Improved microgranulation method and product particles thereof

JP2022546264A5Inactive Publication Date: 2024-10-11NOVONIX BATTERY TECH SOLUTIONS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2022510172
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-05-05
Filing Date
2020-07-24
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Current methods for producing uniform, micron-sized spherical or round particles with narrow size distribution are inefficient, energy-intensive, and generate significant waste, particularly in the production of electrode materials for lithium ion batteries, as they often require additional processing steps and solvents, leading to non-uniform particle sizes and internal voids.

Method used

A high-shear and high-pressure mechanofusion process is employed to agglomerate precursor particles using a templating medium, allowing for the production of uniform, spherical or round product particles with narrow size distribution and smooth surfaces, eliminating the need for solvents and reducing waste.

Benefits of technology

The method efficiently produces uniform, spherical product particles with narrow size distribution and smooth surfaces, suitable for use in battery electrodes, while minimizing environmental impact and reducing production costs.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

A simple, material-efficient microgranulation method is disclosed for agglomerating precursor particles into larger product particles with improved properties and, in some instances, novel structures. The product particles are useful for applications requiring uniform, smooth, spherical, or round particles, such as electrode materials in lithium batteries, and other applications.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] Technical field This invention relates to an improved microgranulation method for aggregating precursor particles into larger product particles having improved properties and, in some examples, novel structures. The product particles are useful as electrode materials for lithium batteries and for other applications. [Background technology]

[0002] background Many applications require powders consisting of high-density particles in a micron diameter range (e.g., 1-100 μm) with a narrow particle size distribution (e.g., active powders for battery electrodes, fertilizers, pharmaceuticals, toners, pigments, fillers, catalysts, etc.). For some of these applications, spherical or round particles are desirable. However, producing particles with uniform shape and diameter within the micron diameter range is difficult.

[0003] For example, in the manufacture of electrodes for rechargeable high-energy-density batteries such as lithium-ion batteries, it may be desirable for particles to be spherical in shape and have a uniform diameter. If there is substantial demand for these batteries, it is also very important to be able to provide a significant and economical supply of such materials. Currently, cathode particles for lithium-ion batteries (e.g., lithium nickel manganese cobalt oxide or NMC) are often manufactured by a coprecipitation process in a continuous flow tank reactor. This results in a wide particle size distribution due to the diverse particle residence times in the reactor. In addition, careful process control and various chemical additives (e.g., chelating agents) are required to maintain a uniform precipitation rate of different metal salts and to achieve a uniform spherical particle shape. Furthermore, after the coprecipitation process, and before sintering, the particles must be separated from their mother liquor by filtration, washing, drying, and blending with a lithium source, thereby generating additional processing steps and energy, chemicals, and wastewater. Anode particles for lithium-ion batteries are typically carbonaceous, such as graphite particles. Typically, to produce battery-grade graphite from natural graphite, the natural graphite is first crushed and classified to obtain powder with the desired diameter distribution (approximately 10-20 μm). Then, a spheronizer is used to spheronize the diameter-defined powder. However, the spheronizing process is typically only 50-60% efficient, resulting in a mixture of the desired spheronized particles and fine particles smaller than 5 μm in diameter. The resulting mixture requires an additional classification step to separate the desired particles from the fine particles, which are typically discarded as waste. Clearly, a significant amount of starting natural graphite is lost as a result.

[0004] Granulation is a method by which smaller particles can aggregate into larger particles. Granulation methods include both wet and dry methods. Wet granulation methods include fluid layer, disk, drum, and mixer methods (e.g., using pins, paddles, and / or blades). Such wet methods require separation of product particles from the liquid and may require additional binders or dispersion aids. Dry granulation methods include roll presses, tableting, ram / piston extrusion, pelletizing mills, radial extrusion, and axial exclusion. However, both wet and dry granulation methods have problems in producing uniform product particles with a diameter of less than 100 μm, and the resulting product particles often contain internal voids.

[0005] Other methods for producing micron-sized spherical or round particles include spray drying and prillation. During spray drying, a fluid containing a liquid (typically water) and suspended fine particles and / or dissolved seeds is sprayed through a nozzle to form droplets. The fluid may further contain additives such as wetting agents and binders. The droplets released from the spray nozzle are dried in the air (e.g., by airflow) and captured by a filter. This method can be expensive and wasteful because removing the liquid during the drying step is typically energy-intensive and often results in the loss of liquid as waste. The resulting powder is often porous and may require further processing (e.g., washing and filtration). Prillation is a method by which a molten liquid spray solidifies in flight. This method is only applicable to materials that can form a molten state.

[0006] There is a need for a method for micro-scale dry granulation (i.e., microgranulation) in which smaller particles (e.g., less than approximately 1 μm) can aggregate to form larger, denser, and more uniform micron-sized particles that are spherical or round, without forming a significant amount of waste fine particles. However, according to U.S. Patent No. 9,132,482, "the extremely insufficient amount of literature on the granulation of inorganic nanopowder demonstrates the problems with conditioning them in granular form."

[0007] Physical methods utilizing dry processes are environmentally friendly and advantageous for industrial applications because they eliminate the use of solvents. The mechanofusion (MF) process was developed in Japan in the mid-1980s and is based on using a high shear field to spheroidize and sizing powder without the use of any liquid, or to dry-coat it (see T. Yokoyania, K. Urayama and T. Yokoyama, KONA Powder Part. J., 1983, 1, 53-63). In the lithium-ion battery field, MF is commonly used to spheroidize and sizing natural graphite for use in negative electrodes (e.g., U.S. Patent No. 9,142,832 or U.S. Patent Application No. 14 / 431,398).

[0008] Despite its industrial utility, MF (microwave manipulation) is rarely documented in the literature. One reason for this may be that the parameters for using MF devices are not widely known. Nevertheless, some publications describe particles that have been spheroidized and sizing by the MF method or coated with another phase (e.g., M. Naito, M. Yoshikawa, T. Tanaka and A. Kondo, KONA Powder Part. J., 1993, 11, 229-234, N. Product and M. Features, 1999, 17, 244-250, M. Alonso, M. Satoh and K. Miyanami, Powder Technol., 1989, 59, 45-52, M. Naito, A. Kondo and T. Yokoyama, ISIJ Int., 1993, 33, 915-924, R. Pfeffer, RN Dave, D. Wei and M. Ramlakhan, Powder Technol., 2001, 117, 40-67, W. Chen, RN Dave, R. (Pfeffer and O. Walton, Powder Technol., 2004, 146, 121-136, and C.-S. Chou, C.-H. Tsou and C.-I. Wang, Adv. Powder Technol., 2008, 19, 383-396). However, most publications do not adequately describe the conditions under which such designed particles are manufactured.

[0009] An interesting type of graphite material known as "onion graphite" has been observed in this technology. According to some, onion graphite refers to spherical or oval graphite particles in which the graphite base planes are arranged in a nested oval or spherical smooth concentric layer with the center around a common point of the particle core, and the arrangement of the edges of the graphite sheet does not extend radially from the central core (onion graphite refers only to a perfect nested buckyball). In other words, the graphene layers in onion graphite are randomly placed on the surface of the concentric nested sphere or oval, except that they are oriented so that their base planes are tangential to the concentric nested sphere or oval. Onion graphite is known to have a microstructure in which graphite base planes are concentrically arranged, but the edges of the planes radiate outwards from a central core, and can be identified from cast iron graphite spheres (for example, as shown in Figure 6-4 of "Mesomolecules: From Molecules to Materials" SEARCH Series, Volume 1, G. David Mendenhall, Arthur Greenberg, and Jeol F. Liebman, eds., Chapman & Hall, New York, 1995). Previously, onion graphite had only been observed in diameters up to 2 μm. As evidenced by their presence in meteorites, they have been found to form in interplanetary space. Conventionally, nanoscale graphite onions were produced in small quantities by synthetic methods, such as high-electron irradiation of carbon particles, annealing of nanodiamonds, arc discharge between two graphite electrodes submerged in water, and carbon ion implantation of silver or copper substrates (see, for example, VD Blank, BA Kulnitskiy and IA Perezhogin, Scripta Materialia, 60 (2009) 407-410).None of these methods can produce particles larger than 2 μm in diameter, in volume (i.e., larger than 1 gram), in a highly graphitized state, and in an economically practical way. For example, U.S. Patent Application Publication No. 2013 / 0189178A1 describes a method for producing onion-like carbon, but the maximum diameter of the achieved carbon onions is only 6 nm. Furthermore, the achieved level of graphitization is not described.

Summary of the Invention

Problems to be Solved by the Invention

[0010] Despite such continuous and substantial overall efforts related to developing improved manufacturing methods for such materials, further improvements are needed. As disclosed below, the present invention addresses these needs and provides additional advantages.

Means for Solving the Problems

[0011] Summary[[ID=--]] It has been discovered that specific high-shear and high-pressure field processes, such as dry mechanical fusion (MF), can be used to prepare desirable aggregates from various precursor particles in a simple manner and with efficient utilization of the precursor particles. Aggregated precursor particles ("product particles") can be desirably produced with a narrow particle size distribution and in a smooth spherical or rounded shape without cavities. In some embodiments, it is possible for cavities to be included in the product particles.

[0012] In particular, the product particles are produced using a microgranulation method comprising the following steps: obtaining a certain amount of precursor particles having an average particle size of less than 1000 μm; obtaining a certain amount of a templating medium having an average particle size of less than 500 μm and a hardness higher than that of the precursor particles; and preparing a mixture containing the above amounts of precursor particles and templating medium. The mixture is then subjected to a suitable high-shear and high-pressure field, such as that obtained by mechanofusion, so that the precursor particles aggregate into the desired product particles. The product particles can then be separated from the templating medium, if desired for the intended application.

[0013] The method described above can be successfully used with a wide range of precursor particles of many types having a broad range of properties. This includes precursor particles with an average diameter of less than 50 μm, particularly less than 10 μm. Suitable types of precursor particles include powders intended for use (directly or after subsequent processing) in battery electrodes, fertilizers, pharmaceuticals, toners, pigments, fillers, or catalysts. As demonstrated in the examples below, suitable precursor particles include carbonaceous powders, mixed metal oxide powders, or metal carbonate powders, such as carbon, graphite flakes, or LiNi 1 / 3 Mn 1 / 3 Co 1 / 3 O2 powder is included. Advantageously, the mixed metal oxide powder used as precursor particles may be produced by an all-solid-state method, which includes ball milling of a certain amount of metal oxide raw material powder to produce the precursor particles. (For example, it should be noted that the precursor particles used in the following examples are not suitable for use in battery electrodes, but can be made suitable for such use by micro-granulation and optionally by subsequent processing steps, such as heating.) Furthermore, and generally, at least a portion of such an amount of precursor particles may be treated in some suitable manner (including ball milling or heating) before preparing the mixture.

[0014] The method of the present invention preferably produces spherical and / or rounded aggregates, but the starting precursor particles can be powders that are very irregularly shaped. Additionally, the method of the present invention preferably produces powders with a narrow particle size distribution, but the particle size distribution of the starting precursor particles can be very large.

[0015] The resulting characteristics of the resulting product particles are, in part, the effect of the characteristics of the mold medium utilized. As described above, the hardness of the mold medium is greater than the hardness of the precursor particles so as not to break the former. Accordingly, suitable mold media can be selected from the group consisting of zirconium oxide, tungsten carbide, tungsten, silicon oxide, aluminum oxide, silicon nitride, hardened steel, stainless steel, and quartz. A mold medium having an average diameter of 100 μm or less can be utilized to yield product particles of a desired diameter and shape. Further, the surface of the mold medium can desirably be smooth and can be spherical. Additionally, it is desirable that the diameter distribution of the mold medium be uniform, such as (D90-D10) / D50<2, preferably (D90-D10) / D50<1, or more preferably (D90-D10) / D50<0.7. Furthermore, it may be desirable that the volume of such an amount of the mold medium utilized be higher than the volume of such an amount of the precursor particles utilized, particularly 3 times or more the volume of such an amount of the precursor particles.

[0016] A mechanofusion system suitable for use in the method of the present invention may include a chamber, a rotating wall within the chamber, a scraper within the rotating wall, and a press head within the rotating wall. A typical distance between the scraper and the rotating wall may be about 0.5 mm. A typical distance between the press head and the rotating wall may be about 1.4 mm. A typical speed for rotating the rotating wall results in a wall surface velocity of about 8 m / s. In some embodiments, mechanofusion times of about 12 hours or more have been shown to yield good results. Shorter processing times can be achieved if a mold medium already coated with a precursor from a previous synthesis is reused in the new synthesis. Although the system produces products in batch form, advantageously, mechanofusion can also be performed in a continuous manner (e.g., appropriate modifications are made to such a system).

[0017] In exemplary embodiments, product particles having an average diameter of 10 to 100 μm can be produced. Furthermore, the diameter distribution of exemplary product particles can be sufficiently uniform such that (D90-D10) / D50 < 2. Furthermore, the surface of the product particles may preferably be smooth. In some embodiments of the present invention, the product particles include particles having a roughness of less than 0.02, less than 0.01, less than 0.006, or even smaller (as defined below). In some embodiments of the present invention, all product particles essentially have a roughness value of less than 0.02, less than 0.01, less than 0.006, or even smaller. In some embodiments of the present invention, the product particles include particles that essentially do not contain cavities. In some embodiments of the present invention, all product particles essentially do not contain cavities. And, as demonstrated in the following examples, spherical or tetrahedral product particles can be produced.

[0018] Optionally, the complete preparation of the product particles may additionally include a high-temperature annealing step (for example, following mechanofusion to recrystallize the particles).

[0019] Product particles produced by the method of the present invention may be considered for use in a number of commercial applications, including battery electrodes, fertilizers, pharmaceuticals, toners, pigments, fillers, or catalysts. They may be particularly suitable for use as anode or cathode electrodes in rechargeable lithium batteries, such as lithium-ion batteries.

[0020] It was further found that the above method can be used to prepare novel structures of graphite nanoparticles, lithium nickel manganese cobalt oxide nanoparticles, and lithium transition metal oxide nanoparticles.

[0021] In one embodiment, the novel graphite microparticles comprise graphite particles formed as spherical or oval shapes, and which include concentric nested spherical or oval layers of graphene. These graphene layers are randomly arranged on the surfaces of the concentric nested spherical or oval shapes, except that the graphene layers are oriented such that their base planes are tangential to the concentric nested spherical or oval shapes. The graphite particles further have an average particle size greater than 2 μm and an average d of less than 3,400 Å. 002 They have spacing. In some embodiments, the graphite particles in the fine particles include a porous concentric layer having hollows or voids near their core. In some embodiments, the graphite particles have an average particle size of 5 μm to 50 μm and a diameter distribution of (D90-D10) / D50 < 2.

[0022] In one embodiment, the novel lithium mixed metal oxide nanoparticles include particles having a core of randomly oriented lithium nickel manganese cobalt crystallites having an average diameter of about 1 μm, which is coated with smaller randomly oriented lithium nickel manganese cobalt crystallites having an average diameter of about 0.3 μm.

[0023] The novel lithium transition metal oxide nanoparticles described above comprise particles having at least two transition metals belonging to the group consisting of Mn, Ni, and Co. Furthermore, the particles have an O3 structure, an average particle size in the range of 1 to 50 μm, and they contain crystallites whose shape and diameter vary randomly throughout their interior. In certain embodiments, the crystallites have an average diameter greater than 0.5 μm, and the average particle size is more than 5 times larger than the average crystallite diameter. In certain embodiments, the composition of one of the two transition metals can vary by at least 5 atomic percent from the core to the shell of the particle.

[0024] This method can be used to produce product particles having a uniform composition, but can also be used to produce product particles having a different composition near their core than near their surface. The precursor particles used may be single-phase, or they may consist of a mixture of particles having different characteristics. For example, the precursor particles may consist of a mixture of first particles of a first composition and second particles of a second composition, where the first and second compositions differ and / or the first and second particles have different average crystallite sizes (e.g., the average crystallite size of the first precursor particles differs from the average crystallite size of the second precursor particles by at least 10%).

[0025] Suitable precursor particles for forming graphite product particles include graphitizable carbons such as natural graphite, coke, and soft carbon. Suitable precursor particles for forming product particles useful as cathode materials for lithium-ion batteries include hydroxides, oxides, sulfates, nitrates, and carbonates of lithium, aluminum, magnesium, transition metals, and mixtures thereof. In the case of lithium nickel manganese cobalt oxide product particles, the suitable precursor particle is lithium nickel manganese cobalt oxide particles. In the case of lithium transition metal oxide product particles, the suitable precursor particle is lithium transition metal oxide particles. [Brief explanation of the drawing]

[0026] Brief explanation of the drawing [Figure 1]A schematic diagram of a mechanofusion system suitable for use in the microgranulation method of the present invention is shown. [Figure 2a] The SEM image of the ZrO2 template medium used in the example is shown. [Figure 2b] The SEM image of the ZrO2 template medium used in the example is shown. [Figure 2c] This shows a cross-section of a ZrO2 particle, including its peripheral region and center of mass. [Figure 2d] The interpolated radial segment values, the interpolated f(x) values, and the remaining plots of the function of x are shown. [Figure 3] The particle size distribution of the ZrO2 template medium used in the examples is shown. [Figure 4a] The SEM image of the graphite flake precursor particles used in the example is shown. [Figure 4b] The SEM image of the graphite flake precursor particles used in the example is shown. [Figure 5a] This image shows a SEM image of the product obtained after mechanofusion of a mixture of graphite flake precursor particles and a ZrO2 template medium. [Figure 5b] This image shows a SEM image of the product obtained after mechanofusion of a mixture of graphite flake precursor particles and a ZrO2 template medium. [Figure 6a] Figure 5a shows SEM images of the graphite spherical product particles after they have been separated from the ZrO2 template medium. [Figure 6b] Figure 5b shows an SEM image of the graphite spherical product particles after they have been separated from the ZrO2 template medium. [Figure 7a] This shows the 20°–65° XRD patterns of graphite flake precursor particles before mechanofusion. [Figure 7b] The XRD patterns of graphite spherical product particles at 20° to 65° after mechanofusion and separation from the mold medium are shown. [Figure 7c] This shows the XRD patterns of annealed graphite spherical product particles at 20° to 65°. [Figure 8]This shows the particle size distribution of graphite spherical product particles after annealing. For comparison, the particle size distribution of the ZrO2 mold medium is also shown (dotted line). [Figure 9a] The voltage curve shows the electrochemical performance of a cell containing graphite spherical product particles of the present invention. [Figure 9b] The electrochemical performance of a cell containing graphite spherical product particles of the present invention is shown, with corresponding differential capacitance curves. [Figure 9c] The electrochemical performance of a cell containing the graphite spherical product particles of the present invention, which demonstrates cycling performance, is shown. [Figure 10a] This image shows a SEM cross-section of a graphite spherical product particle, illustrating the entirety of the product particle. [Figure 10b] This image shows a SEM cross-section of a graphite spherical product particle, revealing various parts of the product particle at a higher magnification. [Figure 10c] This image shows a SEM cross-section of a graphite spherical product particle, revealing various parts of the product particle at a higher magnification. [Figure 10d] This shows a cross-section of a graphite spherical product particle, indicating its peripheral region and center of mass. [Figure 10e] The interpolated radial segment values ​​of the product particles, the interpolated f(x) values, and the remaining plots as a function of x are shown. [Figure 11a] The SEM image of the NMC precursor particles used in the examples, synthesized using the all-solid-state method, is shown. [Figure 11b] The SEM image of the NMC precursor particles used in the examples, synthesized using the all-solid-state method, is shown. [Figure 12a] This image shows a SEM image of the product obtained after mechanofusion of a mixture of NMC precursor particles and a ZrO2 template medium. [Figure 12b] This image shows a SEM image of the product obtained after mechanofusion of a mixture of NMC precursor particles and a ZrO2 template medium. [Figure 13a] Figure 12a shows an SEM image of the tetrahedral NMC product particles after separation from the ZrO2 template medium. [Figure 13b]Figure 12b shows an SEM image of the tetrahedral NMC product particles after separation from the ZrO2 template medium. [Figure 14a] This shows the 10° to 80° XRD patterns of NMC precursor particles before mechanofusion. [Figure 14b] The XRD patterns of tetrahedral NMC product particles at 10° to 80° after mechanofusion and separation from the template medium are shown. [Figure 14c] This shows the XRD patterns of NMC product particles after annealing, from 10° to 80°. [Figure 15] The particle size distribution of NMC product particles after annealing is shown. For comparison, the particle size distribution of the ZrO2 template medium is also shown (dotted line). [Figure 16a] The voltage curve shows the electrochemical performance of a cell containing the NMC product particles of the present invention. [Figure 16b] The electrochemical performance of a cell containing the NMC product particles of the present invention, which demonstrates cycling performance, is shown. [Figure 17a] This image shows a SEM (Scanning Electron Microwave Oxide) cross-section of an NMC product particle, illustrating the entirety of the product particle. [Figure 17b] SEM images of NMC product particle cross-sections are shown, revealing various parts of the product particles at several higher magnifications. [Figure 17c] SEM images of NMC product particle cross-sections are shown, revealing various parts of the product particles at several higher magnifications. [Figure 17d] SEM images of NMC product particle cross-sections are shown, revealing various parts of the product particles at several higher magnifications. [Figure 17e] This shows a cross-section of an NMC product particle, indicating its peripheral region and center of mass. [Figure 17f] The interpolated radial segment values ​​of the product particles, the interpolated f(x) values, and the remaining plots as a function of x are shown. [Figure 18a] The image shows SEM images of comparative NMC particles after long-term automated grinding. [Figure 18b] The image shows SEM images of comparative NMC particles after long-term automated grinding. [Figure 19]Various dimensions related to characterizing particle surface cavities from particle cross-sections or projected areas are shown. [Figure 20a] This shows an SEM image of a cross-section of a core-shell product particle according to Example 3 of the present invention. [Figure 20b] This shows an SEM image of a cross-section of a core-shell product particle according to Example 3 of the present invention. [Figure 21] The cross-sectional images of the core-shell product particles of Example 3 of the present invention are shown at the positions of five points, indicated as Spectrum 1-5. The composition was obtained by EDS. [Figure 22] The XRD pattern of the shell precursor particles of Example 4 of the present invention is shown. [Figure 23] The image shows an SEM image of the shell precursor particles of Example 4 of the present invention. [Figure 24] The XRD pattern of intermediate A in Example 4 of the present invention is shown. [Figure 25] The image shows an SEM image of intermediate A in Example 4 of the present invention. [Figure 26] The image shows an SEM image of the core precursor particles of Example 4 of the present invention. [Figure 27] The XRD pattern of the core precursor particles of Example 4 of the present invention is shown. [Figure 28a] This shows an SEM image of a cross-section of a core-shell product particle according to Example 4 of the present invention. [Figure 28b] This shows an SEM image of a cross-section of a core-shell product particle according to Example 4 of the present invention. [Figure 29] The image shows a cross-sectional view of the core-shell product particles of Example 4 of the present invention, with the positions of five points indicated as Spectrum 1-5 (from right to left). The composition was obtained by EDS. [Figure 30a] This shows an SEM image of a cross-section of a core-shell product particle according to Example 4 of the present invention. [Figure 30b] This shows the EDS elemental mapping of Ni in the cross-section of the core-shell product particle of Example 4 of the present invention. [Figure 31] The XRD pattern of the product particles of Example 4 of the present invention is shown. [Figure 32] The XRD pattern of heated product particles in Example 4 of the present invention is shown. [Figure 33] This shows an SEM image of a heated product particle cross-section according to Example 4 of the present invention. [Figure 34] The images show cross-sectional views of the heated core-shell product particles of Example 4 of the present invention, at the positions of five points indicated as Spectrum 1-5 (from left to right). The composition was obtained by EDS. [Figure 35] This shows the variation in the transition metal composition as a function of the distance from the surface of the heated product particles in Example 4 of the present invention. [Figure 36] This shows an SEM image of a heated product particle cross-section according to Example 5 of the present invention. [Modes for carrying out the invention]

[0027] Detailed explanation Unless the context requires otherwise, terms such as “comprise” and “comprising” throughout this specification and the claims shall be interpreted in a non-restrictive, comprehensive sense. Terms such as “a” and “an” shall be considered to mean at least one, and not limited to one.

[0028] In addition, the following definitions apply throughout this specification.

[0029] In this specification, the term “high shear and high pressure field” means shear and pressure conditions similar to those experienced during a typical mechanofusion process.

[0030] With respect to multiple particles, the term "irregularly shaped" is intended to mean not only individual particles with irregular shapes, but also mixtures of particles that are irregularly shaped in other ways that do not share a common shape.

[0031] The particle size distribution of a given sample is quantified herein by its "Dn" diameter, which, as conventionally defined, is the diameter of the smaller particle size for n% of the sample's mass.

[0032] Therefore, the term "average diameter" of a group of particles is defined as its D50 diameter.

[0033] The term "projected area diameter" of a particle refers to the diameter of a circle that has the same area as the projected image (i.e., its silhouette) of the particle, or the cross-section of the particle passing near its center of mass.

[0034] The term "cavity" is used to refer to a depression on the particle surface having a relative depth in the range of 0.02 to 0.1 and a relative aspect ratio greater than 0.2. Methods for quantifying relative depth and relative aspect ratio are presented in the material characterization of the following examples.

[0035] The term "roughness" is used to mean the variation coefficient determined by the spline deformation method described in the material characterization of the following examples.

[0036] The term "smooth" refers to particles with a roughness of less than 0.02.

[0037] The term "spherical" is used to refer to a particle whose surface does not vary by more than 25% in distance from the particle's center of mass.

[0038] The term "microparticles" refers to multiple particles or aggregated particles.

[0039] In quantitative relationships, the term "approximately" must be interpreted as being within a range of plus 10% and minus 10%.

[0040] The term "anode" refers to the electrode in a metal ion cell that undergoes oxidation during discharge. In a lithium-ion cell, the anode is the electrode that is delithified during discharge and lithified during charging.

[0041] The term "cathode" refers to an electrode where reduction occurs when metal ions are discharged. In a lithium-ion cell, the cathode is the electrode that is lithified during discharge and delithified during charging.

[0042] The terms "metal ion cell" or "metal ion battery" refer to alkali metal ion cells, including lithium ion cells and sodium ion cells.

[0043] The term "half-cell" refers to a cell that has a working electrode and a metal pair / reference electrode. A lithium half-cell has a working electrode and a lithium metal pair / reference electrode.

[0044] The term "active material" refers to a material that can reversibly store metal ions in the anode or cathode.

[0045] The term "anode active material" or "anode material" refers to the active material used to reversibly store metal ions in the anode. In lithium-ion cells, the anode material is lithified during charging and delithified during discharge at a potential of less than 2V relative to Li. In Li half-cells, the anode material is delithified during charging and lithified during discharge at a potential of less than 2V relative to Li.

[0046] The terms "cathode active material" or "cathode material" refer to the active material used to reversibly store metal ions in the cathode. In lithium-ion cells, the cathode material is lithified during discharge and delithified during charging at a potential of less than 2V relative to Li. In Li half-cells, the cathode material is delithified during charging and lithified during discharge at a potential of less than 2V relative to Li.

[0047] The term "cross-section" is understood to mean the cross-section that passes through the vicinity of the particle's center of mass.

[0048] The term "average crystallite size" refers to the grain size of the phase determined by the Scherrer crystallite size determination method, as will be explained in detail below. (Note: In principle, the average crystallite size can be determined not only by X-ray diffraction techniques but also from SEM images. In the former, known as the Scherrer grain size determination method, the Scherrer equation is applied to one of the X-ray diffraction peaks FWHM of the phase between 20° and 60° 2-theta under incident CuKα1 radiation. An explanation of the Scherrer equation can be found in "X-ray Diffraction" by BE Warren, Dover Publications (1990). In the latter, the average crystallite size is determined from the average of the crystallite sizes of randomly sampled crystallites observed by scanning electron microscopy.)

[0049] In this specification, the term "O3 phase" means a phase having an α-NaFeO2 type structure, as described in C. Delmas, C. Fouassier, and P. Hagenmuller, Physica, 99B (1980) 81-85. As an example, LiCoO2, which is widely used as an active cathode material in commercially available lithium-ion batteries, has an O3 structure. X-ray diffraction may be used to determine the structure of the phases in a sample, including whether the material contains a phase having an O3 structure or a phase having a graphite structure.

[0050] It has been discovered that a mechanofusion (MF) dry process method and associated high shear and high pressure fields can be utilized to produce homogeneous aggregates from various precursor particles. The MF process is relatively simple and inexpensive. Most of the precursor particles are incorporated into the product particles, and thus the precursor particles are efficiently utilized. Furthermore, since the MF process is a dry process and does not require solvents, it is potentially attractive for environmentally reliable commercial production. The required steps simply involve obtaining appropriate amounts of precursor particles and a template medium, mechanofusion these amounts of mixture for a sufficient amount of time to properly produce aggregated fine particles. After the mechanofusion process, the product particles may be separated from the template medium by known air classification, sieving, cyclone, washing, deposition, hydrocyclone, or other wet or dry methods to separate the particles based on diameter, shape, or density.

[0051] Figure 1 schematically shows an MF system 1 suitable for preparing fine particles by the method of the present invention. It consists of a rotating cylindrical chamber 2, in which a fixed round press head 3 and a fixed scraper 4 are arranged. The radius of the press head 3 is smaller than the radius of the chamber 2, and the space between the press head 3 and the chamber wall 5 is generally in the range of 1 to 5 mm. The space between the scraper 4 and the chamber wall 5 is smaller (usually about 0.5 mm). Preferably, these clearances can be adjusted for optimization depending on factors such as the chamber diameter, particle size, and powder hardness.

[0052] The operation of the MF system 1 is simple, but the mechanism by which the powder is processed in the chamber is complex (see W. Chen, RN Dave, R. Pfeffer and O. Walton, Powder Technol., 2004, 146, 121-136). During use, a powder mixture 6 (containing an appropriate amount of precursor particles and a mold medium) is placed in the chamber, and the chamber 2 is sealed. As the chamber rotates, the powder mixture 6 is pressed against the chamber wall 5 by centrifugal force. This forces the powder mixture through a confluence space between the fixed press head 3 and the rotating chamber wall 5, establishing a high shear and high pressure field. As the powder particles exit the divergent space in the press head area, they adhere to each other and to the chamber wall. The trowel 4 is useful for scraping off the powder adhering to the chamber wall 5. The sheared powder mixture is then redispersed in the chamber and moved back towards the press head area. While chamber 2 rotates, the powder undergoes a continuous process of compression, frictional shearing, and deaggregation. These interactions result in a variety of effects, including spheroidization, coating of smaller or softer particles onto larger particles, and embedding of smaller particles within larger particles. These effects occur rapidly at high rotational speeds, which are typically utilized (wall surface velocities >1000 rpm or greater than approximately 8 m / s).

[0053] As those skilled in the art will recognize, the appropriate operating parameters for an MF system can be expected to vary depending on the desired product particles and the type and amount of precursor particles and template medium used. Those skilled in the art will be able to readily determine appropriate operating parameters for a given situation based on the guidance presented in the following examples.

[0054] The method of the present invention can be used to aggregate various types of precursor particles into large, uniform product particles. In principle, any amount of any precursor particles having an average particle size of less than 1000 μm can be aggregated. [Note: In principle, it is possible to start with larger particles, up to 1000 μm, as their diameter is expected to decrease during processing. Therefore, precursor particles larger than the template medium may be used. Such particles can be pulverized in situ to smaller diameters during processing.] This method is particularly suitable for producing product particles with an average diameter of less than 100 μm and smaller (e.g., less than 50 μm or less than 10 μm).

[0055] As demonstrated in the following examples, the powder used in the battery electrodes may be agglomerated by the method of the present invention. Such precursor powders may be carbonaceous powders (e.g., graphite flakes) or conventional mixed metal oxide powders (e.g., NMC or LiNi 1 / 3 Mn 1 / 3 Co 1 / 3 This includes anode-active and cathode-active materials such as O2 powder. Suitable precursor powders include mixed metal oxide powders prepared without regard to convention, for example, those prepared using a novel all-solid-state method in which a suitable mixture of metal oxide raw material powders is ball-milled to produce mixed metal oxide precursor particles. However, it is expected that similar aggregates of powders generally intended for use as fertilizers, pharmaceuticals, toners, pigments, fillers or catalysts in other industrial applications can be readily prepared in a similar manner. A useful feature of the method of the present invention is that no special shape or particle size distribution of the starting precursor particles is required to obtain the desired target product. The precursor particles may have a regular shape or, instead, be irregularly shaped powders and may have a narrow, broad, or multimode diameter distribution.

[0056] The microgranulation method of the present invention generally involves preparing a mixture of a selected amount of precursor particles and an appropriate amount of mold medium. The mold medium is generally selected to have an average particle size of less than 500 μm and a hardness higher than that of the precursor particles. Thus, the mold medium does not break down under the high shear and pressure conditions associated with this method. Suitable material choices for the mold medium include zirconium oxide, tungsten carbide, tungsten, silicon oxide, aluminum oxide, silicon nitride, hardened steel, stainless steel, and agate. Furthermore, in other cases, the mold medium is preferably regular, smooth, and spherical, as it may break down during processing and, in particular, eventually decompose into spherical pieces, thereby contaminating the target product.

[0057] The diameter, uniformity, and quantity of the template medium used may also be important with respect to the characteristics of the desired target product fine particles. It is expected that aggregated target product particles will be somewhat smaller, but within the order of the diameter of the template medium used. Therefore, for smaller aggregates, it may be desirable that the average particle size of the template medium be less than 100 μm. Furthermore, the uniformity of the target product fine particles is expected to be approximately similar to the uniformity of the template medium used. Therefore, for a desirablely uniform final product, it may be desirable that the diameter distribution of the template medium be sufficiently uniform such that (D90-D10) / D50 < 2, preferably (D90-D10) / D50 < 1, more preferably (D90-D10) / D50 < 0.7, or that (D90-D10) / D50 is smaller. Furthermore, a sufficient quantity of template medium must be used in this method so that all present precursor particles are completely and successfully processed. In this regard, in some embodiments, the volumetric volume of the mold medium is preferably larger than the volumetric volume of the precursor particles. More specifically, when using a uniform spherical mold medium, the relevant amount of the mixture is preferably selected so that the volume of the precursor particles can fit into the void volume (which is about 1 / 3 of the volumetric volume of the spheres) present between the randomly packed spherical mold medium. Thus, a volumetric ratio of 1:3 between small precursor particles and mold medium may be preferred (i.e., the volumetric volume of the mold medium is preferably about 3 times or more the volumetric volume of the precursor particles).

[0058] The microgranulation process itself involves subjecting a suitable mixture containing a certain amount of precursor particles and a template medium to mechanofusion or other equivalent high-shear and high-pressure fields. This step is useful for agglomerating the precursor particles into product particles. Mechanofusion can be performed, for example, in the mechanofusion system shown in Figure 1. Typical settings for the process include a gap of approximately 0.5 mm between the scraper and the rotating wall, and approximately 1.4 mm between the press head and the rotating wall. Typical rotation speeds are in the order of 1000 rpm or higher, resulting in a wall surface velocity of approximately 8 m / s or higher. A mechanofusion process time of approximately 12 hours or more has been shown to be sufficient. Shorter process times can be achieved when different sample volumes, rotation speeds, powder ratios are used, or when the template medium is recycled.

[0059] In a mechanofusion process, precursor particles and template particles are in a vacuum or fluid environment, typically a gaseous atmosphere. In a simple embodiment, the gaseous atmosphere is air. However, in other embodiments, the gaseous atmosphere may be an inert gas, such as argon or nitrogen. Furthermore, the gaseous atmosphere may be reduced and may contain hydrogen or ammonia, for example, a mixture of 5% hydrogen gas and 95% nitrogen gas. Furthermore, the gaseous atmosphere may be oxidized and may contain an oxidizing gas such as oxygen or carbon dioxide.

[0060] The mechanofusion system shown in Figure 1 and discussed above is used to prepare product particles in a batch process, but the apparatus can be modified so that the preparation can instead be performed continuously. For example, during mechanofusion, particles may be continuously drawn in a particle stream from the mechanofusion machine. Then, by a continuous classification process, the desired product particles may be separated from the particle stream and collected. The unprocessed precursor particles and template medium remaining in the particle stream may then be returned to the mechanofusion machine. Additional precursor particles may be continuously added to the mechanofusion machine to replace the product particles removed by classification. In this way, product particles can be continuously produced and collected.

[0061] After the mechanofusion or equivalent process steps are completed, the product particles are separated from the mold medium. This may be achieved in various conventional ways. For example, if the product particles and mold medium are sufficiently homogeneous but differ in diameter, adequate separation can be achieved simply by sieving. Alternatively, if the densities of the product particles and mold medium differ sufficiently, density separation techniques may be used (as demonstrated, for example, in an example where high-density ZrO2 microspheres are used as the mold medium and then density separation techniques are used to easily separate the significantly lower-density product particles). Methods for separating product particles from the mold medium include air classification, sieving, cyclone, washing, deposition, hydrocyclone, or other wet or dry methods known to separate particles based on diameter, shape, or density.

[0062] It has been observed that some loss of crystallinity associated with precursor particles may occur as a result of the mechanical processing associated with this method. If desired and / or required, this loss can be readily corrected by annealing (heating) the product particles at a high temperature and in an environment appropriate with respect to the materials contained therein (e.g., an inert atmosphere for carbonaceous powders, or air for oxide powders).

[0063] In some embodiments, the synthesis of precursor particles may include a step of reducing the average particle size, for example, by grinding including ball milling or classification. In some embodiments, the synthesis of precursor particles may include a step of reducing the crystallite size, including ball milling. In some embodiments, the synthesis of precursor particles may include a step of increasing the crystallite size, including a heating step or a classification step. In some embodiments, the synthesis of precursor particles may include a step of reacting two or more components together, including coprecipitation, heating, ball milling or other known methods. In some embodiments, the synthesis of precursor particles may include a step of combining particles having different average crystallite sizes and different compositions.

[0064] In some embodiments, by applying the above microgranulation method to template particles and precursor particles comprising a mixture of precursor particles having different crystallite sizes, product particles are obtained that, on average, have larger precursor particle crystallites near the product particle core and smaller precursor particle crystallites near the product particle surface. Furthermore, in some embodiments, when a mixture of precursor particles of different chemical compositions is used, containing precursor particles of one composition having an average crystallite size larger than the average crystallite size of precursor particles of another composition, product particles are obtained in which the product particle core has a composition that is closer to the composition of the precursor particles having the larger crystallite size, and the product particle surface has a composition that is closer to the composition of the precursor particles having the smaller crystallite size. Theoretically, product particles having a continuously fluctuating composition can be produced by applying the above method to template particles and precursor particles comprising a mixture of precursor particle powders having different compositions and average crystallite sizes, such that the composition of the product particles fluctuates from their surface to the core according to the increasing order of the average crystallite sizes of each precursor particle powder.

[0065] The precursor particles may also include particles having different compositions, such that composite product particles are produced, which include aggregated mixtures of precursor particles having different compositions. In some embodiments, the composite product particles may be heated so that the component precursor particles react with each other.

[0066] Product particles can be prepared in a manner that has an average diameter of 10 to 100 μm. Furthermore, product particles can have a narrow particle size distribution similar to the mold medium used, and their diameter can be very uniform. For example, the diameter distribution of product particles can be uniform to be (D90-D10) / D50 < 2, (D90-D10) / D50 < 1, (D90-D10) / D50 < 0.7, or smaller. Furthermore, product particles can preferably be smooth and can be formed into regular circular shapes such as spheres and round tetrahedra. Product particles can further contain features having both a relative depth in the range of 0.1 to 0.2 and a relative aspect ratio greater than 0.2.

[0067] Once prepared according to the above format, the product particles are generally ready for conventional use in their intended applications. In battery applications, electrodes and electrochemical devices utilizing the product particles can be prepared in numerous formats known to those skilled in the art. For example, there are numerous arbitrary designs and methods for manufacturing electrodes for rechargeable lithium-ion batteries, as well as for manufacturing the batteries themselves, and these are extensively documented in the art.

[0068] Mechanofusion has been found to be effective in preparing uniform, round aggregates in this manner, whereas other conventional granulation methods, such as automated grinding and ball milling processes, are not. While not bound by theory, it is assumed that in this method, precursor particles initially coat the mold medium. However, due to the smoothness of the mold medium, the precursor particles adhere poorly. Therefore, after reaching a certain thickness, the layer of precursor particles breaks away from the mold medium. This results in the formation of intermediate particles of relatively uniform volume. These intermediate particles are then spheroidized and sizing to form product particles. Therefore, this process depends on the mechanofusion process's ability to form a high-density coating on the particles. This is only possible in the high-shear and high-compression fields present during the mechanofusion process. Other processes, such as grinding, milling, and high-shear mixing, have been found to lack these properties and therefore did not produce comparable product particles.

[0069] An additional finding related to this method is that several product particles that can be prepared are characterized by novel and potentially useful structures. These include graphite product particles, lithium mixed metal oxide product particles, and lithium transition metal oxide product particles characterized by unique structures. For example, graphite nanoparticles can be prepared that include graphite particles molded as spherical or oval shapes, and concentric nested spherical or oval shapes with graphene layers. These graphene layers are randomly placed on the surfaces of the concentric nested spherical or oval shapes, but the graphene layers are oriented such that their base planes are tangential to the concentric nested spherical or oval shapes. Furthermore, the graphite particles have an average particle size greater than 2 μm and an average db of less than 3,400 Å. 002 They have spacing. In some embodiments, the graphite particles of the fine particles include a porous, concentric layer having hollows or voids near their core. In some embodiments, the graphite particles have an average particle size of 5 μm to 50 μm and a diameter distribution of (D90-D10) / D50 < 2.

[0070] The aforementioned graphite nanoparticles, and furthermore, high-grade graphite-onion graphite, are expected to be advantageous as active anode materials in lithium-ion batteries. It is well known that the basal plane of graphite is a highly reactive region with respect to the lithium-ion battery electrolyte. Therefore, natural graphite is typically spheroidized and granulated to reduce the surface area of ​​the basal plane in contact with the electrolyte, as discussed in M. Yoshio et al., J. Mater. Chem. 14 (3005) 1754-1758. However, conventional spheroidizing methods result in graphite planes that are arranged in the same pattern as jelly rolls, or spirally wound, as described by M. Yoshio et al., who said, "Spherical natural graphite particles look like tightly clenched fists." In other words, the graphite layers of conventional spherical, symmetrically granulated natural graphite particles are arranged concentrically around a central axis (i.e., in a nested, concentric cylinder) rather than concentrically around a single point (i.e., in a nested, concentric sphere or oval) as in the case of onion graphite. The arrangement of the graphite base planes in spherical natural graphite reduces the amount of graphite base plane exposed to the electrolyte, although the graphite base plane remains exposed at either end of the "jelly roll". To reduce the reactivity of the exposed base plane, spherical natural graphite is typically carbon-coated, as described by M. Yoshio et al. In contrast, the microstructure of onion graphite has no base plane exposed to the electrolyte and is therefore expected to have improved performance as a negative electrode material in lithium-ion batteries.Onion graphite is expected to be superior to the types of graphite spheroids found in cast iron, which are known to have a microstructure in which the graphite basal planes are concentrically arranged but the planes radiate from a central core (as shown, for example, in Figure 6-4 of "Mesomolecules: From Molecules to Materials" SEARCH Series, Volume 1, G. David Mendenhall, Arthur Greenberg, and Jeol F. Liebman, eds., Chapman & Hall, New York, 1995). In this structure, the electrolyte is expected to approach the graphite basal planes along radial lines that separate the basal planes extending from the particle core to the surface. For practical use in lithium-ion battery applications, the diameter of the onion graphite should be greater than 5 μm, more preferably between 10 μm and 50 μm. Additionally, onion graphite should have a high level of graphitization. This is known to improve the reversible capacity and reduce cell polarization. When measured by X-ray diffraction, the measurement of the graphitization level is the d. 002 spacing, and the d 002 lower the value of the spacing, the higher the degree of graphitization. A preferred level of graphitization is a d-spacing of less than 3.400 Å, or more preferably less than 3.360 Å, or more preferably less than 3.350 Å. 002 is indicated by the spacing.

[0071] Also, for example, lithium mixed metal oxide microparticles can be prepared that include particles having a core of randomly oriented lithium nickel manganese cobalt crystallites with an average diameter of about 1 μm, coated with smaller randomly oriented lithium nickel manganese cobalt crystallites having an average diameter of about 0.3 μm. In some embodiments, the lithium mixed metal oxide product particles are smooth tetrahedrons.

[0072] Furthermore, lithium transition metal oxide nanoparticles can be prepared, for example, including particles having at least two transition metals located in the group consisting of Mn, Ni, and Co. These particles have an O3 structure, an average particle size in the range of 1 to 50 μm, and they contain crystallites whose shape and diameter vary randomly throughout their interior. In certain embodiments, the crystallites have an average diameter greater than 0.5 μm, and the average particle size is at least 5 times larger than the average crystallite diameter. In certain embodiments, the composition of one of the two transition metals can vary by at least 5 atomic percent from the core to the shell of the particle.

[0073] The following embodiments illustrate specific aspects of the present invention, but should not be construed as limiting the invention in any way. Those skilled in the art will readily recognize that other modifications are possible with respect to the methods and materials manufactured herein. [Examples]

[0074] Examples Exemplary microparticles were prepared using mechanofusion to aggregate precursor particles according to the present invention. Other microparticles were also prepared for comparative purposes. Various characteristics of these microparticles were determined and are shown below. In addition, electrodes and electrochemical cells were prepared using some of these microparticles. The cell performance results obtained from the electrochemical cells are also presented below.

[0075] Microgranulation method (mechanofusion) Microgranulation was achieved using the AM-15F Mechanofusion System (Hosokawa Micron Corporation, Osaka, Japan), as schematically shown in Figure 1 below. To reduce wear, the apparatus was modified by replacing the standard stainless steel chamber, scraper, and press head with components made of the same hardened steel. The chamber had an inner diameter of 15 cm. Unless otherwise specified, mechanofusion was performed at high rpm using a scraper / wall spacing of 0.5 mm and a press head / wall spacing of 1.4 mm. After a given process time, samples were collected from several different areas of the chamber. Unless otherwise specified, the gas atmosphere used during the mechanofusion process was air.

[0076] Characterization of materials The particle size distribution of the particulate samples was obtained using a Horiba Partica LA-950V2 laser dispersion particle size distribution analyzer.

[0077] X-ray diffraction (XRD) patterns were collected using a Rigaku Ultima IV diffractometer equipped with a Cu Kα X-ray source, a diffraction beam graphite monochromator, and a scintillation detector.

[0078] The average crystallite size of different phases was determined by applying the Scherrer equation to the maximum XRD peak of the phase in question, unless otherwise specified.

[0079] SEM and cross-sectional SEM were used to study the sample morphology. For this purpose, a TESCAN MIRA 3 LMU Variable Pressure Schottky Field Emission Scanning Electron Microscope (SEM) was used. Cross-sections of the samples were prepared using a JEOL Cross-Polisher (JEOL Ltd., Tokyo, Japan), which separates the sample by firing argon ions at it.

[0080] To characterize particle surface cavities, the relative depth and relative aspect of the depressions on the particle surface are measured from the particle cross-section or projected area (i.e., silhouette) as follows: As shown in Figure 19, line AB is created above the depression on the particle surface and has both ends tangent to the particle surface. The longest distance measured perpendicularly from line AB to the particle surface (line GC) is described as the characteristic depth, d. Two lines are drawn from point C (lines EC and CF in Figure a) such that they are in contact with the surface contact line AB and have the largest possible acute angle between them without passing through the particle volume. The relative depth of the particle is defined as d / D, where D is the projected area diameter. The relative aspect is defined as {(EC+FC) / EF-1}. Surface cavities are their features that have a relative depth in the range of 0.02 to 0.1 and a relative aspect greater than 0.2.

[0081] To determine particle roughness, the spline deformation method is used. This method determines particle roughness by quantifying the deformation at the radius of the surface when measured from the center of mass. In this method, a scanning electron microscope (SEM) digital image of a cross section or silhouette of the desired particle with minimum image resolution such that at least 1000 pixels are at the periphery of the particle is obtained. After determining more than 1000 outline pixels of the SEM image, the center of mass of this outline silhouette is found. Next, the distance from each point of the outline silhouette to the center of mass is measured ("radial segment value"). Then, the radial segment values ​​are plotted as the action of angles around the center of mass from 0° to 360°, and this plot is fitted to a smoothing spline function.

number

[0082] Electrode preparation Sample electrodes for laboratory testing were prepared from a slurry prepared by mixing fine particles, carbon black (Super C65, Imerys Graphite and Carbon), and lithium polyacrylate (LiPAA, LiPAA is provided in a 10 wt% aqueous solution produced by neutralizing a polyacrylic acid solution (Sigma-Aldrich, average molecular weight approximately 250,000 g / mol, 35 wt% in H2O) with LiOH·H2O (Sigma Aldrich, 98%) in distilled water. The slurry was mixed at 100 rpm for 1 hour using a Retsch PM200 planetary mill equipped with three 13 mm tungsten carbide balls, and then spread onto metal foil (copper or aluminum, for anode and cathode active materials, respectively) using a 0.004 inch spaced coating bar. Next, the coating was air-dried at 120°C for 1 hour, cut into 1.3 cm discs, and then heated under vacuum at 120°C for 1 hour without further exposure to air. The resulting electrode load was approximately 2–2.5 mg / cm². 2 That was the case.

[0083] Cell preparation To evaluate various materials as electrode materials in lithium-ion cells, test lithium half-cells were constructed and tested. Electrodes were assembled into 2325 type coin lithium half-cells with lithium foil (99.9%, Sigma Aldrich) pairs / reference electrodes (Note: As is well known to those skilled in the art, results from these test lithium half-cells allow for reliable prediction of electrode material performance in lithium-ion batteries). Two-layer Celgard 2300 separators were used in each coin lithium half-cell. 1M LiPF6 (BASF) in a solution of ethylene carbonate, diethyl carbonate, and monofluoroethylene carbonate (volume ratio 3:6:1, all from BASF) was used as the electrolyte. Cell assembly was performed in an Ar-filled glove box. Cells were cycled at a constant current at 30.0 ± 0.1 °C.

[0084] Example 1 of the present invention - Microgranulation of graphite flakes Zirconium oxide (ZrO2) microspheres (Glen Mills Inc.) with an average diameter of 57 μm were used as a template medium to aggregate graphite flake precursor particles into graphite product particles. Figures 2a and 2b show SEM images of the ZrO2 template medium at two different magnifications. Figure 2c shows a cross-section of the ZrO2 particles, showing their periphery and center of mass. Figure 2d shows the interpolated radial segment values ​​and the interpolated f(x) values, plotting the rest as a function of x. From this data, roughness was determined. The ZrO2 template medium was smooth, with a roughness of only 0.0022 and no cavities. Figure 3 shows the uniform particle size distribution of the ZrO2 template medium with a D50 of 57.35 μm and (D90-D10) / D50 = 0.61.

[0085] Natural graphite flakes (230U, Asbury Graphite Mills Inc.) were used as graphite precursor particles. Figures 4a and 4b show SEM images of these precursor particles at two different magnifications. As is evident from these images, the graphite flakes are irregularly shaped particles with a layered structure, and the particle diameters vary considerably. Many of the particles have a jagged surface feature, which is a large cavity.

[0086] A mixture containing approximately 225 g of ZrO2 microsphere template medium and approximately 25 g of graphite precursor particles (total powder volume of approximately 50 mL) was prepared and then subjected to a high shear and high pressure field provided by the mechanofusion system. The system was operated for 12 hours at 1500 rpm (wall velocity of 12 m / s). Figures 5a and 5b show SEM images of the product obtained after this mechanofusion at two different magnifications. In these images, the ZrO2 microspheres appear to be partially coated with a thin layer of graphite. It is also clear that the graphite spheres (product particles) have a slightly smaller diameter than the ZrO2 microspheres.

[0087] Next, (5.68 g / cm³ 3 ZrO2 and 2.23 g / cm³ 3 (3.32 g / cm³ of graphite) 3 Diiodomethane with a density of 1 / 2 (MI-GEE, GEO Liquids, Inc., Prospect Heights, IL) was used to separate graphite spherical product particles from ZrO2 microspheres by density. Figures 6a and 6b show SEM images at two different magnifications of the graphite spherical product particles separated by diiodomethane and after drying. Almost all of the ZrO2 was removed, and therefore most of the remaining particles were graphite spheres.

[0088] XRD patterns of graphite were obtained before and after the mechanofusion process. Based on the obtained XRD patterns, it appeared that the mechanofusion process partially disrupted the crystalline structure of the graphite, causing some loss of crystallinity. This was evident from the broadening of peaks and amorphous characteristics in the XRD patterns. The patterns also indicated the presence of small amounts of ZrO2 impurities remaining in the sample (at an industrial scale, it is expected that such impurities can be easily removed using better separation techniques). Therefore, the graphite spherical product particles were recrystallized by annealing (heating) in argon for 3 hours at 3000°C. Subsequent XRD patterns of the tempered product particles were obtained. At this stage, all peaks were sharp and showed good crystallinity. (002) Based on the position of the X-ray diffraction peaks d 002 The spacing was determined to be 3.355 Å with respect to the tempered product particles, indicating a high degree of graphitization. A small amount of ZrC was likely present in the XRD pattern due to the reduction of ZrO2 by carbon at high temperatures in argon. Figures 7a, 7b, and 7c show these various XRD patterns, namely, the graphite flake precursor particles before mechanofusion, the graphite spherical product particles after mechanofusion and separation from the mold medium, and the graphite spherical product particles after annealing, respectively.

[0089] Figure 8 shows the particle size distribution of graphite spherical product particles after annealing. For comparison, the particle size distribution of the ZrO2 mold medium is also shown (dotted line). The graphite spherical product particles have an average diameter of approximately 41 μm, indicating that their diameter is very uniform.

[0090] Electrodes were prepared using these graphite spherical product particles as the anode active material, and lithium half-cells containing such electrodes were fabricated and tested. The cells were cycled from 0.005V to 0.9V. For the first cycle, the cell was cycled at C / 10 and lower potentials, and the cell was held at a constant potential until the current dropped to C / 20 before the start of the next cycle. For subsequent cycles, the cell was cycled at C / 5 and the cell was held at lower potential limits until the current dropped to C / 10 before the start of the next cycle. Figures 9a, 9b, and 9c show the electrochemical performance of this cell. In these figures, the voltage curve, the corresponding differential capacitance curve, and the cycling performance are shown, respectively. The voltage curve is typical for graphite, and the expected staging can be clearly observed in the differential capacitance curve. Good cycling performance yields a reversible capacitance of approximately 275 mAh / g.

[0091] To further analyze the structure of these graphite spherical product particles, representative particles were cross-sectionalized and imaged using a SEM, as detailed above. Figures 10a, 10b, and 10c show some of the obtained SEM images. Figure 10a shows the entire product particle, and Figures 10b and 10c show different parts of the product particle at higher magnification. Some of the product particles contain void spaces (i.e., hollow cores) near the center of the particle. In addition, porosity arranged in concentric layers is observed throughout the particle. Thus, the product particles appear to be characterized by a novel concentric structure. The product particles contain concentric layers of graphene sheet. Figure 10d shows a cross-section of the product particle showing its periphery and center of mass. Figure 10e shows the interpolated radial segment values ​​and the plot of the rest of the interpolated f(x) values, a function of x. From this data, roughness was determined. The graphite product particles are smooth, have a roughness of only 0.0052, and have no cavities.

[0092] Example 2 of the present invention - Microgranulation of lithium transition metal oxide powder Using zirconium oxide (ZrO2) microspheres similar to those in the above examples as a template medium, submicron-sized irregularly formed precursor NMC particles were aggregated into larger, more regularly formed NMC product particles.

[0093] Using the all-solid-state method, the formula LiLi 1 / 3 Mn 1 / 3 Co 1 / 3NMC precursor particles containing O2 were prepared. Specifically, stoichiometric amounts of NiO (Sigma-Aldrich, 99%), MnO (Aldrich, 99%), Co3O4 (Alfa Aesar, 99.7%), and Li2CO3 (Alfa Aesar, 99%) were mixed together with a 10% excess of Li2CO3 by high-energy ball milling using a SPEX8000 mixer. Approximately 2.4 g of the sample was milled for 4 hours using 180 g of 1.6 mm stainless steel balls (Thomson Linear Motion). The resulting ball-milled mixture was then pelletized and heated in air at 900°C for 3 hours. Finally, the pellets were ground into a fine powder to produce NMC precursor particles. Figures 11a and 11b show SEM images of these NMC precursor particles at two different magnifications. Irregular aggregation of submicron NMC particles can be observed.

[0094] A mixture containing approximately 225 g of ZrO2 microsphere template medium and approximately 15 g of NMC precursor particles (total powder volume of approximately 50 mL) was prepared and then subjected to mechanofusion as described above. The system was operated for 24 hours at 1000 rpm (wall speed of approximately 8 m / sec). Figures 12a and 12b show SEM images of the product obtained after this mechanofusion at two different magnifications. In these images, the ZrO2 microspheres appear to be partially coated with a thin layer of NMC. It is also clear that the NMC tetrahedra (product particles) are slightly smaller than the ZrO2 microspheres but have a larger diameter than the NMC precursor particles.

[0095] Next, NMC tetrahedral product particles were separated from ZrO2 microspheres using a 400-mesh sieve. Figures 13a and 13b show SEM images of the tetrahedral NMC product particles separated in this manner at two different magnifications. The product particles are smooth. Again, almost all of the ZrO2 was removed.

[0096] XRD patterns of NMC product particles were obtained before and after the mechanofusion process. Again, the mechanofusion process appeared to have somewhat disrupted the crystalline structure of the product particles, resulting in some loss of crystallinity. This was evident from the broadening of peaks and amorphous characteristics in the XRD patterns. The patterns also showed the presence of small amounts of ZrO2 impurities remaining in the sample (again, it is expected that such impurities can be easily removed using better separation techniques at an industrial scale). Therefore, the NMC product particles were recrystallized by annealing at 900°C in air. Subsequent XRD patterns of the tempered product particles were obtained. At this stage, all peaks were sharp and showed good crystallinity. Small amounts of ZrO2 were still present in the XRD patterns. Figures 14a, 14b, and 14c show these various XRD patterns, namely, the XRD patterns of NMC precursor particles before mechanofusion, NMC tetrahedral product particles after mechanofusion and separation from the template medium, and NMC product particles after annealing, respectively.

[0097] Figure 15 shows the particle size distribution of NMC product particles after annealing. For comparison, the particle size distribution of the ZrO2 template medium is also shown (dotted line). The NMC product particles have an average diameter (D50) of approximately 28 μm and a narrow distribution with (D90-D10) / D50 = 0.66, indicating that the diameter is very uniform.

[0098] Electrodes were prepared using these NMC product particles as cathode active materials, and lithium half-cells containing such electrodes were fabricated and tested. For the first cycle, the cell was cycled at 3.0V to 4.2V at C / 10. For the remaining cycles, the cell was cycled at C / 4 and held at the upper cutoff potential until the current dropped to C / 10 before starting the next cycle. Figures 16a and 16b show the electrochemical performance of this cell. The voltage curve and cycling performance are shown in these figures, respectively. The voltage curve is typical for NMC, and a reversible capacitance of approximately 90 mAh / g is obtained.

[0099] To further analyze the structure of these NMC product particles, representative particles were cross-sectionalized and imaged using SEM as described above. Figures 17a, 17b, 17c, and 17d show some of the obtained SEM images. Figure 17a shows the entire product particle, while Figures 17b, 17c, and 17d show different parts of the product particle at some higher magnifications. The product particles appear to be smooth and tetrahedral in shape with rounded corners. They contain a core of randomly oriented crystallites with an average diameter of approximately 1 μm, coated with smaller randomly oriented crystallites with an average diameter of approximately 0.3 μm. Thus, the aggregated NMC product particles appear to be characterized by a novel structure.

[0100] Figure 17e shows a cross-section of the product particle, indicating its periphery and center of mass. Figure 17f shows the interpolated radial segment values ​​and the plot of the interpolated f(x) values ​​and the rest of the function of x. From this data, roughness was determined. The NMC product particle was smooth, had a roughness of only 0.0094, and had no cavities.

[0101] Comparative Example - An attempt to micro-granulate lithium transition metal oxides using an automated grinding process. Similar zirconium oxide (ZrO2) microspheres and NMC precursor particles to those used in the above examples were employed. A mixture containing the same proportions of ZrO2 and NMC was mixed in a Brinkmann-Retsch automatic grinder. The automatic grinder was set to operate at approximately 120 rpm for two weeks. Figures 18a and 18b show SEM images obtained for this sample undergoing automatic grinding. The SEM images show that all ZrO2 microspheres were loosely coated with NMC, but granulation of the NMC is barely observable. This comparative example demonstrates that very long periods of automatic grinding do not provide the inherent advantages of the mechanofusion process.

[0102] Example 3 of the present invention - Microgranulation of a mixture of precursor particles having different compositions and different average crystallite sizes Using zirconium oxide (ZrO2) microspheres similar to those in the above examples as a template medium, several types of precursor particles with different compositions and average crystallite sizes were aggregated.

[0103] A mixture was prepared containing approximately 180 g of ZrO2 microsphere template medium, 6.94 g of NiO(Sigma-Aldrich, 99%), 2.20 g of MnO(Aldrich, 99%), 2.48 g of Co3O4((Alfa Aesar, 99.7%), and 6.29 g of Li2CO3(Alfa Aesar, 99%). As determined by observation of single crystalline crystallites by SEM, the average crystallite size of Co3O4 was 0.3 μm, and the average crystallite size of NiO was 2 μm. The mixture was then subjected to the above mechanofusion for 18 hours at 1000 rpm (wall velocity of approximately 8 m / s). The product particles were then separated from the ZrO2 microspheres using a 400 mesh sieve. Figures 20a and 20b show SEM images of the cross-section of the product particles at two different magnifications. The particles are smooth, and most have a diameter of 5–10 μm. In cross-section, the particles appear to have a core-shell structure. The brightness differs between the particle core and the particle shell, and they exhibit different elemental compositions with respect to the core and shell. Figure 21 shows a cross-sectional image of the particle at the positions of five data points, indicated as spectrum 1–5. The elemental composition at each point is listed in Table 1 below, according to the EDS determination. The core is Co-rich, while the shell is Mn and Ni-rich.

[0104] [Table 1]

[0105] Example 4 of the present invention - x+y+z=1, comprising O3-phase LiNi particles having a higher Ni content in their core than in their shells. x Mn y Co z Synthesis of O2 powder As a Mn-rich particle shell, LiNi 1 / 3 Mn1 / 3 Co 1 / 3 The target composition for O2 (NMC111) was selected: 12.88 g NiO (Sigma-Aldrich, 99%), 12.24 g MnO (Aldrich, 99%), 13.85 g Co3O4 (Alfa Aesar, 99.7%), and 21.03 g Li2CO3 (Alfa Aesar, 99%) (Formula LiNi 1 / 3 Mn 1 / 3 Co 1 / 3 Shell precursor powder was produced by sealing 10 kg of 0.5-inch stainless steel balls (corresponding to a 10% excess of Li2CO3 according to O2) in a 5 L stainless steel jar mill (US Stoneware) and milling them at 85 rpm for one week. The XRD pattern of the obtained shell precursor powder is shown in Figure 22. It contains a mixture of Li2CO3, Co3O4, NiO, and MnO phases. The SEM image of the obtained shell precursor powder is shown in Figure 23. It contains crystallites with a diameter of less than 0.1 μm.

[0106] As a Ni-rich particle core, LiNi 0.6 Mn 0.2 Co 0.2 The target composition of O2(NMC622) was selected. Core precursor powder was prepared by sealing 41.61 g of NiO(Sigma-Aldrich, 99%), 13.18 g of MnO(Aldrich, 99%), 14.90 g of Co3O4(Alfa Aesar, 99.7%) and 10 kg of 0.5-inch stainless steel balls in a 5 L stainless steel jar mill (US Stoneware) and milling at 85 rpm for one week. Figure 24 shows the XRD pattern of intermediate A, which corresponds to a single-phase rock salt type structure. Figure 25 shows the SEM image of intermediate A. Intermediate A consists of crystallites with a diameter of less than 0.1 μm. Using a mortar and pestle, 15 g of intermediate A was milled using the formula LiNi until a homogeneous mixture was obtained (approximately 10 minutes). 0.6 Mn 0.2 Co 0.2According to O2, 7.83 g of Li2CO3 (Alfa Aesar, 99%), corresponding to a 5% excess of Li2CO3, was mixed with the mixture. The mixture was placed in an alumina crucible and heated at 900°C for 3 hours in air in a box furnace to obtain core precursor particles. The purpose of this heating step was to increase the crystallite size of the core precursor particles so that they were more than 10% larger than the crystallite size of the shell precursor particles. Figure 26 shows an SEM image of the obtained core precursor particles. They have an average crystallite size of approximately 2 μm. Figure 27 shows the XRD pattern of the core precursor particles. It corresponds to the phase-pure O3 phase NMC622.

[0107] A mixture containing approximately 180 g of ZrO2 microsphere template medium, 13.33 g of shell precursor particles, and 6.67 g of core precursor particles was prepared. The mixture was then subjected to the above-described mechanofusion for 20 hours at 1000 rpm (wall velocity of approximately 8 m / s). The product particles were then separated from the ZrO2 microspheres using a 400 mesh sieve.

[0108] Figures 28a and 28b show SEM images of the cross-section of product particles at two different magnifications. Most product particles have a diameter of 5–20 μm. In the cross-section, the particles appear to have a core-shell structure. Brightness differs between the particle core and the particle shell, and they exhibit different elemental compositions with respect to the core and shell. The core consists of randomly oriented crystallites having the same average crystallite diameter as the core precursor particles, and the shell consists of randomly oriented crystallites having the same average crystallite diameter as the shell precursor particles. Both the core and shell contain porosity. Figure 29 shows a cross-sectional SEM image at the locations of five data points, indicated as spectrum 1–5. The elemental composition of each point is listed in Table 2 below, according to the EDS determination. The core is approximately 13% richer in Ni than the shell.

[0109] [Table 2]

[0110] Figure 30a shows a cross-sectional image of the product particle, and Figure 30b shows the EDS Ni mapping of the same product particle. The intensity of the Ni signal from the core is stronger than the signal from the shell, confirming that the product particle consists of a Ni-rich core, and the shell is rich in Co and Mn. Figure 31 shows the XRD pattern of the product particle. The XRD pattern corresponds to that of a mixture of the product particle and the core particle.

[0111] The product particles are placed in an alumina crucible and heated in a box-type furnace in air at 900°C for 3 hours to induce a reaction of the components of the product particles, resulting in LiNi 0.4 Mn 0.3 Co 0.3 Layered lithium nickel manganese cobalt oxide with the full composition of O2 was formed. Figure 32 shows the XRD pattern of the heated product particles. The XRD pattern is LiNi with x+y+z=1. x Mn y Co z It contains peaks corresponding only to the O3 phase of O2. Figure 33 shows an SEM image of a cross-section of heated product particles. The diameter of the heated product particles was the same as that of the product particles before heating. The heated product particles had an average diameter of 2 μm and contained randomly shaped and randomly oriented crystallites. Some of the heated product particles contained voids, while others did not.

[0112] Figure 34 shows a cross-sectional image of a heated product particle at the positions of six data points, indicated as spectrums 1-6. The elemental composition at each point is listed in Table 3 below, according to the EDS determination. Concentration gradients are created due to the diffusion of transition metals during the high-temperature heating process, with the Ni content gradually increasing from the shell to the core, and the Mn content increasing from the core to the shell. Figure 35 shows the variation in transition metal composition as a function of distance from the surface of the heated product particle, determined from spectrums 1-6 in Figure 34. The Ni concentration near the core is approximately 9% higher than in the shell.

[0113] [Table 3]

[0114] Example 5 of the present invention - Microgranulation of graphite flakes Graphite product particles were produced using the same method as in Example 1 of the present invention, except that the product particles were separated from the ZrO2 mold medium by passing the product particle / mold medium mixture through a 38 μm sieve after the mechanofusion process. The product particles were then heated to 2840°C under argon gas for 90 minutes to produce graphite spheres. The tempered product particle spheres had the same shape and average particle size as those of Example 1 of the present invention, but with lower porosity, presumably because diiodomethane was not used during the process. It is thought that diiodomethane penetrated between the graphite layers during heating, creating concentric porosity and void spaces. Figure 36 shows SEM cross-sectional images of some tempered product particles from Example 5 of the present invention. Some of the tempered product particles contained little or no porosity, some concentric porosity, and some central void spaces. All tempered product particles contain layers of graphite concentrically arranged within nested oval or spherical shells, and the base planar edges do not radiate outwards from the center point.

[0115] Example 6 of the present invention - Micro-granulation of petroleum coke Thirty g of petroleum coke in the form of flakes having an average flake thickness of 2 μm and an average flake width of 10 μm, and a mixture of ZrO2 spheres of the same type used in Example 1 of the present invention, were subjected to the high shear and high pressure field described in Example 1 for 32 hours. The resulting product particles were separated from the ZrO2 spheres using a 400 mesh sieve. The resulting product particles had a small nodular shape but were round, smooth, and had an average diameter of 20 μm.

[0116] The above examples demonstrate that mechanofusion can be used to easily and efficiently aggregate various precursor particles into larger product particles. The product particles may be uniform and preferably smooth, and may be spherical or round. In some examples, this method can be used to produce fine particles with novel structures. Furthermore, as demonstrated in laboratory test cells, the present invention can be used to produce fine particles suitable for electrode materials in lithium batteries.

[0117] All of the above-mentioned U.S. patents, U.S. patent applications, foreign patents, foreign patent applications, and non-patent publications described herein are incorporated herein by reference as a whole.

[0118] While specific elements, embodiments, and applications of the present invention have been shown and described, it will be understood that the present invention is not limited thereto, as modifications can, of course, be made by those skilled in the art without departing from the spirit and scope of this disclosure, particularly in consideration of the teachings above. For example, it is expected that similar uniform product particles could also be provided by other methods that can provide shear and pressure field conditions similar to those provided by mechanofusion. Such modifications are considered to be within the scope of the claims appended herein.

Claims

1. A microgranulation process for producing aggregates from precursor particles, comprising the steps of: Obtaining a quantity of precursor particles having an average particle size as D50 of less than 1000 μm; obtaining a quantity of template particles having an average particle size as D50 of less than 500 μm and a hardness higher than the hardness of said precursor particles; preparing a mixture comprising the amounts of precursor particles and template particles; subjecting the mixture to a shear and pressure field to agglomerate the precursor particles to obtain the agglomerates; After obtaining the aggregate, separating the aggregate from the template particles; Including, The method wherein subjecting the mixture to a shear and pressure field is a dry process that does not require a solvent.

2. The method of claim 1, wherein the step of subjecting the mixture to a shear and pressure field includes subjecting the mixture to dry mechanofusion to obtain the agglomerates.

3. 2. The method of claim 1, wherein the precursor particles have an average particle size, D50, of less than 50 μm.

4. 4. The method of claim 3, wherein the precursor particles have an average particle size, D50, of less than 10 μm.

5. 10. The method of claim 1, wherein the precursor particles are a powder for use in a battery electrode, a fertilizer, a pharmaceutical, a toner, a pigment, a filler, or a catalyst.

6. The method of claim 5 , wherein the precursor particles are a carbonaceous powder, or a mixed metal oxide powder, or a metal carbonate powder.

7. The method of claim 6 , wherein the precursor particles comprise carbon.

8. The precursor particles are graphite flakes or LiNi 1/3 Mn 1/3 Co 1/3 O 2 The method of claim 6, which is a powder.

9. the precursor particles are mixed metal oxide powders, and obtaining the quantity of precursor particles comprises: Obtaining a metal oxide raw material powder; ball milling the metal oxide raw material powder to produce the precursor particles; The method of claim 6, comprising:

10. The method of claim 1 , comprising ball milling at least a portion of said quantity of precursor particles prior to preparing said mixture.

11. The method of claim 1 , comprising heating at least a portion of said quantity of precursor particles prior to preparing said mixture.

12. The method of claim 1 , wherein the precursor particles are an irregularly shaped powder.

13. The method of claim 1 , wherein the average particle size of the template particles is 100 μm or less as D50.

14. 10. The method of claim 1, wherein the template particles are selected from the group consisting of zirconium oxide, tungsten carbide, tungsten, silicon oxide, aluminum oxide, silicon nitride, hardened steel, stainless steel, and agate.

15. The method of claim 1 , wherein the surface of the template particle is smooth.

16. The method of claim 15 , wherein the template particles are spherical.

17. The method of claim 1, wherein the size distribution of the template particles satisfies (D90-D10) / D50<2.

18. The method of claim 1 , wherein the bulk volume of said quantity of template particles is greater than the bulk volume of said quantity of precursor particles.

19. The method of claim 1 , wherein the bulk volume of said quantity of template particles is greater than 10% of the bulk volume of said quantity of precursor particles.

20. 20. The method of claim 19, wherein the bulk volume of said quantity of template particles is at least 2.7 times the bulk volume of said quantity of precursor particles.

21. 3. The method of claim 2, wherein the Mechanofusion is carried out in a Mechanofusion system including a chamber, a rotating wall within the chamber, a scraper within the rotating wall, and a press head within the rotating wall.

22. The mechanofusion Setting a distance between the scraper and the rotating wall of 0.45 mm to 0.55 mm; Setting a distance between the press head and the rotating wall of 1.26 mm to 1.54 mm; Rotating the wall surface at a speed of 7.2 m / s or greater; 22. The method of claim 21 , comprising:

23. The method according to claim 1, wherein the aggregates have an average particle size D50 of 10 to 100 μm.

24. The method of claim 1, wherein the aggregate size distribution satisfies (D90-D10) / D50<2.

25. The method of claim 2 , wherein the surface of the aggregate is smooth.

26. The method of claim 2 , wherein the surface of the agglomerates does not contain cavities.

27. The method of claim 2 , wherein the agglomerates have a roughness with a coefficient of variation of less than 0.

02.

28. 26. The method of claim 25, wherein the aggregates are spherical.

29. 26. The method of claim 25, wherein the aggregates are tetrahedral in shape.

30. The method of claim 2 , additionally comprising tempering the aggregate at an elevated temperature.

31. The method of claim 1 , wherein the template particles have a hardness greater than a hardness of the precursor particles such that the template particles are not destroyed in the presence of the precursor particles.

32. 1. A method for producing aggregates for battery electrodes, fertilizers, pharmaceuticals, toners, pigments, fillers, or catalysts from precursor particles, comprising the steps of: Obtaining a quantity of precursor particles having an average particle size as D50 of less than 1000 μm; obtaining a quantity of template particles having an average particle size as D50 of less than 500 μm and a hardness higher than the hardness of said precursor particles; preparing a mixture comprising the amounts of precursor particles and template particles; subjecting the mixture to a shear and pressure field to agglomerate the precursor particles to obtain agglomerates; After obtaining the aggregate, separating the aggregate from the template particles; Including, The method, wherein subjecting the mixture to a shear and pressure field comprises subjecting the mixture to dry mechanofusion to obtain an agglomerate.

33. 13. A rechargeable battery comprising an anode electrode and a cathode electrode, at least one of the anode and cathode electrodes comprising an aggregate produced according to the method of claim 1.

34. The method of claim 1 , wherein the quantity of precursor particles comprises a mixture of first particles of a first composition and second particles of a second composition, the first and second compositions being different.

35. 35. The method of claim 34, wherein the average crystallite size of the first precursor particles differs from the average crystallite size of the second precursor particles by at least 10%.