Titanium-niobium composite oxide and electrode and lithium-ion secondary battery using the same

JP2023093557A5Active Publication Date: 2024-10-09KUBOTA CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023062613
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-12-26
Filing Date
2023-04-07
Publication Date
2024-10-09
Estimated Expiration
2040-12-25

AI Technical Summary

Technical Problem

The synthesis of titanium-niobium composite oxides using the solid-state reaction method faces challenges where low firing temperatures result in impurities like TiO2 and Ti2Nb10O29, while high temperatures lead to excessive crystal grain growth, affecting the performance of lithium-ion secondary batteries.

Method used

A titanium-niobium composite oxide is formulated with controlled amounts of alkali metal elements and additional elements like Al, Y, La, Ce, Pr, and Sm, along with a specific atomic ratio, to suppress impurity formation and crystal grain growth, and optionally coated with carbon, to enhance performance.

Benefits of technology

The solution effectively suppresses the formation of TiO2 and Ti2Nb10O29 impurities and controls crystal grain growth, improving the charge/discharge performance and rate characteristics of lithium-ion secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

To provide a titanium-niobium complex oxide in which the mixing of TiO2 and Ti2 Nb10O29 and the fibrous growth of crystal grains are suppressed, and to provide an electrode and a lithium-ion secondary battery using the same.SOLUTION: A titanium-niobium complex oxide according to the present invention contains less than 0.30 atm% of alkali metal elements and at least one element of Al, Y, La, Ce, Pr and Sm. A ratio of a total atomic weight of Al, Y, La, Ce, Pr and Sm to a total atomic weight of Ti and Nb is 0.001 or more.SELECTED DRAWING: Figure 1A
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This invention relates to a titanium-niobium composite oxide, and more particularly to an electrode using the titanium-niobium composite oxide as an electrode active material, and to a lithium-ion secondary battery using this electrode as a positive or negative electrode. [Background technology]

[0002] Titanium niobium composite oxides are expected to be used as active materials for lithium-ion secondary batteries because they have high electrical capacity and excellent cycle capacity retention (see, for example, Patent Document 1). [Prior art documents] [Patent Documents]

[0003] [Patent Document 1] Japanese Patent Publication No. 2010-287496 [Patent Document 2] Japanese Patent Publication No. 2014-225474 [Overview of the project] [Problems that the invention aims to solve]

[0004] For example, when synthesizing titanium niobium composite oxides by solid-phase reaction, if the calcination temperature is too low and the reaction is insufficient, in addition to the desired product TiNb2O7, other products such as TiO2 and Ti2Nb may be produced. 10 O 29 These are mixed together. TiO2 and Ti2Nb are contained in the titanium niobium composite oxide. 10 O 29 This causes a decrease in the charge-discharge performance of titanium niobium composite oxides.

[0005] On the other hand, TiO2 and Ti2Nb 10 O 29 If the firing temperature is increased to allow the reaction to proceed sufficiently in order to suppress the presence of other elements, crystal grains (primary grains) will grow. This growth of crystal grains can cause a decrease in the rate characteristics of lithium-ion secondary batteries that use titanium niobium composite oxide as the electrode active material.

[0006] Therefore, it is conceivable to improve the reactivity of titanium niobium composite oxide by adding alkali metal elements so that a sufficient reaction can be obtained even at low firing temperatures (see, for example, Patent Document 2). However, simply adding alkali metal elements can lead to adverse effects such as the growth of fibrous crystal grains and a decrease in the active material packing density of electrodes using titanium niobium composite oxide as the electrode active material.

[0007] In view of the above problems, the present invention relates to TiO2 and Ti2Nb 10 O 29 The objective is to provide a titanium-niobium composite oxide in which the coexistence of various materials and the fibrous growth of crystal grains are suppressed, as well as electrodes and lithium-ion secondary batteries using the same. [Means for solving the problem]

[0008] To achieve the above objective, the titanium niobium composite oxide according to the first aspect of the present invention contains 0.05 atomic% or more and less than 0.30 atomic% of alkali metal elements, contains at least one of the elements Al, Y, La, Ce, Pr, and Sm, contains the elements Ti, Nb, and O, the remainder being impurities, and the ratio of the total atomic weights of Al, Y, La, Ce, Pr, and Sm to the total atomic weights of Ti and Nb is 0.001 or more (first configuration).

[0009] Furthermore, in the titanium-niobium composite oxide of the first configuration described above, it is preferable that the ratio of the total atomic weights of Al, Y, La, Ce, Pr, and Sm to the total atomic weights of Ti and Nb is 0.002 or more (second configuration).

[0010] Furthermore, in the titanium-niobium composite oxide of the first or second configuration described above, it is preferable that the ratio of the total atomic weights of Al, Y, La, Ce, Pr, and Sm to the total atomic weights of Ti and Nb is less than 0.024 (third configuration).

[0011] To achieve the above objective, the titanium niobium composite oxide according to the second aspect of the present invention contains 0.05 atomic% or more and less than 0.30 atomic% of alkali metal elements, contains at least one of the elements Al, Y, La, Ce, Pr, and Sm, and has a composition (fourth composition) in which the ratio of the total atomic weight of Y to the total atomic weight of Ti and Nb is 0.001 or more and 0.011 or less.

[0012] To achieve the above objective, the titanium-niobium composite oxide according to the third aspect of the present invention contains 0.05 atomic% or more and less than 0.30 atomic% of alkali metal elements, contains at least one of the elements Al, Y, La, Ce, Pr, and Sm, the ratio of the total atomic weights of Al, Y, La, Ce, Pr, and Sm to the total atomic weights of Ti and Nb is 0.001 or more, and when the aspect ratio, which is expressed as the ratio of the major axis length to the minor axis length of the primary particles of the titanium-niobium composite oxide, is expressed as a volume-based log-normal distribution, the proportion of primary particles with an aspect ratio exceeding 3 is 11 volume% or less (fifth configuration).

[0013] To achieve the above objective, the titanium-niobium composite oxide according to the fourth aspect of the present invention contains 0.05 atomic% or more and less than 0.30 atomic% of alkali metal elements, contains at least one of the elements Al, Y, La, Ce, Pr, and Sm, the ratio of the total atomic weights of Al, Y, La, Ce, Pr, and Sm to the total atomic weights of Ti and Nb is 0.001 or more, and when the long axis lengths of the primary particles of the titanium-niobium composite oxide are expressed in a volume-based log-normal distribution, the proportion of primary particles with a long axis length exceeding 3 μm is 5 volume% or less (sixth aspect).

[0014] Furthermore, in the titanium-niobium composite oxide having any of the above configurations 1 to 6, it is preferable that a portion of the surface of the titanium-niobium composite oxide is coated with a carbon material (configuration 7).

[0015] To achieve the above objective, the electrode according to the present invention comprises an electrode active material, wherein at least a portion of the electrode active material is a titanium niobium composite oxide having one of the first to seventh configurations (the eighth configuration).

[0016] To achieve the above object, the lithium ion secondary battery according to the present invention includes a positive electrode and a negative electrode, and a configuration (ninth configuration) in which either the positive electrode or the negative electrode is the electrode having the eighth configuration.

Effects of the Invention

[0017] According to the present invention, it is possible to provide a titanium niobium composite oxide in which the mixing of TiO2 and Ti2Nb 10 O 29 and the fibrous growth of crystal grains are suppressed, an electrode using the same, and a lithium ion secondary battery.

Brief Description of the Drawings

[0018] [Figure 1A] Analysis results of titanium niobium composite oxides of Examples 1 to 13 and Comparative Examples 1 to 3 [Figure 1B] Analysis results of titanium niobium composite oxides of Examples 14 to 19 [Figure 1C] Analysis results of titanium niobium composite oxides of Examples 20 to 21 [[ID=2�]] [Figure 1D] Analysis results of titanium niobium composite oxides of Examples 22 to 24 [Figure 1E] Analysis results of titanium niobium composite oxides of Examples 25 to 27 [Figure 1F] Analysis results of titanium niobium composite oxides of Examples 28 to 30 [Figure 2] SEM image of the titanium niobium composite oxide of Example 3 [Figure 3] SEM image of the titanium niobium composite oxide of Comparative Example 1 [Figure 4] Volume-based logarithmic normal distribution of the major axis length (L) of the titanium niobium composite oxide of Example 3 [Figure 5] Volume-based logarithmic normal distribution of the major axis length (L) of the titanium niobium composite oxide of Comparative Example 1 [Figure 6] Volume-based logarithmic normal distribution of the aspect ratio (L / D) of the titanium niobium composite oxide of Example ⑶ [Figure 7]Volume-based log-normal distribution of aspect ratio (L / D) for titanium niobium composite oxide in Comparative Example 1 [Figure 8] Schematic diagram of a 2032 type coin cell [Modes for carrying out the invention]

[0019] The following describes embodiments of the titanium niobium composite oxide according to the present invention.

[0020] <Overview> The titanium niobium composite oxide according to the present invention contains less than 0.30 atomic percent of alkali metal elements, contains at least one of the elements Al, Y, La, Ce, Pr, and Sm, and the ratio of the total atomic weights of Al, Y, La, Ce, Pr, and Sm to the total atomic weights of Ti and Nb is 0.001 or more.

[0021] The titanium niobium composite oxide according to the present invention contains alkali metal elements, so TiO2 and Ti2Nb 10 O 29 The presence of these elements is suppressed. However, if alkali metal elements are present in amounts exceeding 0.30 atomic percent, fibrous growth of crystal grains becomes excessive, and even substitution of at least one of the elements Al, Y, La, Ce, Pr, and Sm described below will not sufficiently suppress fibrous growth of crystal grains.

[0022] The titanium-niobium composite oxide according to the present invention contains at least one of the elements Al, Y, La, Ce, Pr, and Sm, and the ratio of the total atomic weights of Al, Y, La, Ce, Pr, and Sm to the total atomic weights of Ti and Nb is 0.001 or greater. As a result, it is presumed that some of the Ti seats and some of the Nb seats in the titanium-niobium composite oxide are substituted with at least one of the elements Al, Y, La, Ce, Pr, and Sm, and it is thought that such substitution suppresses the fibrous growth of crystal grains.

[0023] However, if the ratio of the total atomic weights of Al, Y, La, Ce, Pr, and Sm to the total atomic weights of Ti and Nb exceeds 0.025, it is estimated that the total atomic weights of Al, Y, La, Ce, Pr, and Sm will exceed the substitution limits for some of the Ti and Nb seats, potentially inhibiting the reaction-promoting effect of alkali metal elements. Therefore, it is desirable that the ratio of the total atomic weights of Al, Y, La, Ce, Pr, and Sm to the total atomic weights of Ti and Nb be less than 0.025.

[0024] <Example of manufacturing method> The titanium-niobium composite oxide according to the present invention can be synthesized, for example, by a solid-phase reaction method. An example of a method for synthesizing the titanium-niobium composite oxide according to the present invention by a solid-phase reaction method is described below.

[0025] The titanium niobium composite oxide according to this embodiment is synthesized (manufactured) by a solid-phase reaction method including a mixing step and a calcination step.

[0026] In the mixing process, titanium raw materials (e.g., titanium oxide or titanium compounds that produce titanium oxide upon heating), niobium raw materials (e.g., niobium oxide or niobium compounds that produce niobium oxide upon heating), alkali metal raw materials (e.g., alkali metal carbonates), and raw materials of at least one of the following elements (e.g., alumina, yttria, lanthanum oxide, cerium oxide, praseodymium oxide, samarium oxide) are weighed to the desired content and then uniformly ground and mixed.

[0027] Furthermore, niobium raw materials containing alkali metals as impurities may be used. Similarly, titanium raw materials containing alkali metals as impurities may be used. If the necessary alkali metals can be supplied solely from the aforementioned impurities, then no additional alkali metal raw materials should be added. On the other hand, if the necessary alkali metals are insufficient from the aforementioned impurities, the amount of alkali metal raw material should be determined considering the amount of impurities.

[0028] In the mixing process, it is preferable to use grinding and mixing equipment such as a ball mill, vibratory mill, or bead mill. To prevent the mixture from adhering to the grinding and mixing equipment when using it, alcohol (e.g., ethanol) may be added to the raw materials as an auxiliary agent.

[0029] The above-mentioned auxiliary agents may also use raw materials of at least one element from aluminum, yttrium, lanthanum, cerium, praseodymium, and samarium that are soluble in the aforementioned auxiliary agents (for example, aluminum halide, yttrium halide, lanthanum halide, cerium halide, praseodymium halide, samarium halide, etc.). Furthermore, raw materials of at least one element from aluminum, yttrium, lanthanum, cerium, praseodymium, and samarium that are soluble in the above-mentioned auxiliary agents may be used together with raw materials of at least one element from aluminum, yttrium, lanthanum, cerium, praseodymium, and samarium that are not soluble in the above-mentioned auxiliary agents.

[0030] In the firing process, the mixture obtained in the mixing process is held at an appropriate temperature range for an appropriate time and fired in the atmosphere. This makes it possible to obtain a titanium-niobium composite oxide in which the primary particles are sintered.

[0031] The appropriate temperature range and time described above are values ​​that yield high-quality crystals without excessive grain growth. The appropriate temperature range is preferably 1000°C to 1300°C, more preferably 1100°C to 1200°C. The appropriate time is preferably 1 to 24 hours, more preferably 2 to 6 hours. The mixture may also be calcined in an atmosphere other than air (for example, a nitrogen atmosphere).

[0032] The following describes embodiments of the present invention in more detail, but the present invention is not limited to the embodiments described below. In other words, it goes without saying that the content can be appropriately modified without being limited in any way to the embodiments described below, as long as it is possible to apply known general techniques such as the various processing methods and granulation methods described below. [Examples]

[0033] <Example 1> 100.0 g of titanium dioxide (TiO2) powder, 355.3 g of niobium oxide (Nb2O5) powder, 0.6 g of potassium carbonate (K2CO3) powder, and 2.5 g of alumina (Al2O3) powder were mixed with ethanol as an additive and ground using a vibratory mill.

[0034] The resulting mixture was placed in an alumina crucible and calcined in an electric furnace (processing temperature: 1100°C, processing time: 2 hours) to obtain a titanium niobium composite oxide.

[0035] <Example 2> 100.0 g of titanium dioxide powder, 349.2 g of niobium oxide powder, 0.9 g of potassium carbonate powder, and 1.5 g of alumina powder were mixed with ethanol as an additive and ground using a vibrating mill.

[0036] The resulting mixture was placed in an alumina crucible and calcined in an electric furnace (processing temperature: 1100°C, processing time: 2 hours) to obtain a titanium niobium composite oxide.

[0037] <Example 3> 100.0 g of titanium dioxide powder, 359.7 g of niobium oxide powder, 1.4 g of potassium carbonate powder, and 2.4 g of alumina powder were mixed with ethanol as an additive and ground using a vibrating mill.

[0038] The resulting mixture was placed in an alumina crucible and calcined in an electric furnace (processing temperature: 1100°C, processing time: 2 hours) to obtain a titanium niobium composite oxide.

[0039] <Example 4> 100.0g of titanium dioxide powder, 348.2g of niobium oxide powder, and 1.4g of potassium carbonate powder were mixed with ethanol containing 7.6g of aluminum chloride (AlCl3) powder as an auxiliary agent, and then ground and mixed using a vibrating mill.

[0040] The resulting mixture was placed in an alumina crucible and calcined in an electric furnace (processing temperature: 1100°C, processing time: 2 hours) to obtain a titanium niobium composite oxide.

[0041] <Example 5> 100.0 g of titanium dioxide powder, 352.6 g of niobium oxide powder, 1.6 g of potassium carbonate powder, and 2.7 g of alumina powder were mixed with ethanol as an additive and ground using a vibrating mill.

[0042] The resulting mixture was placed in an alumina crucible and calcined in an electric furnace (processing temperature: 1100°C, processing time: 2 hours) to obtain a titanium niobium composite oxide.

[0043] <Example 6> 100.0 g of titanium dioxide powder, 353.9 g of niobium oxide powder, 2.4 g of potassium carbonate powder, 0.2 g of sodium carbonate (Na2CO3) powder, and 2.8 g of alumina powder were mixed with ethanol as an additive and ground using a vibrating mill.

[0044] The resulting mixture was placed in an alumina crucible and calcined in an electric furnace (processing temperature: 1100°C, processing time: 2 hours) to obtain a titanium niobium composite oxide.

[0045] <Example 7> 100.3g of titanium dioxide powder containing potassium (K) as an impurity, 340.3g of niobium oxide powder, and 1.3g of yttria (Y2O3) powder were mixed with ethanol as an additive and then pulverized using a vibratory mill.

[0046] The resulting mixture was placed in an alumina crucible and calcined in an electric furnace (processing temperature: 1100°C, processing time: 2 hours) to obtain a titanium niobium composite oxide.

[0047] <Example 8> 100.0 g of titanium dioxide powder, 341.7 g of niobium oxide powder, 0.8 g of potassium carbonate powder, 0.1 g of alumina powder, and 1.3 g of yttria powder were mixed with ethanol as an additive and ground using a vibrating mill.

[0048] The resulting mixture was placed in an alumina crucible and calcined in an electric furnace (processing temperature: 1100°C, processing time: 2 hours) to obtain a titanium niobium composite oxide.

[0049] <Example 9> 100.0 g of titanium dioxide powder, 338.1 g of niobium oxide powder, 1.3 g of potassium carbonate powder, 0.1 g of alumina powder, and 1.2 g of yttria powder were mixed with ethanol as an additive and ground using a vibrating mill.

[0050] The resulting mixture was placed in an alumina crucible and calcined in an electric furnace (processing temperature: 1100°C, processing time: 2 hours) to obtain a titanium niobium composite oxide.

[0051] <Example 10> 100.0 g of titanium dioxide powder, 343.8 g of niobium oxide powder containing potassium and sodium (Na) as impurities, 0.1 g of alumina powder, and 0.5 g of yttria powder were mixed with ethanol as an additive and ground using a vibratory mill.

[0052] The resulting mixture was placed in an alumina crucible and calcined in an electric furnace (processing temperature: 1100°C, processing time: 2 hours) to obtain a titanium niobium composite oxide.

[0053] <Example 11> 100.0g of titanium dioxide powder, 367.7g of niobium oxide powder containing potassium and sodium as impurities, 0.1g of alumina powder, and 5.0g of yttria powder were mixed with ethanol as an additive and ground using a vibrating mill.

[0054] The resulting mixture was placed in an alumina crucible and calcined in an electric furnace (processing temperature: 1100°C, processing time: 2 hours) to obtain a titanium niobium composite oxide.

[0055] <Example 12> 100.0 g of titanium dioxide powder, 341.4 g of niobium oxide powder, 0.5 g of potassium carbonate powder, and 0.1 g of alumina powder were mixed with ethanol as an additive and ground using a vibrating mill.

[0056] The resulting mixture was placed in an alumina crucible and calcined in an electric furnace (processing temperature: 1100°C, processing time: 2 hours) to obtain a titanium niobium composite oxide.

[0057] <Example 13> 100.0 g of titanium dioxide powder, 350.5 g of niobium oxide powder, 1.5 g of potassium carbonate powder, and 4.8 g of alumina powder were mixed with ethanol as an additive and ground using a vibrating mill.

[0058] The resulting mixture was placed in an alumina crucible and calcined in an electric furnace (processing temperature: 1100°C, processing time: 2 hours) to obtain a titanium niobium composite oxide.

[0059] <Example 14> 100.0 g of titanium dioxide powder, 346.9 g of niobium oxide powder, 0.8 g of potassium carbonate powder, 0.1 g of alumina powder, and 1.2 g of lanthanum oxide (La2O3) powder were mixed with ethanol as an additive and ground using a vibrating mill.

[0060] The resulting mixture was placed in an alumina crucible and calcined in an electric furnace (processing temperature: 1100°C, processing time: 2 hours) to obtain a titanium niobium composite oxide.

[0061] <Example 15> 100.0 g of titanium dioxide powder, 344.4 g of niobium oxide powder, 1.4 g of potassium carbonate powder, 0.1 g of alumina powder, and 3.6 g of lanthanum oxide powder were mixed with ethanol as an additive and ground using a vibrating mill.

[0062] The resulting mixture was placed in an alumina crucible and calcined in an electric furnace (processing temperature: 1100°C, processing time: 2 hours) to obtain a titanium niobium composite oxide.

[0063] <Example 16> 100.0 g of titanium dioxide powder, 348.3 g of niobium oxide powder, 1.8 g of potassium carbonate powder, and 7.9 g of lanthanum oxide powder were mixed with ethanol as an additive and ground using a vibrating mill.

[0064] The resulting mixture was placed in an alumina crucible and calcined in an electric furnace (processing temperature: 1100°C, processing time: 2 hours) to obtain a titanium niobium composite oxide.

[0065] <Example 17> 100.0g of titanium dioxide powder, 347.8g of niobium oxide powder, 2.1g of potassium carbonate powder, and 8.0g of lanthanum oxide powder were mixed with ethanol as an additive and ground using a vibrating mill.

[0066] The resulting mixture was placed in an alumina crucible and calcined in an electric furnace (processing temperature: 1100°C, processing time: 2 hours) to obtain a titanium niobium composite oxide.

[0067] <Example 18> 100.0g of titanium dioxide powder, 339.5g of niobium oxide powder, 1.1g of potassium carbonate powder, 0.1g of alumina powder, 0.1g of sodium carbonate powder, and 12.0g of lanthanum oxide powder were mixed with ethanol as an additive and ground using a vibrating mill.

[0068] The resulting mixture was placed in an alumina crucible and calcined in an electric furnace (processing temperature: 1100°C, processing time: 2 hours) to obtain a titanium niobium composite oxide.

[0069] <Example 19> 100.0g of titanium dioxide powder, 347.0g of niobium oxide powder, 1.1g of potassium carbonate powder, 0.1g of alumina powder, and 15.0g of lanthanum oxide powder were mixed with ethanol as an additive and ground using a vibrating mill.

[0070] The resulting mixture was placed in an alumina crucible and calcined in an electric furnace (processing temperature: 1100°C, processing time: 2 hours) to obtain a titanium niobium composite oxide.

[0071] <Example 20> 100.0g of titanium dioxide powder, 345.6g of niobium oxide powder, 0.8g of potassium carbonate powder, 0.2g of sodium carbonate powder, 1.9g of yttria powder, and 2.5g of lanthanum oxide powder were mixed with ethanol as an additive and ground using a vibrating mill.

[0072] The resulting mixture was placed in an alumina crucible and calcined in an electric furnace (processing temperature: 1100°C, processing time: 2 hours) to obtain a titanium niobium composite oxide.

[0073] <Example 21> 100.0g of titanium dioxide powder, 349.6g of niobium oxide powder, 2.7g of potassium carbonate powder, 0.5g of alumina powder, 1.6g of yttria powder, and 2.5g of lanthanum oxide powder were mixed with ethanol as an additive and ground using a vibrating mill.

[0074] The resulting mixture was placed in an alumina crucible and calcined in an electric furnace (processing temperature: 1100°C, processing time: 2 hours) to obtain a titanium niobium composite oxide.

[0075] <Example 22> 100.0g of titanium dioxide powder, 339.3g of niobium oxide powder, 1.6g of potassium carbonate powder, 0.1g of alumina powder, and 2.0g of cerium oxide (CeO2) powder were mixed with ethanol as an additive and ground using a vibratory mill.

[0076] The resulting mixture was placed in an alumina crucible and calcined in an electric furnace (processing temperature: 1100°C, processing time: 2 hours) to obtain a titanium niobium composite oxide.

[0077] <Example 23> 100.0g of titanium dioxide powder, 349.7g of niobium oxide powder, 2.0g of potassium carbonate powder, 0.1g of alumina powder, and 3.3g of cerium oxide powder were mixed with ethanol as an additive and ground using a vibrating mill.

[0078] The resulting mixture was placed in an alumina crucible and calcined in an electric furnace (processing temperature: 1100°C, processing time: 2 hours) to obtain a titanium niobium composite oxide.

[0079] <Example 24> 100.0g of titanium dioxide powder, 344.1g of niobium oxide powder, 1.0g of potassium carbonate powder, 0.1g of alumina powder, 0.2g of sodium carbonate powder, and 0.9g of cerium oxide powder were mixed with ethanol as an additive and ground using a vibrating mill.

[0080] The resulting mixture was placed in an alumina crucible and calcined in an electric furnace (processing temperature: 1100°C, processing time: 2 hours) to obtain a titanium niobium composite oxide.

[0081] <Example 25> 100.0 g of titanium dioxide powder, 343.7 g of niobium oxide powder, 2.1 g of potassium carbonate powder, and 0.5 g of praseodymium oxide (Pr2O3) powder were mixed with ethanol as an additive and ground using a vibrating mill.

[0082] The resulting mixture was placed in an alumina crucible and calcined in an electric furnace (processing temperature: 1100°C, processing time: 2 hours) to obtain a titanium niobium composite oxide.

[0083] <Example 26> 100.0g of titanium dioxide powder, 343.3g of niobium oxide powder, 1.1g of potassium carbonate powder, 0.3g of sodium carbonate powder, 0.1g of alumina powder, and 1.9g of praseodymium oxide powder were mixed with ethanol as an additive and ground using a vibrating mill.

[0084] The resulting mixture was placed in an alumina crucible and calcined in an electric furnace (processing temperature: 1100°C, processing time: 2 hours) to obtain a titanium niobium composite oxide.

[0085] <Example 27> 100.0g of titanium dioxide powder, 342.6g of niobium oxide powder, 0.9g of potassium carbonate powder, 0.3g of sodium carbonate powder, 0.1g of alumina powder, and 0.3g of praseodymium oxide powder were mixed with ethanol as an additive and ground using a vibrating mill.

[0086] The resulting mixture was placed in an alumina crucible and calcined in an electric furnace (processing temperature: 1100°C, processing time: 2 hours) to obtain a titanium niobium composite oxide.

[0087] <Example 28> 100.0g of titanium dioxide powder, 347.0g of niobium oxide powder, 1.0g of potassium carbonate powder, and 2.1g of samarium oxide (Sm2O3) powder were mixed with ethanol as an additive and ground using a vibratory mill.

[0088] The resulting mixture was placed in an alumina crucible and calcined in an electric furnace (processing temperature: 1100°C, processing time: 2 hours) to obtain a titanium niobium composite oxide.

[0089] <Example 29> 100.0g of titanium dioxide powder, 352.0g of niobium oxide powder, 1.2g of potassium carbonate powder, 0.1g of alumina powder, and 4.1g of samarium oxide powder were mixed with ethanol as an additive and ground using a vibratory mill.

[0090] The resulting mixture was placed in an alumina crucible and calcined in an electric furnace (processing temperature: 1100°C, processing time: 2 hours) to obtain a titanium niobium composite oxide.

[0091] <Example 30> 100.0 g of titanium dioxide powder, 346.8 g of niobium oxide powder, 2.0 g of potassium carbonate powder, and 10.9 g of samarium oxide powder were mixed with ethanol as an additive and then ground and mixed using a vibrating mill.

[0092] The resulting mixture was placed in an alumina crucible and calcined in an electric furnace (processing temperature: 1100°C, processing time: 2 hours) to obtain a titanium niobium composite oxide.

[0093] <Comparative Example 1> 100.0 g of titanium dioxide powder, 344.4 g of niobium oxide powder, 1.5 g of potassium carbonate powder, and 0.1 g of alumina powder were mixed with ethanol as an additive and ground using a vibrating mill.

[0094] The resulting mixture was placed in an alumina crucible and calcined in an electric furnace (processing temperature: 1100°C, processing time: 2 hours) to obtain a titanium niobium composite oxide.

[0095] <Comparative Example 2> 100.0 g of titanium dioxide powder, 342.4 g of niobium oxide powder, 2.9 g of potassium carbonate powder, and 5.3 g of alumina powder were mixed with ethanol as an additive and ground using a vibrating mill.

[0096] The resulting mixture was placed in an alumina crucible and calcined in an electric furnace (processing temperature: 1100°C, processing time: 2 hours) to obtain a titanium niobium composite oxide.

[0097] <Comparative Example 3> 100.0g of titanium dioxide powder, 332.4g of niobium oxide powder, 2.7g of potassium carbonate powder, 0.4g of alumina powder, and 4.3g of yttria powder were mixed with ethanol as an additive and ground using a vibrating mill.

[0098] The resulting mixture was placed in an alumina crucible and calcined in an electric furnace (processing temperature: 1100°C, processing time: 2 hours) to obtain a titanium niobium composite oxide.

[0099] <Analyzer> The analytical instruments used for the analysis of the titanium niobium composite oxides in Examples 1-30 and Comparative Examples 1-3 are as follows. X-ray diffractometer: Rigaku Corporation, Ultima4, measurement using Cu-Kα rays X-ray fluorescence analyzer: Rigaku Corporation, ZSX PrimusIII+ Scanning electron microscope: JEOL Ltd., JSM-6510

[0100] <Analysis results> Figure 1A shows the analysis results of the titanium niobium composite oxides from Examples 1-13 and Comparative Examples 1-3. Figure 1B shows the analysis results of the titanium niobium composite oxides from Examples 14-19. Figure 1C shows the analysis results of the titanium niobium composite oxides from Examples 20-21. Figure 1D shows the analysis results of the titanium niobium composite oxides from Examples 22-24. Figure 1E shows the analysis results of the titanium niobium composite oxides from Examples 25-27. Figure 1F shows the analysis results of the titanium niobium composite oxides from Examples 28-30. Note that "0.000" in Figures 1A-1F is a value obtained by rounding to the fourth decimal place, and therefore does not mean a perfect zero. Furthermore, in Examples 7, 11, and 14-30, there were no primary particles with a major axis length (L) of 3 μm or more among the 100 measurements. However, it cannot be definitively stated that there are absolutely no primary particles with a major axis length (L) of 3 μm or more in the population. Rather, it can only be said that, based on the normal distribution, the probability of primary particles with a major axis length (L) of 3 μm or more is close to zero. In other words, the "0.0%" in Figures 1A-1F does not mean exactly zero.

[0101] The atomic percentages of Ti, Nb, K, Na, total alkali metals, Al, Y, La, Ce, Pr, and Sm in each titanium-niobium composite oxide were determined from the results of X-ray fluorescence analysis. The atomic weight ratios of each titanium-niobium composite oxide, namely Al / (Ti+Nb), Y / (Ti+Nb), La / (Ti+Nb), Ce / (Ti+Nb), Pr / (Ti+Nb), Sm / (Ti+Nb), and (Al+Y+La+Ce+Pr+Sm) / (Ti+Nb), were determined from the atomic percentages mentioned above.

[0102] The shape of the primary particles of each titanium-niobium composite oxide was determined from observations using a scanning electron microscope. Examples of SEM images of the titanium-niobium composite oxides are shown in Figures 2 and 3. Figure 2 is an SEM image of the titanium-niobium composite oxide of Example 3, and Figure 3 is an SEM image of the titanium-niobium composite oxide of Comparative Example 1.

[0103] SEM images (20,000x magnification) of each titanium-niobium composite oxide were scanned laterally, and the long axis length (L) and short axis length (D) of 100 primary particles located on a line parallel to the horizontal direction were measured sequentially for each titanium-niobium composite oxide. During the measurement, the magnification was changed up to a maximum of 40,000x depending on the size of the primary particles, and the angle of the sample stage was changed according to the orientation of the primary particles.

[0104] Assuming the primary particle's shape is cylindrical, the volume of each primary particle was determined by measuring its major axis length (L) and minor axis length (D). Specifically, the major axis length (L) was considered the height of the cylinder, and the minor axis length (D) was considered the diameter of the cylinder.

[0105] Then, using the volume of the primary particles as the basis rather than the number of primary particles, the distribution of the major axis length (L) of the population (the entire titanium-niobium composite oxide) was estimated from the measured values ​​of 100 primary particles. Examples of the estimation results of the volume-based log-normal distribution of major axis length (L) for titanium-niobium composite oxide are shown in Figures 4 and 5. Figure 4 is the volume-based log-normal distribution of major axis length (L) for titanium-niobium composite oxide in Example 3, and Figure 5 is the volume-based log-normal distribution of major axis length (L) for titanium-niobium composite oxide in Comparative Example 1. Figures 1A to 1F show the volume-based percentage of primary particles with a major axis length (L) of 3 μm or more.

[0106] Furthermore, instead of using the number of primary particles as the basis, the volume of the primary particles was used as the basis to estimate the distribution of the aspect ratio (L / D) of the population (the entire titanium-niobium composite oxide) from the measured values ​​of 100 primary particles. Examples of volume-based log-normal distributions of aspect ratio (L / D) for titanium-niobium composite oxides are shown in Figures 6 and 7. Figure 6 is the volume-based log-normal distribution of aspect ratio (L / D) for titanium-niobium composite oxides in Example 3, and Figure 7 is the volume-based log-normal distribution of aspect ratio (L / D) for titanium-niobium composite oxides in Comparative Example 1. Figures 1A to 1F show the volume-based proportion of primary particles with an aspect ratio (L / D) of 3 or more.

[0107] In the analysis method described above, the shape of the primary particles was assumed to be cylindrical, but the same estimation results can be obtained even if the shape of the primary particles is assumed to be a rectangular prism with a square base.

[0108] Figures 1A to 1F show the intensity (relative value) of peaks in the X-ray diffraction spectra of each titanium niobium composite oxide in Examples 1 to 30 and Comparative Examples 1 to 3, where peaks exist in the diffraction angle 2θ ranges of 26.2° to 26.4°, 24.8° to 25.1°, and 27.2° to 27.6°, respectively. The peaks in the diffraction angle 2θ range of 26.2° to 26.4° are due to the crystal structure of the target product, TiNb2O7. The peaks in the diffraction angle 2θ range of 24.8° to 25.1° are due to Ti2Nb 10 O 29 These peaks are due to the crystal structure. Peaks with diffraction angles 2θ in the range of 27.2° to 27.6° are due to the rutile-type TiO2 crystal structure.

[0109] Furthermore, Figures 1A to 1F show, as percentages, the ratio of the peak intensity in the diffraction angle 2θ range of 24.8° to 25.1° to the peak intensity in the diffraction angle 2θ range of 26.2° to 26.4°, and the ratio of the peak intensity in the diffraction angle 2θ range of 27.2° to 27.6° to the peak intensity in the diffraction angle 2θ range of 26.2° to 26.4°.

[0110] Furthermore, Figures 1A to 1F also show the full width at half maximum (FMAX) of peaks in the diffraction angle 2θ range of 26.2° to 26.4°. The smaller the FMAX of peaks in the diffraction angle 2θ range of 26.2° to 26.4°, the higher the quality of the desired product, TiNb2O7 crystals.

[0111] In each of the titanium-niobium composite oxides in Examples 1 to 30, the volume-based proportion of primary particles with an aspect ratio (L / D) of 3 or more is 11% by volume or less, more precisely 10.8% by volume or less. On the other hand, in each of the titanium-niobium composite oxides in Comparative Examples 1 to 30, the volume-based proportion of primary particles with an aspect ratio (L / D) of 3 or more is 16% by volume or more, more precisely 16.7% or more. In other words, the fibrous grain growth of primary particles is suppressed in each of the titanium-niobium composite oxides in Examples 1 to 30 compared to each of the titanium-niobium composite oxides in Comparative Examples 1 to 3.

[0112] Each of the titanium-niobium composite oxides in Examples 1 to 30 contains less than 0.30 atomic percent of alkali metal elements, contains at least one of the elements Al, Y, La, Ce, Pr, and Sm, and has a composition in which the ratio of the total atomic weights of Al, Y, La, Ce, Pr, and Sm to the total atomic weights of Ti and Nb is 0.001 or more. In contrast, the titanium-niobium composite oxides in Comparative Examples 1 to 3 do not have such a composition. It is preferable that the alkali metal element content is between 0.05 atomic percent and 0.28 atomic percent.

[0113] The titanium-niobium composite oxide of Comparative Example 1 has a ratio of the total atomic weights of Al, Y, La, Ce, Pr, and Sm to the total atomic weights of Ti and Nb that is too small, which is why the fibrous grain growth of primary particles is not sufficiently suppressed. As a result, it is thought to have a tendency for the aspect ratio (L / D) of primary particles to be larger than that of the titanium-niobium composite oxides of Examples 1 to 30. The titanium-niobium composite oxides of Comparative Examples 2 and 3 have an excessive amount of alkali metal elements, which is why the fibrous grain growth of primary particles is not sufficiently suppressed. As a result, it is thought to have a tendency for the aspect ratio (L / D) of primary particles to be larger than that of the titanium-niobium composite oxides of Examples 1 to 30.

[0114] In each of the titanium-niobium composite oxides in Examples 1-11 and 13-30, the volume-based proportion of primary particles with a long axis length (L) of 3 μm or more is 5 volume% or less, more precisely 4.0 volume% or less. On the other hand, in the titanium-niobium composite oxide of Example 12, the volume-based proportion of primary particles with a long axis length (L) of 3 μm or more is 10 volume% or more, more precisely 10.8 volume% or more. In other words, the growth of primary particles is suppressed in each of the titanium-niobium composite oxides in Examples 1-11 and 13-30 compared to the titanium-niobium composite oxide of Example 12.

[0115] While the titanium-niobium composite oxides in Examples 1-11 and 13-30 have a composition in which the ratio of the total atomic weights of Al, Y, La, Ce, Pr, and Sm to the total atomic weights of Ti and Nb is 0.002 or higher, the titanium-niobium composite oxide of Example 12 does not have such a composition.

[0116] Each of the titanium-niobium composite oxides in Examples 1-11 and 13-30 has a larger ratio of the total atomic weights of Al, Y, La, Ce, Pr, and Sm to the total atomic weights of Ti and Nb than the titanium-niobium composite oxide in Example 12. Therefore, it is thought that the growth of primary particles can be suppressed more effectively than in the titanium-niobium composite oxide in Example 12, and as a result, the primary particles tend to have a smaller major axis length (L) than the titanium-niobium composite oxide in Example 12.

[0117] In the titanium-niobium composite oxides of Examples 1-11, 14-17, and 20-30, the ratio of the peak intensity in the diffraction angle 2θ range of 27.2°-27.6° to the peak intensity in the diffraction angle 2θ range of 26.2°-26.4° is 7% or less, more precisely 6.8% or less. On the other hand, in the titanium-niobium composite oxides of Examples 13, 18, and 19, the ratio of the peak intensity in the diffraction angle 2θ range of 27.2°-27.6° to the peak intensity in the diffraction angle 2θ range of 26.2°-26.4° is 8% or more, more precisely 8.5% or more. In other words, the titanium-niobium composite oxides of Examples 1-11, 14-17, and 20-30 have suppressed TiO2 inclusion compared to the titanium-niobium composite oxides of Examples 13, 18, and 19.

[0118] The titanium niobium composite oxides in Examples 1-11, 14-17, and 20-30 have a configuration in which the ratio of the total atomic weights of Al, Y, La, Ce, Pr, and Sm to the total atomic weights of Ti and Nb is less than 0.020, whereas the titanium niobium composite oxides in Examples 13, 18, and 19 do not have such a configuration. It is preferable that the ratio of the total atomic weights of Al, Y, La, Ce, Pr, and Sm to the total atomic weights of Ti and Nb is less than 0.020, and more precisely, 0.018 or less.

[0119] Unlike the titanium niobium composite oxides in Examples 1-11, 14-17, and 20-30, the titanium niobium composite oxides in Examples 13, 18, and 19 have a less excessive ratio of the total atomic weights of Al, Y, La, Ce, Pr, and Sm to the total atomic weights of Ti and Nb. Therefore, it is believed that they can suppress the presence of TiO2 more effectively than the titanium niobium composite oxides in Examples 13, 18, and 19.

[0120] In Examples 7 to 11, the titanium-niobium composite oxides have a configuration in which the ratio of the total atomic weight of Y to the total atomic weight of Ti and Nb is between 0.001 and 0.011, whereas the titanium-niobium composite oxide of Example 13 does not have such a configuration.

[0121] Each of the titanium-niobium composite oxides in Examples 7 to 11 has a moderate Y content and the ratio of the total atomic weight of Y to the total atomic weight of Ti and Nb is within an appropriate range. Therefore, it is considered that they can suppress the presence of TiO2 more effectively than the titanium-niobium composite oxide in Example 13, which has a high Al content.

[0122] <Applications to lithium-ion secondary batteries> For example, electrodes can be prepared using any of the titanium niobium composite oxides from Examples 1 to 30 as the active material. Specifically, 10 parts by weight of polyvinylidene fluoride can be dissolved in N-methyl-2-pyrrolidone, then 10 parts by weight of conductive carbon and 100 parts by weight of any of the titanium niobium composite oxides from Examples 1 to 13 can be added as conductive additives, and the mixture can be kneaded in a rotary-orbiting agitator to create a coating. This coating can then be applied to aluminum foil, vacuum-dried at 120°C, pressed, and then punched out in a circular shape.

[0123] Using the electrodes fabricated as described above, a 2032-type coin cell 1, as shown in Figure 8, can be assembled. The 2032-type coin cell 1 shown in Figure 8 is an example of a lithium-ion secondary battery. The 2032-type coin cell 1 is fabricated by sandwiching the electrode 2, counter electrode 3, non-aqueous electrolyte 4, and separator 5 between the upper case 6a and the lower case 6b, and sealing the perimeter of the upper case 6a and the lower case 6b with a gasket 7.

[0124] For the counter electrode 3, for example, metallic lithium foil may be used. For the non-aqueous electrolyte 4, for example, a solution of ethylene carbonate:dimethyl carbonate 1:1 v / v% with 1 mol / L of LiPF6 dissolved in it may be used. For the separator 5, for example, a porous polypropylene membrane may be used.

[0125] Furthermore, an electrode in which at least a portion of the electrode active material is the titanium-niobium composite oxide according to the present invention may be used as the positive electrode of a lithium-ion secondary battery, or as the negative electrode of a lithium-ion secondary battery.

[0126] <Other> Although embodiments of the present invention have been described above, the configuration of the present invention is not limited thereto, and various modifications can be made without departing from the spirit of the invention. That is, the above embodiments should be considered in all respects to be illustrative and not restrictive, and the technical scope of the present invention is indicated by the claims and should be understood to include all modifications that fall within the meaning and scope equivalent to the claims.

[0127] For example, in the above-described examples, the alkali metal elements contained in the titanium niobium composite oxide were K and Na, but other alkali metal elements such as Li may also be included. Other alkali metal elements such as Li may be included in the titanium niobium composite oxide that does not contain K and Na, may be included in the titanium niobium composite oxide together with K, or may be included in the titanium niobium composite oxide together with Na. Furthermore, comparing Example 18 and Example 19, if there is no significant difference in the content of alkali metal elements between the configuration with one type of alkali metal element and the configuration with two types of alkali metal elements, and there is no significant difference in the ratio of the total atomic weights of Al, Y, La, Ce, Pr, and Sm to the total atomic weights of Ti and Nb, then TiO2 and Ti2Nb 10 O 29 It is considered that the effect of suppressing the mixing and grain growth is of a similar degree. Therefore, for example, if the amount of alkali metal elements is kept approximately the same for each of Examples 1 to 30, and the ratio of the total atomic weights of Al, Y, La, Ce, Pr, and Sm to the total atomic weights of Ti and Nb is kept the same, but the number of types of alkali metal elements is changed, then compared to each of Examples 1 to 30, TiO2 and Ti2Nb 10 O 29 The effects of suppressing the presence of these substances and the growth of crystal grains are considered to be of similar magnitude.

[0128] For example, in the above-described embodiment, a portion of the surface of the titanium-niobium composite oxide was not coated with a carbon material, but a portion of the surface of the titanium-niobium composite oxide may be coated with a carbon material.

[0129] Here, we will describe an example of a method for producing a titanium-niobium composite oxide in which a portion of the surface is coated with a carbon material. For example, after adding an aqueous solution of polyvinyl alcohol (PVA) to any of the titanium-niobium composite oxides from Examples 1 to 30 so that the PVA content is 13% by weight, the mixture is crushed and mixed using a ball mill, and then dried with a spray dryer. After that, the resulting dried product is heat-treated under a nitrogen atmosphere (treatment temperature: 800°C, treatment time: 4 hours). This makes it possible to obtain a titanium-niobium composite oxide in which a portion of the surface is coated with a carbon material. [Industrial applicability]

[0130] The titanium-niobium composite oxide according to the present invention can be used, for example, as an electrode active material used in the electrodes of lithium-ion secondary batteries. [Explanation of Symbols]

[0131] 1. 2032 type coin cell 2 electrodes 3. Opposite 4. Non-aqueous electrolytes 5 Separators 6a Upper case 6b Lower case 7 Gasket

Claims

1. Contains an alkali metal element in an amount of 0.05 atomic % or more and less than 0.30 atomic %; At least one element of Al, Y, La, Ce, Pr, and Sm is included; Contains the elements Ti, Nb, and O, The remainder is impurities, The ratio of the total atomic percentage of Al, Y, La, Ce, Pr, and Sm to the total atomic percentage of Ti and Nb is 0.025 or less; When the aspect ratio, which is the ratio of the long axis length to the short axis length of a primary particle of the titanium-niobium composite oxide, is expressed as a volume-based log-normal distribution, the proportion of the primary particles having an aspect ratio of more than 3 is 11 volume % or less. Titanium niobium composite oxide for electrode active materials.

2. When the major axis length of the primary particles of the titanium-niobium composite oxide is expressed as a volume-based log-normal distribution, the proportion of the primary particles having a major axis length of more than 3 μm is 10.8 vol.% or less. The titanium-niobium composite oxide for use as an electrode active material according to claim 1 .

3. In the X-ray diffraction spectrum of the niobium titanate composite oxide, a ratio of a peak intensity in the diffraction angle 2θ range of 27.2° to 27.6° to a peak intensity in the diffraction angle 2θ range of 26.2° to 26.4° is 8.7% or less, and a ratio of a peak intensity in the diffraction angle 2θ range of 24.8° to 25.1° to a peak intensity in the diffraction angle 2θ range of 26.2° to 26.4° is 9.9% or less. The titanium-niobium composite oxide for electrode active material according to claim 1 or 2.

4. A portion of the surface of the titanium-niobium composite oxide is coated with a carbon material. The titanium-niobium composite oxide for electrode active material according to any one of claims 1 to 3.

5. An electrode comprising an active material, At least a part of the electrode active material is the titanium-niobium composite oxide according to any one of claims 1 to 4. electrode.

6. A battery comprising a positive electrode and a negative electrode, Either the positive electrode or the negative electrode is the electrode according to claim 5. Lithium-ion secondary battery.