Oxygen generation device, and oxygen generation method

JP2023070388A5Active Publication Date: 2024-10-22DOSHISHA UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2021182529
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2021-11-09
Publication Date
2024-10-22
Estimated Expiration
2041-11-09

AI Technical Summary

Technical Problem

Existing anodes used in molten salt electrolysis, such as platinum and carbon electrodes, suffer from low corrosion resistance and react with oxide ions, leading to consumption and the generation of carbon dioxide, a greenhouse gas.

Method used

Employing a composite oxide anode composed of lanthanum, strontium, and cobalt (LSC oxide) with a perovskite structure, which exhibits high corrosion resistance and electrical conductivity, minimizing reaction with oxide ions and suppressing the generation of carbon dioxide.

Benefits of technology

The LSC oxide anode stabilizes oxygen production, reduces anode consumption, and maintains electrical conductivity over a wide temperature range, enabling efficient oxygen generation with minimal impurity formation and lower production costs.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

To provide an oxygen generation device comprising an anode of high corrosion resistance to molten salt, and an oxygen generation method.SOLUTION: An oxygen generation device comprises an electrolytic tank, molten salt including oxide ions and stored in the electrolytic tank, a cathode with at least a portion thereof immersed in the molten salt, an anode with at least a portion thereof immersed in the molten salt, and a power source for applying a voltage between the cathode and the anode. The oxygen generation device generates oxygen by oxidizing the oxide ions. The anode includes a composite oxide including lanthanum, strontium, and cobalt.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an oxygen generator and an oxygen generation method.

Background Art

[0002] Conventionally, a method of electrolyzing a composite oxide using a molten salt has been known. As an anode for this electrolysis, generally, a platinum electrode that is chemically stable or a carbon electrode with high heat resistance is used. Patent Document 1 proposes electrolysis of a composite oxide using a diamond electrode.

Prior Art Documents

Patent Documents

[0003]

Patent Document 1

Summary of the Invention

Problems to be Solved by the Invention

[0004] Platinum electrodes or carbon electrodes are inferior in corrosion resistance to molten salts. Furthermore, since carbon electrodes react with oxide ions generated by electrolysis of composite oxides, they are easily consumed and generate carbon dioxide. Generation of carbon dioxide, which is a greenhouse gas, is undesirable. Diamond electrodes are desirable in that they are difficult to consume and can suppress the generation of carbon dioxide.

[0005] From the viewpoint of effective utilization of resources, it is expected that the targets of electrolysis will become more diverse in the future, and electrolysis using molten salts has attracted more attention. Therefore, an anode with higher corrosion resistance to molten salts is required.

[0006] An object of the present disclosure is to provide an oxygen generator and an oxygen generation method including an anode having high corrosion resistance to a molten salt.

Means for Solving the Problems

[0007] This disclosure includes the following aspects: [1] Electrolytic cell and The electrolytic cell contains a molten salt containing oxide ions, A cathode, at least partially immersed in the molten salt, an anode, at least partially immersed in the molten salt, The system includes a power supply for applying a voltage between the cathode and the anode, An oxygen generator that generates oxygen by oxidizing the aforementioned oxide ions, The anode is an oxygen generator containing a composite oxide comprising lanthanum, strontium, and cobalt. [2] The aforementioned composite oxide is given by the following formula (1): La 1-x Sr x Co 1-y M y O 3-δ (In the formula, M is a transition metal other than lanthanum and cobalt, 0.1 ≤ x ≤ 0.9, 0 ≤ y ≤ 0.1, and δ is the oxygen deficiency.) The oxygen generator described in [1] above, represented by [1]. [3] The aforementioned composite oxide is given by the following formula (2): La 1-x Sr x OO 3-δ (In the formula, 0.2 ≤ x ≤ 0.6, and δ is the oxygen deficiency.) An oxygen generator as described in [1] or [2] above. [4] Electrolytic cell and The electrolytic cell contains a molten salt containing oxide ions, A cathode, at least partially immersed in the molten salt, an anode, at least partially immersed in the molten salt, The system includes a power supply for applying a voltage between the cathode and the anode, The anode contains a composite oxide comprising lanthanum, strontium, and cobalt, and is generated using an oxygen generator. An oxygen generation method in which a voltage is applied between the cathode and the anode to oxidize the oxide ions to generate oxygen. [5] The composite oxide is represented by the following formula (1): La 1-x Sr x Co 1-y M y O 3-δ (In the formula, M is a transition metal other than lanthanum and cobalt, 0.1 ≦ x ≦ 0.9, 0 ≦ y ≦ 0.1, and δ is the amount of oxygen deficiency.) The oxygen generation method according to [4] above, represented by the above formula. [6] The composite oxide is represented by the following formula (2): La 1-x Sr x CoO 3-δ (In the formula, 0.2 ≦ x ≦ 0.6, and δ is the amount of oxygen deficiency.) The oxygen generation method according to [4] or [5] above, represented by the above formula. [7] The temperature of the molten salt is 400 ° C or higher and 850 ° C or lower. The oxygen generation method according to any one of [4] to [6] above.

Effects of the Invention

[0008] According to the present invention, an oxygen generation device and an oxygen generation method including an anode having high corrosion resistance to a molten salt are provided.

Brief Description of the Drawings

[0009] [Figure 1] It is a schematic diagram showing an example of the oxygen generation device of the present invention. [Figure 2] It is a schematic diagram of the experimental apparatus used in the examples. [Figure 3A] It is a graph showing the results of XRD analysis of the mixture after calcination produced in Example 1. [Figure 3B] It is a graph showing the results of XRD analysis of the anode produced in Example 1. [Figure 4]This graph shows the relationship between the conductivity and temperature of the anode fabricated in Example 1. [Figure 5] This graph shows the results of cyclic voltammetry performed in Examples 1 and 2. [Figure 6] This graph shows the change in anode potential over time during constant current electrolysis performed in Example 1. [Figure 7A] This is a secondary electron image (3000x magnification) of the surface of the anode prepared in Example 1 before electrolysis, taken with a scanning electron microscope (SEM). [Figure 7B] This is a backscattered electron image (3000x magnification) of the surface of the anode prepared in Example 1 before electrolysis, taken with a scanning electron microscope (SEM). [Figure 8A] This is a secondary electron image (3000x magnification) of the surface of the anode after electrolysis, fabricated in Example 1, taken with a scanning electron microscope (SEM). [Figure 8B] This is a backscattered electron image (3000x magnification) of the surface of the anode after electrolysis, fabricated in Example 1, taken with a scanning electron microscope (SEM). [Figure 9] This graph shows the results of the XRD analysis of the anode prepared in Example 1 after electrolysis. [Figure 10] This graph shows the results of cyclic voltammetry performed in Examples 3 and 4. [Modes for carrying out the invention]

[0010] As a result of focusing on multifunctional metal composite oxides as anode materials, it was discovered that a composite oxide containing lanthanum, strontium, and cobalt (hereinafter sometimes referred to as LSC oxide) is poorly reactive with oxide ions and has extremely high corrosion resistance to molten salts. When an anode containing this LSC oxide (hereinafter sometimes referred to as LSC anode) is used, oxygen (preferably only oxygen) is stably generated from the anode, suppressing anode wear and dissolution. As a result, impurities are less likely to be generated, and contamination of the electrolytic bath is also suppressed.

[0011] In addition, LSC anodes exhibit extremely excellent conductivity over a wide temperature range. Therefore, oxygen can be efficiently generated even when electrolysis is performed at high temperatures, i.e., even when the temperature of the molten salt is high. Increasing the temperature of the molten salt is desirable because it leads to an increase in the amount of the material to be electrolyzed (usually the oxide ion source) dissolved in the molten salt and an improvement in the reaction rate. Furthermore, LSC electrodes can be manufactured at a lower cost compared to platinum electrodes or diamond electrodes.

[0012] [Oxygen generator] The oxygen generator according to this disclosure comprises an electrolytic cell, a molten salt containing oxide ions housed in the electrolytic cell, a cathode at least partially immersed in the molten salt, an anode at least partially immersed in the molten salt, and a power supply for applying a voltage between the cathode and the anode. The anode contains a composite oxide (LSC oxide) comprising lanthanum, strontium, and cobalt. The LSC anode has high corrosion resistance to the molten salt and excellent conductivity over a wide temperature range.

[0013] The apparatus described herein is used to generate oxygen by oxidizing oxide ions. As oxygen is generated, the oxide ion source is reduced. In other words, the oxygen generator described herein can be used to reduce various compounds containing oxygen atoms. Therefore, for example, the oxygen generator described herein can be used in processes for producing pure metals from various metal oxides (refining) or in the reprocessing process of spent oxide fuel from nuclear power plants.

[0014] In addition, since the oxygen generator according to this disclosure uses molten salt as an electrolyte, substances in any state—solid, liquid, or gas—can be subjected to electrolysis.

[0015] (anode) The anode is the oxygen-evolving electrode (anode). Oxide ions (O) are generated by the electrolysis of the oxide ion source (the material being electrolyzed). 2-) is oxidized on the anode. No reaction between oxide ions and carbon occurs on the LSC anode. Therefore, anode wear is suppressed, and oxygen (preferably oxygen only) is generated from the anode, rather than carbon dioxide and / or carbon monoxide.

[0016] LSC anodes exhibit higher corrosion resistance than carbon or platinum electrodes in electrolysis using molten salt. The corrosion resistance of an electrode can be evaluated, for example, from its corrosion rate. Corrosion rate γ (g / cm²) 2 ·h) can be calculated using the following formula, based on the paper: S. Jiao, Derek J. Fray, The Minerals, Metals & Materials Society and ASM International, 41B (2010). γ = ΔW / t·S △W: Mass change of electrodes before and after electrolysis (g) t: Electrolysis (immersion) time (h) S: Surface area of ​​the immersed portion of the electrode (cm²) 2 )

[0017] According to the above paper, the corrosion rate γ is 1.5 × 10⁻⁶. -3 (g / cm 2 •h) is considered desirable. The anode corrosion rate γ used in this disclosure is 1.5 × 10 -3 (g / cm 2 h) is less than or equal to 1.0 × 10 -3 (g / cm 2 • h) is less than or equal to 0.5 × 10 -3 (g / cm 2 h) may be less than or equal to

[0018] LSC anodes exhibit excellent conductivity (electron conductivity) over a wide temperature range, from room temperature to high temperatures. For example, in the temperature range from 20°C to 850°C, the conductivity of an LSC anode is 8 × 10⁻⁶. 4The conductivity is greater than or equal to S / m. Conductive composite oxides are generally known, and their conductivity increases with increasing temperature. However, the conductivity of composite oxides other than LSC oxides is considerably lower than that of LSC anodes, even at high temperatures. For example, the conductivity of NiO-Fe2O3-Cu is 1.11 × 10⁻¹⁰ at 980°C. 3 It is approximately S / m (Source: I. Galasiu, R. Galasiu, J. Thonstad, “Inert Anodes for Aluminum Electrolysis”, 1 st edition, Alminium-Verlag (2007)).

[0019] In the oxygen evolution process of this embodiment, the reactant is oxide ions. LSC oxide is considered to have particularly excellent affinity for these oxide ions. Therefore, the LSC anode is particularly suitable for the oxygen evolution process of this embodiment. The fact that the affinity for the reactant changes depending on the elemental composition of the electrode is shown, for example, in the papers: MH Seo, HW Park, DU Lee, MG Park, Z. Chen, ACS Catal., 5 (2015) 4337., and J. Suntivich, KJ May, HA Gasteiger, JB Goodenough, YS Horn, Science, 334 (2011) 1383.

[0020] LSC oxides have a perovskite-type crystal structure. Perovskite-type composite oxides are generally represented as ABO3. The A site contains an element with a larger ionic radius than the B site. LSC oxides contain lanthanum (La) and strontium (Sr) as elements located at the A site, and cobalt (Co) as an element located at the B site.

[0021] LSC oxides are, for example, given by the following formula (1): La 1-x Sr x Co 1-y M y O 3-δ (In the formula, M is a transition metal other than lanthanum and cobalt, 0.1 ≤ x ≤ 0.9, 0 ≤ y ≤ 0.1, and δ is the oxygen deficiency.) It is represented as follows.

[0022] La and Sr are arranged at site A. The proportion x of Sr in site A (based on the number of elements) is 0.1 ≤ x ≤ 0.9. When the proportion x of Sr is 0.1 or greater, excellent conductivity can be obtained over a wide temperature range. In particular, since high conductivity can be easily obtained at high temperatures, the proportion x of Sr may be 0.2 or greater, or 0.3 or greater. When the proportion x of Sr is 0.9 or less, the sinterability of the LSC oxide improves, and the relative density tends to increase. From the viewpoint of relative density, the proportion x of Sr may be 0.6 or less, or 0.5 or less. In one embodiment, the proportion x of Sr may be 0.2 ≤ x ≤ 0.6, or 0.3 ≤ x ≤ 0.5.

[0023] Co is placed at site B. A metal element M other than La and Co, which is a transition metal, may also be placed at site B along with Co. Examples of metal elements M include first transition metals such as scandium (Sc), titanium (Ti), vanadium (V), chromium (Cr), manganese (Mn), iron (Fe), nickel (Ni), and copper (Cu). These can be used individually or in combination of two or more.

[0024] From the viewpoint of conductivity at high temperatures, it is desirable for the proportion of metallic element M in the B site to be small. The proportion y (based on the number of elements) of metallic element M in the B site is 0 ≤ y ≤ 0.1, may be 0 ≤ y ≤ 0.05, and may be y = 0.

[0025] A desirable LSC oxide is, for example, the following formula (2): La 1-x Sr x OO 3-δ (In the formula, 0.2 ≤ x ≤ 0.6, and δ is the oxygen deficiency.) It is represented as follows.

[0026] The oxygen deficiency δ can vary depending on the manufacturing conditions of the LSC oxide. For example, the oxygen deficiency δ may be 0 ≤ δ ≤ 0.15, 0 ≤ δ ≤ 0.10, or 0 ≤ δ ≤ 0.05. The proportion of each element in the LSC oxide can be determined, for example, using wavelength dispersive X-ray spectroscopy with an electron probe microanalyzer.

[0027] The LSC anode may contain LSC oxide raw materials or composite oxides other than LSC oxide. From the viewpoint of corrosion resistance and conductivity, the proportion of LSC oxide in the anode may be 80% by mass or more, 90% by mass or more, or 100% by mass. From a similar viewpoint, it is desirable that the anode be formed from a single phase of LSC oxide.

[0028] The relative density of the anode may be 90% or higher, 95% or higher, or 98% or higher. This further improves the corrosion resistance and conductivity of the anode. Relative density is one indicator of the amount of voids. A higher relative density indicates fewer voids and a denser material. The relative density of an anode made of LSC oxide is calculated by dividing the measured mass of the anode by the theoretical mass of the anode, which is calculated by multiplying the specific gravity of the LSC oxide by the apparent volume of the anode.

[0029] (cathode) On the cathode, a reduction reaction of cations originating from the oxide ion source occurs. The material of the cathode is not particularly limited. Examples of cathode materials include metals such as Ag, Cu, Ni, Pb, Hg, Tl, Bi, In, Sn, Cd, Au, Zn, Pd, Ga, Ge, Ni, Fe, Pt, Pd, Ru, Ti, Cr, Mo, W, V, Nb, Ta, Zr and their alloys, as well as carbon materials such as glassy carbon, natural graphite, isotropic graphite, pyrolytic graphite, plastic-formed carbon and conductive diamond.

[0030] (Oxide ion source) The oxide ion source is the object of electrolysis (the material being electrolyzed). The oxide ion source is not particularly limited as long as it contains oxygen atoms. The state of the oxide ion source is also not particularly limited and may be a gas, liquid, or solid at room temperature. Examples of oxide ion sources that are solid at room temperature include metal oxides and metal carbonates (hereinafter collectively referred to as first metal compounds). Examples of oxide ion sources that are gaseous at room temperature (hereinafter referred to as oxide gases) include carbon oxides (i.e., carbon dioxide), sulfur oxides (so-called SOx), and nitrogen oxides (so-called NOx). An example of an oxide ion source that is liquid at room temperature is hydrogen oxide (i.e., water).

[0031] The first metal compound is not particularly limited. According to this disclosure, electrolysis can be performed at high temperatures. Therefore, even a first metal compound that is difficult to melt can be subjected to electrolysis. The first metal may be, for example, aluminum, titanium, zirconium, vanadium, or silicon, or a metal used as fuel for nuclear power generation such as plutonium or uranium, or an alkali metal or alkaline earth metal.

[0032] The amount of the first metal compound added to the molten salt is not particularly limited. According to this disclosure, a larger amount of the first metal compound can be dissolved in the molten salt. From the viewpoint of reaction efficiency, the amount of the first metal compound added is preferably 1 mol% or more, more preferably 2 mol% or more, and particularly preferably 3 mol% or more, based on the total number of moles of molten salt in the electrolytic bath. The amount of the first metal compound added is, for example, 20 mol% or less, may be 15 mol% or less, or may be 10 mol% or less, based on the total number of moles of molten salt in the electrolytic bath. In one embodiment, the amount of the first metal compound added is 1 mol% or more and 20 mol% or less, based on the total number of moles of molten salt in the electrolytic bath.

[0033] Oxide gases are added to the molten salt by blowing them into the gas phase of the electrolytic cell and bringing them into contact with the liquid surface of the molten salt, or by blowing them into the molten salt. A sufficient amount of oxide gas may be added to the molten salt before applying voltage, or the oxide gas may be added to the molten salt while applying voltage. The oxide gas may also be mixed with an inert gas (typically argon gas) before being added to the molten salt. The amount of oxide gas added can be appropriately set considering its solubility in the molten salt, etc. Oxides that are liquid at room temperature can be added to the molten salt in the same way as oxide gases after being heated to a gaseous state, for example.

[0034] (molten salt) Molten salts function as electrolytes in electrolytic baths. Molten salts facilitate the melting of oxide ion sources. Examples of molten salts include salts (metal salts, including metal oxides) of metal ions (hereinafter referred to as second metals) and their counterions (hereinafter referred to as second anions).

[0035] The metal salt is not particularly limited and is appropriately selected depending on the oxide ion source, electrolysis temperature, etc. Examples of secondary metals include alkali metals, alkaline earth metals, rare earth elements, aluminum (Al), gallium (Ga), indium (In), thallium (Tl), zinc (Zn), cadmium (Cd), gold (Au), silver (Ag), and copper (Cu).

[0036] Examples of alkali metals include at least one selected from the group consisting of lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), and francium (Fr). Examples of alkaline earth metals include at least one selected from the group consisting of beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), and radium (Ra). Examples of rare earth elements include scandium (Sc), yttrium (Y), lanthanide elements, and actinide elements. Among these, at least one selected from the group consisting of alkali metals and alkaline earth metals is preferred from the viewpoint of stability and solubility of oxide ion sources.

[0037] Examples of second anions include carbonate ions (CO3). 2- ), sulfate ions, phosphate ions, nitrate ions, acetate ions, carboxylate ions, oxide ions (O2 - Examples include halogen ions. Among these, halogen ions are preferred from the viewpoint of stability and solubility of oxide ion sources.

[0038] Examples of halogens include at least one selected from the group consisting of fluorine (F), chlorine (Cl), bromine (Br), iodine (I), and astatine (At). Preferred halogens include at least one selected from the group consisting of F, Cl, Br, and I.

[0039] Examples of metal salts include alkali metal halides such as LiF, NaF, KF, RbF, CsF, LiCl, NaCl, KCl, RbCl, CsCl, LiBr, NaBr, KBr, RbBr, CsBr, LiI, NaI, KI, RbI, and CsI; alkaline earth metal halides such as MgF2, CaF2, SrF2, BaF2, MgCl2, CaCl2, SrCl2, BaCl2, MgBr2, CaBr2, SrBr2, BaBr2, MgI2, CaI2, SrI2, and BaI2; halides of rare earth elements such as AlCl3; oxides of metals other than primary metals such as Li2O and CaO; metal carbonates such as Li2CO3, Na2CO3, and K2CO3; and metal nitrates such as LiNO3, NaNO3, and KNO3. Among these, at least one selected from the group consisting of lithium salts, sodium salts, and potassium salts is preferred.

[0040] Metal salts can be used individually or in combination of two or more. In particular, it is preferable to use two or more other metal salts in combination, as this tends to lower the melting temperature. Examples include combinations of multiple chlorides, combinations of multiple fluorides, and combinations of one or more chlorides and one or more fluorides. Specific examples include combinations of LiCl and KCl, LiCl and CaCl2, LiCl, KCl and CaCl2, LiF, NaF and KF, NaF and NaCl, and NaCl, KCl and AlCl3.

[0041] In combinations of multiple metal salts, the mixing ratio of each metal salt is not particularly limited. For example, in a combination of LiCl and KCl, the number of moles of LiCl may be 30 mol% or more, 45 mol% or more, or 50 mol% or more, relative to the total number of moles of LiCl and KCl. The number of moles of LiCl may be 90 mol% or less, 70 mol% or less, or 65 mol% or less, relative to the total number of moles of LiCl and KCl. In one embodiment, the number of moles of LiCl is 45 mol% or more and 90 mol% or less, relative to the total number of moles of LiCl and KCl.

[0042] (electrolytic cell) The electrolytic cell is not particularly limited as long as it is heat-resistant and can accommodate the required amount of molten salt. The shape, size, and material of the electrolytic cell are appropriately selected according to the purpose. Examples of electrolytic cell materials include stainless steel, aluminum oxide, Pyrex® glass, and quartz.

[0043] (power supply) The power supply is electrically connected to both the cathode and the anode. The power supply applies a voltage (typically a DC voltage) between the cathode and the anode. Conventional known power supplies can be used as appropriate.

[0044] Figure 1 is a schematic diagram showing an example of an oxygen generator according to this disclosure. The oxygen generator 20 comprises an electrolytic cell 1, a molten salt 2, a cathode 3, an anode 4, and a power supply 5. The molten salt 2 is housed in the electrolytic cell 1 and contains a molten metal salt. At least portions of the cathode 3 and anode 4 are immersed in the molten salt 2. The power supply 5 is electrically connected to the cathode 3 and anode 4, respectively, and applies a voltage between them. The oxygen generator 20 further includes a heater 6 for heating the metal salt to maintain its molten state. The heater 6 is arranged, for example, to surround the outside of the electrolytic cell 1.

[0045] When an oxide ion source MOx is added to the molten salt 2 and a voltage is applied between the cathode 3 and anode 4 by the power supply 5, the oxide ion source MOx is reduced in the molten salt 2 as follows. As a result, elemental M and oxygen O2 are produced. Elemental M precipitates at the bottom of the electrolytic cell 1, for example, and is recovered. Oxygen O2 is discharged into the gas phase of the electrolytic cell 1 and recovered. A recovery tank (not shown) for recovering elemental M may be placed inside the electrolytic cell 1.

[0046] Cathode: M x+ +xe - → M Anode: 2O 2- → O2+4e - Total reaction: MOx → M+x / 2O2

[0047] The oxygen generator according to this disclosure uses LSC oxide as the anode material, which makes it difficult for the anode to react with oxide ions. Therefore, oxygen is efficiently generated from the anode, and anode wear is suppressed. Furthermore, LSC oxide is difficult to dissolve in molten salt, which suppresses the generation of impurities.

[0048] [Oxygen generation method] The oxygen generation method according to this disclosure comprises an electrolytic cell, a molten salt containing oxide ions housed in the electrolytic cell, a cathode at least partially immersed in the molten salt, an anode at least partially immersed in the molten salt, and a power supply for applying a voltage between the cathode and the anode, wherein the anode contains a composite oxide comprising lanthanum, strontium, and cobalt. A voltage is applied between the cathode and the anode using this oxygen generation device. As a result, the oxide ions contained in the molten salt are oxidized, and oxygen (preferably only oxygen) is generated from the anode.

[0049] Details of the oxygen generator are as described above.

[0050] The applied voltage is not particularly limited as long as oxygen is generated. Oxygen evolution potential (Li + The potential (Li reference) is typically between 2.4V and 3.7V. When using an LSC anode, the potential (Li + A stable and high current density can be obtained in the range of 2.4V to 3.7V (Li reference).

[0051] The temperature of the molten salt during electrolysis may be between 400°C and 850°C. Even at such high temperatures, the LSC anode exhibits excellent conductivity, resulting in high electrolysis efficiency, and furthermore, consumption and dissolution are suppressed. In addition, because the molten salt can be heated to a high temperature, a larger number of oxide ion sources can be processed rapidly. Furthermore, various oxide ion sources can be electrolyzed. The temperature of the molten salt may be above 420°C, or above 430°C. The temperature of the molten salt may be below 800°C, or below 700°C.

[0052] [Manufacturing method for LSC anodes] The anode used in this disclosure (LSC anode) is manufactured, for example, by the following method. This yields an anode with high relative density that is suitable as an oxygen-evolving electrode. Below, an anode made of LSC oxide is manufactured, but the anode used in this disclosure may be formed from LSC oxide and other materials.

[0053] LSC anodes are manufactured by a method that includes calcining (pre-calcination) raw materials containing La, Sr, and Co elements at a temperature of 700°C to 1000°C for 10 hours or more, crushing the resulting calcined material, molding the crushed material into a desired shape, and calcining (final calcination) the molded material at a temperature of 1200°C to 1600°C for 5 hours or more.

[0054] (1) Pre-firing The raw materials may contain La, Sr, and Co. The raw materials may be a combination of metal compounds containing La, Sr, and Co, or a combination of metal compounds containing at least two of these elements. The raw materials may optionally further contain metal element M. Examples of raw materials include metal compounds such as oxides, carbonates, and nitrates of the above elements. Specific examples of such metal compounds include lanthanum oxide, lanthanum carbonate, strontium oxide, cobalt oxide, and cobalt carbonate. The raw materials contain La, Sr, Co, and metal element M in proportions that satisfy x and y in formula (1) above.

[0055] The metal compounds are mixed dry and then calcined. Calcination generates the target product, LSC oxide. Calcination is carried out at a temperature between 700°C and 1000°C for at least 10 hours. This facilitates the formation of a single phase of LSC oxide. The single phase can be confirmed, for example, by X-ray diffraction (XRD) analysis.

[0056] The calcination temperature may be 750°C or higher, or 800°C or higher, as it facilitates the further formation of a single phase of LSC oxide. Similarly, the calcination temperature may be 900°C or lower. Likewise, the calcination time may be 20 hours or higher, or 22 hours or higher. From the viewpoint of productivity, the calcination time may be 48 hours or lower, or 30 hours or lower.

[0057] The calcination time is the period excluding the heating and cooling processes. The calcination temperature is the average temperature during the calcination time. During the calcination time, it is permissible for the temperature to briefly fall below 700°C or exceed 1000°C, either momentarily or for a short period. "Momentarily" means for a period of 15 minutes or less. "Short period" means for a period of less than 20% of the calcination time. The same applies to the firing time and firing temperature.

[0058] The calcination process is carried out in an oxygen-containing atmosphere. The oxygen content of the atmosphere used in the calcination process is not particularly limited. For example, calcination may be carried out in an air atmosphere (oxygen content: approximately 20% by volume) or in pure oxygen (oxygen content: 100% by volume).

[0059] Prior to calcination, a pre-calcination may be performed to remove crystal water and organic matter contained in the raw materials. Pre-calcination is performed, for example, at a lower temperature and for a shorter duration than calcination.

[0060] (Crush) The resulting calcined material is then pulverized. This facilitates the formation of a single phase of LSC oxide. In addition, the shape and particle size of the calcined material become more uniform, which tends to increase the relative density of the resulting anode.

[0061] Grinding is carried out using, for example, a bead mill, ball mill, rod mill, grinding roll, or jet mill. Grinding using a planetary ball mill is performed after the calcined material has cooled, for example, at a rotation speed of 200 rpm to 500 rpm for 2 to 10 hours. The diameter of the grinding media used in a bead mill is, for example, 0.01 mm to 50 mm. Examples of materials for the grinding media include zirconium dioxide or aluminum oxide.

[0062] (molding) The crushed material is molded into the desired shape. Molding is performed, for example, by various presses (typically, cold isohydraulic presses). The pressing pressure is not particularly limited. For example, the pressing pressure is between 200 MPa and 400 MPa.

[0063] (Firing) The molded product is fired at a temperature between 1200°C and 1600°C for at least 5 hours. This yields an LSC anode. The LSC anode is preferably formed from a single phase of LSC oxide. The relative density of the LSC anode is, for example, 90% or more.

[0064] The firing temperature may be 1250°C or higher, or 1300°C or higher, as it facilitates the further formation of a single phase of LSC oxide. Similarly, the firing temperature may be 1550°C or lower. Likewise, the firing time may be 6 hours or higher, or 7 hours or higher. From the viewpoint of productivity, the firing time may be 15 hours or lower, or 10 hours or lower. [Examples]

[0065] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples.

[0066] [Experimental equipment] Figure 2 is a schematic diagram of the experimental apparatus used in this embodiment. The experimental apparatus 30 comprises an electrolytic cell 1, molten salt 2, a cathode 3, an anode 4, and a power supply 5. The experimental apparatus 30 further comprises a reference electrode 7, a thermocouple 9, a supply pipe 10, and a discharge pipe 11. The electrolytic cell 1 is housed in a sealed container 12. The sealed container 12 comprises a main body 12a and a lid 12b that closes the upper opening of the main body 12a. A heater 6 is arranged on the outside of the sealed container 12, surrounding it.

[0067] The cathode 3 is a coiled nickel wire. The anode 4 is formed from LSC oxide. The reference electrode 7 is Ag +This is an Ag electrode. Cathode 3, anode 4, and reference electrode 7 are each connected to a potentiostat / galvanostat device (manufactured by Biologic) by nickel wires 8. Molten salt 2 is a molten metal salt and is contained in electrolytic cell 1. Cathode 3, anode 4, and reference electrode 7 are fixed to lid 12b so as to be immersed in the molten salt 2. Argon gas is introduced into electrolytic cell 1 from supply pipe 10, and the experimental apparatus 30 is maintained in an argon atmosphere. The argon gas, along with the generated oxygen, is discharged outside the experimental apparatus 30 from discharge pipe 11, recovered, and its composition is analyzed by gas chromatography or other means as needed.

[0068] [Example 1] (i) Preparation of the anode Lanthanum oxide, strontium oxide, and cobalt oxide were mixed in a ball mill for 2 hours in a molar ratio such that x = 0.4 and y = 0 in equation (1). The resulting mixture was dried and then calcined at 850°C for 24 hours (calcination). The composition of the mixture after calcination was confirmed by X-ray diffraction (XRD) analysis. The results of the XRD analysis are shown in Figure 3A. XRD analysis revealed that the resulting mixture was composed of La 0.6 Sr 0.4 OO 3-δ It was confirmed that it is formed by a single phase.

[0069] The calcined mixture was ground in a bead mill (300 rpm) for 8 hours. Next, this ground material was formed into strips using a hydrostatic press. The resulting molded bodies were calcined at 1400°C for 8 hours in an air atmosphere (main calcination) to obtain an LSC anode. The composition of the anode was confirmed by X-ray diffraction (XRD) analysis. The results of the XRD analysis are shown in Figure 3B. XRD analysis confirmed that the obtained anode also contained La 0.6 Sr 0.4 OO 3-δ It was confirmed that it is formed by a single phase.

[0070] The conductivity of the LSC anode was measured using the four-terminal method while increasing the temperature up to 800°C. The results are shown in Figure 4. The conductivity of the anode containing LSC oxide at 600°C was 1.21 × 10⁻⁶.5 The value was S / m. Figure 4 shows that the anode containing LSC oxide has extremely high conductivity even at high temperatures.

[0071] (ii) Electrolysis LiCl and KCl were mixed so that LiCl / KCl = 58.5 mol% / 41.5 mol%, and the mixture was vacuum-dried at 200°C and 100 Pa or less for 24 hours or more. 3 mol% of Li2O relative to the total number of moles of LiCl and KCl was weighed and added to the mixture to obtain a mixed salt. The mixed salt was placed in the electrolytic cell described above, covered, and heated to 450°C in an argon atmosphere. In this way, a molten LiCl-KCl salt containing Li2O was obtained.

[0072] Next, using a potentiostat / galvanostat apparatus, the potential of the LSC anode relative to the reference electrode was changed from 2.4V to 4.0V (vs. Li + A voltage was applied such that the voltage was equal to ( / Li). Cyclic voltammetry (scanning speed 100 mV / sec) was performed. The results are shown in Figure 5. In Figure 5, the horizontal axis is the anode potential (V, vs. Li). + The graph shows the current density (mA / cm³) at the anode (Li), with the vertical axis representing the anode current density (mA / cm³). -2 This indicates Ag + The potential measured using the Ag standard is calculated by using the potential between the lithium metal electrochemically deposited on the nickel wire and the lithium ions in the bath. + Calibrated to / Li standards.

[0073] Figure 5 shows that the oxidation current, caused by oxygen evolution, rises from around 2.4V and remains stable up to around 3.7V. Since the oxygen evolution potential (vs. Li+ / Li) is approximately 2.4V to 3.7V, it can be seen that the LSC anode can function efficiently as an oxygen evolution electrode.

[0074] Next, constant current electrolysis was performed. The electrolysis conditions were 450°C and a current density of 57.8 mA / cm². 2The electrolysis period was set to 10 hours. Figure 6 is a graph showing the change in the potential of the LSC anode over time during electrolysis. According to Figure 6, during 10 hours of electrolysis, the potential of the LSC anode (vs. Li+ / Li) remained stable between 3.0V and 3.1V. This indicates that oxygen is stably generated in the apparatus using the LSC anode. Furthermore, analysis of the recovered gas by gas chromatography confirmed that the generated gas was only oxygen gas.

[0075] After electrolysis was completed, the LSC anode was removed and observed visually, and its surface was further examined using a scanning electron microscope (SEM). Figure 7A is a secondary electron image (3000x magnification) of the anode surface taken with SEM before electrolysis. Figure 7B is a backscattered electron image (3000x magnification) of the anode surface taken with SEM before electrolysis. Figure 8A is a secondary electron image (3000x magnification) of the anode surface taken with SEM after electrolysis. Figure 8B is a backscattered electron image (3000x magnification) of the anode surface taken with SEM after electrolysis. Visual observation revealed no significant changes in the appearance of the anode before and after electrolysis. In particular, the corners did not become rounded, and the original sharp shape was maintained. Furthermore, as can be seen from the SEM images, no significant changes were observed in the surface condition of the anode, and its smoothness was maintained. From this, it can be seen that anodes containing LSC oxide have low wear and high corrosion resistance to molten salts.

[0076] The high corrosion resistance of LSC anodes can also be confirmed by their low corrosion rate γ. The corrosion rate γ of LSC anodes calculated as described above is 2.4 × 10⁻⁶. -4 (g / cm 2 ·h) and the desirable standard is 1.5 × 10 -3 (g / cm 2 It was an order of magnitude smaller than h).

[0077] Furthermore, the composition of the LSC anode after electrolysis was evaluated by X-ray diffraction (XRD) analysis. The results are shown in Figure 9. The peak of the LSC anode before electrolysis shown in Figure 3B coincides with the peak shown in Figure 9, indicating that no change in the composition of the LSC anode was observed before and after electrolysis. In other words, the LSC anode is chemically stable.

[0078] [Example 2] A molten salt was prepared in the same manner as in Example 1, except that 0.5 mol% of Li2O was added relative to the total number of moles of LiCl and KCl, and cyclic voltammetry (scanning speed 100 mV / sec) was performed. The results are shown in Figure 5. In Example 2 as well, a rise in oxidation current due to oxygen evolution was observed from around 2.4 V potential, and it was confirmed that the current flowed stably up to around 3.7 V potential.

[0079] [Example 3] LiCl and CaCl2 were mixed so that LiCl / CaCl2 = 65.0 mol% / 35.0 mol%, and the mixture was vacuum-dried at 200°C and 100 Pa or less for 24 hours or more. 1 mol% of CaO relative to the total number of moles of LiCl and CaCl2 was weighed and added to the mixture to obtain a mixed salt. The mixed salt was placed in the electrolytic cell described above, covered, and heated to 600°C in an argon atmosphere. In this way, a molten salt of LiCl-CaCl2 containing CaO was obtained.

[0080] Cyclic voltammetry (scanning speed 100 mV / sec) was performed using the molten salt at 600°C mentioned above. The results are shown in Figure 10. Even at high electrolysis temperatures, an oxidation current rise due to oxygen evolution was observed from around 2.4 V potential, and it was confirmed that the current flowed stably up to around 3.7 V potential.

[0081] [Example 4] A molten salt was prepared at 600°C in the same manner as in Example 3, except that 8 mol% of Li2O was added relative to the total number of moles of LiCl and KCl. A higher electrolysis temperature allows for a larger amount of oxide ion source to be added.

[0082] Cyclic voltammetry (scanning speed 100 mV / sec) was performed using the obtained molten salt at 600°C. The results are shown in Figure 10. Even at high electrolysis temperatures, the rise of oxidation current due to oxygen evolution was observed from around 2.9 V potential. Therefore, it can be seen that an anode containing LSC oxide can function efficiently as an oxygen-evolving electrode even under high-temperature conditions.

[0083] [Comparative Example 1] By changing to an LSC anode, La 0.7 Sr 0.3 FeO 3-δ Li2O was electrolyzed in the same manner as in Example 1, except that an anode formed by (LSF anode) was used. The conductivity of the LSF anode was measured in the same manner as in Example 1. The results are shown in Figure 4. The conductivity of the LSF anode at 600°C was 1.32 × 10⁻⁶. 4 It was S / m. The corrosion rate γ of the LSF anode calculated as described above is 1.7 × 10⁻⁶ -1 (g / cm 2 ·h) and the desirable standard is 1.5 × 10 -3 (g / cm 2 It was two orders of magnitude larger than h). [Industrial applicability]

[0084] The oxygen generator and oxygen generation method according to the present invention can be used to generate oxygen from various oxide ion sources. [Explanation of symbols]

[0085] 20. Oxygen generator 30 Experimental apparatus 1 electrolytic cell 2 Molten salt 3 cathode 4 Anode 5 Power supply 6 Heater 7 Reference electrode 8 conductor 9 Thermocouples 10 Supply pipe 11 Discharge pipe 12. Airtight container 12a Main Unit 12b Lid

Claims

1. An electrolytic cell; a molten salt contained in the electrolytic cell and containing oxide ions; a cathode at least partially immersed in the molten salt; an anode at least partially immersed in the molten salt; a power source for applying a voltage between the cathode and the anode; An oxygen generating device that oxidizes the oxide ions to generate oxygen, The anode comprises a composite oxide containing lanthanum, strontium and cobalt.

2. The composite oxide has the following formula (1): La 1-x Sr x Co 1-y M y O 3-δ (In the formula, M is a transition metal other than lanthanum and cobalt, 0.1≦x≦0.9, 0≦y≦0.1, and δ>0.) The oxygen generating device according to claim 1 ,

3. The composite oxide has the following formula (2): La 1-x Sr x CoO 3-δ (Wherein, 0.2≦x≦0.6, δ>0.) The oxygen generating device according to claim 1 or 2, wherein

4. An electrolytic cell; a molten salt contained in the electrolytic cell and containing oxide ions; a cathode at least partially immersed in the molten salt; an anode at least partially immersed in the molten salt; a power source for applying a voltage between the cathode and the anode; The anode includes a composite oxide including lanthanum, strontium, and cobalt, and the oxygen generating apparatus is used. a voltage is applied between the cathode and the anode to oxidize the oxide ions and generate oxygen.

5. The composite oxide has the following formula (1): La 1-x Sr x Co 1-y M y O 3-δ (In the formula, M is a transition metal other than lanthanum and cobalt, 0.1≦x≦0.9, 0≦y≦0.1, and δ>0.) The oxygen generating method according to claim 4 , wherein

6. The composite oxide has the following formula (2): La 1-x Sr x CoO 3-δ (Wherein, 0.2≦x≦0.6, δ>0.) The oxygen generating method according to claim 4 or 5, wherein the oxygen generating method is represented by the formula:

7. The oxygen generating method according to any one of claims 4 to 6, wherein the temperature of the molten salt is 400°C or higher and 850°C or lower.

8. The compound of the formula: La 1-x Sr x Co 1-y M y O 3-δ (In the formula, M is a transition metal other than lanthanum and cobalt, 0.1≦x≦0.9, 0≦y≦0.1, and δ>0.) An electrode comprising a composite oxide represented by the formula:

9. The electrode according to claim 8, wherein in the complex oxide, y=0.

10. An electrode as described in claim 8 or 9, for use in the electrolysis of a molten salt containing oxide ions.