Enhanced magnetic properties due to alignment of non-magnetic components

JP2023550577A5Inactive Publication Date: 2024-10-22AARHUS UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023521436
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-10-13
Filing Date
2021-10-13
Publication Date
2024-10-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing methods for producing permanent magnets often require rare earth metals and involve processes that are undesirable for industrial scale-up, such as heating above the Curie temperature or applying large magnetic fields to break ferromagnetic interactions.

Method used

A new synthetic route is developed to produce iron-based hexaferrite permanent magnets using non-ferromagnetic precursors with anisotropic microcrystals, which are aligned through spark plasma sintering or compaction, eliminating the need for undesirable processes and resulting in improved magnetic properties.

Benefits of technology

The method produces rare earth-free magnets with enhanced magnetic properties and fewer process steps, making them suitable alternatives to commercially available counterparts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000027_0000
    Figure 00000027_0000
  • Figure 00000027_0001
    Figure 00000027_0001
  • Figure 00000027_0002
    Figure 00000027_0002
Patent Text Reader

Abstract

The present invention relates to a method for making rare earth-free permanent magnets. Specifically, the type of magnets made by the present invention are iron-based rare earth-free magnets. More specifically, the magnets of the present invention are of the class hexaferrite. The present invention further relates to magnets made by the present method, which are highly aligned magnets with improved magnetic properties compared to commercially available analogs.
Need to check novelty before this filing date? Find Prior Art

Description

Summary of the Invention

[0001] The present invention relates to a method for making rare earth free permanent magnets. Specifically, the type of magnets made by the present invention are iron-based rare earth free magnets. More specifically, the magnets of the present invention are of the class hexaferrite.

[0002] We have discovered a new synthetic route that allows for the production of iron-based non-ferromagnetic precursors that can be converted into hexaferrite permanent magnets. The non-ferromagnetic precursors thus formed contain large fragments of crystallites with platelet or needle-like morphologies and can be converted into permanent magnets either in a one-step process by spark plasma sintering (SPS) or in a two-step process by first compressing the crystalline powder into pellets followed by sintering. By taking advantage of the anisotropic shape of the precursor, we demonstrate that it is possible to align the precursors and promote the alignment of the crystallites that make up the hexaferrite permanent magnets, resulting in a crystallographically preferred orientation that allows for the alignment of individual atomic magnetic dipole moments during the formation of the hexaferrite permanent magnets.

[0003] Equally important to anisotropic morphology is the non-ferromagnetic nature of the precursor, which eliminates domain shorting during the compaction step of the hexaferrite permanent magnet. This step requires heating the precursor above its Curie temperature, or alternatively, applying a large magnetic field to break the ferromagnetic interactions. Both of these processes are undesirable for industrial scale-up, so eliminating them would be beneficial.

[0004] As a result, by utilizing the non-ferromagnetic anisotropic precursor of the present invention, it is possible to produce rare earth-free magnets on an industrially relevant scale that have improved magnetic properties compared to commercially available equivalents. Furthermore, the non-ferromagnetic anisotropic precursor uses significantly fewer process steps compared to conventional synthesis of rare earth-free magnets.

[0005] Detailed Disclosure One aspect of the present invention relates to a non-ferromagnetic strontium hexaferrite precursor comprising anisotropic crystalline materials at a concentration greater than 15 wt. % of the group consisting of hexaferrihydrite (SLF), α-Fe2O3, and / or α-FeOOH, each having an average aspect ratio A / C≧2, a size C in the range of 2-200 nm, and a size A in the range of 4-2000 nm.

[0006] Non-ferromagnetic: By this is understood a chemical substance that has unpaired electrons and that does not exhibit permanent magnetism (i.e., near-zero magnetization under zero applied external magnetic field) within the temperature range relevant to the present disclosure, preferably at room temperature. The terms "non-ferromagnetic" and "non-magnetic" are used interchangeably herein.

[0007] Precursor: By this is understood a chemical substance that may be converted by technological manipulation into a contemplated product. In this case, an iron-containing precursor is converted into a contemplated product that is a strontium hexaferrite permanent magnet. The terms "non-ferromagnetic precursor," "non-magnetic precursor," and "precursor" can be used interchangeably herein.

[0008] Aspect ratio: By this is understood the ratio of the length of the precursor crystal (direction A) to its height (direction C) (see also Figures 2a and 2b). This difference between A and C is what gives the precursor its unique properties in that it promotes the alignment of the crystallites in the final magnet.

[0009] Anisotropic crystallites: By this it is understood that the crystallites are not spherical, i.e., they are platelets, tabular, needle or acicular in shape, and when compressed, all of the crystallites, i.e. substantial fractions of the crystallites, become aligned in the same direction due to differences in aspect ratio (see also aspect ratio above).

[0010] The crystallite aspect ratio of the precursor materials disclosed herein is defined by A / C, which in one embodiment of the present disclosure must be greater than 2. In the synthesis of hexaferrite permanent magnets, preferably strontium hexaferrite permanent magnets, the aspect ratio is important to the present disclosure as it depends on the preferred orientation of the precursor.

[0011] In one embodiment of the present disclosure, the non-magnetic precursor has an average aspect ratio defined by A / C≧2, such as A / C≧5, for example A / C≧10, such as A / C≧25, for example A / C≧50, such as A / C≧100, for example A / C≧1000.

[0012] In one embodiment of the present disclosure, the non-magnetic precursor comprises crystallites having a platelet or platelet-like morphology.

[0013] In one embodiment of the present disclosure, the non-magnetic precursor comprises crystallites having a needle or acicular morphology.

[0014] Just like a deck of cards, if you drop it on the floor, most of the cards will lie flat on top of each other, and only a few can be expected to land on their narrow sides. Similarly, with needles, if you drop a needle on the floor, the long part of the needle will lie flat, parallel to the floor, and it is very unlikely that the needle will stand upright.

[0015] The higher the crystallite aspect ratio of the precursors of the present disclosure (see Figures 2a and 2b), the greater the likelihood that the crystallites will stack in a preferred orientation, which in turn promotes improved magnetic properties.

[0016] In one embodiment of the present disclosure, the average aspect ratio A / C≧2.

[0017] In one embodiment of the present disclosure, the average aspect ratio A / C≧5.

[0018] In one embodiment of the present disclosure, the average aspect ratio A / C≧10.

[0019] In one embodiment of the present disclosure, the average aspect ratio A / C≧25.

[0020] In one embodiment of the present disclosure, the average aspect ratio A / C≧50.

[0021] In one embodiment of the present disclosure, the average aspect ratio A / C≧100.

[0022] In one embodiment of the present disclosure, the average aspect ratio A / C≧1000.

[0023] In one embodiment of the present disclosure, C is in the range of 2 to 200 nm, for example, 200 to 170 nm, for example, 170 to 140 nm, for example, 140 to 110 nm, for example, 110 to 80 nm, for example, 80 to 50 nm, for example, 50 to 30 nm, for example, 30 to 20 nm, for example, 20 to 15 nm, for example, 15 to 10 nm, for example, 10 to 2 nm.

[0024] In one embodiment of the present disclosure, A is in the range of 4 to 2000 nm, for example, 2000 to 1500 nm, for example, 1500 to 1000 nm, for example, 1000 to 500 nm, for example, 500 to 250 nm, for example, 250 to 125 nm, for example, 125 to 50 nm, for example, 50 to 40 nm, for example, 40 to 30 nm, for example, 30 to 20 nm, for example, 20 to 10 nm, for example, 10 to 4 nm.

[0025] In one embodiment of the present invention, the precursor has a concentration of anisotropic crystalline material constituting 100% by weight, for example 100-15% by weight, for example 95-85% by weight, for example 85-75% by weight, for example 75-65% by weight, for example 65-55% by weight, for example 55-45% by weight, for example 45-35% by weight, for example 35-25% by weight, for example 25-15% by weight.

[0026] In one embodiment, the precursor anisotropic crystalline material is predominantly or consists essentially of α-Fe 2 O 3 .

[0027] In one embodiment, the precursor anisotropic crystalline material consists predominantly of or essentially of hexaline ferrihydrite (SLF).

[0028] In one embodiment, the precursor anisotropic crystalline material is predominantly or consists essentially of α-FeOOH.

[0029] In one embodiment, the precursor anisotropic crystalline material is a mixture of goethite (α-FeOOH) and hematite (α-Fe2O3).

[0030] In one embodiment, a mixture of goethite (α-FeOOH) and hematite (α-FeO) is provided in a ratio ranging from 100 / 0 to 0 / 100, respectively. In one embodiment, the ratio of goethite (α-FeOOH) / hematite (α-FeO) is provided as any one of 100 / 0, 90 / 10, 80 / 20, 70 / 30, 60 / 40, 50 / 50, 40 / 60, 30 / 70, 20 / 80, 10 / 90, and 0 / 100, respectively.

[0031] In one embodiment, mixtures of goethite (α-FeOOH) and hematite (α-FeO) are provided in the following compositions: 100% hematite, 75% hematite and 25% goethite, 50% hematite and 50% goethite, 25% hematite and 75% goethite, and 100% goethite.

[0032] In a further embodiment of the present invention, the non-ferromagnetic strontium hexaferrite precursor further comprises a source of one or more metals such as calcium (Ca), strontium (Sr), barium (Ba), magnesium (Mg), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zinc (Zn), and lanthanum (La).

[0033] The nonferromagnetic strontium hexaferrite precursor of the present invention is prepared under autogenous reaction conditions at a maximum temperature of 200°C, as exemplified in Example 1. This approach produces compositions with platelet-like hexaferrihydrite (SLF) crystallites in an amount of at least 15% by weight. A minimum reaction temperature of 100°C yields a minimum percentage of 15% by weight, with the amount increasing with increasing temperature. At 150°C, the amount is 38% by weight, while at 200°C, the amount decreases to 30% by weight. Therefore, by controlling the reaction temperature, it is possible to tailor the amount of SLF. It is also envisioned that, for fixed temperatures, controlling the reaction time can be used to tailor the amount of SLF in the final composition. The same argument applies to compositions containing anisotropic hematite or goethite.

[0034] One aspect of the present invention is a method of making a non-ferromagnetic precursor comprising: a.Fe 3+ with a strong alkaline solution to form a gel; b. transferring the gel to an autoclave and sealing the autoclave; c. placing the autoclave at a temperature in the range of 200-150°C, such as 150-100°C, for example 100°C, under autogenous pressure for more than 1 hour, such as 1-2 hours, for example 2-4 hours, such as 4-8 hours, for example 8-24 hours; d. isolating the formed anisotropic crystalline non-magnetic precursor material; The method includes:

[0035] One embodiment of the present invention is the method as defined above, wherein the alkaline solution is made by dissolving NaOH or KOH in water.

[0036] One embodiment of the present invention is the process as defined above, wherein the reaction temperature is 200°C.

[0037] One embodiment of the present invention is the process as defined above, wherein the reaction temperature is 150°C.

[0038] One embodiment of the present invention is the process as defined above, wherein the reaction temperature is 100°C.

[0039] One embodiment of the present invention is the process as defined above, wherein the reaction temperature is in the range of 100-200°C, for example, 100-110°C, for example, 110-120°C, for example, 120-130°C, for example, 130-140°C, for example, 140-150°C, for example, 150-160°C, for example, 160-170°C, for example, 170-180°C, for example, 180-190°C, for example, 190-200°C.

[0040] One embodiment of the present invention is the process as defined above, wherein the reaction time is 1 hour.

[0041] One embodiment of the present invention is the process as defined above, wherein the reaction time is between 1 and 2 hours.

[0042] One embodiment of the present invention is the process as defined above, wherein the reaction time is between 2 and 4 hours.

[0043] One embodiment of the present invention is the process as defined above, wherein the reaction time is between 4 and 8 hours.

[0044] One embodiment of the present invention is the process as defined above, wherein the reaction time is between 8 and 24 hours.

[0045] One embodiment of the present invention is the process as defined above, wherein the reaction time is more than 1 hour, such as in the range of 1-24 hours, such as 1-2 hours, for example 2-4 hours, such as 4-8 hours, for example 8-24 hours.

[0046] A further embodiment of the present invention is the process as defined above, wherein a source of divalent metal ions such as calcium (Ca), strontium (Sr), barium (Ba), magnesium (Mg), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zinc (Zn), and trivalent lanthanum (La) may optionally be added during step a.

[0047] In one embodiment, the optionally added metal is strontium (Sr).

[0048] In one embodiment, the anisotropic crystalline material of the non-ferromagnetic strontium hexaferrite precursor consists predominantly of or essentially of α-Fe 2 O 3 and has an Fe / Sr ratio of 12.

[0049] In one embodiment, the anisotropic crystalline material of the non-ferromagnetic strontium hexaferrite precursor consists predominantly of or essentially of hexaferrihydrite (SLF) and has an Fe / Sr ratio of 8.

[0050] In one embodiment, the anisotropic crystalline material of the non-ferromagnetic strontium hexaferrite precursor consists predominantly of or essentially of α-FeOOH and has an Fe / Sr ratio of 12.

[0051] In one embodiment, the anisotropic crystalline material of the non-ferromagnetic strontium hexaferrite precursor consists predominantly of or essentially of α-FeOOH and has an Fe / Sr ratio of 10.

[0052] In one embodiment, the anisotropic crystalline material of the non-ferromagnetic strontium hexaferrite precursor consists predominantly of or essentially of α-FeOOH, with an Fe / Sr ratio in the range of 10-12.

[0053] In one embodiment, the anisotropic crystalline material of the non-ferromagnetic strontium hexaferrite precursor is a mixture of goethite (α-FeOOH) and hematite (α-Fe 2 O 3 ), with an Fe / Sr ratio of 12.

[0054] In one embodiment, the anisotropic crystalline material of the non-ferromagnetic strontium hexaferrite precursor is a mixture of goethite (α-FeOOH) and hematite (α-Fe 2 O 3 ), with an Fe / Sr ratio of 10.

[0055] In one embodiment, the anisotropic crystalline material of the non-ferromagnetic strontium hexaferrite precursor is a mixture of goethite (α-FeOOH) and hematite (α-Fe2O3), with an Fe / Sr ratio in the range of 10-12.

[0056] Non-ferromagnetic strontium hexaferrite precursors containing hexaferrihydrite (SLF) In one embodiment of the present invention, the precursor anisotropic crystalline material is hexaline ferrihydrite (SLF).

[0057] One embodiment of the present invention is a method for producing a non-ferromagnetic strontium hexaferrite precursor comprising hexaferrihydrite (SLF), comprising: a.Fe 3+ and Sr 2+ with a strong alkaline solution to form a gel; b. transferring the gel to an autoclave and sealing the autoclave; c. subjecting the autoclave to a temperature in the range of 200-100°C under autogenous pressure for more than 1 hour; d. isolating the formed anisotropic crystalline non-ferromagnetic strontium hexaferrite precursor material comprising hexaferrihydrite (SLF); The method includes:

[0058] In one embodiment of the above method, the alkaline solution is made by dissolving NaOH in water.

[0059] In one embodiment of the above method, the alkaline solution comprises an 8M NaOH solution.

[0060] In one embodiment of the above method, the alkaline solution is added by slow addition, such as dropwise addition.

[0061] In one embodiment of the above process, the reaction time under autogenous pressure is 5 hours.

[0062] In one embodiment of the above-mentioned method, the reaction temperature is in the range of 100 to 200°C, for example, 100 to 110°C, for example, 110 to 120°C, for example, 120 to 130°C, for example, 130 to 140°C, for example, 140 to 150°C, for example, 150 to 160°C, for example, 160 to 170°C, for example, 170 to 180°C, for example, 180 to 190°C, for example, 190 to 200°C.

[0063] In one embodiment of the above method, the reaction temperature is 100°C.

[0064] In one embodiment of the above method, the reaction temperature is 150°C.

[0065] In one embodiment of the above method, the reaction temperature is 200°C.

[0066] In one embodiment of the above method, the Fe 3+ and Sr 2+ The salts are mixed in an Fe / Sr ratio of 8.

[0067] In one embodiment of the above method, the salt used in the above method is nitric acid (NO3) - It's salt.

[0068] In one embodiment of the above method, Fe 3+ The salt is provided in a 3M solution of Fe(NO3)3·9H2O.

[0069] In one embodiment of the above method, Sr 2+ The salt is provided in a 0.75M solution of Sr(NO3)2.

[0070] In one embodiment of the above-described method, the isolated non-ferromagnetic strontium hexaferrite precursor material comprises at least about 15 wt. % hexaferrihydrite (SLF) crystallites having a platelet or platelet-like morphology with an average aspect ratio A / C≧2, a size C in the range of 2-200 nm, and a size A in the range of 4-2000 nm.

[0071] One embodiment of the present disclosure is a non-ferromagnetic strontium hexaferrite precursor material obtainable by the above-described method, comprising at least about 15 wt. % hexaferrihydrite (SLF) crystallites having a platelet or platelet-like morphology with an average aspect ratio A / C≧2, a size C in the range of 2 to 200 nm, and a size A in the range of 4 to 2000 nm.

[0072] Non-ferromagnetic strontium hexaferrite precursor containing hematite (α-Fe2O3) In one embodiment of the present invention, the precursor anisotropic crystalline material is hematite (α-Fe2O3).

[0073] One embodiment of the present invention is a method for producing a non-ferromagnetic strontium hexaferrite precursor comprising hematite (α-FeO), comprising: a.Fe 3+ with a strong alkaline solution to form a mixture containing a dark red precipitate; b. transferring the mixture to an autoclave and sealing the autoclave; c. subjecting the autoclave to a temperature in the range of 200-100°C under autogenous pressure for more than 1 hour; d. isolating the formed anisotropic crystalline non-magnetic precursor material; e. adding a source of strontium (Sr) to the isolated material to obtain a non-ferromagnetic strontium hexaferrite precursor comprising hematite (α-FeO); The method includes:

[0074] In one embodiment of the above-described method, the isolating step d of the method comprises washing the formed anisotropic crystalline non-magnetic precursor material with water to a neutral pH (pH 7), followed by washing with ethanol and drying at 85°C until dry.

[0075] In one embodiment of the above method, the alkaline solution is made by dissolving NaOH in water.

[0076] In one embodiment of the above method, the alkaline solution comprises an 8M NaOH solution.

[0077] In one embodiment of the above method, the reaction temperature is 160°C.

[0078] In one embodiment of the above process, the reaction time under autogenous pressure is 2 hours.

[0079] In one embodiment of the above method, Fe 3+ The salt is provided in a 2M solution of FeCl3·6H2O.

[0080] In one embodiment of the above method, the method comprises an Fe / OH molar ratio of 4.

[0081] In one embodiment of the above method, the source of strontium (Sr) is selected from SrCO3 and Sr(OH)2.

[0082] In one embodiment of the above method, the method comprises an Fe / Sr molar ratio of 12.

[0083] In one embodiment of the above-described method, the isolated non-ferromagnetic strontium hexaferrite precursor material comprises at least about 15 wt. % hematite (α-Fe2O3) crystallites having a platelet or platelet-like morphology with an average aspect ratio A / C≧2, a size C in the range of 2-200 nm, and a size A in the range of 4-2000 nm.

[0084] One embodiment of the present disclosure is a non-ferromagnetic strontium hexaferrite precursor material obtainable by the above-described method, comprising at least about 15 wt. % hematite (α-Fe2O3) crystallites having platelet or platelet-like morphology with an average aspect ratio A / C≧2, a size C in the range of 2-200 nm, and a size A in the range of 4-2000 nm.

[0085] Non-ferromagnetic strontium hexaferrite precursor containing goethite (α-FeOOH) In one embodiment of the present invention, the precursor anisotropic crystalline material is goethite (α-FeOOH).

[0086] One embodiment of the present invention is a method for producing a non-ferromagnetic strontium hexaferrite precursor comprising goethite (α-FeOOH), comprising: a.Fe 3+ with a strong alkaline solution to form a mixture containing a dark red precipitate; b. transferring the mixture to an autoclave and sealing the autoclave; c. subjecting the autoclave to a temperature in the range of 200-100°C under autogenous pressure for more than 1 hour; d. isolating the formed anisotropic crystalline non-magnetic precursor material; e. adding a source of strontium (Sr) to the isolated material to obtain a non-ferromagnetic strontium hexaferrite precursor comprising goethite (α-FeOOH); The method includes:

[0087] In one embodiment of the above method, the pH of the mixture containing the dark red precipitate is maintained at 11 when the mixture is transferred to an autoclave.

[0088] In one embodiment of the above-described method, the isolating step d of the method comprises washing the formed anisotropic crystalline non-magnetic precursor material with water to a neutral pH (pH 7), followed by washing with ethanol and drying at 85°C until dry.

[0089] In one embodiment of the above method, the source of strontium (Sr) is selected from SrCO3.

[0090] In one embodiment of the above method, the method comprises an Fe / Sr molar ratio of 12.

[0091] In one embodiment of the above method, the method comprises an Fe / Sr molar ratio of 10.

[0092] In one embodiment of the above method, the method includes an Fe / Sr molar ratio in the range of 10-12.

[0093] In one embodiment of the above method, the alkaline solution is made by dissolving NaOH in water.

[0094] In one embodiment of the above method, the alkaline solution comprises an 8M NaOH solution.

[0095] In one embodiment of the above method, Fe 3+ The salt is provided in a 1M solution of Fe(NO3)3·9H2O.

[0096] In one embodiment of the above method, the base is 1.33 of [OH - ] / [NO3 - ] ratio was added.

[0097] In one embodiment of the above method, the reaction temperature is 100°C.

[0098] In one embodiment of the above process, the reaction time under autogenous pressure is 10 hours.

[0099] In one embodiment of the above-described method, the isolated non-ferromagnetic strontium hexaferrite precursor material comprises at least about 15 wt. % goethite (α-FeOOH) crystallites having needle or acicular morphology with an average aspect ratio A / C≧2, a size C in the range of 2-200 nm, and a size A in the range of 4-2000 nm.

[0100] One embodiment of the present disclosure is a non-ferromagnetic strontium hexaferrite precursor material obtainable by the above-described method, comprising at least about 15 wt. % goethite (α-FeOOH) crystallites having needle or acicular morphology with an average aspect ratio A / C≧2, a size C in the range of 2 to 200 nm, and a size A in the range of 4 to 2000 nm.

[0101] Strontium Hexaferrite Permanent Magnet The non-ferromagnetic strontium hexaferrite precursor obtained in Example 1 can be converted into a strontium hexaferrite permanent magnet in either a one-step process by spark plasma sintering (SPS), as in Example 4, or a two-step process by first compressing it into a powder followed by sintering, as in Example 5. In either case, the result is a structurally highly ordered permanent magnet, as evidenced by the X-ray diffraction patterns and associated Rietveld analysis seen in Examples 3 and 4.

[0102] One aspect of the present invention relates to a non-magnetic precursor for use in forming a strontium hexaferrite permanent magnet.

[0103] One embodiment of the present invention is a method of making a strontium hexaferrite permanent magnet as defined herein, wherein the anisotropic crystalline material of the non-ferromagnetic strontium hexaferrite precursor is predominantly or consists essentially of α-FeO.

[0104] One embodiment of the present invention is a method of making a strontium hexaferrite permanent magnet as defined herein, wherein the non-ferromagnetic strontium hexaferrite precursor anisotropic crystalline material is predominantly or consists essentially of hexaferrihydrite (SLF).

[0105] One embodiment of the present invention is a method of making a strontium hexaferrite permanent magnet as defined herein, wherein the anisotropic crystalline material of the non-ferromagnetic strontium hexaferrite precursor is predominantly or consists essentially of α-FeOOH.

[0106] One embodiment of the present invention is a method of making a strontium hexaferrite permanent magnet as defined herein, wherein the non-ferromagnetic strontium hexaferrite precursor anisotropic crystalline material is a mixture of goethite (α-FeOOH) and hematite (α-FeO).

[0107] In one embodiment, a mixture of goethite (α-FeOOH) and hematite (α-FeO) is provided in a ratio ranging from 100 / 0 to 0 / 100, respectively. In one embodiment, the ratio of goethite (α-FeOOH) / hematite (α-FeO) is provided as any one of 100 / 0, 90 / 10, 80 / 20, 70 / 30, 60 / 40, 50 / 50, 40 / 60, 30 / 70, 20 / 80, 10 / 90, and 0 / 100, respectively.

[0108] In one embodiment, the mixtures are provided in the following compositions: 100% hematite, 75% hematite and 25% goethite, 50% hematite and 50% goethite, 25% hematite and 75% goethite, and 100% goethite.

[0109] Spark Plasma Sintering (SPS) One aspect of the present invention is a method of making a strontium hexaferrite permanent magnet, comprising: a. providing a non-ferromagnetic strontium hexaferrite precursor as defined herein; b. compressing the precursor by spark plasma sintering (SPS) at a temperature of 700-1000°C in the absence of an applied magnetic field, thereby inducing a phase change; c. isolating the strontium hexaferrite permanent magnet thus formed; The method includes:

[0110] In one embodiment of the above method, the temperature was set at 750° C. and the applied pressure was 100 MPa during the sintering process, which was completed after 8 minutes.

[0111] Cold pressing and firing Another aspect of the present invention is a method of making a strontium hexaferrite permanent magnet, comprising: a. providing a non-ferromagnetic strontium hexaferrite precursor as defined herein; b. applying pressure to compress the precursor; c. calcining the compacted precursor at a temperature of 700-1220°C in the absence of an applied magnetic field, thereby inducing a phase change; d. isolating the strontium hexaferrite permanent magnet thus formed; The method includes:

[0112] In one embodiment of the above method, the pressure applied in the compression step was 700 MPa for 5 minutes.

[0113] In one embodiment of the above method, the compressed precursor was sintered at a temperature of 700-1220°C. In one embodiment, the temperature was 700-800°C. In one embodiment, the temperature was 800-900°C. In one embodiment, the temperature was 900-1000°C. In one embodiment, the temperature was 1000-1100°C. In one embodiment, the temperature was 1100-1220°C.

[0114] In one embodiment of the above method, the sintering temperature was 750°C.

[0115] In one embodiment of the above method, the sintering temperature was 900°C.

[0116] In one embodiment of the above method, the sintering temperature was 1050°C.

[0117] In one embodiment of the above method, sintering was carried out for 2 hours. In one embodiment, the sample was kept in an Al2O3 crucible during sintering.

[0118] Characterization of highly aligned strontium hexaferrite permanent magnets. X-ray powder diffraction is a technique that is highly sensitive to the crystalline structure and spatial orientation of crystallites within a sample.

[0119] The analysis of powder diffractograms obtained from X-ray powder diffraction is based on Bragg's law of diffraction, given by the following relationship:

number

[0120] As demonstrated in Examples 4, 5, and 8, the X-ray diffraction patterns of the synthesized hexaferrite permanent magnets are characterized by a high degree of preferred orientation along the crystallographic (001) reflections, which are significantly more intense than the other reflections.

[0121] One embodiment of the present invention is a strontium hexaferrite permanent magnet as defined herein, further comprising a prominent Bragg reflection along the (001) reflection, as evidenced by powder X-ray diffraction obtained in reflection mode using Co-Kα radiation.

[0122] As already briefly mentioned, a uniform or non-aligned sample is characterized by the Bragg reflection intensity due to crystallites randomly oriented with respect to all mirror indices. The degree of orientation can be assessed by comparing the relative intensities of orthogonal Bragg reflections, e.g., the (00l) reflection corresponding to crystallites lying flat on the surface with the (hk0) reflection corresponding to crystallites standing on their side.

[0123] One embodiment of the present invention is a strontium hexaferrite permanent magnet comprising highly ordered strontium hexaferrite characterized by its strongest Bragg reflections being the (006), (008), (107), and (0014) reflections, and having an integrated intensity ratio (008) / [(110+008)] of at least 0.5 as determined by X-ray powder diffraction using Co-Kα radiation. In one embodiment, the integrated intensity ratio (008) / [(110+008)] is at least 0.6, such as at least 0.7, such as at least 0.8, such as at least 0.9, for example at least 0.95.

[0124] One embodiment of the present invention is a strontium hexaferrite permanent magnet as defined herein, further comprising an X-ray powder diffraction pattern having characteristic peaks expressed in degrees two-theta (°) at: (006) at 2θ=26.9°±0.2°, (110) at 2θ=35.4°±0.2°, (008) at 2θ=36.3°±0.2°, (107) at 2θ=37.7°±0.2°, and (0014) at 2θ=65.8°±0.2°, when obtained using Co-Kα radiation.

[0125] One embodiment of the present invention is a strontium hexaferrite permanent magnet as defined herein, having a powder x-ray pattern substantially similar to that of FIG.

[0126] As there are many examples in the prior art of making hexaferrite permanent magnets from isotropic precursors, this orientation effect is due to the microcrystalline anisotropy of the precursors utilized, with no orientation being observed in the final product.

[0127] Aligning primarily all of the crystallites in a magnetic sample in the same direction also aligns the magnetic moments of the sample in the same direction. Figuratively speaking, this is equivalent to aligning all of the magnetic field lines of small individual magnets in the same direction to achieve a synergistic effect and generate a larger, unidirectional magnetic field. Thus, a magnet constructed in this manner can have superior magnetic properties compared to a non-aligned version of the same magnet, as evidenced in Examples 5, 6, and 8.

[0128] The criterion for evaluating the magnetic properties of a material is to examine the hysteresis behavior of the magnet (see Figure 1). The key parameter that governs the macroscopic magnetic properties of a material is the remanent magnetization (M r ), saturation magnetization (M s ), coercive force field (H c ), and maximum energy product (BH) max All of these can be extracted from the magnetic hysteresis loop.

[0129] When measuring magnetic hysteresis, a sample is exposed to an external magnetic field that increases from zero. Then, as the external magnetic field increases, the magnetization of the sample increases. When the magnetization of the sample no longer increases with the application of larger magnetic fields, the magnetization is said to have saturated. This value is called the saturation magnetization (M s ) The external magnetic field is then reduced back to zero to demagnetize the sample, which reduces the magnetization to some extent. If the magnetization is non-zero at zero applied field (i.e., H=0), this value is called the remanent magnetization (M r ) corresponds to the external magnetic field changing sign and, figuratively speaking, increasing the field in the opposite direction. Since the magnetization of a magnet is non-zero in zero applied field, a negative magnetic field must be applied to make the magnetization zero. The value of this field is the coercive field (H c ) is called

[0130] The alignment of moments within a sample also affects the shape of the magnetic hysteresis loop, as shown in Figure 1. Highly aligned magnets have very perpendicular hysteresis loops, with magnetization and demagnetization events occurring very abruptly as the coercive field value is reached. The less aligned the sample, the smoother the shape of the hysteresis loop. Similarly, the magnetization and demagnetization events will be more gradual. Maximum Energy Product (BH) max is strongly influenced by the shape of the hysteresis loop. As a result, (BH) max To increase r / M s A high degree of perpendicularity defined by is preferred.

[0131] One embodiment of the present invention is a hysteresis squareness ratio (M r / M s and wherein the strontium hexaferrite permanent magnet is a strontium hexaferrite permanent magnet as defined herein, further comprising:

[0132] One aspect of the present invention is a hysteresis squareness ratio (M r / M s and wherein the strontium hexaferrite permanent magnet is a strontium hexaferrite permanent magnet as defined herein, further comprising:

[0133] One embodiment of the present invention is a hysteresis squareness ratio (M r / M s and wherein the strontium hexaferrite permanent magnet is a strontium hexaferrite permanent magnet as defined herein, further comprising:

[0134] One embodiment of the present invention is a hysteresis squareness ratio (M r / M s and wherein the strontium hexaferrite permanent magnet is a strontium hexaferrite permanent magnet as defined herein, further comprising:

[0135] One embodiment of the present invention is a hysteresis squareness ratio (M r / M s and wherein the strontium hexaferrite permanent magnet is a strontium hexaferrite permanent magnet as defined herein, further comprising:

[0136] One embodiment of the present invention is a hysteresis squareness ratio (M r / M s and wherein the strontium hexaferrite permanent magnet is a strontium hexaferrite permanent magnet as defined herein, further comprising:

[0137] One embodiment of the present invention is a hysteresis squareness ratio (M r / M sand wherein the strontium hexaferrite permanent magnet is a strontium hexaferrite permanent magnet as defined herein, further comprising:

[0138] As a result of the enhanced magnetic properties obtained through the use of anisotropic non-magnetic precursors, the highly aligned strontium hexaferrite permanent magnets of the present disclosure are superior to other ferrite materials or NdFe 14 B Demonstrate the potential for widespread and useful use as an alternative to NIB rare earth magnets.

[0139] One embodiment of the present invention is the use of aligned permanent magnets as defined herein as magnetic components in a device.

[0140] In further embodiments of the present disclosure, the device as defined herein is either: a. storage device; b. Generators, c. Stators of electric motors and / or generators d. Audio equipment; e. Magnetic image scanners; f. Magnetic brakes, g. Linear motors, h. Electrodynamic bearings, or i. Magnetic toys. [Brief explanation of the drawings]

[0141] [Figure 1] Typical magnetic M vs. H hysteresis loops for A) a misaligned magnet and B) a highly aligned magnet. Ms, Mr, and Hc are indicated on the figure. [Figure 2] A) Schematic of platelet-shaped crystallites of the non-magnetic precursor, and B) Schematic of needle-shaped crystallites of the non-magnetic precursor. The lengths of A and C are indicated by arrows. [Figure 3] Powder X-ray diffraction pattern of the non-magnetic precursor prepared according to Example 1. The graph also shows the results of a Rietveld refinement performed according to the specifications of Example 1. The Bragg peak index of each component of the Rietveld refinement is shown and marked with an arrow. [Figure 4]TEM images of non-magnetic precursors prepared according to Example 1 at a) 100°C, b) 150°C, and c) 200°C. [Figure 5] Powder X-ray diffraction pattern of the non-magnetic hematite precursor prepared from FeCl3·6H2O according to Example 2. [Figure 6] HR-TEM image showing the plate-like morphology of hematite particles. Some of the crystallites are tilted, which makes them appear dark. Faint goethite needles are also observed in the TEM image. [Figure 7] Powder X-ray diffraction pattern of the non-magnetic goethite precursor prepared according to Example 3. The graph also shows the results of a Rietveld refinement performed according to the specifications of Example 3. Bragg peak indices are shown below the diffraction pattern. [Figure 8] TEM image of the non-magnetic precursor α-FeOOH prepared according to Example 3 at 100 °C for 12 h. [Figure 9] 1 shows the powder X-ray diffraction pattern of a hexaferrite permanent magnet labeled SPS-3 obtained by SPS according to Example 4, with the indices of the associated Bragg reflections. The graph also shows the results of a Rietveld refinement performed according to the specifications of Example 4. The Bragg peak indices are shown below the diffraction pattern. [Figure 10] Powder X-ray diffraction patterns of hexaferrite permanent magnets obtained by compaction and subsequent sintering according to Example 5, with associated Bragg reflection indices. The graph also shows the results of a Rietveld refinement performed according to the specifications of Example 5. Bragg peak indices are shown below each diffraction pattern. The top and bottom samples differ only in the temperature of formation of the non-magnetic precursor. Permanent strontium hexaferrite magnets obtained by either method have the same associated Bragg reflections and Bragg peak indices. [Figure 11] 10 shows the magnetic hysteresis loops of hexaferrite permanent magnets prepared by SPS according to Example 4, labeled SPS-1, SPS-2, and SPS-3, with the Mr and Hc regions expanded. [Figure 12A]4 shows the magnetic hysteresis loop of a hexaferrite permanent magnet prepared by compaction and subsequent sintering according to Example 5. [Figure 12B] 4 shows the magnetic hysteresis loop of a hexaferrite permanent magnet prepared by compaction and subsequent sintering according to Example 5. [Figure 12C] 4 shows the magnetic hysteresis loop of a hexaferrite permanent magnet prepared by compaction and subsequent sintering according to Example 5. [Figure 13] Powder X-ray diffraction pattern of a hexaferrite permanent magnet obtained by compaction and subsequent sintering according to Example 8, with indices of the associated Bragg reflections. The graph also shows the results of a Rietveld refinement performed according to the specifications of Example 8. The Bragg peak indices of each component of the precursor are shown below the respective diffraction pattern. [Figure 14] Magnetic hysteresis loops of hexaferrite permanent magnets prepared by compaction and subsequent firing according to Example 8, with expanded Mr and Hc regions. A) Comparison of magnetic hysteresis for all samples of Example 8 made by either dry mixing (DM) or wet mixing (WM) and compacted at either low pressure (220 MPa) or high pressure (870 MPa). B) Comparison of magnetic hysteresis for aligned hexaferrite sample (WM 870 MPa) and randomly oriented hexaferrite sample. [Example]

[0142] Example 1: Preparation and structural characterization of non-ferromagnetic strontium hexaferrite precursors containing anisotropic crystallites of hexaferrihydrite (SLF) precursor used in the subsequent fabrication of strontium hexaferrite permanent magnets: A solution of 3 M Fe(NO3)3·9H2O and 0.75 M Sr(NO3)2 in an 8:1 molar ratio was co-precipitated by the slow addition of 8 M NaOH to form a gel. After complete addition of the NaOH, the gel was stirred for approximately 3 hours. The gel was then transferred to a 175 ml Teflon-lined steel autoclave and placed in an oven operating at temperatures of 200°C, 150°C, or 100°C for 5 hours. The resulting samples were identified as SLF-200, SLF-150, and SLF-100, depending on their synthesis temperature.

[0143] The precursors were examined by X-ray powder diffraction (Rigaku SmartLab diffractometer, Co-Kα radiation) and analyzed by Rietveld refinement using the FullProf Suite software package, including parameters such as zero-point correction, scale factor, lattice constant, Lorentzian crystallite size parameters Y and SZ, and preferred orientation. XRD patterns of the three precursor samples are shown in Figure 3. The peak profiles were described using the Thompson-Cox-Hastings pseudo-Voigt function. The compositions of the three samples were obtained by Rietveld refinement. From this, the amount of hexameric ferrihydrite (SLF) present in the nonmagnetic precursors was approximately 15, 38, and 30% for SLF-100, SLF-150, and SLF-200, respectively. In the current analysis, the SLF phase was refined based on the Dritts model. SLF-100 showed lower crystallinity compared to SLF-150 and SLF-200, likely due to the lower hydrothermal temperature used in the reaction. Rietveld refinement of the as-synthesized sample yields platelet-shaped crystallites, and an average A length of 11 nm can be extracted compared to a C length of 5.5 nm.

[0144] Transmission electron microscopy (TEM) and spatially resolved elemental analysis of SLF-150 and SLF-200 were recorded on approximately 200 particles on an FEI TALOS F200A TEM microscope operating at 200 kV and analyzed using Gatan software. TEM micrographs confirmed the presence of microscopic platelets present in the as-synthesized particles of SLF-150 and SLF-200 (see Figure 4). Lognormal fits to the sizes extracted from the TEM images yielded particle sizes of A = 23 nm and C = 7 nm at 150 °C and A = 30 nm and C = 8 nm at 200 °C.

[0145] These non-magnetic nanocrystallites do not interact with each other magnetically, so when optimal pressure is applied using cold pressing or spark plasma sintering (SPS), the crystallites can easily align along their planes. Because there is no need to break the magnetic interactions, alignment can be achieved at room temperature. However, SrFe 12 O 19 High temperatures are required for conversion to

[0146] Example 2: Preparation and structural characterization of a non-ferromagnetic precursor containing anisotropic crystallites of hematite (α-Fe 2 O 3 ) for the subsequent preparation of strontium hexaferrite permanent magnets. Hematite (α-FeO) precursors with platelet morphology can be synthesized by a wet chemistry approach described below. Other reagents known to those skilled in the art can be substituted to produce similar hematite microcrystalline precursors.

[0147] Hematite precursor prepared from FeCl3·6H2O: A 60 mL aqueous solution of 2 M FeCl3·6H2O was added dropwise to 60 mL of 8 M NaOH solution while stirring, resulting in the formation of a dark red precipitate upon addition. The precipitate solution was transferred to a Teflon-lined stainless steel autoclave and heated at 160 °C for 2 h. After cooling, the precipitate was washed with deionized water and centrifuged until the supernatant reached a pH of 7. Finally, it was washed once with ethanol, placed in a drying oven at 85 °C until dry, and then crushed with a pestle and mortar. The precursor thus obtained was further utilized in Examples 8 and 10.

[0148] The precursor was examined by X-ray powder diffraction (Rigaku SmartLab diffractometer, Co-Kα radiation) and analyzed by Rietveld refinement using the FullProf Suite software package, including parameters such as zero-point correction, scale factor, lattice constant, Lorentzian crystallite size parameters Y and SZ, and preferred orientation. The XRD pattern of the precursor at 160 °C is shown in Figure 5. The Thompson-Cox-Hastings pseudo-Voigt function was used to describe the peak profile.

[0149] Particle morphology analysis by TEM revealed hexagonal platelets with sizes on the order of 1-2 μm, as shown in Figure 6. The hematite hexagonal platelets are oriented either with the platelet plane parallel to the field of view (bright platelet shapes) or perpendicular (dark elongated shapes). The observed light needles are goethite (α-FeOOH).

[0150] Example 3: Preparation and structural characterization of a non-ferromagnetic precursor containing anisotropic crystallites of goethite (α-FeOOH) for the subsequent preparation of strontium hexaferrite permanent magnets. Fe(NO3) 3· Goethite (α-FeOOH) precursor prepared from 9H2O Prepare 40 mL of 1 M Fe(NO3)3·9H2O solution and add 8 M NaOH solution dropwise to obtain 1.33 [OH - ] / [NO3 -The precipitation ratio was obtained, and a dark red precipitate formed upon addition of NaOH. The precipitate solution was stirred for 1 hour. The precipitate solution was transferred to a Teflon-lined stainless steel autoclave. The pH was maintained at 11. The autoclave was heated at 100°C for 10 hours. Upon cooling, the precipitate was washed using deionized water and centrifuged until the supernatant reached a pH of 7. It was washed once with ethanol, dried at 85°C until dry, and then crushed with a pestle and mortar. The precursor thus obtained was further utilized in Example 10.

[0151] The precursor was examined by X-ray powder diffraction (Rigaku Smart Lab diffractometer, Co-Kα radiation) and analyzed by Rietveld refinement using the FullProf suite software package, including parameters such as zero-point correction, scale factor, lattice constant, Lorentzian crystallite size parameters Y and SZ, and preferred orientation. The XRD pattern of the precursor at 100 °C is shown in Figure 7. The Thomas-Cox-Hastings pseudo-Voigt function was used to describe the peak profile. A TEM image of the goethite sample is shown in Figure 8, clearly revealing the acicular morphology of the crystallites.

[0152] Example 4: Preparation and structural characterization of aligned magnetic M-type strontium hexaferrite using platelet-shaped hexaferrihydrite (SLF) non-ferromagnetic strontium hexaferrite precursor and spark plasma sintering (SPS).

[0153] The nonmagnetic precursor prepared according to Example 1 was compressed into a bulk strontium hexaferrite magnet using spark plasma sintering (SPS). 0.8 g of precursor powder was weighed and placed in a graphite die with an inner diameter of 12.6 mm, then sealed between two graphite punches. Graphite paper (approximately 0.2 μm) was placed between the powder and the graphite die, and between the die and the upper and lower punches. The die was then inserted into the vacuum chamber of an SPS Synthex Inc. 1500 model, Dr. Sinter Lab series spark plasma sintering system. Within the chamber, uniaxial pressure was applied to the punch while a pulsed DC current was applied to the die, sintering the powder contained within. The sintering process, which reached a maximum temperature of 750 °C and a maximum pressure of 100 MPa, was completed after 8 minutes. The die was allowed to cool before the sintered pellet was removed. Finally, the graphite paper attached to the pellet was removed by grinding. The pellets thus produced consisted of aligned M-shaped strontium hexaferrite permanent magnets with a diameter of 12.6 mm and a thickness of approximately 1 mm. The SPS pellets were designated SPS-1, SPS-2, and SPS-3, corresponding to the precursor samples SLF-100, SLF-150, and SLF-200, respectively.

[0154] The SPS pellets were subjected to X-ray diffraction analysis using the same Rietveld parameters as in Example 1. Powder X-ray diffraction patterns collected for the resulting SPS pellets reveal a predominant suppression of the (hk0) Bragg reflection. This suppression of the selective Bragg reflection is due to the crystallographic orientation of the crystallites within the sample, also known as crystallographic preferred orientation or texture, which is due to the anisotropic shape of the crystallites. The anisotropic effect is particularly pronounced in the SPS-3 sample, where nearly complete suppression of reflections other than (001) is observed, as shown in Figure 9. Preferred orientation was implemented in structural modeling of the powder diffraction data using the March-Drassé multiaxial function. According to Rietveld refinement, SPS-3 exhibits the greatest degree of preferred orientation, while SPS-1 exhibits the least. Other relevant physical properties are further summarized in Table 1 below.

[0155] Example 5: Preparation and structural characterization of aligned magnetic M-type strontium hexaferrite using platelet-shaped hexaferrihydrite (SLF) non-ferromagnetic strontium hexaferrite precursor and low-temperature pressing followed by calcination. The precursor powders described in Example 1 were subjected to conventional co-compression, followed by firing of the compressed pellets. Two 0.15 g pellets were prepared for each of the precursor powders SLF-100, SLF-150, and SLF-200 for sintering at 750°C, 900°C, and 1050°C. The pellets were compressed under similar conditions of 2 tons of pressure, equivalent to 700 MPa, for 5 minutes. After compaction into dense pellets, the samples were sintered at 750°C, 900°C, and 1050°C for 2 hours. During sintering, the samples were kept in Al2O3 crucibles. The compressed and sintered pellets (T for precursors) were Hyd (100), T Hyd (150), and T Hyd (200)) was subjected to X-ray diffraction analysis using Rietveld refinement parameters as set forth in Example 1. See Figure 10. Relevant physical properties are further summarized in Table 1 below.

[0156] Example 6: Characterization of magnetic properties in aligned M-type strontium hexaferrite magnets obtained using platelet-shaped hexaferrihydrite (SLF) non-ferromagnetic strontium hexaferrite precursor and spark plasma sintering (SPS). The magnetic properties of the SPS pellets were measured using a Quantum Design Physical Properties Measurement System (PPMS) equipped with a vibrating sample magnetometer (VSM). For the measurements, the SPS pellets were placed in a tubular brass sample holder and held between two quartz rods. The room-temperature magnetic hysteresis loop measured on the SPS compressed pellet is shown in Figure 11 and was measured using a standard experimental setup well known to those skilled in the art.

[0157] The alignment of the crystallites in the magnet is called M r / M sThe magnetic properties of the magnet can also be indirectly assessed based on the hysteresis squareness ratio, defined as: In the Stoner-Wahlfrass model, an ideally aligned magnet exhibits a ratio equal to 1, while completely randomly oriented crystallites reduce to 0.5. Table 2, further below, summarizes this and other important properties of the presented samples.

[0158] Example 7: Characterization of magnetic properties in aligned M-shaped strontium hexaferrite magnets obtained using platelet-shaped hexaferrihydrite (SLF) non-ferromagnetic strontium hexaferrite precursors and cold pressing followed by sintering. As in Example 6, the permanent magnet (T Hyd (100), T Hyd (150), and T Hyd VSM magnetic measurements were performed on the (200) sample, and the magnetic hysteresis loop was extracted (Figure 12). The extracted physical properties are summarized in Table 2 below. [Table 1]

[0159] The parameter G1 is derived from Rietveld refinement and provides a qualitative measure of the preferred orientation of a sample. The smaller the value, the higher the preferred orientation. The value can vary between 1 and 0, with 1 being a randomly oriented sample and 0 being close to a single crystal. Another way to examine the preferred orientation is to examine the integrated area of ​​several characteristic peaks in the diffraction pattern, such as the (110) and (008) peaks. Here, (008) provides information about crystallites oriented parallel to the desired direction, while (110) is the crystal plane perpendicular to the desired direction. The next index quantifies the alignment using (008) / [(110)+(008)], and should be between 1 and 0.5, with 1 representing the most aligned sample.

[0160] M in Table 1 r / M sThe ratios indicate the squareness ratios of the variously prepared samples. For all magnets listed in Table 2, it is clear that the temperature used to prepare the nonmagnetic anisotropic precursor directly affects the hysteresis squareness ratio, with higher synthesis temperatures resulting in squareness ratios closer to 1. This indicates that if the initial nanoparticles synthesized are thin platelets or needles, the synthesis temperature can control the sample configuration.

[0161] (BH) of all samples max When analyzed, SPS-3 was found to have a 33(4)kJ / m 3 In (BH) max The highest value was SPS-2 (27 kJ / m 3 ) and T Hyd (200)(21kJ / m 3 ) were found to be followed by these samples. These samples also exhibit the highest degree of microcrystalline ordering, as evidenced by the G1 and [008 / (008+110)] values.

[0162] The magnetic properties, evaluated by magnetic hysteresis, were similar to those observed in commercial La-Co-free hexaferrite obtained by dry processing [(BH) max =26-29kJ / m 3 Enhanced maximum energy product (BH) of aligned M-type strontium hexaferrite obtained using anisotropic non-magnetic precursors compared to max =33kJ / m 3 showed.

[0163] Example 8: Preparation and structural characterization of aligned magnetic M-type strontium hexaferrite using platelet-shaped hematite (α-Fe2O3) non-ferromagnetic strontium hexaferrite precursor and low-temperature pressing followed by calcination. Different methods of mixing the precursor powder from Example 2 with SrCO3 and Sr(OH)2 were tested. Various pressures were also applied during cold pressing to see their effect on alignment.

[0164] Dry mixing: 4.003 g (50.1 mmol) of the precursor from Example 2 (70 wt% α-FeO ​​and 30 wt% α-FeOOH) was weighed and hand-mixed with 0.619 g (4.18 mmol) of SrCO in an agate pestle and mortar for 15 minutes. A mixing ratio of 1:10 molar ratio of Sr:Fe was used.

[0165] Wet mixing: To avoid grinding due to the influence of the crystallite shape, the precursor material from Example 2 was wet mixed with Sr(OH)2. A mass of 0.476 g (3.91 mmol) of anhydrous Sr(OH)2 was dissolved in 30 mL of deionized water at 85 °C until a homogeneous solution was obtained. 3.750 g (47.0 mmol) of the precursor from Example 2 was added and stirred continuously at 85 °C for 45 minutes. The resulting slurry was poured into a Petri dish and dried overnight at 35 °C on a hot plate. The dried mixture was scraped and ground with a pestle and mortar for 2 minutes. A mixing ratio of 1:10 molar ratio of Sr:Fe was used.

[0166] Cold pressing and firing: Four pellets of 0.4 g each were prepared: two wet-mixed (WM) and two dry-mixed (DM). All pellets were uniaxially cold pressed in a 12.6 mm diameter press die. The low-pressure pellets were pressed at 2.5 tonnes / cm² for 5 minutes, corresponding to a pressure of 220 MPa. 2 The dry-mixed and wet-mixed pellets were named DM220MPa and WM220MPa, respectively. The high-pressure pellets were produced at a pressure of 10 tonnes / cm, which corresponds to 870MPa. 2 The dry-mixed and wet-mixed pellets were designated DM870MPa and WM870MPa, respectively. After being pressed into dense pellets, all samples were sintered at 1100°C for 2 hours. During sintering, the samples were kept in Al2O3 crucibles.

[0167] After compaction and calcination, the pellets were subjected to X-ray diffraction analysis using the same Rietveld parameters as given in Example 4. Powder X-ray patterns collected on the as-sintered pellets reveal a major suppression of the Bragg reflection due to (hk0). Figure 13 shows the powder diffraction pattern. The preferred orientation was refined using the March-Dracey function as previously described. The XRD data reveal a clear preferred orientation of the sample. A summary of the relevant physical properties is further below in Table 3.

[0168] Example 9: Characterization of magnetic properties in a platelet-shaped hematite (α-Fe2O3) non-ferromagnetic strontium hexaferrite precursor and an ordered M-type strontium hexaferrite obtained using low-temperature pressing and subsequent calcination. As in Example 6, VSM magnetic measurements were performed on the permanent magnets obtained in Example 8 (DM220MPa, DM870MPa, WM220MPa, and WM870MPa), and magnetic hysteresis loops were extracted (FIG. 14). The extracted physical properties are summarized in Table 3 below.

[0169] [Table 2]

[0170] Table 3 shows the feasibility and promise of fabricating rare-earth-free permanent magnets with substantially maximum energy product from anisotropic nonmagnetic precursors using a simple two-step process combining cold compaction and subsequent sintering. Such a simple two-step process is easily scalable to large-scale production facilities due to its low cost and ease of handling.

[0171] Example 10: Preparation and structural characterization of aligned magnetic M-type strontium hexaferrite using a non-ferromagnetic strontium hexaferrite precursor mixture of platelet-shaped hematite (α-Fe2O3) and needle-shaped goethite (α-FeOOH) and low-temperature pressing followed by calcination. Different ratios of hematite and goethite were mixed with the corresponding amount of SrCO3. Hematite and goethite were prepared separately as in Examples 2 and 3. The three powders were mixed as in the dry mix in Example 8.

[0172] Five pellets of approximately 0.4 g each were prepared with the following hematite to goethite ratios: 100% hematite, 75% hematite and 25% goethite, 50% hematite and 50% goethite, 25% hematite and 75% goethite, and finally 100% goethite. All pellets were uniaxially cold pressed in a 6 mm diameter die at 10 tonnes / cm, equivalent to 870 MPa. 2 A pressure of 0.05% was applied for 5 minutes. The samples were labeled (100% / 0% hematite / goethite, 75% / 25% hematite / goethite, 50% / 50% hematite / goethite, 25% / 75% hematite / goethite, 0% / 100% hematite / goethite). After being pressed into dense pellets, all samples were fired at 1100 °C for 2 hours. During sintering, the samples were kept in Al2O3 crucibles.

[0173] Example 11: Characterization of magnetic properties in a non-ferromagnetic strontium hexaferrite precursor mixture of platelet-shaped hematite (α-Fe2O3) and needle-shaped goethite (α-FeOOH) and aligned M-type strontium hexaferrite obtained using low-temperature pressing and subsequent calcination Similar to Example 6, VSM magnetic measurements were performed on the permanent magnets obtained according to Example 10 (100% / 0% hematite / goethite, 75% / 25% hematite / goethite, 50% / 50% hematite / goethite, 25% / 75% hematite / goethite, 0% / 100% hematite / goethite). The extracted physical properties are summarized in Table 4 below. [Table 3]

[0174] Table 4 shows the feasibility and promise of fabricating rare-earth-free permanent magnets with substantially maximum energy product from anisotropic nonmagnetic precursors using a simple two-step process combining cold compaction and subsequent sintering. Such a simple two-step process is easily scalable to large-scale production facilities due to its low cost and ease of handling.

[0175] Clause 1 1. A non-ferromagnetic precursor comprising an anisotropic crystalline material at a concentration of more than 15 wt % from the group consisting of hexaline ferrihydrite (SLF), α-Fe2O3, and / or α-FeOOH, each having an average aspect ratio A / C ≥ 2, a size C in the range of 2-200 nm, and a size A in the range of 4-2000 nm. 2. The precursor according to clause 1, wherein the concentration of the anisotropic crystalline material constitutes 100% by weight, for example 15-95% by weight. 3. A precursor according to any of the preceding clauses, wherein the concentration of said anisotropic crystalline material comprises 25 to 75% by weight. 4. The precursor according to any one of clauses 1 to 3, wherein said anisotropic crystalline material is hexaline ferrihydrite (SLF). 5. A precursor according to any one of clauses 1 to 3, wherein the anisotropic crystalline material is α-Fe2O3. 6. The precursor according to any one of clauses 1 to 3, wherein the anisotropic crystalline material is α-FeOOH. 7. The precursor of any preceding clause, further comprising a source of one or more metals such as calcium (Ca), strontium (Sr), barium (Ba), magnesium (Mg), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zinc (Zn), and lanthanum (La). 8. A non-ferromagnetic precursor according to any of the preceding clauses for use in forming a strontium hexaferrite permanent magnet. 9. A method of making a non-ferromagnetic precursor comprising: a.Fe 3+ with a strong alkaline solution to form a gel; b. transferring the gel to an autoclave and sealing the autoclave; c. subjecting said autoclave to a temperature of up to 200°C under autogenous pressure for more than 1 hour; d. isolating the formed anisotropic crystalline non-magnetic precursor material; The method comprising: 10. The method of clause 9, wherein step a may further comprise adding a source of a divalent metal, such as calcium (Ca), strontium (Sr), barium (Ba), magnesium (Mg), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), and zinc (Zn). 11. A method of making a strontium hexaferrite permanent magnet, comprising: a. providing a non-ferromagnetic precursor according to any one of clauses 1 to 7; b. compressing the precursor by spark plasma sintering (SPS) at a temperature of 700-1000°C in the absence of an applied magnetic field, thereby inducing a phase change; c. isolating the M-shaped permanent magnet thus formed; The method comprising: 12. A method of making a strontium hexaferrite permanent magnet, comprising: a. providing a non-ferromagnetic precursor according to any one of clauses 1 to 7; b. applying pressure to compress the precursor; c. firing the compacted precursor at a temperature of 700-1220°C in the absence of an applied magnetic field, thereby inducing a phase change; d. isolating the M-shaped permanent magnet; The method comprising: 13. A method for preparing strontium hexaferrite permanence according to any one of clauses 11-12, wherein the precursor anisotropic crystalline material is predominantly α-Fe2O3. 14. A method for preparing strontium hexaferrite permanganate according to any of clauses 11-12, wherein the precursor anisotropic crystalline material is predominantly hexaferrihydrite (SLF). 15. A method for preparing strontium hexaferrite permanence according to any one of clauses 11-12, wherein the precursor anisotropic crystalline material is predominantly α-FeOOH. 16. A strontium hexaferrite permanent magnet comprising highly aligned strontium hexaferrite characterized by strongest Bragg reflections being the (006), (008), (107), and (0014) reflections, with a (008) / [(110+008)] integrated intensity ratio of at least 0.5 as obtained by X-ray powder diffraction using Co-Kα radiation. 17. A strontium hexaferrite permanent magnet according to clause 16, further comprising a prominent Bragg reflection along said (001) reflection as evidenced by powder X-ray diffraction obtained using Co-Kα radiation. 18. The strontium hexaferrite permanent magnet according to any one of clauses 16 to 17, further comprising an X-ray powder diffraction pattern, when obtained using Co-Kα radiation, having characteristic peaks expressed in 2-theta angles (°) of (006) at 2θ = 26.9° ± 0.2°, (110) at 2θ = 35.4° ± 0.2°, (008) at 2θ = 36.3° ± 0.2°, (107) at 2θ = 37.7° ± 0.2°, and (0014) at 2θ = 65.8° ± 0.2°. 19. A strontium hexaferrite permanent magnet according to any one of clauses 16 to 18, having a powder X-ray pattern substantially similar to that of Figure 9. 20. A hysteresis squareness ratio (M R / M s 20. The strontium hexaferrite permanent magnet according to any one of clauses 16 to 19, further comprising: 21. Hysteresis squareness ratio (M) between 0.85 and 1.0, e.g., between 0.95 and 1.0 r / M s 21. The strontium hexaferrite permanent magnet according to any one of clauses 16 to 20, further comprising: 22. Use of a strontium hexaferrite permanent magnet according to any of the preceding clauses as a magnetic component in a device. 23. The device, a. storage device; b. Generators, c. Stators of electric motors and / or engines; d. Audio equipment; e. Magnetic image scanners; f. Magnetic brakes, g. Linear motors, h. Electrodynamic bearings, or i. Magnetic toys, any one of the uses described in the preceding clause. Clause 2 1. A non-ferromagnetic precursor comprising an anisotropic crystalline material at a concentration of more than 15 wt % from the group consisting of hexaline ferrihydrite (SLF), α-Fe2O3, and / or α-FeOOH, each having an average aspect ratio A / C ≥ 2, a size C in the range of 2-200 nm, and a size A in the range of 4-2000 nm. 2. The precursor according to clause 1, wherein the concentration of the anisotropic crystalline material constitutes 100% by weight, for example 15-95% by weight. 3. A precursor according to any of the preceding clauses, wherein the concentration of said anisotropic crystalline material comprises 25 to 75% by weight. 4. The precursor of any of the preceding clauses, further comprising a source of one or more metals such as calcium (Ca), strontium (Sr), barium (Ba), magnesium (Mg), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zinc (Zn), and lanthanum (La). 5. A non-ferromagnetic precursor according to any of the preceding clauses for use in forming a strontium hexaferrite permanent magnet. 6. A method of making a non-ferromagnetic precursor comprising: a.Fe 3+ with a strong alkaline solution to form a gel; b. transferring the gel to an autoclave and sealing the autoclave; c. subjecting said autoclave to a temperature of up to 200°C under autogenous pressure for more than 1 hour; d. isolating the formed anisotropic crystalline non-magnetic precursor material; The method comprising: 7. The method of clause 6, wherein step a may further comprise adding a source of a divalent metal, such as calcium (Ca), strontium (Sr), barium (Ba), magnesium (Mg), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), and zinc (Zn). 8. A method of making a strontium hexaferrite permanent magnet comprising: a. providing a non-ferromagnetic precursor according to any one of clauses 1 to 4; b. compressing the precursor by spark plasma sintering (SPS) at a temperature of 700-1000°C in the absence of an applied magnetic field, thereby inducing a phase change; c. isolating the M-shaped permanent magnet thus formed; The method comprising: 9. A method of making a strontium hexaferrite permanent magnet comprising: a. providing a non-ferromagnetic precursor according to any one of clauses 1 to 4; b. applying pressure to compress the precursor; c. firing the compacted precursor at a temperature of 700-1220°C in the absence of an applied magnetic field, thereby inducing a phase change; d. isolating the M-shaped permanent magnet; The method comprising: 10. A strontium hexaferrite permanent magnet comprising highly aligned strontium hexaferrite characterized by strongest Bragg reflections being the (006), (008), (107), and (0014) reflections, with a (008) / [(110+008)] integrated intensity ratio of at least 0.5 as obtained by X-ray powder diffraction using Co-Kα radiation. 11. The strontium hexaferrite permanent magnet of clause 10, further comprising a prominent Bragg reflection along the (001) reflection as evidenced by powder X-ray diffraction obtained using Co-Kα radiation. 12. The strontium hexaferrite permanent magnet according to any one of clauses 10 to 11, further comprising an X-ray powder diffraction pattern, when obtained using Co-Kα radiation, having characteristic peaks expressed in two-theta angles (°) of (006) at 2θ = 26.9° ± 0.2°, (110) at 2θ = 35.4° ± 0.2°, (008) at 2θ = 36.3° ± 0.2°, (107) at 2θ = 37.7° ± 0.2°, and (0014) at 2θ = 65.8° ± 0.2°. 13. A hysteresis squareness ratio (M R / M s 13. The strontium hexaferrite permanent magnet according to any one of clauses 10 to 12, further comprising: 14. Hysteresis squareness ratio (M) between 0.85 and 1.0, e.g., between 0.95 and 1.0 r / M s 14. The strontium hexaferrite permanent magnet according to any one of clauses 10 to 13, further comprising: 15. Use of a strontium hexaferrite permanent magnet according to any of the preceding clauses as a magnetic component in a device.

Claims

1. A strontium hexaferrite permanent magnet comprising highly ordered strontium hexaferrite characterized by strongest Bragg reflections being the (006), (008), (107), and (0014) reflections, with an integrated intensity ratio (008) / [(110+008)] of at least 0.5 as determined by X-ray powder diffraction using Co-Kα radiation.

2. 2. The strontium hexaferrite permanent magnet of claim 1, characterized by a prominent Bragg reflection along the (001) reflection as evidenced by powder X-ray diffraction obtained using Co-Kα radiation.

3. 3. The strontium hexaferrite permanent magnet of claim 1 or claim 2, characterized in that it comprises an X-ray powder diffraction pattern having characteristic peaks expressed in degrees two theta at: (006) at 2θ = 26.9° ± 0.2°, (110) at 2θ = 35.4° ± 0.2°, (008) at 2θ = 36.3° ± 0.2°, (107) at 2θ = 37.7° ± 0.2°, and (0014) at 2θ = 65.8° ± 0.2°, when obtained using Co-Kα radiation.

4. The strontium hexaferrite permanent magnet according to claim 1, characterized in that the hysteresis squareness ratio (Mr / Ms) is 0.65 to 1.

0.

5. The strontium hexaferrite permanent magnet according to claim 1, characterized in that the hysteresis squareness ratio (M r / M s ) is 0.85 to 1.

0.

6. The strontium hexaferrite permanent magnet according to claim 1, characterized in that the hysteresis squareness ratio (M r / M s ) is 0.90 to 1.

0.

7. Use of a strontium hexaferrite permanent magnet according to any one of claims 1 to 6 as a magnetic component in a device.