Active material reuse method using cathode scraps
The method recovers positive electrode active materials from lithium secondary batteries through dry grinding, heat treatment, and lithium compound washing, addressing inefficiencies in existing methods by ensuring high recovery rates and maintaining electrochemical performance.
Patent Information
- Application Number
- JP2024109468
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-10-16
- Filing Date
- 2024-07-08
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-08-30
AI Technical Summary
Existing methods for recycling positive electrode active materials from lithium secondary batteries are environmentally unfriendly and inefficient, as they require acid dissolution and neutralization processes, and fail to recover lithium, leading to increased costs and waste.
A method involving dry grinding, heat treatment, washing with a lithium compound solution, and annealing to separate and recover the active material from the current collector, without using acids, ensuring high recovery rates and maintaining electrochemical performance.
The method allows for the environmentally friendly and cost-effective reuse of positive electrode active materials, with high recovery rates and preserved electrochemical properties, suitable for mass production.
Smart Images

Figure 2024133091000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for recycling resources during the manufacture of a lithium secondary battery. In particular, the present invention relates to a method for recovering and reusing positive electrode scrap generated in the manufacturing process of a lithium secondary battery or a positive electrode active material of a lithium secondary battery that is discarded after use. This application claims priority to Korean Patent Application No. 10-2020-0134325 filed on October 16, 2020, and the contents disclosed in the specification and drawings of the corresponding application are incorporated herein in their entirety. [Background technology]
[0002] Lithium secondary batteries, which can be repeatedly charged and discharged, are attracting attention as an alternative to fossil energy. Lithium secondary batteries have been mainly used in traditional handheld devices such as mobile phones, video cameras, and power tools. However, their application fields are gradually increasing in recent years, including electrically driven automobiles (EV, HEV, PHEV), large-capacity energy storage systems (ESS), and uninterruptible power supplies (UPS).
[0003] A lithium secondary battery includes an electrode assembly in which unit cells are assembled, each having a structure in which a positive electrode plate and a negative electrode plate, each having an active material coated on a current collector, are arranged with a separator sandwiched therebetween, and an exterior material, i.e., a battery case, which seals and houses the electrode assembly together with an electrolyte. The positive electrode active material of a lithium secondary battery mainly uses a lithium-based oxide, and the negative electrode active material uses a carbon material. The lithium-based oxide contains metals such as cobalt, nickel, or manganese. In particular, cobalt, nickel, and manganese are valuable metals that are very expensive, and among them, cobalt is a strategic metal, and countries around the world are particularly interested in supply and demand. Since the number of cobalt producing countries is limited, it is known that the supply and demand of cobalt is unstable worldwide. If an imbalance in supply and demand of raw materials for strategic metals occurs, there is a high possibility that the price of the raw materials will rise.
[0004] So far, research has focused on recovering and recycling these valuable metals from lithium secondary batteries (waste batteries) that are discarded after the end of their lifespan after use. In addition to waste batteries, it would be even more desirable to recover resources from waste materials discarded after punching out positive plates or from positive electrodes that have become defective during the process.
[0005] Currently, in the manufacture of lithium secondary batteries, a long sheet-like positive electrode collector 10 such as an aluminum (Al) foil is coated with a positive electrode slurry, which is a mixture of a positive electrode active material, a conductive material, a binder, a solvent, etc., to form a positive electrode active material layer 20, to manufacture a positive electrode sheet 30, which is then punched out to a certain size as a positive electrode plate 40. The portion remaining after punching is discarded as positive electrode scrap 50. If the positive electrode active material could be recovered from the positive electrode scrap 50 and reused, this would be very desirable in terms of industry, economy, and the environment.
[0006] In most existing methods for recovering positive electrode active materials, the positive electrode is dissolved with hydrochloric acid, sulfuric acid, nitric acid, etc., and active material elements such as cobalt, nickel, manganese, etc. are extracted and used as raw materials for synthesizing positive electrode active materials again. However, the method for extracting active material elements using an acid has disadvantages in that the process for recovering pure raw materials is not environmentally friendly, and a neutralization process and a wastewater treatment process are required, which increases the process cost. In addition, it has a disadvantage in that lithium, which is one of the main elements of the positive electrode active material, cannot be recovered. To overcome these disadvantages, a method is needed that allows the positive electrode active material to be directly reused without dissolving it and extracting the active material in elemental form. Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the present invention is to provide a method for recovering and reusing active material from positive electrode scraps. [Means for solving the problem]
[0008] In order to solve the above problems, the method for reusing a positive electrode active material of the present invention includes the steps of: (a-1) dry-pulverizing positive electrode scrap including a positive electrode active material layer made of a lithium composite transition metal oxide on a current collector to detach the active material layer in a powder form and separating it from the current collector; (a-2) heat-treating the active material layer detached in a powder form in air to thermally decompose the binder and the conductive material in the active material layer, thereby recovering the active material; (b) washing the recovered active material with an aqueous solution of a lithium compound that is basic in an aqueous solution state, and drying it; and (c) adding a lithium precursor to the washed active material, followed by annealing, to obtain a reusable active material.
[0009] In the present invention, the method may further include the step of (d) applying a surface coating to the annealed active material.
[0010] The dry milling may be carried out using any one of a pin mill, a disc mill, a cutting mill, and a hammer mill.
[0011] The method may further include a step of shredding or cutting the cathode scrap before the dry grinding.
[0012] The heat treatment can be carried out at 300 to 1,000°C.
[0013] The heat treatment may be carried out at a temperature rate of 5° C. / min at 550° C. for 30 minutes.
[0014] The aqueous lithium compound solution is prepared to contain greater than 0% and less than or equal to 15% of the lithium precursor, preferably LiOH. The wash can be performed within an hour.
[0015] The washing can be carried out by immersing the recovered active material in an aqueous lithium compound solution and stirring it.
[0016] The lithium precursor can be any one or more of LiOH, Li2CO3, LiNO3, and Li2O.
[0017] The lithium precursor may be added in an amount sufficient to replace the proportion of lithium lost relative to the proportion of lithium and other metals in the raw active material used in the active material layer.
[0018] For example, the lithium precursor may be added in an amount such that the amount of lithium added is 0.001 to 0.4 molar ratio.
[0019] Furthermore, it is desirable to further add lithium in an amount of 0.0001 to 0.1 molar ratio of lithium to the lithium precursor, based on a molar ratio of lithium to other metal of 1:1.
[0020] Annealing may be carried out in air at 400-1,000°C.
[0021] The temperature of the annealing step may be above the melting point of the lithium precursor.
[0022] The active material in the active material layer is recovered in powder form, and no carbon components resulting from carbonization of the binder or conductive material remain on the surface.
[0023] The surface coating step may be a step of coating the surface with at least one of metal, organometallic, and carbon components in a solid or liquid phase manner, followed by heat treatment at 100 to 1,200°C.
[0024] The reusable active material may be represented by Formula 1 below.
[0025] Li a Ni x Mn y Co z M w O 2+δ (chemical formula 1)
[0026] In Chemical Formula 1, M is at least one selected from the group consisting of B, W, Al, Ti, and Mg; <a≦1.1、0≦x<0.95、0≦y<0.8、0≦z<1.0、0≦w≦0.1、-0.02≦δ≦0.02、x+y+z+w=1である。
[0027] The reusable active material may have a fluorine (F) content of 100 ppm or less. Effect of the Invention
[0028] According to the present invention, waste positive electrode active material such as positive electrode scraps generated in the manufacturing process of lithium secondary batteries can be reused without using acid, which is environmentally friendly. The method according to the present invention does not require a neutralization process or a wastewater treatment process, which reduces the burden on the environment and reduces process costs.
[0029] According to the present invention, the positive electrode active material can be recovered without unrecoverable metal elements. The current collector can also be recovered because it is not dissolved. It is economical because the active material elements are not extracted and used as raw materials for further synthesis of the positive electrode active material, but the recovered active material in powder form can be directly reused.
[0030] According to the present invention, since no toxic or explosive solvents such as NMP, DMC, acetone, or methanol are used, the process is safe, and since simple processes such as heat treatment, cleaning, and annealing are used, the process management is easy and it is suitable for mass production.
[0031] According to the present invention, the electrochemical performance of the recovered active material is not deteriorated, and excellent resistance and capacity characteristics can be realized.
[0032] In particular, according to the present invention, the active material and the current collector are first separated using dry pulverization. The current collector and the active material are completely separated by dry pulverization, and a recovery rate of the positive electrode active material of 95% or more can be secured. Dry pulverization has a high processing rate per hour, so the positive electrode active material can be reused with high productivity.
[0033] The following drawings attached to this specification illustrate preferred embodiments of the present invention and, together with the detailed description of the invention, serve to further understand the technical ideas of the present invention. Therefore, the present invention should not be interpreted as being limited to only the matters described in the drawings. [Brief description of the drawings]
[0034] [Figure 1] FIG. 13 is a diagram showing positive electrode scraps that are discarded after the positive electrode plate is punched out of the positive electrode sheet. [Diagram 2] 2 is a flow chart of a method for reusing active materials according to the present invention. [Diagram 3] 6 is a photograph of a result at each step according to an experimental example of the present invention. [Figure 4] 4 is a SEM photograph of an active material layer after dry pulverization in the method for reusing an active material according to the present invention. [Diagram 5] 5 is a SEM photograph of the active material layer of FIG. 4 after being heat-treated in air. [Figure 6] 1 is a SEM photograph of an active material that has been dried after LiF has been removed by washing in a method for reusing an active material according to the present invention. [Figure 7] 1 shows the results of cell evaluation using an active material of a comparative example. [Figure 8] 1 shows the results of cell evaluation using active materials of Examples and Comparative Examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0035] Hereinafter, a preferred embodiment of the present invention will be described in detail with reference to the attached drawings. Prior to this, the terms and words used in this specification and claims should not be interpreted as being limited to their ordinary or dictionary meanings, but should be interpreted as being in accordance with the meaning and concept of the technical idea of the present invention, in accordance with the principle that the inventor himself can appropriately define the concept of the term in order to best describe the invention. Therefore, it should be understood that the embodiment described in this specification and the configuration shown in the drawings are only one most preferred embodiment of the present invention, and do not represent the entire technical idea of the present invention, and therefore there may be various equivalents and modifications that can be substituted for them at the time of this application.
[0036] In the following description, reference will be made to the accompanying drawings, which form a part of this application. The embodiments described in the detailed description, drawings, and claims are not intended to be limiting. Other embodiments may be utilized, and other changes may be made, without departing from the spirit and scope of the subject matter disclosed herein. It will be understood that the aspects of the invention as generally described herein and illustrated in the drawings may be arranged, substituted, combined, separated, and designed in a variety of other configurations, all of which are expressly contemplated herein.
[0037] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs (hereinafter referred to as "person of ordinary skill in the art").
[0038] The present invention is not limited by the specific embodiments described herein. As will be apparent to those skilled in the art, various changes and modifications can be made without departing from the spirit and scope of the present invention. In addition to those enumerated herein, functionally equivalent methods within the scope of the present application will become apparent to those skilled in the art from the foregoing description. Such changes and modifications are within the scope of the appended claims. The present invention is limited only by the claims, along with the full scope of equivalents to which such claims are entitled. It should be understood that the present invention is not limited to the specific manner in which it can be varied, of course. The terminology used herein is used only for the purpose of describing specific embodiments and is not intended to be limiting.
[0039] In the case of the conventional active material recycling process, the main purpose was to extract valuable metals (nickel, cobalt, manganese, etc.) as elements from the active material of a lithium secondary battery whose performance has deteriorated after use, and resynthesize the active material. However, the present invention is different in that it recovers active material from cathode scraps generated during the manufacturing process of a lithium secondary battery.
[0040] In addition, in the case of the existing active material recycling process, valuable metals are extracted using acid / base dissolution or reduction / melting with additives, and then chemical methods such as manufacturing it into metal (direct reduction method) or resynthesizing active material are added, which further increases the process complexity and cost. However, the present invention relates to a method for directly reusing the positive electrode active material without dissolving it.
[0041] To directly reuse the positive electrode active material, the current collector must be removed from the positive electrode, which can be done by high-temperature heat treatment to remove the binder, by dissolving the binder with a solvent, by dissolving the current collector itself, or by dry grinding and sieving to separate the active material.
[0042] When using a solvent to dissolve the binder, the stability of the solvent is important. NMP is the most efficient solvent, but it has the disadvantages of toxicity and high cost. Another disadvantage is that a solvent recovery process, such as reprocessing waste solvent, is required. Dissolving the current collector is less expensive than using a solvent. However, it is difficult to remove foreign matter from the surface of the reused active material, and hydrogen gas is generated during the current collector removal process, which may cause an explosion. It is difficult to completely separate the current collector and active material using dry grinding and sieving. The particle size distribution of the active material changes during the grinding process, making it difficult to remove the binder, which has the disadvantage of deteriorating the battery characteristics when it is reused.
[0043] In the present invention, the active material and the current collector are first separated using dry grinding. Dry grinding completely separates the active material from the current collector, ensuring a recovery rate of 95% or more of the positive electrode active material. Then, the binder and conductive material are removed by heat treatment. This heat treatment is carried out in air, so no special equipment configuration is required, and it is a relatively simple process that requires only heating, which is advantageous for mass production and commercialization. Meanwhile, no foreign matter should remain on the surface of the reused active material. The present invention also proposes a step of removing foreign matter from the surface of the reused active material.
[0044] Hereinafter, a method for reusing an active material according to an embodiment of the present invention will be described with reference to Fig. 2. Fig. 2 is a flow chart of a method for reusing an active material according to the present invention.
[0045] Referring to FIG. 2, first, a cathode scrap to be discarded is prepared (step S10).
[0046] The positive electrode scraps may be the remaining portion after a positive electrode sheet including a positive electrode active material layer is manufactured on a current collector and punched out as described with reference to Fig. 1. In addition, the positive electrode scraps may be prepared by collecting positive electrodes that have become defective during the process. Alternatively, the positive electrode scraps may be prepared by separating positive electrodes from lithium secondary batteries that have been discarded after use.
[0047] For example, a lithium cobalt oxide active material such as LiCoO2 (LCO) or an NCM active material containing nickel, cobalt, and manganese, carbon black as a conductive material, and polyvinylidene fluoride (PVdF) as a binder are mixed with NMP (N-methyl pyrrolidone) to prepare a slurry, which is then coated on a sheet-shaped current collector made of aluminum foil and dried in a vacuum oven at about 120°C to prepare a positive electrode sheet. After that, a positive electrode plate of a certain size is punched out, and the remaining positive electrode scrap is prepared.
[0048] Lithium composite transition metal oxides are used as the positive electrode active material of lithium secondary batteries, and among them, lithium cobalt oxide such as LiCoO2, lithium manganese oxide (LiMnO2 or LiMn2O4, etc.), lithium iron phosphate compound (LiFePO4, etc.), or lithium nickel oxide (LiNiO2, etc.) are mainly used. In addition, as a method for improving the low thermal stability of LiNiO2 while maintaining the excellent reversible capacity, nickel manganese-based lithium composite metal oxides in which part of nickel (Ni) is replaced with manganese (Mn), which has excellent thermal stability, and NCM lithium composite transition metal oxides in which manganese (Mn) and cobalt (Co) are replaced are used. The present invention is particularly suitable for reusing LCO and NCM active materials.
[0049] In this way, the positive electrode scrap has an active material layer on a metal foil current collector such as aluminum foil. The active material layer is formed by coating a slurry containing an active material, a conductive material, a binder, a solvent, etc., and therefore has a structure in which the binder connects the active material and the conductive material after the solvent volatilizes. Therefore, when the binder is removed, the active material can be separated from the current collector.
[0050] Next, the cathode scrap is shredded to an appropriate size (step S20). Shredding refers to cutting the cathode scrap into pieces of a suitable size that is easy to handle. After shredding, the cathode scrap has a size of about 10 cm x 10 cm. This may be further cut into smaller pieces. During cutting, the cathode scrap may be cut into pieces of, for example, 1 cm x 1 cm.
[0051] Crushing, including shredding and cutting, may be performed taking into consideration the handling of the cathode scrap and the desired characteristics of the equipment used in the subsequent processes. For example, when equipment that requires continuous processing for loading and unloading the cathode scrap is used, the cathode scrap should have good fluidity, so that excessively large cathode scrap should be crushed.
[0052] Next, the crushed positive electrode scraps are dry-pulverized to remove the active material layer in a powder form and separate it from the current collector (step S25). The dry pulverization may be performed using any one of a pin mill, a disc mill, a cutting mill, and a hammer mill. A pin mill is preferably used. In this way, the pin mill can ensure a recovery rate of 95% or more of the positive electrode active material in a powder form of 5 mm or less. The pin mill equipment can process 500 kg or more per hour. Thus, if the process is performed for 10 hours per day, an electrode separation effect of up to 5 tons can be achieved.
[0053] A pin mill is a device that has a structure in which rotating pins attached to a rotor and pins attached to a stationary platen mesh with each other, and when raw materials are fed into the center of the grinder, they are dispersed with the air flow generated by the rotation, and are crushed by the impact between the rotating platen and the stationary platen using the brittleness of the raw materials. Only crushed materials that can pass through holes formed in a ring-shaped screen are taken out.
[0054] When such a pin mill is used, it is possible to crush the material to a desired degree and particle size by adjusting the shape and number of pins, the size range of the screen to be filtered, etc. When crushed positive electrode scraps are crushed with a pin mill, the current collector pieces are cut into smaller pieces, and the active material layer, which is more brittle, is separated from the current collector pieces. The current collector pieces, which are more flexible, are rolled into a round shape and remain inside the screen, and only the active material layer in the form of fine powder that passes through the screen can be separated and obtained. Although the active material layer is broken and has lost the continuity that could be called a layer, it still has a powder form with the active material, binder, and conductive material solidified. In this way, the active material layer and the current collector can be separated only by dry grinding by utilizing the difference in brittleness and softness between the two.
[0055] Next, the active material layer separated in powder form is heat-treated in air (step S30).
[0056] In the present invention, the heat treatment is performed to thermally decompose the binder and conductive material in the active material layer. The heat treatment can be performed at 300 to 1,000°C, and is therefore also called high-temperature heat treatment. At temperatures below 300°C, it may be difficult to remove the binder. When the positive electrode scrap is heat-treated in the presence of the current collector without dry pulverization, the heat treatment must be performed at a temperature below the melting point of the current collector. However, in the present invention, the heat treatment is performed on the detached active material layer from which the current collector has already been separated, so there is no restriction on the heat treatment temperature due to the current collector.
[0057] The heat treatment time is maintained so that the binder is sufficiently decomposed. For example, it is set to about 30 minutes. It is preferably set to 30 minutes or more. The longer the heat treatment time, the longer it takes for the binder to decompose, but once it reaches a certain time, there is no difference in the decomposition effect. It is preferably set to 30 minutes or more and 5 hours or less.
[0058] The heat treatment equipment may be a furnace of various types, for example, a box-type furnace, or, in consideration of productivity, a rotary kiln capable of continuous treatment.
[0059] After the heat treatment, the material may be cooled slowly or rapidly in air.
[0060] For example, the heat treatment may be performed at 550°C for 30 minutes with a temperature rise rate of 5°C / min. The temperature rise rate may be a rate that can be easily implemented in, for example, a box-type furnace and that can heat the powder-type active material without causing thermal shock. 550°C facilitates thermal decomposition of the binder. At this temperature, if the heat treatment is performed for less than 10 minutes, the thermal decomposition is insufficient, so the heat treatment must be performed for 10 minutes or more, and it is preferable to perform the heat treatment for 30 minutes or more.
[0061] The heat treatment in air causes the binder and conductive material in the active material layer to be thermally decomposed and removed as CO2 and H2O. As the binder is removed, the active material to be recovered can be separated in powder form after the solidified active material is decomposed.
[0062] It is important that the heat treatment in step S30 is carried out in air. If the heat treatment is carried out in a reducing gas or inert gas atmosphere, the binder and conductive material are not thermally decomposed but are carbonized. If carbonized, the carbon components remain on the surface of the active material, which reduces the performance of the reused active material. If the heat treatment is carried out in air, the carbon substances in the binder and conductive material react with oxygen and are burned into CO and CO2 gas and removed, so that the binder and conductive material are almost completely removed without any residue.
[0063] Therefore, according to the present invention, the active material is recovered in powder form, and carbon components resulting from carbonization of the binder or conductive material do not remain on the surface.
[0064] Next, the recovered active material is washed and dried (step S40). During washing, it is important to wash with an aqueous solution of a lithium compound that is alkaline in aqueous solution. Such an aqueous solution of a lithium compound is prepared to contain more than 0% and not more than 15% of a lithium compound, and preferably LiOH is used. The amount of LiOH is preferably 15% or less. If an excessive amount of LiOH is used, LiOH may remain on the surface of the active material even after washing, which may affect the subsequent annealing process. In order to clean the surface of the active material as much as possible in the step prior to annealing, the addition of an excessive amount of LiOH is not good for the process, so it is limited to 15% or less.
[0065] The washing can be performed by immersing the recovered active material in such an aqueous lithium compound solution. After immersion, washing can be performed within one week, preferably within one day, and more preferably within one hour. If washing is performed for more than one week, there is a risk of capacity reduction due to excessive dissolution of lithium. Therefore, it is preferable to perform washing within one hour. Washing includes immersing the active material in an aqueous lithium compound solution that is alkaline in aqueous solution, stirring while immersed, etc. It is preferable to perform stirring in parallel as much as possible. If only immersion is performed in the aqueous lithium compound solution without stirring, the washing process will be slow and may cause lithium to dissolve. If stirring is performed in parallel, the process time can be minimized, so stirring is preferably performed at the same time as the impregnation with the aqueous lithium compound solution. Drying can be performed in air in an oven (convection type) after filtration.
[0066] When the active material is washed with an aqueous solution of a lithium compound that is alkaline in aqueous solution, LiF and metal fluoride present on the surface of the recovered active material can be removed to modify the surface. During the heat treatment in step S30, the binder and conductive material in the active material layer are vaporized and removed as CO2 and H2O, and in this process, CO2 and H2O react with the lithium on the active material surface to form Li2CO3 and LiOH, or F present in the binder such as PVdF reacts with lithium and other metals in the positive active material and lithium in the added lithium precursor to form LiF or metal fluoride. If such LiF or metal fluoride remains, the battery characteristics will deteriorate when the active material is reused. In the present invention, a washing step is added as step S40 to remove reactants generated on the surface of the reused active material in the heat treatment step S30, so that foreign matter does not remain on the surface of the reused active material.
[0067] In step S40, it is important to wash with an aqueous solution of a lithium compound that is basic in an aqueous solution. If an aqueous solution of sulfuric acid or hydrochloric acid is used instead of an aqueous solution of a lithium compound that is basic in an aqueous solution, F on the surface of the active material can be washed away, but transition metals (Co, Mg) present in the active material will be eluted, lowering the performance of the reused positive electrode active material. The aqueous solution of a lithium compound that is basic in an aqueous solution used in the present invention is highly desirable because it can remove binders that may remain even in trace amounts after the thermal decomposition in step S30, does not elute transition metals present in the active material, and compensates for the amount of lithium that may be eluted during the washing process.
[0068] Furthermore, if LiF remains, it may act as a resistive layer. Through step S40, according to the present invention, the LiF content on the surface of the recovered active material can be adjusted to less than 500 ppm, thereby improving the capacity. Preferably, the F content can be 100 ppm or less. More preferably, the F content can be 30 ppm or less.
[0069] Next, a lithium precursor is added to the washed active material and annealed (step S50).
[0070] During the previous steps S30 and S40, lithium loss may occur in the active material, and in step S50, this lithium loss is replenished.
[0071] Moreover, in step S50, the crystal structure of the active material is restored by annealing, thereby restoring or improving the properties of the reused active material to the same level as that of a fresh active material that has never been used.
[0072] During the previous steps S30 and S40, a deformed structure may appear on the surface of the active material. For example, in the case of an active material that is an NCM-based lithium transition metal composite oxide, Ni may turn into rock salt [NiCO3·2Ni(OH)2)H20] by moisture in step S40, forming a spinel structure. If a battery is manufactured in this state, the battery characteristics, such as a decrease in capacity, may deteriorate. In the present invention, the crystal structure is restored in step S50. For example, the active material that is an NCM-based lithium transition metal composite oxide is further restored to a hexagonal crystal structure. This allows the initial characteristics to be restored or improved to a level similar to that of a fresh active material.
[0073] The lithium precursor of step S50 can be any one or more of LiOH, Li2CO3, LiNO3, and Li2O.
[0074] The lithium precursor is added in an amount that can compensate for the ratio of lost lithium to the ratio of lithium and other metals in the raw active material (i.e., fresh active material) used in the active material layer. For example, when the ratio of lithium and other metals in the fresh active material is 1, the lithium precursor can be added in an amount that gives a lithium addition amount of 0.001 to 0.4 molar ratio. It is preferable to add the lithium precursor so that the molar ratio is 0.01 to 0.2. Addition of an excessive amount of lithium precursor other than the amount of lithium lost by washing or the like causes unreacted lithium precursor to remain in the reused active material, which is a factor that increases the resistance during the reuse of the active material, so it is necessary to add an appropriate amount of lithium precursor.
[0075] In addition, it is preferable to further add lithium to the lithium precursor in an amount of 0.0001 to 0.1 molar ratio based on a 1:1 molar ratio of lithium to other metals. The reason for adding such an excess amount of lithium is to form a surface protective layer by surface coating on the active material, which will be described in detail below. When a secondary battery is manufactured from such an active material, it is possible to maintain the life characteristics while suppressing side reactions caused by the electrolyte.
[0076] The annealing may be performed in air at 400 to 1,000°C. The annealing temperature may be 600 to 900°C. The annealing temperature may vary within a limited range depending on the type of lithium precursor. The annealing time is preferably 1 hour or more, more preferably about 5 hours. If the annealing time is long, the crystal structure recovery is sufficiently performed, but even if the annealing time is long, it does not have a significant effect on the performance. The annealing time is, for example, 15 hours or less. The annealing equipment may be the same as or similar to that of the heat treatment step S30.
[0077] For example, when Li2CO3 is used as the lithium precursor, the annealing temperature is preferably 700 to 900°C, more preferably 710 to 780°C. This is because the melting point of Li2CO3 is 723°C. More preferably, the annealing temperature is 750°C. When LiOH is used as the lithium precursor, the annealing temperature is preferably 400 to 600°C, more preferably 450 to 480°C. This is because the melting point of LiOH is 462°C.
[0078] The annealing temperature is preferably above the melting point of the lithium precursor, but should not exceed 1,000°C, since a temperature above 1,000°C can cause thermal decomposition of the positive electrode active material, resulting in a decrease in the performance of the active material.
[0079] Through this step S50, a reusable active material is obtained.
[0080] In the present invention, the active material in powder form is separated from the current collector by dry pulverization in step S25. Since this is a physical separation, there is no change in the chemical properties of the current collector or the active material.
[0081] Of course, it is also possible to separate the positive electrode active material layer by performing heat treatment with the current collector still present without dry pulverization. However, when the current collector is separated only by heat treatment without dry pulverization, the current collector and electrode have large volumes, and the mixing process by oxygen contact is important, so the processing amount per unit volume is lower than that of the dry pulverization method proposed in the present invention. As proposed in the present invention, the active material powder separated from the current collector by the dry pulverization method can be processed in large quantities by the heat treatment process. When using a pin mill, not only can a positive electrode active material recovery rate of 95% or more be ensured, but the electrode separation processing amount per hour is at least 500 kg or more, and productivity can be maximized due to the advantage that a continuous process is possible.
[0082] In addition, when heat treating cathode scraps in which the current collector remains intact without dry crushing, there is a restriction that the heat treatment must be limited to 550° C. or less due to the problem of oxidation of the aluminum current collector. However, according to the present invention, since the current collector is separated before the heat treatment, the heat treatment temperature can exceed the melting point of the current collector, 550° C. In other words, there is an advantage that the pre-separation of the current collector allows heating at a high temperature without any restriction on the heat treatment temperature during the heat treatment for removing the binder and conductive material.
[0083] Then, as an optional step, step S60 may be further performed, in which a surface coating is performed on the active material annealed in step S50.
[0084] The surface coating step may involve coating the surface with at least one of metal, organometallic, and carbon components in a solid or liquid phase manner, followed by heat treatment at 100 to 1,200°C. If heat treatment is performed at a temperature exceeding 1,200°C, performance may be reduced due to thermal decomposition of the positive electrode active material. In the case of surface coating, the solid or liquid phase method may include mixing, milling, spray drying, grinding, and the like.
[0085] In the case of NCM active material, B, BW, W, etc. may be coated, and in the case of LCO active material, Al, Mg, Ti, etc. If the heat treatment temperature required for coating needs to be high, step S60 may be performed before step S50. That is, the surface is first coated, and then a lithium precursor is added and annealed.
[0086] A surface protective layer made of different metals is formed by the surface coating. When the molar ratio of lithium to other metals in the positive active material is set to 1:1, if the lithium in the active material reacts with the surface coating material and the molar ratio of lithium to other metals in the positive active material decreases to less than 1:1, the capacity cannot be fully expressed. Therefore, in the previous step S30, lithium is further added through the addition of a lithium precursor so that the molar ratio of lithium to other metals in the positive active material is 1:1, and an excess amount of lithium is added so that it is contained in an additional 0.0001 to 0.1 molar ratio relative to the other metals in the positive active material. As a result, a surface protective layer can be formed even when the molar ratio of lithium to other metals in the positive active material is 1:1 during the surface coating.
[0087] Specifically, when metal oxides such as B, W, and BW are coated on the active material and then heat-treated, a lithium boron oxide layer can be formed on the surface of the active material, which acts as a surface protection layer. Lithium, which is further added in a molar ratio of 0.0001 to 0.1 in step S50, reacts with metal oxides such as B, W, and BW in step S60, and the molar ratio of lithium to other metals in the positive electrode active material does not decrease below 1:1, so no capacity loss occurs.
[0088] The reusable active material obtained by the above-described method may be represented by the following Chemical Formula 1:
[0089] Li a Ni x Mn y Co z M w O 2+δ (chemical formula 1)
[0090] In Chemical Formula 1, M is at least one selected from the group consisting of B, W, Al, Ti, and Mg; <a≦1.1、0≦x<0.95、0≦y<0.8、0≦z<1.0、0≦w≦0.1、-0.02≦δ≦0.02、x+y+z+w=1である。
[0091] The reusable active material may have an F content of 100 ppm or less. According to the present invention, since it is possible to recover an active material with a reduced F content, when the active material is reused, excellent resistance and capacitance characteristics can be realized.
[0092] Thus, according to the present invention, LiF or metal fluoride is removed in the washing step S40. The washing and drying steps using an aqueous solution of a lithium compound that is alkaline in an aqueous solution state are safe and inexpensive, and have the advantages of being able to remove LiF or metal fluoride without loss of other elements, preventing the elution of transition metals, etc., and compensating for lithium loss that occurs during the process. The annealing step is also safe and inexpensive, and has the advantages of being able to restore the crystal structure, i.e., improve the crystallinity, thereby restoring the battery characteristics of the reused active material.
[0093] The reusable active material obtained by the present invention has a particle size distribution similar to that of a fresh active material, so no additional treatment is required to adjust the particle size distribution. Carbon components generated by carbonization of the binder or conductive material do not remain on the surface, so a step for removing such carbon components is not required. Therefore, the active material obtained by the method of FIG. 2 above can be reused as it is for manufacturing a positive electrode without any additional treatment.
[0094] The recycled active material can be used as it is without adjusting the composition, or it can be mixed with fresh active material, and then mixed with a conductive material, a binder, and a solvent to prepare a slurry for use.
[0095] Experimental examples of the present invention will now be described in detail.
[0096] <Experimental Example 1> FIG. 3 shows photographs of results at each stage according to an experimental example of the present invention.
[0097] Figure 3(a) is a photograph of shredded positive electrode scraps. Waste positive electrode scraps were collected and shredded into pieces of approximately 10 cm x 10 cm.
[0098] Figure 3(b) is a photograph of the cut cathode scraps. The shredded cathode scraps were further cut into strips measuring 1 cm x 1 cm.
[0099] Figure 3(c) is a photograph of the current collector pieces after the cut positive electrode scraps were crushed with a pin mill, and Figure 3(d) is a photograph of the active material layer in powder form detached from the current collector pieces after crushing with a pin mill. It can be seen that the active material layer is almost completely separated from the current collector by dry crushing such as with a pin mill.
[0100] FIG. 4 is an SEM photograph of the active material layer shown in FIG. 3(d), and FIG. 5 is an SEM photograph of the active material layer of FIG. 4 after heat treatment in air. The SEM photographs were taken with a normal SEM device used in a laboratory. For example, they can be taken with a HITACHI S-4200. However, there is no deviation due to the measurement device or method.
[0101] In Fig. 4, since the active material layer is prior to heat treatment, the binder is present in the active material layer and the active material layer has the form of aggregated particles, whereas in Fig. 5, the binder is removed by heat treatment and the aggregates are broken down. This shows that the binder and conductive material are removed by heat treatment in air alone as proposed in the present invention, and almost no binder or conductive material remains on the surface of the active material.
[0102] 6 is a SEM photograph of an active material that has been washed to remove LiF and then dried in the method for reusing an active material according to the present invention. When a lithium precursor is added to such an active material and annealed, a reused active material with almost the same shape as the fresh active material can be obtained.
[0103] <Experimental Example 2> The positive electrode scraps were prepared using a positive electrode active material made of NCM lithium composite transition metal oxide and using an LCO active material. The powdered active material was separated by a dry grinding step according to the method for reusing an active material according to the present invention, and then heat-treated in air at 550°C for 30 minutes. Some of the scraps were then immersed in an LiOH aqueous solution for 10 minutes to perform the cleaning step according to the method for reusing an active material according to the present invention, and the other scraps were not cleaned. The amount of remaining F was analyzed to determine the Li / metal molar ratio and the amount of remaining LiF in the active material, and the results are shown in Table 1.
[0104] Sample 1 is a fresh LCO active material. Sample 2 is an LCO positive electrode scrap that has been subjected to the above heat treatment but not washed. Sample 3 is an LCO positive electrode scrap that has been subjected to the above heat treatment and then washed.
[0105] Sample 4 is a fresh NCM active material. Sample 5 is NCM positive electrode scrap that was subjected to the above heat treatment but not washed. Sample 6 is NCM positive electrode scrap that was subjected to the above heat treatment and then washed.
[0106] [Table 1]
[0107] ND means that the measured value was 30 ppm or less. Samples 1 and 4 were fresh active materials, so almost no F was detected.
[0108] In Sample 2 and Sample 5, which were not washed, the amount of residual F was measured at 1900mg / kg and 1450mg / kg. However, in Sample 3 and Sample 6, which were washed, it was confirmed that LiF was completely dissolved in the washing solution and removed to the extent that it was not detectable. This shows that LiF is generated when LCO and NCM cathode scraps are heat treated, but is completely removed when the washing step is performed as proposed in the present invention.
[0109] Meanwhile, in samples 2 and 5, the Li / metal molar ratio is reduced by about 0.2 to 0.5 compared to samples 1 and 4, which are fresh active materials, and in samples 3 and 6, the Li / metal molar ratio is further reduced by about 0.2 to 0.5 compared to samples 2 and 5. In particular, in the case of NCM active material, the specific surface area of the particles is larger than that of LCO, and the reduction in the Li / metal molar ratio is likely due to the change to a spinel structure. That is, it can be confirmed that lithium is lost in the heat treatment step for removing the binder and the conductive material, and in the surface modification step by cleaning. Therefore, it is proposed that the method for reusing the active material according to the present invention includes a step of replenishing the missing lithium by adding a lithium precursor during annealing.
[0110] <Experimental Example 3> As the positive electrode scrap, positive electrode scrap having a composition of NCM lithium composite transition metal oxide:carbon black as a conductive material:PVdF as a binder=96.25:1.5:2.25 was prepared.
[0111] Comparative Example 1 is a fresh active material.
[0112] In Comparative Example 2 and Comparative Example 3, the positive electrode scraps were not dry-pulverized, and the positive electrode active material layer was present on the current collector, and the positive electrode scraps were heat-treated in air. The heat treatment was performed at 550°C for 30 minutes. The current collector was separated by the heat treatment, and the active material was recovered in powder form. In Comparative Example 2, the recovered active material was not washed. In Comparative Example 3, washing was performed.
[0113] In Comparative Example 4 and Example 1, the positive electrode scrap was dry-pulverized with a pin mill to separate the current collector and the active material layer, and then only the powder-form active material layer detached from the current collector was heat-treated in air. The heat treatment was performed at 550°C for 30 minutes, as in Comparative Examples 2 and 3. In Comparative Example 4, the recovered active material was not washed. In Example 1, washing was performed in the same manner as in Comparative Example 3.
[0114] In order to examine the Li / metal molar ratio and the content of remaining LiF in the active material, the amount of remaining F was analyzed. The results are shown in Table 2.
[0115] [Table 2]
[0116] The experimental results show that there is a slight difference in the amount of F remaining after heat treatment, but there is no significant difference in the amount of F remaining after cleaning. In addition, the measurement results of the Li / metal molar ratio are also at a similar level (within the error range of ±0.02) between Comparative Example 3 and Example 1, so it can be seen that the analytical values after cleaning are at a similar level even though the process of separating the initial electrode is different.
[0117] <Experimental Example 4> The positive electrode active materials were prepared according to the following examples and comparative examples, and their electrochemical performance was evaluated. 96.25 wt% of the positive electrode active materials recovered or prepared from the examples and comparative examples, 1.5 wt% of carbon black as a conductive material, and 2.25 wt% of PVdF as a binder were weighed and mixed with NMP to prepare a slurry to prepare a positive electrode, and then a coin half cell (CHC) was manufactured and its electrochemical performance was evaluated. The voltage was set to 3 to 4.3 V, and the initial formation charge and discharge was performed at 0.1 C / 0.1 C. The electrolyte constituting the cell was a carbonate-based electrolyte, with ethylene carbonate (EC): ethyl methyl carbonate (EMC) = 3: 7, containing some additives. The discharge conditions were 0.5 C / 1 C and 0.5 C / 2 C.
[0118] In Comparative Example 5, 0.1 mol of lithium precursor (Li2CO3) was added to Comparative Example 3 of Experimental Example 3, and annealed at 750°C for 5 hours. Then, H3BO3 was added to the surface protective layer so that the boron content was 500 ppm, and the surface coating was heat-treated at 300°C for 5 hours.
[0119] In Example 2, Example 1 of Experimental Example 3 was subjected to annealing and surface coating in the same manner as in Comparative Example 5.
[0120] The experimental results are shown in Table 3.
[0121] [Table 3]
[0122] As a result of the evaluation of electrical performance, Comparative Example 5 and Example 2 show the same level in initial capacity (0.1C / 0.1C) and also show the same level at high C-rate. That is, even if the initial current collector separation process is different, the same cell performance results can be obtained by using the same cleaning, lithium precursor addition annealing, and surface coating processes.
[0123] <Experimental Example 5> Positive electrode active materials were prepared according to the methods described below in the examples and comparative examples, and their electrochemical performance was evaluated.
[0124] Example 3 The reused active material was collected according to the method for reusing the active material of the present invention as described above. A cathode scrap to be discarded after punching out a cathode plate having an active material, which is an NCM-based lithium composite transition metal oxide, was prepared, and steps S20 and S25 were performed together to obtain a powdered active material layer. In step 30, heat treatment was performed in air at 550°C for 30 minutes. In step S40, cleaning was performed using LiOH for 10 minutes. In step S50, a lithium precursor (Li2CO3) was added in an amount that allowed lithium to be further added in a molar ratio of 0.09 based on the molar ratio of lithium to other metals in the raw active material (ICP analysis), and annealing was performed at 750°C for 15 hours. Theoretically, in the case of flash active materials, the molar ratio of lithium to other metals is 1:1, but since the average error of the ICP equipment used to confirm this is about ±0.05, preferably about ±0.02, the molar ratio of lithium to other metals in the raw active material measured by ICP may be 1±0.05:1. In this experiment, the lithium precursor was added based on the analysis ratio from the ICP analysis.
[0125] Example 4 In addition to Example 3, the recovery process of the surface protective layer of the active material in step S60 was also carried out.
[0126] Comparative Example 6 Instead of recycled active material, fresh NCM-based lithium composite transition metal oxide was used.
[0127] Comparative Example 7 As described above, in the method for reusing an active material of the present invention, only the heat treatment in step S30 was performed to remove the binder and conductive material. In the method for reusing an active material of the present invention, since step S25 was not performed, the Al current collector was separated during step S30. Step S30 was performed under the same conditions as in Example 3. In the method for reusing an active material of the present invention, the surface modification in step S40, the crystal structure recovery in step S50, and the surface coating process in step S60 were not performed.
[0128] Comparative Example 8 In addition to Comparative Example 7, the active material was collected after the surface modification step S40 of the method for reusing an active material of the present invention was further carried out. That is, the surface modification was carried out, but the crystal structure recovery step S50 and the surface coating step S60 of the method for reusing an active material of the present invention were not carried out. Step S40 was carried out under the same conditions as in Example 3.
[0129] Comparative Example 9 In addition to Comparative Example 7, in the method for reusing an active material according to the present invention as described above, the surface modification of step S40 was not performed, and only the crystal structure recovery of step S50 was performed to obtain an active material that is an NCM-based lithium transition metal composite oxide. Unlike Example 3, the annealing for recovering the crystal structure was performed without adding a lithium precursor.
[0130] Comparative Example 10 As in Example 3, only steps S30, S40, and S50 were performed, except for step S25, which was omitted. Annealing for crystal structure recovery was performed without adding a lithium precursor, unlike Example 3.
[0131] The positive electrode active materials recovered or prepared in the examples and comparative examples were subjected to ICP analysis to analyze the amount of remaining LiF, the ratio of lithium to other metals in the active material, and the amount of specific elements such as B and W.
[0132] The positive electrode active material recovered or prepared in each of the examples and comparative examples was weighed out at 96.25 wt%, the conductive carbon black was weighed out at 1.5 wt%, and the binder PVdF was weighed out at 2.25 wt%, and mixed with NMP to prepare a slurry to manufacture a positive electrode. Then, a coin half cell (CHC) was manufactured and its electrochemical performance was evaluated.
[0133] In order to confirm the amount of LiF remaining in the active materials recovered in Comparative Examples 7 and 8, F was detected and analyzed by ICP. The results are shown in Table 4 below.
[0134] [Table 4]
[0135] Referring to Table 4, it can be seen that the F content in the recovered positive active material was significantly lower in Comparative Example 8 than in Comparative Example 7. That is, it can be seen that LiF was completely dissolved in the lithium compound aqueous solution by washing and was removed to such an extent that it was not detectable by ICP. Therefore, it can be seen that the removal of LiF by step S40 is excellent.
[0136] In order to confirm whether there is a change in the lithium content in the positive electrode active material during steps S30 and S40 of the present invention, the ratio of lithium and other metals in the active material was analyzed by ICP, and the results are shown in Table 5 below.
[0137] [Table 5]
[0138] Referring to Table 5, it can be seen that the ratio of lithium to other metals is reduced by about 0.2 to 0.5 in Comparative Example 7 after heat treatment of S30 compared to Comparative Example 6, and by about 0.2 to 0.5 in Comparative Example 8 after washing and drying of S40 compared to Comparative Example 7. The NCM-based lithium transition metal composite oxide has a relatively large specific surface area of the particles, and the reduction in the ratio of lithium is greater than that of other metals due to the change to a spinel structure. Therefore, it can be seen that it is necessary to supplement the deficient lithium.
[0139] Table 5 shows values measured by ICP analysis, and as mentioned above, ICP analysis has an error value of about ±0.02. Therefore, even in Comparative Example 6, which is a flash active material, the ratio of lithium to other metals may be smaller than 1. Therefore, the amount of lithium precursor added to compensate for the lost lithium is the amount of lithium content added based on the ratio of lithium to other metals (molar ratio by ICP analysis) in the raw active material (i.e., flash active material) used in the active material layer.
[0140] 7 and 8 show the results of cell evaluation using active materials of the examples and comparative examples. The capacity was evaluated according to the number of cycles repeated at different currents, and the rate performance was evaluated. The evaluation was performed using a typical charge / discharge experimental device used in a laboratory. There was no deviation due to the measurement device or method. In the graphs of FIGS. 7 and 8, the horizontal axis is the number of cycles, and the vertical axis is the capacity.
[0141] The voltage was set to 3 to 4.3 V, and the initial formation charge and discharge was performed at 0.1 C / 0.1 C. The electrolyte that constitutes the cell was a carbonate-based electrolyte with an EC:EMC ratio of 3:7, containing some additives.
[0142] 7, after the first heat treatment (550° C. / 30 min) for removing the binder and conductive material, Comparative Example 7 before surface modification and Comparative Example 8 after surface modification show that the electrode capacity is rapidly reduced in Comparative Example 8 where the surface modification was performed. This is because, as described above, Ni in the NCM-based lithium transition metal composite oxide is converted to chlorination by moisture, resulting in a reduction in capacity.
[0143] However, when annealing (750°C / 15 hours) without surface modification is performed, which corresponds to Comparative Example 9, there is almost no effect of improving capacity in proportion to Comparative Example 7. This is because LiF remains on the surface of the active material when surface modification is not performed. Incidentally, it was explained in Table 4 that LiF can be removed to a satisfactory extent only by performing cleaning.
[0144] When surface modification and annealing are performed together after the first heat treatment, the capacity increases as seen in Comparative Example 10. This is because, although the capacity decreases after the surface modification step as in Comparative Example 8, the Ni rock salt is reduced by annealing after LiF is removed by the surface modification, and the structure is restored to a hexagonal crystal.
[0145] Next, referring to FIG. 8, the capacity improvement of Example 3 is confirmed compared to Comparative Example 10. Example 3, compared to Comparative Example 10, is characterized in that a lithium precursor was added during annealing. Thus, it can be seen that the capacity is improved by adding a lithium precursor to compensate for the lithium lost in the previous step. The fact that lithium is lost during the heat treatment and cleaning was explained with reference to Table 5.
[0146] The lithium compound was added in an amount equivalent to the loss in the lithium content of the existing positive electrode active material based on the ICP analysis (Table 5). As a result, it was confirmed by additional experiments that when a 0.09 to 0.1 molar ratio was added, the same level of capacity improvement effect as in Comparative Example 6 was achieved.
[0147] In this way, the present invention can recover active materials from cathode scraps at a level that allows them to be directly reused, is safe because it does not require the use of toxic and explosive solvents such as NMP, DMC, acetone, and methanol, and is suitable for mass production because it uses simple and safe methods such as heat treatment, washing and drying, and annealing.
[0148] As described above, according to the present invention, a cathode scrap can be reused using a simple, environmentally friendly, and economical method. Even if the cathode active material made of the thus-prepared NCM-based lithium transition metal composite oxide is reused as it is to manufacture a lithium secondary battery, there is no problem with the performance of the battery.
[0149] Although the present invention has been described above with reference to limited embodiments and drawings, it goes without saying that the present invention is not limited thereto, and various modifications and variations can be made by those having ordinary skill in the art to which the present invention pertains within the scope of the technical spirit of the present invention and the scope of the claims. [Explanation of symbols]
[0150] 10 Positive electrode current collector 20 Cathode active material layer 30 Positive electrode sheet 40 Positive plate 50 Cathode scrap
Claims
1. (a-1) dry-pulverizing a cathode scrap including a cathode active material layer made of a lithium composite transition metal oxide on a current collector to remove the active material layer in a powder form and separate it from the current collector; (a-2) recovering the active material by thermally treating the active material layer separated in a powder form in air to thermally decompose the binder and the conductive material in the active material layer; (b) washing the recovered active material with an aqueous solution of a lithium compound that is basic in an aqueous solution and drying it; (c) adding a lithium precursor to the washed active material and annealing it to obtain a reusable active material.
2. 2. The method of claim 1, further comprising the step of: (d) surface-coating the annealed active material.
3. 3. The method of claim 1, wherein the dry grinding is performed using any one of a pin mill, a disk mill, a cutting mill, and a hammer mill.
4. The method for reusing a positive electrode active material according to claim 1 , further comprising the step of shredding or cutting the positive electrode scrap before the dry grinding.
5. The method for reusing a positive electrode active material according to any one of claims 1 to 4, wherein the heat treatment is carried out at 300 to 1,000°C.
6. The method for reusing a positive electrode active material according to claim 1 , wherein the lithium compound aqueous solution is prepared to contain more than 0% and not more than 15% of a lithium precursor, and the washing is performed within one hour.
7. 7. The method for reusing a positive electrode active material according to claim 1, wherein the washing is performed by immersing the recovered active material in the aqueous lithium compound solution while stirring the aqueous solution.
8. The lithium precursor is LiOH, Li 2 CO 3 , LiNO 3 and Li 2 The method for reusing a positive electrode active material according to claim 1 , wherein the positive electrode active material is one or more of O.
9. 9. The method for reusing a positive electrode active material according to claim 1, wherein the lithium precursor is added in an amount sufficient to compensate for a ratio of lost lithium relative to a ratio of lithium and other metals in a raw active material used for the active material layer.
10. The method for reusing a positive electrode active material according to claim 9, wherein the lithium precursor is added in an amount such that the amount of lithium added is 0.001 to 0.4 molar ratio.
11. 10. The method of claim 9, wherein the lithium precursor further contains lithium in an amount of 0.0001 to 0.1 molar ratio based on a molar ratio of lithium to another metal of 1:
1.
12. The method for reusing a positive electrode active material according to any one of claims 1 to 11, wherein the annealing is carried out in air at 400 to 1,000°C.
13. The method for reusing a positive electrode active material according to claim 1 , wherein the temperature of the annealing step is a temperature exceeding the melting point of the lithium precursor.
14. 3. The method of claim 2, wherein the surface-coating step comprises coating the surface with at least one of a metal, an organometallic, and a carbon component in a solid or liquid phase manner, and then heat-treating the surface at 100 to 1,200° C.
15. The reusable active material is represented by the following chemical formula 1: Li a Ni xMn y Co z M w O 2+δ (Chemical formula 1) 15. The method of claim 1, wherein, in Formula 1, M is at least one selected from the group consisting of B, W, Al, Ti, and Mg, and 1<a≦1.1, 0≦x<0.95, 0≦y<0.8, 0≦z<1.0, 0≦w≦0.1, -0.02≦δ≦0.02, and x+y+z+w=1.
Citation Information
Patent Citations
Method for recovering and preparing lithium cobaltate from waste lithium ionic cell
CN101383442A
Recovery method of positive electrode leftover material of lithium-ion battery
CN105895854A
Method for producing recycled material
JP2012195073A
Processing method of used lithium ion battery
JP2016149330A
Positive electrode active material for nonaqueous electrolyte secondary battery, method of manufacturing the same, and nonaqueous electrolyte secondary battery
JP2017045633A