Susceptor

The susceptor's alternating contact and non-contact design addresses uneven heat distribution and stress issues, enhancing semiconductor chip yield and susceptor longevity.

JP2024133383AInactive Publication Date: 2024-10-01TOYO TANSO KK
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024117988
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2018-10-04
Filing Date
2024-07-23
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing susceptors in semiconductor manufacturing cause temperature differences and stress concentration on wafers due to uneven conductive heat application and small contact areas, leading to reduced yield and susceptibility to chipping.

Method used

A susceptor design with alternating contact and non-contact portions on its inner peripheral wall, ensuring even heat distribution and reducing stress concentration, by forming support parts, contact parts, and non-contact parts at specific ratios and distances.

Benefits of technology

Improves semiconductor chip yield by minimizing temperature differences and reducing chipping, extending susceptor lifespan.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024133383000001_ABST
    Figure 2024133383000001_ABST
Patent Text Reader

Abstract

To provide a susceptor which can improve a yield of a semiconductor chip formed by a wafer, in which a chipping (a cracking) hardy occurs, and of which a life is long.SOLUTION: In a susceptor having each pocket (2) mounting a wafer (10), at least one of the pockets (2) comprises: a plurality of support parts (3) that supports the wafer (10); a plurality of contact parts (4) that is contacted to a side surface (10a) of the wafer (10); and a plurality of non-contact parts (5) that is not contacted to the side surface (10a) of the wafer (10). Each contact part (4) and each non-contact part (5) are alternately formed into an inner peripheral wall of each pocket (2). At least two of the support parts (3) are formed onto a line connecting a center (O) of each pocket (2) with each non-contact part (5) when viewed from an upper direction of the susceptor.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to susceptors used in semiconductor manufacturing. [Background technology]

[0002] For example, to manufacture good LEDs, it is important to uniformly epitaxially grow the thin-film crystal layer laminated on the surface of the wafer that will become the semiconductor chip. For this reason, the susceptor used in semiconductor manufacturing must apply conductive heat and radiant heat to the wafer to uniformly heat it in order to perform epitaxial growth and form a thin-film crystal layer with a uniform thickness. However, since conductive heat is applied to the wafer placed in the pocket of the susceptor from the part in contact with the pocket, the temperature of the wafer tends to become uneven between the outer periphery in contact with the pocket and the central part not in contact with the pocket. Specifically, the temperature difference is likely to occur in the region of about 3 mm from the outer periphery of the wafer toward the inside, resulting in poor yield of semiconductor chips.

[0003] Therefore, various proposals have been made regarding the shape of the pocket, such as the wafer carrier (susceptor) described in Patent Document 1. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2013-138224 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, the inventors of the present invention have found that the wafer carrier described in Patent Document 1 has a support portion that supports the wafer placed in the pocket and a contact portion that contacts the side of the wafer, which are adjacent to each other, and therefore conductive heat is likely to be locally applied to the wafer. This creates a temperature difference in the wafer between the peripheral portion that contacts the pocket and the central portion that does not, and this causes a problem of poor yield of semiconductor chips.

[0006] Furthermore, the susceptor rotates during semiconductor manufacturing. Therefore, if the contact area between the susceptor and the wafer is made too small, stress due to centrifugal force is concentrated at the contact area (collision area) with the wafer placed in the pocket when the susceptor is rotated during various processes. Therefore, it was found that the wafer carrier (susceptor) described in Patent Document 1 also has a problem in that chipping (chipping) may occur in the susceptor or wafer at the contact area.

[0007] An object of the present invention is to provide a susceptor capable of improving the yield of semiconductor chips produced from a wafer, and a susceptor which is less susceptible to chipping and has a long life. [Means for solving the problem]

[0008] In order to solve the above problems, the present invention provides the following: <1> ~ <3> The present invention includes the following: <1> A susceptor having pockets for placing a wafer, at least one of the pockets having a plurality of support portions for supporting the wafer, a plurality of contact portions for contacting the side surfaces of the wafer, and a plurality of non-contact portions for not contacting the side surfaces of the wafer, the contact portions and non-contact portions being alternately formed on an inner peripheral wall of the pocket, and at least two of the support portions being formed on a line connecting the center of the pocket and the non-contact portions when the susceptor is viewed from above. <2> The circumferential length of one contact part is 2 mm or more. <1> The susceptor according to claim 1. <3> The ratio of the total circumferential length of the plurality of contact portions to the circumference of the pocket is 1.5 to 50%. <1> or <2> The susceptor according to claim 1. Effect of the Invention

[0009] According to one aspect of the present invention, the susceptor has contact and non-contact parts formed alternately on the inner peripheral wall of the pocket, and at least two of the support parts are formed on a line connecting the center of the pocket and the non-contact parts when the susceptor is viewed from above. Therefore, the wafer is less likely to have a temperature difference between the outer peripheral part that is in contact with the pocket and the central part that is not in contact with the pocket, improving the quality. Therefore, it is possible to provide a susceptor that can improve the yield of semiconductor chips manufactured from the wafer. In addition, since a plurality of contact parts and a plurality of non-contact parts are alternately formed on the inner peripheral wall of the pocket, stress concentration due to centrifugal force on the contact part (collision part) with the wafer placed in the pocket is reduced. Therefore, it is possible to provide a susceptor that is less likely to chip (crack) the susceptor or wafer and has a long life. [Brief description of the drawings]

[0010] [Figure 1] 1A and 1B are schematic plan views showing an example of a susceptor according to an embodiment of the present invention. [Diagram 2] FIG. 2 shows one of the pockets formed in the susceptor (Example 1, Comparative Examples 1 and 2), where (a) is a schematic plan view of the pocket, and (b) is a cross-sectional view taken along line AA in (a). [Diagram 3] FIG. 2 is a diagram showing a main part of the pocket (Example 1), where (a) to (c) are schematic plan views of a support part, and (d) to (f) are schematic cross-sectional views of a contact part. [Figure 4] FIG. 11 is a diagram showing a modified example and Example 2 of the pocket according to another embodiment of the present invention, in which (a) is a schematic plan view of the pocket, and (b) is a cross-sectional view taken along line AA in (a). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] An embodiment of the present invention will be described below, but the present invention is not limited thereto. The present invention is not limited to each embodiment or each configuration described below, and various modifications are possible within the scope of the claims. The embodiments and examples obtained by appropriately combining the technical means disclosed in different embodiments and examples are also included in the technical scope of the present invention. In addition, all academic literature and patent documents described in this specification are incorporated herein by reference. In addition, unless otherwise specified in this specification, "A to B" representing a numerical range means "A or more, B or less."

[0012] [Embodiment 1] An embodiment of the present invention will now be described.

[0013] A susceptor according to one embodiment of the present invention is a susceptor having pockets for placing a wafer, at least one of the pockets having a plurality of support portions for supporting the wafer, a plurality of contact portions for contacting the sides of the wafer, and a plurality of non-contact portions that do not contact the sides of the wafer, the contact portions and non-contact portions being formed alternately on the inner wall of the pocket, and at least two of the support portions being formed on a line connecting the center of the pocket and the non-contact portions when the susceptor is viewed from above.

[0014] As shown in Fig. 1, a disk-shaped susceptor (also referred to as a "pedestal," "substrate support," "wafer carrier," etc.) 1 is a member that is attached to a manufacturing device such as an MOCVD device used in the manufacture of semiconductors, and is made of a carbon-based material such as high-purity isotropic graphite or sintered silicon carbide. Specifically, for example, a susceptor in which the surface of high-purity isotropic graphite is coated with SiC is suitable. The diameter of the susceptor 1 is not particularly limited, as it is appropriately set depending on the semiconductor manufacturing device.

[0015] The susceptor 1 is used in the semiconductor manufacturing process to place a semiconductor wafer (hereinafter simply referred to as a wafer) such as a sapphire wafer, a gallium nitride wafer, or a silicon wafer on it, heat it, and rotate it horizontally to epitaxially grow and stack a thin-film crystal layer on the surface of the wafer. The susceptor 1 is also used for surface modification to form an oxide layer or a nitride layer on the surface of the wafer, for surface cleaning to remove contaminants attached to the wafer surface, and for annealing.

[0016] At least one or more pockets (also called "recesses" or "countersinks") 2 are formed on the upper surface of the susceptor 1, and various processes are performed by placing wafers in the pockets 2. A heating device (not shown), such as a heater or a high-frequency induction coil, for heating the susceptor 1 is installed below the susceptor 1. The number and arrangement of the pockets 2 and the arrangement of the heating device are designed so that all wafers placed on the susceptor 1 can be heated evenly. The number and arrangement of the pockets 2 may be determined so that the maximum number of pockets 2 is formed according to the sizes of the susceptor 1 and the wafers, and are not particularly limited. Therefore, the number, arrangement, and size (size) of the pockets 2 formed in the susceptor 1 shown in FIG. 1 are merely an example.

[0017] The diameter (φ) of the pocket 2 refers to the diameter of the inner peripheral wall of the portion where the contact portion 4 is formed (not the diameter of the inner peripheral wall of the portion where the non-contact portion 5 is formed). When the diameter of the pocket 2 is 100, the diameter of the smallest wafer 10 placed in the pocket 2 is usually 98 or more and less than 100. If the diameter of the wafer 10 is less than 98, chipping (chipping) due to collision may easily occur in the susceptor 1 or the wafer 10 when the susceptor 1 starts or stops rotating. Furthermore, when the term "inner peripheral wall" is simply used in this specification, it refers to the inner peripheral wall of the portion where the contact portion 4 is formed.

[0018] The multiple pockets 2 are substantially circular when the susceptor 1 is viewed from above, and may be formed independently of one another as shown in Fig. 1(a) or may be formed to communicate with one another as shown in Fig. 1(b). The pockets 2 are formed by making the depth of each pocket 2 deeper or shallower, taking into consideration the gas flow and temperature distribution when a wafer is placed on the pockets 2.

[0019] A further explanation will be given by taking an example where the pockets 2 are formed independently of each other. As shown in FIG. 2 as Example 1, at least one of the pockets 2 includes a plurality of support parts 3 for supporting the wafer 10, a plurality of contact parts 4 that contact the side surface 10a of the wafer 10, and a plurality of non-contact parts 5 that do not contact the side surface 10a of the wafer 10. The contact parts 4 and the non-contact parts 5 are alternately formed on the inner peripheral wall of the pocket 2, and at least two of the support parts 3 are formed on a line connecting the center O of the pocket 2 and the non-contact parts 5 when the susceptor 1 is viewed from above. The number and arrangement of the support parts 3, the contact parts 4, and the non-contact parts 5 may be appropriately determined according to the formation position of the pocket 2 in the susceptor 1, the position of the heating device, and the like, and are not particularly limited. Therefore, the pocket 2 (Example 1) shown in FIG. 2 in which six support parts 3, six contact parts 4, and six non-contact parts 5 are arranged at equal intervals is merely an example.

[0020] A plurality of support parts (also called "tabs") 3 are formed on one susceptor 1, and are adapted to support the wafer 10 placed in the pocket 2 by contacting the lower surface of the wafer 10. The number of support parts 3 is not particularly limited, and may be at least three so as to stably support the placed wafer 10. The height of the support parts 3 from the bottom surface 2a of the pocket 2 may be a height at which the radiant heat from the bottom surface 2a is appropriately applied to the wafer 10, taking into consideration the warping of the wafer 10, and may be, for example, within a range of 0.02 to 1.5 mm, preferably within a range of 0.02 to 0.5 mm. However, the height of the support parts 3 from the bottom surface 2a of the pocket 2 may be a height at which the wafer 10 and the bottom part 2a do not come into contact with each other, and may be not particularly limited. The contact area of ​​the support parts 3 with the wafer 10 may be an area at which the wafer 10 is stably supported by the support parts 3, and the conductive heat from the support parts 3 is also conducted from the support parts 3, and may be an area at which the conductive heat from the support parts 3 is as small as possible.

[0021] The shape of the support 3 (shape when the pocket 2 is viewed from above) is not particularly limited, but may be various shapes such as a mountain shape, as shown in (a) to (c) of FIG. 3. In addition, in (a) to (c) of FIG. 3, the support 3 protrudes from the bottom surface 2a and is formed in contact with the non-contact portion 5, but may be formed in a position adjacent to the position where the non-contact portion 5 is formed in the pocket 2 without contacting the non-contact portion 5. That is, at least two of the support parts 3, and particularly preferably all of the multiple support parts 3, are formed on a line connecting the center O of the pocket 2 and the non-contact portion 5 when the susceptor 1 is viewed from above, and do not need to be in contact with the non-contact portion 5. In addition, the support part 3 does not need to be located in the center part of the non-contact portion 5 when the susceptor 1 is viewed from above.

[0022] The contact portion 4 constitutes the inner peripheral wall of the pocket 2, and at least when the susceptor 1 rotates, contacts the side surface 10a of the wafer 10, preferably in surface contact with the side surface 10a of the wafer 10. That is, in the pocket 2, the contact portion 4 contacts the side surface 10a of the wafer 10 placed in the pocket 2, preferably in surface contact. Here, "surface contact" includes a state in which the contact portion 4 is substantially in surface contact. Specifically, it refers to a state in which the shortest distance between an arbitrary point on the contact portion 4 in contact with the wafer 10 and the side surface 10a of the wafer 10 placed in the pocket 2 is close to a distance of 0 (a state in which the contact portion 4 is in physical contact with the side surface 10a of the wafer 10) to a distance of 2% or less of the diameter, preferably 1% or less, based on the diameter of the pocket 2 (the diameter of the inner peripheral wall of the portion in which the contact portion 4 is formed). Therefore, it is not necessary for the contact portion 4 to be in physical contact with the side surface 10a of the wafer 10 over the entire contact portion 4.

[0023] The circumferential length of one contact portion 4 (the circumferential length when the pocket 2 is viewed from above) is preferably 2 mm or more in order to reduce stress concentration due to centrifugal force on the contact portion of the wafer 10. The number of contact portions 4 and the circumferential length of each contact portion 4 are not particularly limited as long as they are set so as to make the temperature of the wafer 10 uniform. In addition, the ratio of the total circumferential length of the plurality of contact portions 4 to the circumference of the pocket 2 (the circumference of the circle where the contact portions 4 are formed) is preferably 1.5 to 50%.

[0024] The cross-sectional shape of the inner peripheral wall of the pocket 2 where the contact portion 4 is formed may be vertical from the bottom surface 2a upward as shown in Fig. 3(d), or may be inclined so as to widen from the bottom surface 2a upward as shown in Fig. 3(e), or may be inclined so as to narrow from the bottom surface 2a upward as shown in Fig. 3(f). The angle of inclination is preferably about -10° to 10°, with 0° being defined as an inner peripheral wall formed vertically from the bottom surface 2a upward.

[0025] The non-contact portion 5 is formed at a position adjacent to the position where the support portion 3 is formed on the inner peripheral wall of the pocket 2. Therefore, the contact portion 4 is not formed where the support portion 3 is formed. For this reason, in the pocket 2, the support portion 3 and the contact portion 4 are not formed adjacent to each other, so that conductive heat is not locally applied to the wafer 10.

[0026] The non-contact portion 5 is separated from the wafer 10 so as to prevent the wafer 10 from being affected by heat conducted from the non-contact portion 5. In other words, the non-contact portion 5 may be formed at a position farther from the center O of the pocket 2 than the contact portion 4.

[0027] The non-contact portion 5 may be formed in a position not adjacent to the position where the support portion 3 is formed (where the support portion 3 is not formed) as necessary in order to divide the contact portion 4, etc. Furthermore, as shown in (b) of Fig. 1, when a plurality of pockets 2 communicate with each other, the communication portion a also corresponds to the non-contact portion, and the support portion 3 may not be formed in the communication portion a.

[0028] Moreover, the pocket 2 may have a plurality of locations where the support portion 3, the contact portion 4, and the non-contact portion 5 are formed in the arrangement according to the present embodiment. That is, the pocket 2 according to the present embodiment may have a location where the support portion, the contact portion, and the non-contact portion are formed in a conventional arrangement. Furthermore, when a plurality of pockets 2 are provided in the susceptor 1, the susceptor 1 may have at least one pocket 2 according to the present embodiment. That is, the susceptor 1 in which at least one pocket 2 according to the present embodiment is formed may further have pockets in which the support portion, the contact portion, and the non-contact portion are formed in the conventional number and arrangement. Therefore, a susceptor having a plurality of pockets 2 for placing the wafer 10, at least one of which has the support portion 3, the contact portion 4, and the non-contact portion 5 configured as described above, is also included in the embodiment of the present invention.

[0029] A susceptor according to an embodiment of the present invention is used in the manufacture of semiconductors. The semiconductor manufacturing apparatus includes at least a chamber having an exhaust port, a susceptor housed in the chamber, a source gas supply device for supplying a source gas into the chamber, a carrier gas supply device for supplying a carrier gas into the chamber, a rotation device for rotating the susceptor, and a chamber heating device for heating the inside of the chamber. The semiconductor manufacturing apparatus manufactures a semiconductor by forming and stacking a thin-film crystal layer on a surface of a wafer placed on the susceptor while rotating the susceptor. That is, the semiconductor is manufactured by a method of rotating the susceptor, heating the wafer placed on the susceptor, and forming and stacking a thin-film crystal layer on the surface.

[0030] The wafers that have been subjected to various processes by the above-mentioned manufacturing apparatus are then cut into chips and packaged (modules) to become semiconductor devices, which are then used as various products such as LEDs.

[0031] [Embodiment 2] Other embodiments of the present invention will be described below. For the sake of convenience, the same reference numerals are given to members having the same functions as those described in the first embodiment, and the description thereof will be omitted.

[0032] The support portions 3, contact portions 4, and non-contact portions 5 described in the first embodiment do not need to be formed at equal intervals in the pocket 2 (for example, so as to be line-symmetric or point-symmetric when the pocket 2 is viewed from above), and their number, arrangement, and size (length) are appropriately set depending on the formation position of the pocket 2 in the susceptor 1, the position of the heating device, etc., so that conductive heat can be applied uniformly to the wafer 10. Therefore, when a plurality of pockets 2 are provided in the susceptor 1, the number, arrangement, and size (length) of the support portions 3, contact portions 4, and non-contact portions 5 of the individual pockets 2 may differ from one another.

[0033] Specifically, the pocket 2 (Example 1 in FIG. 2) in which six (even number) of each of the support parts 3, contact parts 4, and non-contact parts 5 are arranged at equal intervals, used in the description of the first embodiment, is merely one example. As other embodiments of the present invention, examples of modified examples (patterns) of the pocket 2 include, as shown in FIG. 4, a pocket 2 (Modification 1) in which five (odd number) of each of the support parts 3, contact parts 4, and non-contact parts 5 are arranged, and a pocket 2 (Modification 2) in which six (odd number) of each of the support parts 3, contact parts 4, and non-contact parts 5 are arranged at unequal intervals. EXAMPLES

[0034] Next, the susceptor according to the present invention will be described in more detail with reference to examples and comparative examples, but the present invention is not limited to these examples.

[0035] Example 1 A pocket 2 shown in (a) and (b) of FIG. 2 was produced as Example 1, which is an independently formed pocket in a susceptor. That is, a susceptor was produced in which the surface of high-purity isotropic graphite was coated with SiC, the diameter (φ) of the pocket 2 was 50 mm, the pocket 2 had six support parts 3, six non-contact parts 5 were formed on the inner peripheral wall of the pocket 2 adjacent to the formation position of the support parts 3, and six contact parts 4, each of which had a length (the circumferential length when the pocket is viewed from above) of 13 mm, were formed between the non-contact parts 5, and the total ratio of the circumferential lengths of the contact parts 4 to the circumference was about 50%. Then, as shown in (b) of FIG. 2, a semiconductor was produced using the susceptor in which a wafer 10 was placed in the pocket 2.

[0036] Example 2 As Example 2, as shown in Figures 4(a) and (b), a susceptor was fabricated in the same manner as in Example 1, except that the diameter (φ) of the pocket 2 was set to 200 mm and the length of each contact portion 4 was set to 2 mm, and a semiconductor was manufactured using the susceptor in which the ratio of the total circumferential length of the contact portions 4 to the circumference was approximately 1.9%.

[0037] Comparative Example 1 A pocket 2' shown in FIG. 2(a) was produced as Comparative Example 1, which is an independently formed pocket in a susceptor. That is, a susceptor was produced in which the surface of high-purity isotropic graphite was coated with SiC, the pocket 2' had six support parts 3', six contact parts 4' each 1 mm long (the length in the circumferential direction when the pocket is viewed from above) were formed on the inner peripheral wall of the pocket 2' adjacent to the formation position of the support parts 3', and six non-contact parts 5' were formed between the contact parts 4'. Then, as shown in FIG. 2(b), a semiconductor was produced using the susceptor with a wafer 10 placed in the pocket 2'.

[0038] Comparative Example 2 A pocket 2'' shown in FIG. 2(a) was produced as Comparative Example 2, which is an independently formed pocket in a susceptor. That is, a susceptor was produced in which the surface of high-purity isotropic graphite was coated with SiC, the pocket 2'' had six support portions 3'', and a contact portion 4'' was formed along the entire periphery of the inner wall of the pocket 2''. Then, as shown in FIG. 2(b), a semiconductor was produced using the susceptor with a wafer 10 placed in the pocket 2''.

[0039] (result) The life of the susceptor of Example 1 was doubled compared to that of the susceptor of Comparative Example 1. In addition, the yield of semiconductor chips manufactured from the wafers was improved by 10%.

[0040] Compared with the susceptor of Comparative Example 2, the susceptor of Example 1 had a similar lifespan, but the yield of semiconductor chips manufactured from the wafers was improved by 20%.

[0041] The life of the susceptor of Example 2 was doubled compared to that of the susceptor of Comparative Example 1. In addition, the yield of semiconductor chips manufactured from the wafers was improved by 15%.

[0042] Compared with the susceptor of Comparative Example 2, the susceptor of Example 2 had a similar lifespan, but the yield of semiconductor chips manufactured from the wafers was improved by 25%.

[0043] In the susceptor of Comparative Example 1, the length of each contact portion 4' is as short as 1 mm, and since the contact portion 4' is also formed where the support portion 3' is formed, conductive heat is likely to be locally applied to the wafer 10. This results in a temperature difference in the wafer 10 between the outer peripheral portion in contact with the pocket 2' and the central portion not in contact, resulting in poor yield of semiconductor chips. In addition, since the length of each contact portion 4' is as short as 1 mm, stress due to centrifugal force is concentrated on the contact portion 4' when the susceptor is rotated during various processes, and chipping is likely to occur in the susceptor and the wafer 10.

[0044] In the susceptor of Comparative Example 2, a contact portion 4'' is formed around the entire inner wall of the pocket 2'', so that not only is a large amount of conductive heat applied around the entire circumference of the wafer 10, but conductive heat is also applied from the support portion 3'' in the vicinity of the support portion 3'', resulting in a large temperature difference in the wafer 10 between the outer periphery in contact with the pocket 2'' and the central portion which is not in contact, resulting in a decrease in the yield of semiconductor chips. [Industrial Applicability]

[0045] The susceptor according to the present invention can be widely used in the manufacture of semiconductors. [Explanation of symbols]

[0046] 1. Susceptor 2 Pockets 3 Support part 4 Contact Part 5 Non-contact part 10 Wafers

Claims

1. A susceptor having a pocket for placing a wafer thereon, At least one of the pockets includes a plurality of support portions for supporting the wafer, a plurality of contact portions for contacting the side surface of the wafer, and a plurality of non-contact portions for not contacting the side surface of the wafer; The contact portions and the non-contact portions are alternately formed on the inner peripheral wall of the pocket, At least two of the support portions are formed on a line connecting a center of the pocket and the non-contact portion when the susceptor is viewed from above.

2. The susceptor according to claim 1 , wherein a circumferential length of one contact portion is 2 mm or more.

3. 3. The susceptor according to claim 1, wherein a ratio of the total circumferential length of said plurality of contact portions to a circumference of said pocket is 1.5 to 50%.

Citation Information

Patent Citations

  • Wafer carrier with varying thermal resistance