Multilayered thin film, and laminate

A fluorine-doped cerium dioxide layer on both sides of a metal thin film enhances the environmental stability and infrared shielding performance of multilayer thin films, addressing cracking issues in high-temperature and high-humidity conditions.

JP2024132893APending Publication Date: 2024-10-01RIKEN TECHNOS CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024019872
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-17
Filing Date
2024-02-14
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Conventional multilayer thin films with metal thin films for infrared shielding suffer from insufficient environmental stability, particularly in high-temperature and high-humidity environments, leading to cracking issues.

Method used

A multilayer thin film structure is developed with a fluorine-doped cerium dioxide thin film laminated on both sides of a metal thin film, such as copper or silver, using a sputtering process to enhance heat and humidity resistance.

Benefits of technology

The multilayer thin film exhibits excellent infrared shielding function and maintains transparency while providing robust protection against environmental stress, including high temperatures and humidity, with reduced cracking.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024132893000001_ABST
    Figure 2024132893000001_ABST
Patent Text Reader

Abstract

To provide a multilayered thin film having infrared-insulating function good in moisture and heat resistance, and a laminate having the multilayered thin film.SOLUTION: A multilayered thin film is laminated with fluorine-doped cerium dioxide thin films directly on both sides of a metal thin film. The rate of fluorine atoms in the fluorine-doped cerium dioxide thin film is preferably 1-60 at% in terms of atomic ratio when a total of atoms in the fluorine-doped cerium dioxide thin film is 100 at%. The metal thin film is composed of copper. The multilayered thin film can be favorably used for a window pane of an architectural structure having adiabaticity, a window of an automobile, and the like.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a multilayer thin film and a laminate having the multilayer thin film. More specifically, the present invention relates to a multilayer thin film having an infrared shielding function and a laminate having the multilayer thin film. [Background technology]

[0002] Conventionally, in order to make the space comfortable with less energy, transparent films having infrared shielding function are often attached to window glass of buildings and roof windows of automobiles. Such transparent films having infrared shielding function include those in which fine particles such as tin-doped indium oxide, antimony-doped tin oxide, and cesium-doped tungsten oxide are contained in any layer of the film, and infrared shielding function is realized by mainly absorbing infrared rays; and those in which a metal thin film such as gold, silver, copper, and palladium is formed as a constituent layer of the film, and infrared shielding function is realized by mainly reflecting infrared rays. In the latter film, transparent thin films such as silicon, silicon oxide, and titanium oxide are often provided on both sides of the metal thin film for the purpose of protecting the metal thin film. However, metal thin films such as gold, silver, copper, and palladium, especially silver thin films, have the disadvantage of insufficient environmental stability, especially wet heat resistance, even if they are protected by providing transparent thin films on both sides. In view of this, it has been proposed to use a thin film of cerium (IV) oxide as a transparent thin film to be provided on both sides of a thin metal film (Patent Document 1).However, when the present inventors conducted further experiments, they found that a multilayer thin film formed by laminating a thin film of cerium (IV) oxide, a thin film of silver, and a thin film of cerium (IV) oxide in this order has the disadvantage that the thin film of cerium (IV) oxide is prone to cracking in a high-temperature and high-humidity environment. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2000-085047 A [Patent Document 2] JP 2022-186664 A Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the present invention is to provide a multilayer thin film having an infrared shielding function and good resistance to moist heat, and a laminate having the multilayer thin film. [Means for solving the problem]

[0005] As a result of extensive research, the present inventors have found that the above object can be achieved by using a specific multilayer thin film.

[0006] That is, the various aspects of the present invention are as follows. [1]. A multilayer film in which a thin film of fluorine-doped cerium dioxide is deposited directly on both sides of a thin metal film. [2]. The multilayer thin film according to item [1], wherein the proportion of fluorine atoms in the fluorine-doped cerium dioxide thin film is, in atomic ratio, 1 to 60 at %, with the total number of atoms in the fluorine-doped cerium dioxide thin film being 100 at %. [3]. Item [1] The multilayer thin film according to item [1], wherein the metal thin film is a copper thin film. [4]. Item 1. The multilayer thin film according to item [1], wherein the metal thin film is an aluminum thin film. [5]. Item 1. The multilayer thin film according to item [1], wherein the metal thin film is a silver thin film. [6]. A laminate having the multilayer thin film according to any one of items [1] to [5] on a part or all of the surfaces of a substrate. [7]. An article having the multilayer thin film according to any one of items [1] to [5]. [8]. A method for producing a multilayer thin film in which a fluorine-doped cerium dioxide thin film is directly laminated on both sides of a metal thin film, the step of forming the fluorine-doped cerium dioxide thin film comprising the steps of: Using a sputtering device, a cerium dioxide target and an organic fluorine compound gas are used. (1) a sub-step of mounting the cerium dioxide target on a target mounting jig of the sputtering apparatus; (2) a sub-step of reducing the pressure in the sputtering chamber of the sputtering apparatus to a predetermined pressure a; (3) a sub-step of introducing a mixed gas of a sputtering gas and the gas of the organic fluorine compound into a sputtering chamber of the sputtering apparatus so that the pressure in the sputtering chamber becomes a predetermined pressure b; and (4) a sub-step of applying power to the cerium dioxide target and sputtering the fluorine-doped cerium dioxide thin film; wherein a mixing ratio of the sputtering gas to the organic fluorine compound gas (volume of the sputtering gas / volume of the organic compound gas) is 95 / 5 to 99.99 / 0.01. forming the fluorine-doped cerium dioxide thin film; A method for producing the multilayer thin film. [9]. The manufacturing method according to item [8], wherein the sputtering apparatus is a roll-to-roll type sputtering apparatus. Effect of the Invention

[0007] The multilayer thin film of the present invention has an infrared shielding function and good moist heat resistance. A preferred multilayer thin film of the present invention has good infrared shielding function and transparency, and good moist heat resistance. Therefore, the multilayer thin film of the present invention and a laminate having the multilayer thin film can be suitably used in articles requiring an infrared shielding function. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] As used herein, the term "inorganic material" includes mixtures containing two or more inorganic materials, and the term "organic compound" includes mixtures containing two or more organic compounds.

[0009] In this specification, the term "resin" is used to include a resin mixture containing two or more resins, and a resin composition containing components other than resin.

[0010] In this specification, the term "film" is used interchangeably or interchangeably with "sheet." In this specification, the terms "film" and "sheet" are used for those that can be industrially wound into a roll. The term "plate" is used for those that cannot be industrially wound into a roll. In addition, in this specification, laminating a certain layer and another layer in order includes both directly laminating the layers and laminating the layers with one or more other layers, such as an anchor coat, interposed between the layers.

[0011] In this specification, the term "more than" in relation to a numerical range means a certain number or more than a certain number. For example, 20% or more means 20% or more than 20%. The term "less than" in relation to a numerical range means a certain number or less than a certain number. For example, 20% or less means 20% or less than 20%. Furthermore, the symbol "~" in relation to a numerical range means a certain number, more than a certain number and less than another certain number, or another certain number. Here, the other certain number is a number larger than the certain number. For example, 10 to 90% means 10%, more than 10% and less than 90%, or 90%. Furthermore, the upper and lower limits of the numerical range can be arbitrarily combined, and an embodiment in which the values ​​are arbitrarily combined can be read. For example, from a statement regarding the numerical range of a certain characteristic such as "usually 10% or more, preferably 20% or more. On the other hand, it is usually 40% or less, preferably 30% or less" or "usually 10 to 40%, preferably 20 to 30%," it can be read that the numerical range of the certain characteristic is 10 to 40%, 20 to 30%, 10 to 30%, or 20 to 40% in one embodiment.

[0012] Other than in the examples, or where otherwise specified, all numerical values ​​used in the specification and claims should be understood to be modified by the term "about." Without attempting to limit the application of the doctrine of equivalents to the scope of the claims, each numerical value should be construed in light of the number of significant digits and by applying ordinary rounding techniques.

[0013] In this specification, terms specifying shapes or geometric conditions, such as parallel, orthogonal, and perpendicular, are intended to include substantially the same state in addition to their strict meanings.

[0014] In this specification, when it is explained that "comprises a certain substance", it is to be understood that in one embodiment, it contains a certain substance, consists of a certain substance, or consists only of a certain substance. For example, from the explanation that "composition A comprises substance a1 and substance a2", it is to be understood that in one embodiment, composition A comprises substance a1 and substance a2, composition A consists of substance a1 and substance a2, or composition A consists only of substance a1 and substance a2.

[0015] 1. Multi-layer thin film: The multilayer thin film of the present invention is a multilayer thin film in which a fluorine-doped cerium dioxide thin film is directly laminated on both sides of a metal thin film.

[0016] 1-1. Fluorine-doped cerium dioxide thin film: The fluorine-doped cerium dioxide thin film functions to protect the metal thin film from environmental loads such as high temperature and high humidity. The fluorine-doped cerium dioxide thin film is a thin film containing atoms derived from cerium dioxide (cerium (IV) oxide, CeO2) and atoms derived from an organic fluorine compound. In a typical embodiment, the fluorine-doped cerium dioxide thin film may include a compound containing atoms derived from the cerium dioxide and atoms derived from the organic fluorine compound, and in which the cerium dioxide is modified with atoms derived from the organic fluorine compound.

[0017] The ratio of fluorine atoms in the fluorine-doped cerium dioxide thin film can be appropriately selected in consideration of the use of the multilayer thin film. The ratio of fluorine atoms in the fluorine-doped cerium dioxide thin film may be, in terms of atomic ratio, usually 1 at% or more, preferably 4 at% or more, more preferably 7 at% or more, even more preferably 10 at% or more, even more preferably 12 at% or more, and most preferably 16 at% or more, with the sum of atoms in the fluorine-doped cerium dioxide thin film being 100 at%, from the viewpoint of wet heat resistance. On the other hand, the ratio of fluorine atoms in the fluorine-doped cerium dioxide thin film may be usually 60 at% or less, preferably 55 at% or less, more preferably 50 at% or less, and even more preferably 45 at% or less, from the viewpoint of transparency.

[0018] The proportion of fluorine atoms in the fluorine-doped cerium dioxide thin film can be determined by X-ray photoelectron spectroscopy (hereinafter sometimes referred to as "XPS analysis"). XPS analysis can be performed, for example, using an XPS analyzer and aluminum Kα rays or magnesium Kα rays as X-rays. For XPS analysis, the following references can be referred to. Reference: MPSeah and WADerch, Surface and Interface Analysis 1, 2 (1979)

[0019] 1 is a spectrum of the fluorine-doped cerium dioxide thin film of Example 1 in the Examples described later, which was analyzed by XPS in the energy range of -10 to 1350 eV. The spectrum shows a peak attributable to the carbon 1s orbital (C1s) at around 290 eV, a peak attributable to the oxygen 1s orbital (O1s) at around 530 eV, a peak attributable to the fluorine 1s orbital (F1s) at around 680 eV, and a peak attributable to the cerium 3d orbital (Ce3d) at around 880 eV, and the atomic ratio of each element can be calculated from the area ratio of these peaks. In the case of the fluorine-doped cerium dioxide thin film of Example 1, the carbon was 30 at%, oxygen was 19 at%, fluorine was 39 at%, and cerium was 12 at%.

[0020] The ratio of fluorine atoms in one of the fluorine-doped cerium dioxide thin films directly laminated on both sides of the metal thin film may be the same as or different from the ratio of fluorine atoms in the other.

[0021] The fluorine-doped cerium dioxide thin film is formed by using the cerium dioxide and the organic fluorine compound. The method for forming the fluorine-doped cerium dioxide thin film by using the cerium dioxide and the organic fluorine compound is not particularly limited. A preferred method for forming the fluorine-doped cerium dioxide thin film by using the cerium dioxide and the organic fluorine compound is a sputtering method.

[0022] When the fluorine-doped cerium dioxide thin film is formed by sputtering, the cerium dioxide may be of high purity, where high purity means a purity of 3N (99.9%) or higher, preferably 4N (99.99%) or higher.

[0023] Preferred methods for forming the fluorine-doped cerium dioxide thin film by sputtering include, for example, the method disclosed in JP 2022-186664 A and the method disclosed in paragraphs 0058 to 0076 of JP 2019-123872 A as a method for producing an organic-inorganic hybrid film by sputtering. All of the disclosures in JP 2022-186664 A and JP 2019-123872 A are incorporated herein by reference.

[0024] When the fluorine-doped cerium dioxide thin film is formed using the method disclosed in JP 2022-186664 A, a gas of an organic fluorine compound is used as the organic fluorine compound. Examples of such organic fluorine compounds include compounds having a structure in which one or more hydrogen atoms of saturated hydrocarbons such as tetrafluoromethane, trifluoromethane, difluoromethane, fluoromethane, and 1,1,1,2-tetrafluoroethane are substituted with fluorine atoms, and which are gaseous under standard conditions (temperature 25°C, pressure 100 KPa); compounds having a structure in which one or more hydrogen atoms of unsaturated hydrocarbons are substituted with fluorine atoms, such as compounds having a structure in which one or more hydrogen atoms of α-olefins such as tetrafluoroethylene, trifluoroethylene, vinylidene fluoride, vinyl fluoride, hexafluoropropylene, pentafluoropropylene, tetrafluoropropylene, trifluoropropylene, and chlorotrifluoroethylene are substituted with fluorine atoms, and which are gaseous under standard conditions (temperature 25°C, pressure 100 KPa); and mixtures thereof. Among these, tetrafluoromethane is preferred as the organic fluorine compound.

[0025] In the case of forming the fluorine-doped cerium dioxide thin film using the method disclosed in paragraphs 0058 to 0076 of JP 2019-123872 A as a case of producing an organic-inorganic hybrid film by a sputtering method, the organic fluorine compound used is preferably a fluorine-based resin from the viewpoint of manufacturability of a molded body as a target. The fluorine-based resin is a resin containing a constituent unit derived from a monomer containing a fluorine atom (a compound having a structure in which one or more hydrogen atoms are substituted with fluorine atoms and having polymerizability). Examples of the fluorine-based resin include polytetrafluoroethylene, polyhexafluoropropylene, polyvinylidene fluoride, polyvinyl fluoride, tetrafluoroethylene-hexafluoropropylene copolymer, tetrafluoroethylene-ethylene copolymer, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, chlorotrifluoroethylene-ethylene copolymer, and polychlorotrifluoroethylene. Among these, the fluorine-based resins are preferably polytetrafluoroethylene and polyvinylidene fluoride.

[0026] The thickness of the fluorine-doped cerium dioxide thin film can be appropriately selected in consideration of the use of the multilayer thin film. The thickness of the fluorine-doped cerium dioxide thin film may be usually 1 nm or more, preferably 5 nm or more, more preferably 10 nm or more, even more preferably 15 nm or more, and most preferably 20 nm or more, from the viewpoint of reliably obtaining the function of protecting the metal thin film from environmental loads such as high temperature and high humidity. On the other hand, the thickness of the fluorine-doped cerium dioxide thin film may be usually 500 nm or less, preferably 400 nm or less, more preferably 300 nm or less, even more preferably 200 nm or less, and most preferably 150 nm or less, from the viewpoint of crack resistance.

[0027] The thickness of one of the fluorine-doped cerium dioxide thin films directly laminated on both sides of the metal thin film may be the same as or different from that of the other.

[0028] 1-2. Metal thin film layer The metal thin film acts to exhibit an infrared shielding function. The metal thin film may be any metal thin film capable of exhibiting an infrared shielding function, and may exhibit the infrared shielding function by mainly reflecting infrared rays, or may exhibit the infrared shielding function by mainly absorbing infrared rays.

[0029] Examples of the metal thin film include thin films of metals such as silver, copper, aluminum, indium, tin, chromium, nickel, gold, and palladium. Of these, silver is preferred as the metal thin film from the viewpoints of reflectivity in the infrared region (high infrared shielding function) and transmittance (transparency) in the visible light region. Of these, copper and aluminum are preferred as the metal thin film from the viewpoints of environmental stability, particularly resistance to moist heat.

[0030] The method for forming the metal thin film is not particularly limited, and examples of the method for forming the metal thin film include sputtering, vacuum deposition, and electron beam deposition.

[0031] The thickness of the metal thin film can be appropriately selected in consideration of the use of the multilayer thin film. From the viewpoint of infrared shielding function, the thickness of the metal thin film may be usually 1 nm or more, preferably 3 nm or more, more preferably 5 nm or more, even more preferably 7 nm or more, and most preferably 10 nm or more. On the other hand, from the viewpoint of transparency, the thickness of the metal thin film may be preferably 50 nm or less, more preferably 40 nm or less, even more preferably 30 nm or less, and most preferably 20 nm or less.

[0032] 2.Laminate: The laminate of the present invention is a laminate having the multilayer thin film of the present invention on a part or all of the surfaces of a substrate. Hereinafter, the present invention will be described with the fluorine-doped cerium dioxide thin film that is directly laminated on both surfaces of the metal thin film being the layer closest to the substrate as fluorine-doped cerium dioxide thin film a, and the other as fluorine-doped cerium dioxide thin film b.

[0033] The substrate can be appropriately selected in consideration of the application of the laminate. The surface of the substrate on which the multilayer thin film is laminated may be smooth or have a three-dimensional shape. Here, the three-dimensional shape means a shape that includes a non-planar shape such as unevenness in at least a part thereof. In one typical embodiment, the substrate is a film, a sheet, or a plate.

[0034] Examples of the substrate include inorganic glass films, inorganic glass sheets, and inorganic glass plates such as soda lime glass, borosilicate glass, and quartz glass.

[0035] Examples of the substrate include resin films, resin sheets, or resin plates such as cellulose ester resins such as triacetyl cellulose; polyester resins such as polyethylene terephthalate; cyclic hydrocarbon resins such as ethylene norbornene copolymers; acrylic resins such as polymethyl methacrylate, polyethyl methacrylate, and vinylcyclohexane-methyl (meth)acrylate copolymers; aromatic polycarbonate resins; polyolefin resins such as polypropylene and 4-methyl-pentene-1; polyamide resins; polyarylate resins; polymeric urethane acrylate resins; and polyimide resins. These resin films include non-stretched films, uniaxially stretched films, and biaxially stretched films. These resin films also include laminated resin films in which one or more of these are laminated in two or more layers. These resin sheets also include non-stretched sheets, uniaxially stretched sheets, and biaxially stretched sheets. These resin sheets also include laminated resin sheets in which one or more of these are laminated in two or more layers. These resin plates include laminated resin plates in which one or more of these materials are laminated in two or more layers.

[0036] The substrate may have a functional layer. As an embodiment of the substrate having a functional layer, for example, the substrate may have a functional layer on at least one surface of the inorganic glass film, the inorganic glass sheet, the inorganic glass plate, the resin film, the resin sheet, or the resin plate, and the surface on the functional layer side or the surface opposite to the functional layer may be laminated with the multilayer thin film.

[0037] Examples of the functional layer include layers having functions such as hardness improvement, anchoring, low refractive index, high refractive index, ultraviolet shielding, electromagnetic wave shielding, electromagnetic wave reflection, visibility control (blinding), and viewing angle control. The functional layer may be a coating film (including a hard coat) formed using a paint, or a film formed by a dry coating method such as a sputtering method, a vacuum deposition method, or a chemical vapor deposition method.

[0038] When the inorganic glass film, the inorganic glass sheet, or the inorganic glass plate is used as the substrate, the thickness of the inorganic glass film, the inorganic glass sheet, or the inorganic glass plate can be appropriately selected in consideration of the use of the laminate. The thickness of the inorganic glass film, the inorganic glass sheet, or the inorganic glass plate may be usually 20 μm or more, preferably 50 μm or more, from the viewpoint of the handleability of the laminate. Also, from the viewpoint of the impact resistance of the inorganic glass, it may be preferably 1 mm or more, more preferably 1.5 mm or more. On the other hand, from the viewpoint of weight reduction of the article using the laminate, it may be usually 6 mm or less, preferably 4.5 mm or less, more preferably 3 mm or less.

[0039] When the resin film, the resin sheet, or the resin plate is used as the substrate, the thickness of the resin film, the resin sheet, or the resin plate can be appropriately selected in consideration of the use of the laminate. The thickness of the resin film, the resin sheet, or the resin plate may be usually 20 μm or more, preferably 50 μm or more, from the viewpoint of the handleability of the laminate. When the laminate is used for an application that does not require high rigidity, it may be usually 250 μm or less, preferably 150 μm or less, from the viewpoint of economic efficiency. When the laminate is used for an application that requires high rigidity, it may be usually 300 μm or more, preferably 500 μm or more, more preferably 600 μm or more, from the viewpoint of maintaining rigidity. In addition, it may be usually 1500 μm or less, preferably 1200 μm or less, more preferably 1000 μm or less, from the viewpoint of responding to the demand for thinning of the article using the laminate.

[0040] The substrate may be transparent, opaque, colored transparent, or colored opaque (having a concealing property), and can be appropriately selected in consideration of the use of the laminate.

[0041] The fluorine-doped cerium dioxide thin film a is present on the side closer to the substrate of the fluorine-doped cerium dioxide thin films directly laminated on both sides of the metal thin film. That is, in the laminate of the present invention, the fluorine-doped cerium dioxide thin film a is laminated on a part or all of the surfaces of the substrate.

[0042] The fluorine-doped cerium dioxide thin film a in the laminate of the present invention, that is, the fluorine-doped cerium dioxide thin film in the multilayer thin film of the present invention, has been explained in "1. Multilayer thin film".

[0043] The substrate and the fluorine-doped cerium dioxide thin film a may be laminated directly or with one or more other layers such as an anchor coat interposed therebetween.

[0044] In the laminate of the present invention, the metal thin film is laminated directly on the surface of the fluorine-doped cerium dioxide thin film a.

[0045] The metal thin film in the laminate of the present invention, that is, the metal thin film in the multilayer thin film of the present invention, has been explained in "1. Multilayer thin film".

[0046] In the laminate of the present invention, the fluorine-doped cerium dioxide thin film b is further laminated directly on the surface of the metal thin film.

[0047] The fluorine-doped cerium dioxide thin film b in the laminate of the present invention, that is, the fluorine-doped cerium dioxide thin film in the multilayer thin film of the present invention, has been explained in "1. Multilayer thin film".

[0048] The laminate of the present invention may further have a topcoat layer on the surface of the fluorine-doped cerium dioxide thin film b, if desired. The topcoat layer may be a coating film (including a hard coat) formed using a paint, or a film formed by a dry coating method such as a sputtering method, a vacuum deposition method, or a chemical vapor deposition method. The thickness of the topcoat layer may be preferably about 0.01 to 5 μm, more preferably about 0.05 to 1 μm.

[0049] 3.Laminate manufacturing method (part 1): An embodiment of the method for producing a laminate of the present invention will be described below, using a batch-type sputtering apparatus, the conceptual diagram of which is shown in FIG.

[0050] 3-1. Deposition of fluorine-doped cerium dioxide thin film a: First, the cerium dioxide target 1 is mounted on the target mounting jig 2. By mounting the cerium dioxide target 1 on the target mounting jig 2, the cerium dioxide target 1 is connected to a power source (not shown). In addition, a flow path for a medium such as water is provided inside the target mounting jig 2, so that the temperature of the cerium dioxide target 1 can be controlled to a predetermined temperature.

[0051] Next, the substrate 4 is attached to the sputtering table 3 and rotated at a predetermined rotation speed. The predetermined rotation speed of the sputtering table 3 may be usually 1 to 1000 rpm, and preferably 2 to 50 rpm. During the formation of the fluorine-doped cerium dioxide thin film a, the rotation speed may be constant, or may be changed as desired.

[0052] Next, the inside of the sputtering chamber 5 is evacuated from the exhaust port 6 by an exhaust device (not shown) to make the inside of the sputtering chamber 5 at a pressure equal to or lower than a predetermined pressure a during film formation. -5 ~10 -2 Pa, preferably 10 -4 ~5×10 -3 It may be on the order of Pa.

[0053] Next, a mixed gas of the sputtering gas and the organic fluorine compound gas is introduced into the sputtering chamber 5 from the sputtering gas inlet 7 so that the inside of the sputtering chamber 5 is at a predetermined pressure b during film formation. At this time, the sputtering gas and the organic fluorine compound gas may be prepared separately and introduced while the two gas flows are joined and mixed, or the mixed gas of the sputtering gas and the organic fluorine compound gas may be prepared in advance and introduced. Also, the amount of the mixed gas introduced may be fixed and the opening of the exhaust port 6 may be feedback-controlled to keep the sputtering pressure constant.

[0054] The mixing ratio of the sputtering gas and the gas of the organic fluorine compound can be appropriately determined from the viewpoint of making the composition of the fluorine-doped cerium dioxide thin film a (the ratio of fluorine atoms in the fluorine-doped cerium dioxide thin film a) a desired composition. The mixing ratio of the sputtering gas and the gas of the organic fluorine compound (volume of the sputtering gas / volume of the gas of the organic compound) may be usually 95 / 5 to 99.99 / 0.01, preferably 97 / 3 to 99.9 / 0.1, more preferably 98 / 2 to 99.7 / 0.3, even more preferably 98.3 / 1.7 to 99.5 / 0.5, and most preferably 98.6 / 1.4 to 99.3 / 0.7, depending on the type of the gas of the organic fluorine compound.

[0055] The sputtering gas is not particularly limited as long as it is a gas that can be used for sputtering, and may be any known sputtering gas. Examples of the sputtering gas include noble gases such as argon and krypton, and mixtures of these gases with oxygen and nitrogen. The sputtering gas may preferably be noble gases such as argon and krypton.

[0056] The above-mentioned organic fluorine compound gas is not limited to an organic fluorine compound gas that is gaseous under standard conditions (temperature 25°C, pressure 100 KPa). The above-mentioned organic fluorine compound gas may be an organic fluorine compound gas that becomes gaseous by heating and / or reducing pressure. In this case, it goes without saying that the gaseous state is adjusted to a predetermined temperature and pressure before use. In this case, it is also preferable that the temperature inside the sputtering chamber 5 is also adjusted to a predetermined temperature.

[0057] Examples of such organic fluorine compounds include compounds having a structure in which one or more hydrogen atoms of saturated hydrocarbons such as tetrafluoromethane, trifluoromethane, difluoromethane, fluoromethane, and 1,1,1,2-tetrafluoroethane are substituted with fluorine atoms, and which are gaseous under standard conditions (temperature 25°C, pressure 100 KPa); compounds having a structure in which one or more hydrogen atoms of unsaturated hydrocarbons are substituted with fluorine atoms, such as compounds having a structure in which one or more hydrogen atoms of α-olefins such as tetrafluoroethylene, trifluoroethylene, vinylidene fluoride, vinyl fluoride, hexafluoropropylene, pentafluoropropylene, tetrafluoropropylene, trifluoropropylene, and chlorotrifluoroethylene are substituted with fluorine atoms, and which are gaseous under standard conditions (temperature 25°C, pressure 100 KPa); and mixtures thereof. Among these, tetrafluoromethane is preferred as the organic fluorine compound.

[0058] As the gas of the above organic fluorine compound, one kind or a mixture of two or more kinds of these gases can be used.

[0059] The predetermined pressure b (sputtering pressure) in the sputtering chamber 5 during the above film formation may be usually 0.05 to 5 Pa, preferably 0.1 to 1 Pa, from the viewpoint of stabilizing the discharge and enabling continuous film formation.

[0060] Next, a predetermined power is applied to the cerium dioxide target 1 to cause discharge, and when the discharge state becomes stable, the shutter 8 is opened to sputter the cerium dioxide target 1 and form the fluorine-doped cerium dioxide thin film a on the surface of the substrate 4. At this time, cooling water of a predetermined temperature and flow rate is made to flow through the target installation jig 2 to control the temperature of the cerium dioxide target 1 to a predetermined temperature. In addition, by keeping the shutter 8 closed until the discharge state becomes stable, it is possible to prevent the above-mentioned contaminants from adhering to the surface of the substrate 4 during pre-sputtering (an operation for removing contaminants such as dirt and water on the surface of the cerium dioxide target 1 (by applying power to blow them away)). Here, the power applied is usually an AC power, preferably a high-frequency AC power, since the target needs to have a sufficiently high conductivity in order to use a DC current.

[0061] The composition of the fluorine-doped cerium dioxide thin film a (the proportion of fluorine atoms in the fluorine-doped cerium dioxide thin film a) can be adjusted to a desired composition by adjusting the power input to the cerium dioxide target 1, the mixing ratio of the sputtering gas and the organofluorine compound gas, and the flow rate of the mixed gas of the sputtering gas and the organofluorine compound gas (predetermined pressure b (sputtering pressure) in the sputtering chamber 5 during film formation). The relationship between the input power amount, the mixing ratio, and the flow rate of the mixed gas and the composition can be determined by conducting a preliminary experiment.

[0062] The thickness of the fluorine-doped cerium dioxide thin film a can be adjusted to a desired thickness by adjusting the power input to the cerium dioxide target 1, the mixture ratio of the sputtering gas and the organofluorine compound gas, the flow rate of the mixed gas of the sputtering gas and the organofluorine compound gas (predetermined pressure b (sputtering pressure) in the sputtering chamber 5 during film formation), and the film formation time. The relationship between the input power amount, the mixture ratio, the flow rate of the mixed gas, the film formation time, and the film thickness can be determined by a preliminary experiment.

[0063] 3-2. Metal thin film deposition: Subsequently, the above-mentioned metal thin film is formed directly on the fluorine-doped cerium dioxide thin film a surface of the intermediate laminate a having the above-mentioned fluorine-doped cerium dioxide thin film a on one surface of the substrate 4 .

[0064] First, a metal target is attached to the target setting jig 2 .

[0065] Next, the intermediate laminate a is attached to the sputtering table 3 so that the surface on the fluorine-doped cerium dioxide thin film a side becomes the deposition surface, and rotated at a predetermined rotation speed. The predetermined rotation speed of the sputtering table 3 may be usually 1 to 1000 rpm, preferably 2 to 50 rpm. The rotation speed may be constant during deposition of the metal thin film, or may be changed as desired.

[0066] Next, the inside of the sputtering chamber 5 is evacuated from the exhaust port 6 by an exhaust device (not shown) to make the pressure in the sputtering chamber 5 at the time of film formation equal to or lower than a predetermined pressure a'. -5 ~10 -2 Pa, preferably 10 -4 ~5×10 -3 It may be on the order of Pa.

[0067] Next, sputtering gas is introduced into the sputtering chamber 5 from the sputtering gas inlet 7 so that the pressure in the sputtering chamber 5 becomes a predetermined pressure b' during film formation. The amount of the sputtering gas introduced may be fixed, and the opening of the exhaust port 6 may be feedback-controlled to keep the sputtering pressure constant. The sputtering gas is not particularly limited as long as it is a gas that can be used for sputtering, and may be any known sputtering gas. The sputtering gas may be a noble gas, such as argon or krypton, preferably.

[0068] The predetermined pressure b' (sputtering pressure) in the sputtering chamber 5 during the above film formation may be usually 0.05 to 5 Pa, preferably 0.1 to 1 Pa, from the viewpoint of stabilizing the discharge and enabling continuous film formation.

[0069] Next, a predetermined power is applied to the metal target to cause discharge, and when the discharge state becomes stable, the shutter 8 is opened to sputter the metal target, and the metal thin film is formed directly on the surface of the intermediate laminate a on the side of the fluorine-doped cerium dioxide thin film a. At this time, cooling water of a predetermined temperature and flow rate is made to flow through the target installation jig 2 to control the temperature of the metal target to a predetermined temperature. In addition, by keeping the shutter 8 closed until the discharge state becomes stable, it is possible to prevent the adhesion of the contaminants on the surface of the intermediate laminate a during pre-sputtering (an operation to remove contaminants such as dirt and water on the surface of the intermediate laminate a (by applying power to blow them away)). Here, the power applied may be DC power or AC power. Since metals such as silver, copper, and aluminum have sufficiently high electrical conductivity, the power applied may preferably be DC power.

[0070] The thickness of the metal thin film can be adjusted to a desired thickness by adjusting the power input to the metal target, the flow rate of the sputtering gas (predetermined pressure b' (sputtering pressure) in the sputtering chamber 5 during film formation), and the film formation time. The relationship between the amount of input power, the flow rate of the sputtering gas, the film formation time, and the film thickness can be determined by a preliminary experiment.

[0071] 3-3. Deposition of fluorine-doped cerium dioxide thin film b: Furthermore, the fluorine-doped cerium dioxide thin film a is formed on one surface of the substrate 4, and the fluorine-doped cerium dioxide thin film b is formed directly on the metal thin film surface of the intermediate laminate b having the metal thin film directly on the fluorine-doped cerium dioxide thin film a surface.

[0072] The fluorine-doped cerium dioxide thin film b can be formed in the same manner as described in "3-1. Formation of fluorine-doped cerium dioxide thin film a".

[0073] The laminate of the present invention can be obtained by forming the fluorine-doped cerium dioxide thin film b directly on the metal thin film surface of the intermediate laminate b.

[0074] 4.Laminate manufacturing method (part 2): An embodiment of the method for producing a laminate of the present invention using a roll-to-roll sputtering apparatus, the conceptual diagram of which is shown in FIG. 2-2, will be described below.

[0075] First, the cerium dioxide targets 9, 9' are mounted on the target mounting jigs 10, 10'. By mounting the cerium dioxide targets 9, 9' on the target mounting jigs 10, 10', the cerium dioxide targets 9, 9' are connected to a power source (not shown). In addition, a flow path for a medium such as water is provided inside the target mounting jigs 10, 10', so that the temperature of the cerium dioxide targets 9, 9' can be controlled to a predetermined temperature.

[0076] Next, the film substrate 11 is passed through. That is, a film roll 13 of the film substrate 11 is set on the pay-out roll 12, a take-up tube (not shown) is set on the take-up roll 14, and the film substrate 11 is paid out from the film roll 13, wrapped around the sputter roll 16 via the transfer roll 15, and taken up by the take-up tube set on the take-up roll 14 via the transfer roll 15'. The film substrate 11 may be passed through before the inorganic targets 9, 9' are attached to the target setting jigs 10, 10', respectively.

[0077] Next, the inside of the sputtering chamber 17 is evacuated from the exhaust port 18 by an exhaust device (not shown) to reduce the pressure to a predetermined pressure a or less in the sputtering chamber 17 during film formation. -5 ~10 -2 Pa, preferably 10 -4 ~6×10 -3 It may be on the order of Pa.

[0078] Next, a mixed gas of the sputtering gas and the organic fluorine compound gas is introduced into the sputtering chamber 17 from the sputtering gas inlet 19 so that the inside of the sputtering chamber 17 becomes a predetermined pressure b during film formation. At this time, the sputtering gas and the organic fluorine compound gas may be prepared separately and introduced while the two gas flows are joined and mixed, or the mixed gas of the sputtering gas and the organic fluorine compound gas may be prepared in advance and introduced. Also, the amount of the mixed gas introduced may be fixed and the opening of the exhaust port 18 may be feedback-controlled to keep the sputtering pressure constant.

[0079] The mixing ratio of the sputtering gas and the gas of the organic fluorine compound can be appropriately determined from the viewpoint of making the composition of the fluorine-doped cerium dioxide thin film a (the ratio of fluorine atoms in the fluorine-doped cerium dioxide thin film a) a desired composition. The mixing ratio of the sputtering gas and the gas of the organic fluorine compound (volume of the sputtering gas / volume of the gas of the organic compound) may be usually 95 / 5 to 99.99 / 0.01, preferably 97 / 3 to 99.9 / 0.1, more preferably 98 / 2 to 99.7 / 0.3, even more preferably 98.3 / 1.7 to 99.5 / 0.5, and most preferably 98.6 / 1.4 to 99.3 / 0.7, depending on the type of the gas of the organic fluorine compound.

[0080] The sputtering gas is not particularly limited as long as it is a gas that can be used for sputtering, and may be any known sputtering gas. Examples of the sputtering gas include noble gases such as argon and krypton, and mixtures of these gases with oxygen and nitrogen. The sputtering gas may preferably be noble gases such as argon and krypton.

[0081] The above-mentioned organic fluorine compound gas is not limited to an organic fluorine compound gas that is gaseous under standard conditions (temperature 25°C, pressure 100 KPa). The above-mentioned organic fluorine compound gas may be an organic fluorine compound gas that becomes gaseous by heating and / or reducing pressure. In this case, it goes without saying that the gaseous state is adjusted to a predetermined temperature and pressure before use. In this case, it is also preferable that the temperature inside the sputtering chamber 17 is also adjusted to a predetermined temperature.

[0082] Examples of such organic fluorine compounds include compounds having a structure in which one or more hydrogen atoms of saturated hydrocarbons such as tetrafluoromethane, trifluoromethane, difluoromethane, fluoromethane, and 1,1,1,2-tetrafluoroethane are substituted with fluorine atoms, and which are gaseous under standard conditions (temperature 25°C, pressure 100 KPa); compounds having a structure in which one or more hydrogen atoms of unsaturated hydrocarbons are substituted with fluorine atoms, such as compounds having a structure in which one or more hydrogen atoms of α-olefins such as tetrafluoroethylene, trifluoroethylene, vinylidene fluoride, vinyl fluoride, hexafluoropropylene, pentafluoropropylene, tetrafluoropropylene, trifluoropropylene, and chlorotrifluoroethylene are substituted with fluorine atoms, and which are gaseous under standard conditions (temperature 25°C, pressure 100 KPa); and mixtures thereof. Among these, tetrafluoromethane is preferred as the organic fluorine compound.

[0083] As the gas of the above organic fluorine compound, one kind or a mixture of two or more kinds of these gases can be used.

[0084] The predetermined pressure b (sputtering pressure) in sputtering chamber 17 during the above film formation may be usually 0.05 to 5 Pa, preferably 0.1 to 1 Pa, from the viewpoint of stabilizing discharge and enabling continuous film formation.

[0085] Next, a predetermined power is applied to the cerium dioxide targets 9, 9' to cause discharge, and when the discharge state becomes stable, the cerium dioxide targets 9, 9' are sputtered while the film substrate 11 is moved at a predetermined line speed, and the above-mentioned fluorine-doped cerium dioxide thin film a is formed on the surface of the film substrate 11. At this time, cooling water of a predetermined temperature and at a predetermined flow rate is flowed through the target installation jigs 10, 10' to control the temperature of the cerium dioxide targets 9, 9' to a predetermined temperature. The power applied here is usually AC power, preferably high-frequency AC power, since the target needs to have a sufficiently high conductivity in order to use a DC current.

[0086] The composition of the fluorine-doped cerium dioxide thin film a (the proportion of fluorine atoms in the fluorine-doped cerium dioxide thin film a) can be adjusted to a desired composition by adjusting the power input to the cerium dioxide targets 9, 9', the mixing ratio of the sputtering gas and the organofluorine compound gas, and the flow rate of the mixed gas of the sputtering gas and the organofluorine compound gas (predetermined pressure b (sputtering pressure) in the sputtering chamber 17 during film formation). The relationship between the input power amount, the mixing ratio, and the flow rate of the mixed gas and the composition can be determined by conducting a preliminary experiment.

[0087] The thickness of the fluorine-doped cerium dioxide thin film a can be adjusted to a desired thickness by adjusting the power input to the cerium dioxide targets 9, 9', the mixture ratio of the sputtering gas and the organofluorine compound gas, the flow rate of the mixed gas of the sputtering gas and the organofluorine compound gas (predetermined pressure b (sputtering pressure) in the sputtering chamber 17 during film formation), and the film formation time. The relationship between the input power amount, the mixture ratio, the flow rate of the mixed gas, the film formation time, and the film thickness can be obtained by performing a preliminary experiment.

[0088] Also, the film substrate 11 may be reciprocated a predetermined distance and passed two or more times through the position facing the cerium dioxide targets 9, 9' of the sputter roll 16 (i.e., the position where the fluorine-doped cerium dioxide thin film a is formed). By increasing the line speed (the running speed of the film substrate 11), it is possible to suppress problems such as the film substrate 11 bending due to heat and the fluorine-doped cerium dioxide thin film a cracking due to the bending of the film substrate 11. Also, when attempting to increase the thickness of the fluorine-doped cerium dioxide thin film a, it becomes easy to ensure a stable line speed.

[0089] In producing the multilayer thin film of the present invention as a film roll, the thickness of the fluorine-doped cerium dioxide thin film a may be, from the viewpoint of crack resistance, preferably 100 nm or less, more preferably 70 nm or less, even more preferably 50 nm or less, still more preferably 40 nm or less, and most preferably 30 nm or less, while from the viewpoint of reliably protecting the metal thin film from environmental loads such as high temperature and high humidity, the thickness may be usually 1 nm or more, preferably 5 nm or more, more preferably 10 nm or more, even more preferably 15 nm or more, and most preferably 20 nm or more.

[0090] 4-2. Metal thin film deposition: Subsequently, the above-mentioned metal thin film is formed directly on the fluorine-doped cerium dioxide thin film a surface of the intermediate laminate a having the above-mentioned fluorine-doped cerium dioxide thin film a on one surface of the film substrate 11 .

[0091] First, a metal target is attached to the target setting jig 10, 10'.

[0092] Next, the intermediate laminate a is passed through so that the surface on the fluorine-doped cerium dioxide thin film a side becomes the film formation surface.

[0093] Next, the inside of the sputtering chamber 17 is evacuated from the exhaust port 18 by an exhaust device (not shown) to make the pressure in the sputtering chamber 17 at the time of film formation equal to or lower than a predetermined pressure a'. -5 ~10 -2 Pa, preferably 10 -4 ~6×10 -3 It may be on the order of Pa.

[0094] Next, sputtering gas is introduced into the sputtering chamber 17 from the sputtering gas inlet 7 so that the pressure in the sputtering chamber 17 becomes a predetermined pressure b' during film formation. The amount of the sputtering gas introduced may be fixed, and the opening of the exhaust port 18 may be feedback-controlled to keep the sputtering pressure constant. The sputtering gas is not particularly limited as long as it is a gas that can be used for sputtering, and may be any known sputtering gas. The sputtering gas may be a noble gas, such as argon or krypton, preferably.

[0095] The predetermined pressure b' (sputtering pressure) in sputtering chamber 17 during the above film formation may be usually 0.05 to 5 Pa, preferably 0.1 to 1 Pa, from the viewpoint of stabilizing discharge and enabling continuous film formation.

[0096] Next, a predetermined power is applied to the metal target to cause discharge, and when the discharge state becomes stable, the intermediate laminate a is moved at a predetermined line speed while the metal target is sputtered to form the metal thin film directly on the surface of the intermediate laminate a on the fluorine-doped cerium dioxide thin film a side. At this time, cooling water of a predetermined temperature and flow rate is made to flow through the target installation jigs 10 and 10' to control the temperature of the metal target to a predetermined temperature. Here, the power applied may be DC power or AC power. Since metals such as silver, copper, and aluminum have sufficiently high electrical conductivity, the power applied may preferably be DC power.

[0097] The thickness of the metal thin film can be adjusted to a desired thickness by adjusting the power input to the metal target, the flow rate of the sputtering gas (predetermined pressure b' (sputtering pressure) in the sputtering chamber 5 during film formation), and the film formation time. The relationship between the amount of input power, the flow rate of the sputtering gas, the film formation time, and the film thickness can be determined by a preliminary experiment.

[0098] 4-3. Deposition of fluorine-doped cerium dioxide thin film b: Furthermore, the fluorine-doped cerium dioxide thin film a is formed on one surface of the film substrate 11, and the fluorine-doped cerium dioxide thin film b is formed directly on the metal thin film surface of an intermediate laminate b having the metal thin film directly on the fluorine-doped cerium dioxide thin film a surface.

[0099] The fluorine-doped cerium dioxide thin film b can be formed in the same manner as described in "4-1. Formation of fluorine-doped cerium dioxide thin film a".

[0100] The laminate of the present invention can be obtained by forming the fluorine-doped cerium dioxide thin film b directly on the metal thin film surface of the intermediate laminate b.

[0101] In producing the multilayer thin film of the present invention as a film roll, the thickness of the fluorine-doped cerium dioxide thin film b may be preferably 25 nm or more, more preferably 30 nm or more, even more preferably 35 nm or more, and most preferably 40 nm or more, from the viewpoint of reliably protecting the metal thin film from environmental loads such as high temperature and high humidity, while from the viewpoint of crack resistance, the thickness may be preferably 120 nm or less, more preferably 100 nm or less, even more preferably 80 nm or less, and most preferably 60 nm or less.

[0102] In producing the multilayer thin film of the present invention as a film roll, the ratio of the thickness of the fluorine-doped cerium dioxide thin film b to the thickness of the fluorine-doped cerium dioxide thin film a (thin film b / thin film a) may be preferably 5.0 or less, more preferably 4.0 or less, even more preferably 3.0 or less, and most preferably 2.5 or less, from the viewpoint of crack resistance. On the other hand, from the viewpoint of reliably obtaining the function of protecting the metal thin film from environmental loads such as high temperature and high humidity, it may be preferably 1.1 or more, more preferably 1.5 or more, and even more preferably 1.8 or more.

[0103] 5. Goods: The article of the present invention includes the multilayer thin film of the present invention or the laminate of the present invention. The article of the present invention has an infrared shielding function by including the multilayer thin film of the present invention or the laminate of the present invention. Examples of the article of the present invention include a member (film for glass) that is attached to window glass of buildings and windows of automobiles to impart heat insulation, window glass of buildings and windows of automobiles having heat insulation, etc. EXAMPLES

[0104] The present invention will be described below with reference to examples, but the present invention is not limited to these.

[0105] Measurement method (a) Solar radiation rejection rate: In accordance with the calculation of the 6.5 shading coefficient and solar heat gain coefficient of JIS A5759:2016, the solar transmittance and solar reflectance were measured with the multilayer thin film surface of the laminate facing the light source using a spectrophotometer "Solid Spec-3700 (product name)" made by Shimadzu Corporation. Next, in accordance with the measurement method of spectral reflectance and spectral transmittance in the wavelength range of room temperature thermal radiation and the calculation method of normal emissivity in Appendix JB of JIS R3106:2019, the glass surface of the laminate was set as the outdoor surface and the multilayer thin film surface was set as the indoor surface, and the normal emissivity of each was measured using an infrared spectrophotometer "Nicolet 380 (product name)" made by Thermo Fisher Scientific Co., Ltd. After that, the modified emissivity of each was calculated in accordance with Appendix A of JIS R3107:2019, the method of determining emissivity, and the method of determining modified emissivity of gas physical properties A.2. The proportion of solar heat absorbed by the test piece that is transferred indoors was calculated by substituting the obtained corrected emissivity of the indoor surface and the corrected emissivity of the outdoor surface into formula (5) of the above JIS standard. Next, the shading coefficient was calculated by substituting the obtained solar transmittance, solar reflectance, and the proportion of solar heat absorbed by the test piece that is transferred indoors into formula (4) of the above JIS standard. The solar heat gain coefficient was calculated by substituting the calculated shading coefficient into formula (6) of the above JIS standard. Next, the solar radiation rejection rate (unit: %) was calculated using the following formula (1). Solar radiation removal rate = 100 - solar heat gain rate × 100 (1)

[0106] (b) Thermal conductivity U: According to JIS R3106:2019, Appendix JB, Methods for measuring spectral reflectance and spectral transmittance in the wavelength range of room temperature thermal radiation and method for calculating normal emissivity, Thermo Fisher Scientific's Nicolet 380 (product name) infrared spectrophotometer was used to measure the normal emissivity of each of the laminated glass surface as the outdoor surface and the multilayer thin film surface as the indoor surface. Then, according to JIS R3107:2019, Appendix A, Method for determining emissivity, and A.2, Method for determining modified emissivity of gas physical properties, the modified emissivity of each was calculated. The modified emissivity of the outdoor surface and the modified emissivity of the indoor surface obtained were substituted into JIS A5759:2016, 6.6, Formula (7) for calculating the thermal transmittance, to obtain the thermal transmittance U (unit: W / m 2 ·K) was calculated.

[0107] (C) Visible light transmittance: In accordance with JIS A5759:2016, 6.4 Visible Light Transmittance Test, the visible light transmittance (unit: %) was measured using a spectrophotometer "Solid Spec-3700 (product name)" manufactured by Shimadzu Corporation, with the multilayer thin film surface of the laminate facing the light source.

[0108] (2) Haze: According to JIS K 7136:2000, the haze (unit: %) of the laminate was measured using a turbidity meter "NDH2000 (product name)" manufactured by Nippon Denshoku Industries Co., Ltd., with the multilayer thin film surface of the laminate facing the light source.

[0109] (E) Moisture and heat resistance 1: The laminate was treated for 168 hours in an environment of 60°C and 90% relative humidity, and then the following (G) appearance and Δhaze (the absolute value of the difference between the haze after moist heat treatment and the haze before moist heat treatment; each was measured according to (D) haze above) were evaluated.

[0110] (f) Moisture and heat resistance 2: Except for changing the treatment time to 480 hours, evaluation was performed in the same manner as in (e) Wet heat resistance 1 above.

[0111] (G) Appearance: A photograph of the multilayer thin film surface of the laminate after the moist heat treatment was binarized using Open CV so that defective areas were colored white and normal areas were colored black, and the proportion of the white area was then calculated as the area of ​​appearance defects.

[0112] In addition, the defects that occurred on the multilayer thin film surface of the laminate after the heat and moisture treatment and their surroundings were observed with a laser microscope and analyzed using SEM-EDS (a combination of a scanning electron microscope and energy dispersive X-ray spectroscopy). As a result, it was found that the defects were cracks in the cerium dioxide thin film and the fluorine-doped cerium dioxide thin film.

[0113] Without intending to be bound by theory, it is believed that the reason that the above-mentioned cracks can be significantly suppressed by doping with fluorine is that if even a small amount of metal migrates, aggregates are formed and the volume changes, the cerium dioxide thin film cannot withstand this and will crack, whereas the fluorine-doped cerium dioxide thin film is given flexibility by the fluorine doping and can withstand it.

[0114] Raw materials used (A) Target: (A-1) A disk-shaped target with a diameter of 76.2 mm and a thickness of 3 mm obtained by sintering cerium dioxide from USTRON Corporation. Purity: 4N. (A-2) A disk-shaped target with a diameter of 76.2 mm and a thickness of 3 mm obtained by melting and rolling silver manufactured by USTRON Corporation. Purity: 4N. (A-3) A disk-shaped target with a diameter of 76.2 mm and a thickness of 3 mm obtained by melting and rolling copper manufactured by USTRON Corporation. Purity: 4N. (A-4) A target in the shape of a rectangular parallelepiped, 127 mm long, 380 mm wide, and 3 mm thick, made by sintering cerium dioxide from USTRON Corporation. Purity 4N. (A-5) A rectangular parallelepiped target of 127 mm length, 380 mm width, and 3 mm thickness obtained by melting and rolling copper from USTRON Corporation. Purity 4N.

[0115] (B) Gas: (B-1) Argon gas (grade 99.999% or higher purity). (B-2) Tetrafluoromethane (grade of 99.999% or higher purity). (B-3) Oxygen (grade of 99.999% or higher purity).

[0116] (C) Base material: (C-1) A smooth soda-lime glass plate from Matsunami Glass Industry Co., Ltd. (product name: microslide glass, water-polished edge, thickness: 1.0 mm, dimensions: 40 × 40 mm). (C-2) Toray Industries, Inc.’s 125 μm-thick, double-sided, easily adhesive, biaxially oriented polyethylene terephthalate resin film “Lumirror (product name).”

[0117] Example 1 (1) Deposition of fluorine-doped cerium dioxide thin film a: First, a batch-type sputtering apparatus, the conceptual diagram of which is shown in FIG. 2, was used to directly deposit a fluorine-doped cerium dioxide thin film a on one surface of the (C-1) using the (A-1), (B-1), and (B-2). First, the (A-1) was attached to the target setting jig 2 of the sputtering apparatus. Next, the inside of the sputtering chamber 5 of the sputtering apparatus was heated to a pressure of 3.0×10 -3 The pressure in the sputtering chamber 5 was reduced to 0.4 Pa. Next, the gas flow (volume flow rate 19.80 sccm) of (B-1) and the gas flow (volume flow rate 0.20 sccm) of (B-2) were joined and mixed together and introduced as a sputtering gas from the sputtering gas inlet 7 into the sputtering chamber 5, and the aperture of the exhaust port 6 was feedback-controlled so that the pressure in the sputtering chamber 5 was 0.4 Pa. Next, the input power of 200 W (input power amount per unit area 4.4 W / cm2) was supplied to the above (A-1). 2) high frequency AC power was applied under the conditions of 0.1 to 1.5 V, and sputtering was performed to form a sputtered film on one surface of (C-1). The film formation time was 13 minutes, and the film formation conditions were such that the thickness of the sputtered film was 70 nm. The spectrum of the sputtered film obtained by XPS analysis in the energy range of -10 to 1350 eV is shown in FIG. 1. From the spectrum, the composition of the sputtered film was calculated to be 30 at % carbon, 19 at % oxygen, 39 at % fluorine, and 12 at % cerium. In other words, the proportion of fluorine atoms in the sputtered film (the fluorine-doped cerium dioxide thin film a) was 39 at %.

[0118] (2) Metal thin film deposition: Next, a batch-type sputtering apparatus, the conceptual diagram of which is shown in FIG. 2, was used to deposit a metal thin film (silver thin film) directly on the surface of the fluorine-doped cerium dioxide thin film a deposited in (1) above, using (A-2) and (B-1) above. First, (A-2) was attached to the target installation jig 2 of the sputtering apparatus. Next, the inside of the sputtering chamber 5 of the sputtering apparatus was heated to a pressure of 3.0×10 -3 The pressure in the sputtering chamber 5 was reduced to 0.4 Pa. Next, the gas flow (volume flow rate 20 sccm) of (B-1) was introduced as a sputtering gas from the sputtering gas inlet 7 into the sputtering chamber 5, and the aperture of the exhaust port 6 was feedback-controlled so that the pressure in the sputtering chamber 5 was 0.4 Pa. Next, the input power of 100 W (input power amount per unit area 2.2 W / cm2) was input to the (A-2). 2 A direct current was applied under the conditions of (1) above, and sputtering was performed to form a sputtered film (silver thin film) on the surface of the fluorine-doped cerium dioxide thin film a formed in (1) above. The film formation time was 15 seconds, and the sputtered film had a thickness of 10 nm.

[0119] (3) Deposition of fluorine-doped cerium dioxide thin film b: Next, a batch-type sputtering apparatus, the conceptual diagram of which is shown in FIG. 2, was used to deposit a fluorine-doped cerium dioxide thin film b directly on the surface of the metal thin film (silver thin film) deposited in (2) above, using (A-1), (B-1), and (B-2). First, (A-1) was attached to the target installation jig 2 of the sputtering apparatus. Next, the inside of the sputtering chamber 5 of the sputtering apparatus was heated to a pressure of 3.0×10 -3 The pressure in the sputtering chamber 5 was reduced to 0.4 Pa. Next, the gas flow (volume flow rate 19.80 sccm) of (B-1) and the gas flow (volume flow rate 0.20 sccm) of (B-2) were joined and mixed together and introduced as a sputtering gas from the sputtering gas inlet 7 into the sputtering chamber 5, and the aperture of the exhaust port 6 was feedback-controlled so that the pressure in the sputtering chamber 5 was 0.4 Pa. Next, the input power of 200 W (input power amount per unit area 4.4 W / cm2) was supplied to the above (A-1). 2 ) high-frequency AC power was applied to perform sputtering to form a sputtered film on one surface of the above (C-1). The film formation time was 5 minutes, and the film formation conditions were such that the thickness of the sputtered film was 30 nm.

[0120] The laminate thus obtained was subjected to the above tests (a) to (g). The results are shown in Table 1.

[0121] In this specification, the unit of volumetric flow rate "sccm" is the volume (unit: cc) of gas flowing per minute normalized under standard conditions (temperature 0° C., 1 atmospheric pressure).

[0122] Example 2 A laminate was obtained in the same manner as in Example 1, except that in the deposition of the above (1) fluorine-doped cerium dioxide thin film a, the volumetric flow rate of each of the sputtering gases was changed as shown in Table 1, i.e., fluorine was not doped, and in the deposition of the above (3) fluorine-doped cerium dioxide thin film b, the volumetric flow rate of each of the sputtering gases was changed as shown in Table 1, i.e., fluorine was not doped. The above tests (a) to (g) were carried out. The results are shown in Table 1.

[0123] Examples 3 and 4 A laminate was obtained in the same manner as in Example 1, except that in the above (1) formation of the fluorine-doped cerium dioxide thin film a, the volumetric flow rate of each of the sputtering gases was changed as shown in Table 1, and in the above (3) formation of the fluorine-doped cerium dioxide thin film b, the volumetric flow rate of each of the sputtering gases was changed as shown in Table 1. The above tests (a) to (g) were carried out. The results are shown in Table 1. The proportion of fluorine atoms in the fluorine-doped cerium dioxide thin film a of Example 3 was 15 at %. The proportion of fluorine atoms in the fluorine-doped cerium dioxide thin film a of Example 4 was 56 at %.

[0124] Example 5 A laminate was obtained in the same manner as in Example 1, except that in the deposition of the metal thin film (2), the above (A-3) was used instead of the above (A-2) and the deposition time was 40 seconds (the thickness of the obtained metal film was 15 nm). The above tests (a) to (g) were carried out. The results are shown in Table 1.

[0125] Example 6 A laminate was obtained in the same manner as in Example 1 except that in the deposition of the fluorine-doped cerium dioxide thin film a above (1), the volumetric flow rate of each of the sputtering gases was changed as shown in Table 1, i.e., fluorine was not doped, in the deposition of the metal thin film above (2), the above (A-3) was used instead of the above (A-2), and the deposition time was 40 seconds (the thickness of the obtained metal film was 15 nm), and in the deposition of the fluorine-doped cerium dioxide thin film b above (3), the volumetric flow rate of each of the sputtering gases was changed as shown in Table 1, i.e., fluorine was not doped. The above tests (a) to (g) were performed. The results are shown in Table 1.

[0126] [Table 1]

[0127] It was confirmed that the multi-layer thin film of the present invention has an infrared shielding function and good resistance to moist heat.

[0128] Example 7 (1') Deposition of fluorine-doped cerium dioxide thin film a: Using a roll-to-roll sputtering apparatus, the conceptual diagram of which is shown in Figure 2-2, a fluorine-doped cerium dioxide thin film a was formed on one surface of (C-2) using (A-4), (B-1), and (B-2). (1'-1) First, the above (C-2) was passed through the sputtering device, and then the above (A-4) (target 9) was attached to the target setting jig 10. Note that the target setting jig 10' was not used. In other words, only one (A-4) was used. (1'-2) Next, the sputtering chamber 17 of the sputtering apparatus is filled with gas at a pressure of 5.0×10 -3 The pressure was reduced to 10 Pa. (1'-3) Next, the gas flow (B-1) (volume flow rate 199.0 sccm) and the gas flow (B-2) (volume flow rate 1.0 sccm) were merged and mixed and introduced as a sputtering gas into the sputtering chamber 17 from the sputtering gas inlet 19, and the aperture of the exhaust port 18 was feedback-controlled so that the pressure inside the sputtering chamber 17 was 0.4 Pa. (1'-4) Next, while winding the (C-2) at a line speed of 1.0 m / min, the (A-4) (target 9) was supplied with 1500 W of power (power input per unit area: 3.1 W / cm). 2 ), high-frequency AC power was applied to perform sputtering, forming a sputtered film on one surface of the (C-2). At this time, the (C-2) was reciprocated a predetermined distance, passing the position of the sputter roll 4 facing the (A-2) (target 9) nine times. These were the film formation conditions that resulted in the thickness of the sputtered film being 35 nm.

[0129] (2') Deposition of thin metal films: Next, using a roll-to-roll sputtering device whose conceptual diagram is shown in Figure 2-2, a metal thin film (silver thin film) was formed directly on the surface of the fluorine-doped cerium dioxide thin film a formed in the above (1) using the above (A-5) and (B-1). (2'-1) First, the intermediate laminate a having the fluorine-doped cerium dioxide thin film a formed in (1) above on the surface of the (C-2) was passed through the intermediate laminate a so that the surface on the fluorine-doped cerium dioxide thin film a side became the film formation surface, and then the (A-5) was attached to the target setting jig 10. Note that the target setting jig 10' was not used. That is, only one (A-5) was used. (2'-2) Next, the sputtering chamber 17 of the sputtering apparatus is filled with gas at a pressure of 5.0×10 -3 The pressure was reduced to 10 Pa. (2'-3) Next, the gas flow (volume flow rate 200.0 sccm) of (B-1) above was introduced as a sputtering gas into the sputtering chamber 17 from the sputtering gas inlet 19, and the opening of the exhaust port 18 was feedback-controlled so that the pressure inside the sputtering chamber 17 was 0.4 Pa. (2'-4) Next, while the intermediate laminate a was being wound at a line speed of 2.0 m / min, the electric power input amount of 1500 W (electric power input amount per unit area of ​​3.1 W / cm) was input to the (A-5). 2 A direct current was applied under the conditions of (1) above, and sputtering was performed to form a sputtered film (thin copper film) on the surface of the fluorine-doped cerium dioxide thin film a formed in (1) above. The film formation conditions were such that the thickness of the sputtered film was 15 nm.

[0130] (3) Deposition of fluorine-doped cerium dioxide thin film b: Next, a fluorine-doped cerium dioxide thin film b was formed directly on the surface of the metal thin film (copper thin film) formed in the above (2') in the same manner as in the above (1') formation of a fluorine-doped cerium dioxide thin film a, except that the number of reciprocations in the above step (1'-4) was changed to 18. The film formation conditions were such that the thickness of the sputtered film was 70 nm.

[0131] The laminate thus obtained was subjected to the above tests (a) to (d). The results were a solar radiation rejection rate of 48% and a thermal transmission coefficient U of 3.6 W / m 2 ·K, visible light transmittance 56%, and haze 3.4%.

[0132] The laminate was also treated for 480 hours in an environment at a temperature of 60°C and a relative humidity of 90%, and then the thermal conductivity U after the moist heat treatment was measured using the above (g) Appearance and (b) Thermal conductivity U. The results were 0.4% for appearance and 3.8 W / m 2 It was K.

[0133] Furthermore, the thermal conductivity U after wet heat treatment was also measured after the laminate was treated for 960 hours in an environment with a temperature of 60°C and a relative humidity of 90%. The result was 3.8 W / m 2 It was K.

[0134] Example 8 In the step (1'-3), the gas flow of (B-1) (volume flow rate: 197.0 sccm), the gas flow of (B-2) (volume flow rate: 1.0 sccm), and the gas flow of (B-3) (volume flow rate: 2.0 sccm) were introduced as a sputtering gas from the sputtering gas inlet 19 into the sputtering chamber 17 while being joined and mixed; in the step (1'-4), the gas flow was made to pass through the position of the sputtering roll 4 facing the (A-2) (target 9) 11 times; A laminate was obtained in the same manner as in Example 7, except that the gas flow of (B-1) (volume flow rate 197.0 sccm), the gas flow of (B-2) (volume flow rate 1.0 sccm), and the gas flow of (B-3) (volume flow rate 2.0 sccm) were joined and mixed and introduced into the sputtering chamber 17 from the sputtering gas inlet 19 as a sputtering gas; and that in the step corresponding to the step (1'-4) of the step (3), the position facing the sputtering roll 4 (A-2) (target 9) was passed 20 times.

[0135] The laminate thus obtained was subjected to the above tests (a) to (d). The results were a solar radiation rejection rate of 48% and a thermal transmittance U of 3.8 W / m 2 ·K, visible light transmittance 58%, and haze 3.0%.

[0136] The laminate was also treated for 480 hours in an environment at a temperature of 60°C and a relative humidity of 90%, and then the thermal conductivity U after the moist heat treatment was measured using the above (g) Appearance and (b) Thermal conductivity U. The results were 1.3% for appearance and 4.1 W / m 2 It was K.

[0137] It was confirmed that the multi-layered thin film of the present invention maintained a good infrared shielding function even after the moist heat treatment. [Brief description of the drawings]

[0138] [Figure 1] This is a spectrum of an XPS analysis of a fluorine-doped cerium dioxide thin film in the energy range of -10 to 1350 eV. [Diagram 2] FIG. 2 is a conceptual diagram of a batch-type sputtering apparatus used in the examples. [Figure 2-2] FIG. 1 is a conceptual diagram of a roll-to-roll sputtering apparatus used in the examples. [Diagram 3] The laminate of Example 5 was subjected to the moist heat treatment in the above-mentioned Test (d) Moist Heat Resistance 2, and then a photograph of the multilayer thin film surface was binarized using the method of the above-mentioned Test (e) Appearance. [Figure 4] The laminate of Example 2 was subjected to the moist heat treatment in the above-mentioned Test (iv) Moist Heat Resistance 2, and then a photograph of the multilayer thin film surface was binarized using the method in the above-mentioned Test (e) Appearance. [Explanation of symbols]

[0139] 1: Target 2: Target installation jig 3: Spatter table 4: Base material 5: Sputtering chamber 6: Exhaust port 7: Sputtering gas inlet 8: Shutter 9. Target 10: Target installation jig 11: Film substrate 12: Payout roll 13: Film roll 14: Winding roll 15:Transport roll 16: Sputter roll 17: Sputtering chamber 18: Exhaust vent 19: Sputtering gas inlet

Claims

1. A multilayer film in which a thin film of fluorine-doped cerium dioxide is deposited directly on both sides of a thin metal film.

2. 2. The multilayer thin film according to claim 1, wherein the proportion of fluorine atoms in said fluorine-doped cerium dioxide thin film is, in atomic ratio, 1 to 60 at %, with the total number of atoms in said fluorine-doped cerium dioxide thin film being 100 at %.

3. 2. The multi-layered thin film of claim 1, wherein said metal thin film is a copper thin film.

4. 2. The multi-layered thin film according to claim 1, wherein said metal thin film is an aluminum thin film.

5. 2. The multilayer thin film according to claim 1, wherein said metal thin film is a silver thin film.

6. A laminate having the multilayer thin film according to any one of claims 1 to 5 on a part or all of the surfaces of a substrate.

7. An article comprising the multilayer thin film according to any one of claims 1 to 5.

8. 1. A method for producing a multilayer thin film, comprising depositing a fluorine-doped cerium dioxide thin film directly on both sides of a metal thin film, the method comprising the steps of: The step of forming the fluorine-doped cerium dioxide thin film comprises: Using a sputtering device, a cerium dioxide target and an organic fluorine compound gas are used. (1) a sub-step of mounting the cerium dioxide target on a target mounting jig of the sputtering apparatus; (2) a sub-step of reducing the pressure in the sputtering chamber of the sputtering apparatus to a predetermined pressure a; (3) a sub-step of introducing a mixed gas of a sputtering gas and the organic fluorine compound gas into a sputtering chamber of the sputtering apparatus so that the pressure in the sputtering chamber becomes a predetermined pressure b; and (4) a sub-step of applying power to the cerium dioxide target and sputtering the fluorine-doped cerium dioxide thin film; wherein the mixing ratio of the sputtering gas to the organic fluorine compound gas (volume of the sputtering gas / volume of the organic compound gas) is 95 / 5 to 99.99 / 0.01; forming the fluorine-doped cerium dioxide thin film; A method for producing the multilayer thin film.

9. 9. The method according to claim 8, wherein the sputtering apparatus is a roll-to-roll type sputtering apparatus.

Citation Information

Patent Citations

  • Transparent electromagnetic wave shielding film

    JP2000085047A

  • Method for manufacturing composite film and method for manufacturing organic-inorganic hybrid film

    JP2022186664A