document is silent on the temperature and duration of the first step. Thus, the advantage of the process according to the invention also lies in the reduction of the production steps, which leads to time savings.

[0084] Another object of the invention is therefore also the aqueous polyorganosiloxane hybrid resin dispersion produced according to the inventive method.

[0085] Another advantage of the process according to the invention is the increase in the flash point of an aqueous polyorganosiloxane hybrid resin dispersion produced according to the process according to the invention.

[0086] The use of the polyorganosiloxane hybrid resin dispersion according to the invention in coating materials, as well as varnishes and paints, substrate coatings, adhesives, structural adhesives, compounding matrices and sizing agents is also an object of the invention. Further areas of application include the production of printing inks or 3D printing materials.

[0087] Substrates according to the invention, in particular baking trays, baking molds, pans, metal pots and the like, coated with a composition containing a polyorganosiloxane hybrid resin dispersion according to the invention, are also included. Substrates are preferably ceramic, polymeric or metallic substrates.

[0088] The objects according to the invention are described below by way of example, without the invention being limited to these exemplary embodiments. Methods: Measurement of particle size

[0089] The particle size of the dispersions was determined according to ISO 13320:2009. A Beckman-Coulter LS13320 instrument was used. The particle size was calculated assuming a refractive index nd = 1.51. The calculated mean particle diameter is volume-weighted. Determination of the solid state:

[0090] The determination of the content of non-volatile components is carried out in accordance with DIN EN ISO 3251:2008, whereby, within the scope of the present invention, the testing of the polyorganosiloxanes and the polyorganosiloxane hybrid resin solutions is carried out for 60 minutes at 180°C for the determination of the solids and for 60 minutes at 105°C for the dispersion. Viscosity determination

[0091] Unless otherwise specified, viscosity was determined using a Brookfield LV-DV-I+ spindle viscometer. Brookfield viscometers are rotational viscometers with defined spindle sets as rotating bodies. The rotating bodies used were an LV spindle set. Due to the temperature dependence of viscosity, the temperatures of the viscometer and the sample liquid were kept constant to within ±0.5 °C during the measurement. In addition to the LV spindle set, other materials used included a thermostatically controlled water bath, a thermometer (0-100 °C, scale increments of 1 °C or less), and a timer (scale increments no greater than 0.1 seconds). For the measurement, 100 ml of the sample was placed in a wide-mouth bottle, pre-calibrated, and measured at temperature to ensure it was free of air bubbles.To determine the viscosity, the viscometer was positioned relative to the sample so that the spindle was immersed in the product up to the mark. The measurement was initiated using the start button, ensuring that the measurement was taken within the optimal measuring range of 50% (+ / - 20%) of the maximum measurable torque. The measurement result was displayed on the viscometer in mPas, and dividing this by the density (g / ml) yields the viscosity in mm² / s. Residual solvent content

[0092] The determination of the residual solvent content was carried out in accordance with the European Pharmacopoeia 5.4 Residual solvents. Pendulum hardness according to König

[0093] In the König pendulum hardness test (DIN 53157 or EN ISO 1522), the damping of an oscillating pendulum serves as the measure. The pendulum, with two stainless steel balls, is placed on a coating film. There is a physical relationship between the duration of the pendulum's oscillation, its amplitude, and its geometric dimensions. The viscoelastic behavior of the coating is crucial for its hardness. When the pendulum is set in motion, the balls roll on the surface, exerting pressure upon it. The degree of rebound depends on the coating's elasticity. A lack of elastic forces results in strong damping of the pendulum's motion. Conversely, high elastic forces cause only slight damping. Pendulum hardness according to "König": Number of oscillations in oscillations: 1 oscillation = 1.4 seconds Further conditions

[0094] Unless otherwise stated, percentages given in the context of the present invention are expressed as percentages by weight. In the case of compositions, percentages refer to the total composition unless otherwise stated. Where average values ​​are given in the following examples, these are numerical averages unless otherwise stated. Where measured values ​​are given below, these were obtained at a pressure of 101,325 Pa, a temperature of 23 °C, and an ambient relative humidity of approximately 40% unless otherwise stated. Determination of the flash point:

[0095] The flash point was determined using a closed-cup flash point tester according to the Pensky-Martens method, based on DIN EN ISO 2719.

[0096] The Pensky-Martens closed-cup flash point tester measures the flash point. This measures the lowest temperature at which an ignition source ignites the vapor phase of a sample.

[0097] 70 mL of each of the dispersions according to the invention from Table 5 were used. Before measurement, the samples were pretreated as follows: Dispersions with a residual solvent content > 2.0 wt% were cooled to 10 °C and measured immediately. Dispersions with a residual solvent content ≤ 2.0% were cooled to 15 °C.

[0098] All dispersions were adjusted to a solids content of 50 wt.%

[0099] A heating rate of 1.5 °C / min and a stirring speed of 120 rpm were selected. The atmospheric pressure was 994 mbar. No conversions were performed, as the correction is smaller than the measurement uncertainty. Materials and equipment:

[0100] Glass plates, Gläserei Glänzer, dimensions: 90 x 150 x 5 mm; PVC sheets, material no.: 4364002858, KVG Kunststoff Betriebs GmbH; 300 µm box doctor blade, Simex; 300 µm cube doctor blade, TQC GmbH; Dispermat, VMA Getzmann with Teflon disc; wide-mouth glass bottles; flash point tester with closed crucible - PMA 4 (semi-automatic), Petrotest; Silikopon® EW, Evonik Industries; Poval® 04-88, Kuraray; Poval® 03-80, Kuraray; Poval® 18-88, Kuraray; Gohsenol® KL-03, Nippon Gohsei; Gohsenol® KL-05, Nippon Gohsei; Tergitol® 15-S-5, DOW Chemical Examples Production of aqueous polyorganosiloxane hybrid dispersions according to the invention

[0101] To produce the aqueous polyorganosiloxane hybrid dispersion according to the invention, a solvent-based polyorganosiloxane hybrid solution is first prepared. The solvent is then removed using the process according to the invention. 1. Preparation of a solvent-based polyorganosiloxane hybrid solution with polyester (for simplicity, this will be referred to as a silicone-polyester hybrid solution below) 1.1 Production of a polyorganosiloxane as component A

[0102] Solvents used: Methyl isobutyl ketone (MIBK), diethyl carbonate (DEC), methyl propyl ketone (MPK), ethyl acetate (EtAc), isobutyl acetate (iBuAc), ethyl isobutyrate (EtiBu). Initially, three polyorganosiloxanes POS 1, POS 2, and POS 3 were prepared according to EP 0 157 318 with the parameters listed in Table 1. POS 4 is a commercially available polyorganosiloxane from Dow Corning. Table 1: Designation Chemical name alkoxy content [%] Viscosity [mPas] solvent Festive meal per [%] POS 1 Phenylmethylmethoxypolysiloxane 14,7 1760 - 95,7 POS 2 Phenylmethoxy polysiloxane 17,4 4470 - 98,4 POS 3 Phenylmethylethoxypolysiloxane 15,1 450 MIBK 90,2 POS 4 Dow Corning® 3074 16,8 184 - 88,4 1.2 Production of a hydroxy-functional polyester as component C

[0103] The hydroxy-functional polyesters PES 1 - PES 5 were produced according to a process described in DE 37 28 414 C1 by esterification of trimethylolpropane, isophthalic acid, and ethylene glycol. The solids content and viscosity were adjusted using the solvents listed in Table 2. Table 2: Designation: Polymer solution solvent Viscosity [mPas] Solids [%] PES 1 EtiBu 5930 70,2 PES 2 DEC 6270 71,5 PES 3 MPK 730 68,8 PES 4 MIBK 860 70,4 PES 5 iBuAc 4590 72,1 1.3 Production of solvent-based silicone-polyester hybrid solutions (Variant 1)

[0104] The silicone-polyester hybrid solutions SiPES 6 - SiPES 11 were produced according to a process in accordance with EP 0092701. The silicone-polyester hybrid solution SiPES 12 was produced according to a process in accordance with EP 1072 660. Components A and C from Tables 1 and 2 were used. Table 3 shows further relevant data. Table 3: Name: Polyorganosiloxane polyester Solvent Silicone content [%] Viscosity [mPas] Solids [%] SiPES 6 POS 1 PES 1 EtiBu 30 18010 69,8 SiPES 7 POS 2 PES 2 DEC 30 4270 61,8 SiPES 8 POS 2 PES 3 MPK 30 1983 69,8 SiPES 9 POS 2 PES 4 MIBK 30 2490 69,1 SiPES 10 POS 3 PES 5 iBuAc 30 29740 70,4 SiPES 11 POS 3 PES 3 MPK 50 2370 71,3 SiPES 12 POS 3 PES 4 MIBK 80 2150 75,9 1.4 Production of solvent-based silicone-polyester hybrid solutions (Variant 2)

[0105] The silicone-polyester hybrid solutions SiPES 1 - SiPES 5 were produced according to a process as described in DE102013218981, Example 1. In this process, the organic polymers were used as monomers. Table 4 shows relevant data for these silicone-polyester hybrid solutions SiPES 1 - SiPES 5. Table 4: Designation Polyorganosiloxane used Solvent Silicone content [%] Viscosity [mPas] Solids [%] SiPES 1 POS 1 MIBK 30 7220 91,2 SiPES 2 POS 2 MIBK 30 6400 89,8 SiPES 3 DC 3074 MIBK 30 6530 90,4 SiPES 4 DC 3074 EtAc 30 6210 89,1 SiPES 5 DC 3074 EtAc 40 5740 88,4 1.5 Solvent-based, epoxy-based polyorganosiloxane hybrid solution (hereinafter referred to as silicone polyepoxide hybrid solution for simplicity)

[0106] The commercially available Silikopon® EW from Evonik Industries was used. 2. Production of polyorganosiloxane hybrid dispersions

[0107] The solvent-based silicone-polyester hybrid solutions (variants 1 and 2) and the solvent-based silicone-polyepoxide hybrid solution were used, which are referred to as polyorganosiloxane hybrid resin in the ug specification description. 2.1 Regulation 1, according to the invention:

[0108] 100.0 grams of a 20% solution of Poval® 4-88 in fully deionized (DI) water are placed in a container at room temperature. Then, 360.0 grams of a polyorganosiloxane hybrid resin, dissolved in appropriate amounts of solvent, are added. The stirring speed is 1000 rpm. A highly viscous paste is formed, which, after the resin addition is complete, is stirred for a further 60 minutes at 1000 rpm. Subsequently, 140.0 grams of DI water are added. In the next step, the solvent is separated by distillation. For this, the temperature is increased to 50 °C and the pressure is reduced to 40 mbar. The solids content of the dispersion is then determined. This is subsequently adjusted to 50.0% by adding DI water while stirring. 2.2 Regulation 2, according to the invention:

[0109] As per regulation 1, with the proviso that the emulsifier solution is a 20% solution of Poval® 3-80 in fully deionized (DI) water. 2.3 Regulation 3, according to the invention:

[0110] As per regulation 1, with the proviso that the emulsifier solution is a 12.5% ​​solution of Poval® 18-88 in fully deionized (DI) water. 2.4 Regulation 4, according to the invention:

[0111] As per regulation 1, with the proviso that the emulsifier solution is a 20% solution of Gohsenol® KL-03 in fully deionized (DI) water. 2.5 Regulation 5, according to the invention:

[0112] As per regulation 1, with the proviso that the emulsifier solution is a 20% solution of Gohsenol® KL-05 in fully deionized (DI) water. 2.6 Regulation 6, according to the invention:

[0113] As per Regulation 1, with the proviso that 70.0 grams of a 20% solution of Poval® 4-88 in fully deionized (DI) water and 30.0 grams of a 50% solution of Tergitol® 15-S-5 in fully deionized (DI) water are placed in a container at room temperature.

[0114] The particle size, flash point, and residual solvent content of each produced dispersion E1–E30 were determined. The values ​​can be found in Table 5. All dispersions were adjusted to a solids content of 50 wt%. Table 5: Dispersion Polyorganosiloxane hybrid resin Regulation Diameter [nm] Flash point [°C] Residual solvent content [wt.%] E1 SiPES 1 1 634 >100 0,5 E2 SiPES 1 2 587 >100 0,6 E3 SiPES 2 3 434 >100 0,4 E4 SiPES 3 4 635 >100 0,3 E5 SiPES 4 5 403 >100 0,5 E6 SiPES 5 6 515 >100 0,6 E7 SiPES 6 1 423 >100 0,6 E8 SiPES 6 2 528 >100 0,5 E9 SiPES 7 3 393 >100 0,6 E10 SiPES 7 4 448 >100 0,4 E11 SiPES 8 3 432 >100 0,5 E12 SiPES 8 4 439 >100 0,7 E13 SiPES 8 1 695 >100 0,3 E14 SiPES 8 1 854 >100 0,1 E15 SiPES 8 3 545 49 3,3 E16 SiPES 9 1 603 >100 0,9 E17 SiPES 9 2 719 >100 0,2 E18 SiPES 9 3 727 >100 0,3 E19 SiPES 9 4 728 >100 0,3 E20 SiPES 10 5 472 >100 0,5 E21 SiPES 11 1 503 >100 0,4 E22 SiPES 11 1 628 42 2,0 E23 SiPES 11 1 625 31 4,0 VE24 SiPES 11 1 729 23 6,1 E25 SiPES 12 4 607 >100 0,2 E26 Silikopon EW 1 564 >100 0,1 E27 Silikopon EW 2 434 >100 0,2 E28 Silikopon EW 3 397 >100 0,2 E29 Silikopon EW 4 494 >100 0,3 E30 Silikopon EW 5 827 >100 0,5

[0115] The residual solvent content of the dispersions according to the invention was less than 6 wt.%. The flash points of the dispersions according to the invention were in all cases higher than the flash point of the comparative example (VE24). In particular, for the dispersions according to the invention with a residual solvent content of <1 wt.%, the flash point of >100°C was reported, since these dispersions boiled due to their water content and a flash point could not be determined.

[0116] As a comparative example, VE24, a dispersion with a residual solvent content of 6.1 wt.% and a solids content of 50 wt.%, was used. To produce VE24 with this residual solvent content, the process according to the invention was expediently terminated early. The flash point was correspondingly lower.

[0117] Thus, it was found that the flash point of an aqueous polyorganosiloxane hybrid resin dispersion can be increased using the inventive method. 3. Differentiation from WO 2015 / 091901, hereinafter referred to as "Wacker"

[0118] A silicone-modified polyester resin according to Examples 5, 6, 7, 10, 11 and 12 according to Wacker with a solvent content of 40 wt.% was used and a dispersion was produced according to the "Wacker" process.

[0119] For this purpose, the silicone-polyester resin was distilled under vacuum at a maximum temperature of 90°C until the resin mass reached a viscosity at which it was still processable. Processability is necessary to enable emulsification in the next step. Since WO 2015 / 091901 does not specify the temperature and duration, a temperature below the boiling point of water was used. The solids content was then determined: It was found that the resin mass was no longer processable above a solids content of 85% by weight. It was no longer emulsifiable.

[0120] At a maximum solids content of 80 wt%, the resin mass still exhibits sufficient processability, which was used to produce a dispersion with a solids content of 30 wt% based on the polyorganosiloxane hybrid resin dispersion. This dispersion results in a calculated residual solvent content of 6 wt%. It is conceivable to reduce the residual solvent content of this dispersion by diluting it with additional water; however, this would correspondingly reduce the solids content of the dispersion.

[0121] It is therefore not possible to use the method according to WO 2015 / 091901 to obtain the dispersion according to the invention. Application-related measurements 1. Application and curing methods 1.1 Method 1: 2K Isocyanate Crosslinking

[0122] The dispersions E1 - E15 according to the invention were mixed with Bayhydur® 3100 in a 3:1 ratio and applied to Q-Panel® aluminum color test panels from Q-Lab (Alloy 3003H14; 0.025" thick (0.6 mm); bare mill finish) using a spiral squeegee. The wet film thickness is 100 µm. After 24 hours of drying at room temperature, clear, defect-free films with a dry film thickness of 50 µm result. The test panels were aged for 10 days at 23 °C and 65% relative humidity. 1.2 Method 2: Thermal Crosslinking

[0123] The dispersions E16-E23 and E25-E30 according to the invention are applied to Q-Panel® aluminum color test panels from Q-Lab (Alloy 3003H14; 0.025" thick (0.6 mm); bare mill finish) using a spiral squeegee. The wet film thickness is 100 µm. After 0.5 hours of drying at room temperature, clear, defect-free films with a dry film thickness of 50 µm result. After this drying time at room temperature, the air-dried test panels were baked in a convection oven at 250°C for 15 minutes.

[0124] Similarly, the solvent-based SiPES 1, SiPES 2, SiPES 8, SiPES 9 and SiPES 12 were applied and cured. 4. Measurement of pendulum hardness

[0125] The films were characterized using pendulum hardness according to König (DIN 53 157). The values ​​can be found in Table 6. Table 6: Pendulum hardness Dispersion hardening method Pendulum hardness E1 1 134 E2 1 120 E3 1 133 E4 1 126 E5 1 126 E6 1 127 E7 1 139 E8 1 132 E9 1 121 E10 1 119 E11 1 129 E12 1 145 E13 1 134 E14 1 122 E15 1 139 E16 2 157 E17 2 163 E18 2 162 E19 2 168 E20 2 162 E21 2 158 E22 2 166 E23 2 155 E25 2 160 E26 2 159 E27 2 160 E28 2 171 E29 2 158 E30 2 155 Comparative examples, solvent-based SiPES 1 1 129 SiPES 2 1 132 SiPES 8 2 159 SiPES 9 2 168 SiPES 12 2 161

[0126] It has been shown that the aqueous dispersions according to the invention exhibit equally good pendulum hardness values ​​as the solvent-based polyorganosiloxane hybrid resins. Pendulum hardness is important because it provides direct information about the serviceability of the final coating of the polyorganosiloxane hybrid resin dispersion according to the invention.

Claims

1. Aqueous polyorganosiloxane hybrid resin dispersion comprising: - at least one polyorganosiloxane hybrid resin, wherein the polyorganosiloxane hybrid resin consists of reaction products of a composition containing: • Component A) 5 to 95 parts by weight, preferably 10 to 70 parts by weight, of one or more polyorganosiloxanes of the general formula ∘ R a Si(OR') b O (4-a-b / 2) Formula (I) ∘ with 0 <a<2, 0<b<2 und a+b<4, • optional Komponente B) 0 - 20 Gew.-Teile, bevorzugt 1 -10 Gew.-Teile eines oder mehrerer linearer und / oder verzweigter Polyorganosiloxane der Formel ∘          R"O-[R"'2Si-O] n - Formula (II) • Component C) 5 to 95 parts by weight, preferably 30 to 90 parts by weight of an organic polymer, wherein R a, R', R" and R'" each independently represent an alkyl group with 1 to 8 C atoms or an aromatic group with 6 to 20 C atoms and n represents a number in the range of 4 to 250, - at least one emulsifier based on partially hydrolyzed polyvinyl acetates, - wherein it has a solids content of 30.0 wt.% - 70.0 wt.%, preferably 45.0 wt.% - 55.0 wt.%, based on the polyorganosiloxane hybrid resin dispersion and the residual solvent content is < 6.0 wt.%, preferably < 2.5 wt.%, particularly preferably < 1.0 wt.%, based on the polyorganosiloxane hybrid resin dispersion.

2. Polyorganosiloxane hybrid resin dispersion according to claim 1, characterized by the fact thatthe organic polymer selected from the group of polyepoxides, polyesters, polyacrylates and / or methacrylates and copolymers thereof, polyurethanes, cellulose derivatives, polysulfones, polyethersulfones, polyphenylene sulfides and oxides, polyamides, polyamide-imide, polyimides, polyethers, aromatic and aliphatic glycidyl-functional polymers, oligomers, phenoxy resins, polycarbonates, ketone formalaldehyde resins, polyvinyl resins selected from polyvinyl alcohol, polyglycerols, polyvinyl acetate, their (partial) hydrolysates and derivatives, phenolic resins, fluoropolymers, alkyd resins and mixtures thereof.

3. Polyorganosiloxane hybrid resin dispersion according to claim 1 or 2, characterized by the fact that the organic polymer contains hydroxyl groups and / or acidic hydrogen.

4. Polyorganosiloxane hybrid resin dispersion according to one of claims 1-3, characterized by the fact thatThe emulsifiers are partially hydrolyzed polyvinyl acetates with a degree of alcoholysis between 10% and 99% (mol / mol), preferably between 50% and 95% (mol / mol), and particularly preferably between 70% and 90% (mol / mol).

5. Polyorganosiloxane hybrid resin dispersion according to one of claims 1 - 4, characterized by the fact that The partially hydrolyzed polyvinyl acetates have a viscosity, measured in a 4% aqueous polyvinyl acetate solution at 20°C according to DIN 53015, of 1 - 50 mPa s, preferably 1 - 40 mPa s and particularly preferably 1 - 30 mPa s.

6. Polyorganosiloxane hybrid resin dispersion according to one of the preceding claims, characterized by the fact that it contains further emulsifiers selected from the group of anionic, cationic, zwitterionic or non-ionic emulsifiers.

7. Polyorganosiloxane hybrid resin dispersion according to one of the preceding claims, characterized by the fact thatthe flash point of the dispersion according to the method described is > 30.0°C, preferably > 60.0°C and particularly preferably > 90.0°C.

8. Polyorganosiloxane hybrid resin dispersion according to one of the preceding claims, characterized by the fact that the weight ratio of polyorganosiloxane hybrid resin to emulsifier or emulsifier system is between 5 - 50, preferably between 7 - 40, particularly preferably between 10 - 30.

9. Polyorganosiloxane hybrid resin dispersion according to one of the preceding claims, characterized by the fact that it contains further additives, selected from defoamers, deaerators, rheology additives, preservatives, substrate wetting agents, crosslinkers, drying aids, catalysts, antioxidants, skin-preventing agents, anti-segregation agents, thickeners, coalescing agents, film-forming aids, fillers, pigments and / or dispersing agents.

10. Polyorganosiloxane hybrid resin dispersion according to any of the preceding claims, characterized by the fact thatFungicides, bactericides, pesticides, algicides and / or herbicides are used as preservatives.

11. Polyorganosiloxane hybrid resin dispersion according to one of the preceding claims, characterized by the fact that the mean volume-weighted diameter of the polyorganosiloxane hybrid resin particles, measured according to ISO 13320:2009, is between 0.1 - 10.0 µm, preferably between 0.1 - 2.0 µm, particularly preferably between 0.2 - 1.0 µm and most preferably between 0.2 - 0.7 µm.

12. Method for the production of aqueous polyorganosiloxane hybrid resin dispersion, comprising the steps of a. emulsifying a polyorganosiloxane hybrid resin solution containing an organic or semi-organic solvent with an emulsifier solution comprising at least one emulsifier based on partially hydrolyzed polyvinyl acetates and b. separating the solvent.

13. Procedure according to one of the aforementioned claims, characterized by the fact thatan aqueous emulsifier solution or an aqueous emulsifier system solution is used, wherein its concentration is between 5 - 40 wt.%, preferably 10 - 30 wt.%, particularly preferably 15 - 25 wt.% based on the emulsifier solution.

14. Procedure according to one of the aforementioned claims, characterized by the fact that In step a), additional water is added.

15. Procedure according to one of the aforementioned claims, characterized by the fact that After step b), the solids content for the aqueous polyorganosiloxane hybrid resin dispersion is adjusted.

16. Procedure according to one of the aforementioned claims, characterized by the fact that The polyorganosiloxane hybrid resin consists of reaction products of a composition containing - component A) 5 to 95 parts by weight, preferably 10 to 70 parts by weight of one or more polyorganosiloxanes of the general formula R a Si(OR') b O (4-a-b / 2)Formula (I) with 0 <a<2, 0<b<2 und a+b<4, - optional Komponente B) 0 - 20 Gew.-Teile, bevorzugt 1 -10 Gew.-Teile eines oder mehrerer linearer und / oder verzweigter Polyorganosiloxane der Formel          R"O-[R"'2Si-O] n - Formula (II) - Component C) 5 to 95 parts by weight, preferably 30 to 90 parts by weight of an organic polymer, wherein R a , R', R" and R'" each independently represent an alkyl group with 1 to 8 C atoms or an aromatic group with 6 to 20 C atoms, and n represents a number in the range of 4 to 250.

17. Procedure according to one of the aforementioned claims, characterized by the fact thatThe organic polymer is an organic polymer containing hydroxyl groups, preferably selected from the group consisting of polyepoxides, polyesters, polyacrylates and / or methacrylates and copolymers thereof, polyurethanes, cellulose derivatives, polysulfones, polyethersulfones, polyphenylene sulfides and oxides, polyamides, polyamide-imide, polyimides, polyethers, aromatic and aliphatic glycidyl-functional polymers, oligomers, phenoxy resins, polycarbonates, ketone formalaldehyde resins, polyvinyl resins selected from polyvinyl alcohol, polyglycerols, polyvinyl acetate, their (partial) hydrolysates and derivatives, phenolic resins, fluoropolymers, alkyd resins and mixtures thereof.

18. Procedure according to one of the aforementioned claims, characterized by the fact that The emulsifiers are partially hydrolyzed polyvinyl acetates with a degree of alcoholysis between 10% and 99% (mol / mol), preferably between 50% and 95% (mol / mol), and particularly preferably between 70% and 90% (mol / mol).

19. Procedure according to one of the aforementioned claims, characterized by the fact that The partially hydrolyzed polyvinyl acetates have a viscosity, measured in a 4% aqueous polyvinyl acetate solution at 20°C according to DIN 53015, of 1 - 50 mPa s, preferably 1 - 40 mPa s and particularly preferably 1 - 30 mPa s.

20. Procedure according to one of the aforementioned claims, characterized by the fact that Other emulsifiers selected from the group of anionic, cationic, zwitterionic or non-ionic emulsifiers may be used.

21. Procedure according to one of the aforementioned claims, characterized by the fact that The solvent is at least an organic solvent that was used in the manufacture of the polyorganosiloxane hybrid resin, or at least a semi-organic solvent.

22. Procedure according to one of the aforementioned claims, characterized by the fact thatthe organic solvent or mixtures thereof has a boiling point range of 50°C - 150°C, preferably 90°C - 120°C.

23. Procedure according to one of the aforementioned claims, characterized by the fact that The separation of the solvent is carried out by distillation at reduced pressure with or without stripping gas, steam distillation, by means of a membrane process, a thin-film evaporator or a countercurrent process.

24. Procedure according to one of the aforementioned claims, characterized by the fact that the polyorganosiloxane hybrid resin solution has a polyorganosiloxane hybrid resin concentration of 40.0 wt.% - 95.0 wt.%, preferably 60.0 wt.% - 70.0 wt.%, based on the polyorganosiloxane hybrid resin solution.

25. Procedure according to one of the aforementioned claims, characterized by the fact that The flash point of the aqueous polyorganosiloxane hybrid resin dispersion produced by the process can be increased.

26. Use of the polyorganosiloxane hybrid resin dispersion according to one of claims 1 - 11 in coating materials, as well as varnishes and paints, substrate coatings, semi-finished products, adhesives, inks, sealants, compounding matrices and sizing agents.

27. Substrates, in particular baking trays, baking molds, pans, metal pots and the like, coated with a composition containing a dispersion according to any one of claims 1 to 11.