Manufacturing method for assembling type container and assembling type container
The method addresses sealing issues in assembly-type paper containers by forming solid protrusions on the resin film that cross container steps, ensuring effective sealing and preventing leakage or oozing through specific manufacturing processes.
Patent Information
- Application Number
- JP2023043331
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-17
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-03-17
AI Technical Summary
Conventional assembly-type paper containers with a resin film face challenges in sealing gaps and steps, leading to potential leakage or oozing of contents due to hollow protrusions and cavities formed by the resin film and top seal, which are difficult to close effectively.
A method involving the formation of protrusions on the resin film that cross the steps of the container flange, bonded from tip to base, using a hot plate molding machine with specific suction and cooling processes to ensure the protrusions are solid and uniform, followed by attaching a top seal that covers these protrusions to prevent gaps.
The method effectively seals the container, preventing leakage or oozing of contents by ensuring the protrusions are solid and uniformly formed, thus enhancing the container's sealing integrity and handling stability.
Smart Images

Figure 2024132530000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a prefabricated container, and a prefabricated container. [Background technology]
[0002] Conventionally, there has been known a prefabricated paper container in which a tray-shaped container body having a flange portion at the upper end is assembled from blank sheets made mainly of paper. Some of these prefabricated paper containers have a thermoplastic resin film having resin properties attached to the inner surface of the container body, including the upper surface of the flange portion (see Patent Documents 1 and 2, etc.). Because this prefabricated paper container with a resin film has resin properties, it is mainly used as a tray or bowl for containing food, etc.
[0003] Furthermore, compared to plastic containers, the prefabricated paper container is an environmentally friendly product, for example, because it can suppress the generation of secondary microplastics in the environment. Furthermore, the resin film can be peeled off from the container body, and the resin film and the paper container body can be separated, and the resin film and the container body can be recycled separately. Due to these advantages, it is expected that the prefabricated paper container can be used as a packaging container for food and the like and a storage container for food and the like by applying, for example, Modified Atmosphere Packaging (MAP). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 6-293334 [Patent Document 2] JP 2019-172339 A Summary of the Invention [Problem to be solved by the invention]
[0005] In the container body of such a conventional assembled paper container, a gap is formed on the upper surface of the flange portion due to the close proximity of the end faces of the blank sheets. At present, it is difficult to completely fill this gap even if the inner surface of the container body, including the upper surface of the flange portion, is covered with a resin film. Furthermore, the resin film is thin, and when the resin film is covered on the inner surface of the container body, including the upper surface of the flange portion, for example, by vacuum pressure, the resin film is sucked into the gap, making it difficult to close the gap with the resin film alone.
[0006] Also, a packaging method has been developed in which the air in the storage section of the container body is replaced with a food gas suitable for packaging the food (e.g., MAP). When this packaging method is applied to a prefabricated paper container with a resin film, a top seal is attached to the resin film on the upper surface of the flange section. However, because the top seal is also thin, even if the top seal is attached to the resin film, a cavity is created along the gap between the upper surface of the resin film and the lower surface of the top seal. In other words, it is difficult to completely seal the cavity even with the top seal. Moreover, both ends of the cavity are open. Therefore, the storage section of the container body communicates with the outside of the container body through this cavity.
[0007] In addition, the flange of the container body may have a step formed by laminating the folded pieces of the blank sheet so that they overlap each other. If a top seal is applied to this step, a cavity may be formed along the step. Therefore, as shown in the figure, it is possible to prevent the cavity by forming a hollow protrusion that stands up against the flange using a resin film above the step so as to cross the step, and crushing this hollow protrusion with the top seal.
[0008] The procedure for forming a hollow protrusion will be described with reference to FIG. 21. As shown in FIG. 21(a), the container body is placed on the lower mold 910 of the hot plate molding machine, and the resin film 93 is placed on the upper surface of the flange 913. The upper surface side of the resin film 3 is vacuum-sucked by the hot plate 920 (upper mold) of the hot plate molding machine, which is heated to at least one or more resin melting points of the resins constituting the resin film 93. The resin film 3 is deformed along the inner surface of the hot plate 920 by suction with the hot plate 920. Then, as shown in FIG. 21(b), the lower surface side of the resin film 3 is vacuum-sucked by the lower mold 910 of the hot plate molding machine. This allows the resin film 3 to cover the storage portion of the container body (not shown). Thereafter, as shown in FIG. 21(c), suction by the lower mold 910 is stopped while suction is being performed by the hot plate 920. Then, as shown in FIG. 21(d), suction by the hot plate 920 is stopped. Then, as shown in FIG. 21(e), the hot plate 920 is raised and the hollow protrusion 931 is released from the hot plate 920. As a result, the hollow protrusion 931 is formed in the flange 913. Then, the heated protrusion 931 is exposed to the outside air and naturally cooled. Therefore, as shown in FIG. 21(f), the hollow protrusion 931 is crystallized by natural cooling and freely shrinks. As a result, there is a risk of defective shaping, such as uneven thickness or height difference in the hollow protrusion 931.
[0009] When such a hollow protrusion with poor shaping is crushed by the top seal, a cavity may be formed between the top seal and the hollow protrusion. Furthermore, since the protrusion is hollow, it may be crushed randomly, resulting in a cavity. As a result, the contents may leak or seep out of the storage section through the cavity.
[0010] For the above reasons, in the case of a prefabricated container with a resin film, even if the storage section is covered with a top seal, there is a risk that the contents will leak or seep out of the storage section through the cavity.
[0011] The present invention has been devised in consideration of the above-mentioned problems, and its object is to provide a method for manufacturing an assembled container, and an assembled paper container, that are capable of preventing the contents from leaking or seeping out of the storage portion of the container body. [Means for solving the problem]
[0012] The method for manufacturing a prefabricated container according to the present invention is a method for manufacturing a prefabricated container comprising a container body having a storage section formed by raising a plurality of side surfaces from the bottom surface of a blank sheet and a flange section in which upper portions of the plurality of side surfaces are folded back and extended toward the outside of the storage section, and a resin film covering the inner surface of the container body, the flange section having a step formed by bonding together the folded back pieces of the blank sheet so as to overlap each other, and the method includes a positioning step of placing the container body on a receiving mold provided opposite a hot plate of a hot plate molding machine and placing the resin film between the container body and the hot plate, and a step of sucking the resin film toward the hot plate to form a container body above the step. and a covering process for forming a protrusion that crosses the step in the resin film and covering the inner surface of the container body with the resin film, the covering process comprising a suction process for sucking the protrusion-forming area that crosses the step in the resin film using a molding part of the hot plate, the cross section of which is cut out in a triangular shape along the direction from the storage part to the outside, and then sucking the protrusion-forming area with the receiving mold with a suction force smaller than that of the molding part, and a stopping process for forming the protrusion in which the resin films are bonded to each other from the tip end to the base end that rises up against the flange portion by stopping the suction of the molding part while the receiving mold is still suctioning.
[0013] The prefabricated container of the present invention is an assembly-type container comprising a container body having a storage section formed by raising a plurality of side surfaces from the bottom surface of a blank sheet, and a flange section in which the upper parts of the plurality of side surfaces are folded back and extended toward the outside of the storage section, and a resin film covering the inner surface of the container body, wherein the flange section has a step formed by bonding together the folded-back pieces of the blank sheet so that they overlap after assembly, and the resin film has a protrusion portion above the step that crosses the step, and the protrusion portion is formed by bonding the resin films to each other from their tip ends to their base ends that rise up relative to the flange portions. Effect of the Invention
[0014] According to the present invention having the above-mentioned configuration, it is possible to provide a knockdown container that is capable of preventing the contained contents from leaking or seeping out from the containing portion of the container body. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1(a) is a plan view showing the prefabricated container of the first embodiment, FIG. 1(b) is a side view showing the prefabricated container of FIG. 1(a), and FIG. 1(c) is a perspective view showing the prefabricated container of FIG. 1(a). [Diagram 2] FIG. 2 is a development view showing a blank sheet used in the knockdown container of FIG. [Diagram 3] FIG. 3 is an enlarged cross-sectional view of a portion viewed from the arrow AA in FIG. 1, and is a schematic cross-sectional view showing an example of a protrusion. [Figure 4] FIG. 4 is a plan view showing an embodiment in which the storage section of the prefabricated container of FIG. 1 is covered with a top seal. [Diagram 5] FIG. 5 is a cross-sectional view of the vicinity of a laminated portion formed by tilting a protruding portion by a top seal in the prefabricated container of FIG. [Figure 6] FIG. 6 is a schematic diagram showing an example of a hot plate forming machine. [Figure 7]FIG. 7 is a flowchart showing an example of a method for manufacturing a prefabricated container. [Figure 8] 8(a) and 8(b) are schematic cross-sectional views showing an example of a method for producing a prefabricated container. [Figure 9] 9(a) and 9(b) are schematic cross-sectional views showing an example of a method for producing a prefabricated container. [Figure 10] 10(a) and 10(b) are schematic cross-sectional views showing an example of a method for producing a prefabricated container. [Figure 11] 11(a) and 11(b) are schematic cross-sectional views showing an example of a method for producing a prefabricated container. [Figure 12] FIG. 12 is a schematic diagram showing an example of a manufacturing system for a prefabricated container according to an embodiment of the present invention. [Figure 13] FIG. 13 is a plan view showing the assembly container according to the first embodiment. [Figure 14] FIG. 14 is a photograph showing the protrusions of Experimental Examples 1 to 3. [Figure 15] FIG. 15 is a photograph showing the protrusions of Experimental Examples 4 and 5. [Figure 16] FIG. 16(a) is a photograph showing the protrusions of Experimental Example 6, and FIG. 16(b) is a photograph showing the protrusions of Experimental Example 7. [Figure 17] FIG. 17 is a diagram for explaining a molding section of the fourth embodiment. [Figure 18] FIG. 18(a) is a photograph showing the protrusions of Experimental Example 8, and FIG. 18(b) is a photograph showing the protrusions of Experimental Example 9. [Figure 19] FIG. 19(a) is a photograph showing the protrusions of Experimental Example 10, and FIG. 19(b) is a photograph showing the protrusions of Experimental Example 11. [Figure 20] 20(a) and 20(b) are diagrams for explaining the relationship between the apex angle of the apex of the molded part and the resin film. [Figure 21] 21(a) to 21(f) are diagrams illustrating the procedure for forming hollow protrusions. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, embodiments of the present invention will be described with reference to the drawings.
[0017] First Embodiment The prefabricated container 1 according to the first embodiment includes a container body 11 and a resin film 3 covering the inner surface of the container body 11, as shown in Figs. 1(a) to 1(c).
[0018] The container body 11 has a storage section 12 and a flange section 13. The container body 11 is assembled from one blank sheet 2, shown in FIG. 2, which is made mainly of paper, for example. In FIG. 2, dotted lines indicate "valley folds" and dashed lines indicate "mountain folds". The valley folds and mountain folds are, for example, perforations, half cuts, or lines. The solid lines in the blank sheet 2 indicate "notches". The blank sheet 2 is made to have "valley folds" and "mountain folds", and the folded pieces 13a and 13b are attached together so that they overlap, thereby forming the container body 11. The blank sheet 2 may be made mainly of paper, or may be a well-known breathable blank sheet.
[0019] In this embodiment, the storage section 12 has eight side surfaces 122 rising from the bottom surface 121. The storage section 12 can be configured so long as it has three or more side surfaces 122.
[0020] The flange portion 13 is continuous with the upper end of each side surface 122 and extends in a direction toward the outside of the storage portion 12. An upper surface 131 of this flange portion 13 has steps 22 formed by bonding the folded pieces 13a, 13b of the blank sheet 2 together so that they overlap each other after assembly. The steps 22 are formed extending from the storage portion 12 side toward the outside of the storage portion 12. There are two steps 22 at each of the four corners of the flange portion 13.
[0021] The resin film 3 covers the inner surface of the container body 11 including the upper surface 131 of the flange portion 13. The resin film 3 has a protrusion 31 that crosses the step 22 above the step 22 in the portion that is covered by the upper surface 131 of the flange portion 13 of the container body 11. In the prefabricated container 1 of this embodiment, there are eight steps 22, and a protrusion 31 is formed for each step 22. Note that a plurality of protrusions 31 may be provided for one step 22.
[0022] As shown in FIG. 3, the protrusion 31 is formed by bonding together resin films 3 from a tip end 31a to a base end 31b rising up relative to the flange 13.
[0023] Examples of resins suitable for covering the inner surface of the container body 11 and used for the resin film 3 capable of forming the protrusions 31 include thermoplastic resins such as polyolefins such as polyethylene (PE) and polypropylene (PP) and modified resins thereof (adhesive resins), polyesters such as polyvinyl chloride and polyethylene terephthalate (PET), ethylene-vinyl acetate copolymers (EVA), ethylene-vinyl alcohol copolymers (EVOH), ethylene-acrylic acid copolymers, polyamides, polyvinylidene chloride, polystyrene, polycarbonate, polybutene, and polyvinyl alcohol. The resin film 3 may be a single film of any of the above materials, or may be a film in which a plurality of the above materials are mixed. The resin film 3 may also be a single-layer film, or a laminated film in which a plurality of layers are laminated.
[0024] Next, a description will be given of a prefabricated container 1 in which the storage section 12 is covered with a top seal 4, in addition to the above-mentioned embodiments.
[0025] As shown in FIG. 4, the assembled container 1 can package and store food or other contents by covering the storage section 12 with the top seal 4. The top seal 4 is attached to the resin film 3 on the upper surface 131 of the flange section 13. As a result, the top seal 4 covers the storage section 12. In this embodiment, the top seal 4 is attached to the resin film 3 above the upper surface 131 of the flange section 13, crossing the step 22, while the protrusion 31 is laid down either to the storage section 12 side or to the outside of the storage section 12. When the top seal 4 is attached to the resin film 3, the top seal 4 is pressed by a press machine while being heated in a pressing area 32 shown by a dotted line. In this embodiment, the protrusion 31 is designed so that the entire protrusion 31 fits within the width of the pressing area 32. As a result, the protrusion 31 can be reliably pressed down by the press machine.
[0026] Top seal 4 is attached to the upper surface of resin film 3 so as to traverse step 22. For top seal 4, for example, polyolefins such as polyethylene (PE) and polypropylene (PP) or modified resins thereof (adhesive resins), polyesters such as polyvinyl chloride and polyethylene terephthalate (PET), ethylene-vinyl acetate copolymer (EVA), ethylene-vinyl alcohol copolymer (EVOH), ethylene-acrylic acid copolymer, polyamide, polyvinylidene chloride, polystyrene, polycarbonate, polybutene, polyvinyl alcohol, etc. are used as a sealing layer.
[0027] 5, the protrusion 31 is disposed so as to be inclined either towards the storage section 12 or towards the outside of the storage section 12 along the top seal 4. The resin film 3 is folded into three layers to form a laminated section 33 by the portion attached to the flange section 13 and the protrusion 31. Furthermore, since no or almost no space is formed inside the protrusion 31, the direction in which the protrusion 31 falls when the top seal 4 is attached can be controlled to be either towards the storage section 12 or towards the outside of the storage section 12.
[0028] <Hot plate forming machine 600> Next, a hot plate forming machine 600 used to manufacture the prefabricated container 1 according to the first embodiment will be described with reference to FIG.
[0029] As shown in Fig. 6, the hot plate molding machine 600 is a manufacturing device used to manufacture the prefabricated container 1. The hot plate molding machine 600 covers the container body 11 with the flange portion 13 with the resin film 3, and can form the protrusion portion 31 on the resin film 3 during the covering. The hot plate molding machine 600 includes a receiving mold 610 and a hot plate 620. The hot plate molding machine 600 may have a trimming function.
[0030] (Receiving type 610) The receiving mold 610 accommodates the container body 11 by placing it thereon. The receiving mold 610 is disposed below the hot plate 620. The receiving mold 610 is set to a temperature of, for example, about 25°C. The receiving mold 610 can suck the resin film 3 in a direction toward the container body 11. It has a first placing portion 611 on which the accommodation portion 12 of the container body 11 is placed, and a second placing portion 612 on which the flange portion 13 of the container body 11 is placed.
[0031] The first placement portion 611 is connected to a vacuum pump (not shown) and can suck the lower side of the accommodation portion 12. The first placement portion 611 and the second placement portion 612 are connected to a vacuum pump (not shown) and can suck the lower side of the flange portion 13.
[0032] (hot plate 620) The hot plate 620 is disposed, for example, above the receiving mold 610 in opposition, and can move up and down to open and close. The hot plate 620 is heated to a temperature at which the resin film 3 can be deformed, for example, about 170°C to 190°C. The hot plate 620 is connected to a vacuum pump (not shown), and can apply a vacuum to the resin film 3 in a direction to pull it away from the container body 11. The hot plate 620 can also send air in a direction toward the container body 11 to move the resin film 3. The hot plate 620 has a facing portion 621 facing the first placement portion 611, a forming portion 622 facing the second placement portion 612, and a cutter portion 623 for cutting the resin film 3.
[0033] The facing portion 621 is connected to a vacuum pump (not shown) and can draw a vacuum on the upper side of the resinous film 3. The facing portion 621 can also send compressed air to the upper side of the resinous film 3. The lower surface side of the facing portion 621 is formed with a dome-shaped concave surface. As a result, when the heated facing portion 621 sucks the resinous film 3, the resinous film 3 sticks to the lower surface of the facing portion 621 and is heated, and the resinous film 3 can be stretched uniformly. Therefore, when air is sent from the facing portion 621, the resinous film 3 can cover the entire storage portion 12.
[0034] The molding section 622 is connected to a vacuum pump (not shown) and can apply a vacuum to the projection-forming area of the resinous film 3 on the flange section 13. The molding section 622 has a cross section cut out in a triangular shape along the direction from the accommodation section 12 toward the outside. By forming the cross section in a triangular shape, the amount of resin that can be sucked in can be increased when the resinous film 3 is sucked to form the projection. This makes it possible to ensure the amount of resin necessary to fill the step 22 with the formed projection.
[0035] Molding section 622 can take in air from the triangularly cut-out apex into the space inside molding section 622. Molding section 622 is preferably cut in an isosceles triangle shape in cross section along the direction from storage section 12 to the outside. This makes it possible to make the amount of resin in resin films 3 on both sides of tip end 31a of protrusion 31 uniform when resin films 3 are bonded together to form protrusion 31.
[0036] The apex angle θ of the apex of the molding part 622 cut out in an isosceles triangle shape is preferably 45° or less. This makes it possible to suppress deviation of the center line of the protrusion 31 when the hot plate 620 is released to form the protrusion 31, compared to when the apex angle θ is 64° or more. This makes it easier to form the protrusion 31 at the designed position. Although the molding part 622 is preferably an isosceles triangle, the protrusion 31 can be formed if it is triangular.
[0037] The cutter section 623 is provided on the hot plate 620 and cuts the resin film 3 .
[0038] In addition, in the hot plate molding machine 600 shown in Fig. 6, the hot plate 620 is described as facing the upper side of the receiving mold 610. In addition, the hot plate molding machine 600 may be one in which the hot plate 620 faces the lower side of the receiving mold 610, or the receiving mold 610 and the hot plate 620 face each other in the left-right direction.
[0039] <An example of a manufacturing method for a prefabricated container> Next, an example of a method for manufacturing a knockdown container will be described with reference to Figures 7 to 11. The method for manufacturing a knockdown container includes, for example, a blank sheet cutting step S10, a box making step S20, an arrangement step S30, a covering step S40, an item accommodating step S50, a bonding step S60, and a trimming step S70.
[0040] (Blank sheet cutting process S10) First, in the method for producing a knockdown container, the blank sheet 2 is produced by performing the blank sheet cutting step S10 of cutting the blank sheet 2 described above.
[0041] (Box manufacturing process S20) Next, in the manufacturing method for a knockdown container, a box-making process S20 is performed in which a container body 11 is assembled from the blank sheets 2 manufactured by cutting in the blank sheet cutting process S10. The container body 11 has a storage section 12 formed by raising a plurality of side surfaces 122 from a bottom surface 121 of the blank sheet 2, and a flange section 13 formed by folding back the upper portions of the plurality of side surfaces 122 and extending toward the outside of the storage section 12. The flange section 13 has a step 22 formed by bonding the folded-back pieces of the blank sheet 2 together so that they overlap each other.
[0042] (Placement process S30) Next, in the manufacturing method for an assembled container, as shown in Figure 8(a), a placement process S30 is performed in which the container body 11 is placed on a receiving mold 610 provided below a hot plate 620 of a hot plate molding machine 600, and a resin film 3 is placed between the container body 11 and the hot plate 620.
[0043] (Coating process S40) Next, in the manufacturing method of the assembled container, as shown in FIG. 8(b) to FIG. 11(b), the resin film 3 is heated by the hot plate forming machine 600 and sucked toward the hot plate 620 to form a protrusion 31 that crosses the step 22 above the step 22, and a covering step S40 is performed to cover the inner surface of the container body 11 with the resin film 3. The covering step S40 has a suction step S41 and a stop step S42. The dotted arrows in FIG. 8 to FIG. 11 indicate suction by the hot plate forming machine 600. In the following example, the resin film 3 is heated in the suction step S41. In the present invention, the resin film 3 may be heated before the suction step S41. For example, in the arrangement step S30, the resin film 3 may be heated in advance before being arranged between the container body 11 and the hot plate 620, and then the suction step S41 may be performed.
[0044] In the suction process S41, the upper side of the protrusion formation area crossing the step 22 of the resin film 3 is sucked by the molding portion 622 of the hot plate 620, whose cross section extending from the storage portion 12 toward the outside is cut into a triangular shape, and then the lower side of the protrusion formation area is sucked by the receiving mold 610 with a suction force smaller than that of the molding portion 622.
[0045] 8(b), in the suction step S41, the upper side of the resinous film 3 is sucked by the facing part 621 and the shaping part 622 of the heated hot plate 620. As the facing part 621 sucks the resinous film 3, the heated resinous film 3 adheres to the facing part 621 and can be uniformly stretched. In addition, as the shaping part 622 sucks the resinous film 3, the upper surface of the protrusion formation region of the resinous film 3 adheres to the shaping part 622.
[0046] 9(a), the suction process S41 lowers the hot plate 620 toward the receiving mold 610 and closes the hot plate 620. This causes the molding portion 622 of the hot plate 620 and the second mounting portion 612 of the receiving mold 610 to press the resinous film 3. The suction process S41 then lowers the cutter portion 623 to cut the resinous film 3 on the outer side of the hot plate 620.
[0047] Then, in the suction step S41, as shown in FIG. 9(b), suction of the facing portion 621 is stopped, and the lower surface side of the resinous film 3 is sucked by the first mounting portion 611 and the second mounting portion 612 of the receiving mold 610. For example, when the blank sheet 2 is mainly made of paper, it has air permeability, so that the lower surface side of the resinous film 3 can be sucked by sucking the lower side of the container body 11 by the receiving mold 610. Note that, for example, when the blank sheet 2 does not have air permeability, an opening may be provided in the blank sheet 2 in advance. In this case, by sucking the lower side of the container body 11 by the receiving mold 610, the lower surface side of the resinous film 3 can be sucked through the formed opening.
[0048] In the suction step S41, suction of the facing portion 621 is stopped, and the lower surface side of the resinous film 3 is sucked by the first mounting portion 611 and the second mounting portion 612 of the receiving mold 610, so that the resinous film 3 attached to the facing portion 621 is released from the facing portion 621. In addition, the second mounting portion 612 performs suction with a suction force smaller than that of the molding portion 622. As a result, the resinous film 3 attached to the molding portion 622 is maintained in that state.
[0049] 10(a), in the suction step S41, compressed air is sent by the facing part 621 to the upper surface side of the resinous film 3. This allows the resinous film 3 to cover the containing part 12.
[0050] Next, a stopping step S42 is performed. In the stopping step S42, suction of the molding part 622 is stopped while the receiving mold 610 is suctioned, and then suction of the receiving mold 610 is stopped, thereby forming the protrusion 31 in which the resin films 3 are bonded to each other from the tip end 31a to the base end 31b rising up against the flange portion 13.
[0051] 10(b), the stopping step S42 stops the air supply by the facing part 621 of the hot plate 620 and the suction by the forming part 622. By stopping the suction by the forming part 622, outside air is taken in from the apex of the triangle of the forming part 622. At this time, the second placement part 612 of the receiving mold 610 is in a state of sucking the resinous film 3. As a result, the resinous film 3 attached to the forming part 622 is released from the forming part 622 and is cooled by the outside air taken in from the apex of the triangle of the forming part 622.
[0052] When the resin film 3 is released from the molding part 622, as shown in FIG. 11(a), the tip 31a of the protrusion 31 is formed starting from the apex of the notched triangle of the molding part 622, and the resin film 3 is bonded to each other from the tip 31a to the base end 31b of the protrusion 31. In this way, the stopping step S42 forms the protrusion 31 in which the resin films 3 are bonded to each other from the tip 31a to the base end 31b that stands up against the flange part 13. Since the protrusion 31 is formed by bonding the resin films 3 to each other from the tip 31a to the base end 31b, it is not hollow as in the conventional case, and no or almost no space is formed inside the protrusion 31. In addition, since the protrusion 31 has already been released and is sufficiently cooled by the outside air taken in from the triangular apex of the molding part 622, it is possible to prevent the protrusion 31 from being cold crystallized and free shrinking due to natural cooling after the hot plate 620 is opened. As a result, it is possible to prevent defective shaping, such as uneven thickness or height difference, from occurring in the protrusions 31. Then, in the stopping step S42, the suction of the receiving mold 610 is stopped.
[0053] Thereafter, in the stopping step S42, as shown in FIG. 11(b), the hot plate 620 is raised and the mold is opened.
[0054] (Item storage process S50) Next, in the manufacturing method for the assembled container, a content storage process S50 is performed in which content items such as food are stored in the storage section 12 of the assembled container 1 in a state where the top seal 4 manufactured in the covering process S40 is not yet attached.
[0055] (Passing process S60) Next, in the manufacturing method for the assembled container, an attachment step S60 is performed in which a top seal 4 is attached to the resin film 3 covering the upper surface of the flange portion 13 of the assembled container 1 in a state in which food or other contents are contained in the storage portion 12 in the content storage step S50, using a pressing machine to cross the step 22 while tilting the protrusion portion 31 either toward the storage portion 12 or to the outside of the storage portion 12 above the upper surface of the flange portion 13.
[0056] In the attachment step S60, when attaching the top seal 4, the protrusion 31 is tilted either toward the storage section 12 side or toward the outside of the storage section 12 so as to follow the top seal 4, and a laminated section 33 is formed in the resin film 3 by the portion of the resin film 3 attached to the flange section 13 and the protrusion 31, which is folded in three layers. This allows the laminated section 33 to be embedded in the step 22. This makes it possible to prevent contamination of the contents stored in the storage section 12.
[0057] (Trimming process S70) Finally, a trimming step S70 is performed to remove excess resin film 3 from around the prefabricated container 1, thereby producing the prefabricated container 1 and completing the method for producing the prefabricated container 1 according to this embodiment.
[0058] Next, a manufacturing system 700 for a prefabricated container will be described with reference to FIG.
[0059] In the manufacturing system 700 , the resin film 3 wound around a feed roller 710 is wound around a winding roller 720 , while the resin film 3 is coated onto the container body 11 with the flange portion 13 .
[0060] 12, the manufacturing system 700 includes a feed roller 710, a take-up roller 720, and a hot plate forming machine 600. The hot plate forming machine 600 has a trimming function for trimming the resinous film 3.
[0061] A roll of the band-shaped resin film 3 is attached to the feed roller 710.
[0062] One end of the strip-shaped resin film 3 is attached to the winding roller 720, which winds up the strip-shaped resin film 3. The strip-shaped resin film 3 advances from the feed roller 710 towards the winding roller 720.
[0063] The hot plate former 600 is disposed between a feed roller 710 and a take-up roller 720 .
[0064] The prefabricated container 1 manufactured by the hot plate molding machine 600 is detached from the strip-shaped resin film 3 by a trimming function of the hot plate molding machine 600 .
[0065] In this manner, the prefabricated container manufacturing system 700 includes the hot plate forming machine 600. Therefore, the prefabricated container 1 can be manufactured by this manufacturing system 700. Moreover, the prefabricated container 1 can be manufactured continuously from a strip-shaped resin film 3 by this manufacturing system 700.
[0066] According to this embodiment, the covering process S40 includes a suction process S41 in which the upper side of the protrusion formation area crossing the step 22 of the resin film 3 is sucked by the molding portion 622 of the hot plate 620, and then the lower side of the protrusion formation area is sucked by the receiving mold 610 with a suction force smaller than that of the molding portion 622, and a stopping process S42 in which the suction of the molding portion 622 is stopped while the receiving mold 610 is still suctioning, thereby forming the protrusion 31 in which the resin films 3 are bonded together from the tip portion 31a to the base portion 31b that rises up against the flange portion 13.
[0067] As a result, the protrusion 31 is not hollow as in the past, and no or almost no space is formed inside the protrusion 31. In addition, since the protrusion 31 has already been sufficiently cooled by the outside air taken in from the triangular apex of the mold release and molding part 622, it is possible to prevent the protrusion 31 from crystallizing and shrinking freely due to natural cooling after mold opening. As a result, it is possible to prevent the protrusion 31 from having a shape defect such as uneven thickness or height difference. Therefore, when the top seal 4 is attached to the protrusion 31, it is possible to prevent a cavity between the protrusion 31 and the top seal 4, and it is possible to prevent the leakage or seepage of the contained contents from the storage part 12 of the container body 11.
[0068] Furthermore, since the protrusions 31 are not hollow as in the past and no or almost no space is formed inside the protrusions 31, the protrusions 31 are less likely to deform when the prefabricated containers 1 are stacked or transported. This ensures the quality of the protrusions 31 and makes the prefabricated containers 1 easier to handle.
[0069] According to this embodiment, after the covering step S40, a bonding step S60 is further provided in which the top seal 4 is bonded to the upper surface of the resin film 3 so as to cross the step 22. In the bonding step S60, when the top seal 4 is bonded, the protrusion 31 is tilted to either the storage section 12 side or the outside of the storage section 12 so as to follow the top seal 4, and the part of the resin film 3 bonded to the flange section 13 and the protrusion 31 form a laminated section 33 in the resin film 3 that is folded in three layers. This allows the laminated section 33 to be embedded in the step 22. This makes it possible to suppress leakage or seepage of the contents from the storage section 12 of the container body 11.
[0070] According to this embodiment, the cross section of the molded portion 622 along the direction from the accommodation portion 12 toward the outside is cut out in an isosceles triangle shape, and the apex angle of the molded portion 622 is less than 45°. This makes it possible to suppress deviation of the molded portion 622 from the center line when the molded portion 622 is released from the mold to form the protrusion 31, compared to a case where the apex angle θ is 64° or more. This makes it easier to form the protrusion 31 at the designed position.
[0071] According to this embodiment, the protrusion 31 is formed by bonding the resin films 3 together from the tip end 31a to the base end 31b rising up relative to the flange portion 13.
[0072] As a result, the protrusion 31 is not hollow as in the past, and no or almost no space is formed inside the protrusion 31. In addition, since the protrusion 31 has already been released from the mold and sufficiently cooled by the outside air taken in from the triangular apex of the molding part 622, it is possible to prevent the protrusion 31 from crystallizing and shrinking freely due to natural cooling after the hot plate 620 is opened. As a result, it is possible to prevent the protrusion 31 from having a shape defect such as uneven thickness or height difference. Therefore, when the top seal 4 is attached to the protrusion 31, it is possible to prevent a cavity between the protrusion 31 and the top seal 4, and it is possible to prevent the leakage or seepage of the contained contents from the containing part 12 of the container body 11.
[0073] According to this embodiment, the resin film 3 is folded into three layers to form a laminated portion 33 by the portion attached to the flange portion 13 and the protrusion portion 31. This allows the laminated portion 33 to be embedded in the step 22. This makes it possible to prevent the contents from leaking or seeping out of the storage portion 12 of the container body 11.
[0074] <Second embodiment> 13, in the prefabricated container 1 according to the second embodiment, a single connected protrusion 31 is formed for each step 22. That is, the protrusion 31 is disposed on the flange portion 13 so as to surround the entire periphery of the storage portion 12. Even in this case, the above-mentioned advantageous effects can be achieved.
[0075] Although the embodiment of the present invention has been described above, this embodiment is presented as an example and is not intended to limit the scope of the invention. These novel embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the gist of the invention. These embodiments and their modifications are included in the scope and gist of the invention, and are included in the scope of the invention and its equivalents described in the claims. EXAMPLES
[0076] In Example 1, the cross section of the protrusion made of the resin film was observed under a microscope. Experimental Example 1 is a protrusion formed by the procedure explained in FIG. 21. Experimental Examples 2 and 3 are protrusions formed by the manufacturing method of the prefabricated container of the present invention. In Experimental Example 2, a protrusion is formed so as to surround the entire periphery of the storage section of the container body. In Experimental Example 3, a protrusion is formed at a step formed in the flange section of the container body.
[0077] As shown in Fig. 14, in Experimental Example 1, it was confirmed that the protrusions were formed in which the resin films were not bonded to each other, and were hollow. In contrast, in Experimental Examples 2 and 3, the protrusions were formed by bonding the resin films to each other from the tip to the base end. Therefore, unlike Experimental Example 1, it was confirmed that almost no space was formed inside. EXAMPLES
[0078] In Example 2, a protrusion made of a resin film was formed on the step of the flange portion, and a test specimen was prepared in which a top seal was attached to the protrusion, and leakage from the step was confirmed. A leakage confirmation test was performed by spraying Ageless Seal Check Spray. Experimental Examples 4 and 5 are protrusions formed by the manufacturing method of a prefabricated container of the present invention. In Experimental Example 4, a protrusion was formed so as to surround the entire circumference of the storage portion of the container body. In Experimental Example 5, a protrusion was formed on the step formed in the flange portion of the container body.
[0079] As shown in Fig. 15, no leakage from the step formed in the flange was observed in Experimental Examples 4 and 5. Experimental Examples 4 and 5 have a protrusion in which resin films are bonded together from the tip to the base that rises from the flange. This makes it possible to prevent a cavity from being formed between the protrusion and the top seal, and to prevent the contents from leaking or seeping out of the storage section of the container body.
[0080] In addition, the portion attached to the flange and the protrusions form a laminated portion folded in three layers on the resin film. This allows the laminated portion to be embedded in the step. This makes it possible to prevent the contents from leaking or seeping out of the storage portion of the container body. EXAMPLES
[0081] In Example 3, a protrusion made of a resin film was formed on the step of the flange, and a test specimen was prepared in which a top seal was attached to the protrusion, and the cross section of the protrusion was observed under a microscope. Experimental Example 6 is a protrusion formed by the procedure described in Fig. 21. Experimental Example 7 is a protrusion formed by the manufacturing method of a prefabricated container according to the present invention.
[0082] As shown in Fig. 16(a) in Experimental Example 6, when the hollow protrusions were crushed by the top seal, the protrusions were crushed randomly, and a space was created between the top seal and the hollow protrusions. In contrast, as shown in Fig. 16(b) in Experimental Example 7, the protrusions are made of resin films bonded together from the tip to the base end that stands up against the flange. This makes it possible to prevent cavities from forming between the protrusions and the top seal, and to prevent the contents from leaking or seeping out of the storage section of the container body.
[0083] In addition, the portion attached to the flange and the protrusions form a laminated portion folded in three layers on the resin film. This allows the laminated portion to be embedded in the step. This makes it possible to prevent the contents from leaking or seeping out of the storage portion of the container body. EXAMPLES
[0084] In Example 4, a specimen was prepared in which the shape of the hot plate of the hot plate molding machine was changed to form a protrusion, and the protrusion was observed under a microscope. As shown in FIG. 17, the apex angle θ at the apex of the molding part was changed. Table 1 shows the outline and results of Example 4. FIG. 18(a) is a photograph showing the protrusion of Experimental Example 8, and FIG. 18(b) is a photograph showing the protrusion of Experimental Example 9. FIG. 19(a) is a photograph showing the protrusion of Experimental Example 10, and FIG. 19(b) is a photograph showing the protrusion of Experimental Example 11. The dotted lines in FIG. 18 and FIG. 19 indicate the design position of the protrusion.
[0085] [Table 1]
[0086] In Experimental Example 8, the apex angle θ was 64°, and in Experimental Example 9, the apex angle θ was 102°. As a result, as shown in Table 1 and FIG. 18, protrusions were formed at positions shifted from the designed positions of the protrusions. This is thought to be because, as shown in FIG. 20(a), when the apex angle θ is large, the resin film tends to lean to one side when released from the molding part, resulting in a large deviation from the center line C passing through the apex of the triangular molding part. Note that the thick dotted line in FIG. 20 diagrammatically shows the resin film after release from the molding part, and the thin dotted line in FIG. 20 diagrammatically shows the resin film after release at a later time than the thick dotted line.
[0087] In Experimental Example 10, the apex angle θ was 45°, and in Experimental Example 11, the apex angle θ was 23°. As a result, as shown in Table 1 and Figure 19, there was no deviation between the designed position of the protrusion and the position of the actually formed protrusion. This is thought to be because, as shown in Figure 20(b), when the apex angle θ is small, the resin film is less likely to shift to one side when released from the molded part, and deviation from the center line C passing through the apex of the triangular molded part is reduced.
[0088] From the above, the apex angle θ of the forming part is preferably 45° or less. This makes it possible to suppress deviation of the center line of the protrusion when the hot plate is released to form the protrusion, compared to when the apex angle θ is 64° or more. Therefore, it is considered that it is easier to form the protrusion at the designed position. EXAMPLES
[0089] In Example 5, the peel strength and sealing strength of a prefabricated container in which a top seal was attached to a protrusion at a step were measured. Experimental Example 12 is a protrusion formed by the procedure described in FIG. 21. Experimental Examples 13 and 14 are protrusions formed by the manufacturing method of a prefabricated container of the present invention. In Experimental Example 13, a protrusion was formed so as to surround the entire circumference of the storage section of the container body. In Experimental Example 14, a protrusion was formed at a step formed in the flange section of the container body.
[0090] The peel strength was measured by attaching a mechanical force gauge to the top seal 4 attached to the container body 11, and pulling the mechanical force gauge at an angle of 45° in the direction to open the top seal, and measuring the strength at which the container body 11 and the top seal 4 peeled off. The sealing strength was measured by sealing air in the container body 11 using a seal tester, and measuring the pressure at which the top seal 4 attached to the container body 11 was opened. The sealing conditions were 170°C-0.1 MPa-1.0 sec. Three specimens (N=3) were prepared for each test. Table 2 shows the results of Experimental Example 5. The results in Table 2 show the average values of the three specimens.
[0091] [Table 2]
[0092] Experimental Example 13 had higher peel strength and sealing strength than Experimental Example 12. Experimental Example 14 had higher peel strength than Experimental Example 12, but the sealing strength was the same. [Explanation of symbols]
[0093] 1: Assembled container 11: Container body 12: Storage section 13: Flange part 13a: Folded piece 13b: Folded piece 121: Bottom 122: Side 131:Top surface 2: Blank sheet 22: Step 3: Plastic film 31:Protrusion 31a:Tip 31b: Proximal end 32: Pressed area 33: Laminated section 4: Top seal 600: Hot plate forming machine 610: Receiving type 611: First placement section 612: Second placement section 620: Hot plate 621: Opposing part 622: Molding section 623: Cutter section 700: Manufacturing System 710: Feed roller 720: Winding roller S10: Blank sheet cutting process S20: Box manufacturing process S30: Placement process S40: Covering process S41: Suction process S42: Stop process S50: Storage process for stored items S60: Pasting process S70: Trimming process θ: vertical angle
Claims
1. A method for manufacturing a prefabricated container comprising: a container body having a storage section formed by raising a plurality of side surfaces from a bottom surface of a blank sheet, and flange sections in which upper portions of the plurality of side surfaces are folded back and extended toward the outside of the storage section; and a resin film covering an inner surface of the container body, The flange portion has a step formed by bonding the folded pieces of the blank sheet together so as to overlap each other, a placement step of placing the container body on a receiving mold provided opposite to a hot plate of a hot plate molding machine, and placing the resin film between the container body and the hot plate; a coating step of sucking the resin film toward the hot plate to form a protrusion above the step that crosses the step, and coating the inner surface of the container body with the resin film, The coating step includes: a suction step in which a molding part of the hot plate having a triangular cut-out cross section along a direction from the housing part toward the outside is used to suck a protrusion-forming area of the resin film that crosses the step, and then the receiving mold is used to suck the protrusion-forming area with a suction force smaller than that of the molding part; and a stopping step of stopping suction of the molding part while suction is being performed by the receiving mold, thereby forming the protrusion part in which the resin films are bonded to each other from the tip end part to the base end part standing up against the flange part. A method for manufacturing a prefabricated container, comprising:
2. In the covering step, the resin film is heated by the hot plate forming machine and the resin film is sucked toward the hot plate. The method for manufacturing a collapsible container according to claim 1,
3. The method further includes a bonding step of bonding the top seal to the upper surface of the resin film so as to cross the step after the covering step, In the bonding step, When the top seal is attached, the protrusion is tilted toward either the storage section side or the outside of the storage section so as to be aligned with the top seal, and a laminated section folded into three layers is formed in the resin film by the portion of the resin film attached to the flange section and the protrusion. The method for manufacturing a collapsible container according to claim 1,
4. The molded portion has a cross section cut out in an isosceles triangle shape along a direction from the storage portion to the outside. The method for manufacturing a collapsible container according to claim 1,
5. A prefabricated container comprising: a container body having a storage section formed by raising a plurality of side surfaces from a bottom surface of a blank sheet; and a flange section in which upper portions of the plurality of side surfaces are folded back and extended toward the outside of the storage section; and a resin film covering the inner surface of the container body, the flange portion has a step formed by bonding the folded pieces of the blank sheet together so that the folded pieces overlap each other after assembly, the resin film has a protrusion above the step that crosses the step, The protrusion is formed by bonding the resin films together from a tip end to a base end rising from the flange. A prefabricated container characterized by:
6. Further comprising a top seal attached to an upper surface of the resin film, the top seal is attached to the upper surface of the resin film so as to cross the step, The protrusion is disposed along the top seal so as to be inclined toward either the storage section side or the outside of the storage section, The resin film is folded into three layers by a portion attached to the flange portion and the protrusion portion to form a laminated portion. The collapsible container according to claim 5,
Citation Information
Patent Citations
Flat-pack paper container and film adhesion molding machine
WO2021131164A1
Assembled paper container, method for manufacturing assembled paper container, and device for manufacturing assembled paper container
WO2022195923A1
Package container and its blank
JP1994293334A
Assembly paper container, and manufacturing method of assembly paper container
JP2019172339A