Composite positive electrode active material, positive electrode and lithium battery using the same, and manufacturing method for the same
A composite positive electrode active material with a core-shell structure addresses the issues of side reactions and thermal instability in lithium batteries, enhancing cycle characteristics and reducing resistance.
Patent Information
- Application Number
- JP2024041245
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-15
- Filing Date
- 2024-03-15
- Publication Date
- 2024-10-01
AI Technical Summary
Conventional positive electrode active materials in lithium batteries suffer from deterioration due to side reactions and insufficient thermal stability, leading to reduced performance and life span.
A composite positive electrode active material is developed, comprising a core of lithium transition metal oxides with different particle sizes and a shell made of metal oxides and carbon-based materials, which suppresses side reactions and improves thermal stability.
The composite material enhances high-temperature cycle characteristics and reduces internal resistance, thereby improving the performance and lifespan of lithium batteries.
Smart Images

Figure 2024133028000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a composite positive electrode active material, a positive electrode and a lithium battery using the same, and a method for producing the composite positive electrode active material. [Background technology]
[0002] In order to meet the trend of miniaturization and high performance of various devices, it is becoming important for lithium batteries to have high energy density in addition to miniaturization and weight reduction, i.e., high capacity lithium batteries are becoming important.
[0003] In order to realize a lithium battery that meets the above-mentioned applications, positive electrode active materials having high capacity have been investigated.
[0004] Conventional positive electrode active materials have poor life characteristics due to side reactions and also have insufficient thermal stability.
[0005] Therefore, a method is required that can prevent deterioration of battery performance while still containing a positive electrode active material. Summary of the Invention [Problem to be solved by the invention]
[0006] The problem to be solved by the present invention is to provide a new composite positive electrode active material capable of suppressing side reactions of the composite positive electrode active material and preventing deterioration of the life span due to the rate of increase in resistance.
[0007] Another problem to be solved by the present invention is to provide a positive electrode comprising the composite positive electrode active material.
[0008] Another problem to be solved by the present invention is to provide a lithium battery using the above positive electrode.
[0009] Another problem to be solved by the present invention is to provide a method for producing the composite positive electrode active material. [Means for solving the problem]
[0010] In one aspect, a first core (1 st core) containing a first lithium transition metal oxide, a second core (2 nd core) containing a second lithium transition metal oxide, and a shell disposed along the surface of one or more of the first core and the second core, wherein the shell contains one or more first metal oxides, a first carbon-based material, and a second carbon-based material, the first metal oxide is disposed within the first carbon-based material matrix, the first metal oxide is represented by the chemical formula M a O b (where 0 < a ≤ 3, 0 < b < 4, and if a is 1, 2, or 3, then b is not an integer), and M is one or more metals selected from Groups 2 to 13 of the Periodic Table of the Elements, Groups 15 and 16 of the Periodic Table of the Elements, the second carbon-based material includes a fibrous carbon-based material having an aspect ratio of 10 or more, a composite cathode active material is provided, wherein the first lithium transition metal oxide and the second lithium transition metal oxide have different particle sizes from each other.
[0011] In another aspect, a cathode including the composite cathode active material is provided.
[0012] In yet another aspect, a lithium battery including the cathode is provided.
[0013] In yet another aspect, providing a first lithium transition metal oxide; providing a second lithium transition metal oxide; providing a composite; providing a second carbon-based material; mechanically milling the first lithium transition metal oxide, the composite, and the second carbon-based material to obtain a first core / shell structure; Mechanically milling the second lithium transition metal oxide, the composite, and the second carbon-based material to obtain a second core / shell structure; Mixing the first core / shell structure and the second core / shell structure to obtain a composite cathode active material, wherein the composite includes one or more first metal oxides represented by the chemical formula M a O b (0 < a ≤ 3, 0 < b < 4, and if a is 1, 2, or 3, then b is not an integer), and a first carbon-based material, wherein the first metal oxide is disposed within a first carbon-based material matrix, and M is one or more metals selected from Groups 2 to 13 of the Periodic Table of the Elements, Group 15, and Group 16 of the Periodic Table of the Elements; wherein the second carbon-based material includes fibrous carbon having an aspect ratio of 10 or more, and the first lithium transition metal oxide and the second lithium transition metal oxide have different particle sizes, and a method for manufacturing a composite cathode active material is provided.
Advantages of the Invention
[0014] According to one aspect, the composite cathode active material includes a shell containing a first metal oxide, a first carbon-based material, and a second carbon-based material, thereby improving the high-temperature cycle characteristics of the lithium battery, suppressing an increase in internal resistance, and improving high-rate characteristics.
Brief Description of the Drawings
[0015] [Figure 1] It is a cross-sectional schematic view of composite cathode active material particles according to an embodiment. [Diagram 2] It is a scanning electron microscope image of the surface of the composite cathode active material particles manufactured in Example 2. [Figure 3A] In Example 1, it is a scanning electron microscope image showing the shape of the bimodal polycrystalline cathode active material used as a starting material. [Figure 3B] It is a schematic diagram related to a cross-section of single-crystalline first lithium transition metal oxide particles used in Comparative Example 1. [Figure 4]1 is a graph showing changes in capacity retention rate depending on the number of cycles in the lithium batteries according to Examples 5 to 8 and Comparative Example 2. [Diagram 5] 1 is a graph showing the change in specific capacity depending on the number of cycles in the lithium batteries according to Examples 5 to 8 and Comparative Example 2. [Figure 6] 1 is a schematic diagram of a lithium battery according to an embodiment. [Figure 7] 1 is a schematic diagram of a lithium battery according to an embodiment. [Figure 8] 1 is a schematic diagram of a lithium battery according to an embodiment. [Figure 9] 1 is a graph showing XPS (X-ray photoelectron spectroscopy) spectra of the composite prepared in Preparation Example 1, NMX of Comparative Example 1, and the composite positive electrode active material prepared in Example 1. [Figure 10] 1 is a graph showing Raman spectrum analysis results for the composite prepared in Preparation Example 1 and the composite positive electrode active material prepared in Example 1. [Figure 11A] FIG. 2 is a schematic diagram showing the shape of a plate particle. [Figure 11B] 1 is a diagram illustrating a definition of a radial shape of secondary particles of a nickel-based active material according to an embodiment; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The present inventive concept described below can be modified in various ways and can have various embodiments, but specific embodiments are illustrated in the drawings and described in detail in the detailed description. However, they do not limit the present inventive concept to specific embodiments, and should be understood to include all modifications, equivalents, or alternatives that fall within the technical scope of the present inventive concept.
[0017] The terms used below are merely used to describe specific embodiments and are not intended to limit the present invention. A singular expression includes a plural expression unless the context clearly dictates otherwise. In the following, terms such as "comprise" or "have" indicate the presence of a feature, number, step, operation, component, part, ingredient, material, or combination thereof described in the specification, and should be understood not to preclude the presence or addition of one or more other features, numbers, steps, operations, components, parts, ingredients, materials, or combinations thereof. In the following, " / " can be interpreted as "and" or "or" depending on the context.
[0018] In the drawings, thicknesses may be exaggerated or reduced to clearly depict the various layers and regions. Similar parts are designated by the same reference numerals throughout the specification. Throughout the specification, when a part, such as a layer, film, region, or plate, is described as being "on" or "above" another part, this includes not only when it is directly on top of the other part, but also when there is another part between them. Throughout the specification, terms such as first and second may be used to describe various components, but the components are not limited by these terms. These terms are used only to distinguish one component from another.
[0019] In this specification, the "particle size" of a particle refers to the average diameter when the particle is spherical, and the average major axis length when the particle is non-spherical. The particle size of a particle can be measured using a particle size analyzer (PSA) or an electron microscope. The "particle size" of a particle is the average particle size. The average particle size is, for example, the median particle size (D50). The median particle size (D50) is calculated from the side of the particle with the smallest particle size in the cumulative distribution curve of the particle size in which the particles are accumulated in the order of particle size from the smallest particle to the largest particle, and is the size of the particle corresponding to the 50% cumulative value. The cumulative value is, for example, the cumulative volume. The median particle size (D50) can be measured, for example, by the laser diffraction method. The average thickness and average length can be evaluated in the same manner as the particle size evaluation method. The aspect ratio means the average aspect ratio and can be evaluated by an SEM image.
[0020] Hereinafter, a composite cathode active material, a cathode and a lithium battery including the same, and a method for manufacturing the same according to exemplary embodiments will be described in more detail.
[0021] The composite cathode active material includes a core including a lithium transition metal oxide and a shell disposed along the surface of the core, and the shell has the chemical formula M a O b (where 0 < a ≤ 3, 0 < b < 4, and if a is 1, 2, or 3, then b is not an integer), and includes one or more first metal oxides, a first carbon-based material, and a second carbon-based material. The first metal oxide is disposed within a first carbon-based material matrix, and M is one or more metals selected from Groups 2 to 13 of the periodic table of the elements, Groups 15 and 16 of the periodic table of the elements, and the second carbon-based material includes fibrous carbon having an aspect ratio of 10 or more.
[0022] The first lithium transition metal oxide and the second lithium transition metal oxide each contain secondary particles including a plurality of primary particles, the first lithium transition metal oxide being a large particle size lithium transition metal oxide having a larger particle size than the second lithium transition metal oxide, and the second lithium transition metal oxide being a small particle size lithium transition metal oxide having a smaller particle size than the first lithium transition metal oxide.
[0023] The first lithium transition metal oxide and the second lithium transition metal oxide have a polycrystalline structure.
[0024] Hereinafter, the theoretical basis for why the composite positive electrode active material according to one embodiment provides excellent effects will be described. However, this is intended to aid in understanding the present invention and is not intended to limit the present invention in any manner.
[0025] In order to improve the mixed density of the positive electrode, it is necessary to minimize the content of the conductive material, which occupies a large volume inside the electrode. If the conductive material content is reduced, the side reaction of the positive electrode caused by the conductive network member increases, and the resistance increases, which may cause a deterioration in the lifespan. Therefore, in order to solve such problems, there is a need to develop a technology that uses a small amount of conductive material to form an effective conductive network and a positive electrode surface protective film to reduce side reactions.
[0026] In addition, when an inexpensive cobalt-free lithium transition metal oxide is used as the positive electrode active material, such a cobalt-lithium transition metal oxide tends to have high resistance. Therefore, a bimodal positive electrode active material including polycrystalline large grain size and polycrystalline small grain size particles as shown in FIG. 3A is used to reduce resistance and increase surface area, thereby improving the high rate characteristics of the lithium battery.
[0027] In this specification, "polycrystalline" is a term that is contrasted with single crystal, and refers to secondary particles that are an aggregate of multiple primary particles while having crystallinity. "Polycrystalline" means, for example, particles that have a radial structure and have crystallinity. The polycrystalline also includes plate primary particles. The plate primary particle means a structure in which the length t in one axial direction (i.e., thickness direction) is shorter than the long axis length a in the other direction (i.e., longitudinal direction) as shown in FIG. 11A.
[0028] FIG. 11A is a schematic diagram showing the shape of a plate primary particle according to an embodiment.
[0029] With reference thereto, the plate primary particles can have a polygonal nanoplate shape, such as a hexagon, as in (A), a nanodisk morphology, as in (B), or a rectangular shape, as in (C).
[0030] In Fig. 11A, the thickness t of the plate particle is smaller than the lengths a and b in the longitudinal direction. The length a in the longitudinal direction is longer than or equal to b. In the plate particle, the direction in which the thickness t is defined is defined as the thickness direction, and the direction in which the lengths a and b are included is defined as the longitudinal direction.
[0031] As used herein, "radial" means that the thickness t direction of the plate (the (001) direction) is aligned perpendicular to the direction R emanating from the center in the secondary particles, as shown in FIG. 11B.
[0032] The average length of the plate primary particles is 150nm to 500nm, for example, 200nm to 380nm, specifically, 290nm to 360nm. The average length of the plate primary particles means the average length of the average major axis length and the average minor axis length in the longitudinal direction of the plate particle. The average thickness of the plate primary particles is 100nm to 200nm, for example, 120nm to 180nm, specifically, 130nm to 150nm. The ratio of the average thickness to the average length is 1:2 to 1:5, for example, 1:2.1 to 1:5, specifically, 1:2.2 to 1:2.4.
[0033] In contrast, a single crystal is a particle having crystallinity and a single particle (one body particle or monolith particle) morphology, where the single particle means a structure in which particles are not mutually aggregated and exist as an independent phase in terms of morphology.
[0034] According to one embodiment, the polycrystal has an uneven surface when observed through a scanning electron microscope, compared to a single crystal. According to another embodiment, the polycrystal can be more clearly identified through particle cross-sectional analysis, and the crystal morphology can be confirmed through transmission electron microscope (TEM) analysis. Thus, the polycrystal can be identified through particle shape and / or particle cross-section observation through an electron scanning microscope.
[0035] Referring to FIG. 1, a composite active cathode material 100 includes a core 10 and a shell 20 disposed continuously or discontinuously along a surface of the core 10. The core 10 includes a first core (1 st and / or a second core (2 nd For convenience, we will explain using only one core.
[0036] The first lithium transition metal oxide and the second lithium transition metal oxide each contain secondary particles including a plurality of primary particles, the first lithium transition metal oxide being a large particle size lithium transition metal oxide having a larger particle size than the second lithium transition metal oxide, and the second lithium transition metal oxide being a small particle size lithium transition metal oxide having a smaller particle size than the first lithium transition metal oxide.
[0037] The first lithium transition metal oxide and the second lithium transition metal oxide have a bimodal particle size distribution, and the particle size ratio of the first lithium transition metal oxide to the second lithium transition metal oxide is 2.5:1 to 40:1.
[0038] The particle size ratio of the first lithium transition metal oxide to the second lithium transition metal oxide may be, for example, 2.5:1 to 40:1, 2.9:1 to 40:1, 3:1 to 40:1, 3:1 to 30:1, 3:1 to 20:1, 3:1 to 10:1, or 3:1 to 5:1. When the first lithium transition metal oxide to the second lithium transition metal oxide have a particle size ratio in such a range, the energy density and cycle characteristics of a lithium battery including the composite positive electrode active material may be further improved.
[0039] The particle size of the first lithium transition metal oxide is, for example, 3 μm to 15 μm, 3 μm to 12 μm, 3 μm to 10 μm, 5 μm to 10 μm, 7 μm to 10 μm, 8 μm to 10 μm, or 9 μm to 10 μm. The particle size of the first lithium transition metal oxide is, for example, a median particle size (D50). The particle size of the second lithium transition metal oxide is, for example, 1 μm to less than 7 μm, 1 μm to 7 μm, 1 μm to 6 μm, 1 μm to 5 μm, or 1 μm to 4 μm. The particle size of the second lithium transition metal oxide is, for example, a median particle size (D50). When the first lithium transition metal oxide and the second lithium transition metal oxide have average particle sizes in such ranges, the energy density and / or cycle characteristics of a lithium battery including the composite positive electrode active material can be further improved. The particle size of the first lithium transition metal oxide and the second lithium transition metal oxide is measured, for example, using a measuring device of a laser diffraction method or a dynamic light scattering method. The particle size is measured, for example, using a laser scattering particle size distribution meter (e.g., HORIBA LA-920), and is the median particle size (D50) value when 50% is accumulated from the smallest particle side in volume conversion.
[0040] The weight ratio of the first lithium transition metal oxide to the second lithium transition metal oxide may be, for example, 92:8 to 60:40, 90:10 to 60:40, 85:15 to 65:35, 80:20 to 65:35, or 75:25 to 65:35. When the first lithium transition metal oxide to the second lithium transition metal oxide have a weight ratio in such a range, the energy density and / or cycle characteristics of a lithium battery including the composite positive electrode active material may be further improved.
[0041] The shell may be disposed only on the first core, or the shell may be disposed only on the second core, or the shell may be disposed on both the first core and the second core, making it a composite positive electrode active material.
[0042] In the composite positive electrode active material, for example, the shell may be disposed only on the first core. That is, the shell is disposed on the first core, but not on the second core. For example, the shell is disposed on the first lithium transition metal oxide, which is a large particle size lithium transition metal oxide, and is not disposed on the second lithium transition metal oxide, which is a small particle size lithium transition metal oxide. By disposing the shell on the first core, the first core / shell structure is obtained. By disposing the shell on the surface of the large particle size lithium transition metal oxide, the specific surface area of the large particle size composite positive electrode active material is reduced, the side reaction between the large particle size lithium transition metal oxide and the electrolyte is also reduced, and the electronic conductivity of the large particle size lithium transition metal oxide can be improved. As a result, the energy density and / or cycle characteristics of the lithium battery can be further improved.
[0043] In the composite positive electrode active material, for example, the shell may be disposed only on the second core. That is, the shell is disposed on the second core, but not on the first core. For example, the shell is disposed on the second lithium transition metal oxide, which is a small particle size lithium transition metal oxide, but not on the first lithium transition metal oxide, which is a large particle size lithium transition metal oxide. By disposing the shell on the second core, the second core / shell structure is obtained. By disposing the shell on the surface of the small particle size lithium transition metal oxide, the side reaction between the small particle size composite positive electrode active material and the electrolyte is reduced, and the electronic conductivity of the small particle size composite positive electrode active material may be improved. As a result, the energy density and / or cycle characteristics of the lithium battery may be further improved.
[0044] In the composite positive electrode active material, for example, a shell may be disposed on both the first core and the second core. That is, the shell may be disposed on the first core and at the same time on the second core. For example, the shell may be disposed on the first lithium transition metal oxide, which is a large particle size lithium transition metal oxide, and on the second lithium transition metal oxide, which is a small particle size lithium transition metal oxide. The shell may be disposed on the first core to obtain the first core / shell structure, and the shell may be disposed on the second core to obtain the second core / shell structure. The composite positive electrode active material may include both the first core / shell structure and the second core / shell structure, thereby further improving the energy density and / or cycle characteristics of a lithium battery.
[0045] The content of the shell is 5 wt % or less, for example, 0.01 to 5 wt %, based on the total weight of the composite positive electrode active material.
[0046] The shell 20 may cover all or a part of the core 10. The core 10 includes a lithium transition metal oxide, and the shell 20 includes a first metal oxide 21, a first carbon-based material 22, and a second carbon-based material 23. The second carbon-based material 23 includes fibrous carbon having an aspect ratio of 10 or more. When manufacturing the composite positive electrode active material 100, the shell 20 may be disposed on the lithium transition metal oxide core 10 using a composite including a plurality of first metal oxides 21 disposed in a matrix of the first carbon-based material 22. Thus, the shell 20 may be uniformly disposed on the core 10 while preventing aggregation of the first carbon-based material 22. The shell 20 disposed on the core 10 may effectively block contact between the core 10 and the electrolyte. The shell 20 may effectively block contact between the core 10 and the electrolyte, thereby preventing side reactions caused by contact between the core 10 and the electrolyte. In addition, by disposing the shell 20 on the core 10, cation mixing due to contact between the core 10 and the electrolyte can be suppressed. By suppressing cation mixing due to contact between the core 10 and the electrolyte, generation of a resistance layer can be suppressed inside and / or on the surface of the composite positive electrode active material 100. In addition, by disposing the shell 20 on the core 10, elution of transition metal ions from the lithium transition metal oxide core 10 can also be suppressed. The first carbon-based material 22 can be, for example, a crystalline carbon-based material. The first carbon-based material 22 can be, for example, a carbon-based nanostructure. The first carbon-based material 22 can be, for example, a carbon-based two-dimensional nanostructure. The first carbon-based material 22 can be, for example, graphene. In this case, the shell including graphene and / or its matrix has flexibility, and can easily accommodate the volume change of the composite positive electrode active material 100 during charging and discharging, thereby suppressing the occurrence of cracks inside the composite positive electrode active material 100. Graphene has high electronic conductivity, so that it can reduce the interfacial resistance between the composite positive electrode active material 100 and the electrolyte. Therefore, even if a shell containing graphene is introduced, the internal resistance of the lithium battery can be maintained or reduced. In contrast, conventional carbon-based materials are easily aggregated, so that it is difficult to uniformly coat the lithium transition metal oxide core.
[0047] The shell includes the second carbon-based material 23, which is fibrous carbon having an aspect ratio of 10 or more. Therefore, the conductive path of the composite positive electrode active material 100 can be further lengthened. The second carbon-based material 23 forms a three-dimensional conductive network between the multiple composite positive electrode active materials, and can reduce the internal resistance of the positive electrode including the composite positive electrode active material 100. Since the fibrous carbon is fixed on the composite positive electrode active material 100, a uniform and stable three-dimensional conductive network can be formed between the multiple composite positive electrode active materials. Therefore, since the composite positive electrode active material 100 includes the second carbon-based material 23, the high rate characteristics of a lithium battery including the composite positive electrode active material 100 can be improved. On the other hand, a simple mixture of the lithium transition metal oxide core and the fibrous carbon, which is the second carbon-based material 23, is difficult to form a uniform three-dimensional conductive network between the multiple lithium transition metal oxide particles due to aggregation of the fibrous carbon. As can be seen from FIG. 1, the second carbon-based material 23 may be disposed on the surface of the composite positive electrode active material 100. Also, as can be seen from FIG. 1, the second carbon-based material 23 may protrude from the surface of the composite positive electrode active material 100. Therefore, the second carbon-based material 23 may effectively provide a conductive network between a plurality of composite positive electrode active materials 100. The second carbon-based material 23 may be easily coated on the core 10 by being disposed in the matrix of the first carbon-based material 22. The matrix of the first carbon-based material 22 may act as a binder that binds the core 10 and the second carbon-based material 23. Therefore, without the matrix of the first carbon-based material 22, the second carbon-based material 23 may not be easily attached to the core 10, or the second carbon-based material 23 may be easily detached from the core 10 during the process of manufacturing the slurry for the positive electrode. When a binder is added to bind the lithium transition metal oxide core 20 and the second carbon-based material 23, the core 10 may be coated with an insulating binder, which may increase the internal resistance of the composite positive electrode active material 100. When the second carbon-based material 23 and the core coated with the binder are subjected to high-temperature heat treatment to carbonize the binder, the core 10 and the second carbon-based material 23 may be deteriorated during the heat treatment process.
[0048] The aspect ratio of the second carbon-based material is greater than or equal to 10 or greater than or equal to 20. The aspect ratio of the second carbon-based material is, for example, between 10 and 100,000, between 10 and 80,000, between 10 and 50,000, between 10 and 10,000, between 10 and 5000, between 10 and 1,000, between 10 and 500, between 10 and 100, or between 10 and 50. The aspect ratio of the second carbon-based material is, for example, the ratio of the length of the major axis passing through the center of the second carbon-based material, i.e., the length of the second carbon-based material, to the length of the minor axis passing through the center of the second carbon-based material and perpendicular to the major axis, i.e., the diameter of the second carbon-based material.
[0049] The diameter of the second carbon-based material is, for example, 50 nm or less, 30 nm or less, 20 nm or less, or 10 nm or less. The diameter of the second carbon-based material is, for example, 1 nm to 50 nm, 1 nm to 30 nm, or 1 nm to 10 nm. If the diameter of the second carbon-based material is too large, the absolute number of strands per volume will decrease, and the effect of reducing internal resistance will be insignificant. If the diameter of the second carbon-based material is too small, it will be difficult to uniformly disperse the material.
[0050] The length of the second carbon-based material can be, for example, 1,000 μm or less, 100 μm or less, 50 μm or less, 10 μm or less, 5 μm or less, 2 μm or less, 1 μm or less, 500 nm or less, or 300 nm or less. The length of the second carbon-based material can be, for example, 100 nm to 1,000 μm, 100 nm to 500 μm, 100 nm to 100 μm, 100 nm to 50 μm, 100 nm to 10 μm, 100 nm to 5 μm, 100 nm to 2 μm, 100 nm to 1 μm, 100 nm to 500 nm, or 100 nm to 300 nm. The length of the second carbon-based material can be, for example, 500 nm to 1,000 μm, 500 nm to 500 μm, 500 nm to 100 μm, 500 nm to 50 μm, 500 nm to 10 μm, 500 nm to 5 μm, or even 500 nm to 2 μm. The greater the length of the second carbon-based material, the lower the internal resistance of the electrode can be. If the length of the second carbon-based material is too short, it is difficult to provide an effective conductive path.
[0051] The second carbon-based material may include, for example, carbon nanofibers, carbon nanotubes, or a combination thereof.
[0052] The carbon nanotubes may include, for example, a primary carbon nanotube structure, a secondary carbon nanotube structure formed by agglomeration of a plurality of primary carbon nanotube particles, or a combination thereof.
[0053] A carbon nanotube primary structure is one carbon nanotube unit. The carbon nanotube unit has a graphite sheet with a nano-sized cylindrical shape and an sp2 bond structure. Depending on the curved angle and structure of the graphite sheet, it may exhibit conductive or semiconductive properties. The carbon nanotube unit may be classified into single-walled carbon nanotubes (SWCNT), double-walled carbon nanotubes (DWCNT), and multi-walled carbon nanotubes (MWCNT), depending on the number of bonds forming the wall. The thinner the wall thickness of the carbon nanotube unit, the lower the resistance.
[0054] The carbon nanotube primary structure may include, for example, single-wall carbon nanotubes (SWCNT), double-wall carbon nanotubes (DWCNT) and multi-wall carbon nanotubes (MWCNT), or a combination thereof. The diameter of the carbon nanotube primary structure may be, for example, 1 nm or more or 2 nm or more. The diameter of the carbon nanotube primary structure may be, for example, 20 nm or less or 10 nm or less. The diameter of the carbon nanotube primary structure may be, for example, 1 nm to 20 nm, 1 nm to 15 nm, or 1 nm to 10 nm. The length of the carbon nanotube primary structure may be, for example, 100 nm or more or 200 nm or more. The length of the carbon nanotube primary structure may be, for example, 2 μm or less, 1 μm or less, 500 nm or less, or 300 nm or less. The length of the carbon nanotube primary structure may be, for example, 100 nm to 2 μm, 100 nm to 1 μm, 100 nm to 500 nm, 100 nm to 400 nm, 100 nm to 300 nm, or 200 nm to 300 nm. The diameter and length of the carbon nanotube primary structure may be measured from a scanning electron microscope (SEM) image or a transmission electron microscope (TEM) image. Alternatively, the diameter and / or length of the carbon nanotube primary structure may be measured by laser diffraction.
[0055] The carbon nanotube secondary structure is a structure formed by assembling the carbon nanotube primary structures in a bundle or bundle shape, either in whole or in part. The carbon nanotube secondary structure may include, for example, a bundle-type carbon nanotube, a rope-type carbon nanotube, or a combination thereof. The diameter of the carbon nanotube secondary structure may be, for example, 2 nm or more or 3 nm or more. The diameter of the carbon nanotube secondary structure may be, for example, 50 nm or less, 30 nm or less, 20 nm or less, or 10 nm or less. The diameter of the carbon nanotube secondary structure may be, for example, 2 nm to 50 nm, 2 nm to 30 nm, or 2 nm to 20 nm. The length of the carbon nanotube secondary structure may be, for example, 500 nm or more, 700 nm or more, 1 μm or more, or 10 μm or more. The length of the carbon nanotube secondary structure can be, for example, 1,000 μm or less, 500 μm or less, or 100 μm or less. The length of the carbon nanotube secondary structure can be, for example, 500 nm to 1,000 μm, 500 nm to 500 μm, 500 nm to 200 μm, 500 nm to 100 μm, or 500 nm to 50 μm. The diameter and length of the carbon nanotube secondary structure can be measured from a scanning electron microscope (SEM) image or an optical microscope. Alternatively, the diameter and / or length of the carbon nanotube secondary structure can be measured by laser diffraction.
[0056] The carbon nanotube secondary structure may be dispersed in a solvent or the like, converted into the carbon nanotube primary structure, and then used to manufacture a composite positive electrode active material.
[0057] The content of the second carbon-based material is, for example, 0.1 wt% to 75 wt%, 0.1 wt% to 50 wt%, 1 wt% to 40 wt%, or 5 wt% to 30 wt% based on the total weight of the first carbon-based material and the second carbon-based material. When the composite positive electrode active material includes the first carbon-based material and the second carbon-based material in such a range, a conduction path is more effectively secured in the composite positive electrode active material, and the internal resistance of the composite positive electrode active material can be further reduced. As a result, the cycle characteristics of a lithium battery including the composite positive electrode active material can be further improved. The content of the second carbon-based material is 5 wt% or less, or 1 wt% or less. The content of the second carbon-based material is, for example, 0.001 wt% to 5 wt%, 0.01 wt% to 3 wt%, 0.01 wt% to 1 wt%, 0.01 wt% to 0.5 wt%, or even 0.01 wt% to 0.1 wt% of the total weight of the composite positive electrode active material. By including the second carbon-based material in such a range, the conductive path in the composite positive electrode active material can be secured, and the internal resistance of the composite positive electrode active material can be further reduced. As a result, the cycle characteristics of a lithium battery including the composite positive electrode active material can be further improved.
[0058] The shell also includes a first metal oxide and a first carbon-based material. The first carbon-based material is derived from, for example, a graphene matrix, and therefore has a relatively low density and a high porosity compared to conventional carbon-based materials derived from graphite-based materials. The d002 interplanar distance of the first carbon-based material is, for example, 3.38 Å or more, 3.40 Å or more, 3.45 Å or more, 3.50 Å or more, 3.60 Å or more, 3.80 Å or more, or 4.00 Å or more. The d002 interplanar distance of the first carbon-based material included in the shell is, for example, 3.38 to 4.0 Å, 3.38 to 3.8 Å, 3.38 to 3.6 Å, 3.38 to 3.5 Å, or 3.38 to 3.45 Å. In contrast, the d002 interplanar distance of conventional carbon-based materials derived from graphite-based materials is, for example, 3.38 Å or less, or 3.35 to 3.38 Å. The first metal oxide has voltage resistance, so that it can prevent the lithium transition metal oxide contained in the core from deteriorating during charging and discharging at high voltages. The shell may, for example, contain one type of first metal oxide, or two or more different types of first metal oxides. As a result, the high-temperature cycle characteristics of a lithium battery containing the composite positive electrode active material are improved. The content of the shell may, for example, be 0.1 wt% to 5 wt%, 0.1 wt% to 4 wt%, 0.1 wt% to 3 wt%, 0.1 wt% to 2.5 wt%, 0.1 wt% to 2 wt%, or 0.1 wt% to 1.5 wt% of the total weight of the composite positive electrode active material. The content of the first metal oxide may be, for example, 0.06 wt% to 3 wt%, 0.06 wt% to 2.4 wt%, 0.06 wt% to 1.8 wt%, 0.06 wt% to 1.5 wt%, 0.06 wt% to 1.2 wt%, or 0.06 wt% to 0.9 wt% of the total weight of the composite positive electrode active material. When the composite positive electrode active material contains the shell and the first metal oxide in such a content range, the cycle characteristics of the lithium battery are further improved.
[0059] The first metal oxide includes a first metal, and the first metal is, for example, one or more selected from the group consisting of Al, Nb, Mg, Sc, Ti, Zr, V, W, Mn, Fe, Co, Pd, Cu, Ag, Zn, Sb, and Se. The first metal oxide may be, for example, Al.2 O z (0 < z < 3), NbO x (0 < x < 2.5), MgO x (0 < x < 1), Sc 2 O z (0 < z < 3), TiO y (0 < y < 2), ZrO y (0 < y < 2), V 2 O z (0 < z < 3), WO y (0 < y < 2), MnO y (0 < y < 2), Fe 2 O z (0 < z < 3), Co 3 O w (0 < w < 4), PdO x (0 < x < 1), CuO x (0 < x < 1), AgO x (0 < x < 1), ZnO x (0 < x < 1), Sb 2 O z (0 < z < 3) and SeO y (0 < y < 2) is also one or more selected therefrom. By arranging such a first metal oxide in the first carbon-based material matrix, the uniformity of the shell arranged on the core is improved, and the voltage resistance of the composite positive electrode active material is further improved. For example, the shell contains, as the first metal oxide, Al 2 O x (0 < x < 3).
[0060] The shell further contains one or more second metal oxides represented by the chemical formula M a O c (0 < a ≤ 3, 0 < c ≤ 4, and if a is 1, 2, or 3, then c is an integer). The M is one or more metals selected from Groups 2 to 13 of the Periodic Table of the Elements, Groups 15 and 16 of the Periodic Table of the Elements. For example, the second metal oxide contains the same metal as the first metal oxide, and the ratio c / a of the second metal oxide has a value further greater than the ratio b / a of the first metal oxide. For example, c / a > b / a. The second metal oxide is, for example, Al 2 O 3, NbO, NbO 2 , Nb 2 O 5 , MgO, Sc 2 O 3 , TiO 2 , ZrO 2 , V 2 O 3 , WO 2 , MnO 2 , Fe 2 O 3 , Co 3 O 4 , PdO, CuO, AgO, ZnO, Sb 2 O 3 and SeO 2 is selected from among them. The first metal oxide is, for example, a reduction product of the second metal oxide. By reducing part or all of the second metal oxide, the first metal oxide is obtained. Therefore, the first metal oxide has a lower oxygen content and a lower oxidation number of the metal compared to the second metal oxide. The shell is, for example, the first metal oxide Al 2 O x (0 < x < 3), and also includes the second metal oxide Al 2 O 3 .
[0061] The shell may include, for example, a first carbon-based material, and the core may include, for example, a lithium transition metal oxide. The first carbon-based material and the transition metal of the lithium transition metal oxide are chemically bound (bound) through, for example, a chemical bond. The carbon atom (C) of the first carbon-based material and the transition metal (Me) of the lithium transition metal oxide are chemically bound through, for example, a CO-Me bond (for example, a CO-Ni bond or a CO-Co bond) via an oxygen atom. The first carbon-based material disposed in the shell and the lithium transition metal oxide disposed in the core are chemically bound through a chemical bond, thereby forming a composite of the core and the shell. Therefore, the composite positive electrode active material is distinguished from a simple physical mixture of the first carbon-based material and the lithium transition metal oxide. The first metal oxide and the first carbon-based material may also be chemically bound through a chemical bond. Here, the chemical bond is, for example, a covalent bond or an ionic bond.
[0062] The shell may include, for example, one or more selected from a first metal oxide and a second metal oxide, and the particle size of the one or more selected from the first metal oxide and the second metal oxide may be, for example, 1 nm to 100 nm, 1 nm to 50 nm, 1 nm to 30 nm, 5 nm to 30 nm, or 10 nm to 30 nm. The first metal oxide and / or the second metal oxide may be more uniformly distributed in the first carbon-based material matrix by having such a nano-range particle size. If the particle size of one or more of the first metal oxide and the second metal oxide is excessively increased, the thickness of the shell may increase, and the internal resistance of the composite positive electrode active material may increase. If the particle size of one or more of the first metal oxide and the second metal oxide is excessively reduced, uniform dispersion may be difficult.
[0063] The shell includes a first metal oxide and / or a second metal oxide, and also includes a first carbon-based material. The first carbon-based material can be arranged in a direction protruding from the surface of the first metal oxide and / or the second metal oxide. The first carbon-based material can be arranged in a direction protruding from the surface of the first metal oxide and / or the second metal oxide by directly growing from the surface of the first metal oxide and / or the second metal oxide. The first carbon-based material arranged in a direction protruding from the surface of the first metal oxide and / or the second metal oxide can be, for example, a carbon-based two-dimensional nanostructure, a carbon-based flake, or graphene.
[0064] The thickness of the shell is, for example, 1 nm to 5 μm, 1 nm to 1 μm, 1 nm to 500 nm, 1 nm to 200 nm, 1 nm to 100 nm, 1 nm to 90 nm, 1 nm to 80 nm, 1 nm to 70 nm, 1 nm to 60 nm, 1 nm to 50 nm, 1 nm to 40 nm, 1 nm to 30 nm, or 1 nm to 20 nm. When the shell has a thickness in such a range, the electronic conductivity of the positive electrode including the composite positive electrode active material can be further improved.
[0065] The composite positive electrode active material may further include, for example, a third metal doped on the core and / or a third metal oxide coated on the core. A shell may be disposed on the third metal doped on the core and / or on the third metal oxide coated on the core. For example, the surface of the lithium transition metal oxide core may be doped with the third metal, or the surface of the lithium transition metal oxide may be coated with the third metal oxide, and then a shell may be disposed on the third metal and / or the third metal oxide. For example, the composite positive electrode active material may include a core, an intermediate layer disposed on the core, and a shell disposed on the intermediate layer, the intermediate layer including the third metal or the third metal oxide. The third metal is one or more metals selected from Al, Zr, W, and Co, and the third metal oxide is Al. 2 O 3 , Li 2 O-ZrO2 , WO 2 , CoO, Co 2 O 3 , Co 3 O 4 , or a combination thereof.
[0066] The shell disposed along the surface of the core may comprise, for example, one or more selected from a composite comprising a first metal oxide and a first carbon-based material, for example, graphene, and / or a milling result of the composite. The first metal oxide is disposed in a matrix of the carbon-based material, for example, a graphene matrix. The shell may be produced, for example, from a composite comprising the first metal oxide and the first carbon-based material, for example, graphene. The composite may further comprise a second metal oxide in addition to the first metal oxide. The composite may comprise, for example, two or more kinds of first metal oxides. The composite may comprise, for example, two or more kinds of first metal oxides and two or more kinds of second metal oxides.
[0067] The content of one or more of the composite and milling products thereof may be, for example, 5 wt% or less, 3 wt% or less, 2 wt% or less, 2.5 wt% or less, or 1.5 wt% or less of the total weight of the composite positive electrode active material. The content of one or more of the composite and milling products thereof may be 0.01 wt% to 5 wt%, 0.01 wt% to 4 wt%, 0.01 wt% to 3 wt%, 0.01 wt% to 2.5 wt%, 0.01 wt% to 2 wt%, or 0.01 wt% to 1.5 wt% of the total weight of the composite positive electrode active material. When the composite positive electrode active material includes one or more of the composite and milling products thereof within such ranges, the cycle characteristics of a lithium battery including the composite positive electrode active material are further improved.
[0068] The composite may also include one or more selected from a first metal oxide and a second metal oxide. The particle size of the one or more selected from the first metal oxide and the second metal oxide may be 1 nm to 100 nm, 1 nm to 50 nm, 1 nm to 30 nm, 5 nm to 30 nm, or 10 nm to 30 nm. The first metal oxide and / or the second metal oxide may have such a nano-range particle size, so that they can be more uniformly distributed in the first carbon-based material matrix of the composite. Thus, such a composite may be uniformly coated on the core without agglomeration to form a shell. Furthermore, the first metal oxide and / or the second metal oxide may have such a particle size range, so that they may be more uniformly arranged on the core. Thus, the first metal oxide and / or the second metal oxide may be uniformly arranged on the core, so that the voltage resistance characteristics may be more effectively exhibited. The particle size of the first metal oxide and / or the second metal oxide may be measured using, for example, a measuring device using a laser diffraction method or a dynamic light scattering method. The particle size is, for example, measured using a laser scattering particle size distribution meter (e.g., HORIBA LA-920) and is the median particle size (D50) value when 50% is accumulated from the smallest particle side in volume conversion. The uniformity deviation of one or more selected from the first metal oxide and / or the second metal oxide is 3% or less, 2% or less, or 1% or less. The uniformity can be determined, for example, by XPS (X-ray photoelectron spectroscopy). Thus, one or more selected from the first metal oxide and the second metal oxide can be uniformly distributed in the composite with a deviation of 3% or less, 2% or less, or 1% or less.
[0069] The composite includes a first carbon-based material. The first carbon-based material may have, for example, a branched structure, and one or more metal oxides selected from the first metal oxide and the second metal oxide may be distributed in the branched structure of the first carbon-based material. The branched structure of the first carbon-based material may include, for example, a plurality of first carbon-based material particles that are in contact with each other. The first carbon-based material may have a branched structure to provide various conductive paths. The first carbon-based material may be, for example, graphene. The graphene may have, for example, a branched structure, and one or more metal oxides selected from the first metal oxide and the second metal oxide may be distributed in the branched structure of graphene. The branched structure of graphene may include, for example, a plurality of graphene particles that are in contact with each other. The graphene may have a branched structure to provide various conductive paths.
[0070] The first carbon-based material may have a spherical structure, for example, and one or more metal oxides selected from the first metal oxide and the second metal oxide may be distributed within the spherical structure. The size of the spherical structure of the first carbon-based material may be 50 nm to 300 nm. There may be a plurality of first carbon-based materials having the spherical structure. Since the first carbon-based material has a spherical structure, the composite may have a robust structure. The first carbon-based material may be, for example, graphene. The graphene may have a spherical structure, for example, and one or more metal oxides selected from the first metal oxide and the second metal oxide may be distributed within the spherical structure. The size of the spherical structure of the graphene may be 50 nm to 300 nm. There may be a plurality of graphenes having the spherical structure. Since the graphene has a spherical structure, the composite may have a robust structure.
[0071] The first carbon-based material may have a spiral structure in which a plurality of spherical structures are connected, and one or more metal oxides selected from the first metal oxide and the second metal oxide may be distributed in the spiral structure. The size of the spiral structure of the first carbon-based material may be 500 nm to 100 μm. Since the first carbon-based material has a spiral structure, the composite may have a robust structure. The first carbon-based material may be graphene. Graphene may have a spiral structure in which a plurality of spherical structures are connected, and one or more metal oxides selected from the first metal oxide and the second metal oxide may be distributed in the spiral structure. The size of the spiral structure of graphene may be 500 nm to 100 μm. Since the graphene has a spiral structure, the composite may have a robust structure.
[0072] The first carbon-based material may have a cluster structure in which a plurality of spherical structures are aggregated, and one or more metal oxides selected from the first metal oxide and the second metal oxide may be distributed within the spherical structures of the cluster structure. The size of the cluster structure of the first carbon-based material may be 0.5 mm to 10 cm. Since the first carbon-based material has a cluster structure, the composite may have a robust structure. The first carbon-based material may be graphene, for example. Graphene may have a cluster structure in which a plurality of spherical structures are aggregated, and one or more metal oxides selected from the first metal oxide and the second metal oxide may be distributed within the spherical structures of the cluster structure. The size of the graphene cluster structure may be 0.5 mm to 10 cm. Since the graphene has a cluster structure, the composite may have a robust structure.
[0073] The composite may be, for example, a faceted-ball structure, and one or more selected from the first metal oxide and the second metal oxide may be distributed inside or on the surface of the structure. Because the composite has such a polyhedral ball structure, the composite may be easily coated on the irregular surface irregularities of the core.
[0074] The composite may be, for example, a planar structure, and one or more selected from the first metal oxide and the second metal oxide may be distributed inside or on the surface of the structure. Because the composite has such a two-dimensional planar structure, the composite may be easily coated on the irregular surface unevenness of the core.
[0075] The first carbon-based material may extend from the first metal oxide by a distance of 10 nm or less and include at least 1 to 20 carbon-based material layers. For example, a plurality of first carbon-based material layers may be stacked to provide a first carbon-based material having a total thickness of 12 nm or less on the first metal oxide. For example, the total thickness of the first carbon-based material may be 0.6 nm to 12 nm. The first carbon-based material may be graphene. The graphene may extend from the first metal oxide by a distance of 10 nm or less and include at least 1 to 20 graphene layers. For example, a plurality of graphene layers may be stacked to provide a first carbon-based material having a total thickness of 12 nm or less on the first metal oxide. For example, the total thickness of the graphene may be 0.6 nm to 12 nm.
[0076] The composite positive electrode active material includes a core, which may include a lithium transition metal oxide, for example, represented by any one of Formulas 1 to 8 below.
[0077] [Chemical formula 1] Li a Ni x Mn y M' z O 2-b A b
[0078] In the above Chemical Formula 1, 1.0≦a≦1.2, 0≦b≦0.2, 0 <x≦0.85、0.1≦y<0.3、0<z≦0.1であり、x+y+z=1であり、 M' is cobalt (Co), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), boron (B), or a combination thereof; A is F, S, Cl, Br, or a combination thereof;
[0079] [Chemical formula 2] LiNi x Co y Mn z O 2
[0080] [Chemical formula 3] LiNi x Co y Al z O 2
[0081] In the formulas 2 and 3, 0.8≦x≦0.95, 0≦y≦0.2, 0 <z≦0.2であり、x+y+z=1である。
[0082] [Chemical formula 4] LiNi x Co y Mn z Al w O 2
[0083] In the formula 4, 0.8≦x≦0.95, 0≦y≦0.2, 0 <z≦0.2、0<w≦0.2であり、x+y+z+w=1である。
[0084] The lithium transition metal oxides of Formulas 1 to 4 may have a high nickel content of 80 mol% or more, 85 mol% or more, 90 mol% or more, or 90 mol% or more, based on the total transition metal moles, while providing excellent initial capacity, room temperature life characteristics, and high temperature life characteristics. For example, in the lithium transition metal oxides of Formulas 1 to 4, the nickel content is 80 mol% to 99 mol%, 85 mol% to 99 mol%, or 90 mol% to 97 mol% based on the total transition metal moles.
[0085] [Chemical formula 5] Li a Co x M y O 2-b A b
[0086] In the above Chemical Formula 5, 1.0≦a≦1.2, 0≦b≦0.2, 0.9≦x≦1, 0≦y≦0.1, and x+y=1; M is manganese (Mn), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), boron (B), or a combination thereof; and A is F, S, Cl, Br, or a combination thereof.
[0087] [Chemical formula 6] Li a Ni x Co y M z O 2-b A b
[0088] In the above Chemical Formula 6, 1.0≦a≦1.2, 0≦b≦0.2, 0.8≦x<1, 0≦y≦0.3, 0 <z≦0.3であり、x+y+z=1であり、 M is manganese (Mn), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), boron (B), or a combination thereof; A is F, S, Cl, Br, or a combination thereof.
[0089] [Chemical formula 7] Li a M1 x M2 y PO 4-b X b
[0090] In the formula 7, 0.90≦a≦1.1, 0≦x≦0.9, 0≦y≦0.5, 0.9 <x+y<1.1であり、0≦b≦2であり、 M1 is chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zirconium (Zr), or a combination thereof; M2 is magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), zinc (Zn), boron (B), niobium (Nb), gallium (Ga), indium (In), molybdenum (Mo), tungsten (W), aluminum (Al), silicon (Si), chromium (Cr), vanadium (V), scandium (Sc), yttrium (Y), or a combination thereof; and X is O, F, S, P, or a combination thereof.
[0091] [Chemical formula 8] Li a M3 z PO 4
[0092] In the formula 8, 0.90≦a≦1.1 and 0.9≦z≦1.1; M3 is chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zirconium (Zr), or a combination thereof.
[0093] According to an embodiment, the composite positive electrode active material uses bimodal polycrystalline large particle size and polycrystalline small particle size as a core material, and a shell formed on at least one surface of the core material includes a composite and fibrous carbon to provide a composite positive electrode active material.
[0094] In the shell, the composite can anchor carbon nanotubes (CNTs) through π-π bonds with fibrous carbon such as CNTs. Since the coating of CB (carbon black) and CNTs is produced by a dry method, separation of CNTs, which occurs in wet coating, is suppressed, and the carbon nanotubes (CNTs) do not separate from the composite positive electrode active material even during the electrode slurry production process.
[0095] In the shell, the content of the fibrous carbon, which is the second carbon-based material, is in the range of 1 wt% or less based on the total weight of the composite positive electrode active material. When in such a range, the viscosity of the electrode slurry is not increased, and workability is excellent.
[0096] According to another embodiment, a positive electrode includes the composite positive electrode active material, which provides improved energy density, improved cycle characteristics, and increased conductivity.
[0097] The shell of the composite positive electrode active material includes a second carbon-based material, so that the composite positive electrode active material can additionally function as a conductive material. Therefore, the content of the conductive material used in the positive electrode can be reduced. The conductive material is necessary for improving the conductivity of the battery, but if the content of the conductive material increases, the mixed density of the positive electrode decreases, and as a result, the energy density of the lithium battery decreases. In contrast, the positive electrode of the present invention can reduce the content of the conductive material without increasing the internal resistance by using the above-mentioned composite positive electrode active material. Therefore, the mixed density of the positive electrode increases, and as a result, the energy density of the lithium battery can be improved. In particular, in a high-capacity lithium battery, the energy density of the lithium battery can be greatly increased by increasing the content of the composite positive electrode active material while reducing the content of the conductive material.
[0098] If the shell of the composite positive electrode active material contains only the second carbon-based material, the second carbon-based material may be detached during preparation of the slurry containing the second carbon-based material, causing the electrode slurry viscosity to increase and the electrode plate quality to deteriorate, making the electrode essentially unusable.
[0099] However, in the composite positive electrode active material according to one embodiment, the shell includes one or more first metal oxides, a first carbon-based material, and a second carbon-based material, and the composite in which the first metal oxide is disposed within the matrix of the first carbon-based material stably attaches the second carbon-based material to the surface of the positive electrode active material, forming a coating layer from which the second carbon-based material is not easily detached.
[0100] The positive electrode can be produced, for example, by a wet process. The positive electrode can be produced, for example, by the following exemplary method, but is not necessarily limited to such a method and can be adjusted according to the required conditions.
[0101] First, the composite positive electrode active material, a conductive material, a binder, and a solvent are mixed to prepare a positive electrode active material composition. The prepared positive electrode active material composition is directly coated on an aluminum current collector and dried to manufacture a positive electrode plate having a positive electrode active material layer. Alternatively, the positive electrode active material composition is cast on a separate support and then peeled off from the support to obtain a film, which is then laminated on the aluminum current collector to manufacture a positive electrode plate having a positive electrode active material layer.
[0102] The conductive material may be, for example, denka black. The conductive material may be, but is not limited to, carbon black, graphite particles, natural graphite, artificial graphite, acetylene black, ketjen black, carbon fiber, carbon nanotubes, metal powder, metal fiber or metal tube, such as copper, nickel, aluminum, silver, etc., or conductive polymers such as polyphenylene derivatives. As an alternative, the positive electrode may not include a separate conductive material.
[0103] Examples of binders that can be used include vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, polytetrafluoroethylene (PTFE), mixtures of the aforementioned polymers, and styrene-butadiene rubber-based polymers. Examples of solvents that can be used include N-methylpyrrolidone (NMP), acetone, and water, but the present invention is not limited to these and any solvent that is used in the relevant technical field can be used.
[0104] A plasticizer or pore-forming agent may be further added to the positive electrode active material composition to form pores within the electrode plate.
[0105] The contents of the composite positive electrode active material, conductive material, binder, and solvent used in the positive electrode are at the levels generally used in lithium batteries, and one or more of the conductive material, binder, and solvent may be omitted depending on the application and configuration of the lithium battery.
[0106] The content of the binder used in the positive electrode is 0.1 wt% to 10 wt%, or 0.1 wt% to 5 wt% of the total weight of the positive electrode active material layer. The content of the composite positive electrode active material used in the positive electrode is 80 wt% to 99 wt%, 90 wt% to 99 wt%, or 95 wt% to 99 wt% of the total weight of the positive electrode active material layer. The content of the conductive material used in the positive electrode is 0.01 wt% to 10 wt%, 0.01 wt% to 5 wt%, 0.01 wt% to 3 wt%, 0.01 wt% to 1 wt%, 0.01 wt% to 0.5 wt%, or 0.01 wt% to 0.1 wt% of the total weight of the positive electrode active material layer. The conductive material may be omitted.
[0107] The positive electrode may further include, in addition to the composite positive electrode active material, other common positive electrode active materials.
[0108] A typical positive electrode active material is a lithium-containing metal oxide, and any of those commonly used in the art may be used without limitation. For example, one or more composite oxides of lithium and a metal selected from cobalt, manganese, nickel, and combinations thereof may be used. Specific examples of the composite oxides include Li a A 1-b B b D 2 (wherein, 0.90≦a≦1 and 0≦b≦0.5); Li a E 1-b B b O 2-c D c (wherein, 0.90≦a≦1, 0≦b≦0.5, and 0≦c≦0.05); LiE 2-b B b O 4-c D c (wherein, 0≦b≦0.5 and 0≦c≦0.05); Li a Ni 1-b-c Co b B c D α (wherein, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α≦2); Lia Ni 1-b-c Co b B c O 2-α F' α (wherein, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni 1-b-c Co b B c O 2-α F' 2 (wherein, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni 1-b-c Mn b B c D α (wherein, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α≦2); Li a Ni 1-b-c Mn b B c O 2-α F' α (wherein, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni 1-b-c Mn b B c O 2-α F' 2 (wherein, 0.90≦a≦1, 0≦b≦0.5, 0≦c≦0.05, and 0<α<2); Li a Ni b E c G d O 2 (wherein, 0.90≦a≦1, 0≦b≦0.9, 0≦c≦0.5, and 0.001≦d≦0.1); Li a Ni b Co c Mn d G e O 2 (wherein, 0.90≦a≦1, 0≦b≦0.9, 0≦c≦0.5, 0≦d≦0.5, and 0.001≦e≦0.1); Li a NiG b O 2(wherein, 0.90≦a≦1, 0.001≦b≦0.1); Li a CoG b O 2 (wherein, 0.90≦a≦1, 0.001≦b≦0.1); Li a MnG b O 2 (wherein, 0.90≦a≦1, 0.001≦b≦0.1); Li a Mn 2 G b O 4 (wherein, 0.90≦a≦1, 0.001≦b≦0.1); QO 2 ;QS 2 ;LiQS 2 ;V 2 O 5 ;LiV 2 O 5 ;LiIO 2 ;LiNiVO 4 Li (3-f) J 2 (PO 4 ) 3 (0≦f≦2);Li (3-f) Fe 2 (PO 4 ) 3 (0≦f≦2); LiFePO 4 A compound represented by any one of the following chemical formulas can be used.
[0109] In the chemical formula expressing the above-mentioned compound, A is Ni, Co, Mn, or a combination thereof, B is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element, or a combination thereof, D is O, F, S, P, or a combination thereof, E is Co, Mn, or a combination thereof, F' is F, S, P, or a combination thereof, G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or a combination thereof, Q is Ti, Mo, Mn, or a combination thereof, I is Cr, V, Fe, Sc, Y, or a combination thereof, and J is V, Cr, Mn, Co, Ni, Cu, or a combination thereof. It is also possible to use a compound having a coating layer added to the surface of the above-mentioned compound, and it is also possible to use a mixture of the above-mentioned compound and a compound having a coating layer added thereto. The coating layer added to the surface of the above-mentioned compound includes, for example, a coating element compound such as an oxide of the coating element, a hydroxide of the coating element, an oxyhydroxide of the coating element, an oxycarbonate of the coating element, or a hydroxycarbonate of the coating element. The compound forming such a coating layer is amorphous or crystalline. The coating element contained in the coating layer is Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or a mixture thereof. The coating layer forming method is selected within a range that does not adversely affect the physical properties of the positive electrode active material. The coating method is, for example, a spray coating method, a dipping method, etc. A detailed description of the specific coating method is omitted because it is a content that can be fully understood by those engaged in the field.
[0110] Alternatively, the positive electrode may be a dry positive electrode manufactured by a dry process.
[0111] The dry positive electrode includes a dry composite positive electrode active material, a dry conductive material, and a dry binder, the dry composite positive electrode active material including a core including a lithium transition metal oxide and a shell disposed along a surface of the core, the shell being represented by the chemical formula M a Ob One or more first metal oxides represented by (0 < a ≤ 3, 0 < b < 4, and if a is 1, 2, or 3, then b is not an integer), a first carbon-based material, and a second carbon-based material, wherein the first metal oxide is disposed within a first carbon-based material matrix, M is one or more metals selected from Groups 2 to 13 of the Periodic Table of the Elements, Groups 15 and 16 of the Periodic Table of the Elements, and the second carbon-based material is fibrous carbon having an aspect ratio of 10 or more.
[0112] The method for manufacturing a dry cathode includes, for example, a step of dry-mixing a dry composite cathode active material, a dry conductive material, and a dry binder to prepare a dry mixture, a step of providing a cathode current collector, a step of disposing an intermediate layer on one surface of the cathode current collector, and a step of disposing the dry mixture on the intermediate layer and rolling it to manufacture a cathode having a cathode active material layer disposed on one surface of the cathode current collector.
[0113] First, a composite cathode active material, a dry conductive material, and a dry binder are dry-mixed to prepare a dry mixture. The dry mixing means mixing in a state without including a process solvent. The process solvent is, for example, a solvent used for manufacturing an electrode slurry. The process solvent is, for example, water, N-methylpyrrolidone (NMP), etc., but is not limited thereto, as long as it is a process solvent used during the manufacture of the electrode slurry. The dry mixing can be performed using a stirrer, for example, at a temperature of 25°C to 65°C. The dry mixing can be performed using a stirrer, for example, at a rotational speed of 10 to 10,000 rpm, or 100 to 10,000 rpm. The dry mixing can be performed using a stirrer, for example, for 1 minute to 200 minutes, or 1 minute to 150 minutes. The composite cathode active material is a dry composite cathode active material.
[0114] The dry mixing may be performed, for example, one or more times. First, the composite positive electrode active material, the dry conductive material, and the dry binder may be primarily dry mixed to prepare a first mixture. The primary dry mixing may be performed, for example, at a temperature of 25° C. to 65° C. and at a rotation speed of 2,000 rpm or less for a time period of 15 minutes or less. The primary dry mixing may be performed, for example, at a temperature of 25° C. to 65° C. and at a rotation speed of 500 to 2,000 rpm for a time period of 5 to 15 minutes. The primary dry mixing may allow the composite positive electrode active material, the dry conductive material, and the dry binder to be uniformly mixed. Then, the composite positive electrode active material, the dry conductive material, and the dry binder may be secondary dry mixed to prepare a second mixture. The secondary dry mixing may be performed, for example, at a temperature of 25° C. to 65° C. and at a rotation speed of 4,000 rpm or more for a time period of 10 minutes or more. The secondary dry mixing can be carried out, for example, at a temperature of 25° C. to 65° C. and a rotation speed of 4,000 to 9,000 rpm for 10 to 60 minutes. The secondary dry mixing results in a dry mix containing a fibrillated dry binder.
[0115] The agitator is, for example, a kneader. The agitator includes, for example, a chamber, one or more rotating shafts arranged inside the chamber and rotating, and a blade rotatably coupled to the rotating shaft and arranged in the longitudinal direction of the rotating shaft. The blade may be, for example, one or more selected from a ribbon blade, a sigma blade, a jet (Z) blade, a dispersion blade, and a screw blade. By including the blade, the dry composite positive electrode active material, the dry conductive material, and the dry binder can be effectively mixed without a solvent to produce a dough-like mixture.
[0116] The prepared dry mixture can be put into an extrusion device and extruded into a sheet. The pressure during extrusion is, for example, 4 MPa to 100 MPa, or 10 MPa to 90 MPa. The obtained sheet-shaped extrudate is also a sheet for a positive electrode active material layer.
[0117] Examples of the dry conductive material include, but are not limited to, carbon black, graphite particles, natural graphite, artificial graphite, acetylene black, ketjen black, carbon fiber, carbon nanotube, metal powder, metal fiber or metal tube such as copper, nickel, aluminum, silver, etc., and conductive polymer such as polyphenylene derivative. Any material used as a conductive material in the art is acceptable. The conductive material is, for example, a carbon-based conductive material. The dry conductive material is a conductive material that is not in contact with a process solvent.
[0118] The dry binder may be, but is not limited to, vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, polytetrafluoroethylene (PTFE), a mixture of the above polymers, styrene butadiene rubber-based polymers, etc. Any binder used in the art may be used. The dry binder may be, for example, polytetrafluoroethylene (PTFE). The dry binder is a binder that has not come into contact with a process solvent.
[0119] A plasticizer or pore-forming agent may be further added to the dry mixture to form pores within the positive electrode active material layer.
[0120] The contents of the dry composite positive electrode active material, the dry conductive material, and the dry binder used in the dry positive electrode are in the same ranges as the contents of the composite positive electrode active material, the conductive material, and the binder used in the wet positive electrode.
[0121] Next, a positive electrode current collector is provided.
[0122] The positive electrode current collector is, for example, a plate or foil made of indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof. The positive electrode current collector is, for example, aluminum foil.
[0123] The positive electrode current collector can be omitted. The thickness of the positive electrode current collector is, for example, 1 μm to 100 μm, 1 μm to 50 μm, 5 μm to 25 μm, or 10 μm to 20 μm.
[0124] The positive electrode current collector may include, for example, a base film and a metal layer disposed on one or both sides of the base film. The base film may include, for example, a polymer. The polymer may include, for example, a thermoplastic polymer. The polymer may include, for example, polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof. When the base film includes a thermoplastic polymer, the base film is liquefied when a short circuit occurs, and a sudden increase in current can be suppressed. The base film may be, for example, an insulator. The metal layer may include, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), or an alloy thereof. The positive electrode current collector may further include a metal chip and / or a lead tab. For more details regarding the base film, metal layer, metal chip, and lead tab of the positive electrode current collector, please refer to the negative electrode current collector described below. By having such a structure of the positive electrode current collector, the weight of the electrode can be reduced, and as a result, the energy density can be improved.
[0125] Next, an intermediate layer is disposed on at least one surface of the positive electrode current collector. The intermediate layer also includes a carbon-based conductive material and a binder. The intermediate layer may be omitted.
[0126] Next, the prepared positive electrode active material layer sheet is placed on the intermediate layer and rolled to produce a positive electrode in which a positive electrode active material layer is placed on one side of the positive electrode current collector. The intermediate layer is placed between the positive electrode current collector and the positive electrode active material layer. The rolling may be, for example, a roll press or a flat plate press, but is not necessarily limited thereto. The pressure during rolling is, for example, 0.1 ton / cm. 2 or 10.0 ton / cm 2 However, the pressure is not limited to such a range. If the pressure during rolling is too high, cracks may occur in the positive electrode current collector. If the pressure during rolling is too low, the bonding strength between the positive electrode current collector and the positive electrode active material layer may be reduced.
[0127] A lithium battery according to another embodiment employs a positive electrode including the composite positive electrode active material described above.
[0128] The lithium battery employs a positive electrode containing the above-mentioned composite positive electrode active material, thereby providing improved energy density, cycle characteristics and thermal stability.
[0129] The lithium battery can be manufactured, for example, by the following exemplary method, but is not necessarily limited to such a method, and can be adjusted according to the required conditions.
[0130] First, the positive electrode is produced by the above-mentioned positive electrode production method.
[0131] Next, the negative electrode is prepared as follows. The negative electrode is prepared in substantially the same manner as the positive electrode, except that, for example, a negative electrode active material is used instead of the composite positive electrode active material. In addition, the conductive material, binder, and solvent in the negative electrode active material composition may be substantially the same as those in the positive electrode.
[0132] For example, a negative electrode active material, a conductive material, a binder, and a solvent are mixed to prepare a negative electrode active material composition, which is then directly coated onto a negative electrode current collector to prepare a negative electrode plate. Alternatively, the prepared negative electrode active material composition is cast onto a separate support, and the negative electrode active material film peeled off from the support is laminated onto a copper current collector to prepare a negative electrode plate.
[0133] The negative electrode active material may be any material known in the art that is used as a negative electrode active material for lithium batteries. For example, the negative electrode active material may include at least one selected from the group consisting of lithium metal, metals capable of being alloyed with lithium, transition metal oxides, non-transition metal oxides, and carbon-based materials. The metals capable of being alloyed with lithium may be, for example, Si, Sn, Al, Ge, Pb, Bi, Sb, Si-Y alloy (wherein Y is an alkali metal, alkaline earth metal, Group 13 element, Group 14 element, transition metal, rare earth element, or a combination thereof, but is not Si), Sn-Y alloy (wherein Y is an alkali metal, alkaline earth metal, Group 13 element, Group 14 element, transition metal, rare earth element, or a combination thereof, but is not Sn), etc. The element Y is, for example, Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Ti, Ge, P, As, Sb, Bi, S, Se, Te, Po, or a combination thereof. The transition metal oxide is, for example, lithium titanium oxide, vanadium oxide, lithium vanadium oxide, etc. The non-transition metal oxide is, for example, SnO 2 , SiO xIt is, for example, (0 < x < 2). The carbon-based material is, for example, crystalline carbon, amorphous carbon, or a mixture thereof. The crystalline carbon is, for example, graphite such as amorphous, plate-like, flaky, spherical or fibrous natural graphite or artificial graphite. The amorphous carbon is, for example, soft carbon (low-temperature calcined carbon) or hard carbon, mesophase pitch carbide, calcined coke, etc.
[0134] The contents of the negative electrode active material, conductive material, binder and solvent are at levels generally used in lithium batteries. Depending on the use and configuration of the lithium battery, one or more of the aforementioned conductive material, binder and solvent can be omitted.
[0135] The binder content used for the negative electrode is, for example, 0.1 wt% to 10 wt%, or even 0.1 wt% to 5 wt% of the total weight of the negative electrode active material layer. The conductive material content used for the negative electrode is, for example, 0.1 wt% to 10 wt%, or even 0.1 wt% to 5 wt% of the total weight of the negative electrode active material layer. The negative electrode active material content used for the negative electrode is, for example, 80 wt% to 99 wt%, 90 wt% to 99 wt%, or even 95 wt% to 99 wt% of the total weight of the negative electrode active material layer. When the negative electrode active material is lithium metal, the negative electrode does not contain a binder and a conductive material.
[0136] The negative electrode current collector is composed of, for example, a material that does not react with lithium, that is, does not form any alloys and compounds. The material constituting the negative electrode current collector is, for example, copper (Cu), stainless steel, titanium (Ti), iron (Fe), cobalt (Co) and nickel (Ni), etc., but is not necessarily limited thereto. As long as it is used as an electrode current collector in the technical field, any of them is possible. The negative electrode current collector can be composed of one of the aforementioned metals, or an alloy of two or more metals, or a coating material. The negative electrode current collector is, for example, plate-like or foil-like.
[0137] The negative electrode current collector may include, for example, a base film and a metal layer disposed on one or both sides of the base film. The base film may include, for example, a polymer. The polymer may include, for example, a thermoplastic polymer. The polymer may include, for example, polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof. When the base film includes a thermoplastic polymer, the base film may be liquefied in the event of a short circuit, thereby suppressing a sudden increase in current. The base film may be, for example, an insulator. The metal layer may include, for example, copper (Cu), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), or an alloy thereof. The metal layer may act as an electrochemical fuse and may be cut off in the event of an overcurrent, thereby performing a short circuit prevention function. The thickness of the metal layer may be adjusted to adjust the limit current and maximum current. The metal layer may be electrochemically plated or vapor-deposited on the base film. If the thickness of the metal layer is reduced, the limiting current and / or maximum current of the negative electrode current collector may be reduced, and the stability of the lithium battery during a short circuit may be improved. A lead tab may be added to the metal layer for connection to the outside. The lead tab may be welded to the metal layer or the metal layer / base film laminate by ultrasonic welding, laser welding, spot welding, or the like. During welding, the base film and / or the metal layer may be melted and the metal layer may be electrically connected to the lead tab. In order to further strengthen the welding between the metal layer and the lead tab, a metal piece may be added between the metal layer and the lead tab. The metal piece may be a thin piece of the same material as the metal of the metal layer. The metal piece may be, for example, a metal foil, a metal mesh, or the like. The metal piece may be, for example, aluminum foil, copper foil, or SUS (steel use stainless) foil.After disposing a metal piece on the metal layer, the lead tab can be welded to the metal piece / metal layer laminate or the metal piece / metal layer / base film laminate. During welding, the base film, the metal layer, and / or the metal piece can be melted and the metal layer or the metal layer / metal piece laminate can be electrically connected to the lead tab. The metal piece and / or the lead tab can be added to a portion on the metal layer. The thickness of the base film can be, for example, 1 to 50 μm, 1.5 to 50 μm, 1.5 to 40 μm, or 1 to 30 μm. The weight of the electrode assembly can be further effectively reduced by the base film having a thickness in such a range. The melting point of the base film can be, for example, 100° C. to 300° C., 100° C. to 250° C., or 100° C. to 200° C. Since the base film has a melting point in such a range, the base film can be melted and easily bonded to the lead tab during the process of welding the lead tab. In order to improve the adhesive strength between the base film and the metal layer, a surface treatment such as a corona treatment can be performed on the base film. The thickness of the metal layer can be, for example, 0.01 to 3 μm, 0.1 to 3 μm, 0.1 to 2 μm, or 0.1 to 1 μm. Since the metal layer has a thickness in such a range, the stability of the electrode assembly can be ensured while maintaining conductivity. The thickness of the metal piece can be, for example, 2 to 10 μm, 2 to 7 μm, or 4 to 6 μm. Since the metal piece has a thickness in such a range, the connection between the metal layer and the lead tab can be more easily performed. Since the negative electrode current collector has such a structure, the weight of the electrode can be reduced, and as a result, the energy density can be improved.
[0138] Next, a separator to be inserted between the positive electrode and the negative electrode is prepared.
[0139] The separator may be any separator that is generally used in lithium batteries. For example, the separator has low resistance to ion migration of the electrolyte and excellent electrolyte moisture-absorbing ability. The separator is, for example, selected from glass fiber, polyester, Teflon (registered trademark), polyethylene, polypropylene, polytetrafluoroethylene (PTFE), or a combination thereof, and is in the form of a nonwoven or woven fabric. For example, a rollable separator such as polyethylene or polypropylene is used for a lithium ion battery, and a separator with excellent organic electrolyte impregnation ability is used for a lithium ion polymer battery.
[0140] The separator is manufactured by the following exemplary method, but is not necessarily limited to such method, and may be adjusted according to the required conditions.
[0141] First, a separator composition is prepared by mixing a polymer resin, a filler, and a solvent. The separator composition is directly coated on the top of an electrode and dried to form a separator. Alternatively, the separator composition is cast on a support and dried, and the separator film is peeled off from the support and laminated on the top of an electrode to form a separator.
[0142] The polymer used for the separator is not particularly limited, and any polymer that is used as a binder for electrode plates can be used, such as vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, or a mixture thereof.
[0143] Next, the electrolyte is prepared.
[0144] The electrolyte is, for example, an organic electrolytic solution, which is produced, for example, by dissolving a lithium salt in an organic solvent.
[0145] The organic solvent may be any organic solvent used in the art, such as propylene carbonate, ethylene carbonate, fluoroethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, dibutyl carbonate, benzonitrile, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, γ-butyrolactone, dioxolane, 4-methyldioxolane, N,N-dimethylformamide, dimethylacetamide, dimethylsulfoxide, dioxane, 1,2-dimethoxyethane, sulfolane, dichloroethane, chlorobenzene, nitrobenzene, diethylene glycol, dimethyl ether, or mixtures thereof.
[0146] The lithium salt may be any lithium salt known in the art. For example, LiPF 6 , LiBF 4 , LiSbF 6 , LiAsF 6 , LiClO 4 , LiCF 3 SO 3 , Li(CF 3 SO 2 ) 2 N, LiC 4 F 9 SO 3 , LiAlO 2 , LiAlCl 4 , LiN(C x F 2x+1 SO 2 )(C y F 2y+1 SO 2 ) (wherein x and y are each an integer from 1 to 20), LiCl, LiI, or a mixture thereof.
[0147] Alternatively, the electrolyte is a solid electrolyte, such as, but not limited to, boron oxide, lithium oxynitride, or any other material known in the art for use as a solid electrolyte, which may be formed on the negative electrode, for example, by sputtering, or a separate solid electrolyte sheet may be laminated on the negative electrode.
[0148] The solid electrolyte is, for example, an oxide-based solid electrolyte, a sulfide-based solid electrolyte, a polymer solid electrolyte, or a combination thereof. The solid electrolyte is, for example, an oxide-based solid electrolyte.
[0149] The oxide-based solid electrolyte is Li 1+x+y Al x Ti 2-x S y P 3-y O 12 (0 <x<2、0≦y<3)、BaTiO 3 , Pb(Zr,Ti)O 3 (PZT), Pb 1-x La x Zr 1-y Ti y O 3 (PLZT)(O≦x<1, O≦y<1), PB(Mg 3 Nb 2 / 3 )O 3 -PbTiO 3 (PMN-PT), HfO 2 , SrTiO 3 , SnO 2 , CEO 2 , Na 2 O, MgO, NiO, CaO, BaO, ZnO, ZrO 2 , Y 2 O 3 , Al 2 O 3 , TiO 2 , SiO 2 , Li 3 PO 4 , Li x Ti y (PO 4 ) 3(0 < x < 2, 0 < y < 3), Li x Al y Ti z (PO 4 ) 3 (0 < x < 2, 0 < y < 1, 0 < z < 3), Li 1+x+y (Al, Ga) x (Ti, Ge) 2-x Si y P 3-y O 12 (0 ≤ x ≤ 1, 0 ≤ y ≤ 1), Li x La y TiO 3 (0 < x < 2, 0 < y < 3), Li 2 O, LiOH, Li 2 CO 3 , LiAlO 2 , Li 2 O - Al 2 O 3 - SiO 2 - P 2 O 5 - TiO 2 - GeO 2 , Li 3+x La 3 M 2 O 12 (M is Te, Nb, or Zr, and x is an integer from 1 to 10), and one or more selected from among them. The solid electrolyte is produced by a sintering method or the like. For example, the oxide-based solid electrolyte is Li 7 La 3 Zr 2 O 12 (LLZO) and Li 3+x La 3 Zr 2-a M a O 12 (M doped LLZO) (M is Ga, W, Nb, Ta, or Al, x is an integer from 1 to 10, 0 < a < 2) is a garnet-type solid electrolyte selected from among them.
[0150] The sulfide-based solid electrolyte also includes, for example, lithium sulfide, silicon sulfide, phosphorus sulfide, boron sulfide, or a combination thereof. The sulfide-based solid electrolyte particles are Li 2 S, P2 S 5 , SiS 2 , GeS 2 , B 2 S 3 or a combination thereof. The sulfide-based solid electrolyte particles include Li 2 S or P 2 S 5 It is also known that the sulfide-based solid electrolyte particles have a higher lithium ion conductivity than other inorganic compounds. For example, the sulfide-based solid electrolyte has a Li 2 S and P 2 S 5 The sulfide solid electrolyte material constituting the sulfide-based solid electrolyte is Li 2 SP 2 S 5 If it contains Li 2 S and P 2 S 5 The molar ratio of Li to Li is, for example, in the range of about 50:50 to about 90:10. 3 PO 4 , halogens, halogen compounds, Li 2+2x Zinc 1-x GeO 4 (LISICON)(0≦x<1), Li 3+y PO 4-x N x (LIPON)(0 <x<4、0<y<3)、Li 3.25 Ge 0.25 P 0.75 S 4 (ThioLISICON), Li 2 O-Al 2 O 3 -TiO 2 -P 2 O 5 (LATP), etc., 2 SP 2 S 5 , SiS 2 , GeS 2 , B 2 S 3 or a combination thereof may be used as the sulfide solid electrolyte. A non-limiting example of the sulfide solid electrolyte material is Li 2S-P 2 S 5 ;Li 2 S-P 2 S 5 -LiX (X is a halogen element); Li 2 S-P 2 S 5 -Li 2 O; Li 2 S-P 2 S 5 -Li 2 O-LiI; Li 2 S-SiS 2 ;Li 2 S-SiS 2 -LiI; Li 2 S-SiS 2 -LiBr; Li 2 S-SiS 2 -LiCl; Li 2 S-SiS 2 -B 2 S 3 -LiI; Li 2 S-SiS 2 -P 2 S 5 -LiI; Li 2 S-B 2 S 3 ;Li 2 S-P 2 S 5 -Z m S n (0 < m < 10, 0 < n < 10, Z = Ge, Zn or Ga); Li 2 S-GeS 2 ;Li 2 S-SiS 2 -Li 3 PO 4 ; and Li 2 S-SiS 2 -Li p MO q (0 < p < 10, 0 < q < 10, and M is P, Si, Ge, B, Al, Ga or In) is included. And, the sulfide-based solid electrolyte material is a raw material starting material of the sulfide-based solid electrolyte substance (for example, Li 2 S, P 2 S 5The sulfide-based solid electrolyte can be manufactured by treating the sulfide-based solid electrolyte with a melt quenching method, a mechanical milling method, etc., and a sintering process can be performed after the treatment. The sulfide-based solid electrolyte can be amorphous, crystalline, or a mixture thereof.
[0151] The polymer solid electrolyte may, for example, include a mixture of a lithium salt and a polymer, or may include a polymer having an ion-conducting functional group. The polymer solid electrolyte may, for example, be a polymer electrolyte that is in a solid state at 25° C. and 1 atm. The polymer solid electrolyte may, for example, be one that does not include a liquid.The polymer solid electrolyte includes a polymer, and the polymer is, for example, polyethylene oxide (PEO), polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene (PVDF-HFP), poly(styrene-b-ethylene oxide) block copolymer (PS-PEO), poly(styrene-butadiene), poly(styrene-isoprene-styrene), poly(styrene-b-divinylbenzene) block copolymer, poly(styrene-ethylene oxide-styrene) block copolymer, polystyrene sulfonate (PSS), polyvinyl fluoride (PVF), polyvinyl fluoride), poly(methylmethacrylate) (PMMA), polyethylene glycol (PEG), polyacrylonitrile (PAN), polytetrafluoroethylene (PTFE), polyethylenedioxythiophene (PEDOT), polypyrrole (PPY), polyacrylonitrile (PAN), polyaniline, polyacetylene, Nafion, Aquivion, Flemion, Gore, Aciplex, Morgane ADP, sulfonated poly(ether ether ketone) (SPEEK), sulfonated poly(arylene ether ketone ketone) (SPAEKKS), sulfonated poly(aryl ether ketone) (SPAEK) ketone), poly[bis(benzimidazobenzisoquinolinones)] (SPBIBI), poly(styrene sulfonate) (PSS), and lithium 9,10-diphenylanthracene-2-sulfonate (DPASLi). +The lithium salt may be, but is not limited to, any of those used as a polymer electrolyte in the art. The lithium salt may be any of those used as a lithium salt in the art. The lithium salt may be, for example, LiPF 6 , LiBF 4 , LiSbF 6 , LiAsF 6 , LiClO 4 , LiCF 3 SO 3 , Li(CF 3 SO 2 ) 2 N, LiC 4 F 9 SO 3 , LiAlO 2 , LiAlCl 4 , LiN(C x F 2x+1 SO 2 )(C y F 2y+1 SO 2 ) (x and y are each 1 to 20), LiCl, LiI, or a mixture thereof. The polymer contained in the polymer solid electrolyte is, for example, a compound containing 10 or more, 20 or more, 50 or more, or 100 or more repeating units. The weight average molecular weight of the polymer contained in the polymer solid electrolyte is, for example, 1,000 Dalton or more, 10,000 Dalton or more, 100,000 Dalton or more, or 1,000,000 Dalton or more.
[0152] The gel electrolyte is, for example, a polymer gel electrolyte. The gel electrolyte can have a gel state without including a polymer, for example.
[0153] The polymer gel electrolyte may, for example, include a liquid electrolyte and a polymer, or may include an organic solvent and a polymer having an ion-conducting functional group. The polymer gel electrolyte may, for example, be a polymer electrolyte that is in a gel state at 25° C. and 1 atm. The polymer gel electrolyte may, for example, be in a gel state without including liquid. The liquid electrolyte used in the polymer gel electrolyte may, for example, be a mixture of an ionic liquid, a lithium salt, and an organic solvent; a mixture of a lithium salt and an organic solvent; a mixture of an ionic liquid and an organic solvent; or a mixture of a lithium salt, an ionic liquid, and an organic solvent. The polymer used in the polymer gel electrolyte may be selected from the polymers used in the solid polymer electrolyte. The organic solvent may be selected from the organic solvents used in the liquid electrolyte. The lithium salt may be selected from the lithium salts used in the solid polymer electrolyte. The ionic liquid refers to a salt that has a melting point below room temperature, is composed of only ions, and is in a liquid state at room temperature, or a room temperature molten salt. The ionic liquid may, for example, comprise: a) one or more cations selected from ammonium, pyrrolidinium, pyridinium, pyrimidinium, imidazolium, piperidinium, pyrazolium, oxazolium, pyridazinium, phosphonium, sulfonium, triazolium, and mixtures thereof; and b) BF 4 - , P.F. 6 - , AsF 6 - , SbF 6 - , AlCl 4 - , HSO 4 - , ClO 4 - , C.H. 3 SO 3 - , C.F. 3 CO 2 - , Cl - , Br - , I - , B.F. 4 - , S.O. 4 - , C.F.3 SO 3 - , (FSO 2 ) 2 N - , (C 2 F 5 SO 2 ) 2 N - , (C 2 F 5 SO 2 )(CF 3 SO 2 )N - and (CF 3 SO 2 ) 2 N - and one or more selected from compounds containing one or more anions selected from the group consisting of. The polymer solid electrolyte can be impregnated with a liquid electrolyte in a secondary battery to form the polymer gel electrolyte. The polymer gel electrolyte further includes inorganic particles. The polymer contained in the polymer gel electrolyte is, for example, a compound containing 10 or more, 20 or more, 50 or more, or 100 or more repeating units. The weight average molecular weight of the polymer contained in the polymer gel electrolyte is, for example, 500 Dalton or more, 1,000 Dalton or more, 10,000 Dalton or more, 100,000 Dalton or more, or 1,000,000 Dalton or more.
[0154] 6, a lithium battery 1 according to an embodiment includes a positive electrode 3, a negative electrode 2, and a separator 4. The positive electrode 3, the negative electrode 2, and the separator 4 are wound or folded to form a battery structure 7. The formed battery structure 7 is housed in a battery case 5. An organic electrolyte is injected into the battery case 5, and the battery case 5 is sealed with a cap assembly 6 to complete the lithium battery 1. The battery case 5 is cylindrical, but is not necessarily limited to such a shape, and may be, for example, a square type, a thin film type, etc.
[0155] Referring to FIG. 7, a lithium battery 1 according to an embodiment includes a positive electrode 3, a negative electrode 2, and a separator 4. The separator 4 is disposed between the positive electrode 3 and the negative electrode 2, and the positive electrode 3, the negative electrode 2, and the separator 4 are wound or folded to form a battery structure 7. The formed battery structure 7 is housed in a battery case 5. The battery structure 7 also includes electrode tabs 8 that serve as electrical paths for directing a current formed in the battery structure 7 to the outside. An organic electrolyte is injected into the battery case 5 and sealed, completing the lithium battery 1. The battery case 5 is rectangular, but is not necessarily limited to such a shape, and may be, for example, cylindrical or thin-film type.
[0156] Referring to FIG. 8, a lithium battery 1 according to an embodiment includes a positive electrode 3, a negative electrode 2, and a separator 4. The separator 4 is disposed between the positive electrode 3 and the negative electrode 2 to form a battery structure. The battery structure 7 is stacked in a bi-cell structure and then housed in a battery case 5. The battery structure 7 also includes electrode tabs 8 that act as electrical paths for directing current generated in the battery structure 7 to the outside. An organic electrolyte is injected into the battery case 5 and sealed to complete the lithium battery 1. The battery case 5 is rectangular, but is not necessarily limited to such a shape and may be, for example, cylindrical or thin-film type.
[0157] The pouch-type lithium battery corresponds to the lithium batteries of FIGS. 6 to 8, in which a pouch is used as a battery case. The pouch-type lithium battery includes one or more battery structures. A separator is disposed between a positive electrode and a negative electrode to form a battery structure. The battery structures are stacked in a bi-cell structure, impregnated with an organic electrolyte, and then housed in the pouch and sealed to complete the pouch-type lithium battery. For example, although not shown in the drawings, the above-mentioned positive electrode, negative electrode, and separator are simply stacked and housed in a pouch in the form of an electrode assembly, or wound into an electrode assembly in the form of a jelly roll, or folded and then housed in a pouch. Subsequently, an organic electrolyte is injected into the pouch and sealed to complete the lithium battery.
[0158] Lithium batteries have excellent life characteristics and high rate characteristics, and are therefore used, for example, in electric vehicles (EVs), hybrid vehicles such as plug-in hybrid electric vehicles (PHEVs), and fields requiring large amounts of power storage, such as electric bicycles and power tools.
[0159] A plurality of lithium batteries are stacked to form a battery module, and the plurality of battery modules form a battery pack. Such a battery pack can be used in all devices that require high capacity and high power output, such as notebook computers, smartphones, and electric vehicles. The battery module includes, for example, a plurality of batteries and a frame for positioning the batteries. The battery pack includes, for example, a plurality of battery modules and a bus bar for connecting the batteries. The battery module and / or the battery pack further includes a cooling device. The plurality of battery packs are regulated by a battery management system. The battery management system includes the battery pack and a battery control device connected to the battery pack.
[0160] According to yet another embodiment, a method for preparing a composite positive electrode active material includes providing a first lithium transition metal oxide, providing a second lithium transition metal oxide, providing a composite, providing a second carbon-based material, mechanically milling the first lithium transition metal oxide, the composite, and the second carbon-based material to obtain a first core / shell structure, mechanically milling the second lithium transition metal oxide, the composite, and the second carbon-based material to obtain a second core / shell structure, and mixing the first core / shell structure and the second core / shell structure to obtain a composite positive electrode active material.
[0161] The complex has the formula M a O bOne or more first metal oxides represented by (0 < a ≤ 3, 0 < b < 4, and if a is 1, 2, or 3, then b is not an integer), and a first carbon-based material, wherein the first metal oxide is disposed within a first carbon-based material matrix, wherein M is one or more metals selected from Groups 2 to 13 of the Periodic Table of the Elements, Groups 15 and 16 of the Periodic Table of the Elements, and the second carbon-based material includes fibrous carbon having an aspect ratio of 10 or more. And the first lithium transition metal oxide and the second lithium transition metal oxide have different particle sizes from each other.
[0162] The first lithium transition metal oxide and the second lithium transition metal oxide are, for example, compounds represented by the aforementioned Chemical Formulas 1 to 6.
[0163] A composite is provided. The step of providing the composite includes, for example, supplying a reaction gas composed of a carbon source gas to a structure containing a second metal oxide and performing heat treatment to provide the composite. The step of providing the composite includes, for example, M a O c Supplying a reaction gas composed of a carbon source gas to one or more second metal oxides represented by (0 < a ≤ 3, 0 < c ≤ 4, and when a is 1, 2, or 3, b is an integer) and performing heat treatment to produce a composite, wherein M is one or more metals selected from Groups 2 to 13 of the Periodic Table of the Elements, Groups 15 and 16 of the Periodic Table of the Elements. The second metal oxide can undergo a gradual heat treatment process up to a heat treatment temperature (T). The time for heating to the heat treatment temperature (T) is also about 10 minutes to about 4 hours. The heat treatment temperature (T) is also about 700 °C to about 1100 °C. During the reaction time, heat treatment can be performed at the heat treatment temperature (T). The reaction time is, for example, also 4 hours to 8 hours. The heat-treated product can be cooled to room temperature to produce the composite. The time during the process of cooling from the heat treatment temperature (T) to room temperature is, for example, also about 1 hour to about 5 hours.
[0164] The carbon source gas is a gas consisting of a compound represented by the following chemical formula 9, or a mixed gas consisting of a compound represented by the following chemical formula 9, a compound represented by the following chemical formula 10, and an oxygen-containing gas represented by the following chemical formula 11.
[0165] [Chemical formula 9] C n H (2n+2-a) [OH] a
[0166] In the above formula 9, n is 1 to 20, and a is 0 or 1;
[0167] [Chemical formula 10] C n H 2n
[0168] In the above formula 10, n is 2 to 6;
[0169] [Chemical formula 11] C x H y O z
[0170] In the above formula 11, x is 0 or an integer from 1 to 20; y is 0 or an integer from 1 to 20; and z is 1 or 2.
[0171] The compound represented by Chemical Formula 9 and the compound represented by Chemical Formula 10 are one or more selected from the group consisting of methane, ethylene, propylene, methanol, ethanol, and propanol. The oxygen-containing gas represented by Chemical Formula 11 is, for example, carbon dioxide (CO 2 ) and carbon monoxide (CO), water vapor (H 2 O), or a mixture thereof.
[0172] M a O c(0 < a ≤ 3, 0 < c ≤ 4, and if a is 1, 2, or 3, then c is an integer) After the step of supplying a reaction gas composed of a carbon source gas to the second metal oxide represented by and performing heat treatment, a cooling step using one or more inert gases selected from the group consisting of nitrogen, helium, and argon is further performed. The cooling step refers to the step of adjusting to room temperature (20 - 25°C). The carbon source gas also contains one or more inert gases selected from the group consisting of nitrogen, helium, and argon.
[0173] In the method for producing a composite, the process of growing a carbon-based material, for example, graphene, by a gas-phase reaction can be carried out under various conditions.
[0174] According to the first condition, for example, M a O c First, methane is supplied to a reactor in which a second metal oxide represented by (0 < a ≤ 3, 0 < c ≤ 4, and if a is 1, 2, or 3, then c is an integer) is arranged, and the temperature is raised to the heat treatment temperature (T). The temperature rising time to the heat treatment temperature (T) is 10 minutes to 4 hours, and the heat treatment temperature (T) is in the range of 700°C to 1,100°C. At the heat treatment temperature (T), heat treatment is carried out during the reaction time. The reaction time is, for example, 4 hours to 8 hours. The heat-treated product is cooled to room temperature to produce a composite. The time taken during the process of cooling from the heat treatment temperature (T) to room temperature is, for example, 1 hour to 5 hours.
[0175] According to the second condition, for example, M a O cFirst, hydrogen is supplied to a reactor in which a second metal oxide represented by (0 < a ≤ 3, 0 < c ≤ 4, and if a is 1, 2, or 3, c is an integer) is disposed, and the temperature is raised to a heat treatment temperature (T). The temperature rising time to the heat treatment temperature (T) is 10 minutes to 4 hours, and the heat treatment temperature (T) is in the range of 700°C to 1,100°C. After heat treatment for a certain reaction time at the heat treatment temperature (T), methane gas is supplied, and heat treatment is carried out for the remaining reaction time. The reaction time is, for example, 4 hours to 8 hours. The heat-treated product is cooled to room temperature to produce a composite. Nitrogen is supplied during the cooling process. The time taken for cooling from the heat treatment temperature (T) to room temperature is, for example, 1 hour to 5 hours.
[0176] According to the third condition, for example, M a O c First, hydrogen is supplied to a reactor in which a second metal oxide represented by (0 < a ≤ 3, 0 < c ≤ 4, and if a is 1, 2, or 3, c is an integer) is disposed, and the temperature is raised to a heat treatment temperature (T). The temperature rising time to the heat treatment temperature (T) is 10 minutes to 4 hours, and the heat treatment temperature (T) is in the range of 700°C to 1,100°C. After heat treatment for a certain reaction time at the heat treatment temperature (T), a mixed gas of methane and hydrogen is supplied, and heat treatment is carried out for the remaining reaction time. The reaction time is, for example, 4 hours to 8 hours. The heat-treated product is cooled to room temperature to produce a composite. Nitrogen is supplied during the cooling process. The time taken for cooling from the heat treatment temperature (T) to room temperature is, for example, 1 hour to 5 hours.
[0177] In the process of producing the composite, when the carbon source gas contains water vapor, a composite having very excellent conductivity can be obtained. The content of water vapor in the gas mixture is not limited, and is, for example, 0.01% by volume to 10% by volume based on 100% by volume of the entire carbon source gas. The carbon source gas is, for example, methane, a mixed gas containing methane and an inert gas, or a mixed gas containing methane and an oxygen-containing gas.
[0178] The carbon source gas can be, for example, methane; a mixture of methane and carbon dioxide; or a mixture of methane, carbon dioxide, and water vapor. In the mixture of methane and carbon dioxide, the molar ratio of methane to carbon dioxide is about 1:0.20 to 1:0.50, about 1:0.25 to 1:0.45, or about 1:0.30 to 1:0.40. In the mixture of methane, carbon dioxide, and water vapor, the molar ratio of methane to carbon dioxide to water vapor is about 1:0.20 to 0.50:0.01 to 1.45, about 1:0.25 to 0.45:0.10 to 1.35, or about 1:0.30 to 0.40:0.50 to 1.0.
[0179] The carbon source gas is, for example, carbon monoxide or carbon dioxide. The carbon source gas is, for example, a mixture of methane and nitrogen. In the mixture of methane and nitrogen, the molar ratio of methane to nitrogen is about 1:0.20 to 1:0.50, about 1:0.25 to 1:0.45, or about 1:0.30 to 1:0.40. The carbon source gas does not include an inert gas such as nitrogen.
[0180] The heat treatment pressure can be selected taking into consideration the heat treatment temperature, the composition of the gas mixture, and the amount of carbon coating desired. The heat treatment pressure can be controlled by adjusting the amount of the gas mixture flowing in and the amount of the gas mixture flowing out. The heat treatment pressure is, for example, 0.5 atm or more, 1 atm or more, 2 atm or more, 3 atm or more, 4 atm or more, or 5 atm or more. The heat treatment pressure is, for example, 0.5 atm to 10 atm, 1 atm to 10 atm, 2 atm to 10 atm, 3 atm to 10 atm, 4 atm to 10 atm, or 5 atm to 10 atm.
[0181] The heat treatment time is not particularly limited and can be appropriately adjusted according to the heat treatment temperature, the pressure during heat treatment, the composition of the gas mixture, and the amount of the desired carbon coating. For example, the reaction time at the heat treatment temperature is, for example, from 10 minutes to 100 hours, from 30 minutes to 90 hours, or from 50 minutes to 40 hours. For example, as the heat treatment time increases, the amount of carbon deposited, for example, the amount of graphene (carbon), increases, whereby the electrical properties of the composite can be improved. However, such a tendency is not necessarily directly proportional to the time. For example, after a predetermined time has elapsed, no further carbon deposition, for example, graphene deposition, may occur, or the deposition rate may decrease.
[0182] Through the gas-phase reaction of the aforementioned carbon source gas, even at a relatively low temperature, M a O c (where 0 < a ≤ 3, 0 < c ≤ 4, and if a is 1, 2, or 3, then c is an integer), and the reduced product thereof, M a O b A composite is obtained by providing a uniform coating of a first carbon-based material, for example, a graphene coating, on one or more selected from the first metal oxides represented by (0 < a ≤ 3, 0 < b < 4, where a is 1, 2, or 3 and b is not an integer).
[0183] The composite has, for example, a matrix of a first carbon-based material having one or more structures selected from a spherical structure, a helical structure in which a plurality of spherical structures are connected, a cluster structure in which a plurality of spherical structures are aggregated, and a sponge structure, for example, a graphene matrix, and M disposed within the graphene matrix a O b (where 0 < a ≤ 3, 0 < b < 4, where a is 1, 2, or 3 and b is not an integer), and a first metal oxide, and M a O c (where 0 < a ≤ 3, 0 < c ≤ 4, and if a is 1, 2, or 3, then c is an integer), and contains one or more selected from the second metal oxides represented by.
[0184] The lithium transition metal oxide, the composite, and the second carbon-based material are then mechanically milled.
[0185] The milling method in the mechanical milling step is not particularly limited, and any method that can be used in the art for mechanically contacting a lithium transition metal oxide, a composite, and a second carbon-based material is acceptable.
[0186] For example, a Nobilta mixer can be used during the milling. The rotation speed of the mixer during the milling is, for example, 1,000 rpm to 5,000 rpm, or 2,000 rpm to 4,000 rpm. If the milling speed is too slow, the shear force applied to the lithium transition metal oxide, the composite, and the second carbon-based material is weak, making it difficult for the lithium transition metal oxide and the composite to form a chemical bond. If the milling speed is too fast, the composite is formed in an excessively short time, making it difficult for the composite and the second carbon-based material to be uniformly coated on the lithium transition metal oxide and to form a uniform and continuous shell. The milling time is, for example, 5 minutes to 100 minutes, 5 minutes to 60 minutes, or 5 minutes to 30 minutes. If the milling time is too short, it is difficult for the composite and the second carbon-based material to be uniformly coated on the lithium transition metal oxide and to form a uniform shell. If the milling time is too long, production efficiency may be reduced. The content of the complex may be 5 wt% or less, 4 wt% or less, 3 wt% or less, 2 wt% or less, or 1 wt% or less of the total weight of the lithium transition metal oxide and the complex. The content of the complex may be, for example, 0.01 to 5 wt%, 0.01 to 4 wt%, 0.01 to 3 wt%, 0.1 to 2 wt%, or 0.1 to 1 wt% of the total weight of the first lithium transition metal oxide and the complex. For example, the content of the complex may be 0.01 to 5 parts by weight, 0.01 to 4 parts by weight, 0.01 to 3 parts by weight, 0.1 to 3 parts by weight, 0.1 to 2 parts by weight, or 0.1 to 1 part by weight per 100 parts by weight of the mixture of the first lithium transition metal oxide and the complex. The average particle size (D50) of the composite used in mechanical milling of the first lithium transition metal oxide with the composite is, for example, 50 nm to 200 nm, 100 nm to 300 nm, or 200 nm to 500 nm.
[0187] The present invention will be described in more detail with reference to the following examples and comparative examples. However, the examples are intended to illustrate the present invention and are not intended to limit the scope of the present invention.
[0188] (Manufacture of Composite) Production example 1: Al 2 O 3 @Gr complex Al 2 O 3 After placing AlO particles (average particle size: about 20 nm) in the reactor, in the reactor, CH 4 was supplied at about 300 sccm and 1 atm for about 30 minutes, and the internal temperature of the reactor was raised to 1,000 °C.
[0189] Subsequently, it was maintained at the above temperature for 7 hours and heat-treated. Subsequently, the internal temperature of the reactor was adjusted to room temperature (20 - 25 °C), and a composite in which Al 2 O 3 particles and its reduction product Al 2 O z (0 < z < 3) particles were embedded in graphene was obtained.
[0190] The content of aluminum oxide (Al 2 O 3 particles and its reduction product, Al 2 O z (0 < z < 3) particles) in the composite was about 75 wt%.
[0191] Production example 2: Al 2 O 3 @Gr complex Al 2 O 3 Instead of AlO particles (average particle size: about 20 nm), a composite was manufactured in the same manner as in Production Example 1, except that Al 2 O 3 particles (average particle size: about 200 nm) were used.
[0192] Manufacturing Example 3: Polycrystalline large particle size positive electrode active material LiNi with an average particle size of 10 μm 0.75 Mn 0.22 Al 0.03 O 2 Manufacturing NiSO 4 , aluminum sulfate (CoSO 4 7H 2 O) and MnSO 4 Each was made into a 1.5M aqueous solution, and Ni 0.75 Mn 0.22 Al 0.03 (OH) 2 The content of the aqueous solution was adjusted so that a compound of the composition was synthesized, and the solution was introduced into a coprecipitation reactor to synthesize a coprecipitate. At this time, an aqueous ammonia solution was introduced to form a complex compound, and the concentration of the aqueous ammonia solution and the amount of sodium hydroxide introduced were adjusted to control the pH so that the coprecipitate would grow uniformly. When the coprecipitate had an average particle size of 10 μm, the reaction was stopped and the coprecipitate was separated. Thereafter, the solution was heat-treated (dried) in a vacuum oven at 120° C. for 10 hours to obtain Ni 0.75 Mn 0.22 Al 0.03 (OH) 2 A transition metal hydroxide precursor having the following composition was prepared.
[0193] The obtained transition metal hydroxide precursor was mixed with a lithium compound (lithium hydroxide:lithium carbonate mixed in a molar ratio of 1.0:0.5) so that the Li / (Ni+Al+Mn) molar ratio was 1.01, and the mixture was heat-treated at a temperature of 850° C. for 20 hours in an oxidizing gas atmosphere containing 80 to 100% by volume of oxygen to produce a positive electrode active material.
[0194] The produced positive electrode active material has a polycrystalline structure with an average grain size of 10 μm, and the composition of the positive electrode active material is LiNi 0.75 Mn 0.22 Al 0.03 O 2 The above measured values were measured based on the cross section of the secondary particle.
[0195] Manufacturing Example 4: Polycrystalline small particle size positive electrode active material LiNi with an average particle size of 3.5 μm 0.75 Mn 0.22 Al 0.03 O 2 Manufacturing A positive electrode active material was prepared in the same manner as in Preparation Example 3, except that when the average particle size of the coprecipitate was 3.5 μm during the preparation of the transition metal hydroxide precursor, the reaction was stopped and the coprecipitate was separated.
[0196] It was confirmed that the positive electrode active materials of Preparation Examples 3 and 4 were polycrystalline by observing the particle shape and cross section of the particles using a scanning electron microscope.
[0197] Production Example 5: Production of large single crystal NMX with an average particle size of 10 μm Nickel sulfate (NiSO 4 6H 2 O), aluminum sulfate (CoSO 4 7H 2 O) and manganese sulfate (MnSO 4 H 2 A mixture solution was prepared by dissolving ammonium hydroxide (NH O) in distilled water, which is a solvent. 4 A dilution solution of ammonium hydroxide (NH3) and sodium hydroxide (NaOH) as a precipitant were prepared. Then, the metal raw material mixed solution, ammonia water, and sodium hydroxide were each put into the reactor. Next, the reaction was allowed to proceed for about 20 hours while stirring. After that, the slurry solution in the reactor was filtered, washed with high-purity distilled water, and then dried for 24 hours to obtain Ni with an average particle size of 10 μm. 0.75 Mn 0.22 Al 0.03 (OH) 2 This powder is mixed with LiOH so that Li / (Ni+Co+Mn)=1.05 is satisfied, and the mixture is placed in a sintering furnace and subjected to a second heat treatment at 910°C for 8 hours in an oxygen atmosphere to obtain a positive electrode LiNi 0.75 Mn 0.22 Al 0.03 O 2 The positive electrode active material is then ground for about 30 minutes to separate / disperse it into a large number of positive electrode active materials having a single crystal structure. The average particle size of the obtained positive electrode active material having a single crystal structure is about 10.0 μm.
[0198] Production Example 6: Production of single crystal small particle size NMX with an average particle size of 3.5 μm Ni with an average particle size of 10 μm 0.75 Mn 0.22 Al0.03 (OH) 2 Instead of the powder, Ni with an average particle size of 3.5 μm 0.75 Mn 0.22 Al 0.03 (OH) 2 The positive electrode active material was produced in the same manner as in Production Example 5, except that the reaction process was controlled so that a powder was obtained.
[0199] Comparative production example 1: SiO 2 @Gr complex SiO 2 After positioning particles (average particle size: about 15 nm) in the reactor, in the reactor, CH 4 was supplied at about 300 sccm and 1 atm for about 30 minutes, and the internal temperature of the reactor was raised to 1,000 °C.
[0200] Subsequently, it was maintained at the above temperature for 7 hours for heat treatment. Subsequently, the internal temperature of the reactor was adjusted to room temperature (20 to 25 °C), and a composite in which SiO 2 particles and SiO y (0 < y < 2) particles which are reduction products thereof are embedded in graphene was obtained.
[0201] (Production of composite positive electrode active material) Example 1: Polycrystalline NMX large grain size + polycrystalline NMX small grain size + GB (Al 2 O 3 @Gr composite) 0.2wt% + CNT 0.02wt% coating composite positive electrode active material As starting materials, polycrystalline large-particle LiNi with an average particle size of 10 μm obtained in Production Example 3 0.75 Mn 0.22 Al 0.03 O 2 (hereinafter referred to as large-particle NMX), the composite prepared in Production Example 1, and CNT were milled for about 5 to 30 minutes at a rotational speed of about 1,000 to 2,000 rpm using a Nobilta Mixer (Hosokawa, Japan) to obtain a first core / shell structure. The large-particle NMX, the composite, and the carbon nanotube (CNT) were mixed at a weight ratio of 100:0.2:0.02.
[0202] Polycrystalline large particle size NMX is a secondary particle having a structure in which multiple plate primary particles are arranged in a radial shape. Large particle size NMX has a structure in which the long axes of multiple plate primary particles contained therein are arranged in a radial shape. In the polycrystalline large particle size NMX, the average length of multiple plate primary particles means the average length of the average long axis length and the average short axis length in the longitudinal direction of the plate particle, and the average length of the plate primary particles is about 320 nm, and the average thickness of the plate particles is about 140 nm.
[0203] Polycrystalline small-grain LiNi having an average grain size of 3.5 μm obtained by Production Example 4 0.75 Mn 0.22 Al 0.03 O 2 (hereinafter referred to as small particle size NMX), the composite and CNT prepared in Production Example 1 were milled for about 5 to 30 minutes at a rotation speed of about 1,000 to 2,000 rpm using a Nobilta Mixer (Hosokawa, Japan) to obtain a second core / shell structure. The small particle size NMX, the composite and the carbon nanotubes (CNT) were mixed in a weight ratio of 100:0.2:0.02.
[0204] Polycrystalline small particle size NMX is a secondary particle having a structure in which a plurality of plate primary particles are arranged in a radial shape. The long axes of the plurality of plate primary particles contained in the small particle size NMX are arranged in a radial shape. In the polycrystalline small particle size NMX, the average length of the plurality of plate primary particles means the average length of the average long axis length and the average short axis length in the longitudinal direction of the plate particle, and the average length of the plate primary particles is about 320 nm, and the average thickness of the plate particles is about 140 nm.
[0205] The first core / shell structure and the second core / shell structure were mixed in a weight ratio of 92:8 to prepare a composite positive electrode active material.
[0206] In Example 1, the polycrystalline large particle size NMX and polycrystalline small particle size NMX used as starting materials were as shown in Figure 3A before being coated with the composite and carbon nanotubes (CNTs), and after being coated, the composite positive electrode active material had a structure as shown in Figure 2. Furthermore, the particle size distribution was measured using a particle size analyzer (PSA), and it was confirmed that the composite had a bimodal particle size distribution.
[0207] Example 2: Polycrystalline large grain NMX + polycrystalline small grain NMX + GB (Al 2 O 3 @Gr) 0.2wt% + CNT 0.03wt% A composite positive electrode active material was prepared in the same manner as in Example 1, except that the mixing ratio of NMX, the composite, and the carbon nanotubes was changed from 100:0.2:0.02 to 100:0.2:0.03.
[0208] As can be seen from Fig. 2, it was confirmed that carbon nanotubes were disposed on the surface of the composite positive electrode active material. The carbon nanotubes included a carbon nanotube primary structure and a carbon nanotube secondary structure formed by agglomerating a plurality of carbon nanotube units.
[0209] The carbon nanotube primary structure was composed of one carbon nanotube unit, the length of which was 200 nm to 300 nm, and the diameter of the carbon nanotube was about 10 nm.
[0210] The carbon nanotube secondary structure was formed by agglomerating a plurality of carbon nanotube units, and had a length of 500 nm or more and a diameter of about 40 nm.
[0211] Example 3: Large polycrystalline grain size + small polycrystalline grain size + GB 0.2wt% + CNT 0.05wt% A composite positive electrode active material was prepared in the same manner as in Example 1, except that the mixing ratio of NMX, the composite, and the carbon nanotubes was changed from 100:0.2:0.02 to 100:0.2:0.05.
[0212] Example 4: Large polycrystalline grain size + small polycrystalline grain size + GB 0.2wt% + CNT 0.1wt% A composite positive electrode active material was prepared in the same manner as in Example 1, except that the mixing ratio of NMX, the composite, and the carbon nanotubes was changed from 100:0.2:0.02 to 100:0.2:0.1.
[0213] Reference example 1: Polycrystalline large grain size + polycrystalline small grain size + GB 0.2wt% Polycrystalline large-grain LiNi with an average grain size of 10 μm 0.75 Mn 0.22 Al 0.03 O 2 (hereinafter referred to as large particle size NMX) and the composite prepared in Production Example 1 were milled for about 5 to 30 minutes at a rotation speed of about 1,000 to 2,000 rpm using a Nobilta Mixer (Hosokawa, Japan) to obtain a first core / shell structure. NMX and the composite were mixed in a ratio of 99.8:0.2. Large particle size NMX is a secondary particle having a structure in which multiple plate primary particles are arranged in a radial shape. Large particle size NMX has a structure in which the major axes of multiple plate primary particles contained therein are arranged in a radial shape.
[0214] Polycrystalline small-grain LiNi with an average grain size of 3.5 μm 0.75 Mn 0.22 Al 0.03 O 2 (hereinafter referred to as small particle size NMX) and the composite prepared in Production Example 1 were milled for about 5 to 30 minutes at a rotation speed of about 1,000 to 2,000 rpm using a Nobilta Mixer (Hosokawa, Japan) to obtain a second core / shell structure. The small particle size NMX and the composite were mixed in a ratio of 99.8:0.2. The small particle size NMX contains multiple plate primary particles whose long axes are arranged in a radial pattern.
[0215] The first core / shell structure and the second core / shell structure were mixed in a weight ratio of 92:8 to prepare a composite positive electrode active material.
[0216] The particle size distribution was measured using a particle size analyzer (PSA) and was found to have a bimodal particle size distribution.
[0217] Comparative Example 1: Large single crystal grain size NMX + Small single crystal grain size NMX + Uncoated A composite positive electrode active material was prepared in the same manner as in Example 1, except that the first core / shell structure was replaced with the large single-crystal particle size NMX obtained in Preparation Example 5, and the second core / shell structure was replaced with the small single-crystal particle size NMX obtained in Preparation Example 6.
[0218] The large particle size NMX and the small particle size NMX were mixed in a weight ratio of 92:8 to produce a composite positive electrode active material.
[0219] The particle size distribution was measured using a particle size analyzer (PSA) and was found to have a bimodal particle size distribution.
[0220] Comparative Example 2 A composite positive electrode active material was prepared in the same manner as in Example 1, except that the composite prepared in Comparative Preparation Example 1 was used instead of the composite prepared in Preparation Example 1.
[0221] (Lithium battery (half cell) manufacturing (dry type)) Example 5 (Production of positive electrodes) The composite cathode active material prepared in Example 1 as a dry cathode active material, a carbon conductive material (Denka Black) as a dry conductive material, and polytetrafluoroethylene (PTFE) as a dry binder were charged into a blade mixer in a weight ratio of 92:4:4, and then primary dry-mixed at 25° C. and 1,000 rpm for 10 minutes to prepare a first mixture in which the dry cathode active material, the dry conductive material, and the dry binder were uniformly mixed.
[0222] Next, in order to promote fiberization of the binder, the first mixture was further mixed at 25° C. and 5,000 rpm for 20 minutes to prepare a second mixture. No separate solvent was used when preparing the first and second mixtures.
[0223] The prepared second mixture was put into an extruder and extruded to prepare a sheet-shaped positive electrode active material layer self-standing film. The pressure during extrusion was 50 MPa.
[0224] A carbon layer was disposed as an interlayer on one surface of a 12 μm-thick aluminum thin film, and the interlayer was disposed on one surface of a second positive electrode current collector to prepare a first laminate.
[0225] The intermediate layer was prepared by coating a composition containing a carbon conductive material (Danka Black) and polyvinylidene fluoride (PVDF) on an aluminum thin film and then drying it. The thickness of the intermediate layer disposed on one side of the aluminum thin film was about 1 μm.
[0226] A positive electrode active material layer free-standing film was disposed on the intermediate layer of the prepared first laminate and rolled to produce a positive electrode.
[0227] (Coin cell manufacturing) Using the positive electrode prepared above, lithium metal was used as the counter electrode, and a polytetrafluoroethylene (PTFE) separator was used to prepare a 1.5M LiPF 6 A solution of ethylene carbonate (EC) + ethyl methyl carbonate (EMC) + dimethyl carbonate (DMC) (volume ratio 2:1:7) was used as the electrolyte to fabricate coin cells.
[0228] Examples 6 to 8 A coin cell was manufactured in the same manner as in Example 5, except that the composite positive electrode active material of Example 1 was replaced with the composite positive electrode active material of Examples 2 to 4.
[0229] Reference example 2 A coin cell was manufactured in the same manner as in Example 5, except that the composite positive electrode active material of Reference Example 1 was used instead of the composite positive electrode active material of Example 1 when manufacturing the positive electrode.
[0230] Comparative Example 3 A coin cell was manufactured in the same manner as in Reference Example 2, except that the composite positive electrode active material of Comparative Example 1 was used instead of the composite positive electrode active material of Example 1 when manufacturing the positive electrode.
[0231] Comparative Example 4 A coin cell was manufactured in the same manner as in Reference Example 2, except that the composite positive electrode active material of Comparative Example 2 was used instead of the composite positive electrode active material of Example 1 when manufacturing the positive electrode.
[0232] Evaluation example 1: Evaluation of room temperature high rate discharge characteristics The lithium batteries prepared in Examples 5 to 8, Reference Example 2, and Comparative Example 3 were charged at a constant current of 0.1 C rate at 25° C. until the voltage reached 4.45 V (vs. Li), and then cut off at a current of 0.05 C rate while maintaining 4.45 V in constant voltage mode. Then, the batteries were discharged at a constant current of 0.1 C rate until the voltage reached 3.0 V (vs. Li) (formation cycle).
[0233] The lithium battery that had undergone the formation cycle was charged at a constant current of 0.2C rate at 25°C until the voltage reached 4.45V (relative to Li), and then cut-off at a current of 0.05C rate while maintaining 4.45V in constant voltage mode. It was then discharged at a constant current of 0.2C rate until the voltage reached 3.0V (relative to Li) (first cycle).
[0234] The lithium battery that had undergone the first cycle was charged at a constant current of 0.2C rate at 25°C until the voltage reached 4.45V (relative to Li), and then cut-off at a current of 0.05C rate while maintaining 4.45V in constant voltage mode. It was then discharged at a constant current of 0.5C rate until the voltage reached 3.0V (relative to Li) (second cycle).
[0235] The lithium battery after the second cycle was charged at a constant current of 0.2 C rate at 25°C until the voltage reached 4.45 V (relative to Li), and then cut off at a current of 0.05 C rate while maintaining 4.45 V in constant voltage mode. It was then discharged at a constant current of 1.0 C rate until the voltage reached 3.0 V (relative to Li) (third cycle).
[0236] The lithium battery after the third cycle was charged at a constant current of 0.2 C rate at 25°C until the voltage reached 4.45 V (relative to Li), and then cut off at a current of 0.05 C rate while maintaining 4.45 V in constant voltage mode. It was then discharged at a constant current of 2.0 C rate until the voltage reached 3.0 V (relative to Li) (fourth cycle).
[0237] In all charge / discharge cycles, a 10-minute rest period was allowed after each charge / discharge cycle. Some of the results of the room temperature charge / discharge experiments are shown in Tables 1 and 2 below. The results in Table 1 below are for the positive electrode with an L / L of 10 mg / cm 2 The high rate characteristic is defined by the following formula 1.
[0238] [Formula 1] High-rate discharge characteristic [%] = [0.5C, 1C or 2C rate discharge capacity (discharge capacity at one of the 2nd to 5th cycles) / 0.2C rate discharge capacity (discharge capacity at the first cycle)] x 100
[0239] [Table 1]
[0240] As can be seen from Table 1, the lithium batteries of Examples 5 to 8 were improved in discharge capacity characteristics and high-rate discharge characteristics compared to the lithium batteries of Comparative Example 3 and Reference Example 2.
[0241] Also, although not shown in Table 1, it was confirmed that the lithium battery of Comparative Example 4 had deteriorated discharge capacity characteristics and high discharge rate characteristics compared to the lithium batteries of Examples 5 to 8.
[0242] Evaluation example 2: Evaluation of high-rate charging characteristics at room temperature The lithium batteries prepared in Examples 5 to 8, Reference Example 2, and Comparative Example 3 were charged at a constant current of 0.1 C rate at 25° C. until the voltage reached 4.45 V (vs. Li), and then cut-off at a current of 0.05 C rate while maintaining 4.45 V in constant voltage mode. Then, the batteries were discharged at a constant current of 0.1 C rate until the voltage reached 3.0 V (vs. Li) (formation cycle).
[0243] The lithium battery that had undergone the formation cycle was charged at a constant current of 0.2C rate at 25°C until the voltage reached 4.45V (relative to Li), and then discharged at a constant current of 0.2C rate until the voltage reached 3.0V (relative to Li) (first cycle).
[0244] The lithium battery that had undergone the first cycle was charged at a constant current of 0.5C rate at 25°C until the voltage reached 4.45V (relative to Li), and then discharged at a constant current of 0.2C rate until the voltage reached 3.0V (relative to Li) (second cycle).
[0245] The lithium battery after the second cycle was charged at a constant current of 1.0 C rate at 25°C until the voltage reached 4.45 V (relative to Li), and then discharged at a constant current of 0.2 C rate until the voltage reached 3.0 V (relative to Li) (third cycle).
[0246] The lithium battery after the third cycle was charged at a constant current of 2.0 C rate at 25°C until the voltage reached 4.45 V (relative to Li), and then discharged at a constant current of 0.2 C rate until the voltage reached 3.0 V (relative to Li) (fourth cycle).
[0247] In all charge / discharge cycles, a 10-minute rest period was allowed after each charge / discharge cycle. Some of the results of the room temperature charge / discharge experiments are shown in Table 2 below. The results in Table 2 below are for the positive electrode with an L / L of 10 mg / cm 2 The high rate characteristic is defined by the following Equation 2.
[0248] [Formula 2] High-rate charging characteristic [%] = [0.5C, 1C or 2C rate charging capacity (charging capacity at one of the 2nd to 5th cycles) / 0.2C rate charging capacity (charging capacity at the first cycle)] x 100
[0249] [Table 2]
[0250] As can be seen from Table 2, the lithium batteries of Examples 5 to 8 have improved charge capacity characteristics and high-rate charging characteristics compared to the lithium batteries of Comparative Example 3 and Reference Example 2, and are expected to have improved rapid charging characteristics in particular.
[0251] In addition, although not shown in Table 2, it was confirmed that the lithium battery of Comparative Example 4 had deteriorated charging capacity characteristics and charging high rate characteristics compared to the lithium batteries of Examples 5 to 8.
[0252] Evaluation example 3: High temperature (45℃) charge / discharge characteristic evaluation The lithium batteries prepared in Example 5, Reference Example 2, and Comparative Example 3 were charged at a constant current of 0.2 C rate at 25° C. until the voltage reached 4.45 V (vs. Li), and then cut-off at a current of 0.05 C rate while maintaining 4.45 V in constant voltage mode. Subsequently, the batteries were discharged at a constant current of 0.2 C rate until the voltage reached 3.0 V (vs. Li) (formation cycle).
[0253] The lithium battery that had undergone the formation cycle was charged at a constant current of 1C rate at 45°C until the voltage reached 4.45V (relative to Li), and then cut-off at a current of 0.05C rate while maintaining 4.45V in constant voltage mode. It was then discharged at a constant current of 1C rate until the voltage reached 3.0V (relative to Li) (first cycle). Such cycles were repeated under the same conditions up to the 50th cycle.
[0254] In all charge / discharge cycles, a rest period of 10 minutes was allowed after each charge / discharge cycle. Some results of the room temperature charge / discharge experiments are shown in Table 3 below. The capacity retention rate is defined by the following Equation 4.
[0255] [Formula 4] Capacity retention rate [%] = [discharge capacity at 50th cycle / discharge capacity at first cycle] x 100
[0256] Evaluation example 4: Evaluation of direct current internal resistance (DC-IR) before and after high-temperature charging and discharging For the lithium batteries prepared in Examples 5 to 8, Comparative Example 3, and Reference Example 2, the direct current internal resistance (DC-IR) was measured before and after the high temperature charge / discharge evaluation by the following method.
[0257] In the first cycle, the battery was charged at a constant current of 0.2C rate until the voltage reached 4.45V (relative to Li), and then cut-off at a current of 0.05C rate while maintaining 4.45V in constant voltage mode. The battery was then discharged at a constant current of 0.2C rate until the voltage reached 3.0V (relative to Li) (formation step). In the second cycle, the battery was charged at a constant current of 0.2C rate until 4.45V (relative to Li), and then cut-off at a current of 0.05C rate while maintaining 4.45V in constant voltage mode. The battery was then discharged at a 0.2C rate for 2 hours and 30 minutes until the SOC (state of charge) reached 50%, and then discharged at a constant current of 3C for 10 seconds, then discharged at a constant current of 0.2C for 10 seconds, and finally discharged at a constant current of 3C for another 10 seconds.
[0258] The DC internal resistance (DC-IR (R = ΔV / ΔI)) was calculated from the ratio of the average voltage change (ΔV) and the average current change (ΔI) during constant current discharge at each C-rate, and the average value was taken as the measured value.
[0259] The evaluation of the high-temperature charge-discharge life and some of the measurement results of the direct current internal resistance are shown in Table 5 below. The results in Table 5 below are for the positive electrode with an L / L of 10 mg / cm 2 This applies when:
[0260] [Table 3]
[0261] As can be seen from Table 3, it was found that the lithium battery of Example 5 had improved high-temperature life characteristics and an improved DC-IR increase rate compared to the lithium batteries of Comparative Example 3 and Reference Example 2. The lithium battery of Example 7 had improved high-temperature life characteristics and DC-IR characteristics compared to the lithium battery of Comparative Example 3, and compared to the lithium battery of Reference Example 2, the high-temperature characteristics were improved and the DC-IR showed the same characteristics. Such results are because the composite forms a coating layer that stably adheres carbon nanotubes (CNT) to the surface of the positive electrode active material and does not easily cause desorption.
[0262] The lithium battery of Comparative Example 3 had insufficient high-temperature life characteristics compared to the lithium battery of Example 5. In the lithium battery of Comparative Example 3, it was determined that there was no coating film on the NMX core and the side reaction between the NMX core and the electrolyte could not be effectively blocked.
[0263] The lithium battery of Reference Example 2 had insufficient high-temperature life characteristics compared to the lithium battery of Example 5.
[0264] Evaluation example 5: SEM, HR-TEM and SEM-EDS analysis Scanning electron microscopy, high-resolution transmission electron microscopy, and EDS (energy-dispersive X-ray spectroscopy) analysis were performed on the composite produced in Production Example 1, the composite positive electrode active material produced in Example 1, and the composite positive electrode active material produced in Comparative Example 1.
[0265] During SEM-EDS analysis, FEI Titan 80-300 from Philips was used.
[0266] The composite produced in Production Example 1 shows a structure in which Al 2 O 3 particles and its reduction product Al 2 O z (0 < z < 3) particles are embedded in graphene. Al 2 O 3 particles and Al 2 O zIt was confirmed that a graphene layer was disposed on the outer contour of one or more particles selected from (0 < z < 3). Al 2 O 3 Particles and Al2O z One or more particles selected from (0 < z < 3) are uniformly dispersed in the graphene matrix. Al 2 O 3 Particles and Al 2 O z The particle size of one or more of the (0 < z < 3) particles was about 20 nm. The particle size of the composite produced in Production Example 1 was about 50 nm to 200 nm. In the composite positive electrode active material produced in Example 1, it was confirmed that a shell formed by a composite containing graphene was disposed on the NMX core.
[0267] In the SEM-EDS mapping analysis of the composite positive electrode active materials produced in Comparative Example 1 and Example 1, it was confirmed that the concentration of aluminum (Al) distributed on the surface of the composite positive electrode active material of Example 1 increased compared to the surface of the composite positive electrode active material of Comparative Example 1.
[0268] In the composite positive electrode active material of Example 1, it was confirmed that the composite produced in Production Example 1 was uniformly coated on the NMX core to form a shell.
[0269] Evaluation example 6: XPS spectrum evaluation (graphene-NMX chemical bond) For the composite produced in Production Example 1, the NMX of Comparative Example 1, and the composite positive electrode active material produced in Example 1, XPS spectra related to the O1s orbital were measured using Quantum 2000 (Physical Electronics), and the results are shown in FIG. 9.
[0270] As can be seen from FIG. 9, in the composite positive electrode active material of Example 1, a peak due to a CO-Ni bond was observed at around 530.2 eV. It was determined that such a peak was due to a bond formed between the NiO phase present on the NCM surface and the carbon of the graphene. Therefore, it was confirmed that the graphene contained in the shell formed on the core forms a covalent bond with Ni, which is a transition metal contained in the core.
[0271] Evaluation example 7: Raman spectrum evaluation (graphene-NMX chemical bond) The Raman spectra of the composite produced in Production Example 1 and the composite positive electrode active material produced in Example 1 were measured, and the results are shown in FIG.
[0272] As can be seen from FIG. 10, the composite produced in Production Example 1 had a 1,338.7 cm -1 The D band peak at 1,575.0 cm -1 The G-band peak at
[0273] In contrast, in the composite positive electrode active material of Example 1, the graphene-containing shell causes the D band peak to be at 1,351.3 cm -1 Approximately 12cm -1 The G-band peak shifts to 1,593.6 cm -1 Approximately 18cm -1 It's shifting.
[0274] The shift in the D-band peak was determined to be due to strain in the graphene that is bonded onto the core by milling to form the shell.
[0275] The shift in the G-band peak was determined to be due to charge transfer between the core and graphene in the complex formed by the CO-Ni bond. Therefore, it was confirmed that the graphene contained in the shell formed on the core forms a covalent bond with Ni, a transition metal contained in the core. [Explanation of symbols]
[0276] 1 Lithium battery 2 negative electrode 3 Positive electrode 4. Separator 5 Battery case 6 Cap Assembly 7 Battery structure 8 Electrode tab 10 cores 20 Shell 21 First metal oxide 22 Carbon-based materials No. 1 23 Secondary carbon-based materials 100 Composite positive electrode active material
Claims
1. a first core comprising a first lithium transition metal oxide; a second core comprising a second lithium transition metal oxide; a shell disposed along at least one surface of the first core and the second core; the shell comprises one or more first metal oxides, a first carbon-based material, and a second carbon-based material; the first metal oxide is disposed within a matrix of the first carbon-based material; The first metal oxide is represented by the formula M a O b (0<a≦3, 0<b<4, and if a is 1, 2, or 3, then b is not an integer), and M is one or more metals selected from Groups 2 to 13 of the Periodic Table, Groups 15 and 16 of the Periodic Table; the second carbon-based material includes a fibrous carbon-based material having an aspect ratio of 10 or more; the first lithium transition metal oxide and the second lithium transition metal oxide have different particle sizes.
2. 2. The composite active cathode material of claim 1, wherein the first lithium transition metal oxide and the second lithium transition metal oxide each comprise secondary particles comprising a plurality of primary particles.
3. the first lithium transition metal oxide is a large particle size lithium transition metal oxide having a larger particle size than the second lithium transition metal oxide, the second lithium transition metal oxide is a small particle size lithium transition metal oxide having a smaller particle size than the first lithium transition metal oxide, 2. The composite cathode active material of claim 1, wherein the first lithium transition metal oxide and the second lithium transition metal oxide are polycrystalline.
4. The first lithium transition metal oxide and the second lithium transition metal oxide have a bimodal particle size distribution in particle size distribution degree, 2. The composite cathode active material of claim 1, wherein a particle size ratio of the first lithium transition metal oxide to the second lithium transition metal oxide is from 2.5:1 to 40:
1.
5. 2. The composite cathode active material of claim 1, wherein the first lithium transition metal oxide has a particle size of 3 μm to 15 μm and the second lithium transition metal oxide has a particle size of 1 μm to less than 7 μm.
6. 2. The composite positive electrode active material of claim 1, wherein a weight ratio of the first lithium transition metal oxide to the second lithium transition metal oxide is from 92:8 to 60:
40.
7. the shell is disposed only on the first core, the shell is disposed only on the second core, or the shell is disposed on both the first core and the second core; The composite positive electrode active material of claim 1 , wherein the content of the shell is 5 wt % or less based on the total weight of the composite positive electrode active material.
8. The content of the second carbon-based material is 5 wt % or less based on the total weight of the composite positive electrode active material; The content of the second carbon-based material is 0.1 wt % to 50 wt % based on the total weight of the first carbon-based material and the second carbon-based material; the second carbon-based material comprises carbon nanofibers, carbon nanotubes, or a combination thereof; 10. The composite active cathode material of claim 1, wherein the second carbon-based material is disposed on a surface of the composite active cathode material.
9. The carbon nanotubes include a carbon nanotube primary structure, a carbon nanotube secondary structure formed by agglomeration of a plurality of carbon nanotube primary particles, or a combination thereof; The carbon nanotube primary structure is a carbon nanotube unit, the carbon nanotube primary structure comprises a single-walled carbon nanotube (SWCNT), a double-walled carbon nanotube (DWCNT), a multi-walled carbon nanotube (MWCNT), or a combination thereof; The carbon nanotube primary structure has a diameter of 1 nm to 20 nm and a length of 100 nm to 2 μm; the carbon nanotube secondary structures include bundled carbon nanotubes, bundled carbon nanotubes, or a combination thereof; 9. The composite cathode active material of claim 8, wherein the carbon nanotube substructures have a diameter of 2 nm to 50 nm and a length of 500 nm to 1,000 μm.
10. the first metal contained in the first metal oxide is one or more metals selected from Al, Nb, Mg, Sc, Ti, Zr, V, W, Mn, Fe, Co, Pd, Cu, Ag, Zn, Sb, and Se; The first metal oxide is Al 2 O z (0<z<3), NbO x (0<x<2.5), MgO x (0<x<1), Sc 2 O z (0<z<3), TiO y (0<y<2), ZrO y (0<y<2), V 2 O z (0<z<3), WO y (0<y<2), MnO y (0<y<2), Fe 2 O z (0<z<3), Co 3 O w (0<w<4), PdO x (0<x<1), CuO x (0<x<1), AgO x (0<x<1), ZnO x (0<x<1), Sb 2 O z (0<z<3) and SeO y 2. The composite positive electrode active material of claim 1 , wherein y is one or more selected from (0<y<2).
11. The shell is represented by the formula M a O c (where 0<a≦3, 0<c≦4, and if a is 1, 2, or 3, then c is an integer), the second metal oxide contains the same metal as the first metal oxide; a ratio of a to c in the second metal oxide, c / a, is greater than a ratio of a to b in the first metal oxide, b / a, The second metal oxide is Al 2 O 3 , NbO, NbO 2 , Nb 2 O 5 , MgO, Sc 2 O 3 , TiO 2 , ZrO 2 , V 2 O 3 , W.O. 2 , MnO 2 , Fe 2 O 3 , Co 3 O 4 , PdO, CuO, AgO, ZnO, Sb 2 O 3 and SeO 2 is selected from 2. The composite active cathode material of claim 1 , wherein the first metal oxide is a reduction product of the second metal oxide.
12. the shell includes a first carbon-based material arranged in a direction protruding from a surface of one or more of the first metal oxide and the second metal oxide, 2. The composite cathode active material of claim 1, wherein the shell has a thickness of 1 nm to 5 μm.
13. the shell includes at least one selected from a composite including the first metal oxide, a first carbon-based material, and a second carbon-based material, and a milling result of the composite; 2 . The composite positive electrode active material of claim 1 , wherein the content of at least one of the composite and the milled product of the composite is 0.01 wt % to 5 wt % of the total weight of the composite positive electrode active material.
14. 2. The composite positive electrode active material of claim 1, wherein the lithium transition metal oxide is represented by a formula selected from the following formulas 1 to 8: [Chemical formula 1] Li a Ni x Mn y M' z O 2-b A b In the above Chemical Formula 1, 1.0≦a≦1.2, 0≦b≦0.2, 0<x≦0.85, 0.1≦y<0.3, 0<z≦0.1, and x+y+z=1; M' is cobalt (Co), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), boron (B), or a combination thereof; A is F, S, Cl, Br, or a combination thereof; [Chemical formula 2] L)) x Co y Mn z O 2 [Chemical formula 3] L)) x Co y Al z O 2 In the formulas 2 and 3, 0.8≦x≦0.95, 0≦y≦0.2, 0<z≦0.2, and x+y+z=1; [Chemical formula 4] L)) x Co y Mn z Al w O 2 In the formula 4, 0.8≦x≦0.95, 0≦y≦0.2, 0<z≦0.2, 0<w≦0.2, and x+y+z+w=1; [Chemical formula 5] Li a Co x MyO 2-b A b In the above Chemical Formula 5, 1.0≦a≦1.2, 0≦b≦0.2, 0.9≦x≦1, 0≦y≦0.1, and x+y=1; M is manganese (Mn), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), boron (B), or a combination thereof; A is F, S, Cl, Br, or a combination thereof; [Chemical formula 6] Li a Ni x Co y M z O 2-b A b In the above Chemical Formula 6, 1.0≦a≦1.2, 0≦b≦0.2, 0.8≦x<1, 0≦y≦0.3, 0<z≦0.3, and x+y+z=1; M is manganese (Mn), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), boron (B), or a combination thereof; A is F, S, Cl, Br, or a combination thereof; [Chemical formula 7] Li a M1 x M2 y PO 4-b X b In the formula 7, 0.90≦a≦1.1, 0≦x≦0.9, 0≦y≦0.5, 0.9<x+y<1.1, and 0≦b≦2; M1 is chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zirconium (Zr), or a combination thereof; M2 is magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), zinc (Zn), boron (B), niobium (Nb), gallium (Ga), indium (In), molybdenum (Mo), tungsten (W), aluminum (Al), silicon (Si), chromium (Cr), vanadium (V), scandium (Sc), yttrium (Y), or a combination thereof; X is O, F, S, P, or a combination thereof; [Chemical formula 8] Li a M3 z PO 4 In the formula 8, 0.90≦a≦1.1 and 0.9≦z≦1.1; M3 is chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zirconium (Zr), or a combination thereof.
15. A positive electrode comprising the composite active positive electrode material of claim 1 .
16. The positive electrode according to claim 15 ; A negative electrode; and an electrolyte disposed between the positive electrode and the negative electrode.
17. 17. The lithium battery of claim 16, wherein the electrolyte comprises a liquid electrolyte, a solid electrolyte, a gel electrolyte, or a combination thereof.
18. The solid electrolyte includes an oxide-based solid electrolyte, a sulfide-based solid electrolyte, a polymer solid electrolyte, or a combination thereof; 20. The lithium battery of claim 17, wherein the gel electrolyte comprises a polymer gel electrolyte.
19. The positive electrode includes a positive electrode current collector, and the negative electrode includes a negative electrode current collector. At least one of the positive electrode current collector and the negative electrode current collector includes a base film and a metal layer disposed on one surface or both surfaces of the base film; the base film comprises a polymer, the polymer comprising polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polybutylene terephthalate (PBT), polyimide (PI), or a combination thereof; 20. The lithium battery of claim 18, wherein the metal layer comprises indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li), or an alloy thereof.
20. providing a first lithium transition metal oxide; providing a second lithium transition metal oxide; Providing a complex; providing a second carbon-based material; mechanically milling the first lithium transition metal oxide, the composite, and the second carbon-based material to obtain a first core / shell structure; mechanically milling the second lithium transition metal oxide, the composite, and the second carbon-based material to obtain a second core / shell structure; mixing the first core / shell structure with the second core / shell structure to obtain a composite positive electrode active material; The complex has the formula M a O b (where 0<a≦3, 0<b<4, and if a is 1, 2, or 3, then b is not an integer), and a first carbon-based material, The first metal oxide is disposed in a matrix of a first carbon-based material, and the M is one or more metals selected from Groups 2 to 13 of the Periodic Table, Groups 15 and 16 of the Periodic Table; the second carbon-based material includes fibrous carbon having an aspect ratio of 10 or more; The first lithium transition metal oxide and the second lithium transition metal oxide have different particle sizes.