Fabric custom-printed with antibacterial nanoparticles

JP2022059590A5Inactive Publication Date: 2024-10-02XEROX CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2021162913
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-10-01
Filing Date
2021-10-01
Publication Date
2024-10-02
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional methods for synthesizing silver/polymer nanostructured materials lack morphological control and often require time-consuming processes like filtration and centrifugation, resulting in poor properties and potential toxicity of uncoated silver nanoparticles.

Method used

A method involving the formation of core-shell antimicrobial toner particles with silver nanoparticles encapsulated in a polymer shell, applied to fabrics using a carrier layer and adhesive, allowing for precise placement and biocompatible antimicrobial properties.

Benefits of technology

The method provides fabrics with enhanced antimicrobial properties, reducing toxicity and improving stability, while enabling high-quality imaging and effective microbial protection on various fabric types.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

To provide a method of forming an image with antibacterial particles on a fabric and an obtained fabric.SOLUTION: The present method includes providing a printable medium including a carrier layer 52 having a first surface 58 including a first region 60 and a second surface 62 opposite the first surface 58. The present method includes providing a fabric layer 54 having a third surface 64 and a fourth surface 66 opposite the third surface 64, and the third surface 64 includes a second region. The fabric layer 54 is fixed to the carrier layer 52 by an adhesive which adheres the first portion of the fourth surface 66 to the first surface 58. The present method includes applying a toner to the first portion of the third surface 64 of the fabric layer 54. The toner contains antibacterial nanoparticles on an outer surface of the toner. The present method includes fusion of the toner to the first portion of the third surface 64 of the fabric layer 54.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] (Field of the Invention) The present disclosure relates, in various embodiments, to fabrics printed with antimicrobial particles and methods thereof.

Background Art

[0002] In today's situation, during the COVID-19 virus pandemic, there is a pressing need in the medical field for antibacterial, antimicrobial and antifungal applications in equipment, accessories and clothing.

[0003] Due to potential applications that are possible, there is a growing interest in embedding nanometals into polymer matrices. Most methods for nanometal structured materials such as silver nanoparticles require that a silver salt precursor be reduced in a chemical reaction prior to incorporation into the polymer matrix. The most widely used silver ion precursor for the synthesis of silver nanoparticles (AgNP) is silver nitrate (AgNO3). The reducing agents most readily used for the synthesis of AgNP are sodium borohydride or sodium citrate. The most common stabilizers for nanosilver are citrate and PVP (polyvinylpyrrolidone).

[0004] Conventional methods for making silver / polymer nanostructured materials generally require melt mixing or extrusion of AgNP in a polymer matrix to obtain aggregated silver particles. Other methods use in-situ synthesis of metal nanoparticles in a polymer matrix, which involves dissolution and reduction of metal salts, and / or polymer synthesis simultaneously. The polymer matrix serves to keep the AgNP dispersed and to maintain overall chemical and mechanical stability.

[0005] Current methods for synthesizing core-shell or hybrid colloidal dispersions lack morphological control, and the resulting properties are generally inferior. Most conventional methods have been found to require filtration, deposition, and centrifugation processes, which are difficult and time-consuming.

[0006] Furthermore, while uncoated silver nanoparticles can be toxic, it is known that their toxicity decreases, or in other words, they become biocompatible, when protected by an organic layer or embedded in an organic matrix. [Overview of the Initiative] [Problems that the invention aims to solve]

[0007] It would be desirable for textiles to be impregnated or imprinted with bio-silver nanoparticles (AgNP). This would broaden the possibilities for use in medical environments and agricultural clothing as a means of preventing the spread of microorganisms. This would also enable the prevention of microbial growth in textiles for common use such as face masks, gloves, and scarves.

[0008] In various embodiments, methods for forming an image on a fabric are provided. The method includes providing a printable medium comprising a carrier layer having a first surface including a first region and a second surface opposite to the first surface. The carrier layer has a first rigidity. The method includes providing a fabric layer having a third surface and a fourth surface opposite to the third surface, the third surface including the second region. The fabric layer has a second rigidity lower than the first rigidity. A first adhesive is present. The fabric layer is fixed to the carrier layer by a first adhesive that adheres a first portion of the fourth surface to the first surface. The method includes applying toner to a first portion of the third surface of the fabric layer. The toner has a size of 4 microns (μm) to about 20 microns. The toner includes antimicrobial nanoparticles on its outer surface, the antimicrobial nanoparticles having a size of 5 nanometers to 500 nanometers. The method includes fusing the toner to the first portion of the third surface of the fabric layer.

[0009] Further embodiments described herein include a printed material comprising a fabric having a first surface and a second surface opposite to the first surface. A toner image is placed on the first surface of the fabric, and the toner image comprises toner particles having a size of 4 microns to about 20 microns, and antimicrobial nanoparticles on the outer surface of the toner. The antimicrobial nanoparticles have a size of 5 nanometers to 500 nanometers.

[0010] Further embodiments described herein are methods for forming an image on a fabric. The method includes providing a printable medium having a carrier layer having a first surface and a first region, a second surface opposite to the first surface, and a first rigidity. The method includes a fabric layer having a third surface, a fourth surface having a second region opposite to the third surface, and a second rigidity lower than the first rigidity. The method includes an adhesive. The fabric layer is fixed to the carrier layer by an adhesive that adheres a first portion of the fourth surface to the first surface. The method includes applying toner to a first portion of the third surface of the fabric layer, the toner having a size of 4 microns to about 20 microns. The toner includes antimicrobial nanoparticles having a size of 5 nanometers to 500 nanometers. The method includes fusing the toner to the first portion of the third surface of the fabric layer. [Brief explanation of the drawing]

[0011] The accompanying drawings incorporated herein and constituting part of this specification illustrate several embodiments of this teaching and, together with the descriptions, serve to illustrate the principles of this teaching.

[0012] [Figure 1] Figure 1 is a perspective view of one embodiment of a carrier layer and a fabric layer that are separated from each other.

[0013] [Figure 2] Figure 2 is a cross-sectional view of one embodiment of the printable medium of the present invention, showing a fabric layer releasably fixed to a carrier layer via an adhesive.

[0014] [Figure 3] Figure 3 is a plan view of the first surface of one embodiment of the fabric layer.

[0015] [Figure 4] Figure 4 is a side elevation view of one embodiment of a printing system having a single fusion machine and arranged to deposit antimicrobial toner onto a fabric layer.

[0016] [Figure 5] FIG. 5 is a cross-sectional view of an antibacterial toner.

[0017] [Figure 6] FIGS. 6A, 6B, and 6C show antibacterial toner particles printed on a fabric.

[0018] [Figure 7] FIG. 7 shows water droplet absorption in a fabric printer using antibacterial toner particles.

[0019] Note that some details of these figures are simplified and do not maintain exact structural accuracy, details, and scale, and are drawn to facilitate understanding of the embodiments.

DETAILED DESCRIPTION OF THE INVENTION

[0020] In the following description, reference is made to chemical formulas that exemplify specific exemplary embodiments that form part of and enable the implementation of the present teachings. These embodiments are described in sufficient detail to enable those skilled in the art to implement the present teachings, and it is understood that other embodiments may be utilized and that changes may be made without departing from the scope of the present teachings. Accordingly, the following description is merely illustrative and non-limiting.

[0021] The numerical ranges and parameters setting forth the broad scope of this disclosure are approximations, but the numerical values set forth in the specific examples are reported as accurately as possible. However, any numerical value inherently contains certain errors necessarily resulting from the standard deviation found in the respective test measurements. Further, all ranges disclosed herein are to be understood to encompass any and all sub-ranges subsumed therein. For example, a range of "less than 10" includes any and all sub-ranges between the minimum value of zero and the maximum value of 10 (including the boundary values), that is, any and all sub-ranges having a minimum value of at least zero and a maximum value of less than 10, such as, for example, 1 to 5. In certain instances, the numerical values described for the parameters can take on negative values. In this case, exemplary values of the range described as "less than 10" can assume negative values, such as, for example, -1, -2, -3, -10, -20, -30, etc.

[0022] Embodiments of the disclosure herein are not limited in this regard, but as used herein, the terms "plurality" and "a plurality" can include, for example, "multiple" or "two or more." The terms "plurality" or "a plurality" can be used throughout this specification to describe two or more components, devices, elements, units, parameters, etc. For example, "a plurality of resistors" can include two or more resistors.

[0023] Broadly speaking, as shown in FIGS. 1 and 2, in some embodiments, the printable medium 50 includes a carrier layer 52, a fabric layer 54, and an adhesive 56. The carrier layer 52 includes a surface 58 having a region 60, a surface 62 opposite the surface 58, and a first rigidity. The fabric layer 54 includes a surface 64, a surface 66 opposite the surface 64, and a second rigidity lower than the first rigidity. The fabric layer 54 is fixed to the carrier layer 52 by an adhesive 56 that adheres a portion of the surface 66 to the surface 58.

[0024] In some embodiments, the adhesive 56 is deposited on a region 60, and in some embodiments, the region 60 is less than or equal to the total area of ​​the surface 58. In some embodiments, the adhesive 56 is deposited on a surface 66, and in some embodiments, the region on the surface 66 is less than or equal to the total area of ​​the surface 58. In some embodiments, the region 60 is substantially equal to the region on the surface 66. In summary, the adhesive can be deposited on the carrier layer 52 and / or the fabric layer 54. Furthermore, the adhesive can be deposited on a region with an area less than or equal to the total area of ​​the carrier layer 52 and / or the fabric layer 54.

[0025] The embodiments described above enable image formation on a fabric layer 54 using an antimicrobial toner. As described above with respect to the attachment of the fabric layer 54 to the surface of the carrier layer 52, the adhesive can be deposited on the carrier layer 52 and / or the fabric layer 54. That is, in embodiments in which the fabric layer 54 is encased in the carrier layer, the adhesive can be applied to each surface of the carrier layer and / or the non-image-holding surface of the fabric layer 54, such that, regardless of the difference, the image-holding surface always faces outward from the carrier layer, i.e., never comes into contact with the carrier layer.

[0026] In some embodiments, as shown in Figure 3, the present disclosure includes a method for forming an image 88 on a fabric layer 54. Some embodiments of the method include fixing the fabric layer 54 to a carrier layer 52 in a releasable manner, wherein the carrier layer 52 includes a surface 58 having a region 60, a surface 62 opposite to the surface 58, and a first stiffness, and the fabric layer 54 includes a surface 64 having a region, a surface 66 opposite to the surface 64, and a second stiffness lower than the first stiffness, and the fabric layer 54 is fixed to the carrier layer 52 by an adhesive 56 that bonds the surface 66 to the surface 58, applying an antimicrobial toner to a portion of the surface 64 of the fabric layer 54, and fusing the dried antimicrobial toner to the portion of the surface 64 with a fusion machine.

[0027] In some embodiments, the fabric layer may benefit from a “pretreatment” step. For example, the fabric may be porous, and such porosity allows the passage of dry toner. However, depositing the toner first, for example, on a base layer before forming an image on the fabric can significantly reduce the subsequent passage of the marking material through the pores, thereby greatly improving the final image quality. Thus, the initial deposition of white dry marking material on the fabric can provide a more compatible base medium that substantially fills the pores and on which an image can then be formed.

[0028] In addition, in some embodiments, the printing system may include a sensor used to detect the color of the printing medium, e.g., cream / naturally colored cotton, before depositing the base layer. The printing system can then be configured to print its custom-made base layer, i.e., a color-matched base layer, on top of the fabric layer before forming the image on it. It should be noted that the aforementioned custom-made base layer provides a higher degree of consistency to areas of flexible material that do not accept background / non-printing material and marking material, e.g., the outer edges of the flexible material.

[0029] Similarly, in some embodiments, the first toner deposited on the fabric layer may function as a base layer that alters the appearance of the first toner, for example, as a glossy or highly reflective layer, and / or improve the adhesion of a subsequently deposited marking material, such as a primer layer. The embodiments described above are included in the claims relating to the application of the first and second marking materials.

[0030] Furthermore, the fabric layer 54 may include already formed articles, such as T-shirts, blouses, pants, face masks, scarves, etc. Such articles may be placed on the carrier layer in an orientation that allows for the formation of an image on one or more surfaces of the article, for example, the front and / or back of a T-shirt. Similarly, household items such as window coverings, such as curtains, shower curtains, towels, pillowcases, blankets, etc., can also be fixed to the carrier layer and then an image can be formed on them. In short, any fabric layer may be attached to the carrier layer disclosed herein in a manner that allows for the formation of an image on one or more locations on the material, and the material may be a ready-made article.

[0031] The fabric layers described herein can be used in various printing systems. For example, in Figure 4, printer 113 includes, in part, a transfer belt 114, toner dispensers 116, 118, 120, and 122, an ATA device 112, and a fusion splicer 94, while printer also includes, in part, a transfer belt 114, toner dispensers 116, 118, 120, 122, and 126, an ATA device 112, and a fusion splicer 94.

[0032] Furthermore, some embodiments, such as those involving toner-based image formation, may benefit from printing systems that include known acoustic transfer assist (ATA) devices. Those skilled in the art will understand that a printing system that uses a flexible belt in a process of forming an image on it, and then transfers the image from the flexible belt to a printing medium, may include one or more ATA devices (Figure 4, 112). The ATA device uses acoustic energy to drive a dry marking material, such as toner, from the belt to the printing medium. Thus, in some embodiments, an ATA device such as ATA device 112 assists in the transfer of the dry marking material from the belt to the flexible printing medium, eliminating the need for direct contact between the belt and the flexible material. It should be understood that such an arrangement can minimize image defects and thereby increase image quality.

[0033] Using the apparatus shown in Figure 4, the resolution of the image on the fabric layer is 600 dots / inch (dpi) to 2400 (dpi). In some embodiments, the resolution may be 1200 dpi to 2400 dpi. In some embodiments, the resolution may be 600 dpi to 1200 dpi. Antibacterial toner

[0034] Embodiments described herein utilize EA toner technology to form antimicrobial toner particles containing silver nanoparticles for enhanced antimicrobial properties. For example, such toners may include toner particles having a core / shell configuration (i.e., a shell formed around a core) in which silver nanoparticles are arranged within a shell. When such toner particles are transported and fused onto a fabric layer, the silver nanoparticles are exposed to oxygen, thereby releasing silver ions that can act as a potent antimicrobial agent. Toner particles having silver nanoparticles within a shell have a size of 4 μm to 20 μm.

[0035] As disclosed herein, the development of a synthesis process for core-shell organic / inorganic nanoparticles in which silver nanoparticles are precisely positioned on the surface of nanoparticles provides reactive or stimulus-responsive colloidal particles having a precisely defined structure, homogeneous encapsulation, and a precisely defined morphology. Other problems arising in conventional methods and solved by the methods herein include, in particular, incompatibility between polymers and inorganic materials when highly hydrophobic monomers are used in any polymerization step of the process.

[0036] This specification describes core-shell nanoparticles as functional composites for use in a wide range of biomedical devices. These core-shell materials are also economically desirable because the bulk or core is primarily organic, while the shell contains organic materials with more expensive precious metals such as gold, copper, and silver.

[0037] Several embodiments provide the preparation and characterization of core-shell nanocomposites in which silver nanoparticles are selectively immobilized within the outer shell layer of core-shell nanoparticles. The methods of the present invention disclosed herein are environmentally friendly processes for synthesizing silver nanoparticles that do not require the use of toxic chemicals. The methods combine chemical friendliness and biocompatibility when preparing hybrid organic / inorganic nanocomposites. Hybrid nanocomposites have the ability to incorporate inorganic material properties related to coating performance (such as robustness) and thermal stability. The planned placement of silver nanoparticles (AgNPs) within the shell facilitates access to silver for antimicrobial applications.

[0038] Some of the silver-containing toners of the embodiments described herein can be introduced as coatings for antimicrobial applications (printed on clothing or other fabrics requiring antimicrobial properties). Some of the toners of the embodiments described herein can be printed on fabric 54. Pigment-containing or non-pigment-containing emulsion aggregates can be formulated to contain silver nanoparticles that can be printed on fabric.

[0039] In one embodiment, antimicrobial toner particles can be prepared using emulsion polymerized composite resin latex, the core comprising at least one styrene acrylate polymer resin, and the shell comprising at least one composite styrene / acrylate-metal ion polymer resin. Nanoparticle composite latex

[0040] Some embodiments of the present invention provide a method for synthesizing composite nanoparticles in which metal ions, such as silver ions, are immobilized in the shell (and optionally within the core) of core-shell resin particles. The placement of the metal composite ionomer within the shell provides access for silver ions for antimicrobial applications.

[0041] The core may contain any styrene / acrylate polymer resin useful for forming nanoparticles such as binder resins. The polymer may be synthesized by using any of the above-mentioned styrene / acrylate monomers and / or comonomers, or those known in the art and optionally containing metal ions, by conventional methods known in the art for forming resin polymers, including bulk polymerization, solution polymerization, and emulsion polymerization, and the method of synthesizing the polymer is not intentionally limited.

[0042] In some embodiments, core resin particles are provided, and the polymer is poly(styrene-alkyl acrylate), poly(styrene-1,3-diene), poly(styrene-alkyl methacrylate), poly(styrene-alkyl acrylate-acrylic acid), poly(styrene-1,3-diene-acrylic acid), poly(styrene-alkyl methacrylate-acrylic acid), poly(alkyl methacrylate-alkyl acrylate), poly(alkyl methacrylate-aryl acrylate), poly(aryl methacrylate-alkyl acrylate), poly(alkyl methacrylate-acrylic acid), poly(styrene-alkyl acrylate-acrylonitrile-acrylic acid), poly(styrene-1,3-diene-acrylonitrile-acrylic acid), poly(alkyl acrylate-acrylonitrile-acrylic acid), poly(styrene-butadiene), poly(methylstyrene-butadiene), poly(methyl methacrylate-butadiene), poly(ethyl methacrylate-butadiene), poly(propyl methacrylate-butadiene), poly(butyl methacrylate-butadiene), poly(methyl acrylate-butadiene), poly(ethyl acrylate-butadiene), poly(propyl Poly(butyl acrylate-butadiene), poly(styrene-isoprene), poly(methylstyrene-isoprene), poly(methyl methacrylate-isoprene), poly(ethyl methacrylate-isoprene), poly(propyl methacrylate-isoprene), poly(butyl methacrylate-isoprene), poly(methyl acrylate-isoprene), poly(ethyl acrylate-isoprene), poly(propyl acrylate-isoprene), poly(butyl Poly(styrene-propyl acrylate), poly(styrene-butyl acrylate), poly(styrene-butadiene-acrylic acid), poly(styrene-butadiene-methacrylic acid), poly(styrene-butadiene-acrylonitrile-acrylic acid), poly(styrene-butyl acrylate-acrylic acid), poly(styrene-butyl acrylate-methacrylic acid), poly(styrene-butyl acrylate-acrylonitrile), poly(styrene-butyl acrylate-acrylonitrile-acrylic acid), poly(styrene-butadiene), poly(styrene-isoprene), poly(styrene-butyl methacrylate), poly(styrene-butyl acrylate-acrylic acid), poly(styrene-butyl methacrylate-acrylic acid), poly(butyl methacrylate-butyl acrylate), poly(butyl methacrylate-acrylic acid), poly(acrylonitrile-butyl acrylate-acrylic acid), and combinations thereof are selected.

[0043] In some embodiments, the core is prepared via polymerization reactions, and the monomers are styrene, alkyl acrylates, e.g., methyl acrylate, ethyl acrylate, butyl acrylate, isobutyl acrylate, dodecyl acrylate, n-octyl acrylate, 2-chloroethyl acrylate; β-CEA, phenyl acrylate, methyl ethoxylated chloroacrylate, MMA, ethyl methacrylate and butyl methacrylate; butadiene, isoprene; methacrylonitrile; acrylonitrile; vinyl ethers, e.g., vinyl methyl ether, vinyl isobutyl ether, vinyl ethyl ether, etc.; vinyl esters, e.g. These are selected from vinyl acetate, vinyl propionate, vinyl benzoate and vinyl butyrate; vinyl ketones, e.g., vinyl methyl ketone, vinyl hexyl ketone and methyl isopropenyl ketone; vinylidene halides, e.g., vinylidene chloride and vinylidene chlorofluoride; N-vinylindole; pyrrolidone; MA; acrylic acid; methacrylic acid; acrylamide; methacrylamide; vinylpyridine; vinylpyrrolidone; vinyl-N-methylpyridinium chloride; vinylnaphthalene; p-chlorostyrene; vinyl chloride; vinyl bromide; vinyl fluoride; ethylene; propylene; butane; isobutylene, etc., and mixtures thereof.

[0044] In some embodiments, the core particles optionally further comprise a styrene / acrylate latex copolymer. Exemplary examples of styrene / acrylate latex copolymers include poly(styrene-n-butylacrylate-β-CEA), poly(styrene-alkylacrylate), poly(styrene-1,3-diene), poly(styrene-alkyl methacrylate), poly(alkyl methacrylate-alkyl acrylate), poly(alkyl methacrylate-aryl acrylate), poly(aryl methacrylate-alkyl acrylate); poly(alkyl methacrylate), poly(styrene-alkyl acrylate-acrylonitrile), poly(styrene-1,3-diene acrylonitrile), poly(alkyl acrylate-acrylonitrile), poly(styrene-butadiene), poly(methylstyrene-butadiene), poly(methyl methacrylate-butadiene), polyethyl methacrylate-butadiene), poly(propyl methacrylate-butadiene), poly(butyl Further examples include poly(methyl acrylate-butadiene), poly(methyl acrylate-butadiene), poly(polyacrylate-butadiene), poly(propyl acrylate-butadiene), poly(butyl acrylate-butadiene), poly(styrene-isoprene), poly(methylstyrene-isoprene), poly(methyl methacrylate-isoprene), poly(ethyl methacrylate-isoprene), poly(propyl methacrylate-isoprene), poly(butyl methacrylate-isoprene), poly(methyl acrylate-isoprene), poly(ethyl acrylate-isoprene), poly(propyl acrylate-isoprene), poly(butyl acrylate-isoprene); poly(styrene-propyl acrylate), poly(styrene-butyl acrylate), poly(styrene-butadiene-acrylonitrile), and poly(styrene-butyl acrylate-acrylonitrile).

[0045] In some embodiments, metal acrylates are included in the emulsion. Examples of metal acrylates include silver acrylates such as silver methacrylate.

[0046] In the embodiment, the styrene / acrylate polymer resin of the core optionally further comprises either the chain transfer agent and / or branching agent described above, in the amount described above. The styrene / acrylate polymer of the core comprises a styrene monomer, an acrylate monomer, an optionally chain transfer agent, and an optionally branching agent.

[0047] In some embodiments, there are methods for preparing latex composed of composite antimicrobial nanoparticles. The styrene / acrylate resin particles of the core can be synthesized by an emulsion polymerization reaction, followed by polymerization of the shell monomer on the surface of the core particles. In an alternative embodiment, a shell resin is formed and then added to an emulsion of core particles to form a layer that encapsulates the core particles. surfactant

[0048] In the preparation of latex, dye, or wax dispersions according to this disclosure, any suitable surfactant may be used. Depending on the emulsion system, any desired nonionic, anionic, or cationic surfactant may be considered.

[0049] Suitable anionic surfactants include, but are not limited to, sodium dodecylsulfate (SDS), sodium dodecylbenzenesulfate, sodium dodecylnaphthalenesulfate, dialkylbenzene alkyl sulfates and sulfonates, abitic acid, NEOGEN R® and NEOGEN SC® available from Kao, Tayca Power® RTM available from Tayca Corp., DOWFAX® available from Dow Chemical Co., and mixtures thereof.

[0050] Other suitable cationic surfactants include dialkylbenzenealkylammonium chloride, lauryltrimethylammonium chloride, alkylbenzylmethylammonium chloride, alkylbenzyldimethylammonium bromide, benzalkonium chloride, cetylpyridinium bromide, C 12 , C 15 and C 17 Examples include, but are not limited to, trimethylammonium bromide, halogenated salts of quaternized polyoxyethylalkylamines, dodecylbenzyltriethylammonium chloride, MIRAPOL® and ALKAQUAT® (available from Alkaril Chemical Company), SANIZOL® (benzalkonium chloride, available from Kao Chemicals), and mixtures thereof.

[0051] Examples of suitable nonionic surfactants include, but are not limited to, polyvinyl alcohol, polyacrylic acid, metalose, methylcellulose, ethylcellulose, propylcellulose, hydroxyethylcellulose, carboxymethylcellulose, polyoxyethylene cetyl ether, polyoxyethylene lauryl ether, polyoxyethylene octyl ether, polyoxyethylene octylphenyl ether, polyoxyethylene oleyl ether, polyoxyethylene sorbitan monolaurate, polyoxyethylene stearyl ether, polyoxyethylene nonylphenyl ether, dialkylphenoxypoly(ethyleneoxy)ethanol (available from Sanofi as ANTAROX 890 (trademark), IGEPAL CA-210 (trademark), IGEPAL CA-520 (trademark), IGEPAL CA-720 (trademark), IGEPAL CO-890 (trademark), IGEPAL CO-720 (trademark), IGEPAL CO-290 (trademark), IGEPAL CA-210 (trademark), and ANTAROX 897 (trademark)), and mixtures thereof.

[0052] Surfactants may be used in any desired or effective amount, for example, at least about 0.01% of the reactant, at least about 0.1% of the reactant, no more than about 10% of the reactant, or no more than about 5% by weight of the reactant, although these amounts may also be outside these ranges. Initiator

[0053] Suitable initiators or mixtures of initiators may be selected in the latex process and the toner process. In embodiments, the initiator is selected from known free radical polymerization initiators. Examples of suitable free radical initiators include, but are not limited to, peroxides, pertriphenyl acetate, tert-butylpropanate, sodium persulfate, and azo compounds.

[0054] The initiator may be present in amounts of approximately 0.1% to 5%, 0.4% to 4%, or 0.5% to 3% based on the total weight of the monomer, but may also be present in larger or smaller amounts. Chain transfer agent

[0055] The degree of polymerization of latex can be controlled by the optional use of chain transfer agents, thereby controlling the molecular weight and molecular weight distribution of the product latex. As can be understood, the chain transfer agent can become part of the latex polymer.

[0056] Chain transfer agents may have carbon-sulfur covalent bonds. An example of a chain transfer agent is nC 3-15 Examples of such chain transfer agents include, but are not limited to, alkyl mercaptans, branched alkyl mercaptans, and aromatic ring-containing mercaptans. Examples of such chain transfer agents include, but are not limited to, dodecanethiol, butanethiol, isooctyl-3-mercaptopropionate, 2-methyl-5-t-butylthiophenol, carbon tetrachloride, and carbon tetrabromide. The terms "mercaptan" and "thiol" can be used interchangeably to mean a C-SH group.

[0057] Based on the total weight of monomers, the chain transfer agent may be present in amounts of approximately 0.1% to 7%, approximately 0.5% to 6%, or approximately 1.0% to 5%, but may be present in greater or lesser amounts. Branching agent

[0058] In some embodiments, branching agents may be optionally included to control the degree of branching, crosslinking, and / or structure of the target latex. Exemplary branching agents include, but are not limited to, decanediol diacrylate (ADOD), trimethylolpropane, pentaerythritol, trimellitic acid, pyromellitic acid, and mixtures thereof.

[0059] The branching agent may be present in amounts of approximately 0.001% to 2%, approximately 0.05% to 1.0%, or approximately 0.1% to 0.8% based on the total weight of the monomers, or in amounts greater or less than these. Toner manufacturing method

[0060] In the latex and toner processes of this disclosure, emulsification may optionally be carried out by a preferred process, such as mixing at high temperatures. For example, the emulsion mixture may be mixed in a homogenizer set to about 200 to about 400 rpm at a temperature of about 20°C to about 80°C for about 1 to about 20 minutes, although these speeds, temperatures, and times may be outside these ranges.

[0061] Any type of reactor can be used, without limitation, to prepare the antimicrobial toner. The reactor may include means for stirring the composition therein, such as an impeller. The reactor may include at least one impeller. The reactor can be operated so that the impeller operates at an effective mixing rate of about 10 to about 1,000 rpm to form the latex and / or toner.

[0062] After the addition of monomers is complete, the latex can be stabilized by maintaining the conditions for a certain period of time, for example, about 10 to 300 minutes, before cooling. Optionally, the latex formed by the above process can be isolated by standard methods known in the art, such as coagulation, dissolution, precipitation, filtration, washing, and drying.

[0063] The latex of this disclosure may be melt-mixed or otherwise mixed with various toner formulation components, such as optionally selected wax dispersions, optionally selected colorants, optionally selected coagulants, optionally selected silica, optionally selected charge-enhancing or charge-controlling additives, optionally selected surfactants, optionally selected emulsifiers, optionally selected flow additives, etc. Optionally, the latex (e.g., about 40% solids) may be diluted to a desired solids loading (e.g., about 12 to about 15% by weight) before being incorporated into the toner composition.

[0064] Based on the total toner weight, latex may be present in an amount of about 50% to about 98%, but may be present in a smaller amount. A method for producing such latex resin may be carried out as described in U.S. Patent No. 7,524,602, which is incorporated herein by reference in its entirety. Optional colorants

[0065] In some embodiments, the antimicrobial toner particles may optionally contain one or more colorants. In some embodiments, the toner particles may be colorless or transparent. A variety of known and suitable colorants, such as dyes, pigments, mixtures of dyes, mixtures of pigments, and mixtures of dyes and pigments, can be incorporated into the toner. The colorants may be included in amounts, for example, about 0 to about 35% by weight of the toner, about 1 to about 25% by weight of the toner, or about 3 to about 20% by weight of the toner, but amounts outside these ranges may also be available.

[0066] Examples of suitable colorants include carbon black-like REGAL 330™, magnetites such as Mobay magnetite MO8029™ and MO8060™, Columbia magnetite, MAPICO BLACKS™, surface-treated magnetite, Pfizer magnetite CB4799™, CB5300™, CB5600™, and MCX6369™, Bayer magnetite, BAYFERROX 8600™ and 8610™, Northern Pigments magnetite, NP-604™ and NP-608™, Magnox magnetite TMB-100™ or TMB-104™. As coloring pigments, cyan, magenta, yellow, red, green, brown, blue, or mixtures thereof can be selected. Generally, cyan, magenta, or yellow pigments or dyes, or mixtures thereof, are used. The pigment(s) can be used as an aqueous pigment dispersion.

[0067] Specific examples of pigments include SUNSPERSE 6000, FLEXIVERSE, and AQUATONE aqueous pigment dispersions from SUN Chemicals; HELIOGEN BLUE L6900 (trademark), D6840 (trademark), D7080 (trademark), D7020 (trademark), PYLAM OIL BLUE (trademark), PYLAM OIL YELLOW (trademark), and PIGMENT BLUE I (trademark) from Paul Uhlich & Company, Inc.; PIGMENT VIOLET I (trademark), PIGMENT RED 48 (trademark), LEMON CHROME YELLOW DCC 1026 (trademark), EDTOLUIDINE RED (trademark), and BON RED C (trademark) from Dominion Color Corporation, Ltd. (Toronto, CA); and NOVAPERM YELLOW FGL (trademark) and HOSTAPERM PINK (trademark) from Sanofi. Examples include E (trademark), CINQUASIA MAGENTA (trademark), available from EIDuPont de Nemours & Co. Possible colorants include black, cyan, magenta, yellow, and mixtures thereof. Examples of magenta colorants include 2,9-dimethyl-substituted quinacridone and anthraquinone dyes, identified as CI 60710 and CI Dispersed Red 15 in the Color Index (CI), and diazo dyes, identified as CI 26050 and CI Solvent Red 19 in the Color Index. Exemplary examples of cyanides include copper tetra(octadecylsulfonamide) phthalocyanine, x-copper phthalocyanine pigment, listed as CI 74160 and CI Pigment Blue and Pigment Blue 15:3 in the Color Index, and Anthrathrene Blue, identified as CI 69810 and Special Blue X-2137 in the Color Index. An example of yellow is diaryloid yellow 3, which is identified as a monoazo pigment in the color index as CI 12700, CI Solvent Yellow 16.These include 3-dichlorobenzdene acetacetanilide, nitrophenylamine sulfonamide identified as Foron Yellow SE / GLN and CI Dispersed Yellow 33 in the color index, 2,5-dimethoxy-4-sulfonanilide, phenylazo-4'-chloro-2,5-dimethoxyacetacetanilide, and Permanent Yellow FGL. Colored magnetites, such as mixtures of MAPICO BLACK® and cyanide components, may also be selected as colorants. For example, Levanyl Black A-SF (Miles, Bayer) and Sunsperse Carbon Black LHD 9303 (Sun Chemicals), as well as coloring dyes, for example, Neopen Blue (BASF), Sudan Blue OS (BASF), PV FAST Blue B2G01 (Sanofi), Sunsperse Blue BHD 6000 (Sun Chemicals), Irgalite Blue BCA (Ciba-Geigy), Paliogen Blue 6470 (BASF), Sudan III (Matheson, Coleman, Bell), Sudan II (Matheson, Coleman, Bell), Sudan IV (Matheson, Coleman,Bell), Sudan Orange G(Aldrich), Sudan Orange 220(BASF), Paliogen Orange 3040(BASF), Ortho Orange OR 2673(Paul Uhlich), Paliogen Yellow 152, 1560(BASF), Lithol Fast Yellow 0991K(BASF), Paliotol Yellow 1840(BASF), Neopen Yellow(BASF), Novoperm Yellow FG 1(Sanofi), Permanent Yellow YE 0305(Paul Uhlich), Lumogen Yellow D0790(BASF), Sunsperse Yellow YHD 6001(Sun Chemicals), Suco Gelb L1250(BASF), Suco Yellow D1355(BASF), Hostaperm Pink E(Sanofi), Fanal Pink D4830(BASF), Cinquasia Other known colorants may be used, such as Magenta (DuPont), Lithol Scarlet D3700 (BASF), Toluidine Red (Aldrich), Scarlet for Thermoplast NSD PS PA (Ugine Kuhlmann, CA), ED Toluidine Red (Aldrich), Lithol Rubine Toner (Paul Uhlich), Lithol Scarlet 4440 (BASF), Bon Red C (Dominion Color Co.), Royal Brilliant Red RD-8192 (Paul Uhlich), Oracet Pink RF (Ciba-Geigy), Paliogen Red 3871K (BASF), Paliogen Red 3340 (BASF), Lithol Fast Scarlet L4300 (BASF), and combinations thereof. Optional wax

[0068] The antimicrobial toners of this disclosure may optionally contain wax, which may be either a single type of wax or a mixture of two or more different waxes. If wax is present, it may be present in an amount of, for example, about 1% to about 25% by weight of the toner particles, or about 5% to about 20% by weight of the toner particles. The melting point of the wax may be at least about 60°C, at least about 70°C, or at least about 80°C. Examples of waxes that can be selected include waxes having a weight-average molecular weight of about 500 to about 20,000 and about 1,000 to about 10,000. The wax particles may have a size of about 125 nm to about 250 nm, about 150 to about 225 nm, or about 175 to about 200 nm.

[0069] Examples of waxes that can be used include polyolefins such as polyethylene, polypropylene, and polybutene waxes commercially available from Allied Chemical and Petrolite Corporation, such as POLYWAX® polyethylene wax from BAKER Petrolite, wax emulsions available from Michaelman, Inc. and Daniels Products Company, EPOLENE N-15® commercially available from Eastman Chemical Products, Inc., and VISCOL, a low weight-average molecular weight polypropylene available from Sanyo Kasei KK. Examples include: 550-P (trademark), plant-based waxes such as carnauba wax, rice wax, candelilla wax, lacquer wax, and jojoba oil; animal-based waxes such as beeswax; mineral waxes and petroleum-based waxes such as montane wax, ozokerite, ceresin, paraffin wax, microcrystalline wax, and Fischer-Tropsch wax; ester waxes obtained from higher fatty acids and higher alcohols such as stearyl stearate and behenyl behenate; ester waxes obtained from higher fatty acids and monohydric or polyhydric lower alcohols such as butyl stearate, propyl oleate, glyceride monostearate, glyceride distearate, and pentaerythritol tetrabehenate; ester waxes obtained from higher fatty acids and polyhydric alcohol multimers such as diethylene glycol monostearate, dipropylene glycol distearate, diglyceryl distearate, and triglyceryl tetrastearate; sorbitan higher fatty acid ester waxes such as sorbitan monostearate, and cholesterol higher fatty acid ester waxes such as cholesteryl stearate.Examples of functionalized waxes that may be used include, for example, amines, amides, e.g., AQUA SUPERSLIP 6550™ and SUPERSLIP 6530™ available from Micro Powder Inc.; fluorinated waxes, e.g., POLYFLUO 190™, POLYFLUO 200™, POLYSILK 19™, and POLYSILK 14™ available from Micro Powder Inc.; mixed fluorinated amide waxes (e.g., MICROSPERSION 19™ available from Micro Powder Inc.); imides, esters, quaternary amines, carboxylic acids, or acrylic polymer emulsions (e.g., JONCRYL 74™, 89™, 130™, 537™, and 538™, all available from SC Johnson Wax); and chlorinated polypropylene and polyethylene available from Allied Chemical, Petrolite Corporation, and SC Johnson Wax. The aforementioned wax mixtures and combinations may also be used in the embodiments. shell

[0070] The toner particles of this disclosure include a shell surrounding aggregated core particles, the shell containing metal(I) ions. Silver metal ions are known to have antimicrobial properties and may be referred to as antimicrobial metal ions. Suitable antimicrobial metals and metal ions include, but are not limited to, silver, copper, zinc, gold, mercury, tin, lead, iron, cobalt, nickel, manganese, arsenic, antimony, bismuth, barium, cadmium, chromium, and thallium. In some embodiments, metal oxides, such as zinc oxide, magnesium oxide, aluminum oxide, copper oxide, and titanium dioxide, can be used as antimicrobial particles. For example, metal ions of silver, copper, zinc, and gold, or combinations thereof, are considered safe for human contact. Therefore, silver ions, alone or in combination with copper or zinc or both, have a high ratio of effectiveness to toxicity, i.e., high effectiveness to low toxicity.

[0071] For example, a combination of silver and copper ions provides both the antibacterial properties of silver ions and the antifungal properties of copper ions. Therefore, toner particles can be formulated by selecting specific metal ions and their combinations to be incorporated into the surrounding shell for a particular end application.

[0072] The shell contains metal ions such as AgNP. In some embodiments, the shell further comprises a styrene / acrylate resin and / or a polyester resin. In some embodiments, the shell may include non-antimicrobial reagents such as resins, conductive materials such as colorants, etc., as known in the art. The shell can coat all or part of the outer surface of the core of the toner particles.

[0073] The particle size of metal nanoparticles is measured by the average diameter of the particles. Metal nanoparticles can have particle sizes in the following ranges: approximately 5 nm to 500 nm, approximately 10 nm to 200 nm, and approximately 20 nm to 50 nm.

[0074] In some embodiments, metal nanoparticles may have a particle size of about 1 nm to about 15 nm, or 3 nm to 10 nm. In some embodiments, metal nanoparticles may have a uniform particle size with a narrow particle size distribution. The particle size distribution can be quantified using the standard deviation of the average particle size of the population. In some embodiments, metal nanoparticles have a narrow particle size distribution with a standard deviation of average particle size of about 3 nm or less, or about 2.5 nm or less. In some embodiments, metal nanoparticles have an average particle size of about 1 nm to about 10 nm, with a standard deviation of about 1 nm to about 3 nm. Although not bound by theory, it is thought that small particle sizes with a narrow particle size distribution can allow for easy dispersion of metal nanoparticles when added to a solvent, providing a more uniform coating of core toner particles.

[0075] In some embodiments, the metal nanoparticles may consist solely of elemental silver or may be silver composites, such as composites with other metals. Such silver composites may contain either or both (i) one or more other metals and (ii) one or more nonmetals. Suitable other metals include, for example, Al, Au, Pt, Pd, Cu, Co, Cr, In, and Ni, transition metals such as Au, Pt, Pd, Cu, Cr, Ni, and mixtures thereof. Exemplary metal composites are Au-Ag, Ag--Cu, Au--Ag-Cu, and Au--Ag--Pd. Suitable nonmetals in the silver composite include, for example, Si, C, and Ge. The various non-silver components in the silver composite may be present in amounts ranging, for example, about 0.01% to about 99.9% by weight and about 10% to about 90% by weight. In some embodiments, the silver composite is a metal alloy comprising silver and one, two, or more other metals, where silver constitutes, for example, at least about 20% and more than about 50% of the weight of the nanoparticles. Unless otherwise specified, the weight percentages of the silver-containing nanoparticles described herein refer to those without stabilizers.

[0076] Silver nanoparticles composed of silver composites can be produced, for example, by using a mixture of (i) a silver compound (one or more, such as a silver(I) ion-containing compound) and (ii) another metal salt (one or more) or another nonmetal (one or more) during the reduction process. In some embodiments, a surfactant solution can be prepared from an anionic surfactant and water, heated, and purged with nitrogen. Once thermal equilibrium is reached, an emulsion of core monomers (optionally containing a surfactant), including styrene acrylate monomers (e.g., styrene and butyl acrylate), optional chain transfer monomers, and optional branching monomers, can be slowly added to the heated aqueous surfactant solution. An aqueous solution of an initiator such as ammonium persulfate or potassium can be slowly added to the reactor to form a core resin polymer.

[0077] After the formation of the core latex, an emulsion of shell monomers may be prepared and added to the core particle emulsion, thereby forming a shell containing a composite styrene / acrylate-metal ion polymer resin to cover or encapsulate a portion of the surface of the core particles, i.e., to cover the entire or completely surface. The shell emulsion, shell monomers, such as silver (meth)acrylate and methyl methacrylate, optional chain transfer monomers, and optional chain branching monomers may be added to an aqueous solution optionally containing a surfactant. The shell emulsion may be added to a reactor containing optionally heated core particle latex, thereby forming a "surface seed" on the core resin particles. To complete the polymerization of the shell resin, an aqueous solution of an initiator such as ammonium persulfate or potassium may be slowly added to the reactor. After all reactants have been added, the emulsion may be mixed and the temperature may be maintained for a long period of time, such as about 6 to 24 hours. After the polymerization reaction is complete, the emulsion may be cooled, and the resin particles may be filtered or sieved using a 25 μm screen or the like.

[0078] In some embodiments, the shell monomer comprises at least one of the above-mentioned metal acrylate monomers and the above-mentioned styrene / acrylate monomer, and in some embodiments, the shell comprises a polymer comprising a metal methacrylate and / or metal acrylate, for example, silver acrylate or silver methacrylate.

[0079] Composite antimicrobial nanoparticles can have sizes ranging from approximately 5 nm to 500 nm, or 10 to 200 nm, or approximately 25 to 150 nm, or 50 to 100 nm. Composite nanoparticles may be smaller in size than composite resin particles, for example, when measured by dynamic light scattering. This may stem from polymerizing the shell resin in situ instead of forming a shell resin and adding it to the core particles. Polymerization of composite ionomer resins can result in entanglement of ionic polymer chains, as can be seen from molecular weight measurements, and the particles have a larger diameter than composite nanoparticles. Furthermore, the interaction between the ionic metal and carboxyl groups of the composite resin functions as an ionic crosslink, improving solubility in chemical solvents. g This can affect the properties of composite ionomers and nanoparticles, including those composite ionomers, such as molecular weight and water sensitivity.

[0080] In some embodiments, the toner particles may contain a composite styrene acrylate ionomer resin. In the case of core-shell toner particles, the ionomer resin may be present in the core, the shell, or both. In the case of core-shell toner particles, the composite nanoparticles may be present in the core, the shell, or both. Methods for preparing toner particles, such as emulsion agglutination methods for producing toner particles containing a core and a shell, are well known, as described in U.S. Patents 5,302,486, 6,294,306, 7,985,526, and 8,383,310, each of which is incorporated herein by reference in whole.

[0081] Therefore, the ionomer or core-shell particles of interest can be combined with other optional resins, such as different types of or metal ion-free styrene / acrylate resins, polyester resins, other resins, optional surfactants, optional waxes, optional colorants, and optional other toner reagents. After growing the toner particles to a technically appropriate size, such as about 2 μm to about 8 μm, the surface of the toner particles can be polished to form smooth, rounded particles for use as toner in any known imaging material and method in which the toner is displayed as an image on a fabric layer.

[0082] The binder resin core may further comprise at least one of additional resins, waxes, coagulants, and stabilizers. In one embodiment, the binder resin core essentially comprises a binder resin and at least one of additional resins, waxes, coagulants, and stabilizers. In one embodiment, the binder resin core comprises an amorphous polyester and optionally a crystalline polyester.

[0083] In one embodiment, the antimicrobial toner may contain a plurality of toner particles. As shown in Figure 5, each toner particle 300 may include a binder resin core 301 and a shell 302 arranged around the binder resin core. The binder resin core 301 may contain a single binder resin. The shell 302 may contain a plurality of metal nanoparticles 303. For example, the shell 302 may be formed of a matrix material on which the metal nanoparticles 303 are arranged. The shell may have a shell thickness of about 0.001 μm to about 2.0 μm. In one embodiment, the toner particles may contain metal nanoparticles in an amount of about 0.00001% to about 10% by weight of the toner particles, or about 0.01% to 10% by weight of the metal nanoparticles. The binder resin core may be prepared by a method that includes forming an aggregate of binder resin. To avoid the metal nanoparticles being incorporated into the binder resin core, the binder resin aggregate should not be formed in the presence of metal nanoparticles.

[0084] The binder resin core 301 can be encapsulated within the shell 302. In addition to metal nanoparticles, the shell may include a matrix on which the metal nanoparticles are arranged, a matrix formed of a resin such as an amorphous polyester resin. The shell may not contain crystalline polyester. In one embodiment, the shell matrix is ​​the same resin as the binder resin of the core. In another example, the shell matrix is ​​formed of a resin having a Tg higher than that of the core resin.

[0085] In one embodiment, each metal nanoparticle may include silver (Ag) nanoparticles. The silver nanoparticles formed in the shell portion of the toner particles can be sourced from silver nanoparticles, such as redispersible dried silver nanoparticles available from NanoComposix (San Diego, Calif.), which are formulated to have a surface coating with a polymer or alkanethiol so that the nanoparticles can be easily redispersed as non-aggregating dispersions in various solvents. Preferred silver nanoparticles include those having a polyvinylpyrrolidone (PVP) surface coating of only 0.3 to 4.0% by mass, and the nanoparticle size can be in the range of 10 to 100 nm with a narrow distribution (coefficient of variation (CV) < 15%). Organically dispersible silver nanoparticles that do not aggregate after dispersion in hexane, toluene, chloroform and many other organic solvents can be used in some embodiments. These silver nanoparticles may be available in a size of 4 nm (CV < 20%). In some embodiments, the other silver nanoparticles formed on the shell portion of the toner particles may be those available from Sigma-Aldrich (St. Louis, Mo, product numbers 730785, 730777, 730793, 730807, 730815), having diameters of 10 nm, 20 nm, 40 nm, 60 nm, and 100 nm, and having a citrate-stabilized surface with a concentration of 0.02 mg / mL.

[0086] Silver nanoparticles can be synthesized. For example, 1.0 × 10⁶ in 100 mL of deionized water (DIW) -3 A cold, ice-cold aqueous solution of silver nitrate (M) is added to 300 mL of DIW (Dioxide-Induced Water) in a volume of 2.0 × 10⁻⁶ -3 It can be mixed with an ice-cold aqueous solution of sodium borohydride (M). When the two solutions are mixed, the Ag ions are reduced, forming monodisperse nanoparticles as a clear solution in the aqueous solvent. This reaction can be described by the equation AgNO3 + NaBH4 → Ag + 1 / 2H2 + 1 / 2B2H6 + Na-NO3.

[0087] The formed Ag solution is yellow due to its absorbance at approximately 400 nm, which is characteristic of silver nanoparticles due to surface plasmon excitation. The solution can be repeatedly stirred until it stabilizes (approximately 1 hour) once it darkens. Once stabilized, the Ag nanoparticle solution may remain color-unchanged for approximately 3 months without a stabilizer.

[0088] As shown in Figure 3, toner particles can be deposited to form a printed image 88. Substantially all toner particles, or each toner particle 300 (Figure 5), may include a binder resin core 301 (Figure 5) and a shell 302 (Figure 5) positioned around the binder resin core. The binder resin core 301 (Figure 5) may include at least one of the binder resins. The shell 302 may include a plurality of metal nanoparticles 303 (Figure 5). The binder resin core may be prepared by a method that includes forming an aggregate of binder resins. To avoid the metal nanoparticles being incorporated into the binder resin core, the binder resin aggregate should not be formed in the presence of metal nanoparticles.

[0089] The hydrophobic properties of the antimicrobial image prevent droplets from passing through the fabric. The droplets remain on the surface of the printed cotton sheet and are then absorbed by the antimicrobial toner image disclosed above within up to 60 seconds. Untreated cotton absorbs water in less than 1 second.

[0090] Woven cotton fabrics typically have pore sizes of 1 μm to 5 μm. Chiffon and silk have larger pore sizes. Canvas has smaller pore sizes.

[0091] This disclosure leverages known and recently developed hardware configurations for image formation and fusion / drying technologies using fabrics to enable highly practical applications for printing on fabrics such as cotton (natural and synthetic), canvas, chiffon, and silk. In addition to facilitating high-quality printing on flexible materials, this disclosure also describes a method for significantly increasing the printable format size beyond known system capabilities.

[0092] The smaller the pore size of the fabric used to make the mask, the more surface area is covered, making the image printing of antimicrobial AgNP more effective. Therefore, the fabric can be made N95 quality by printing a solid layer of toner on each surface (up to 5 layers in iGen). This layering scheme brings some of the pores in the fabric (0.5 μm pores) closer to the N95 range (0.3 μm pores).

[0093] Many types of face masks exist. They are evaluated based on their ability to filter very small particles. This specification discloses antimicrobial protection by providing a printed pattern of silver nanoparticles on any (typically at least three) fabric layers. The outer layer also provides a fashionable appearance.

[0094] The smaller the pore size of the fabric used to manufacture items such as face masks, scarves, T-shirts, and bandanas, the more surface area the image covers, making the printing of antimicrobial AgNP images more effective. Therefore, woven fabrics can achieve N95-like quality by printing a solid layer of toner on each surface (up to 5 layers in iGen).

[0095] It will be understood that various features and functions disclosed above, or alternatives thereof, may be desirablely combined with many other different systems or applications. Various alternatives, modifications, variations, or improvements not currently anticipated or anticipated may be made thereafter by those skilled in the art, and these are also intended to be covered by the following claims. [Examples]

[0096] This invention discloses a method for producing a type of fabric layer having antimicrobial properties using silver nanoparticles via printing.

[0097] In Figure 6A illustrating this method, AgNP 22 is impregnated into the fabric 21. The AgNP 22 is randomly dispersed throughout the fibers of the fabric 21. Figure 6B shows one embodiment disclosed herein, in which the fibers of the fabric 21 are coated with fused antimicrobial toner 23. In the embodiments disclosed herein, the fibers of the fabric 21 are coated with fused antimicrobial toner 24 to a thickness of 60 μm to 100 μm using acoustic transfer assistance (ATA) technology as shown in Figure 6C. By using ATA, the fibers can be coated more effectively, and better antimicrobial protection is provided.

[0098] Figure 7 shows a water droplet 40 on a cotton fabric 41 printed with the antimicrobial toner 42 described above. The water droplet was not absorbed by the cotton fabric for at least 60 seconds.

[0099] It will be understood that various features and functions disclosed above, or alternatives thereof, may be desirablely combined with many other different systems or applications. Furthermore, various currently unforeseen or unprecedented alternatives, modifications, variations, or improvements may be made by those skilled in the art, and these are also intended to be covered by the following "Claims." Unless specifically enumerated in the Claims, no process or component of the Claims should be implied or understood in any particular order, number, position, size, shape, angle, color, or material from this Specified or any other Claims.

Claims

1. 1. A method for forming an image on a fabric, comprising: a carrier layer including a first surface including a first region, a second surface opposite the first surface, and a first stiffness; a fabric layer including a third surface, a fourth surface opposite the third surface including the second region, and a second stiffness lower than the first stiffness; Adhesive and A printable medium comprising: providing, the fabric layer being secured to the carrier layer by adhering a first portion of the fourth surface to the first surface; applying a pretreatment to the fabric layer by depositing a white dry marking material onto the fabric layer to fill one or more pores in the fabric layer with the white dry marking material; applying a toner to a first portion of the third surface of the fabric layer, the toner comprising a size between 4 microns and about 20 microns, the toner comprising antimicrobial nanoparticles on an outer surface of the toner, the antimicrobial nanoparticles having a size between 5 nanometers and 500 nanometers; fusing the toner to the first portion of the third surface of the fabric layer.

2. The method of claim 1, wherein the fused toner forms an image having a resolution of from 600 dpi to 2400 dpi.

3. The method of claim 1 , wherein the fused toner forms an image in which water droplets are not absorbed for at least 60 seconds.

4. The method of claim 1 , wherein the fabric layer is selected from the group consisting of cotton, chiffon, silk, and canvas.

5. The method of claim 1 , wherein the fabric layer having the fused toner thereon has a pore size of less than 3 microns.

6. The method of claim 1 , wherein the antimicrobial nanoparticles comprise silver.

7. The method of claim 1 , wherein the toner comprises a polyester resin.

8. The method of claim 7, wherein the polyester resin is amorphous or crystalline.

9. The method of claim 1, wherein applying a pretreatment to the fabric layer is performed prior to applying a toner to the fabric layer.

10. 1. A printed article comprising: a fabric having a first surface and a second surface opposite the first surface; a pretreatment layer disposed on the first surface of the fabric, the pretreatment layer comprising a white dry marking material filling one or more pores of the fabric layer, the pretreatment layer reducing the porosity of the first surface of the fabric compared to the porosity of the first surface of the fabric absent the pretreatment layer; a toner image disposed on the pretreatment layer, the toner image comprising toner particles having a size between 4 microns and about 20 microns and antimicrobial nanoparticles on an outer surface of the toner, the antimicrobial nanoparticles having a size between 5 nanometers and 500 nanometers.

11. The printed article of claim 10, wherein the toner image has a resolution of 600 dpi to 2400 dpi at 2400 dpi.

12. 11. The printed article of claim 10, wherein the fused toner forms an image in which water droplets are not absorbed for at least 60 seconds.

13. 11. The printed article of claim 10, wherein the fabric is selected from the group consisting of cotton, chiffon, silk, and canvas.

14. The printed article of claim 10 comprising a face mask.

15. 15. The printed article of claim 14 having a pore size of less than 3 microns.

16. The printed article of claim 10 , wherein the antimicrobial nanoparticles comprise silver.

17. The printed article of claim 10 , wherein the toner comprises a polyester resin.

18. 20. The printed article of claim 17, wherein the polyester resin is amorphous or crystalline.

19. 1. A method for forming an image on a fabric, comprising: a fabric layer comprising a carrier layer including a first surface including a first region, a second surface opposite the first surface, and a first stiffness; a third surface, a fourth surface opposite the third surface including the second region, and a second stiffness lower than the first stiffness; Adhesive and A printable medium comprising: providing, the fabric layer being secured to the carrier layer by the adhesive adhering a first portion of the fourth surface to the first surface; applying a pretreatment to the fabric layer, the pretreatment comprising depositing a white dry marking material on the fabric layer, thereby filling one or more pores of the fabric layer with the white dry marking material; applying a toner to a first portion of the third surface of the fabric layer, the toner comprising a size between 4 microns and about 20 microns, the toner comprising antimicrobial nanoparticles, the antimicrobial nanoparticles having a size between 5 nanometers and 500 nanometers; fusing the toner to the first portion of the third surface of the fabric layer to form a fused toner image.

20. 20. The method of claim 19, wherein the toner is applied using an acoustic transfer technique.

21. The method of claim 19, wherein the fused toner has a resolution of from 600 dpi to 2400 dpi.

22. 1. A printed article comprising: a fabric having a first surface and a second surface opposite the first surface; a pretreatment layer disposed on the first surface of the fabric, the pretreatment layer comprising a white dry marking material filled into one or more pores of the fabric layer, the porosity of the first surface of the fabric being reduced compared to the porosity of the first surface of the fabric absent the pretreatment layer; a toner image disposed on said pretreatment, said toner image comprising toner particles having a size of from 4 microns to about 20 microns, and antimicrobial nanoparticles, said antimicrobial nanoparticles having a size of from 5 nanometers to 500 nanometers, said toner image having a resolution of from 600 dpi to 2400 dpi.

23. 23. The printed article of claim 22, wherein the antimicrobial toner particles are selected from the group consisting of silver, copper, zinc, gold, mercury, tin, lead, iron, cobalt, nickel, manganese, arsenic, antimony, bismuth, barium, cadmium, chromium, and thallium, zinc oxide, magnesium oxide, aluminum oxide, copper oxide, and titanium dioxide.

24. 23. The printed article of claim 22, wherein the fabric is selected from the group consisting of cotton, chiffon, silk, and canvas.