Reflection type mask blank, reflection type mask, method for producing reflection type mask blank, method for producing reflection type mask

By using Rh as the main component in the protective film and optimizing film formation conditions, the etching resistance of EUV lithography masks is enhanced, addressing the etching issues with oxygen-based gases and maintaining reflectance.

JP2024133671APending Publication Date: 2024-10-02AGC INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024110123
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-04-01
Filing Date
2024-07-09
Publication Date
2024-10-02

AI Technical Summary

Technical Problem

The protective film in existing EUV lithography masks has insufficient etching resistance, particularly when using oxygen-based gases, which compromises the integrity of the multilayer reflective film.

Method used

Incorporating rhodium (Rh) as the main component of the protective film, with a density enhancement achieved through specific film formation methods, including ion beam sputtering in a controlled vacuum environment, to improve the etching resistance and maintain reflectance.

Benefits of technology

The use of Rh in the protective film significantly enhances etching resistance, particularly against oxygen-based gases, while maintaining the reflectance of the mask, thus protecting the multilayer reflective film and ensuring effective pattern transfer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024133671000001_ABST
    Figure 2024133671000001_ABST
Patent Text Reader

Abstract

To provide a technology that improves etching resistance of a protective film that protects a multilayer reflective film.SOLUTION: A reflection type mask blank includes a substrate, a multilayer reflective film that reflects EUV light, a protective film that protects the multilayer reflective film, and an absorbing film that absorbs the EUV light. The protective film contains 50 at% or more of Rh. By imaging a cross-section of the protective film with a transmission electron microscope (TEM), a band-shaped grayscale image parallel to an interface between the protective film and the multilayer reflective film is acquired, and a luminance profile of the grayscale image in the longitudinal direction of the grayscale image is created, then there are 50 or more peaks of the luminance profile per 100 nm in the longitudinal direction of the grey scale image.SELECTED DRAWING: Figure 7
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a reflective mask blank, a reflective mask, a method for manufacturing a reflective mask blank, and a method for manufacturing a reflective mask. [Background technology]

[0002] In recent years, with the miniaturization of semiconductor devices, EUV lithography (EUVL), an exposure technology using extreme ultraviolet (EUV) light, has been developed. EUV includes soft X-rays and vacuum ultraviolet light, and specifically refers to light with a wavelength of about 0.2 nm to 100 nm. At present, EUV with a wavelength of about 13.5 nm is mainly being considered.

[0003] In EUVL, a reflective mask is used. A reflective mask has, in this order, a substrate such as a glass substrate, a multilayer reflective film that reflects EUV light, a protective film that protects the multilayer reflective film, and an absorbing film that absorbs EUV light. An opening pattern is formed in the absorbing film. In EUVL, the opening pattern in the absorbing film is transferred to a target substrate such as a semiconductor substrate. Transferring includes reducing and transferring.

[0004] The protective film of Patent Document 1 contains Ru, and further contains at least one additive material selected from Al, Y, Zr, Rh, and Hf. The content of the additive material is 5 at % or more and less than 50 at %. In other words, the main component of the protective film of Patent Document 1 is Ru. Patent Document 2 also discloses a similar protective film. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 2021-056502 [Patent Document 2] Japanese Patent Publication No. 2014-170931 Summary of the Invention [Problem to be solved by the invention]

[0006] The protective film protects the multilayer reflective film from an etching gas when an opening pattern is formed in the absorbing film using the etching gas. As the etching gas, halogen-based gas, oxygen-based gas, or a mixture of these gases is being considered.

[0007] When the main component of the protective film is Ru, the etching resistance of the protective film is insufficient, particularly when an oxygen-based gas is used as the etching gas (including the case where a mixed gas is used).

[0008] One aspect of the present disclosure provides a technique for improving the etching resistance of a protective film. [Means for solving the problem]

[0009] A reflective mask blank according to an embodiment of the present disclosure includes, in this order, a substrate, a multilayer reflective film that reflects EUV light, a protective film that protects the multilayer reflective film, and an absorbing film that absorbs the EUV light. The protective film contains 50 at% or more of Rh. A cross section of the protective film is imaged with a transmission electron microscope (TEM) to obtain a band-shaped grayscale image parallel to the interface between the protective film and the multilayer reflective film, and a luminance profile of the grayscale image in the longitudinal direction is created, whereby the number of peaks in the luminance profile per 100 nm in the longitudinal direction of the grayscale image is 50 or more. Effect of the Invention

[0010] According to one embodiment of the present disclosure, the protective film uses Rh as a main component and has improved density, thereby improving the etching resistance of the protective film. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a cross-sectional view showing a reflective mask blank according to one embodiment. [Diagram 2] FIG. 2 is a cross-sectional view showing a reflective mask according to an embodiment. [Diagram 3] FIG. 3 is a cross-sectional view showing an example of EUV light reflected by the reflective mask of FIG. [Figure 4] FIG. 4 is a cross-sectional view showing a reflective mask blank according to a modified example. [Diagram 5] FIG. 5 is a diagram showing TEM images of the multilayer reflective film and the protective film of Example 1 in Table 1. [Figure 6] FIG. 6 is an enlarged view of the area enclosed by the dashed line VI in FIG. [Figure 7] FIG. 7 is a diagram showing the luminance profile of FIG. [Figure 8] FIG. 8 is a flowchart showing a method for manufacturing a reflective mask blank according to one embodiment. [Figure 9] FIG. 9 is a flowchart showing a method for manufacturing a reflective mask according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, the embodiments of the present disclosure will be described with reference to the drawings. In each drawing, the same or corresponding configurations are denoted by the same reference numerals, and the description may be omitted. In the specification, the symbol "~" indicating a range of values ​​means that the values ​​before and after the symbol are included as the lower and upper limits.

[0013] 1 to 6, the X-axis direction, the Y-axis direction, and the Z-axis direction are perpendicular to each other. The Z-axis direction is perpendicular to the first main surface 10a of the substrate 10. The X-axis direction is perpendicular to the incidence surface of the EUV light (the surface including the incident light beam and the reflected light beam). As shown in FIG. 3, when viewed from the X-axis direction, the incident light beam is inclined toward the positive Y-axis direction as it moves toward the negative Z-axis direction, and the reflected light beam is inclined toward the positive Y-axis direction as it moves toward the positive Z-axis direction.

[0014] A reflective mask blank 1 according to one embodiment will be described with reference to Fig. 1. The reflective mask blank 1 has, for example, a substrate 10, a multilayer reflective film 11, a protective film 12, an absorbing film 13, and an etching mask film 14 in this order. The multilayer reflective film 11, the protective film 12, the absorbing film 13, and the etching mask film 14 are formed in this order on a first main surface 10a of the substrate 10. It should be noted that the reflective mask blank 1 only needs to have at least the substrate 10, the multilayer reflective film 11, the protective film 12, and the absorbing film 13.

[0015] The reflective mask blank 1 may further have a functional film not shown in Fig. 1. For example, the reflective mask blank 1 may have a conductive film on the opposite side of the substrate 10 to the multilayer reflective film 11. The conductive film is formed on the second main surface 10b of the substrate 10. The second main surface 10b is the surface facing opposite to the first main surface 10a. The conductive film is used, for example, to attach the reflective mask 2 to an electrostatic chuck of an exposure device.

[0016] Although not shown, the reflective mask blank 1 may have a buffer film between the protective film 12 and the absorbing film 13. The buffer film protects the protective film 12 from an etching gas that forms an opening pattern 13a in the absorbing film 13. The buffer film is etched more slowly than the absorbing film 13. Unlike the protective film 12, the buffer film will ultimately have the same opening pattern as the opening pattern 13a of the absorbing film 13.

[0017] Next, a reflective mask 2 according to one embodiment will be described with reference to Figures 2 and 3. The reflective mask 2 is produced, for example, by using the reflective mask blank 1 shown in Figure 1, and includes an opening pattern 13a in an absorbing film 13. Note that the etching mask film 14 shown in Figure 1 is removed after the opening pattern 13a is formed in the absorbing film 13.

[0018] In EUVL, the opening pattern 13a of the absorbing film 13 is transferred to a target substrate such as a semiconductor substrate. The transfer includes reducing and transferring. The substrate 10, the multilayer reflective film 11, the protective film 12, the absorbing film 13, and the etching mask film 14 will be described below in this order.

[0019] The substrate 10 is, for example, a glass substrate. The material of the substrate 10 is preferably quartz glass containing TiO2. Quartz glass has a smaller linear expansion coefficient and a smaller dimensional change due to temperature change than general soda-lime glass. Quartz glass may contain 80% to 95% by mass of SiO2 and 4% to 17% by mass of TiO2. When the TiO2 content is 4% to 17% by mass, the linear expansion coefficient is approximately zero near room temperature, and there is almost no dimensional change near room temperature. Quartz glass may contain a third component or impurities other than SiO2 and TiO2. The material of the substrate 10 may be crystallized glass in which a β-quartz solid solution is precipitated, silicon, metal, or the like.

[0020] The substrate 10 has a first main surface 10a and a second main surface 10b facing opposite to the first main surface 10a. A multilayer reflective film 11 and the like are formed on the first main surface 10a. The size of the substrate 10 in plan view (viewed in the Z-axis direction) is, for example, 152 mm long and 152 mm wide. The vertical and horizontal dimensions may be 152 mm or more. The first main surface 10a and the second main surface 10b each have, for example, a square quality assurance area in the center. The size of the quality assurance area is, for example, 142 mm long and 142 mm wide. The quality assurance area of ​​the first main surface 10a preferably has a root mean square roughness (RMS) of 0.150 nm or less and a flatness of 100 nm or less. In addition, it is preferable that the quality assurance area of ​​the first main surface 10a does not have a defect that causes a phase defect.

[0021] The multilayer reflective film 11 reflects EUV light. The multilayer reflective film 11 is, for example, formed by alternately laminating a high refractive index layer and a low refractive index layer. The material of the high refractive index layer is, for example, silicon (Si), and the material of the low refractive index layer is, for example, molybdenum (Mo), and a Mo / Si multilayer reflective film is used. Note that a Ru / Si multilayer reflective film, a Mo / Be multilayer reflective film, a Mo compound / Si compound multilayer reflective film, a Si / Mo / Ru multilayer reflective film, a Si / Mo / Ru / Mo multilayer reflective film, a Si / Ru / Mo / Ru multilayer reflective film, etc. can also be used as the multilayer reflective film 11.

[0022] The film thickness of each layer constituting the multilayer reflective film 11 and the number of repeating units of the layer can be appropriately selected according to the material of each layer and the reflectivity with respect to EUV light. When the multilayer reflective film 11 is a Mo / Si multilayer reflective film, in order to achieve a reflectivity of 60% or more with respect to EUV light with an incident angle θ (see Fig. 3) of 6°, a Mo film with a film thickness of 2.3 ± 0.1 nm and a Si film with a film thickness of 4.5 ± 0.1 nm may be laminated so that the number of repeating units is 30 or more and 60 or less. The multilayer reflective film 11 preferably has a reflectivity of 60% or more with respect to EUV light with an incident angle θ of 6°. More preferably, the reflectivity is 65% or more.

[0023] The film formation method of each layer constituting the multilayer reflective film 11 is, for example, a DC sputtering method, a magnetron sputtering method, or an ion beam sputtering method. When forming a Mo / Si multilayer reflective film using the ion beam sputtering method, an example of the film formation conditions for each of the Mo film and the Si film is as follows. <Film formation conditions of Si film> Target: Si target, Sputtering gas: Ar gas, Gas pressure: 0.013 Pa to 0.027 Pa, Ion acceleration voltage: 300 V to 1500 V, Film formation rate: 0.030 nm / sec to 0.300 nm / sec, Film thickness of Si film: 4.5 ± 0.1 nm. <Film formation conditions of Mo film> Target: Mo target, Sputtering gas: Ar gas, Gas pressure: 0.013 Pa to 0.027 Pa, Ion acceleration voltage: 300 V to 1500 V, Film deposition rate: 0.030 nm / sec to 0.300 nm / sec, Thickness of Mo film: 2.3 ± 0.1 nm. <Repeating unit of Si film and Mo film> Number of repeating units: 30 to 60 (preferably 40 to 50).

[0024] The protective film 12 is formed between the multilayer reflective film 11 and the absorption film 13 and protects the multilayer reflective film 11. The protective film 12 protects the multilayer reflective film 11 from the etching gas that forms the opening pattern 13a (see FIG. 2) in the absorption film 13. The protective film 12 remains on the multilayer reflective film 11 without being removed during the manufacture of the reflective mask 2.

[0025] The etching gas is, for example, a halogen-based gas, an oxygen-based gas, or a mixed gas thereof. Examples of the halogen-based gas include a chlorine-based gas and a fluorine-based gas. Examples of the chlorine-based gas include Cl2 gas, SiCl4 gas, CHCl3 gas, CCl4 gas, BCl3 gas, or a mixed gas thereof. Examples of the fluorine-based gas include CF4 gas, CHF3 gas, SF6 gas, BF3 gas, XeF2 gas, or a mixed gas thereof. The oxygen-based gas is O2 gas, O3 gas, or a mixed gas thereof. The oxygen-based gas is preferably used when the main component of the absorption film 13 is ruthenium (Ru).

[0026] The ratio (ER1 / ER2) of the etching rate ER1 of the absorption film 13 by the etching gas to the etching rate ER2 of the protective film 12 by the etching gas is also called the selection ratio. The greater the selection ratio, the better the processability of the absorption film 13. The selection ratio is preferably 10 or more, more preferably 30 or more. The selection ratio is preferably 200 or less, more preferably 100 or less.

[0027] The protective film 12 contains Rh in an amount of 50 at % or more and 100 at % or less. From the viewpoint of productivity, the protective film 12 is preferably made of a single layer as shown in FIG. 1, etc., but from the viewpoint of multi-functionality, it may be made of multiple layers as shown in FIG. 4. For example, the protective film 12 may have a lower layer 12L and an upper layer 12U. The lower layer 12L and the upper layer 12U are formed in this order on the multilayer reflective film 11. In any case, it is sufficient that the protective film 12 as a whole contains 50 at % or more of Rh.

[0028] The protective film 12 contains Rh as a main component. By using Rh instead of Ru as the main component of the protective film 12, it is possible to improve the etching resistance of the protective film 12. In particular, when an oxygen-based gas is used as an etching gas (including the case where a mixed gas is used), it is possible to improve the etching resistance of the protective film 12.

[0029] Resistance to SPM can also be improved by using Rh instead of Ru as the main component of protective film 12. SPM is used for removing resist films, which will be described later, or for cleaning reflective mask 2. Furthermore, reduction in reflectance to EUV light can be suppressed by using Rh instead of Ru as the main component of protective film 12.

[0030] The protective film 12 has a number of peaks Np per 100 nm in the longitudinal direction of a grayscale image, which will be described later, of 50 or more. Hereinafter, the number of peaks Np per 100 nm in the longitudinal direction of a grayscale image in the luminance profile will also be simply referred to as the number of peaks Np.

[0031] The grayscale image is obtained by imaging the cross section of the protective film 12 with a transmission electron microscope (TEM). The electron acceleration voltage of the TEM is, for example, 200 kV. The grayscale image has, for example, 256 gradations, a magnification of 2.5 million times, and a resolution of 0.16 nm / pixel.

[0032] The grayscale image captured by the TEM may include a cross section of the multilayer reflective film 11 in addition to the cross section of the protective film 12, as shown in Fig. 5. The grayscale image for creating the brightness profile (an image of the region surrounded by dashed line VI in Fig. 5) is a strip parallel to the interface between the protective film 12 and the multilayer reflective film 11, and is cut out on the center line of the protective film 12 in the thickness direction.

[0033] The grayscale image for creating the luminance profile has a vertical dimension of 1 nm and a horizontal dimension of 74 nm. The vertical direction is the direction perpendicular to the interface between the protective film 12 and the multilayer reflective film 11 (Z-axis direction). The horizontal direction is the direction parallel to the interface between the protective film 12 and the multilayer reflective film 11 (Y-axis or X-axis direction). The horizontal dimension may be 60 nm or more.

[0034] The brightness profile is created using the Plot profile function of ImageJ (version 1.53e) distributed by the National Institutes of Health (NIH). ImageJ is an open source, public domain image processing software.

[0035] The intensity of the intensity profile is output as the average value of 1 nm in the vertical direction. The intensity profile is smoothed by polynomial approximation using the least squares method. For smoothing, a Savitzky-Golay filter is used using Python 3. The filter is expressed in the Python code as follows: savgol_filter(x,y,z) x: Brightness y: window_length (coarseness of the filter when smoothing) z: polynomial_order (the order of the polynomial approximation used for smoothing) x is the total intensity in the intensity profile acquired in the lateral direction from the TEM image, y is 11, and z is 5.

[0036] Figure 7 shows an example of a smoothed intensity profile. In Figure 7, the horizontal axis represents the longitudinal position of the grayscale image, the vertical axis represents the magnitude of the intensity, and the black circle represents the position of the peak. The peak of the smoothed intensity profile is detected by scipy.signal.argrelmax. The order value of signal.argrelmax is 2.

[0037] The number of peaks Np is calculated by the following formula (1): Np = Np0 × (100 / L X0 ) · · · (1) In the above formula (1), Np0 is the number of peaks in the luminance profile, L X0 is the lateral dimension of the brightness profile (unit: nm). L X0 For example, L is 74 nm. X0 It is sufficient that the thickness is 60 nm or more.

[0038] In a grayscale image captured by a TEM, the brightness of the image differs between the inside of a crystal and the grain boundaries. In the image, the grain boundaries are brighter than the inside of the crystal. The denser the protective film 12, the smaller the crystal grain size, the more grain boundaries there are, and the greater the number of peaks Np. The denser the protective film 12, the better the etching resistance. Therefore, the greater the number of peaks Np, the better the etching resistance. The number of peaks Np is preferably 50 or more, and more preferably 55 or more. The number of peaks Np is also preferably 120 or less, and more preferably 100 or less.

[0039] According to the findings of the present inventors, when the main component of the protective film 12 is Rh, if the multilayer reflective film 11 is formed by magnetron sputtering and then the protective film 12 is formed by ion beam sputtering, the protective film 12 has low density and the number of peaks Np is less than 50. When the main component of the protective film 12 is Ru, even if the multilayer reflective film 11 is formed by magnetron sputtering and then the protective film 12 is formed by ion beam sputtering, the protective film 12 has high density and the number of peaks Np is 50 or more.

[0040] When the multilayer reflective film 11 and the protective film 12 are formed by different methods, a vacuum chamber used for forming the multilayer reflective film 11 and a vacuum chamber used for forming the protective film 12 are provided separately. Therefore, after the formation of the multilayer reflective film 11 and before the formation of the protective film 12, the multilayer reflective film 11 is exposed to the atmosphere, and the top layer of the multilayer reflective film 11 is oxidized. The top layer of the multilayer reflective film 11 refers to the layer that contacts the protective film 12 among the multiple layers that constitute the multilayer reflective film 11. When the main component of the protective film 12 is Rh, unlike when the main component of the protective film 12 is Ru, it is considered that the density of the protective film 12 decreases when the top layer of the multilayer reflective film 11 is oxidized.

[0041] The present inventors, as will be described in detail in the Examples section, have found that even when the main component of protective film 12 is Rh, the denseness of protective film 12 can be improved by depositing multilayer reflective film 11 and protective film 12 in this order in the same vacuum chamber. In other words, the present inventors have found that even when the main component of protective film 12 is Rh, the denseness of protective film 12 can be improved by suppressing exposure of multilayer reflective film 11 to the atmosphere and suppressing oxidation of the uppermost layer of multilayer reflective film 11.

[0042] The multilayer reflective film 11 has a Si film having an oxygen atom content of preferably 15 at % or less as the uppermost layer in contact with the protective film 12. The oxygen atom content of the Si film, which is the uppermost layer of the multilayer reflective film 11, is measured by, for example, TEM-EDX (Energy Dispersive X-ray).

[0043] By depositing the multilayer reflective film 11 and the protective film 12 in this order in the same vacuum chamber, it is possible to suppress oxidation of the Si film that is the uppermost layer of the multilayer reflective film 11, and to reduce the O content of the Si film that is the uppermost layer to 15 at% or less. The O content of the Si film that is the uppermost layer is more preferably 10 at% or less, and further preferably 5 at% or less.

[0044] It is preferable to control the pressure of the vacuum chamber to 0.035 Pa or less when forming the protective film 12. If the pressure of the vacuum chamber is 0.035 Pa or less, the degree of vacuum is high and oxidation is suppressed. The pressure of the vacuum chamber is more preferably 0.030 Pa or less. Moreover, the pressure of the vacuum chamber may be 0.001 Pa or more.

[0045] The multilayer reflective film 11 and the protective film 12 are formed in the same vacuum chamber, and therefore are formed by the same film formation method. From the viewpoint of the degree of vacuum, the ion beam sputtering method is suitable as the film formation method. With the ion beam sputtering method, the vacuum chamber and the plasma source can be separated, and the degree of vacuum of the vacuum chamber can be increased.

[0046] According to the findings of the present inventors, for example, when forming a protective film by ion beam sputtering, the number of peaks Np of the protective film 12 can be adjusted by adjusting the ion acceleration voltage. By reducing the ion acceleration voltage, the energy of the sputtered particles decreases, the density of the protective film 12 increases, and the gas barrier properties of the protective film 12 improve. Specifically, by setting the ion acceleration voltage to 400V or more and 800V or less, the number of peaks Np can be set to 50 or more.

[0047] According to the findings of the present inventors, for example, when forming a protective film by ion beam sputtering, the number of peaks Np of protective film 12 can be adjusted by adjusting the gas pressure of the sputtering gas (e.g., Ar). By adjusting the gas pressure of the sputtering gas, the energy of the sputtered particles decreases, and the density of protective film 12 increases. Therefore, the number of peaks Np can be made 50 or more. Specifically, the number of peaks Np can be made 50 or more by setting the gas pressure of the sputtering gas to 0.0050 Pa or more and 0.050 Pa or less.

[0048] The protective film 12 may contain only Rh as a metal element, or may contain, in addition to Rh, at least one element X selected from Ru, Pd, Ir, Pt, Zr, Nb, Ta, and Ti. The protective film 12 is formed of Rh alone or an Rh compound. The Rh compound contains Rh and X. Ru, Zr, Nb, and Ti can improve the reflectance to EUV light. Pd, Ir, and Pt can improve the etching resistance. Ta can improve the resistance to hydrogen.

[0049] When the protective film 12 contains, as a metal element, Rh and at least one element X selected from Ru, Pd, Ir, Pt, Zr, Nb, Ta, and Ti, the element ratio of Rh to X (Rh:X) is preferably 50:50 to 99:1. In this specification, the element ratio means a molar ratio. The element ratio (Rh:X) is more preferably 70:30 to 95:5.

[0050] In addition to the above metal elements, the protective film 12 may contain at least one nonmetallic element selected from O, N, C, and B. The Rh compound constituting the protective film 12 may contain at least Rh and a nonmetallic element, and may further contain X. By adding a nonmetallic element to a metal element, crystallization of the protective film 12 can be suppressed, and the surface of the protective film 12 can be formed smoothly. Therefore, the absorbing film 13 formed on the protective film 12 can be formed smoothly. In addition, the reflectance to EUV light can be improved.

[0051] The thickness of the protective film 12 is preferably 1.5 nm to 4.0 nm, more preferably 2.0 nm to 3.5 nm. If the thickness of the protective film 12 is 1.5 nm or more, the etching resistance is good. If the thickness of the protective film 12 is 4.0 nm or less, the decrease in reflectance to EUV light can be suppressed.

[0052] The film density of the protective film 12 is preferably 10.0 g / cm 3 More than 14.0g / cm 3 The film density of the protective film 12 is 10.0 g / cm or less. 3If the film density of the protective film 12 is 14.0 g / cm or more, the etching resistance is good. 3 If it is equal to or less than this, a decrease in reflectance for EUV light can be suppressed.

[0053] The upper surface of the protective film 12, i.e., the surface of the protective film 12 on which the absorbing film 13 is formed, preferably has a root-mean-square roughness RMS of 0.300 nm or less, more preferably 0.150 nm or less. If the root-mean-square roughness RMS is 0.300 nm or less, the absorbing film 13 and the like can be formed smoothly on the protective film 12. In addition, scattering of EUV light can be suppressed, and the reflectance for EUV light can be improved. The root-mean-square roughness RMS is preferably 0.050 nm or more.

[0054] 4, the protective film 12 may be composed of multiple layers, and may include, for example, a lower layer 12L and an upper layer 12U. The lower layer 12L and the upper layer 12U are formed in this order on the multilayer reflective film 11. In other words, the lower layer 12L is provided between the upper layer 12U and the multilayer reflective film 11.

[0055] The upper layer 12U contains Rh in an amount of 50 at % or more and 100 at % or less. The upper layer 12U containing Rh as a main component has the following effects (A) to (C). (A) The etching resistance of the absorbing film 13 can be improved. In particular, when an oxygen-based gas is used as the etching gas, the etching resistance of the protective film 12 can be improved. (B) The resistance to sulfuric acid / hydrogen peroxide can be improved. (C) The reflectance to EUV light can be improved.

[0056] The upper layer 12U may contain only Rh as a metal element, or may contain, in addition to Rh, at least one element X selected from Ru, Pd, Ir, Pt, Zr, Nb, Ta, and Ti. The upper layer 12U is formed of Rh alone or an Rh compound. The Rh compound contains Rh and X. The element ratio of Rh to X (Rh:X) in the upper layer 12U is preferably 99:1 to 1:1, and more preferably 70:30 to 95:5.

[0057] The upper layer 12U may contain at least one nonmetallic element selected from O, N, C, and B in addition to the above metal elements. The Rh compound constituting the upper layer 12U may contain at least Rh and a nonmetallic element, and may further contain X. By adding a nonmetallic element to a metal element, crystallization of the protective film 12 can be suppressed, and the surface of the protective film 12 can be formed smoothly. Therefore, the absorbing film 13 and the like can be formed smoothly on the protective film 12. In addition, scattering of EUV light can be suppressed, and the reflectance for EUV light can be improved.

[0058] The thickness of the upper layer 12U is preferably 0.1 nm to 4.0 nm, more preferably 0.2 nm to 3.5 nm, even more preferably 0.5 nm to 3.0 nm, and particularly preferably 1.0 nm to 2.5 nm. If the thickness of the upper layer 12U is 0.1 nm or more, the etching resistance is good. Furthermore, if the thickness of the upper layer 12U is 4.0 nm or less, the decrease in reflectance to EUV light can be suppressed.

[0059] The lower layer 12L preferably contains Ru, Pd, Ir, Pt, Zr, Nb, Ta or Ti in an amount of 50 at% or more and 100 at% or less. In other words, the main component of the lower layer 12L is a metal element other than Rh, and is preferably Ru, Pd, Ir, Pt, Zr, Nb, Ta or Ti. In other words, the lower layer 12L is formed of a simple substance or a compound of the above metal element. Ru, Zr, Nb and Ti can improve the reflectance to EUV light. Pd, Ir and Pt can improve the etching resistance of the protective film 12. Ta can improve the resistance to hydrogen. The main component of the lower layer 12L is more preferably Ru.

[0060] In addition to the above metal elements, the lower layer 12L may contain at least one nonmetal element selected from O, N, C, and B. The metal compound constituting the lower layer 12L may contain at least the above metal elements and nonmetal elements.

[0061] The thickness of the lower layer 12L is preferably 0.5 nm or more and 2.0 nm or less, more preferably 0.5 nm or more and 1.5 nm or less. If the thickness of the lower layer 12L is 0.5 nm or more, diffusion of the material of the upper layer 12U into the multilayer reflective film 11 can be suppressed. Also, if the thickness of the lower layer 12L is 2.0 nm or less, a decrease in reflectivity with respect to EUV light can be suppressed. The thickness of the lower layer 12L containing a metal element other than Rh as a main component is preferably thinner than the thickness of the upper layer 12U containing Rh as a main component. However, as long as the protective film 12 contains 50 at% or more of Rh as a whole, the thickness of the lower layer 12L may be thicker than the thickness of the upper layer 12U.

[0062] When forming a Ru film as the lower layer 12L using the ion beam sputtering method, an example of the film formation conditions is as follows. <Film formation conditions of Ru film (lower layer)> Target: Ru target, Sputtering gas: Ar gas, Gas pressure: 0.010 Pa to 0.020 Pa, Ion acceleration voltage: 300 V to 1500 V, Film formation rate: 0.010 nm / sec to 0.100 nm / sec, Film thickness of Ru film: 0.5 nm to 2.0 nm.

[0063] When forming a Rh film as the upper layer 12U using the ion beam sputtering method, an example of the film formation conditions is as follows. <Film formation conditions of Rh film (upper layer)> Target: Rh target, Sputtering gas: Ar gas, Gas pressure: 0.010 Pa to 0.035 Pa, Ion acceleration voltage: 300 V to 1500 V, Film formation rate: 0.010 nm / sec to 0.100 nm / sec, Film thickness of Rh film: 0.5 nm to 4.0 nm.

[0064] The absorbing film 13 is a film in which an opening pattern 13a is formed. The opening pattern 13a is not formed in the manufacturing process of the reflective mask blank 1, but is formed in the manufacturing process of the reflective mask 2. The absorbing film 13 may not only absorb EUV light, but also shift the phase of the EUV light. That is, the absorbing film 13 may be a phase shift film. The phase shift film shifts the phase of the second EUV light L2 with respect to the first EUV light L1 shown in FIG. 3.

[0065] The first EUV light L1 is light that passes through the opening pattern 13a without passing through the absorbing film 13, is reflected by the multilayer reflective film 11, and passes through the opening pattern 13a without passing through the absorbing film 13 again. The second EUV light L2 is light that passes through the absorbing film 13 while being absorbed by the absorbing film 13, is reflected by the multilayer reflective film 11, and passes through the absorbing film 13 while being absorbed by the absorbing film 13 again.

[0066] The phase difference (≧0) between the first EUV light L1 and the second EUV light L2 is, for example, 170° to 250°. The phase of the first EUV light L1 may be ahead of or behind the phase of the second EUV light L2. The absorbing film 13 improves the contrast of the transferred image by utilizing the interference between the first EUV light L1 and the second EUV light L2. The transferred image is an image obtained by transferring the opening pattern 13a of the absorbing film 13 onto the target substrate.

[0067] In EUVL, a so-called projection effect (shadowing effect) occurs. The shadowing effect refers to a region in which the sidewall of the opening pattern 13a blocks the EUV light due to the incident angle θ of the EUV light being not 0° (for example, 6°), resulting in a positional or dimensional shift of the transferred image. In order to reduce the shadowing effect, it is effective to lower the height of the sidewall of the opening pattern 13a, and it is also effective to thin the absorbing film 13.

[0068] The thickness of the absorbing film 13 is, for example, 60 nm or less, and preferably 50 nm or less, in order to reduce the shadowing effect. The thickness of the absorbing film 13 is preferably 20 nm or more, and more preferably 30 nm or more, in order to ensure a phase difference between the first EUV light L1 and the second EUV light L2.

[0069] The absorbing film 13 preferably contains at least one metal element selected from Ru, Ta, Cr, Nb, Pt, Ir, Re, W, Mn, Au, Si, and Al. These metal elements have a relatively small refractive index, so that the thickness of the phase shift film can be reduced while maintaining the phase difference. Among the above metal elements, the absorbing film 13 preferably contains Ru. The absorbing film 13 is formed of a simple substance or a compound of the above metal elements.

[0070] The absorbing film 13 contains at least one nonmetallic element selected from O, N, C, and B in addition to the above metal elements. The compound constituting the absorbing film 13 may contain the above metal elements and nonmetallic elements. By adding a nonmetallic element to a metal element, crystallization of the absorbing film 13 can be suppressed, and roughness of the sidewall of the opening pattern 13a can be reduced. The absorbing film 13 preferably contains oxygen as a nonmetallic element, and more preferably contains oxygen and nitrogen.

[0071] The refractive index n of the absorbing film 13 is preferably 0.930 or less, more preferably 0.920 or less, even more preferably 0.910 or less, and particularly preferably 0.90 or less. The refractive index n is preferably 0.885 or more. In this specification, the refractive index is the refractive index for light with a wavelength of 13.5 nm.

[0072] The extinction coefficient k of the absorbing film 13 is preferably 0.015 or more, and more preferably 0.020 or more. The extinction coefficient k is preferably 0.065 or less. In this specification, the extinction coefficient is the extinction coefficient for light with a wavelength of 13.5 nm.

[0073] The absorption film 13 preferably has an etching rate of 0 nm / min to 0.05 nm / min with sulfuric acid peroxide. If the etching rate of the absorption film 13 with sulfuric acid peroxide is 0.05 nm / min or less, damage to the absorption film 13 during cleaning can be suppressed.

[0074] Examples of the method for forming the absorption film 13 include the DC sputtering method, the magnetron sputtering method, the ion beam sputtering method, or reactive sputtering. The oxygen content of the absorption film 13 can be controlled by the content of O2 gas in the sputtering gas. Also, the nitrogen content of the absorption film 13 can be controlled by the content of N2 gas in the sputtering gas.

[0075] When forming a RuN film as the absorption film 13 using the reactive sputtering method, an example of the film formation conditions is as follows. <Film Formation Conditions of RuN Film> Target: Ru target, Sputtering gas: Mixed gas of Ar gas and N2 gas, Volume ratio of N2 gas in the sputtering gas (N2 / (Ar + N2)): 0.3 to 0.7, Gas pressure: 0.05 Pa to 0.40 Pa, Input power: 100 W to 300 W, Film formation rate: 0.010 nm / sec to 0.030 nm / sec, Film thickness: 20 nm to 60 nm.

[0076] The etching mask film 14 is formed on the side opposite to the protective film 12 with respect to the absorption film 13 and is used to form the opening pattern 13a in the absorption film 13. A resist film (not shown) is provided on the etching mask film 14. In the manufacturing process of the reflective mask 2, first, a first opening pattern is formed in the resist film, then a second opening pattern is formed in the etching mask film 14 using the first opening pattern, and then a third opening pattern 13a is formed in the absorption film 13 using the second opening pattern. The first opening pattern, the second opening pattern, and the third opening pattern 13a have the same dimensions and the same shape in a plan view (viewed in the Z-axis direction). The etching mask film 14 enables thinning of the resist film.

[0077] The etching mask film 14 preferably contains at least one metal element selected from Cr, Nb, Ti, Mo, Ta, and Si. The etching mask film 14 is formed of a simple substance or a compound of the above metal element. In addition to the above metal element, the etching mask film 14 may contain at least one nonmetal element selected from O, N, C, and B. The compound constituting the etching mask film 14 may contain the above metal element and the nonmetal element.

[0078] The thickness of the etching mask film 14 is preferably 2 nm or more and 30 nm or less, more preferably 2 nm or more and 25 nm or less, and further preferably 2 nm or more and 10 nm or less.

[0079] The etching mask film 14 may be formed by, for example, DC sputtering, magnetron sputtering, or ion beam sputtering.

[0080] Next, a manufacturing method of a reflective mask blank 1 according to one embodiment will be described with reference to Fig. 8. The manufacturing method of the reflective mask blank 1 includes, for example, steps S101 to S105 shown in Fig. 8. In step S101, a substrate 10 is prepared. In step S102, a multilayer reflective film 11 is formed on a first main surface 10a of the substrate 10. In step S103, a protective film 12 is formed on the multilayer reflective film 11. In step S104, an absorbing film 13 is formed on the protective film 12. In step S105, an etching mask film 14 is formed on the absorbing film 13.

[0081] The method for manufacturing the reflective mask blank 1 only needs to include at least steps S101 to S104. The method for manufacturing the reflective mask blank 1 may further include a step of forming a functional film not shown in FIG.

[0082] Next, a method for manufacturing a reflective mask 2 according to an embodiment will be described with reference to FIG. 9. The method for manufacturing a reflective mask 2 includes steps S201 to S204 shown in FIG. 9. In step S201, a reflective mask blank 1 is prepared. In step S202, an etching mask film 14 is processed. A resist film (not shown) is provided on the etching mask film 14. First, a first opening pattern is formed in the resist film, and then a second opening pattern is formed in the etching mask film 14 using the first opening pattern. In step S203, a third opening pattern 13a is formed in the absorbing film 13 using the second opening pattern. In step S203, the absorbing film 13 is etched using an etching gas. In step S204, the resist film and the etching mask film 14 are removed. For example, sulfuric acid / hydrogen peroxide is used to remove the resist film. For example, an etching gas is used to remove the etching mask film 14. The etching gas used in step S204 (removal of the etching mask film 14) may be the same as the etching gas used in step S203 (etching the absorbing film 13). The method for manufacturing the reflective mask 2 only needs to include at least steps S201 and S203. EXAMPLES

[0083] Experimental data will be described below. Examples 1 to 4 are working examples, and Examples 3 and 5 are comparative examples.

[0084] [Example 1] In Example 1, a reflective mask blank was produced that included a substrate, a multilayer reflective film, a protective film, and an absorbing film in that order. A SiO2-TiO2-based glass substrate (6-inch (152 mm) square outer dimensions, 6.3 mm thick) was prepared as the substrate. This glass substrate had a thermal expansion coefficient of 0.02×10 at 20°C. -7 / °C, Young's modulus is 67 GPa, Poisson's ratio is 0.17, and specific stiffness is 3.07 × 10 7 m 2 / s 2It was as follows. The quality assurance area of the first main surface of the substrate had a root mean square roughness (RMS) of 0.150 nm or less and a flatness of 100 nm or less by polishing. On the second main surface of the substrate, a Cr film with a thickness of 100 nm was formed using the magnetron sputtering method. The sheet resistance of the Cr film was 100 Ω / □.

[0085] As the multilayer reflective film, a Mo / Si multilayer reflective film was formed. The Mo / Si multilayer reflective film was formed by repeating 40 times the film formation of a Si film (film thickness: 4.5 nm) and a Mo film (film thickness: 2.3 nm) using the ion beam sputtering method. The total film thickness of the Mo / Si multilayer reflective film was 272 nm ((4.5 nm + 2.3 nm) × 40). On the outermost layer, a Si film was used to prevent oxidation of the Mo film. Generally, the Mo film is more likely to oxidize than the Si film.

[0086] The film formation conditions for the Si film and the Mo film were as follows. <Film formation conditions for Si film> Target: Si target (boron-doped), Sputtering gas: Ar gas, Gas pressure: 0.020 Pa, Ion acceleration voltage: 700 V, Film formation rate: 0.077 nm / sec, Film thickness: 4.5 nm. <Film formation conditions for Mo film> Target: Mo target, Sputtering gas: Ar gas, Gas pressure: 0.020 Pa, Ion acceleration voltage: 700 V, Film formation rate: 0.064 nm / sec, Film thickness: 2.3 nm.

[0087] As the protective film, a Rh film (single layer) was formed. The Rh film was formed using the ion beam sputtering method. The multilayer reflective film and the protective film were formed in this order in the same vacuum chamber. After the formation of the multilayer reflective film and before the formation of the protective film, the multilayer reflective film was not exposed to the atmosphere, and the outermost layer of the multilayer reflective film was not oxidized. The film formation conditions for the Rh film were as follows. <Film formation conditions of Rh film (single layer)> Target: Rh target, Sputtering gas: Ar gas, Gas pressure: 0.027 Pa, Ion acceleration voltage: 600 V, Film formation rate: 0.077 nm / sec, Film thickness: 3.0 nm.

[0088] As the absorption film, a RuN film (film thickness 39 nm) was formed. The RuN film was formed using the reactive sputtering method. The film formation conditions of the RuN film were as follows. <Film formation conditions of RuN film> Target: Ru target, Sputtering gas: Mixed gas of Ar gas and N2 gas, Volume ratio of N2 gas in sputtering gas (N2 / (Ar + N2)): 0.5, Gas pressure: 0.20 Pa, Input power: 200 W, Film formation rate: 0.017 nm / sec, Film thickness: 39 nm.

[0089] A reflective mask blank was obtained by the above procedure. The O content of the Si film, which is the top layer of the multilayer reflective film, the number of peaks Np of the protective film, and the etching resistance of the protective film were measured in the state before forming the absorption film.

[0090] The O content of the Si film, which is the top layer of the multilayer reflective film, was measured using TEM-EDX (manufactured by JEOL Ltd., product name ARM200F) before performing the following etching test. The measurement lower limit was 4 at%.

[0091] The number of peaks Np of the protective film was measured using TEM (manufactured by JEOL Ltd., product name ARM200F) before performing the following etching test. The measurement procedure was as described above. The larger the number of peaks Np, the denser the protective film is considered to be.

[0092] The etching test was carried out using an ICP (inductively coupled plasma) etching device. The specific etching conditions were as follows: <Etching conditions> ICP antenna bias: 200W, Substrate bias: 550W, Etching time: 15 sec. Trigger pressure: 3.5×10 2 Pa, Etching pressure: 3.0×10 -1 Pa, Etching gas: a mixture of Cl2 gas and O2 gas, Gas flow rate (Cl2 gas / O2 gas): 10sccm / 10sccm.

[0093] The etching resistance of the protective film was evaluated based on the amount of etching gas transmitted, that is, the increase in the number of chlorine atoms or oxygen atoms in the multilayer reflective film.

[0094] Before the etching test, the multilayer reflective coating did not contain chlorine atoms. Therefore, after the etching test, a line profile of the chlorine atom content (unit: at%) in the depth direction (Z-axis negative direction in FIG. 5) was obtained using TEM-EDX, and the maximum value T Clmax I asked for T Clmax The smaller the value, the more difficult it is for chlorine atoms to permeate the protective film, and the better the etching resistance of the protective film.

[0095] Before the etching test, the multilayer reflective film may contain oxygen atoms. The multilayer reflective film may be oxidized during deposition. Therefore, a line profile of the oxygen atom content (unit: at%) in the depth direction (Z-axis negative direction in FIG. 5) was obtained using TEM-EDX before and after the etching test, and the maximum value T of the difference (>0) between the two line profiles was obtained. Omax I asked for T Omax The smaller the value, the more difficult it is for oxygen atoms to permeate the protective film, and the better the etching resistance of the protective film.

[0096] [Example 2] In Example 2, an EUV mask blank was fabricated under the same conditions as in Example 1, except that an Ru film (lower layer) and an Rh film (upper layer) were formed as the protective film under the following conditions. The multilayer reflective film and the protective film were formed in the same vacuum chamber in this order. After the formation of the multilayer reflective film and before the formation of the protective film, the multilayer reflective film was not exposed to the atmosphere, and the outermost layer of the multilayer reflective film was not oxidized. Also, in Example 2, the number of peaks Np of the protective film and the etching resistance of the protective film were measured in the same procedure as in Example 1. <Film formation conditions of Ru film (lower layer)> Target: Ru target, Sputtering gas: Ar gas, Gas pressure: 0.027 Pa, Ion acceleration voltage: 600 V, Film formation rate: 0.056 nm / sec, Film thickness: 1.0 nm. <Film formation conditions of Rh film (upper layer)> Target: Rh target, Sputtering gas: Ar gas, Gas pressure: 0.027 Pa, Ion acceleration voltage: 600 V, Film formation rate: 0.077 nm / sec, Film thickness: 1.5 nm.

[0097] [Example 3] In Example 3, an EUV mask blank was fabricated under the same conditions as in Example 1, except that an Rh film (single layer) was formed as the protective film under the following conditions. The Rh film was formed by DC magnetron sputtering. Therefore, the multilayer reflective film and the protective film were formed in different vacuum chambers. After the formation of the multilayer reflective film and before the formation of the protective film, the multilayer reflective film was exposed to the atmosphere, and the outermost layer of the multilayer reflective film was oxidized. Also, in Example 3, the number of peaks Np of the protective film and the etching resistance of the protective film were measured in the same procedure as in Example 1. <Film formation conditions of Rh film (single layer)> Target: Rh target, Sputtering gas: Ar gas, Gas pressure: 0.130 Pa, Input power: 300 W, Film formation rate: 0.090 nm / sec, Film thickness: 2.5 nm.

[0098] [Example 4] In Example 4, an Rh film (single layer) was formed as the protective film. An EUV mask blank was fabricated under the same conditions as in Example 1 except for the film thickness of the Rh film (single layer). The multilayer reflective film and the protective film were formed in the same vacuum chamber in this order. After the formation of the multilayer reflective film and before the formation of the protective film, the multilayer reflective film was not exposed to the atmosphere, and the outermost layer of the multilayer reflective film was not oxidized. Also, in Example 4, the number of peaks Np of the protective film and the etching resistance of the protective film were measured in the same procedure as in Example 1. <Film formation conditions of Rh film (single layer)> Target: Rh target, Sputtering gas: Ar gas, Gas pressure: 0.027 Pa, Ion acceleration voltage: 600 V, Film formation rate: 0.077 nm / sec, Film thickness: 2.5 nm.

[0099] [Example 5] In Example 5, an EUV mask blank was fabricated under the same conditions as in Example 1 except that an Ru film (lower layer) and an Rh film (upper layer) were formed as the protective film under the following conditions. The multilayer reflective film and the protective film were formed in the vacuum chamber in this order. After the formation of the multilayer reflective film and before the formation of the Ru film (lower layer) which is the protective film, the multilayer reflective film was not exposed to the atmosphere. After the formation of the Ru film (lower layer), the Ru film (lower layer) was exposed to the atmosphere, and the outermost layer of the multilayer reflective film was oxidized. After the atmospheric exposure, the Rh film (upper layer) was formed on the Ru film (lower layer). Also, in Example 5, the number of peaks Np of the protective film and the etching resistance of the protective film were measured in the same procedure as in Example 1. <Film formation conditions of Ru film (lower layer)> Target: Ru target, Sputtering gas: Ar gas, Gas pressure: 0.027 Pa, Ion acceleration voltage: 600 V, Film formation rate: 0.056 nm / sec, Film thickness: 1.0 nm. <Film formation conditions of Rh film (upper layer)> Target: Rh target, Sputtering gas: Ar gas, Gas pressure: 0.027Pa, Ion acceleration voltage: 600V, Deposition rate: 0.077nm / sec, Film thickness: 2.0 nm.

[0100] [result] Table 1 shows the results of Examples 1 to 5.

[0101] [Table 1] As shown in Table 1, in Examples 1 to 4, unlike Examples 3 and 5, the multilayer reflective film and the protective film were formed successively without exposure to the atmosphere, so the Si film, which is the top layer of the multilayer reflective film, was not oxidized and the O content of the Si film was 15 at % or less. Also, in Examples 1 to 4, unlike Examples 3 and 5, the number of peaks Np of the protective film was 50 or more, and the T Clmax and T Omax Furthermore, in Examples 1 and 2, the root mean square roughness RMS of the protective film surface was smaller than that in Example 3.

[0102] The reflective mask blank, the reflective mask, the manufacturing method of the reflective mask blank, and the manufacturing method of the reflective mask according to the present disclosure have been described above, but the present disclosure is not limited to the above-mentioned embodiments. Various changes, modifications, substitutions, additions, deletions, and combinations are possible within the scope of the claims. These naturally fall within the technical scope of the present disclosure.

[0103] This application claims priority based on Patent Application No. 2022-061684 filed with the Japan Patent Office on April 1, 2022, and the entire contents of Patent Application No. 2022-061684 are incorporated by reference into this application. [Explanation of symbols]

[0104] 1 Reflective mask blank 2 Reflective mask 10 Substrate 11 Multilayer reflective film 12 Protective film 13 Absorbing membrane

Claims

1. A reflective mask blank having, in this order, a substrate, a multilayer reflective film that reflects EUV light, a protective film that protects the multilayer reflective film, and an absorbing film that absorbs EUV light, the protective film contains 50 at % or more of Rh, a reflective mask blank in which a band-shaped grayscale image parallel to the interface between the protective film and the multilayer reflective film is obtained by imaging a cross section of the protective film with a transmission electron microscope (TEM), and a luminance profile of the grayscale image in the longitudinal direction of the grayscale image is created, the number of peaks in the luminance profile per 100 nm in the longitudinal direction of the grayscale image is 50 or more.

2. 2. The reflective mask blank according to claim 1, wherein the multilayer reflective film has, as an uppermost layer in contact with the protective film, a Si film having an oxygen atom content of 15 at % or less.

3. 2. The reflective mask blank according to claim 1, wherein the protective film contains, as a metal element, only Rh, or contains, in addition to Rh, at least one element selected from Ru, Pd, Ir, Pt, Zr, Nb, Ta, and Ti.

4. the protective film contains, as a metal element, Rh and at least one element X selected from Ru, Pd, Ir, Pt, Zr, Nb, Ta, and Ti; 2. The reflective mask blank according to claim 1, wherein the protective film has an element ratio of Rh to X (Rh:X) of 50:50 to 99:

1.

5. the protective film has an upper layer containing 50 at % or more of Rh and a lower layer containing 50 at % or more of Ru, Pd, Ir, Pt, Zr, Nb, Ta or Ti, The reflective mask blank according to claim 1 , wherein the lower layer is provided between the upper layer and the multilayer reflective film.

6. 6. The reflective mask blank according to claim 5, wherein the protective film has a lower layer having a thickness of 0.5 nm or more and 2.0 nm or less, and an upper layer having a thickness of 0.5 nm or more and 4.0 nm or less.

7. 2. The reflective mask blank according to claim 1, wherein the protective film is made of a single layer containing 50 at % or more of Rh.

8. 2. The reflective mask blank according to claim 1, wherein the protective film has a thickness of 1.5 nm or more and 4.0 nm or less.

9. The film density of the protective film is 10.0 g / cm 3 14.0g / cm or more 3 2. The reflective mask blank according to claim 1, wherein:

10. 2. The reflective mask blank according to claim 1, wherein the surface of said protective film on which said absorbing film is formed has a root mean square roughness RMS of 0.300 nm or less.

11. 2. The reflective mask blank according to claim 1, wherein the absorbing film contains at least one metal element selected from Ru, Ta, Cr, Nb, Pt, Ir, Re, W, Mn, Au, Si, and Al.

12. The reflective mask blank according to claim 11 , wherein the absorbing film further contains at least one nonmetallic element selected from O, N, C, and B.

13. an etching mask film is provided on the opposite side of the protection film with respect to the absorption film; 2. The reflective mask blank according to claim 1, wherein the etching mask film contains at least one metal element selected from the group consisting of Cr, Nb, Ti, Mo, Ta and Si.

14. The reflective mask blank according to claim 13 , wherein the etching mask film further contains at least one nonmetallic element selected from O, N, C, and B.

15. A reflective mask blank according to any one of claims 1 to 14, A reflective mask including an aperture pattern in the absorbing film.

16. A method for manufacturing a reflective mask blank having, in this order, a substrate, a multilayer reflective film that reflects EUV light, a protective film that protects the multilayer reflective film, and an absorbing film that absorbs EUV light, the method comprising: A method for producing a reflective mask blank, comprising depositing the multilayer reflective film and the protective film in this order in the same vacuum chamber.

17. The method for producing a reflective mask blank according to claim 16, further comprising controlling the pressure in the vacuum chamber to 0.035 Pa or less when forming the protective film.

18. Preparing a reflective mask blank manufactured by the manufacturing method according to claim 16 or 17; forming an opening pattern in the absorbing film; A method for manufacturing a reflective mask comprising the steps of:

Citation Information

Patent Citations

  • Substrate with multilayer reflection film, manufacturing method therefor, method for manufacturing reflection-type mask blank, method for manufacturing reflection-type mask, and method for manufacturing semiconductor device

    JP2014170931A

  • Substrate with multi-layered reflecting film, reflective mask blank, reflective mask and method for manufacturing the same, and method for manufacturing semiconductor device

    JP2021056502A