Rubber composition for cover rubber and conveyor belt

JP2024012526A5Inactive Publication Date: 2024-10-29BANDO CHEM IND LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023189511
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2016-08-08
Filing Date
2023-11-06
Publication Date
2024-10-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional conveyor belts lack adequate heat resistance, flame retardancy, and abrasion resistance, making them insufficient for demanding applications.

Method used

A rubber composition for the cover layer of conveyor belts comprising ethylene-propylene rubber (EPR) with a specified ratio of brominated flame retardant, along with specific additives and crosslinking agents, enhances heat resistance, flame retardancy, and abrasion resistance.

Benefits of technology

The composition provides conveyor belts with excellent flame retardancy, abrasion resistance, and heat resistance, ensuring durability and safety in various applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

To provide a rubber composition capable of allowing a conveyor belt to exhibit characteristics excellent in flame retardancy, abrasion resistance, and heat resistance, and to provide a conveyor belt excellent in strength, flame retardancy, abrasion resistance, and heat resistance.SOLUTION: A rubber composition for a cover rubber is used for forming a cover rubber layer of a conveyor belt and contains a rubber and a bromine-based flame retardant, the bromine-based flame retardant is contained so that the mass of bromine is 10 pts.mass or more and 35 pts.mass or less relative to 100 pts.mass of the rubber and the main component of the rubber is ethylene-propylene rubber (EPR).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a rubber composition used to form a cover rubber layer of a conveyor belt, and a method for manufacturing the same. and a conveyor belt having a cover rubber layer formed from the composition. [Background technology]

[0002] Belt conveyors have been widely used as devices for transporting goods and the like. Conveyor belts, which are a main component of a conveyor, are known in various forms. The conveyor belt is made of a belt body made of a long belt processed into an endless belt. In addition to the above, there are also belts having horizontal bars extending in the width direction of the belt body. Conventionally, a widely known type has a lug provided along the side edge of the main body. As the conveyor belt, the belt body formed from a rubber composition is widely used. For example, a traction layer with canvas or steel cord is placed between two cover rubber layers. The type that is sandwiched between the two is widely used.

[0003] The rubber composition used to form the cover rubber layer of the conveyor belt usually has strength and Abrasion resistance is required. In addition, depending on the application, a conveyor belt may be required to be flame retardant. In this case, a flame retardant is blended into the rubber composition for the conveyor belt (see Patent Document 1 below). reference). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2012-092182 A Summary of the Invention [Problem to be solved by the invention]

[0005] The cover rubber layer of the conveyor belt may be required to have even better heat resistance. do. However, in the field of conveyor belts, heat resistance as well as wear resistance and flame retardancy are also required. A rubber composition that achieves the desired level has not yet been found. Therefore, conventional conveyor belts do not meet these requirements for the cover rubber layer (wear resistance, However, it is difficult to fully satisfy the requirements for flame retardancy and heat resistance.

[0006] The present invention aims to solve the above problems, and has the following features: flame retardancy, abrasion resistance, And a rubber composition capable of providing excellent heat resistance to a conveyor belt. This provides a conveyor belt that is excellent in strength, flame retardancy, abrasion resistance, and heat resistance. The challenge is to provide [Means for solving the problem]

[0007] The present inventors have conducted extensive research to solve the above problems, and have found that A specific rubber is used for the rubber, and a brominated flame retardant is contained in the rubber at a specified ratio. The present invention has been completed based on the discovery that the above-mentioned needs can be satisfied by .

[0008] That is, the rubber composition for cover rubber of the present invention is used for forming a cover rubber layer of a conveyor belt. A rubber composition for a cover rubber is provided, the rubber composition comprising a rubber and a brominated flame retardant, The mass of the bromine in the flame retardant is 10 parts by mass or more and 35 parts by mass or less per 100 parts by mass of the rubber. The main component of the rubber is ethylene-propylene rubber (EPR). do.

[0009] In order to solve the above problems, the present invention provides a traction layer and a traction material provided on at least one side of the traction layer. and a cover rubber layer formed thereon, The present invention provides a conveyor belt comprising the above-mentioned rubber composition for cover rubber. Effect of the Invention

[0010] According to the present invention, a conveyor belt having excellent properties in terms of flame retardancy, abrasion resistance, and heat resistance is provided. It is possible to provide a rubber composition capable of exhibiting the desired properties. Therefore, according to the present invention, a composite material having excellent properties such as flame retardancy, abrasion resistance, and heat resistance is provided. A bear belt may be provided. [Brief description of the drawings]

[0011] [Figure 1] 1 is a schematic cross-sectional view showing a structure of a conveyor belt according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Preferred embodiments of the present invention will now be described. In this example, only the belt body is considered, which is a flat, long belt processed into an endless belt. The present invention will be described taking as an example a conveyor belt that does not have cross rails or lug rails. FIG. 1 is a diagram showing a conveyor belt according to the present embodiment, in which the belt body is arranged perpendicular to its longitudinal direction. FIG. 2 is a schematic cross-sectional view taken along a virtual plane.

[0013] As shown in this figure, the conveyor belt according to this embodiment has three layers in the thickness direction. The belt body has a laminated structure. Specifically, the belt body 1 of this embodiment has a traction layer 20 between two cover rubber layers 10. is inserted. In other words, the belt body 1 of this embodiment has the cover rubber layer 1 on both the front and back sides of the traction layer 20. 0 is stacked. The belt body 1 of the conveyor belt in this embodiment has an outer circumferential surface (surface) on which conveyed objects are placed. The upper cover rubber layer 10a forms the inner circumferential surface (rear surface side), and the lower cover rubber layer 10b forms the inner circumferential surface (rear surface side). The traction layer 20 between the two cover rubber layers 10b is made of canvas. In this embodiment, the canvas and the cover rubber layer are bonded with an adhesive rubber (not shown). It is glued by.

[0014] The upper cover rubber layer 10a and the lower cover rubber layer of the conveyor belt in this embodiment The layer 10b is formed of a crosslinked rubber having excellent flame retardancy, abrasion resistance, and heat resistance. and a flame retardant. The rubber composition for the cover rubber forming the cover rubber layer (hereinafter, also referred to simply as "rubber composition") The main component of these rubbers is ethylene-propylene rubber (EPR). The rubber composition contains a brominated flame retardant as the flame retardant. Furthermore, the rubber composition contains an inorganic filler, a crosslinking agent, and the like.

[0015] The ethylene-propylene rubber (EPR) in the rubber composition of the present embodiment is a rubber made of ethylene and It is a polymer made up of propylene and ethylidene norbornene, 1,4-hexa Does not contain diene or diene monomers such as dicyclopentadiene as structural units It is something. In this way, the structural units do not contain diene monomers and double bonds are not actively introduced into the main chain. The low-temperature ethylene-propylene rubber (EPR) provides excellent heat resistance to the cover rubber layer. It is effective in making the Therefore, in this embodiment, rubber other than ethylene-propylene rubber (EPR) is used. It is preferable to keep the content of any substances that may be contained in the rubber composition as small as possible.

[0016] Other rubbers that can be included in the rubber composition besides ethylene-propylene rubber (EPR) include: For example, ethylene-propylene-diene rubber (EPDM), natural rubber (NR), butadiene Rubber (BR), Styrene-butadiene rubber (SBR), Polyisoprene rubber (IR), Acrylonitrile-butadiene rubber (NBR), isobutylene-isoprene rubber (IIR ), chloroprene rubber (CR), chlorosulfonated polyethylene (CSM), chlorinated butyrate butyl rubber (CIIR), brominated butyl rubber (BIIR), silicone rubber (SR), urethane Examples include rubber (UR) and fluororubber (FR).

[0017] In this embodiment, the ethylene-propylene rubber accounts for the entire rubber contained in the rubber composition. The proportion of the ethylenediaminetetraacetate (EPR) is preferably 90% by mass or more, and more preferably 95% by mass or more. It is more preferable that the content is 99% by mass or more, and particularly preferable that the content is 99% by mass or more. The rubber composition contains substantially only ethylene-propylene rubber (EPR). is most preferred. In other words, rubber other than the ethylene-propylene rubber (EPR) as described above is The proportion of the total rubber in the composition is preferably 10% by mass or less, and more preferably 5% by mass or less. It is more preferably equal to or less than 1 mass %, and particularly preferably equal to or less than 1 mass %. The rubber composition is a rubber other than the above-mentioned ethylene-propylene rubber (EPR). It is most preferable that the composition is substantially free of

[0018] The brominated flame retardant is an effective component for imparting excellent flame retardancy to the cover rubber layer. It is. In addition, when considering imparting the same flame retardancy to the cover rubber layer, red phosphorus-based flame retardants and metallic water Bromine-based flame retardants provide superior abrasion resistance to the cover rubber compared to oxide-based flame retardants. This will be advantageous. However, if an excessive amount of bromine-based flame retardants is mixed in, the wear resistance of the cover rubber layer decreases. Cause. Therefore, the rubber composition of the present embodiment has a ratio of bromine-based flame retardant to 100 parts by mass of rubber of 1 It is between 5 parts by mass and 50 parts by mass. The reason why the ratio is 15 parts by mass or more is that the cover rubber layer exhibits excellent flame retardancy. This is because. Therefore, the ratio is preferably 18 parts by mass or more, and more preferably 20 parts by mass or more. More preferably, the content is 25 parts by mass or more, and particularly preferably 25 parts by mass or more. On the other hand, the reason why the ratio is 50 parts by mass or less is that the cover rubber layer has excellent abrasion resistance. This is to enable it to perform to its full potential. Therefore, the ratio is preferably 45 parts by mass or less and 40 parts by mass or less. more preferably, and particularly preferably 35 parts by mass or less. It is particularly preferable that said proportion is less than 30 parts by weight.

[0019] The bromine-based flame retardant preferably has a bromine content, which is an active ingredient, of at least a certain level. Specifically, the bromine-based flame retardant preferably contains 50% by mass or more of bromine. It is more preferable that the content of the inorganic filler is 60 mass % or more. The bromine content in the brominated flame retardant is usually 90 mass % or less. The bromine-based flame retardant is added to the rubber composition so that the content of bromine, which is an active ingredient, is a predetermined ratio. The amount of ingredients added has been adjusted. Specifically, the brominated flame retardant is a flame retardant having a total mass of bromine contained therein of The rubber is contained in an amount of 10 parts by mass or more per 100 parts by mass of the rubber, and 12 parts by mass or more It is preferable that the content exceeds 1.0. The bromine-based flame retardant is a flame retardant having a total mass of bromine of 100% by mass of the rubber. The content is 35 parts by weight or less, and less than 30 parts by weight. It is preferable that the composition is contained in the above-mentioned compound. The total mass of bromine in the brominated flame retardant is 25 parts by mass or less per 100 parts by mass of the rubber. It is more preferable that the content be such that

[0020] The rubber composition in this embodiment contains one or more brominated flame retardants. Examples of the bromine-based flame retardant include decabromodiphenyl oxide and octabromodiphenyl oxide. Phenyl oxide, tetrabromo diphenyl oxide, tetrabromo phthalic anhydride, Tetrabromophthalate ester, hexabromocyclododecane, bis(pentabromophthalate) phenyl)ethane, 1,2-bis(2,4,6-tribromophenoxy)ethane, 2,4, 6-Tris(2,4,6-tribromophenoxy)-1,3,5-triazine, 2,4- Dibromophenol and its polymers, 2,6-dibromophenol and its polymers, Brominated polystyrene and its polymers, ethylene bis tetrabromophthalimide, hexa Bromocyclodecane, hexabromobenzene, pentabromobenzyl acrylate and others and the like. The rubber composition of the present embodiment is used for the cover rubber layer to have excellent heat resistance at a temperature of 300°C. It is preferable that the flame retardant contains a bromine-based flame retardant having a melting point of 330°C or higher. It is more preferable that the composition contains a halogen-based flame retardant. The melting point of the brominated flame retardant is particularly preferably 400° C. or higher. The melting point of the brominated flame retardant is determined, for example, by a DSC method (heating rate: 10° C. / min). It can be done. The melting point of brominated flame retardants is usually 500°C or lower. In the rubber composition of the present embodiment, a part or all of the brominated flame retardant has a high melting point as described above. It may be. It is preferable that 90% by mass or more of the brominated flame retardant has a high melting point as described above. The proportion of the high melting point brominated flame retardant is more preferably 95% by mass or more, and more preferably 99% by mass or more. % or more is even more preferable.

[0021] The rubber composition of the present embodiment is effective in providing the cover rubber layer with excellent heat resistance and abrasion resistance. As bromine-based flame retardants, bis(pentabromophenyl)ethane and ethylenebistetrabromo It is preferable that the copolymer contains at least one of the following mophthalimides: The proportion of bis(pentabromophenyl)ethane and ethylene in the brominated flame retardants contained in rubber compositions The total ratio of tetrabromophthalimide and tetrabromophthalimide is preferably 90 mass% or more, It is more preferable that the content is 95% by mass or more.

[0022] The rubber composition of the present embodiment may further contain a flame retardant assistant such as antimony trioxide. preferable. The antimony trioxide alone does not exhibit much flame retardancy, and when combined with the organic bromine compound, When used in combination, they provide a flame retardant effect. More specifically, antimony trioxide (Sb2O3) promotes the radical scavenging function of bromine. At the same time, the organic bromine compound reacts with the gas to generate water vapor, which is used to supply oxygen to the combustion material. This has the effect of cutting off the supply.

[0023] In this embodiment, in order to reliably exert the above-mentioned effect, the antimony trioxide is It is preferable that the rubber composition contains the compound in an amount of 1 part by mass or more per 100 parts by mass of the rubber. It is preferable that the rubber composition contains the fluorine-containing polymer in an amount of 2 parts by mass or more, and more preferably 2 parts by mass or more. The antimony trioxide is added in a proportion of 15 parts by mass or less relative to 100 parts by mass of the rubber. It is preferable that the rubber composition contains the fluorine-containing compound, and the rubber composition contains the fluorine-containing compound in an amount of 10 parts by mass or less. It is more preferable to make it so.

[0024] In addition, it acts in conjunction with antimony trioxide to make rubber and plastics flame-retardant. Chlorinated paraffins and the like are known as organic chlorine compounds that exhibit this effect. Here, the organic chlorine compound such as chlorinated paraffin is used to improve the flame retardancy of the rubber composition. While it is useful in the field, it can cause a decrease in heat resistance. Therefore, in the rubber composition of the present embodiment, an organic chlorine compound such as chlorinated paraffin is used. It is preferable to refrain from using Specifically, the rubber composition has a content of organic chlorine compounds (chlorinated paraffin, etc.) of the above rubber. It is preferable that the content of the chlorinated paraffin is 5 parts by mass or less per 100 parts by mass of the rubber. It is particularly preferable that the compound is not contained in the above.

[0025] In addition to the above, water can also be used as a material for imparting flame retardancy to a rubber composition. Inorganic fillers based on metal hydroxides such as aluminum oxide and magnesium hydroxide are known. There are. Although these are effective in improving the flame retardancy of the cover rubber layer, such inorganic fillers If a filler is contained, the abrasion resistance of the cover rubber layer may decrease. In the rubber composition of the present embodiment, the addition of these compounds provides the advantages of flame retardancy and wear resistance. Considering the disadvantages of wear and tear, the disadvantages may outweigh the advantages. The decrease in abrasion resistance is due to the presence of aluminum hydroxide, which acts as a flame retardant. In addition to inorganic fillers such as silica and magnesium hydroxide, calcium carbonate, talc, clay, etc. The same can be said for inorganic fillers such as silica that act as reinforcing agents. In addition, carbon black and other rubber-reinforcing materials have a particularly excellent effect. For those that are not likely to reduce the abrasion resistance of the cover rubber layer by adding them, Rather, the addition of such an element is expected to improve the abrasion resistance of the cover rubber layer. Therefore, the rubber composition of the present embodiment contains carbon black as a filler. However, it is preferable to reduce the content of fillers other than carbon black as much as possible. I wish. Specifically, the rubber composition of the present embodiment contains carbon black, and The content of fillers other than carbon black per 100 parts by mass is 20 parts by mass or less. It is preferred. The content of fillers other than carbon black is 15 parts by mass or less per 100 parts by mass of rubber. More preferably, it is 10 parts by mass or less, and even more preferably, it is 5 parts by mass or less. It is particularly preferred that:

[0026] The carbon black is contained in an amount of 20 parts by mass or more per 100 parts by mass of rubber. It is preferable that the rubber composition contains the fluorine-containing compound so that the content of the fluorine-containing compound is 30 parts by mass or more. It is more preferable that the rubber composition contains 40 parts by mass or more of the above-mentioned rubber composition. It is particularly preferable that the rubber composition contains the above-mentioned polyether ether. The carbon black is contained in an amount of 100 parts by mass or less per 100 parts by mass of rubber. It is preferable that the amount of the rubber composition be 90 parts by mass or less. It is more preferable that the rubber composition contains the above-mentioned fluorine-containing rubber in an amount of 80 parts by mass or less. It is particularly preferable that the rubber composition contains the above-mentioned polyether ether copolymer.

[0027] In the rubber composition according to the present embodiment, the carbon black is ASTM D 17 Carbon dioxide with an average particle size of 28 nm to 36 nm, classified as "N330" in 65 It is preferable to employ high-availability fluorine-containing polymer (HAF).

[0028] The rubber composition of the present embodiment is a rubber composition for crosslinking the ethylene-propylene rubber (EPR). It contains a cross-linking agent for this purpose. In the crosslinking reaction of the ethylene-propylene rubber (EPR), the propylene structure portion This results in proton abstraction from the tertiary carbon at In ethylene-propylene rubber (EPR), this proton abstraction creates crosslinking points and Since radicals that cause crosslinking are generated and molecular scission due to β-cleavage occurs easily, it is difficult to adjust the degree of crosslinking. difficult. Therefore, it is easy to adjust the degree of crosslinking when the crosslinking agent is contained in the rubber composition. In this respect, sulfur-based crosslinking agents are advantageous. In addition, from the viewpoint of the material cost of the rubber composition, sulfur-based crosslinking agents are more cost-effective than organic peroxide-based crosslinking agents. This is advantageous compared to other agents. Furthermore, a sulfur-based crosslinking agent is also used to provide flexibility to the cover rubber layer. is more advantageous than the organic peroxide crosslinking agents. However, in this embodiment, the cover rubber layer can exhibit excellent heat resistance. Therefore, it is preferable to use an organic peroxide-based crosslinking agent as the crosslinking agent. That is, in the present embodiment in which the heat resistance of the cover rubber layer is important, a sulfur-based crosslinking agent is used. It can be said that organic peroxide-based crosslinking agents are more suitable than these. The rubber composition of the present embodiment contains an organic co-crosslinking agent together with the organic peroxide crosslinking agent. It is preferable to include it. In this embodiment, the ethylene-propylene copolymer crosslinked with the organic peroxide crosslinking agent is The pyrene rubber (EPR) preferably contains many propylene units which become crosslinking points. Furthermore, in this embodiment, ethylene-propylene rubber (EPR) is used instead of a sulfur-based crosslinking agent. Since the ethylene-propylene rubber (EPR) is crosslinked with an organic peroxide crosslinking agent, It is preferable that the elasticity is low to some extent. Specifically, the ethylene-propylene rubber (EPR) has a propylene unit ratio of 3 5% to 60% by mass (ethylene content: 40% to 65% by mass) It is preferable that: The ethylene-propylene rubber (EPR) has a propylene unit ratio of 40% by mass or more. It is more preferable that the content is 45 mass % or more, and particularly preferable that the content is 45 mass % or more. The ethylene-propylene rubber (EPR) is JIS K6300-1:201 3. Unvulcanized rubber - Physical properties - Part 1: Determination of viscosity and scorch time by Mooney viscometer The Mooney viscosity (ML(1+4)) at 100°C measured according to the "Method of Measurement" is 60 or less. It is preferable that the ratio is 50 or less, more preferable that the ratio is 45 or less. It is nice. In addition, ethylene-propylene rubber (EPR) has a certain degree of resilience in the cover rubber layer. It is preferable that the Mooney viscosity (ML(1+4)100℃) is 30 or more. It is preferable that there is. In addition, when a rubber composition contains multiple types of ethylene-propylene rubber, A mixture of ethylene-propylene rubber blended in the same ratio as that contained in the rubber composition. It is preferable that the propylene content and Mooney viscosity of the copolymer are within the above ranges.

[0029] As the organic peroxide contained in the rubber composition as a crosslinking agent, for example, di-t-b Chill peroxide, dicumyl peroxide, t-butylcumyl peroxide, 1, 1-t-Butylperoxy-3,3,5-trimethylcyclohexane, 2,5-dimethyl -2,5-di-(t-butylperoxy)hexane, 2,5-dimethyl-2,5-di-t -butylperoxy)hexyne-3, Bis(t-butylperoxy-diisopropyl)be benzene, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, t-butyl Peroxybenzoate, t-butylperoxy-2-ethyl-hexyl carbonate, etc. Some examples include: The rubber composition of the present embodiment contains one kind of organic peroxide-based crosslinking agent alone. It may contain one or more types. The organic peroxide crosslinking agent of the present embodiment is preferably dicumyl peroxide. .

[0030] The organic co-crosslinking agent has multiple highly reactive functional groups, such as (meth)acrylic groups, in one molecule. It is an organic compound that suppresses the β-cleavage of ethylene-propylene rubber (EPR) while crosslinking. It is effective in improving bridge density. The rubber composition may contain one or more organic co-crosslinking agents. Examples of organic co-crosslinking agents suitable for inclusion in the rubber composition of the present embodiment include ethylene glycol, ethylenediaminetetraacetate ... ethylene glycol dimethacrylate, triethylene glycol dimethacrylate, tetraethylene glycol Ethylene glycol dimethacrylate, polyethylene glycol dimethacrylate, trimethacrylate (Meth)acrylic group-containing organic compounds such as methylolpropane trimethacrylate; Allyl cyanurate, diallyl fumarate, diallyl phthalate, tetraallyloxyethene (Meth)allyl groups such as triaryl isocyanurate, trimethallyl isocyanurate, etc. Organic compounds containing N,Nm-phenylenedimaleimide, maleimide, phenylmaleimide and maleimide group-containing organic compounds such as dimethylaminoethyl ether. The organic co-crosslinking agent in this embodiment is a methacrylic acid having a plurality of methacrylic groups in the molecule. It is preferably a group-containing organic compound.

[0031] The organic peroxide crosslinking agent contained in the rubber composition is a ratio based on 100 parts by mass of rubber. It is preferable that the rubber composition contains 0.5 parts by mass or more of the carboxylic acid ester. It is more preferable that the rubber composition contains the fluorine-containing polymer so that the above-mentioned formula is satisfied. The ratio of organic peroxide crosslinking agent to 100 parts by mass of rubber is 10 parts by mass or less. is preferable, and 5 parts by mass or less is more preferable.

[0032] The organic co-crosslinking agent contained in the rubber composition is in a ratio of 0.5 to 100 parts by mass of rubber. It is preferable that the rubber composition contains the silsesquioxane in an amount of 1 part by mass or more, and more preferably 1 part by mass or more. It is more preferable that the rubber composition contains the above-mentioned polyvinyl chloride. The ratio of the organic co-crosslinking agent to 100 parts by mass of rubber is preferably 10 parts by mass or less. It is preferably 5 parts by mass or less.

[0033] The rubber composition of the present embodiment may further contain components other than those described above. For example, For example, rubber compounding agents that are compounded in general rubber compositions may be used as other components in the present embodiment. The rubber composition may be contained in the above-mentioned form. Examples of the compounding agents for rubber include hardness adjusters such as paraffin oil; amine-ketones; Ton compounds, aromatic secondary amine compounds, benzimidazole compounds, special waxes anti-aging agents such as stearate; and processability improvers such as lubricants, peptizers, and scorch inhibitors. do.

[0034] The rubber composition of the present embodiment may contain zinc oxide to aid vulcanization. preferable. The zinc oxide is added in an amount of 1 part by mass or more and 10 parts by mass or less per 100 parts by mass of rubber. It is preferable that the rubber composition contains the above-mentioned polyvinyl chloride. The mineral oil is contained in an amount of more than 0 parts by mass and less than 30 parts by mass per 100 parts by mass of rubber. In this case, it is preferable that the rubber composition contains the above-mentioned fluorine-containing compound in an amount of 5 parts by mass or more and 25 parts by mass or less. It is preferable that the rubber composition contains the above-mentioned component (A) so that the above-mentioned component (A) is satisfied.

[0035] The conveyor belt is made up of the upper cover rubber layer 10a and the lower cover rubber layer 10b. A common rubber composition may be used for forming the two, or each may be formed from a different rubber composition. It may be formed. In addition, the upper cover rubber layer 10a and the lower cover rubber layer 10b may have different thicknesses. It may be passed through.

[0036] The canvas for forming the traction layer 20 is not particularly limited, and may be any ordinary canvas. The same materials as those used in conveyor belts can also be used in this embodiment. Moreover, the traction layer 20 may be formed using steel cords instead of canvas.

[0037] Furthermore, the adhesive rubber is not particularly limited and can be used for general conveyor belts. The above-mentioned method can be used in this embodiment.

[0038] The conveyor belt of the present embodiment is not particularly limited in its manufacturing method, and may be manufactured by a general method. The conveyor belt can be manufactured in the same manner as a conveyor belt. The conveyor belt may be, for example, a Banbury mixer, a kneader mixer, an open row mixer, or the like. After kneading the rubber composition for the cover rubber using a calender or the like, the rubber composition is The composition was formed into a sheet to prepare an unvulcanized sheet for cover rubber, and the adhesive rubber was applied to the surface. It can be manufactured by vulcanizing and integrating the canvas and the unvulcanized sheet.

[0039] In this embodiment, the rubber composition for the cover rubber is used only for the cover rubber layer. It is not necessary to use this, and it may be used to form adhesive rubber, ear rubber, etc. In this embodiment, a cover rubber layer is provided on both sides of the traction layer. However, the cover rubber layer formed from the rubber composition for the cover rubber of this embodiment is at least It is sufficient that the insulating layer is provided on one side of the body layer. In this embodiment, the conveyor belt has only a flat belt-shaped main body. The example shows a heat press with unevenness on the press surface. Conveyor belts with a three-dimensional shape on the belt body itself, or a flat belt body with a lateral The conveyor belt of the present invention also includes a type in which the crosspieces and the edge crosspieces are attached as separate parts. This is within the scope of what is intended as a belt. In the case of a conveyor belt having a cross bar or an edge bar, the conveyor belt rubber of the present invention is It is also possible to use a rubber composition for forming the crosspieces and the lugs. EXAMPLES

[0040] The present invention will be described in more detail below with reference to examples of the present invention, but the present invention is not limited thereto. It is not something that is done.

[0041] (Materials used) Table 1 below shows the abbreviations of the raw materials used in the evaluation and their specific details. [Table 1]

[0042] A vulcanized rubber sheet was produced using a rubber composition containing the above-mentioned raw materials in the blending ratio shown in Table 2. The vulcanized rubber sheets were then subjected to various evaluations.

[0043] (Rating 1: Heat resistance) Rubber sheets for evaluation were prepared using the compounding content shown in Table 2 and subjected to JIS K6251 "Vulcanized rubber and In accordance with the "Method of Determining Tensile Properties of Thermoplastic Rubber and Thermoplastic Rubber" The "elongation at break" (break elongation: unit: %) was measured using three micrometer-sized test pieces (n=3). The No. 3 dumbbell test piece taken from the evaluation rubber sheet was subjected to the test specified in JIS K6257. In accordance with the method for determining heat aging properties, a heat aging test was performed at 165°C for 7 days using a gear aging tester. The experiment was carried out using Then, the "elongation at break" of the test pieces after aging was measured in the same manner as above. The heat resistance of a rubber composition is determined by the ratio of the "elongation at break (E0)" before aging to the "elongation at break (E1)" after aging. The effect was evaluated by calculating the ratio (E / E0) of "(E)" to "(E)". Based on the evaluation results, the elongation at break and heat resistance were evaluated according to the following criteria. The results are shown in Table 2. (A: Criteria for evaluation of elongation at break) "○": Elongation at break (E0) is 500% or more "△": Elongation at break (E0) is 400% or more but less than 500% "X": Elongation at break (E0) is less than 400% (B: Criteria for heat resistance evaluation results) "○": Magnification (E / E0) is 0.8 or more "△": Magnification (E / E0) is 0.7 or more and less than 0.8 "X": Magnification (E / E0) is less than 0.7

[0044] (Rating 2: Flame retardant) Conveyor belts with cover rubber layer formed with the compounding content shown in Table 2 were subjected to JIS K6 The flame retardancy was evaluated in accordance with the test method for fabric-layered conveyor belts specified in 324. The evaluation was carried out by measuring the duration of the flame after the burner was removed. The flame retardancy was evaluated according to the following criteria based on the flame duration. The results are shown in Table 2. (C: Criteria for flame retardancy evaluation) "○": Flame duration is 15 seconds or less 「△」: Flame duration is 16~59 seconds "X": Fire lasts for 60 seconds or more

[0045] (Rating 3: Abrasion resistance) JIS K6264-2 "Vulcanized and thermoplastic rubber - Determination of abrasion resistance - Part 2: Test The abrasion resistance was evaluated by the DIN abrasion test in the "Test Method for Wear Resistance Testing." The abrasion resistance was evaluated based on the amount of abrasion according to the following criteria. The results are shown in Table 2. (D: Criteria for evaluation of wear resistance) "○": Wear amount is 180mm 3 less than "△": Wear amount is 180mm 3 More than 230mm 3 below "X": Wear amount is 230mm 3 super

[0046] (Overall evaluation criteria) A comprehensive evaluation was made based on the four evaluation results A to D above. The judging criteria are as follows: "○": All four judgment results are either "○" or "△", and there is one or less "△" "△": All four judgment results are either "○" or "△", and there are two or more "△"s. "X": At least one of the four judgement results is "X".

[0047] (Reference example 1) As Reference Example 1 for comparison with the test examples in Table 2 below, Table 3 shows a test example in which natural rubber is the main component (rubber Evaluation of composition: natural rubber / butadiene rubber = 85% by mass / 15% by mass The results are shown. In addition, the brominated flame retardant used in Reference Example 1 was the same as that used in Test Example 1. In addition, in Reference Example 1, "N-oxydiethylene-2-benzothiazolyl" is used as the "vulcanization accelerator". "Sulfenamide" was used. Furthermore, the "anti-aging agent A" in Reference Example 1 is an aromatic secondary amine-based anti-aging agent manufactured by Ouchi Shinko Chemical Co., Ltd. Antioxidant, product name "Nocrac 6c", "Antioxidant B" is manufactured by Ouchi Shinko Chemical Co., Ltd., amine -Ketone-based anti-aging agent, product name "Nocrac 224".

[0048] The rubber composition of Reference Example 1 was also evaluated in the same manner as above. However, the rubber composition of Reference Example 1 has low heat resistance and is not heat resistant after a heat aging test at 165°C for 7 days. It was determined that the specimen could not withstand the test, so the test temperature was set at 70°C and the elongation ratio at break E / E 0) was calculated. As a result, as shown in Table 3, the rubber composition of Reference Example 1 was tested in the evaluation of heat resistance. Even when the temperature was set at a fairly low 70°C, the "residual rate" was only 0.78. For this reason, the rubber composition of Reference Example 1 was rated as "X" in the heat aging test at 165°C for 7 days. It was confirmed that this is the case. Thus, the general flame-retardant rubber composition shown in Reference Example 1 has insufficient heat resistance. It was confirmed that this was the case.

[0049] (Additional Study: Test Examples 12-15) In order to observe the change in properties depending on the amount of bromine-based flame retardant, a bromine-based flame retardant was added to the composition of Test Example 11. The amount of flame retardant (FR3) was changed and the evaluation was carried out in the same manner as before. The results are shown in Table 4 together with the evaluation results of Test Example 11. In this study, it was confirmed that excellent heat resistance was exhibited in all test examples. In addition, from Table 4, it can be seen that in order to provide excellent flame retardancy to the cover rubber layer, it is necessary to use 100% rubber. The ratio of the brominated flame retardant to the total weight of the mixture is preferably 20 parts by weight or more, and more preferably 25 parts by weight or more. It can be understood that the above is particularly preferable. In addition, the results shown in Table 4 indicate that the cover rubber layer exhibits excellent abrasion resistance. In particular, the ratio of brominated flame retardants to 100 parts by mass of rubber should be less than 30 parts by mass. This can be understood as being preferable.

[0050] [Table 2]

[0051] [Table 3]

[0052] [Table 4]

[0053] From the above results, it is apparent that the present invention provides excellent flame retardancy and abrasion resistance for conveyor belts. It can be seen that the composition can exhibit excellent thermal resistance and heat resistance. [Explanation of symbols]

[0054] 1: belt body (conveyor belt), 10: cover rubber layer (10a: upper cover rubber layer, 10b: Lower cover rubber layer, 20: Traction layer

Claims

1. A rubber composition for a cover rubber used for forming a cover rubber layer of a conveyor belt, comprising: The rubber composition includes a brominated flame retardant. The brominated flame retardant is contained in an amount of 25 parts by mass or less relative to 100 parts by mass of the rubber, and the mass of bromine is contained in an amount of 10 parts by mass or more relative to 100 parts by mass of the rubber, The main component of the rubber is a rubber that does not contain a diene and has ethylene-derived structural units and structural units that contain a tertiary carbon.

2. 2. A rubber composition for a cover rubber according to claim 1, wherein a part or all of said brominated flame retardants have a melting point of 300° C. or higher.

3. 3. The rubber composition for cover rubber according to claim 1, further comprising carbon black, and a content of a filler other than carbon black is 20 parts by mass or less per 100 parts by mass of said rubber.

4. 4. The rubber composition for a cover rubber according to claim 1, further comprising an organic peroxide-based crosslinking agent and an organic co-crosslinking agent.

5. A conveyor belt having a traction layer and a cover rubber layer provided on at least one side of the traction layer, wherein the rubber composition for the cover rubber forming the cover rubber layer is the rubber composition for the cover rubber described in any one of claims 1 to 4.