Diffuser and manufacturing method thereof
The gas diffuser, made from combustion ash and a binder, addresses the high manufacturing and maintenance costs of existing diffusers by providing an efficient, low-cost solution for microbubble generation.
Patent Information
- Application Number
- JP2024116691
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-10-17
AI Technical Summary
Existing diffuser plates, such as those made from thin metal or ceramic materials, are costly and time-consuming to manufacture, and require frequent replacement, leading to high maintenance costs.
A gas diffuser composed of a porous body containing combustion ash and a binder, which can be easily manufactured using inexpensive raw materials and optimized composition and firing conditions to produce microbubbles efficiently.
The diffuser achieves low-cost manufacturing and efficient microbubble generation with a pressure resistance of 0.2 MPa and a flow rate of 200L/min, reducing material costs and environmental impact.
Smart Images

Figure 2024133336000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an air diffuser and a method for manufacturing the same. [Background technology]
[0002] There is known an air diffuser plate that receives gas from the outside and releases fine air bubbles into liquid. Air diffuser plates are used in various fields, such as neutralization treatment of concrete wastewater and aeration in aquaculture farms. Ceramic air diffuser plates are widely used as air diffuser plates. Patent Document 1 discloses an air diffuser plate in which a plurality of air diffuser holes are formed in a thin metal plate. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2010-158631 A Summary of the Invention [Problem to be solved by the invention]
[0004] The air diffuser plate of Patent Document 1 is manufactured by processing a thin metal plate, and therefore has problems of laborious manufacturing and high manufacturing costs, and ceramic air diffuser plates have similar problems. Air diffuser plates are consumables and need to be replaced at regular intervals to maintain their performance, so it is desired that they be available at the lowest possible cost. Such problems are not limited to air diffuser plates, but also exist in other shapes of diffusers such as air diffuser cylinders.
[0005] The present invention has been made against this background, and has an object to provide an air diffuser that can be easily manufactured using inexpensive raw materials, and a manufacturing method thereof. [Means for solving the problem]
[0006] In order to achieve the above object, the air diffuser according to the present invention comprises: A diffuser that is composed of a porous body containing combustion ash and a binder, changes the received gas into fine bubbles by passing the gas through the diffuser, and releases the bubbles into the liquid. It has a pressure resistance of 0.2 MPa or more, and when pressurized gas is received from the outside, the diffuser is 2 It is configured to be able to release fine bubbles into the liquid at a flow rate of 200 L / min or more per nozzle. Effect of the Invention
[0007] According to the present invention, it is possible to provide an air diffuser that can be easily manufactured using inexpensive raw materials, and a manufacturing method thereof. [Brief description of the drawings]
[0008] [Figure 1] FIG. 2 is a front view showing a configuration of an air diffusing plate according to an embodiment of the present invention. [Diagram 2] 2 is a cross-sectional view of the air diffuser plate of FIG. 1 taken along line AA. [Diagram 3] 4 is a flowchart showing a flow of a method for manufacturing an air diffuser plate according to an embodiment of the present invention. [Figure 4] 3 is a flowchart showing the flow of an assembly method for an air diffusion device according to an embodiment of the present invention. [Diagram 5] FIG. 2 is a photograph of the appearance of a test specimen sintered at a sintering temperature of 1000° C. in Example 1. [Figure 6] FIG. 2 is a photograph of the appearance of a test specimen sintered at a sintering temperature of 1100° C. in Example 1. [Figure 7] FIG. 2 is a photograph of the appearance of a test specimen sintered at a sintering temperature of 1200° C. in Example 1. [Figure 8] FIG. 13 is a diagram showing the blending amounts of raw materials of test specimens in Example 2. [Figure 9] FIG. 13 is a photograph of the appearance of a test specimen after firing in Example 2. [Figure 10] FIG. 11 is a diagram showing the component ratios of clay, combustion ash A, and B in Example 3. [Figure 11]FIG. 13 is a photograph of the appearance of a test specimen after firing in Example 3. [Figure 12] FIG. 13 is a photograph showing a process of producing a test specimen by a slurry molding method in Example 4. [Figure 13] FIG. 13 is a photograph showing the process of producing a test specimen by the slice molding method in Example 5. [Figure 14] FIG. 13 is a diagram showing the results of a performance test of the air diffusing plate in Example 6. [Figure 15] FIG. 13 is a schematic diagram showing the configuration of a test device for pH measurement in Example 6. [Figure 16] 1 is a graph showing the change in pH value over time in Example 7. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, an air diffuser and a manufacturing method thereof according to an embodiment of the present invention will be described in detail with reference to the drawings. In each drawing, the same or equivalent parts are given the same reference numerals. In the embodiment, an air diffuser plate is used as an example of the air diffuser.
[0010] The air diffuser 1 is a device that is installed in a liquid, receives compressed gas, and generates fine bubbles in the liquid. The fine bubbles that the air diffuser 1 emits are, for example, fine bubbles with a bubble diameter of 2.5 mm or less, and are formed of any gas, for example, air, oxygen, or carbon dioxide, depending on the application. The liquid in which the air diffuser 1 is installed is any liquid, for example, water. The air diffuser 1 can be used, for example, for neutralizing alkaline effluent such as concrete drainage, for supplying carbon dioxide gas for the growth of aquatic plants such as algae, and for supplying oxygen or air for land-based aquaculture and sewage treatment. The following will be described taking as an example a case in which air is used as the gas and water is used as the liquid.
[0011] As shown in Fig. 1, the air diffuser 1 includes an air diffuser plate 2 that receives compressed air and generates fine bubbles that are released into water, and a case 3 that is attached to cover a part of the air diffuser plate 2 and supplies compressed air to the air diffuser plate 2. The air diffuser plate 2 has a pair of opposing surfaces, receives air on one surface (back surface) and releases fine bubbles containing air from the other surface (front surface). The air diffuser plate 2 is formed of a porous body with a large number of internal pores, and converts the compressed air that flows in from one surface into fine bubbles by passing it through the large number of pores, and discharges the fine bubbles from the other surface.
[0012] The air diffuser plate 2 is, for example, disk-shaped. Compared to air diffuser plates of other shapes, for example, rectangular shapes, the disk-shaped air diffuser plate has no corners and is less likely to break, and high-pressure air does not concentrate locally, making it easier to generate uniform fine air bubbles from the entire surface. The air diffuser plate 2 can be formed in any dimensions, but considering the efficiency of the number of pieces to be installed in the equipment, the area of the air diffuser plate 2 is set to 100 cm or less. 2 As an example, the dimensions of the disk-shaped air diffuser plate 2 are a diameter of 165 mm and a thickness of 15 mm.
[0013] The case 3 is attached to the air diffusion plate 2 so as to seal the side and back sides of the air diffusion plate 2 and expose the front side. The case 3 includes a main body 3a that supplies air toward the back side of the air diffusion plate 2, and a connection member 3b to which a hose that supplies air to the main body 3a is connected. The main body 3a is formed in a shape corresponding to the air diffusion plate 2, and is a concave member that has an opening for mounting the air diffusion plate 2.
[0014] As shown in FIG. 2, the main body 3a receives air supplied from the connection member 3b in the space 3c and supplies the air toward the air diffusion plate 2 installed on the upper side of the space 3c. The main body 3a has a ring-shaped step 3d for installing the air diffusion plate 2 on the upper side of the space 3c. The air diffusion plate 2 is sealed to the case 3 so that air does not leak from the gap between the case 3. More specifically, the air diffusion plate 2 is adhered to the step 3d using an adhesive, and the gap generated between the air diffusion plate 2 and the case 3 is sealed using a sealant.
[0015] The air diffuser plate 2 is a sintered body (ceramics) obtained by sintering a mixture containing combustion ash. Specifically, the air diffuser plate 2 is obtained by mixing combustion ash with a binder, adding water to the mixture, molding it into a desired shape, and then sintering the resulting molded body. As a result of intensive research by the inventors, it was found that it is possible to manufacture an air diffuser plate 2 capable of uniformly spraying air bubbles from the entire surface through a simple manufacturing process, even when the raw material contains combustion ash, by optimizing the composition and blending ratio of the raw materials, the components of the combustion ash, and the firing conditions.
[0016] The raw materials of the diffuser plate 2 include combustion ash and a binder. Other additives may be added to the raw materials of the diffuser plate 2. The combustion ash is the main component of the raw materials of the diffuser plate 2, and is, for example, coal ash and biomass combustion ash. The coal ash is ash obtained by burning coal, and is preferably fly ash. The fly ash is coal ash generated when pulverized coal is burned and collected by a dust collector. The biomass combustion ash is ash obtained by burning biological resources derived from animals and plants, such as wood, livestock manure, sewage sludge, and agricultural residue. The combustion ash is continuously discharged from a thermal power plant, so it can be obtained stably and cheaply. It is preferable that the raw materials of the diffuser plate 2, excluding moisture, contain at least 50 wt% combustion ash.
[0017] It is preferable to select combustion ash with as low a calcium and iron content as possible. This is because calcium and iron are factors that cause shrinkage and cracking of the fired body. It is preferable that the calcium and iron content in the combustion ash is less than that of the clay to be mixed together. Specifically, for example, it is preferable that the calcium and iron content in the combustion ash is 5 wt% or less.
[0018] The binder, also called a binding material, binds the particles of the combustion ash together. The binder is, for example, clay or a cellulose-based water-soluble polymer. Of these, clay is particularly suitable as a binder because of its excellent toughness. The cellulose-based water-soluble polymer is, for example, carboxymethyl cellulose (CMC). A plurality of types of binders may be mixed with the combustion ash. The weight ratio of the binder contained in the raw material of the air diffuser plate 2 excluding moisture is 50 wt% or less, but in order to prevent cracking and deformation during drying and firing, it is preferable that it is 30 wt% or more and 50 wt% or less. The configuration of the air diffusion device 1 and the air diffusion plate 2 has been described above.
[0019] (Manufacturing method) Next, a method for manufacturing the air diffuser plate 2 according to the embodiment will be described with reference to Fig. 3. Either a casting method or a press molding method may be used as a method for manufacturing the air diffuser plate 2. In both the casting method and the press molding method, the air diffuser plate 2 can be manufactured into any shape by changing the mold. Hereinafter, an example will be described in which coal ash and clay are used as the raw materials for the air diffuser plate 2.
[0020] First, water is added to the raw materials and mixed to create a mixture (step S11). In the casting method, coal ash and clay are mixed, water is added, and the mixture is stirred to create a slurry. On the other hand, in the press molding method, coal ash and clay are mixed, water is added, and the mixture is kneaded to create a clay-like mixture.
[0021] Next, the mixture prepared in step S11 is molded (step S12). In the casting molding method, the slurry is poured into a mold and the surface shape of the slurry is adjusted using a scraper. The mold used in the casting molding method does not need to be strong and is made of plastic, for example. On the other hand, in the press molding method, the clay-like kneaded material is pressed into the mold and the kneaded material in the mold is pressed by a press. The mold used in the press molding method needs to be strong, so it is preferably a metal mold. In the press molding method, the mold is removed from the molded body after pressing by the press.
[0022] Next, the molded body produced in step S12 is dried (step S13). The molded body may be dried naturally, or may be dried by heating or blowing using a dryer. In the case of heating and drying, the air in the dryer may be heated to, for example, a temperature range of 50°C to 150°C, preferably 100°C to 110°C. In the case of the casting molding method, the molded body is dried with the mold attached, and when it is dry, it is removed from the mold. The dried molded body is slightly shrunk against the inner surface of the mold, so it can be easily removed.
[0023] Next, the molded body dried in step S13 is fired (step S14). Specifically, the dried molded body is set in a heating furnace, and the temperature in the heating furnace is maintained at a constant temperature (firing temperature) for a certain time (firing time), thereby changing the molded body into a fired body. The firing temperature is, for example, within a range of 1000°C to 1200°C, preferably within a range of 1050°C to 1150°C, and is, for example, 1100°C. The firing time may be set according to the size of the molded body, and is, for example, within a range of 1 hour to 3 hours, and is, for example, 2 hours. The manufacturing method of the air diffuser plate 2 has been described above.
[0024] The air diffuser 2 manufactured under the above conditions has an average bubble diameter of 1 mm or less when gas is sprayed into water, has a pressure resistance of 0.2 MPa or more, and is suitable for a unit area of 1 m. 2 Micro bubbles can be sprayed into water at a flow rate of 200 L / min or more per sintering. In addition, the shrinkage rate during sintering is controlled to 5% or less based on the molded body before drying, so cracks and deformations in the air diffuser plate 2 can be prevented.
[0025] The decision as to whether to use the casting molding method or the press molding method as the manufacturing method for the air diffuser plate 2 can be made comprehensively, taking into consideration the skill of the worker, the required quality, and the necessity for mass production. The casting molding method can obtain an air diffuser plate 2 that uniformly releases fine bubbles, but it is more time-consuming to manufacture than the press molding method and is not suitable for mass production. On the other hand, the press molding method is more difficult to obtain an air diffuser plate 2 that uniformly releases fine bubbles than the casting molding method, and the mold for molding is expensive, but the kneaded body is easier to handle than a slurry, and it is more suitable for mass production.
[0026] (Assembling method) Hereinafter, a method for assembling the air diffusion device 1 according to the embodiment will be described with reference to Fig. 4. First, the air diffusion plate 2 is attached to the case 3 using an adhesive (step S21). Specifically, the adhesive is applied to the step 3d of the case 3, and the bottom surface of the air diffusion plate 2 is pressed against the step 3d. It is preferable to use an adhesive with high viscosity, for example, an epoxy adhesive.
[0027] Next, the gap between the air diffusion plate 2 and the case 3 is sealed with a sealant (step S22). Specifically, a syringe is used to pour the sealant into the gap between the air diffusion plate 2 and the case 3 so as to fill it. As the sealant, it is preferable to use a hardener that has a lower viscosity and a higher fluidity than an adhesive, and for example, an epoxy resin is used. The above is the method for assembling the air diffuser 1.
[0028] As described above, the air diffuser plate 2 according to the embodiment is made of a porous body containing combustion ash and a binder, has a pair of opposing surfaces, and receives air on one surface in liquid and releases fine bubbles from the other surface. Therefore, it can be manufactured in a simple process using combustion ash, which is a cheap raw material. As a result, the air diffuser plate 2 can be manufactured at low cost, and the combustion ash discharged in large quantities from facilities equipped with combustion equipment such as thermal power plants and steelworks can be effectively utilized, reducing the cost of disposing of the combustion ash and the burden on the environment.
[0029] The present invention is not limited to the above-described embodiment, and the following modifications are possible.
[0030] (Modification) In the above embodiment, the air diffuser plate 2 is formed in a disk shape, but the present invention is not limited to this. The air diffuser plate 2 can be formed in any shape, for example, it may be formed as a rectangular plate. In addition, the air diffuser plate 2 is merely one example of an air diffuser that has a pair of surfaces at different positions and receives air at one surface in liquid and releases fine bubbles from the other surface, and the air diffuser may be formed, for example, as a cylindrical air diffuser that receives air at the inner surface and releases fine bubbles from the outer surface.
[0031] In the above embodiment, in order to prevent cracking during firing, the ratio of binder contained in the raw material excluding moisture is set to 50 wt% or less, and the component ratios of calcium and iron contained in the combustion ash are each set to 5 wt% or less, but the present invention is not limited to this. As factors of shrinkage during firing can be other factors such as the particle size of the raw material in addition to the composition and blending ratio of the raw material and the components of the combustion ash, a condition may be set to use raw materials with a shrinkage rate of 5% or less during firing.
[0032] In the above embodiment, the raw material containing combustion ash and clay is mixed, water is added to the mixture, the mixture is molded using a frame, and the molded body is dried and fired to manufacture the air diffuser plate 2, but the present invention is not limited to this. For example, a slice molding method may be used in which molding and firing are performed in the same manner as for making bricks, and the obtained block-shaped fired body is sliced.
[0033] The procedure of the slice molding method will be described in detail. A block-shaped molded body is produced by kneading, extruding, and cutting the raw materials in sequence, and then drying and firing are performed to produce a block-shaped fired body having a shape equivalent to that of a brick. The extruded mixture may be cut into individual blocks with a piano wire, for example, to produce a block-shaped molded body. Next, the obtained block-shaped fired body is sliced to a desired thickness using a cutting means such as a diamond cutter. Although it is difficult to produce the air diffuser plate 2 in any shape using the slice molding method, it is suitable for mass production and quality control is also easy.
[0034] The above-mentioned embodiments are merely examples, and the present invention is not limited to these, and various embodiments are possible without departing from the spirit of the invention described in the claims. The components described in the embodiments and modifications can be freely combined. In addition, inventions equivalent to the inventions described in the claims are also included in the present invention.
[0035] The present invention will be specifically described below with reference to examples, although the present invention is not limited to these examples.
[0036] Example 1 In Example 1, various test specimens were prepared by using coal ash and clay as raw materials and varying the type of coal (coal type) from which the coal ash was made, the mixing ratio of the raw materials, and the firing conditions. The test specimens were prepared using a press molding method. After that, air bubbles were generated while the test specimens were set in a case in water to verify whether the test specimens functioned as air diffusers.
[0037] Coal ash is fly ash (FA) separated from the exhaust of a coal-fired power plant. The FA used as the raw material was three types: coal ash A 100%, coal ash B 70%, coal ash C 30%, coal ash D 80%, and coal ash E 20%. Coal ashes A to E are coal types with different component ratios. For example, coal ash B 70% and coal ash C 30% means that coal ash B is mixed at 70% and coal ash C at 30% by weight. The raw material mixing ratio was three patterns: FA:clay = 80%:20%, FA:clay = 70%:30%, and FA:clay = 50%:50% by weight. The size of the prepared test specimens was 100 mm square and 10 mm thick. The firing temperatures were three patterns: 1000°C, 1100°C, and 1200°C, and the firing time was two hours in each case.
[0038] As a result, as shown in Figs. 5 to 7, when the molded body was fired at firing temperatures of 1000°C, 1100°C, and 1200°C, a fired body was obtained, and it was confirmed that the molded body functions as an air diffuser plate in water. Specifically, when the firing temperature was 1100°C, a good test body was obtained in terms of strength, shape, and function, but when the firing temperature was 1200°C, the test body was easily distorted, and some of the coal types melted and peeled off. In addition, when the firing temperature was less than 1000°C, the strength of the test body was insufficient, and it could not withstand the gas pressure when bubbles were generated, and cracks and peeling occurred. From the above, it can be understood that the firing temperature during firing is preferably 1100°C. It can also be understood that the blending ratio of the coal type and the raw material has almost no effect on the strength and performance of the air diffuser plate.
[0039] Example 2 In Example 2, the relationship between the composition and blending ratio of the raw materials and cracking of the fired body was examined. First, the raw materials were mixed under the conditions shown in Samples 1 to 4 in FIG. 8, molded using a press molding method, dried, and fired to create eight test specimens for each condition. The combustion ash A in FIG. 8 is fly ash. The weight of the raw materials excluding water is 500 g for all test specimens. The diameter of the test specimen before firing is 165 mm, and the thickness is about 15 mm. The pressing pressure applied to the test specimen before firing is 5 tons. The drying conditions are natural drying or heat drying at a temperature of 105°C. Based on the results of Example 1, the firing temperature was set to 1100°C and the firing time was set to 2 hours.
[0040] As a result, as shown in FIG. 9, fired bodies were obtained for all of samples 1 to 4. Sample 1 was made by simply kneading clay with water, which caused a large shrinkage and many fine cracks. For samples 2 and 3, seven out of eight pieces had no cracks, and the remaining one only had a small crack at the edge. For sample 4, which does not contain clay and is thought to have low toughness, large cracks occurred during firing. From the above, it can be seen that if the shrinkage during firing is large, the fired body is likely to crack or deform, and that a combination of coal ash and clay is suitable as a raw material for the air diffuser plate.
[0041] Example 3 In Example 3, the relationship between the component ratio of coal ash and the shrinkage rate during firing was examined. Specifically, 1% CMC was added to each of combustion ash A and B having the component ratio shown in Figure 10, and then water was added and kneaded, and test specimens were prepared by press molding, and the shrinkage rate during firing was measured. Combustion ash A and B in Figure 10 are fly ashes derived from different coal types. The other conditions are the same as in Example 2. For comparison, a similar experiment was also conducted on clay having the component ratio shown in Figure 10. Only water was added to the clay and kneaded, and test specimens were prepared by press molding.
[0042] As a result, the shrinkage rate of the specimen using combustion ash A was 1.8%, while the shrinkage rates of the specimens using clay and combustion ash B were 6.1% and 7.3%, respectively. The specimen using combustion ash A showed almost no deformation, whereas the specimens using clay and combustion ash B showed cracks and warping due to their large shrinkage rates, as shown in Figure 11. From the above, it can be understood that it is preferable to use combustion ash with a small calcium and iron content ratio as the raw material for the air diffuser plate.
[0043] Example 4 In Example 4, it was verified whether the casting method can be used as a manufacturing method for the air diffuser plate. Specifically, first, combustion ash and clay were mixed, and water was added to create a slurry. The combustion ash was fly ash. The mixing ratio of the raw materials was 80% combustion ash and 20% clay, taking into consideration the results of Example 2, and the total weight was 1000 g. The amount of water added was 40% by weight. Next, as shown in FIG. 12, the slurry was poured into a mold, and after the surface shape was adjusted, it was heated and dried at 105°C for 24 hours using a dryer. The shape of the mold was 165 mm in diameter and about 15 mm to 34 mm in thickness. Next, after drying, the mold was removed, and firing was performed at a firing temperature of 1100°C and for 2 hours in the same manner as in Example 2. As a result, it was confirmed that a fired body of combustion ash and clay could be obtained using the casting method, as shown in FIG. 12.
[0044] Example 5 In Example 5, it was verified whether the slicing method can be used as a manufacturing method for the diffuser plate. Specifically, combustion ash and clay were mixed, water was added to create a kneaded product, and the process from kneading to firing was carried out in the same manner as in the case of bricks using a production line in a brick factory. The combustion ash was fly ash. The raw material blend ratio was 50% combustion ash and 50% clay. As a result, a fired block could be obtained as shown in FIG. 13. The cross section of this block was rectangular, with dimensions of 100 mm x 100 mm. Using a diamond cutter, it was possible to slice it to a thickness of 15 mm, which is suitable as the thickness of the diffuser plate. It was confirmed that this sliced diffuser plate was also capable of releasing fine bubbles in water.
[0045] Example 6 In Example 6, the average bubble diameter of bubbles generated by the air diffuser plate was measured. Specifically, air was sent to the air diffuser plate to which the case was attached to generate bubbles, and the bubbles in the water were visualized by the backlight method, photographed by a high-speed camera, and the photographed image was subjected to image analysis to calculate the bubble diameter. The Sauter average value was calculated from the calculated bubble diameter to obtain the average bubble diameter. The test specimens were three patterns: an air diffuser plate with a thickness of 15 mm created by the press molding method, and air diffusers with thicknesses of 27 mm and 34 mm created by the casting molding method. All of the air diffusers were disk-shaped.
[0046] As a result, as shown in Figure 14, fine bubbles with an average bubble diameter of 1 mm or less were generated in all test specimens. The air diffuser plate made by the casting method had a smaller average bubble diameter than the air diffuser plate made by the press molding method. Also, while fine bubbles were generated uniformly in the air diffuser plate made by the casting method, the air diffuser plate made by the press molding method had some surfaces with fewer bubbles from the center, and there was variation in the generation of bubbles. This is thought to be because with the press molding method, unevenness is likely to occur when filling the mold with raw materials and when applying press pressure.
[0047] Example 7 In Example 7, it was verified whether or not a diffuser plate can be used to neutralize wastewater from a concrete factory. In the experimental apparatus, as shown in FIG. 15, 20 L of wastewater from a concrete factory with a pH of 12.42 was stored in a water tank, and carbon dioxide gas was supplied to the wastewater from a concrete factory, and the change in pH value over time was measured. Carbon dioxide gas was supplied from a liquefied gas cylinder (CO2 99.5%), and the gas flow rate was 1.0 L / min. The test specimens were a diffuser plate with a thickness of 34 mm made by the casting method, and commercially available diffuser plates A and B. All had an area of 60 cm. 2 The commercially available diffuser plate A is an aeration plate that is actually used in neutralization treatment equipment, and the commercially available diffuser plate B is an aeration plate that is commercially available as an air stone for fish breeding.
[0048] As a result, as shown in Figure 16, the air diffuser plate made by the casting method had the same neutralization efficiency as commercial air diffuser plate A, and was more efficient than commercial air diffuser plate B. Furthermore, when it was verified whether neutralization could be carried out by replacing carbon dioxide gas containing 99.5% CO2 with exhaust gas (component ratio: CO2 10%, O2 10%, N2 80%) collected from a thermal power plant, the pH of concrete waste liquid was similarly successfully lowered to 7. [Explanation of symbols]
[0049] 1 Air diffuser 2. Air diffuser 3 Cases
Claims
1. A diffuser that is composed of a porous body containing combustion ash and a binder, changes the received gas into fine bubbles by passing the gas through the diffuser, and releases the bubbles into the liquid. It has a pressure resistance of 0.2 MPa or more, and when pressurized gas is received from the outside, the pressure of the diffuser is 1 m2 per unit area from the surface of the diffuser. 2 The nozzle is configured to emit microbubbles into the liquid at a flow rate of 200 L / min or more per unit time. Aeration body.
2. The calcium and iron contained in the combustion ash are each 5% by weight or less; The air diffuser according to claim 1.
3. The binder is clay. The air diffuser according to claim 1 or 2.
4. The ratio of the combustion ash in the raw material of the diffuser is 50 wt % or more, and the ratio of the binder is 50 wt % or less. The air diffuser according to claim 1 or 2.
5. A method for producing the air diffuser according to claim 1 or 2, A mixing step of mixing the combustion ash, the binder, and water; a molding step of molding the mixture mixed in the mixing step; a drying step of drying the molded body obtained by the molding step; A firing step of firing the dried molded body; A method for manufacturing an aeration body comprising the steps of:
6. In the firing step, the dried molded body is fired at a constant temperature set within a range of 1000°C to 1200°C. A method for manufacturing the air diffuser according to claim 5.
7. In the mixing step, a slurry containing the combustion ash, the binder, and the water is generated, In the molding step, the generated slurry is poured into a mold. A method for manufacturing the air diffuser according to claim 5.
8. In the mixing step, a kneaded material containing the combustion ash, the binder, and the water is generated, In the molding step, the produced kneaded material is pressed into a mold and pressurized. A method for manufacturing the air diffuser according to claim 5.
Citation Information
Patent Citations
Method of converting waste matter to ceramics
JP1987212260A
Ceramics porous body
JP1995242473A
Production of porous ceramic body
JP1998218686A
Diffusion plate
JP2010158631A
Air diffusing body
JP2011230068A