Nonwoven fabric with high heat resistance and barrier properties

JP2023502109A5Active Publication Date: 2024-10-18BERRY GLOBAL INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2022528631
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-11-18
Filing Date
2020-11-10
Publication Date
2024-10-18
Estimated Expiration
2040-11-10

AI Technical Summary

Technical Problem

Medical grade papers and nonwovens like Tyvek® face challenges with steam sterilization due to low melting points, leading to the need for chemical sterilization, and exhibit higher particle lint, lower tear strength, and lower breathability compared to nonwovens.

Method used

A nonwoven fabric with outer spunbond layers and meltblown or melt-fibrillated layers in between, where the outer layers are thermally bonded and compressed to form a microporous film, allowing steam sterilization while maintaining breathability and barrier properties.

Benefits of technology

The nonwoven fabric enables steam sterilization without chemical agents, while providing improved barrier properties and breathability, with reduced lint and enhanced tear strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

A nonwoven fabric includes a first outermost spunbond layer, a second outermost spunbond layer, and at least a first meltblown and / or melt fibrillated layer disposed directly or indirectly between the first and second outermost spunbond layers. The first outermost spunbond layer includes a first plurality of continuous fibers that are heat fused and compressed to each other to define a microporous film on the outermost surface of the nonwoven fabric. The first plurality of continuous fibers includes a first polymer composition having a first melting point, and the first meltblown and / or melt fibrillated layer includes a first plurality of meltblown and / or melt fibrillated fibers that include a third polymer composition having a third melting point, the first melting point being lower than the third melting point.
Need to check novelty before this filing date? Find Prior Art

Description

Content of disclosure

[0001] [Cross-reference to related applications] This application claims priority under 35 U.S.C. § 119(e) to U.S. Provisional Application No. 62 / 936,826, filed on 18 November 2019, which is expressly incorporated herein by reference in its entirety.

[0002] [Technical Field] The embodiments of the invention disclosed generally relate to nonwoven fabrics having generally an outer spunbond layer and one or more meltblown and / or molten fibrillated layers located between the outer spunbond layers, the nonwoven fabrics may be suitable for use as permeable barrier materials in sterilizable and / or serializable packages.

[0003] 〔background〕 Medical packaging materials currently include medical-grade paper and nonwoven fabrics. One such nonwoven fabric is Tyvek®, which is made from flash-spun high-density polyethylene (HDPE) fibers. Medical-grade paper can be steam-sterilized (e.g., at a temperature of about 134°C for about 6 minutes). Steam sterilization is often considered the most convenient and chemical-free sterilization method. However, medical-grade paper often exhibits higher particle lint, lower tear strength, lower air permeability, and lower wet strength compared to nonwoven fabrics like Tyvek®. For example, Tyvek® offers a lower lint and higher air permeability alternative to medical-grade paper. However, Tyvek® cannot be steam-sterilized due to the low melting point of HDPE. In this respect, sterilization using Tyvek® must rely on chemical sterilization, such as ethylene oxide in hydrogen peroxide plasma sterilization.

[0004] Therefore, there remains a need in this field for nonwoven fabrics that can be used in various packaging applications and various sterilization modalities.

[0005] 〔overview〕 One or more embodiments of the present invention can address one or more of the aforementioned problems. A particular embodiment of the present invention provides a nonwoven fabric comprising a first outermost spunbond layer comprising a first plurality of continuous fibers, the first plurality of continuous fibers being thermally fused and compressed with respect to one another to define a microporous film on the outermost surface of the nonwoven fabric (for example, the first plurality of continuous fibers being softened and at least partially flowing to form a microporous film structure). The first plurality of continuous fibers comprises a first polymer composition having a first melting point. The nonwoven fabric also comprises a second outermost spunbond layer comprising a second plurality of continuous fibers. According to a particular embodiment of the present invention, the nonwoven fabric may also comprise at least a first meltblown layer and / or molten fibrillated layer comprising a first plurality of meltblown fibers and / or molten fibrillated fibers located directly or indirectly between the first outermost spunbond layer and the second outermost spunbond layer. The first plurality of meltblown fibers and / or molten fibrillated fibers comprise a third polymer composition having a third melting point, the first melting point being lower than the third melting point.

[0006] In another embodiment, the present invention provides a method for forming a nonwoven fabric. According to a particular embodiment of the present invention, the method is The method may include providing or forming a first outermost spunbond layer comprising a first plurality of continuous fibers, wherein the first plurality of continuous fibers comprises a first polymer composition having a first melting point. The method may further include depositing at least a first meltblown layer and / or molten fibrillated layer comprising a first plurality of meltblown fibers and / or molten fibrillated fibers located directly or indirectly on the first outermost spunbond layer, wherein the first plurality of meltblown fibers and / or molten fibrillated fibers comprises a third polymer composition having a third melting point higher than the first melting point. According to a particular embodiment of the present invention, the method is The method may also include providing or forming a second outermost spunbond layer containing a second plurality of continuous fibers directly or indirectly on a first meltblown layer and / or molten fibrillated layer forming a precursor web, the first meltblown layer and / or molten fibrillated layer being located directly or indirectly between the first outermost spunbond layer and the second outermost spunbond layer. The method may also include calendering the first outermost spunbond layer of the precursor web to compress the first plurality of continuous fibers relative to each other, forming a substantially smooth outer surface in the form of a microporous film that allows water vapor to pass through and also functions as a barrier against bacteriological contamination.

[0007] In another embodiment, the present invention provides a package. According to a particular embodiment of the present invention, the package may include a sealed or sealable container having an interior defined at least partially by a container wall, where at least a portion of the sealed or sealable container includes a breathable material such as a nonwoven fabric as described and disclosed herein, through which a sterilization gas such as ethylene oxide, hydrogen peroxide plasma, or vapor can enter and exit the interior of the sealed or sealable container.

[0008] In yet another aspect, the Disclosure provides a method for sterilizing a package, the method comprising (i) providing a package as disclosed and described herein, (ii) placing the package in an air chamber, (iii) removing air from the air chamber and the package, (iv) filling the air chamber and the package with a sterilizing gas, (v) retaining the sterilizing gas in the air chamber and the package for a predetermined period of time, and (vi) removing the sterilizing gas.

[0009] The present invention will be described in more detail below with reference to the accompanying drawings. While the accompanying drawings show some embodiments of the present invention, not all embodiments are shown. In fact, the present invention can be carried out in many different forms and should not be construed as being limited to the embodiments described herein. Rather, these embodiments are provided to satisfy the legal requirements to which this disclosure is applicable. Similar reference numerals refer to similar elements throughout. [Brief explanation of the drawing]

[0010] [Figure 1] This shows a nonwoven fabric according to a specific embodiment of the present invention. [Figure 2] This shows a magnified cross-sectional image of a nonwoven fabric according to a specific embodiment of the present invention. [Figure 3] This diagram shows a schematic representation of a method for manufacturing a nonwoven fabric according to a specific embodiment of the present invention.

[0011] [Detailed explanation] The present invention will be described in more detail below with reference to the accompanying drawings. The accompanying drawings show some embodiments of the present invention, but not all embodiments. In fact, the present invention can be carried out in many different forms and should not be construed as being limited to the embodiments described herein. Rather, these embodiments are provided to satisfy the legal requirements to which this disclosure is applicable. As used herein and in the accompanying claims, the singular forms “a,” “an,” and “the” include plural nouns unless explicitly specified otherwise in the context.

[0012] The disclosed invention generally relates to nonwoven fabrics comprising an outermost spunbond layer and one or more meltblown and / or molten fibrillated layers located between the outer spunbond layers, and the nonwoven fabric may be suitable for use as a permeable barrier material in sterile and / or serializable packages. According to certain embodiments of the invention, the nonwoven fabric may include a plurality of meltblown and / or molten fibrillated layers located directly or indirectly between two outermost spunbond layers. According to certain embodiments of the invention, the nonwoven fabric may include a plurality of meltblown and / or molten fibrillated layers having finer fibers than the outermost spunbond layers. According to certain embodiments of the invention, the meltblown and / or molten fibrillated layers may be formed from a polymer composition having a significantly higher melt flow rate (MFR) compared to that used to form the outermost spunbond layers. According to certain embodiments of the invention, the melting point of one or both of the outermost spunbond layers is lower than that of the meltblown and / or molten fibrillated layers, as described below. In this regard, one or both of the outermost spunbond layers can be melted (e.g., softened and flowed by a smoothing calendering operation) to form a microporous film structure on at least one of the outermost surfaces of the nonwoven fabric, preferably without melting (e.g., softening and flowing) the fibers of the meltblown layer and / or molten fibrillated layer. In this regard, the nonwoven fabric can provide barrier properties while maintaining vapor permeability.

[0013] The terms “substantial” or “substantially” may, according to certain embodiments of the Invention, encompass the entire specified amount, or, according to other embodiments of the Invention, encompass a majority of the specified amount (e.g., 95%, 96%, 97%, 98%, or 99% of the specified total amount).

[0014] As used interchangeably herein, the terms “polymer” or “polymeric” may include homopolymers, copolymers, e.g., block, graft, random, and alternating copolymers, terpolymers, and blends and modifications thereof. Furthermore, unless otherwise specified, the terms “polymer” or “polymeric” shall include all possible structural isomers; including but not limited to geometric isomers, optical isomers, or stereoisomers; and / or any chiral molecular form of such polymer or polymeric material. These configurations include, but are not limited to, isotactic, syndiotactic, and atactic configurations of such polymer or polymeric material. The terms “polymer” or “polymeric” shall also include polymers produced from various catalyst systems, including, but not limited to, Ziegler-Natta catalyst systems and metallocene / single-site catalyst systems. The terms “polymer” or “polymeric” shall also include, according to certain embodiments of the present invention, biosourced polymers produced by fermentation processes or of bio-derived origin.

[0015] As used herein, the terms “nonwoven fabric” and “nonwoven web” may include a web having a structure of individual fibers, filaments, and / or yarns interspersed between them, but not in a repetitive manner that is identifiable like a knitted or woven fabric. A nonwoven fabric or web may be formed by any process conventionally known in the art, such as, for example, melt-blown processes, spunbond processes, needle punching, water-flow entanglement, air-laid, and bonded-carded web processes, according to certain embodiments of the present invention. As used herein, a “nonwoven web” may include a plurality of individual fibers that have not been subjected to an integration process.

[0016] As used herein, the term “layer” may include a generally recognizable combination of similar material types and / or functions existing in the XY plane.

[0017] As used herein, the term "multicomponent fiber" can include fibers formed from at least two different polymer materials or compositions (e.g., two or more) that are extruded from separate extruders but are spun together to form one fiber. As used herein, the term "bicomponent fiber" can include fibers formed from two different polymer materials or compositions that are extruded from separate extruders but are spun together to form one fiber. The polymer materials or polymers are disposed in substantially constant positions in distinct zones across the cross-section of the multicomponent fiber and extend continuously along the length of the multicomponent fiber. Such configurations of multicomponent fibers can be, for example, sheath / core arrangements where one polymer is surrounded by another polymer, eccentric sheath / core arrangements, side-by-side arrangements, pie arrangements, or "sea-island" arrangements, as are each known in the art of multicomponent fibers including bicomponent fibers.

[0018] As used herein, the term "machine direction" or "MD" includes the direction in which the fabric is manufactured or conveyed. As used herein, the term "cross direction" or "CD" includes the direction of the fabric that is substantially perpendicular to the MD.

[0019] As used herein, the term "continuous fiber" refers to fibers that are not cut from their original length prior to being formed into a nonwoven web or fabric. Continuous fibers can range from greater than about 15 centimeters to greater than 1 meter and can have an average length up to the length of the web or fabric being formed. For example, continuous fibers as used herein can include fibers where the length of the fiber is at least 1,000 times greater than the average diameter of the fiber, such as where the length of the fiber is at least about 5,000, 10,000, 50,000, or 100,000 times greater than the average diameter of the fiber.

[0020] As used herein, the term "aspect ratio" includes the ratio of the length of the long axis to the length of the short axis of the cross-section of the fiber in question.

[0021] As used herein, the term "spunbond" can include fibers formed by extruding a molten thermoplastic material as filaments from a plurality of fine, usually circular, capillaries of a spinneret and then rapidly reducing the diameter of the extruded filaments. According to one embodiment of the present invention, spunbond fibers are generally not tacky when deposited on a collecting surface and may be generally continuous as disclosed and described herein. It should be noted that the spunbond used in certain composites of the present invention may include nonwoven fabrics described in the literature as SPINLACE®.

[0022] As used herein, the term "meltblown" can include fibers formed, according to certain embodiments of the present invention, by extruding a molten thermoplastic material as a melt stream or filaments through a plurality of fine die capillaries into a converging, high velocity, and usually hot gas (e.g., air) stream that can narrow and reduce their diameters to microfiber diameters. According to one embodiment of the present invention, the die capillaries may be circular. Thereafter, the meltblown fibers are carried by the high velocity gas stream and deposited on a collecting surface to form a web of randomly disbursed meltblown fibers. The meltblown fibers may be continuous or discontinuous and may include microfibers that are generally tacky when deposited on a collecting surface. However, meltblown fibers are shorter in length than spunbond fibers.

[0023] As used herein, the term “melt fibrillation” can include a general class of fiber manufacturing, in which one or more polymers are melted and extruded into many possible configurations (e.g., co-extrusion, homogeneous or binary film or filament), and then fibrillated or fiberized into a plurality of individual filaments for the formation of melt fibrillated fibers. Non-limiting examples of melt fibrillation methods may include meltblown, melt fiber bursting, and melt film fibrillation. As used herein, the term “melt film fibrillation” can include a method of producing a melt film from a melt, and then using a fluid to form fibers (e.g., melt film fibrillated fibers) from the melt film. Examples include U.S. Patents 6,315,806, 5,183,670, 4,536,361, 6,382,526, 6,520,425, and 6,695,992, the contents of which are incorporated herein by reference to the extent that such disclosures are consistent with this disclosure. Further examples include U.S. Patents 7,628,941, 7,722,347, 7,666,343, 7,931,457, 8,512,626, and 8,962,501, which describe the Arium® melt film fibrillation process and the melt film fibrillated fibers formed thereby, the contents of which are incorporated herein by reference to the extent that such disclosures are consistent with this disclosure.

[0024] All integer endpoints disclosed herein that can produce smaller ranges within a given range disclosed herein are within the scope of specific embodiments of the invention. For example, the disclosure of about 10 to about 15 includes intermediate range disclosures such as about 10 to about 11; about 10 to about 12; about 13 to about 15; about 14 to about 15. Furthermore, all single decimal endpoints (e.g., numbers reported to one decimal place) that can produce smaller ranges within a given range disclosed herein are within the scope of specific embodiments of the invention. For example, the disclosure of about 1.5 to about 2.0 includes intermediate range disclosures such as about 1.5 to about 1.6; about 1.5 to about 1.7; about 1.7 to about 1.8.

[0025] In one embodiment, the present invention provides a nonwoven fabric comprising a first outermost spunbond layer comprising a first plurality of continuous fibers, the first plurality of continuous fibers being thermally fused and compressed with respect to one another to define a microporous film on the outermost surface of the nonwoven fabric (for example, the first plurality of continuous fibers being softened and at least partially flowing to form a microporous film structure). The first plurality of continuous fibers comprises a first polymer composition having a first melting point. The nonwoven fabric also comprises a second outermost spunbond layer comprising a second plurality of continuous fibers. According to a particular embodiment of the present invention, the nonwoven fabric may also comprise at least a first meltblown layer and / or molten fibrillated layer comprising a first plurality of meltblown fibers and / or molten fibrillated fibers located directly or indirectly between the first outermost spunbond layer and the second outermost spunbond layer. The first plurality of meltblown fibers and / or molten fibrillated fibers comprise a third polymer composition having a third melting point, the first melting point being lower than the third melting point. According to a particular embodiment of the present invention, a microporous film structure can be formed by at least partial softening and flow of the first plurality of continuous fibers to form a microporous film structure that allows water vapor to permeate the nonwoven fabric while at least partially preventing penetration of the nonwoven fabric by polar liquids and / or microorganisms. The microporous film structure can be defined by at least partial melting and flow of at least a portion of the first plurality of continuous fibers on at least one of the outermost surfaces of the nonwoven fabric, for example, via thermal area bonding. According to a particular embodiment of the present invention, for example, the first polymer composition of the first plurality of continuous fibers softens and flows to form a microporous film on at least one of the outermost surfaces of the nonwoven fabric. In this regard, a particular embodiment of the present invention provides a breathable material in the form of a nonwoven fabric (e.g., a breathable barrier material).

[0026] According to certain embodiments of the present invention, the first melting point of the first polymer composition is at least about 1°C to about 30°C lower than the third melting point of the third polymer composition, for example, at most about 30°C, 25°C, 20°C, 15°C, or 10°C lower than the third melting point, and / or at least about 1°C, 2°C, 3°C, 4°C, 5°C, 6°C, 7°C, 8°C, 9°C, or 10°C lower than the third melting point. In this regard, for example, one or both of the outermost spunbond layers can be at least partially softened and flowed to form a microporous film on one or both of the outermost surfaces of the nonwoven fabric, while at least the first meltblown layer and / or molten fibrillated layer formed from the third polymer composition does not soften and flow. In this regard, at least the first meltblown layer and / or molten fibrillated layer formed from the third polymer composition substantially retains their cross-sectional shape (e.g., substantially circular). In particular embodiments of the present invention, the outermost spunbond layer can be melted and flowed to form a microporous film structure on at least the outermost surface of the nonwoven fabric, while one or more internal meltblown layers and / or molten fibrillated layers are not softened and flowed. In this regard, the first outermost spunbond layer and the second outermost spunbond layer can each define a sheath component that protects (e.g., reduces lint formation) the one or more internal meltblown layers and / or molten fibrillated layers. In this regard, the one or more internal meltblown layers and / or molten fibrillated layers can have a lower degree of bonding compared to one or both of the outermost spunbond layers. In particular embodiments of the present invention, the second polymer composition has a second melting point lower than the third melting point. The second melting point may be the same as or different from the first melting point, according to particular embodiments of the present invention.

[0027] For example, Figure 1 shows a nonwoven fabric 1 according to a particular embodiment of the present invention. The nonwoven fabric 1 includes a first outermost spunbond layer 10 and a second outermost spunbond layer 20. The nonwoven fabric shown in Figure 1 includes three internal meltblown nonwoven layers and / or molten fibrillated nonwoven layers 30, 40, and 50. As described above, one or both of the outermost spunbond layers 10, 20 can be subjected to smoothing thermal calendering (e.g., area bonding) under conditions such that at least a portion of the outermost surface of the nonwoven fabric is softened and flows to form a microporous film structure, while the internal nonwoven layers substantially retain their individual fiber structures.

[0028] For example, Figure 2 shows a magnified cross-sectional image of a nonwoven fabric 1 according to a particular embodiment of the present invention. Figure 2 shows the first outermost spunbond layer 10, which has been softened and flowed to form a microporous film structure. Figure 2 also shows the inner layers of the meltblown layer, which substantially retain their individual fiber structures (for example, the individual fibers forming the layer are visually identifiable).

[0029] According to certain embodiments of the present invention, the first polymer composition may include a first polyolefin composition. For example, the first polyolefin composition may include a first polypropylene, a first polyethylene, a first polypropylene copolymer, a first polyethylene copolymer, or a combination thereof. As described above, the first polyolefin composition may include polymers produced from various catalyst systems, including but not limited to Ziegler-Natta catalyst systems and metallocene / single-site catalyst systems. For example, the first polymer composition may include a first single-site catalyst polypropylene (metallocene catalyst polypropylene). According to certain embodiments of the present invention, the second plurality of continuous fibers may include a second polymer composition, the second polymer composition may be the same as or different from the first polymer composition. In this regard, the second polymer composition may include a second polyolefin composition. For example, the second polyolefin composition may include a second polypropylene, a second polyethylene, a second polypropylene copolymer, a second polyethylene copolymer, or a combination thereof. As described above, the second polyolefin composition may include polymers produced from various catalyst systems, including but not limited to Ziegler-Natta catalyst systems and metallocene / single-site catalyst systems. For example, the second polymer composition may include a second single-site catalyst polypropylene (metallocene catalyst polypropylene).

[0030] According to certain embodiments of the present invention, the third polymer composition may include a third polyolefin composition. For example, the third polyolefin composition may include a third polypropylene, a third polyethylene, a third polypropylene copolymer, a third polyethylene copolymer, or a combination thereof. As described above, the third polyolefin composition may include polymers produced from various catalyst systems, including but not limited to Ziegler-Natta catalyst systems and metallocene / single-site catalyst systems. For example, the third polymer composition may include a third single-site catalyst polypropylene (metallocene catalyst polypropylene). According to certain embodiments of the present invention, the third melting point is higher than both the first and second melting points. According to certain embodiments of the present invention, the first and / or second melting points may be less than 150°C, and the third melting point may be greater than 150°C.

[0031] According to a particular embodiment of the present invention, the nonwoven fabric may include one of the following structures: S1a-Mb-S2c (Formula 1) During the ceremony, "M" includes meltblown nonwoven fabrics and / or molten fibrillated nonwoven fabrics; "S1" includes the first spunbond nonwoven fabric; "S2" includes a second spunbond nonwoven fabric; "a" represents the number of layers, independently selected from 1, 2, 3, 4, and 5; "b" represents the number of layers, independently selected from 1, 2, 3, 4, and 5; "c" represents the number of layers, independently selected from 1, 2, 3, 4, and 5; "S1" includes a first outermost spunbond layer, "S2" includes a second outermost spunbond layer, and "M" includes a first meltblown layer and / or molten fibrillated layer.

[0032] According to a particular embodiment of the present invention, for example, the nonwoven fabric may have a structure according to Formula 1, where "a" is 1, "b" is 3, and "c" is 1.

[0033] In this regard, certain embodiments of the present invention include SMS, as described above, in which meltblown fibers and / or molten fibrillated fibers are sandwiched directly or indirectly between outer layers of spunbond fibers. According to certain embodiments of the present invention, the SMS nonwoven fabric can be calendered (e.g., smooth surface calendering) as described above to densely pack the continuous fibers of the spunbond layer and form a microporous film structure on at least one outermost surface of the nonwoven fabric. According to certain embodiments of the present invention, the meltblown fibers and / or molten fibrillated fibers may include one or more polyolefins or non-polyolefins (e.g., PET).

[0034] According to certain embodiments of the present invention, the first plurality of meltblown fibers and / or molten fibrillated fibers may include an average diameter of about 0.4 to about 0.5 μm, for example, at least any of about 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, and 1 μm, and / or at most any of about 5, 4, 3, 2.5, 2, 1.5, 1.2, 1.1, and 1 μm. According to certain embodiments of the present invention, the first plurality of meltblown fibers and / or molten fibrillated fibers may include a substantially undeformed configuration. For example, the first plurality of meltblown fibers and / or molten fibrillated fibers may have a substantially circular cross-section having an aspect ratio of at least 0.8 to 1.2, for example, 1.0 + / - 0.1. According to certain embodiments of the present invention, the first plurality of molten fibrillated fibers include molten film fibrillated fibers.

[0035] According to certain embodiments of the present invention, the first plurality of continuous fibers (e.g., spunbond fibers) and / or the second plurality of continuous fibers (e.g., spunbond fibers) may have an average diameter before partial softening and melting (e.g., present in the precursor web as described later) of about 10 to about 30 μm, for example, at least any of about 10, 12, 14, 16, 18, 20, 22 μm and / or at most any of about 30, 28, 26, 24, 22, 20, 18, 16 μm. According to certain embodiments of the present invention, the first plurality of continuous fibers (e.g., spunbond fibers) and / or the second plurality of continuous fibers (e.g., spunbond fibers) may include single-component fibers or multi-component fibers (e.g., two-component sheath-core fibers in which at least the sheath component comprises the first polymer material). According to certain embodiments of the present invention, the first plurality of continuous fibers (e.g., spunbond fibers) and / or the second plurality of continuous fibers (e.g., spunbond fibers) may include a non-circular cross-section having an aspect ratio of, for example, 1.5 or greater. Alternatively, the first plurality of continuous fibers (e.g., spunbond fibers) and / or the second plurality of continuous fibers (e.g., spunbond fibers) may include a substantially circular cross-section having an aspect ratio of at least 0.8 to 1.2, for example, 1.0+ / -0.1.

[0036] According to a particular embodiment of the present invention, the nonwoven fabric may contain about 1 to about 50% by weight of meltblown fibers and / or molten fibrillated fibers, for example, at least about 1, 2, 3, 4, 5, 8, 10, 12, 15, 20, or 25% by weight of the nonwoven fabric is meltblown fibers and / or molten fibrillated fibers, and / or at most about 50, 45, 40, 35, 30, 25, 20, 15, 12, 10, or 5% by weight of the nonwoven fabric is meltblown fibers and / or molten fibrillated fibers.

[0037] According to certain embodiments of the present invention, the first polymer composition may contain a first melt flow rate (MFR), and the third polymer composition may contain a third MFR, wherein the third MFR is greater than the first MFR. For example, the MFR ratio between the third MFR and the first MFR (third MFR:first MFR) may range from about 20:1 to about 150:1, for example, at least any of about 20:1, 30:1, 40:1, 50:1, 60:1, 70:1 and / or at most any of about 150:1, 140:1, 130:1, 120:1, 110:1, 100:1, 90:1, 80:1, 70:1, 60:1. According to certain embodiments of the present invention, the third MFR may be about 1000 dg / min to about 2500 dg / min, for example, at least any of about 1000, 1200, 1400, 1600, or 1800 dg / min, and / or at most any of about 2500, 2400, 2200, 2000, or 1800 dg / min. According to certain embodiments of the present invention, the first MFR and / or the second MFR (i.e., the MFR of the second polymer composition) may be about 10 dg / min to about 150 dg / min, for example, at least any of about 10, 15, 20, 25, or 30 dg / min, and / or at most any of about 150, 125, 100, 75, 50, 40, or 30 dg / min.

[0038] According to a particular embodiment of the present invention, the nonwoven fabric may have a thickness in the z-direction perpendicular to the longitudinal and transverse directions, and its thickness may range from about 100 μm to about 200 μm, for example, at least any of about 100, 110, 120, 130, 140, 150 μm and / or at most any of about 200, 190, 180, 175, 170, 160, 150 μm.

[0039] According to certain embodiments of the present invention, the nonwoven fabric may have a hydrostatic head of about 100 to about 250 mbar when measured by AATCC TM127, for example, at least about 100, 110, 120, 130, 140, or 150 mbar when measured by AATCC TM127, and / or at most about 250, 225, 200, 175, 170, 160, or 150 when measured by AATCC TM127. According to certain embodiments of the present invention, the nonwoven fabric may include a head-to-thickness ratio (head in mbar as measured by AATCC TM127:thickness in μm) of about 0.8:1 to about 2:1, for example, at least any of 0.8:1, 0.9:1, 1:1, 1.1:1, 1.15:1, 1.2:1, 1.25:1, 1.3:1 and / or at most any of 2:1, 1.9:1, 1.8:1, 1.7:1, 1.6:1, 1.5:1, 1.4:1, 1.3:1.

[0040] According to a particular embodiment of the present invention, the nonwoven fabric has a density of approximately 300 to approximately 1000 mL / dm² when measured by ASTM D737-75. 2 For example, at least about 300, 400, 500, 550, 600, and 650 mL / dm³ as measured by ASTM D737-75. 2 Any of the following values ​​per minute, and / or at most about 1000, 900, 800, 700, 650, or 600 mL / dm² as measured by ASTM D737-75 2 The nonwoven fabric may have an air permeability of any of the following values: perm / min. According to a particular embodiment of the present invention, the nonwoven fabric may have an air permeability to thickness ratio (mL / dm² as measured by ASTM D737-75) of about 2.5:1 to about 5:1, for example, at least any of 2.5:1, 2.75:1, 3:1, 3.25:1, 3.5:1, 3.75:1, 4:1 and / or at most any of 5:1, 4.5:1, 4:1, 3.5:1, 3:1. 2 Air per minute: (thickness in μm units) can be included.

[0041] According to certain embodiments of the present invention, the nonwoven fabric may have longitudinal Elmendorf tear values ​​of about 4 to about 10 N when measured according to ASTM D1424-EN21974, for example, at least about 4, 4.5, 5, 5.5, 6, or 6.5 N and / or at most about 10, 9, 8, 7, or 6.5 N when measured according to ASTM D1424-EN21974. According to certain embodiments of the present invention, the nonwoven fabric may have transverse Elmendorff tear values ​​of about 5 to about 20 N when measured according to ASTM D1424-EN21974, for example, at least about 5, 6, 7, 8, 9, and 10 N when measured according to ASTM D1424-EN21974, and / or at most about 20, 18, 16, 14, 12, and 10 N when measured according to ASTM D1424-EN21974.

[0042] According to certain embodiments of the present invention, the nonwoven fabric may include transverse Elmendorff tear-to-thickness ratios (transverse Elmendorff tear in N units as measured by ASTM D1424-EN21974: thickness in μm units) of about 1:8 to about 1:30, for example, at least about 1:30, 1:25, 1:20, 1:18, 1:15 and / or at most about 1:8, 1:9, 1:10, 1:11, 1:12, 1:13, 1:14, 1:15.

[0043] According to a specific embodiment of the present invention, the nonwoven fabric weighs approximately 750 to approximately 2500 g / m² when measured by ASTM E96D. 2 For example, over 24 hours, measured by ASTM E96D, at least approximately 750, 800, 850, 900, 950, 1000, 1100, 1200, 1300, 1400 g / m² 2 At most approximately 2500, 2250, 2000, 1800, 1600, and 1500 g / m² per 24-hour period and / or as measured by ASTM E96D. 2The nonwoven fabric may include a water vapor transmission rate (WVTR) of any of the following values: / 24 hours. According to certain embodiments of the present invention, the nonwoven fabric may have a WVTR to thickness ratio (g / m² as measured by ASTM E96D) of about 7:1 to about 20:1, for example, at least any of about 7:1, 8:1, 9:1, 10:1, 11:1, 12:1 and / or at most any of about 20:1, 18:1, 16:1, 15:1, 14:1, 13:1, 12:1. 2 / 24-hour WVTR (thickness in μm units) can be included.

[0044] According to certain embodiments of the present invention, the nonwoven fabric may have an average pore size of about 1.5 to about 3 μm when measured by ASTM F316-86, for example, at least about 1.5, 1.8, 2.0, 2.2, 2.5, or 2.5 μm when measured by ASTM F316-86, and / or at most about 3, 2.9, 2.8, 2.7, 2.6, 2.5, or 2.4 μm when measured by ASTM F316-86. According to a particular embodiment of the present invention, the nonwoven fabric may contain a maximum pore diameter of about 3.5 to about 6 μm when measured by ASTM F316-86, for example, at least about 3.5, 3.8, 4, 4.2, 4.3, 4.4, or 4.5 μm and / or at most about 6, 5.8, 5.6, 5.4, 5.2, 5, 4.8, 4.6, or 4.5 μm when measured by ASTM F316-86. According to a particular embodiment of the present invention, the maximum pore diameter may be 2.8 μm or less larger than the average pore diameter, for example, 2.8, 2.7, 2.6, 2.5, 2.4, 2.3, 2.2, 2.1, 2, 1.8, or 1.6 μm or less larger than the average pore diameter.

[0045] According to certain embodiments of the present invention, the nonwoven fabric may have a bacterial filtration efficiency (BFE) of at least 90% as measured by ASTM F2101-14, for example, at least about 90, 92, 94, 95, 96, 97, 98, or 99% as measured by ASTM F2101-14. According to certain embodiments of the present invention, the nonwoven fabric may have an aerosol spore challenge value (logarithmically reduced value or LRV) greater than 3LRV as measured by ASTM F1608.

[0046] According to certain embodiments of the present invention, the nonwoven fabric may have a lint level of 1,000 or fewer particles when measured according to ISO 9073-10, for example, about 900, 800, 700, 600, 500, 400, or 300 or fewer particles when measured according to ISO 9073-10.

[0047] According to certain embodiments of the present invention, the nonwoven fabric may include a nonwoven fabric that has been smoothed calendered at a high temperature and, for example, at a nip pressure of about 1500 to about 3000 pounds / linear inch, so that the first polymer composition softens and flows to form a microporous film.

[0048] According to certain embodiments of the present invention, the nonwoven fabric may include a basis weight of about 30 to about 200 g / m² (GSM), for example, at least any of about 200, 180, 160, 140, 120, 100, 80, and 60 gsm, and / or at least any of about 30, 40, 50, 60, 70, 80, and 90 gsm.

[0049] In another embodiment, the present invention provides a method for forming a nonwoven fabric. According to a particular embodiment of the present invention, the method is The method may include providing or forming a first outermost spunbond layer comprising a first plurality of continuous fibers, wherein the first plurality of continuous fibers comprises a first polymer composition having a first melting point. The method may further include depositing at least a first meltblown layer and / or molten fibrillated layer comprising a first plurality of meltblown fibers and / or molten fibrillated fibers located directly or indirectly on the first outermost spunbond layer, wherein the first plurality of meltblown fibers and / or molten fibrillated fibers comprises a third polymer composition having a third melting point higher than the first melting point. According to a particular embodiment of the present invention, the method is The method may also include providing or forming a second outermost spunbond layer containing a second plurality of continuous fibers directly or indirectly on a first meltblown layer and / or molten fibrillated layer forming a precursor web, the first meltblown layer and / or molten fibrillated layer being located directly or indirectly between the first outermost spunbond layer and the second outermost spunbond layer. The method may also include calendering the first outermost spunbond layer of the precursor web to compress the first plurality of continuous fibers relative to each other, forming a substantially smooth outer surface in the form of a microporous film that allows water vapor to pass through and also functions as a barrier against bacteriological contamination.

[0050] According to certain embodiments of the present invention, the step of calendering a first outermost spunbond layer includes smoothing the first outermost spunbond layer (e.g., area bonding) at a nip pressure of about 1500 to about 3000 pounds / linear inch and at a high temperature so that the first polymer composition softens and flows to form a microporous film. In this regard, a second outermost spunbond layer may also undergo a smoothing calendering operation to provide a second microporous film on the second outermost surface of the nonwoven fabric. According to such embodiments of the present invention, both outermost surfaces of the nonwoven fabric include a microporous film structure formed from the softening and flow of the respective continuous spunbond fibers.

[0051] According to a particular embodiment of the present invention, the step of calendering a first outermost spunbond layer includes heating a first plurality of continuous fibers to a calendering temperature that is (i) above a first melting point and (ii) below a third melting point. According to a particular embodiment of the present invention, the second outermost spunbond layer includes heating a second plurality of continuous fibers to a calendering temperature that is (i) above a second melting point and (ii) below a third melting point.

[0052] According to certain embodiments of the present invention, the method may also include pre-binding a precursor web before calendering (e.g., smoothing calendering) the first outermost spunbond layer. For example, the step of pre-binding a precursor web includes imparting a binding area of ​​about 1% to about 30% of the precursor web before secondary calendering (e.g., smoothing calendering).

[0053] For example, Figure 3 shows a schematic diagram of a method 100 for producing a nonwoven fabric according to a specific embodiment of the present invention. As shown in Figure 3, a first spunbond beam 101 deposits a first plurality of continuous spunbond fibers 105, followed by three continuous meltblown beams 110, 120, and 130 depositing layers of meltblown fibers 115, 125, and 135, respectively. Subsequently, a final beam, a spunbond beam 140, deposits a second plurality of continuous spunbond fibers 145 on top of the final deposited layer of meltblown fibers 135 to form a precursor web. The precursor web can then be pre-bound by a thermal calender 150. Optionally, the precursor web may be surface-treated with additives (e.g., hydrophobic finish) via a kissroll applicator 160. The precursor web can then undergo a secondary thermal calendering step, such as a smoothing calendering operation 170, during which the first plurality of continuous fibers soften and flow, forming a microporous film on the outermost surface of the nonwoven fabric. The resulting nonwoven fabric can be stored on the winding machine 180.

[0054] In another embodiment, the present invention provides a package. According to a particular embodiment of the present invention, the package may include a sealed or sealable container having an interior defined at least partially by a container wall, where at least a portion of the sealed or sealable container includes a breathable material such as a nonwoven fabric as described and disclosed herein, through which a sterilization gas such as ethylene oxide, hydrogen peroxide plasma, or vapor can enter and exit the interior of the sealed or sealable container.

[0055] According to certain embodiments of the present invention, the package may include an adhesive placed on the container wall and / or on a portion of the breathable material. Alternatively, the package may be without an adhesive.

[0056] According to certain embodiments of the present invention, the package may include a sealing film disposed on the container wall and / or on a portion of a breathable material. For example, the breathable material may be sealed to the container wall via the sealing film.

[0057] According to certain embodiments of the present invention, the package may include a flexible package, and the breathable material may define a window portion of the flexible package. Alternatively, the package may include a rigid package, and the breathable material may define a peelable lid or flexible portion of the rigid package.

[0058] According to certain embodiments of the present invention, the package includes an article, such as a medical device, placed inside the container. For example, the medical device may be sterile. According to certain embodiments of the present invention, the atmosphere inside the container is substantially free of sterilization gases.

[0059] In yet another aspect, the present disclosure provides a method for sterilizing a package, the method comprising: (i) providing a package as disclosed and described herein; (ii) placing the package in an air chamber; (iii) evacuating air from the air chamber and the package; (iv) filling the air chamber and the package with a sterilizing gas; (v) allowing the sterilizing gas to remain in the air chamber and the package for a predetermined period; and (vi) evacuating the sterilizing gas. According to certain embodiments of the present invention, the sterilizing gas can include ethylene oxide, ethylene oxide and nitrogen, ethylene oxide and carbon dioxide, ethylene oxide including one or more chlorofluorocarbon diluents, ozone, hydrogen peroxide gas plasma, chlorine dioxide, moisture (e.g., steam), and mixtures thereof. According to certain embodiments of the present invention, steps (iii)-(vi) are repeated sequentially for a plurality of sterilization cycles.

[0060] 〔Examples〕 The present disclosure is further illustrated by the following examples, which should in no way be construed as limiting. That is, the specific features described in the following examples are merely illustrative and not limiting.

[0061] Test Methods Pore Size: The pore size was measured with a PMI porometer using a 25 mm diameter sample holder. The pore size measurement method PMI automatic capillary flow porometer system complies with ASTM F316-86 / EN868-6-2017 Annex C. WVTR: The WVTR was evaluated using ASTM E96D---Standard Test Method for Water Vapor Transmission of Materials. This test method is for measuring the water vapor transmission rate of materials through which water vapor passes at 50% relative humidity (RH) and 32 °C in Procedure B, and is reported in grams per square meter per 24 hours (g / m 2 / 24 h). Air Permeability: Air permeability is a measure of the air flow passing through a sheet at a defined pressure difference between the surfaces of the sheet, and is carried out in accordance with ASTM D 737, with a test area of 38 cm 2 , a test pressure of 125 Pa, and mL / dm2 Reports are sent every minute. Moist microbial penetration: A test for bacterial barrier resistance under humidity, in accordance with DIN 58953-6, Section 3.8 Tests - Sterilized supplies - Part 6: Microbial barrier testing of packaging materials for medical devices, sterilized and then tested for bacterial resistance in humidity. The materials of the examples of the present invention were sterilized with steam (134°C / 5 mins) and H2O2-plasma (Steriplas / 50°C / 2 injections), then tested for bacterial resistance under humidity, and were evaluated as "sufficiently bacterial resistant" according to DIN 58953-6, Section 3.8. Bacterial Filtration Efficiency (BFE): BFE was evaluated according to ASTM F2101-14a, Standard Test Method for Evaluating the Bacterial Filtration Efficiency (BFE) of Medical Materials Using a Biological Aerosol of Staphylococcus aureus. The BFE test is performed to determine the filtration efficiency of the test material by comparing the number of bacteria upstream of the test material with the number of bacteria downstream. A suspension of Staphylococcus aureus was aerosolized using a sprayer and delivered to the test material at a constant flow rate and constant air pressure. This test method conforms to ASTM F2101-14, Annex B, and AS4381:2015. Aerosol Spore Challenge (Exposure Chamber Method): The aerosol spore challenge was evaluated according to ASTM F1608, the standard test method for microbial ranking of porous packaging materials (exposure chamber method). This test method is used to measure the passage of airborne bacteria through porous materials intended for use in packaging sterile medical devices. This test method is designed to test materials under conditions in which the passage of bacterial spores through the test material is detectable. In the laboratory, porous materials were tested to determine the logarithmic reduction value (LRV) materials tested under standard conditions. The aerosol spore challenge (exposure chamber method) ASTM F1608 test employs low flow rates, long exposure times, and high challenge levels, allowing for the testing of materials with high differential pressure values. All flow rates were at standard levels. Particle linting tests were conducted according to Gelbo Flex Linting: ISO 9073-10: Standard test method for measuring lint and other particles generated in a dry state (Gelbo Flex). Using the Gelbo Flex mechanism, a combined torsional and compressive action was applied to the test article (sample size: 22 cm wide x 28.5 cm long) in a test chamber. During flexing, air was removed from the chamber, and the generated particles were counted and classified by size using a laser particle counter. Particle sizes of 0.3 μm, 0.5 μm, 1.0 μm, 5.0 μm, and 10.0 μm to 25 μm were collected and counted for each type of material.

[0062] sample Comparative sample 1: Tyvek® 1073B, a brand of nonwoven fabric formed from flash-spun high-density polyethylene (HDPE) fibers. The fibers of this sample material have an average diameter of approximately 1.54 μm (0.66 μm to 2.54 μm). Comparison Sample 2: Commercially available medical-grade paper was purchased and used as another comparison sample. Examples of the Invention: The sample material of the Invention has an SMMMS structure and was manufactured on a 5-beam manufacturing line (i.e., Reicofil 4 line). The process for forming the sample of the Invention included forming a first spunbond layer from beam 1 of continuous metallocene polypropylene filaments deposited on a migratory surface, and then forming three separate layers of meltblown fibers via beams 2, 3, and 4 placed on the first spunbond layer. The meltblown fibers were formed from metallocene polypropylene having a higher melting point (i.e., 9°C higher) than the first spunbond layer. Next, a second spunbond layer covering the meltblown layer was spun and deposited using beam 5. The resulting precursor web (e.g., an SMMMS web that has not undergone integration operation) was then fed to the nip point of a calender (e.g., pre-bonded) and point-bonded under pressure (i.e., 1080 N / cm and a temperature of 165°C). Next, the pre-bonded precursor web (i.e., Example 0 of the present invention (base nonwoven fabric)) was thermally bonded with a smooth metal calender nip at a temperature of 310°F (154.40°C), a line speed of 38 meters / min, and under high pressure of 1500-2500 pounds / linear inch to obtain the embodiment of the present invention. The properties of the obtained nonwoven fabric are summarized in Table 1 below.

[0063] In the embodiments of the present invention, metallocene PP spunbond and metallocene PP meltblown resins with different melt flow rates (MFRs) were used. Specifically, the spunbond layers were formed from metallocene polypropylene with an MFR of 30 dg / min, and the meltblown layers were formed from metallocene polypropylene with an MFR of 1800 dg / min. The melting point of the polymer composition forming each spunbond layer was 9°C lower than that of the polymer composition forming each meltblown layer. In this regard, the difference in melting points between the spunbond and meltblown layers allowed for easier melting (e.g., softening and at least partial flow) of the outer spunbond layer during secondary calendering (e.g., smooth calendering to impart a microporous film structure) while maintaining separate, finer fibers (e.g., unmelted) in the center or core of the nonwoven fabric, as shown, for example, in Figure 2. In this regard, the samples of the present invention were able to maintain a desired level of permeability. The total basis weight of the precursor web, identified as Example 0 (base nonwoven fabric) in Table 1, was 76.8 g / m². 2 That was the case.

[0064] In the sample of the present invention, each meltblown fiber in each meltblown layer had a circular cross-section and an average diameter of 1.06 μm (0.33 μm to 3 μm), and the spunbond fibers in each spunbond layer had an average diameter of approximately 17.22 μm (15.84 μm to 20 μm). The first layer of continuous spunbond fibers in the precursor web (Example 0 of the present invention) was approximately 33.3 gsm, the total of all three meltblown layers was approximately 10.2 gsm, and the second layer of continuous spunbond fibers was approximately 33.3 gsm. The precursor web (Example 0 of the present invention) was pre-bonded with an embossing roll to obtain a point-bonded bonding area of ​​18% of the surface of the nonwoven fabric.

[0065] Table 1 summarizes the test results data of the precursor web (Example 0 of the present invention) and the examples of the present invention compared with comparative sample 1 and comparative sample 2. [Table 1]

[0066] As shown in Table 1, the embodiments of the present invention had a smaller average pore size than medical-grade paper and Tyvek®. Furthermore, the average pore size was 29% smaller than that of 76gsm Tyvek material and 67% smaller than that of medical paper. The maximum pore size of the embodiments of the present invention was 42% lower than that of 76gsm Tyvek material and 40% lower than that of medical paper. In this respect, the embodiments of the present invention exhibited superior uniformity and lower variability than both Tyvek and medical paper.

[0067] According to certain embodiments of the present invention, such as those described in the examples of the present invention, the structure of the nonwoven fabric allows vapor to pass through the nonwoven fabric while simultaneously providing sufficient and / or desirable barrier properties against bacteria and polar liquids (e.g., water, blood, etc.). Furthermore, the examples of the present invention demonstrate that embodiments according to certain embodiments of the present invention provide higher hydrostatic head and higher barrier properties (e.g., LRV > 3) than Tyvek®.

[0068] These and other modifications and variations of the present invention can be implemented by those skilled in the art without departing from the spirit and scope of the invention, as more specifically described in the appended claims. Furthermore, it should be understood that the various embodiments may be interchangeable in whole or in part. Moreover, those skilled in the art will understand that the above description is merely illustrative and not intended to limit the invention as further described in the appended claims. Accordingly, the spirit and scope of the appended claims should not be limited to the illustrative description of the version contained herein.

[0069] [Implementation Method] (1) Nonwoven fabric, (i) A first outermost spunbond layer comprising a first plurality of continuous fibers that are thermally fused and compressed with respect to each other and define a microporous film on the outermost surface of the nonwoven fabric, wherein the first plurality of continuous fibers comprise a first polymer composition having a first melting point, (ii) A second outermost spunbond layer comprising a second set of continuous fibers, (iii) at least a first meltblown layer and / or molten fibrillated layer comprising a plurality of first meltblown fibers and / or molten fibrillated fibers located directly or indirectly between the first outermost spunbond layer and the second outermost spunbond layer, wherein the plurality of first meltblown fibers and / or molten fibrillated fibers comprise a third polymer composition having a third melting point, the first melting point being lower than the third melting point, Nonwoven fabric, including (2) The nonwoven fabric according to Embodiment 1, wherein the first polymer composition of the first plurality of continuous fibers softens and flows to form the microporous film, the microporous film allowing water vapor to permeate the nonwoven fabric and at least partially preventing the penetration of the nonwoven fabric by polar liquids. (3) The nonwoven fabric according to Embodiments 1 to 2, wherein the first melting point is at least about 1°C to about 30°C lower than the third melting point, for example, at most about 30°C, 25°C, 20°C, 15°C, or 10°C lower than the third melting point, and / or at least about 1°C, 2°C, 3°C, 4°C, 5°C, 6°C, 7°C, 8°C, 9°C, or 10°C lower than the third melting point. (4) The nonwoven fabric according to Embodiments 1 to 3, wherein the first polymer composition comprises a first polyolefin composition, for example, a first polypropylene, a first polyethylene, a first polypropylene copolymer, a first polyethylene copolymer, or a combination thereof. (5) The nonwoven fabric according to Embodiments 1 to 4, wherein the second plurality of continuous fibers comprises a second polymer composition, the second polymer composition may be the same as or different from the first polymer composition, and the second polymer composition has a second melting point, the second melting point being lower than the third melting point.

[0070] (6) The nonwoven fabric according to Embodiments 1 to 5, wherein the first melting point is less than 150°C and the third melting point is greater than 150°C. (7) The nonwoven fabric comprises one of the following structures: S1 a -M b -S2 c During the ceremony, "M" includes meltblown nonwoven fabrics and / or molten fibrillated nonwoven fabrics; "S1" includes the first spunbond nonwoven fabric; "S2" includes a second spunbond nonwoven fabric; "a" represents the number of layers, independently selected from 1, 2, 3, 4, and 5; "b" represents the number of layers, independently selected from 1, 2, 3, 4, and 5; "c" represents the number of layers, independently selected from 1, 2, 3, 4, and 5; The nonwoven fabric according to embodiments 1 to 6, wherein "S1" comprises the first outermost spunbond layer, "S2" comprises the second outermost spunbond layer, and "M" comprises the first meltblown layer and / or molten fibrillated layer. (8) The nonwoven fabric according to Embodiments 1 to 7, wherein the first polymer composition has a first melt flow rate (MFR), and the third polymer composition has a third MFR, the third MFR being greater than the first MFR. (9) The nonwoven fabric according to Embodiment 8, wherein the MFR ratio of the third MFR to the first MFR (third MFR:first MFR) is approximately 20:1 to approximately 150:1, for example, at least any of approximately 20:1, 30:1, 40:1, 50:1, 60:1, 70:1 and / or at most any of approximately 150:1, 140:1, 130:1, 120:1, 110:1, 100:1, 90:1, 80:1, 70:1, 60:1. (10) The nonwoven fabric according to Embodiments 8 to 9, wherein the third MFR is approximately 1000 dg / min to approximately 2500 dg / min, for example, at least any of approximately 1000, 1200, 1400, 1600, 1800 dg / min and / or at most any of approximately 2500, 2400, 2200, 2000, 1800 dg / min, and the first MFR is approximately 10 dg / min to approximately 150 dg / min, for example, at least any of approximately 10, 15, 20, 25, 30 dg / min and / or at most any of approximately 150, 125, 100, 75, 50, 40, 30 dg / min.

[0071] (11) The nonwoven fabric is as follows: (i) A head-to-thickness ratio (head in mbar:thickness in μm as measured with AATCC TM127) of approximately 0.8:1 to approximately 2:1, for example, at least one of approximately 0.8:1, 0.9:1, 1:1, 1.1:1, 1.15:1, 1.2:1, 1.25:1, 1.3:1 and / or at most one of approximately 2:1, 1.9:1, 1.8:1, 1.7:1, 1.6:1, 1.5:1, 1.4:1, 1.3:1 (head in mbar:thickness in μm as measured with AATCC TM127); (ii) A permeability-to-thickness ratio (mL / dm³ as measured by ASTM D737-75) of approximately 2.5:1 to approximately 5:1, for example, at least one of approximately 2.5:1, 2.75:1, 3:1, 3.25:1, 3.5:1, 3.75:1, or 4:1, and / or at most one of approximately 5:1, 4.5:1, 4:1, 3.5:1, or 3:1. 2 Air per minute: Thickness in μm units); (iii) Transverse Elmendorf tear-to-thickness ratios of approximately 1:8 to approximately 1:30, for example, at least one of approximately 1:30, 1:25, 1:20, 1:18, 1:15 and / or at most one of approximately 1:8, 1:9, 1:10, 1:11, 1:12, 1:13, 1:14, 1:15 (Transverse Elmendorf tear in N units: thickness in μm units as measured by ASTM D1424-EN21974); or, (iv) WVTR to thickness ratio (g / m² as measured by ASTM E96D) of approximately 7:1 to approximately 20:1, for example, at least one of approximately 7:1, 8:1, 9:1, 10:1, 11:1, 12:1 and / or at most one of approximately 20:1, 18:1, 16:1, 15:1, 14:1, 13:1, 12:1 2 WVTR in 24-hour units (thickness in μm units), A nonwoven fabric according to embodiments 1 to 10, having one or more of the above. (12) A method for forming a nonwoven fabric, (i) To provide or form a first outermost spunbond layer comprising a first plurality of continuous fibers, wherein the first plurality of continuous fibers comprises a first polymer composition having a first melting point, (ii) Depositing at least a first meltblown layer and / or molten fibrillated layer, which comprises a first plurality of meltblown fibers and / or molten fibrillated fibers located directly or indirectly on the first outermost spunbond layer, wherein the first plurality of meltblown fibers and / or molten fibrillated fibers comprise a third polymer composition having a third melting point, the first melting point being lower than the third melting point, (iii) Providing or forming a second outermost spunbond layer containing a second plurality of continuous fibers directly or indirectly on the first meltblown layer and / or molten fibrillated layer forming a precursor web, wherein the first meltblown layer and / or molten fibrillated layer is located directly or indirectly between the first outermost spunbond layer and the second outermost spunbond layer, (iv) Calendering the first outermost spunbond layer of the precursor web and compressing the first plurality of continuous fibers relative to each other to form a substantially smooth outer surface in the form of a microporous film that allows water vapor to pass through and also functions as a barrier against bacteriological contamination, Includes, Calendering the first outermost spunbond layer optionally includes smoothing the first outermost spunbond layer at a nip pressure of about 1500 to about 3000 pounds / linear inch and at a high temperature so that the first polymer composition softens and flows to form the microporous film, wherein the high temperature is (i) above the melting point of the first and (ii) below the melting point of the third. (13) Package, A sealed or sealable container comprising an interior defined at least partially by the container wall, wherein at least a portion of the sealed or sealable container comprises a permeable material through which a sterilization gas can enter and exit the interior of the sealed or sealable container, the permeable material comprising (i) a first outermost spunbond layer comprising a first plurality of continuous fibers that are thermally fused and compressed with respect to each other and define a microporous film on the outermost surface of the nonwoven fabric, the first plurality of continuous fibers comprising a first polymer composition having a first melting point; and (ii) a second A package comprising: (iii) a second outermost spunbond layer comprising a plurality of continuous fibers; (iii) at least a first meltblown layer and / or molten fibrillated layer comprising a plurality of first meltblown fibers and / or molten fibrillated fibers located directly or indirectly between the first outermost spunbond layer and the second outermost spunbond layer, wherein the plurality of first meltblown fibers and / or molten fibrillated fibers comprise a third polymer composition having a third melting point, the first melting point being lower than the third melting point; and at least a first meltblown layer and / or molten fibrillated layer. (14) The package according to embodiment 13, further comprising a sealing film disposed on the container wall and / or on a portion of the breathable material, wherein the breathable material is sealed to the container wall via the sealing film. (15) A method for sterilizing a package, (i) To provide the package described in Embodiment 14, (ii) Placing the package in an air chamber, (iii) removing air from the air chamber and the package, (iv) Filling the air chamber and the package with sterilization gas, (v) Allowing the sterilization gas to remain in the air chamber and the package for a predetermined period of time, (vi) The sterilization gas is removed, Methods that include...

Claims

1. A nonwoven fabric, (i) a first outermost spunbond layer comprising a first plurality of continuous fibers heat fused and compressed to one another and defining a microporous film on an outermost surface of the nonwoven fabric, the first plurality of continuous fibers comprising a first polymer composition having a first melting point; (ii) a second outermost spunbond layer comprising a second plurality of continuous fibers; and (iii) at least a first meltblown and / or melt fibrillated layer comprising a first plurality of meltblown and / or melt fibrillated fibers located directly or indirectly between the first outermost spunbond layer and the second outermost spunbond layer, the first plurality of meltblown and / or melt fibrillated fibers comprising a third polymer composition having a third melting point, the first melting point being lower than the third melting point; Nonwoven fabrics, including:

2. 10. The nonwoven fabric of claim 1, wherein the first polymer composition of the first plurality of continuous fibers softens and flows to form the microporous film, which allows water vapor to permeate the nonwoven fabric while at least partially preventing penetration of the nonwoven fabric by polar liquids.

3. 3. The nonwoven fabric according to claim 1, wherein the first melting point is at least about 1°C to about 30°C lower than the third melting point, e.g., at most about 30°C, 25°C, 20°C, 15°C, or 10°C lower than the third melting point, and / or at least about 1°C, 2°C, 3°C, 4°C, 5°C, 6°C, 7°C, 8°C, 9°C, or 10°C lower than the third melting point.

4. 4. The nonwoven fabric of claims 1-3, wherein the first polymer composition comprises a first polyolefin composition, such as a first polypropylene, a first polyethylene, a first polypropylene copolymer, a first polyethylene copolymer, or a combination thereof.

5. 5. The nonwoven fabric of claims 1-4, wherein the second plurality of continuous fibers comprises a second polymer composition, which may be the same as or different from the first polymer composition, and wherein the second polymer composition has a second melting point, the second melting point being lower than the third melting point.

6. 6. The nonwoven fabric according to claim 1, wherein the first melting point is less than 150°C and the third melting point is greater than 150°C.

7. The nonwoven fabric comprises one of the following structures: S1 a -M b -S2 c During the ceremony, "M" includes meltblown and / or melt fibrillated nonwovens; "S1" comprises a first spunbond nonwoven; "S2" comprises a second spunbond nonwoven; "a" represents the number of layers and is independently selected from 1, 2, 3, 4, and 5; "b" represents the number of layers and is independently selected from 1, 2, 3, 4, and 5; "c" represents the number of layers and is independently selected from 1, 2, 3, 4, and 5; 7. The nonwoven fabric of claims 1-6, wherein "S1" comprises the first outermost spunbond layer, "S2" comprises the second outermost spunbond layer, and "M" comprises the first meltblown and / or melt fibrillated layer.

8. 8. The nonwoven fabric of claims 1-7, wherein the first polymer composition has a first melt flow rate (MFR) and the third polymer composition has a third MFR, the third MFR being greater than the first MFR.

9. 9. The nonwoven fabric of claim 8, wherein the MFR ratio of the third MFR to the first MFR (third MFR:first MFR) is from about 20:1 to about 150:1, e.g., at least about any of 20:1, 30:1, 40:1, 50:1, 60:1, and 70:1, and / or at most about any of 150:1, 140:1, 130:1, 120:1, 110:1, 100:1, 90:1, 80:1, 70:1, and 60:

1.

10. 10. The nonwoven fabric according to claim 8, wherein the third MFR is from about 1000 dg / min to about 2500 dg / min, e.g., at least about any of 1000, 1200, 1400, 1600, 1800 dg / min, and / or at most about any of 2500, 2400, 2200, 2000, 1800 dg / min, and the first MFR is from about 10 dg / min to about 150 dg / min, e.g., at least about any of 10, 15, 20, 25, 30 dg / min, and / or at most about any of 150, 125, 100, 75, 50, 40, 30 dg / min.

11. The nonwoven fabric may be made of the following: (i) a hydrostatic head to thickness ratio (hydrostatic head in mbar:thickness in μm as measured by AATCC TM127) of about 0.8:1 to about 2:1, e.g., at least about any of 0.8:1, 0.9:1, 1:1, 1.1:1, 1.15:1, 1.2:1, 1.25:1, 1.3:1, and / or at most about any of 2:1, 1.9:1, 1.8:1, 1.7:1, 1.6:1, 1.5:1, 1.4:1, 1.3:1; (ii) an air permeability to thickness ratio (mL / dm as measured by ASTM D737-75) of from about 2.5:1 to about 5:1, e.g., at least about any of 2.5:1, 2.75:1, 3:1, 3.25:1, 3.5:1, 3.75:1, 4:1, and / or at most about any of 5:1, 4.5:1, 4:1, 3.5:1, and 3:1; 2 / min:thickness in μm); (iii) a transverse Elmendorf tear to thickness ratio (transverse Elmendorf tear in N:thickness in μm as measured by ASTM D1424-EN21974) of about 1:8 to about 1:30, e.g., at least about any of 1:30, 1:25, 1:20, 1:18, 1:15, and / or at most about any of 1:8, 1:9, 1:10, 1:11, 1:12, 1:13, 1:14, 1:15; or (iv) a WVTR to thickness ratio (g / m as measured by ASTM E96D) of from about 7:1 to about 20:1, e.g., at least about any of 7:1, 8:1, 9:1, 10:1, 11:1, 12:1, and / or at most about any of 20:1, 18:1, 16:1, 15:1, 14:1, 13:1, 12:1; 2 / WVTR in 24 hours: thickness in μm), The nonwoven fabric according to claims 1 to 10, having one or more of the following:

12. 1. A method of forming a nonwoven fabric, comprising: (i) providing or forming a first outermost spunbond layer comprising a first plurality of continuous fibers, the first plurality of continuous fibers comprising a first polymer composition having a first melting point; (ii) depositing at least a first meltblown and / or melt fibrillated layer comprising a first plurality of meltblown and / or melt fibrillated fibers located directly or indirectly on the first outermost spunbond layer, the first plurality of meltblown and / or melt fibrillated fibers comprising a third polymer composition having a third melting point, the first melting point being lower than the third melting point; (iii) providing or forming a second outermost spunbond layer comprising a second plurality of continuous fibers directly or indirectly on the first meltblown and / or melt fibrillated layer forming a precursor web, the first meltblown and / or melt fibrillated layer being located directly or indirectly between the first outermost spunbond layer and the second outermost spunbond layer; (iv) calendering the first outermost spunbond layer of the precursor web to compress the first plurality of continuous fibers against one another to form a substantially smooth outer surface in the form of a microporous film that allows water vapor to pass therethrough and also acts as a barrier to bacteriological contamination; Including, Calendering the first outermost spunbond layer optionally includes smooth calendering the first outermost spunbond layer at a nip pressure of about 1500 to about 3000 pounds per linear inch and at an elevated temperature so that the first polymer composition softens and flows to form the microporous film, the elevated temperature being (i) at or above the first melting point and (ii) below the third melting point.

13. A package, The present invention also includes a sealed or sealable container including an interior defined at least in part by a container wall, at least a portion of the sealed or sealable container comprising a breathable material through which a sterilizing gas can pass into and out of the interior of the sealed or sealable container, the breathable material comprising: (i) a first outermost spunbond layer comprising a first plurality of continuous fibers heat fused and compressed to one another to define a microporous film on an outermost surface of the nonwoven fabric, the first plurality of continuous fibers comprising a first polymer composition having a first melting point; and (ii) a second outermost spunbond layer comprising a first plurality of continuous fibers heat fused and compressed to one another to define a microporous film on an outermost surface of the nonwoven fabric, the first plurality of continuous fibers comprising a first polymer composition having a first melting point. and (iii) at least a first meltblown and / or melt fibrillated layer comprising a first plurality of meltblown and / or melt fibrillated fibers located directly or indirectly between the first outermost spunbond layer and the second outermost spunbond layer, the first plurality of meltblown and / or melt fibrillated fibers comprising a third polymer composition having a third melting point, the first melting point being lower than the third melting point.

14. 14. The package of claim 13, further comprising a sealing film disposed on the container wall and / or on a portion of the breathable material, the breathable material being sealed to the container wall via the sealing film.

15. 1. A method for sterilizing a package, comprising: (i) providing a package according to claim 14; (ii) placing the package in an air chamber; (iii) removing air from the air chamber and the package; (iv) filling the air chamber and the package with a sterilizing gas; (v) allowing the sterilizing gas to remain within the air chamber and the package for a predetermined period of time; (vi) venting the sterilizing gas; A method comprising: