Surface light emission laser element and manufacturing method of surface light emission laser element
The surface-emitting laser device with a photonic crystal layer and optimized manufacturing method reduces cavity loss, enabling efficient operation at low threshold current density through enhanced optical coupling.
Patent Information
- Application Number
- JP2024110817
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2038-09-03
AI Technical Summary
Surface-emitting lasers with photonic crystals face high cavity loss, necessitating a low threshold current density for efficient operation.
A surface-emitting laser device with a photonic crystal layer and specific manufacturing method, including a first buried layer with pits at hole positions and a second buried layer to enhance optical coupling, reducing cavity loss and enabling low threshold current density operation.
The device achieves reduced cavity loss and operates at a low threshold current density by increasing the coupling coefficient, enhancing diffraction efficiency and resonance effects.
Smart Images

Figure 2024133145000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a surface-emitting laser element and a method for manufacturing the surface-emitting laser element. [Background technology]
[0002] In recent years, the development of surface emitting lasers using photonic crystals has progressed. For example, Patent Document 1 discloses a semiconductor laser element that is intended to be manufactured without fusion bonding.
[0003] Also, Patent Document 2 discloses a manufacturing method for producing a photonic crystal microstructure in a GaN-based semiconductor. Non-Patent Document 1 discloses the production of a photonic crystal by increasing the lateral growth rate through reduced pressure growth.
[0004] Furthermore, Non-Patent Document 2 discloses the in-plane diffraction effect and threshold gain difference of a photonic crystal laser, and Non-Patent Document 3 discloses a three-dimensional coupled-wave model of a square lattice photonic crystal laser. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 5082447 [Patent Document 2] Patent No. 4818464 [Non-patent literature]
[0006] [Non-Patent Document 1] H. Miyake et al. : Jpn. J. Appl. Phys.Vol.38(1999) pp.L1000-L1002 [Non-Patent Document 2] Tanaka et al., 2016 Autumn Applied Physics Society Proceedings 15p-B4-20 [Non-Patent Document 3] Y. Lian et al.:Phys. Rev.B Vol.84(2011)195119 Summary of the Invention [Problem to be solved by the invention]
[0007] In a surface-emitting laser equipped with a photonic crystal, it is necessary to reduce the cavity loss in order to perform oscillation operation at a low threshold current density. In order to reduce the cavity loss in a photonic crystal surface-emitting laser, it is effective to increase the coupling coefficient (one-dimensional coupling coefficient: κ3) of the light wave propagating in a direction parallel to the photonic crystal layer.
[0008] The present invention has been made in consideration of the above-mentioned points, and aims to provide a surface-emitting laser equipped with a photonic crystal, which has a large coupling coefficient with respect to light waves propagating through a photonic crystal layer and is capable of oscillating at a low threshold current density, and a method for manufacturing the same. [Means for solving the problem]
[0009] A surface-emitting laser element according to one embodiment of the present invention is a surface-emitting laser element made of a group III nitride semiconductor, a first cladding layer of a first conductivity type; a first guide layer of a first conductivity type, the first guide layer including: a photonic crystal layer formed on a first clad layer, the photonic crystal layer having holes arranged with two-dimensional periodicity in a plane parallel to the layer; and a first burying layer formed on the photonic crystal layer to close the holes; a second buried layer crystal-grown on the first buried layer; an active layer formed on the second buried layer; a second guide layer formed on the active layer; A second clad layer of a second conductivity type opposite to the first conductivity type is formed on the second guide layer. a layer; The surface of the first buried layer has pits disposed at surface positions corresponding to the voids.
[0010] A method for manufacturing a surface emitting laser element according to another embodiment of the present invention includes the steps of: (a) growing a first cladding layer of a first conductivity type on a substrate; (b) growing a first guiding layer of a first conductivity type on the first cladding layer; (c) forming holes in the first guide layer by etching, the holes being arranged with two-dimensional periodicity in a plane parallel to the first guide layer; (d) supplying a gas containing a nitrogen source to form a first buried layer by mass transport to close the opening of the hole; (e) after the formation of the first buried layer, supplying a group III source to form a second buried layer that fills and flattens the first buried layer, In the above step (d), the surface of the first buried layer has pits resulting from the voids. [Brief description of the drawings]
[0011] [Figure 1] 1 is a cross-sectional view showing a schematic example of the structure of a surface-emitting laser element including a photonic crystal layer according to an embodiment of the present invention. [Diagram 2] 2 is an enlarged cross-sectional view showing a schematic diagram of the photonic crystal layer of FIG. 1 and holes (cavities) arranged in the photonic crystal layer. FIG. [Diagram 3] 4 is a cross-sectional view that illustrates a process of forming holes CH. FIG. [Figure 4A] 13 is a diagram showing an SEM image of the surface of the guide layer substrate in a process after the formation of holes CH. FIG. [Figure 4B] 13 is a diagram showing an SEM image of a cross section of a guide layer substrate in a process after the formation of holes CH. FIG. [Figure 5A] 13 is a diagram showing a cross-sectional SEM image of a portion of the n-guide layer 14 where voids CH are filled. FIG. [Figure 5B] FIG. 5B is a diagram showing a schematic cross section shown in FIG. 5A. [Figure 6A] 1 is an AFM image showing the surface morphology of a first buried layer 14A. [Figure 6B]6B is a graph showing the surface roughness of a cross section taken along line AA in FIG. 6A. [Figure 6C] 6B is a graph showing the surface roughness of a cross section taken along line BB in FIG. 6A. [Figure 7A] 13 is a diagram showing a cross-sectional SEM image of a portion of the n-guide layer 14 where holes 14C are filled. FIG. [Figure 7B] FIG. 7B is a diagram showing a schematic cross section shown in FIG. 7A. [Figure 8A] 2 is an AFM image showing the surface morphology of the second burying layer 21. [Figure 8B] 8B is a graph showing the surface roughness of a cross section taken along line AA in FIG. 8A. [Figure 9] FIG. 13 is a diagram showing a cross-sectional structure of a GaN-based photonic crystal surface-emitting laser element used for calculating an optical coupling coefficient κ3 by a coupled-wave equation. [Figure 10A] 13 is a graph showing the change in coupling coefficient κ3 relative to the layer thickness DP of buried layer 14D (the distance between active layer 15 and photonic crystal layer 14P). [Figure 10B] 13 is a graph showing the change in threshold gain with respect to the layer thickness DP of the buried layer 14D. [Figure 11] FIG. 13 is a schematic diagram showing a method of filling holes, which is a comparative example of the present embodiment. [Figure 12] 4 is a graph showing the results of a SIMS analysis of the semiconductor structure layer 11 of the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] In the following, preferred embodiments of the present invention will be described, which may be modified and combined as appropriate. In the following description and accompanying drawings, substantially the same or equivalent parts are designated by the same reference numerals. [Threshold gain of photonic crystal surface-emitting lasers] Generally, in a photonic crystal surface emitting laser (hereinafter also simply referred to as a photonic crystal laser), the diffraction efficiency of a diffraction grating inside a resonator is represented by a coupling coefficient κ, and the larger the coupling coefficient κ, the smaller the threshold gain.
[0013] In a photonic crystal surface emitting laser, light waves propagating in a plane parallel to the photonic crystal layer are diffracted not only in the ±180° direction but also in the ±90° direction with respect to the light wave propagation direction. Therefore, in addition to the optical coupling coefficient κ3 (one-dimensional coupling coefficient) of the light waves propagating in the ±180° direction, the optical coupling coefficient κ 2D (2-dimensional coupling coefficient) exists.
[0014] That is, in a surface-emitting laser with a photonic crystal, the light waves propagating in the plane are diffracted by the diffraction effect of the photonic crystal, forming a two-dimensional resonance mode. Here, if the components of light that are not diffracted by the photonic crystal leak in the in-plane direction, the cavity loss increases, leading to an increase in the threshold gain. Therefore, if this cavity loss can be suppressed, the threshold gain can be reduced, and oscillation can be performed at a low threshold current density.
[0015] In order to reduce the cavity loss in a photonic crystal surface emitting laser and achieve oscillation at a low threshold current density, it is effective to increase the coupling coefficient (κ3) of the light wave propagating within the photonic crystal layer plane. [An example of the structure of a photonic crystal surface-emitting laser] FIG. 1 is a cross-sectional view showing a schematic example of a structure of a surface-emitting laser element (hereinafter, simply referred to as a photonic crystal laser) 10 having a photonic crystal layer. As shown in FIG. 1, a semiconductor structure layer 11 is formed on a substrate 12. More specifically, an n-clad layer 13, an n-guide layer 14 including a first buried layer 14A, a second buried layer 21, an active layer 15, a guide layer 16, an electron barrier layer (EBL: Electron Blocking Layer) 17, and a p-clad layer 18 are formed in this order on the substrate 12. That is, the semiconductor structure layer 11 is composed of semiconductor layers 13, 14, 15, 16, 17, and 18. The n-guide layer 14 includes a photonic crystal layer 14P. The semiconductor structure layer 11 is made of a hexagonal nitride semiconductor. For example, it is made of a GaN-based semiconductor.
[0016] In addition, an n-electrode 19A is formed on the back surface of substrate 12, and a p-electrode 19B is formed on the top surface of p-cladding layer 18. For example, p-electrode 19B can be formed in an appropriate shape such as a circular ring surrounding the photonic crystal region.
[0017] In this case, light from the surface-emitting laser element 10 is extracted in a direction perpendicular to the active layer 15 from the upper surface of the semiconductor structure layer 11 (that is, the surface of the p-cladding layer 18) to the outside.
[0018] In addition, the light from the surface-emitting laser element 10 can be extracted to the outside from the lower surface side of the semiconductor structure layer 11. In this case, for example, the n-electrode 19A can be formed in a circular ring shape, and the p-electrode 19B can be provided in a position opposite to the center of the n-electrode 19A.
[0019] Fig. 2 is an enlarged cross-sectional view showing photonic crystal layer 14P and holes (cavities) 14C arranged in photonic crystal layer 14P in Fig. 1. Holes 14C are formed in the crystal growth plane (semiconductor layered plane), i.e., in a plane (AA cross section in the figure) parallel to n-guide layer 14, with a period PC of, for example, a square lattice, two-dimensionally arranged at square lattice points and embedded in n-guide layer 14. The arrangement of holes 14C is not limited to a square lattice, and may be any periodic two-dimensional arrangement such as a triangular lattice or hexagonal lattice.
[0020] N-guide layer 14 is a semiconductor layer on the upper surfaces of two-dimensionally arranged holes 14C (i.e., a semiconductor layer whose bottom surface is the upper surfaces of holes 14C), and is composed of first embedded layer 14A in which photonic crystal layer (PCL) 14P is embedded, photonic crystal layer (PCL) 14P, and base layer 14B which is a crystal layer closer to the substrate than photonic crystal layer (PCL) 14P. In addition, second embedded layer 21 is formed on first embedded layer 14A. [Resonance effect of photonic crystal surface-emitting laser] In order to obtain a resonance effect in a surface emitting laser having a photonic crystal portion (hereinafter sometimes simply referred to as a photonic crystal surface emitting laser), it is desirable for the diffraction effect in the photonic crystal portion to be high.
[0021] That is, in order to enhance the diffraction effect in a photonic crystal surface emitting laser, (1) Let λ be the oscillation wavelength and n be the effective refractive index of the photonic crystal. eff Then, the two-dimensional refractive index period P in the photonic crystal part is P=mλ / n in the case of a square lattice two-dimensional photonic crystal. eff (m is a natural number), and in the case of a triangular lattice two-dimensional photonic crystal, P = mλ × 2 / (3 1 / 2 ×n eff ) (m is a natural number), (2) The ratio of the modified refractive index area to the base material in the photonic crystal portion (FF: filling factor) is sufficiently large. (3) The ratio of the light intensity distributed in the photonic crystal part to the light intensity distribution in the photonic crystal surface emitting laser (Γ PC It is desirable that the confinement factor (Tc) is sufficiently large.
[0022] In order to satisfy the above (1), it is necessary to appropriately set the lattice constant (period PC) of the photonic crystal in accordance with the oscillation wavelength of the photonic crystal laser. Here, since the refractive index period P = period PC, PC can be set based on P that satisfies the above (1). For example, when oscillating at a wavelength of 405 nm using a gallium nitride-based material, n eff is about 2.5, so when a square lattice two-dimensional photonic crystal is used, the lattice constant should be set to about 163 nm.
[0023] In a two-dimensional photonic crystal with a square lattice, the direction in which light waves are diffracted is the same as the direction of the lattice arrangement, but in a two-dimensional photonic crystal with a triangular lattice, light waves are diffracted in a direction tilted by 30 degrees from the direction of the lattice arrangement. As a result, in the above (1), the P that a two-dimensional photonic crystal with a triangular lattice satisfies is 2 / 3 1 / 2 is multiplied. EXAMPLES
[0024] [Growth of cladding and guide layers] The following is a detailed description of the steps for fabricating the semiconductor structure layer 11. The semiconductor structure layer 11 was grown on the growth substrate 12 by normal pressure (atmospheric pressure) growth using MOVPE (Metalorganic Vapor Phase Epitaxy) as a crystal growth method.
[0025] An n-type GaN substrate 12 with a growth surface of +c-plane and a c-axis inclined 0.4° along the a-axis was used as a substrate for growing the semiconductor structure layer 11. The inclination (off-angle) of the c-axis may be changed as appropriate within the range in which epitaxial growth is possible in GaN-based semiconductors. On the substrate 12, n-type AlGaN (layer thickness: 2 μm) with an Al (aluminum) composition of 4% was grown as the n-cladding layer 13. III Trimethylgallium (TMG) and trimethylaluminum (TMA) were used as the group V MO (metal organic) materials, and ammonia (NH3) was used as the group V material. Silane (SiH4) was also supplied as the doping material. The carrier density at room temperature was approximately 2×10 18 cm -3 It was.
[0026] Next, TMG and NH3 were supplied to grow n-type GaN (layer thickness: 300 nm) as the n-guide layer 14. Silane (SiH4) was also supplied simultaneously with the growth to perform doping. The carrier density was approximately 2×10 18 cm -3 It was. [Hole formation in guide layer] The substrate after the growth of the n-guide layer 14, i.e., the substrate with the n-guide layer 14 (hereinafter also referred to as the guide layer substrate), was taken out of the MOVPE apparatus, and fine voids (holes) were formed in the n-guide layer 14. The formation of the voids will be described in detail below with reference to FIG. 3, FIG. 4A, and FIG. 4B. FIG. 3 is a cross-sectional view that typically illustrates the process of forming the voids CH. FIG. 4A and FIG. 4B respectively show scanning electron microscope (SEM) images of the surface and cross section of the guide layer substrate in the process after the formation of the voids CH. FIG. 4B shows a cross-sectional SEM image along the dashed line (white) shown in the surface SEM image of FIG. 4A.
[0027] The guide layer substrate, on which the n-cladding layer 13 and the n-guide layer 14 were grown on the substrate 12, was cleaned to obtain a clean surface (FIG. 3, (i)). After that, a silicon nitride film (SiNx) SN (thickness: 110 nm) was formed by plasma CVD (FIG. 3, (ii)).
[0028] Next, a resist RZ for electron beam (EB) lithography was applied to the SiNx film SN by spin coating to a thickness of about 300 nm, and then placed in an electron beam lithography device to form a pattern with a two-dimensional periodic structure on the surface of the guide layer substrate (Figure 3, (iii)). More specifically, a pattern was performed in which circular dots with a diameter of 100 nm were arranged two-dimensionally in the plane of the resist RZ in a square lattice shape with a period PC = 163 nm.
[0029] After developing the patterned resist RZ, the SiNx film SN was selectively dry etched using an ICP-RIE (Inductive Coupled Plasma - Reactive Ion Etching) device (Fig. 3, (iv)). As a result, cylindrical through-holes arranged two-dimensionally in a square lattice shape with an in-plane periodicity PC were formed in the SiNx film SN.
[0030] Next, the resist RZ was removed, and the patterned SiNx film SN was used as a hard mask to form vacancies CH extending from the surface to the inside of the n-guide layer 14 (GaN). More specifically, two-dimensionally arranged vacancies CH were formed in the n-guide layer 14 by dry etching using a chlorine-based gas in an ICP-RIE apparatus (Fig. 3, (v)).
[0031] A surface SEM image and a cross-sectional SEM image of the voids CH formed in the n-guide layer 14 at this time are shown in Figures 4A and 4B, respectively. As shown in the surface SEM image, a plurality of voids CH were formed, which were arranged two-dimensionally in a square lattice pattern (i.e., square lattice points) with a void interval (period) PC of 163 nm between the voids. Also, as shown in the cross-sectional SEM image in Figure 4B, the voids CH formed in the n-guide layer 14 had a depth of about 150 nm and a diameter of about 100 nm. That is, the voids CH were holes that opened on the upper surface and had a substantially cylindrical shape. [First buried layer] The SiNx film SN of the guide layer substrate, in which two-dimensional periodic vacancies CH were formed in the n-guide layer 14, was removed using hydrofluoric acid (HF) (Figure 3, (vi)), and the substrate was cleaned to obtain a clean surface, and then reintroduced into the MOVPE apparatus.
[0032] In the MOVPE apparatus, the temperature was raised while supplying NH3 as a nitrogen source without supplying III-group raw materials, the guide layer substrate was heated to 1150°C, and annealing was performed for 1 minute (1 min) after the temperature was raised, thereby filling the vacancies CH by mass transport and forming the first buried layer 14A. Nitrogen (N2) was supplied as the atmospheric gas.
[0033] A cross-sectional SEM image of the portion of n-guide layer 14 where voids CH are filled is shown in Fig. 5A, and a schematic cross-sectional view thereof is shown in Fig. 5B. As shown in Fig. 5A and Fig. 5B, a hexagonal columnar void (cavity) 14C was formed with an inner surface consisting of a {10-11} facet (a facet with a specified plane orientation), a width (WC) of 70 nm, and a depth (HC) of 118 nm. More specifically, a (000-1) plane appeared on the surface (top surface) of void 14C facing active layer 15, a {10-10} plane appeared on the side surface of void 14C, and a {1-102} facet appeared on the bottom on the substrate 12 side.
[0034] At this time, a first buried layer 14A was formed on the n-guide layer 14, extending from the plane formed by the upper surfaces of the holes 14C to the surface of the n-guide layer 14. The thickness (D1) of the first buried layer 14A was 26 nm.
[0035] Fig. 6A is an atomic force microscope (AFM) image showing the surface morphology of the first burying layer 14A, Fig. 6B is a graph showing the surface roughness of a cross section taken along line AA in Fig. 6A, and Fig. 6C is a graph showing the surface roughness of a cross section taken along line BB in Fig. 6A. It was confirmed that the surface of the first burying layer 14A was composed of a GaN (0001) plane, and had a step-terrace structure bunched with a width equivalent to the period PC (=163 nm).
[0036] 6A, it was confirmed that pits PT appeared in a square lattice pattern at the period of the vacancies 14C on the surface of the first buried layer 14A at surface positions corresponding to the vacancies 14C. That is, it was confirmed that the pits PT appeared on the crystal orientation
[0001] relative to the vacancies 14C, and in this embodiment, when the first buried layer 14A is viewed from above, the pits PT appeared at positions overlapping the vacancies 14C. That is, the pits PT originating from or caused by the vacancies 14C appeared on the surface of the first buried layer 14A. Note that, when the off-angle of the crystal is large, when the first buried layer 14A is viewed from above, the pits PT may not overlap the vacancies 14C, but appear on the crystal orientation
[0001] relative to the vacancies 14C.
[0037] In the formation of the first embedded layer 14A, the pits PT do not need to be arranged in a two-dimensional regular pattern on the surface of the first embedded layer 14A. It is sufficient that the first embedded layer 14A is formed by mass transport so that the surface of the first embedded layer 14A has a surface state in which the pits PT remain.
[0038] The first embedded layer 14A is not limited to GaN. The first embedded layer 14A may be formed of other crystals, for example, a GaN-based semiconductor crystal layer of a ternary crystal or a quaternary crystal, and preferably has a higher refractive index than the n-cladding layer 13. For example, AlGaN, InGaN, or the like having a lower Al composition than the n-cladding layer 13 may be used. [Second buried layer] After the first buried layer 14A was formed, the second buried layer 21 was formed by supplying a group III material gas (TMG) and a group V material gas (NH3) while maintaining the temperature at 1150° C. In this embodiment, hydrogen (H2) was supplied at the same time.
[0039] FIG. 7A shows a cross-sectional SEM image of the portion of n-guide layer 14 where holes 14C are filled, and FIG. 7B shows a schematic cross-sectional view thereof.
[0040] The second burying layer 21 could be formed without changing the shape of the holes 14C. In this case, the sum of the thickness of the first burying layer 14A (D1=26 nm) and the thickness of the second burying layer 21 (D2=34 nm) was 60 nm.
[0041] 8A and 8B are an AFM image showing the surface morphology of the second buried layer 21 and a graph showing the surface roughness of a cross section taken along line AA in FIG. 8A, respectively.
[0042] As shown in FIG. 8B, the surface of the second burying layer 21 has a step-terrace structure with a step height of one GaN bilayer, and it was confirmed that an atomically flat GaN (0001) surface was obtained.
[0043] As described above, in the formation of the first embedded layer 14A, the embedding by mass transport is completed and the first embedded layer 14A is formed so that the surface state of the first embedded layer 14A has pits PT appearing on it. Note that the first embedded layer 14A is preferably formed so that the surface of the first embedded layer 14A has pits PT remaining regularly arranged at least partially.
[0044] This is because, when the first buried layer 14A is formed, the pits PT are completely filled with migration atoms and / or molecules made of Ga and / or GaN during mass transport, and the surface condition becomes equivalent to that of other parts. Then, the migration atoms and / or molecules aggregate in the parts of the first buried layer 14A that have defects or dislocations remaining therein, forming hillocks (convex portions) and hindering the planarization of the second buried layer 21.
[0045] In addition, if the pits PT serve as starting points for the growth (regrowth) of the second embedded layer 21, or if the surface condition is such that the pits PT remain even if not necessarily regular, then the second embedded layer 21 can be made uniform and flat.
[0046] In order to fill in the pits PT and flatten the surface, the thickness of the second buried layer 21 is preferably greater than the thickness of the first buried layer 14A.
[0047] Although the case where GaN is grown as the second buried layer 21 has been described as an example, the crystal composition of the second buried layer 21 may be different from that of the first buried layer 14A. The second buried layer 21 may be formed of other crystals, for example, a GaN-based semiconductor crystal layer of a ternary crystal or a quaternary crystal. For example, a crystal layer containing In in its composition, such as an InGaN layer, may be used as the second buried layer 21. In addition, by forming a crystal layer having a higher refractive index for the emission wavelength than the first buried layer as the second buried layer 21, the coupling coefficient κ3 can be made larger than that of a GaN crystal layer. The temperature for forming the second buried layer 21 is preferably within a range of 750° C. to 1150° C. when the constituent material is GaN, and 750° C. to 900° C. when the constituent material is InGaN. [Growth of active layer and p-side semiconductor layer] Next, a multiple quantum well (MQW) layer was grown as the active layer 15. The barrier layer and well layer of the MQW were GaN and InGaN, respectively. The barrier layer was grown by lowering the temperature of the substrate to 800°C, and then supplying triethylgallium (TEG) as a group III atom source and NH3 as a nitrogen source. The well layer was grown at the same temperature as the barrier layer, and by supplying TEG and trimethylindium (TMI) as group III atom sources and NH3 as a nitrogen source. The center wavelength of the PL (Photoluminescence) emission from the active layer 15 in this example was 410 nm.
[0048] After the active layer 15 was grown, the substrate was kept at 800° C., and the p-side guide layer 16 was grown to a thickness of 100 nm. The p-side guide layer 16 was grown as undoped GaN (u-GaN) without doping with a dopant by supplying TEG and NH3.
[0049] After the growth of the p-side guide layer 16, the substrate temperature was raised to 1050°C at a high speed, and the electron barrier layer (EBL) 17 and the p-cladding layer 18 were grown. The growth of the EBL 17 was performed by supplying TMG and TMA as group III atom sources and NH3 as a nitrogen source. The growth of the p-cladding layer 18 was performed by supplying TMG and TMA as group III atom sources and NH3 as a nitrogen source. The Al concentrations of the EBL 17 and the p-cladding layer 18 were 18% and 6%, respectively, and the layer thicknesses were 17nm and 600nm. During the growth of the EBL 17 and the p-cladding layer 18, Cp2Mg (Bis-cyclopentadienyl magnesium) was supplied as a dopant simultaneously with the group III atom source gas and the nitrogen source. The carrier density of the p-cladding layer (p-AlGaN cladding layer) 18 after activation at 700°C for 5 minutes in air was 4×10 17 cm -3 It was. [Coupling coefficient κ3] As described above, in order to reduce the cavity loss in a photonic crystal surface emitting laser and achieve oscillation at a low threshold current density, it is effective to increase the coupling coefficient κ3 of the light wave propagating within the plane of photonic crystal layer 14P.
[0050] To examine this point, the optical coupling coefficient κ3 was calculated by solving the coupled-wave equation for a GaN-based photonic crystal surface-emitting laser element having the structure shown in FIG.
[0051] The photonic crystal surface emitting laser used in the calculation of the optical coupling coefficient κ3 shown in FIG. 9 has an n-cladding layer 13 (n-Al 0.04 Ga 0.96 N: layer thickness 2,000 nm), n-guide layer 14 (n-GaN: layer thickness 120 nm), photonic crystal layer 14P (n-GaN: layer thickness 120 nm), buried layer 14D (n-GaN: layer thickness DP = 0 to 120 nm), active layer 15 (quantum well layer (u-In 0.08 Ga 0.92 N) is a two-layer MQW), p-side guide layer 16 (u-GaN: layer thickness 120 nm), EBL 17 (p-Al 0.18 Ga 0.82 N: layer thickness 17 nm), p-cladding layer 18 (p-Al 0.06 Ga 0..94 N: layer thickness 600 nm) are laminated in this order.
[0052] 10A and 10B show the change in coupling coefficient κ3 and threshold gain, respectively, with respect to thickness DP of buried layer 14D, i.e., the distance between active layer 15 and photonic crystal layer 14P, for a filling factor (FF) of 6%.
[0053] 10A and 10B, in order to increase coupling coefficient κ3 and perform oscillation at a low threshold current density, it is preferable that the total thickness DP of first embedding layer 14A and second embedding layer 21 (or the distance between active layer 15 and photonic crystal layer 14P) is 100 nm or less. Moreover, it is preferable that the total thickness is within the range of 20 nm to 100 nm.
[0054] As described above, in this embodiment, a guide layer substrate in which holes CH having two-dimensional periodicity are formed in the n-guide layer 14 is (i) annealing while supplying a gas containing a nitrogen source to fill the openings of the voids by mass transport to form a first buried layer; (ii) A gas containing a group III source and a nitrogen source is supplied to form a first buried layer.
[0055] When the temperature is raised to the temperature at which mass transport occurs, the shape of the vacancies changes so that the surface energy becomes the smallest. That is, for example, the side of the vacancies in c-plane GaN is transformed into the {10-10} plane with a small dangling bond density. Also, the vacancies are blocked by annealing, and a first buried layer with a surface composed of a (0001) plane is formed. At this time, the surface of the first buried layer has a step-terrace structure bunched with a width equal to the periodic interval of the vacancies. Since the annealing temperature is the temperature at which mass transport occurs, the annealing temperature for blocking the vacancies CH is preferably within the range of 1000°C to 1200°C when the n-guide layer is composed of GaN.
[0056] Moreover, the first buried layer is made of the same element as the n-guide layer in which the voids are formed.
[0057] The second buried layer is newly grown by supplying group III materials. Therefore, unlike the first buried layer, it does not need to be made of the same elements as the n-guide layer in which holes are formed. However, from the viewpoint of optical confinement, it is preferable that the second buried layer is made of a material having a refractive index equal to or higher than that of the first buried layer.
[0058] The bunched surface structure of the first buried layer is restored by the second buried layer, resulting in a step-and-terrace surface with a step height of 1 bilayer, and therefore the surface of the second buried layer becomes an atomically flat (0001) surface.
[0059] By using the above method, the distance between the photonic crystal layer and the active layer in a GaN-based photonic crystal surface-emitting laser can be set to 100 nm or less. That is, in a GaN-based photonic crystal surface-emitting laser, the optical coupling coefficient κ3 can be increased, and a photonic crystal surface-emitting laser capable of oscillating at a low threshold current density can be realized. [Comparative Example of Hole Filling Method and Structure] Fig. 11 is a schematic diagram showing a void filling method, which is a comparative example of the above-mentioned embodiment. The SiNx film SN of the guide layer substrate in which voids CH having two-dimensional periodicity are formed in the n-guide layer 14 is removed using hydrofluoric acid (HF), cleaned to obtain a clean surface, and then introduced again into the MOVPE apparatus, as in the above-mentioned embodiment (Fig. 11(a)).
[0060] In this comparative example, the guide layer substrate was heated to 1050°C in an MOVPE apparatus, and Group III material gas (TMG) and Group V material gas (NH3) were supplied to perform crystal growth so as to form recesses having {10-11} facets on the substrate surface, thereby blocking the openings of the vacancies CH (Figure 11(b)).
[0061] At this time, the distance E1 between the (000-1) plane, which is the upper surface of the buried hole CH, and the (0001) plane, which is the outermost surface of the n-guide layer 14, was approximately 140 nm (FIG. 11(b)).
[0062] After the vacancies CH were blocked by the {10-11} facets, the supply of the group III material gas was stopped, and the temperature was raised to 1150°C at a heating rate of 100°C / min while supplying group V material gas (NH3), and the temperature was maintained for 1 minute. As a result, the {10-11} facets formed on the surface of the n-guide layer 14 disappeared, and the surface became a flat (0001) surface. In other words, the surface was flattened by mass transport.
[0063] At this time, the distance E2 between the surface (upper surface, (000-1) surface) of the buried void (cavity) 14C facing the active layer 15 and the surface (i.e., the (0001) surface) of the n-guide layer 14 was approximately 105 nm.
[0064] That is, according to the hole filling method of this comparative example, the {10-11} facet grows preferentially to close the holes, and then annealing is performed to form a (0001) surface. With this manufacturing method, the distance between photonic crystal layer 14P and active layer 15 can be reduced to only about 100 nm. That is, with this method, it is not possible to increase the optical coupling coefficient κ3 in a GaN-based photonic crystal surface-emitting laser, and it is difficult to achieve oscillation operation at a low threshold current density. [Crystallinity: SIMS analysis] When the voids CH are formed in the n-guide layer 14 by etching, oxygen is taken in, and therefore oxygen is unintentionally taken in the first buried layer as well.
[0065] In the above embodiment, the second buried layer 21 is formed by supplying a group III material gas (TMG), a group V material gas (NH3), and hydrogen (H2), so that the amount of oxygen unintentionally incorporated into the second buried layer 21 is drastically reduced. For example, the amount of oxygen unintentionally incorporated into the second buried layer 21 is 5×10 16 cm -3 The result is as follows.
[0066] The results of SIMS (Secondary Ion Mass Spectrometry) analysis of the semiconductor structure layer 11 of this embodiment formed as described above are shown in Fig. 12. Fig. 12 shows the analysis results from a part of the p-cladding layer 18 to a part of the n-cladding layer 13. As shown in the concentration profile of oxygen (O), the first buried layer 14A contains 3 x 10 oxygen atoms mixed in during etching to form the vacancies CH. 18 m -3 The oxygen concentration in the second buried layer 21 is 2×10 16 cm -3 It was confirmed that the levels were below the detection limit.
[0067] Thus, it was confirmed that the generation of group III atomic vacancies in the crystal due to high-concentration oxygen doping is suppressed in the second embedding layer 21, and a film with good crystallinity is obtained. Therefore, the crystal layer grown on the second embedding layer 21 also has good crystallinity.
[0068] It should be noted that the various numerical values in the above embodiment are merely examples and can be appropriately changed without departing from the scope of the present invention.
[0069] In the above embodiment, the semiconductor structure layer 11 has the electron barrier layer 17, but the semiconductor structure layer 11 does not have to have the electron barrier layer 17. Alternatively, the semiconductor structure layer 11 may include a contact layer, a current diffusion layer, or other semiconductor layers.
[0070] In addition, in this specification, a case has been described in which a first conductivity type semiconductor (n-type semiconductor), an active layer, and a second conductivity type semiconductor (p-type semiconductor having an opposite conductivity type to the first conductivity type) are grown in that order, but the first conductivity type may be p-type and the second conductivity type may be n-type.
[0071] As described above in detail, according to the present invention, it is possible to provide a surface-emitting laser and a manufacturing method thereof that can increase the coupling coefficient κ3 of light waves propagating in a direction parallel to the photonic crystal layer, reduce cavity loss, and perform oscillation operation at a low threshold current density. [Explanation of symbols]
[0072] 10: Photonic crystal surface emitting laser 12: Substrate 13: n-cladding layer 14: n-guide layer 14A: First buried layer 14P: Photonic crystal layer 14C: Vacancy 15:Active layer 16: Guide layer 18: p-cladding layer 21: Second buried layer
Claims
[Claim 1] A surface-emitting laser element comprising a substrate and a hexagonal semiconductor structure layer provided on the substrate, the surface-emitting laser element emitting light from an upper surface side or a lower surface side of the semiconductor structure layer, The semiconductor structure layer is a first cladding layer of a first conductivity type; a first guide layer of the first conductivity type formed on the first clad layer, the first guide layer comprising: a photonic crystal layer having a plurality of holes arranged with two-dimensional periodicity in a plane parallel to the layer, a base layer located below the photonic crystal layer and in contact with the photonic crystal layer, and a first buried layer located above the photonic crystal layer and closing openings of the holes; a second buried layer formed on the first guide layer; an active layer formed on the second buried layer; a second guide layer formed on the active layer; a second clad layer of a second conductivity type formed on the second guide layer, the base layer, the photonic crystal layer, and the first buried layer are composed of the same element; a total thickness of the first buried layer and the second buried layer is 100 nm or less; A surface-emitting laser element, wherein the oxygen concentration in the second buried layer is smaller than the oxygen concentration in the photonic crystal layer.
Citation Information
Patent Citations
Photonic crystal built-in substrate, manufacturing method thereof, and surface-emitting quantum cascade laser device
CN110011182A
P-type group iii nitride semiconductor, its manufacturing method, and manufacturing method of semiconductor light emitting device using p-type group iii nitride semiconductor
JP2001298030A
Group iii nitride semiconductor crystal substrate and semiconductor device
JP2009126722A
Semiconductor element, semiconductor device, semiconductor wafer, and method of growing semiconductor crystal
JP2010219269A
Gallium nitride-based semiconductor optical device, and method of fabricating the same
JP2011023536A