Steel sheet and method for producing the same
A steel plate with controlled composition and manufacturing process addresses the challenge of achieving high yield strength, low yield ratio, and good low-temperature toughness, ensuring structural integrity and safety in buildings.
Patent Information
- Application Number
- JP2024112698
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-02
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional methods struggle to achieve high yield strength, low yield ratio, and good low-temperature toughness in steel plates, particularly in thicker materials, which are essential for structural integrity and safety in buildings.
A steel composition with specific element ranges and controlled microstructure, including a hard structure fraction and size, combined with a manufacturing process involving controlled heating, rolling, and two-phase region normalization, ensures high yield strength, low yield ratio, and excellent low-temperature toughness.
The steel plate achieves yield strength over 600 MPa, a yield ratio of 85% or less, and a ductile-brittle fracture surface transition temperature of -13°C or lower, even in plates thicker than 80 mm, enhancing structural safety and performance.
Smart Images

Figure 2024133715000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a steel plate and a manufacturing method thereof, and in particular to a steel plate exhibiting a lower yield ratio together with high yield strength and good low temperature toughness, and a manufacturing method thereof. [Background technology]
[0002] Steel plates for construction are primarily required to have the following characteristics to ensure the safety of buildings: (i) high yield strength. With the recent trend toward taller and larger span buildings, it is expected that steel plates will increasingly be designed to bear heavier loads. In order to prevent deformation of buildings under normal conditions, steel plates are required to have high yield strength.
[0003] In addition, in emergencies such as earthquakes (when a load exceeding the yield stress is applied), the plastic deformation of the components is believed to absorb the energy of the earthquake and ensure safety. The higher the plastic deformation capacity before a building collapses, i.e., the lower the yield ratio (yield strength / tensile strength), the greater the amount of energy absorbed, so steel plates are required to have a low yield ratio.
[0004] Furthermore, even if a steel plate is plastically designed, if it does not have excellent low-temperature toughness, it may undergo brittle fracture without plastic deformation. Therefore, from the viewpoint of ensuring safety, a certain low-temperature toughness is required to prevent the initiation and propagation of cracks.
[0005] As a steel plate mainly used for building structures and the like, for example, Patent Document 1 discloses a steel plate for low yield ratio thick-walled circular steel pipes having a predetermined chemical composition, a hardenability index DI defined by a predetermined formula (1) of 8 inches or more, and a tensile strength of 780 MPa or more, which are characterized by satisfying the following requirements (A), (B), and (C): (A) In the microstructure at 1 / 4 of the plate thickness, bainite is 90% or more by area; (B) In the microstructure at 1 / 4 of the sheet thickness, the average circular equivalent diameter d of the region surrounded by high-angle grain boundaries with a misorientation of 15° or more is 4 μm or less; (C) The microstructure at the 1 / 4 sheet thickness region contains 3 to 10 area % of island martensite having an average equivalent circle diameter of 0.5 to 3 μm and a Vickers hardness Hv of 700 or more. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2013-57105 A Summary of the Invention [Problem to be solved by the invention]
[0007] There is a demand for achieving a lower yield ratio along with high yield strength and good low-temperature toughness, but this has been difficult to achieve with current technology.
[0008] Furthermore, with conventional techniques, it has been difficult to stably obtain the above-mentioned high yield strength, good low-temperature toughness, and lower yield ratio even in a steel plate having a greater plate thickness.
[0009] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a steel plate having high yield strength, low yield ratio and excellent low-temperature toughness, and a manufacturing method thereof, and further to provide a steel plate capable of achieving the above properties even when the plate is thick, and a manufacturing method thereof. [Means for solving the problem]
[0010] Aspect 1 of the present invention is C: 0.040% by mass to 0.060% by mass, Si: 0.20% by mass to 0.30% by mass, Mn: 1.80% by mass to 2.00% by mass, P: more than 0% by mass, 0.010% by mass or less, S: more than 0% by mass, 0.003% by mass or less, Al: 0.040% by mass to 0.080% by mass, Cu:0.40 mass%~0.50 mass%, Ni: 1.40% by mass to 1.50% by mass, Cr:0.90 mass%~1.10 mass%, Mo: 0.17% by mass to 0.23% by mass, V: 0% by mass to 0.005% by mass, Nb: 0% by mass to 0.005% by mass, Ti: 0.010% by mass to 0.020% by mass, B: 0.0005% by mass to 0.0020% by mass, N: 0.0030% by mass to 0.0065% by mass, and Ca: Contains 0.0005% by mass to 0.0035% by mass, The balance is iron and unavoidable impurities, Pcm represented by the following formula (1) is 0.30 or less, and Dh represented by the following formula (2) is 21.7 or more, The steel plate has a hard structure constituted of at least one of bainite and island martensite MA, and the hard structure accounts for 23.3 area % to 29.4 area % of the total steel structure, and has an average equivalent circle diameter of 5.2 μm or less. Pcm=[C]+[Si] / 30+[Mn] / 20+[Cu] / 20+[Ni] / 60+[Cr] / 20+[Mo] / 15+[V] / 10+5×[B]...(1) Dh=DI×([C]+0.91×[Mn]+0.97×[Cr]+0.88×[Mo]) ···(2) In formula (2), DI = 1.16 × ([C] / 10) 0.5 ×(0.7×[Si]+1)×(5.1×([Mn]-1.2)+5)×(0.35×[Cu]+1)×(0.36×[Ni]+1)×(2.16×[Cr]+1)×(3×[Mo]+1)×(1.75×[V]+1)×(200×[B]+1) ···(3) In formulas (1) to (3), the [element symbol] indicates the content of each element in the steel expressed in mass %, and elements that are not contained are represented as zero.
[0011] Aspect 2 of the present invention is The steel plate according to embodiment 1, having a plate thickness of 80 mm or more.
[0012] Aspect 3 of the present invention is A method for producing a steel sheet according to aspect 1 or 2, comprising the steps of: A step of heating a steel slab having the composition according to embodiment 1 to 900 to 1250°C; A process of rolling at a finish rolling temperature of 800 ° C. to 970 ° C. on the surface, and then cooling from a cooling start temperature of Ar3 point or higher obtained by the following formulas (4) and (5) to a cooling stop temperature of 400 ° C. or lower at an average cooling rate of 1.0 ° C. / s or higher; After the cooling, the temperature is within the range of Ac1 point calculated by the following formula (6) to Ac3 point calculated by the following formula (7), and the parameter P calculated by the following calculation method is N A process of performing two-phase region normalization within a range of 21.04 to 22.12; The method for producing a steel sheet further comprises a step of performing tempering in a temperature range of 300°C to 600°C after the two-phase normalizing. Ar3 points = 910-310×[C]+25×[Si]-80×[Mneq] ···(4) In formula (4), [Mneq]=[Mn]+[Cr]+[Cu]+[Mo]+[Ni] / 2+10([Nb]-0.02)+1 ···(5) Ac1 point = 723-10.7×[Mn]-16.9×[Ni]+29.1×[Si]+16.9×[Cr]+290×[As]+6.38×[W]...(6) Ac3 points=910-203×[C] 0.5 -15.2×[Ni]+44.7×[Si]+104×[V]+31.5×[Mo]+13.1×[W] ···(7) In the formulas (4) to (7), the [element symbol] indicates the content of the element in the steel expressed in mass %, and elements that are not contained are set to zero. [Parameter P N Calculation method] Parameter P indicates the degree of normalization when the material is kept isothermal at temperature Tx (℃) and time Kx (sec). xUsing the following formula (8) to calculate the parameter P, which represents the degree of normalization when the temperature of the steel sheet increases with time, according to the steps shown in [1] to [5] below. N Calculate. P x =(T x +273) × log(K x / 3600+20) ···(8) [1] A temperature rise curve of the steel plate center temperature is created, with the vertical axis representing the steel plate center temperature (°C) and the horizontal axis representing the elapsed time (seconds) from the start of heating. The curve is then divided into 1-second intervals and approximated as a rectangle. In the above temperature rise curve, the point when the steel sheet center temperature is at point Ac1 is set as the starting point, and the elapsed time from the start of temperature rise at this starting point is t 0 (=0)(seconds), steel plate center temperature T 0 Let (=Ac1)(℃). [2] Degree of normalization after 1 second from the starting point P 0 The degree of normalization P 0 In equation (8), X = 0, that is, T x =T 0 = Ac1 (℃), K x =K 0 =1 (seconds) to calculate. [3] The degree of normalization P obtained in [2] above after 1 second has elapsed from the starting point 0 The temperature T at the center of the steel sheet after 1 second has elapsed since the starting point. 1 Required retention time k 1 The required retention time k 1 In the following formula (9), X = 0, that is, P x =P 0 , T x+1 =T 1 Substitute (℃) to calculate. k x+1 =(exp(P X / (T X+1 +273))-20)×3600 ···(9) In equation (9), k x+1 is from the starting point (Ac1) to T x+1 (℃) P x The steel plate center temperature T required to obtain x+1The required retention time at [4] Steel plate center temperature T 1 The converted retention time at k is calculated from the following equation (10): 1 +1=K 1 (Seconds) and then. K x+1 =k x+1 +1 ···(10) In equation (10), K x+1 is the steel plate center temperature T x+1 indicates the reduced retention time at X+1 is from the starting point (Ac1) to T x+1 (℃) P x The steel plate center temperature T required to obtain x+1 The required retention time at [5] P shown in [2] to [4] above x , k x+1 , K x+1 The calculation of X = 1, 2, 3, ... is repeated until normalization in the two-phase region is completed, and P X =P f In search of this P f P N Let us assume that. Effect of the Invention
[0013] According to the present invention, it is possible to provide a steel plate that can realize high yield strength, low yield ratio, and excellent low-temperature toughness even in the case of a thick steel plate, and a manufacturing method for said steel plate. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is a graph showing the relationship between the hard tissue fraction and vTrs. [Diagram 2] FIG. 2 is a graph showing the relationship between the fraction of hard structure and yield strength. [Diagram 3] FIG. 3 is a graph showing the relationship between the average circular equivalent diameter of hard tissues and vTrs. [Figure 4] FIG. 4 is a graph showing the relationship between Dh and the average equivalent circular diameter of the hard tissue. [Diagram 5] FIG. 5 is a diagram for explaining a method of calculating the parameter PN. [Figure 6] FIG. 6 is another diagram for explaining the method of calculating the parameter PN. [Figure 7] FIG. 7 is another diagram for explaining the method of calculating the parameter PN. [Figure 8] FIG. 8 is another diagram for explaining the method of calculating the parameter PN. [Figure 9] FIG. 9 is a graph showing the relationship between PN and hard tissue fraction. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The present inventors have conducted extensive research to obtain a steel plate that satisfies high yield strength, low yield ratio, and good low-temperature toughness. As a result, they have found that these mechanical properties (strength, yield ratio, toughness) depend on the fraction and size of the "hard structure" composed of one or more of bainite and island martensite MA, and that in order to control the fraction and size of this hard structure, it is necessary to control the reverse transformation structure fraction during two-phase normalizing in the manufacturing process and the component factors. In particular, when the steel plate is a thick material, it takes time to raise the temperature to the heat treatment temperature during the manufacturing process, and the influence of the thermal history during the heating (the temperature of the steel plate and the time spent in the furnace) is large, which tends to affect the structure to satisfy the above properties. In the present invention, they have found manufacturing conditions and component compositions that can realize the above properties, and further manufacturing conditions and component compositions that can realize the above properties even if the steel plate is a thick material. In the following, first, the hard structure that affects the mechanical properties will be described.
[0016] [The percentage of hard structure in the total steel structure is 23.3% to 29.4% by area, and the average equivalent circle diameter is 5.2 μm or less] To achieve both high strength and low-temperature toughness, hard structure is necessary to ensure strength, and the lower limit of its fraction is set to 23.3% by area. On the other hand, hard structure can be the starting point of fracture, so if it is present in excess, toughness will deteriorate. Therefore, the upper limit of the fraction of the hard coating is set to 29.4% by area. Furthermore, toughness is affected not only by the hard structure fraction, but also by the hard structure size. If the hard structure size is large, it is more likely to become the starting point of fracture, and toughness will deteriorate. Therefore, the upper limit of the average circular equivalent diameter of the hard structure is set to 5.2 μm.
[0017] FIG. 1 is a graph showing the relationship between the fraction of hard structure and vTrs, which is an index of low-temperature toughness evaluation, obtained using data from the Examples described later. It can be seen from FIG. 1 that in order to achieve a vTrs of -13°C or less as good low-temperature toughness, the fraction of hard structure should be 29.4 area% or less. FIG. 2 is a graph showing the relationship between the fraction of hard structure and yield strength, obtained using data from the Examples described later. It can be seen from FIG. 2 that in order to achieve a high yield strength of 600 MPa or more, the fraction of hard structure should be 23.3 area% or more.
[0018] From the viewpoint of further increasing low temperature toughness, it is preferable that the fraction of the hard structure is 28.9 area % or less, whereas from the viewpoint of further increasing yield strength, it is preferable that the fraction of the hard structure is 23.8 area % or more.
[0019] The hard structure can be generated by performing two-phase region normalizing under predetermined conditions in the manufacturing process, as described later.
[0020] Fig. 3 is a graph showing the relationship between the average equivalent circle diameter of hard structures and vTrs, which is an index of low-temperature toughness evaluation, obtained using data from the Examples described later. It can be seen from Fig. 3 that in order to achieve a vTrs of -13°C or less as a good low-temperature toughness, the average equivalent circle diameter of hard structures should be 5.2 µm or less.
[0021] From the viewpoint of further improving low-temperature toughness, the average equivalent circular diameter of the hard structure is preferably 4.0 μm or less. The smaller the average equivalent circular diameter of the hard structure, the more preferable it is, but considering the manufacturing conditions, etc., the lower limit of the average equivalent circular diameter of the hard structure is about 2.0 μm.
[0022] Furthermore, in order to obtain a hard tissue having the above average equivalent circle diameter, the component parameter Dh represented by the following formula (2) must be 21.7 or more. Dh=DI×([C]+0.91×[Mn]+0.97×[Cr]+0.88×[Mo]) ···(2) In formula (2), DI = 1.16 × ([C] / 10) 0.5 ×(0.7×[Si]+1)×(5.1×([Mn]-1.2)+5)×(0.35×[Cu]+1)×(0.36×[Ni]+1)×(2.16×[Cr]+1)×(3×[Mo]+1)×(1.75×[V]+1)×(200×[B]+1) ···(3) In formulas (2) and (3), the [element symbol] indicates the content of the element in the steel expressed in mass%, and elements that are not contained are set to zero.
[0023] The above Dh is an index describing the average equivalent circle diameter of the hard structure. The derivation of Dh will be explained below. It is considered that the hard structure is formed from cementite formed between the laths of bainite obtained before two-phase normalizing, i.e., at the stage of hot rolling and cooling (hereinafter referred to as "as-rolled and cooled bainite"). Therefore, the size of the hard structure strongly depends on the dispersion state of cementite in the as-rolled and cooled bainite. In addition, it is considered that the dispersion state of cementite is determined by the number of nucleation sites of cementite and the nucleation frequency.
[0024] The number of nucleation sites depends on the lath spacing of the bainite after rolling and cooling, so it is believed that the higher the hardenability index DI, the smaller the lath spacing, i.e., the more nucleation sites there are. Therefore, the hardenability index DI is used as an index of the number of nucleation sites.
[0025] The nucleation frequency is also related to the cementite (Fe 3 It was assumed that the effect of carbide formation on the hardness of cementite was dependent on the amount of element C, which forms carbide (C), and the amount of element X, which has a high affinity with cementite and attracts C more easily than Fe. As the element X, Mn, Cr, and Mo were extracted after considering the degree of solid solubility in cementite as an index of affinity with cementite, and the ability to form carbides as an index of ease of attracting C.
[0026] Therefore, it was thought that the size of the hard structure could be estimated by the parameter Dh, which is calculated by multiplying the hardenability index DI, which is an index of the number of nucleation sites, by the nucleation frequency, which is composed of the contents of C, Mn, Cr and Mo (C + 0.91Mn + 0.97Cr + 0.88Mo).
[0027] Figure 4 is a graph showing the relationship between Dh and the average equivalent circle diameter of hard tissue, obtained using data from the examples described below. From Figure 4, it can be seen that in order to achieve an average equivalent circle diameter of hard tissue of 5.2 μm or less, Dh should be 21.7 or more. Dh is preferably 25.0 or more. There is no particular limit to the upper limit of Dh, but considering the range of the specified component composition, it is approximately 34.0.
[0028] Next, the reasons for specifying the ranges of each element and Pcm in the chemical composition of the steel sheet will be described.
[0029] [C:0.040 mass%~0.060 mass%] C is an essential element for ensuring the strength of the base metal and welded parts, and must be contained at 0.040% by mass or more. The C content is preferably 0.045% by mass or more. On the other hand, if the C content is too high, the HAZ toughness and weldability deteriorate. Furthermore, if the C content is excessive, island martensite is likely to form. Therefore, the C content is set to 0.060% by mass or less. The C content is preferably 0.055% by mass or less.
[0030] [Si:0.20 mass%~0.30 mass%] Silicon has a deoxidizing effect and is an effective element for improving the strength of the base metal and the welded part. To obtain these effects, the amount of silicon is set to 0.20 mass% or more. The amount of silicon is preferably 0.22 mass% or more. However, if the amount of silicon is too large, the weldability and toughness deteriorate, so the amount of silicon is set to 0.30 mass% or less. The amount of silicon is preferably 0.28 mass% or less.
[0031] [Mn:1.80 mass%~2.00 mass%] Mn is an element that has the effect of improving the hardenability and improving the strength and toughness of the steel plate. In order to exert this effect, the present invention contains Mn at 1.80 mass% or more. The Mn content is preferably 1.89 mass% or more. However, if the Mn content is too high, the HAZ toughness and weldability deteriorate. Therefore, the Mn content is 2.00 mass% or less. The Mn content is preferably 1.99 mass% or less.
[0032] [P: more than 0 mass%, 0.010 mass% or less] P is an element that is inevitably contained in steel materials, and if the P content exceeds 0.010 mass%, the toughness of the base material and HAZ is significantly deteriorated, and the resistance to hydrogen-induced cracking is also deteriorated. Therefore, in the present invention, the P content is limited to 0.010 mass% or less. However, it is industrially difficult to reduce the P content to 0 mass%, so the lower limit is more than 0 mass%.
[0033] [S: More than 0 mass%, 0.003 mass% or less] If there is too much S, it will generate a large amount of MnS, which will deteriorate the weld crack resistance. Therefore, in the present invention, the S content is set to 0.003 mass% or less. However, it is industrially difficult to make the S content 0 mass%, so the lower limit of the S content is more than 0 mass%.
[0034] [Al:0.040 mass%~0.080 mass%] Al is an element that improves the hardenability of B by deoxidizing and fixing free nitrogen. In order to exert these effects, the Al content is set to 0.040 mass% or more, preferably 0.045 mass% or more in the present invention. On the other hand, if the Al content is too large, coarse alumina-based inclusions are formed, and the toughness of the base material decreases. Therefore, the Al content is set to 0.080 mass% or less, preferably 0.075 mass% or less.
[0035] [Cu:0.40 mass%~0.50 mass%] Cu is an element that is effective in improving hardenability and increasing strength. To obtain this effect, the Cu content must be 0.40 mass% or more. However, if the Cu content exceeds 0.50 mass%, toughness deteriorates, so the Cu content is set to 0.50 mass% or less.
[0036] [Ni: 1.40 mass% to 1.50 mass%] Ni is an element that is effective in improving the strength and toughness of the base metal and welded parts. To obtain this effect, the Ni content must be 1.40 mass% or more. However, if a large amount of Ni is included, scale defects are likely to occur during rolling, so the Ni content is set to 1.50 mass% or less.
[0037] [Cr:0.90 mass%~1.10 mass%] Cr is an element necessary for improving hardenability and strength. To obtain this effect, the Cr content is set to 0.90 mass% or more. The Cr content is preferably 0.95 mass% or more. On the other hand, if a large amount of Cr is contained, the weld crack resistance deteriorates, so the Cr content is set to 1.10 mass% or less. The Cr content is preferably 1.05 mass% or less.
[0038] [Mo:0.17 mass%~0.23 mass%] Mo is an element that improves hardenability and strength. To achieve this effect, the Mo content is set to 0.17 mass% or more. However, if the Mo content exceeds 0.23 mass%, the weld crack resistance deteriorates. Therefore, the Mo content is set to 0.23 mass% or less.
[0039] [V:0 mass%~0.005 mass%] V is an element that may be unavoidably contained. V has the effect of suppressing recrystallization, which leads to an increase in the acoustic anisotropy of the steel sheet. Therefore, the V content is limited to 0.005 mass% or less. The V content is preferably 0.003 mass% or less.
[0040] [Nb:0 mass%~0.005 mass%] Nb is an element that may be unavoidably contained, similar to V. Nb has the effect of suppressing recrystallization, similar to V, and leads to an increase in the acoustic anisotropy of the steel sheet. Therefore, the Nb content is limited to 0.005 mass% or less. The Nb content is preferably 0.003 mass% or less.
[0041] [Ti:0.010 mass%~0.020 mass%] Ti is an element that is effective in preventing coarsening of austenite grains in the HAZ during welding by precipitating in the steel as TiN and improving the toughness of the HAZ. To obtain this effect, the Ti content is set to 0.010 mass% or more, preferably 0.012 mass% or more. On the other hand, if the Ti content is excessive, TiN will coarsen and the base material toughness will deteriorate, so the Ti content is set to 0.020 mass% or less, preferably 0.018 mass% or less.
[0042] [B:0.0005 mass%~0.0020 mass%] B is an element effective for improving hardenability and increasing base material strength. To achieve this effect, the B content is set to 0.0005% by mass or more. The B content is preferably 0.0008% by mass or more. However, if the B content is excessive, inclusions are formed and the base material toughness is deteriorated, so the B content is set to 0.0020% by mass or less. The B content is preferably 0.0018% by mass or less.
[0043] [N:0.0030 mass%~0.0065 mass%] N is an element that precipitates as TiN in the steel structure, suppresses the coarsening of austenite grains in the HAZ, and improves the toughness of the HAZ. To obtain this effect, it is necessary to contain N at 0.0030 mass% or more. However, if the N content is too high, the HAZ toughness will deteriorate due to the presence of solid solution N, so the N content is set to 0.0065 mass% or less. The N content is preferably 0.0050 mass% or less.
[0044] [Ca:0.0005 mass%~0.0035 mass%] Ca is an element that is effective in making MnS spheroidized and thus detoxifying weld crack resistance. To obtain this effect, the Ca content is set to 0.0005% by mass or more. However, if the Ca content is too high, it will cause inclusions to become coarse and the base material toughness to deteriorate, so the Ca content is set to 0.0035% by mass or less. The Ca content is preferably 0.0030% by mass or less, and more preferably 0.0025% by mass or less.
[0045] The above elements are included, and the balance is composed of iron and inevitable impurities. As inevitable impurities, the inclusion of trace elements brought in due to the conditions of raw materials, materials, manufacturing facilities, etc. is permitted. Note that, for example, there are elements such as P and S, which are usually preferable to have a lower content and therefore are inevitable impurities, but whose composition ranges are separately specified as above. For this reason, in this specification, when referring to the "unavoidable impurities" that constitute the balance, it is a concept that excludes elements whose composition ranges are separately specified.
[0046] [Pcm represented by the following formula (1) is 0.30 or less] Pcm=[C]+[Si] / 30+[Mn] / 20+[Cu] / 20+[Ni] / 60+[Cr] / 20+[Mo] / 15+[V] / 10+5×[B]...(1) In formula (1), each [element symbol] indicates the content of the element in the steel expressed in mass%, and elements that are not contained are set to zero. Pcm is an index showing the susceptibility to weld cracking. If Pcm is large, the susceptibility to weld cracking increases and the cracking resistance decreases, so the upper limit is set at 0.30.
[0047] As described above, the steel plate of the present invention exhibits a lower yield ratio together with high yield strength and good low-temperature toughness. Each of the properties will be described below.
[0048] (1) Yield strength (YS) It has a yield strength (YS) of 600 MPa or more. As a result, as described above, even if the steel plate is designed to bear a large load, sufficient strength can be ensured to prevent deformation of the building under normal conditions. The yield strength is preferably 620 MPa or more, and more preferably 660 MPa or more. The upper limit of the yield strength can be set to, for example, 750 MPa based on the standards for building materials.
[0049] (2) Low temperature toughness It means that the ductile-brittle fracture transition temperature measured by the method described in the Examples below is not higher than -13°C. The ductile-brittle fracture transition temperature is preferably not higher than -20°C, more preferably not higher than -25°C.
[0050] (3) Low yield ratio The steel sheet of the present invention exhibits a low yield ratio of 85% or less, preferably 80% or less.
[0051] The steel sheet of the present invention exhibits the above-mentioned properties even when the sheet has a thickness of 80 mm or more, preferably more than 80 mm.
[0052] [Manufacturing method] Next, a method for producing a steel sheet according to the present invention will be described. The method includes the steps of heating a steel slab having the above-mentioned composition to 900 to 1250°C, A process of rolling at a finish rolling temperature of 800 ° C to 970 ° C on the surface, and then cooling from a cooling start temperature of Ar3 point or higher to a cooling stop temperature of 400 ° C or lower at an average cooling rate of 1.0 ° C / s or higher; After the cooling, within the temperature range of Ac1 to Ac3, and the parameter P obtained by the following method N A process of performing two-phase region normalization within a range of 21.04 to 22.12; After the normalizing, a step of tempering is included in the temperature range of 300°C to 600°C.
[0053] Here, the Ar3 point is calculated by the following formulas (4) and (5). The Ac1 point is calculated by the following formula (6), and the Ac3 point is calculated by the following formula (7). Ar3 points = 910-310×[C]+25×[Si]-80×[Mneq] ···(4) In formula (4), [Mneq]=[Mn]+[Cr]+[Cu]+[Mo]+[Ni] / 2+10([Nb]-0.02)+1 ···(5) Ac1 point = 723-10.7×[Mn]-16.9×[Ni]+29.1×[Si]+16.9×[Cr]+290×[As]+6.38×[W]...(6) Ac3 points=910-203×[C] 0.5 -15.2×[Ni]+44.7×[Si]+104×[V]+31.5×[Mo]+13.1×[W] ···(7) In the formulas (4) to (7), the [element symbol] indicates the content of the element in the steel expressed in mass %, and elements that are not contained are set to zero.
[0054] [Parameter P N Calculation method] Parameter P indicates the degree of normalization when the material is kept isothermal at temperature Tx (℃) and time Kx (sec). x Using the following formula (8) to calculate the parameter P, which represents the degree of normalization when the temperature of the steel sheet increases with time, according to the steps shown in [1] to [5] below. N Calculate. P x =(T x +273) × log(K x / 3600+20) ···(8) [1] A temperature rise curve of the steel plate center temperature is created, with the vertical axis representing the steel plate center temperature (°C) and the horizontal axis representing the elapsed time (seconds) from the start of heating. The curve is then divided into 1-second intervals and approximated as a rectangle. In the above temperature rise curve, the point when the steel sheet center temperature is at point Ac1 is set as the starting point, and the elapsed time from the start of temperature rise at this starting point is t 0 (=0)(seconds), steel plate center temperature T 0 Let (=Ac1)(℃). [2] Degree of normalization after 1 second from the starting point P 0 The degree of normalization P 0 In equation (8), x = 0, that is, T x =T 0 = Ac1 (℃), K x =K 0 =1 (seconds) to calculate. [3] The degree of normalization P obtained in [2] above after 1 second has elapsed from the starting point 0 The temperature T at the center of the steel sheet after 1 second has elapsed since the starting point. 1 Required retention time k 1 The required retention time k 1 In the following equation (9), x = 0, that is, P x =P 0 , T x+1 =T 1 Substitute (℃) to calculate. k x+1 =(exp(P X / (T X+1 +273))-20)×3600 ···(9) In equation (9), k x+1 is from the starting point (Ac1) to T x+1 (℃) P x The steel plate center temperature T required to obtain x+1 The required retention time at [4] Steel plate center temperature T 1 The converted retention time at k is calculated from the following equation (10): 1 +1=K 1 (Seconds) and then. K x+1 =k x+1 +1 ···(10) In equation (10), K x+1 is the steel plate center temperature T x+1 indicates the reduced retention time at X+1 is from the starting point (Ac1) to T x+1(℃) P x The steel plate center temperature T required to obtain x+1 The required retention time at [5] P shown in [2] to [4] above x , k x+1 , K x+1 The calculation of X = 1, 2, 3, ... is repeated until normalization in the two-phase region is completed, and P X =P f In search of this P f P N Let us assume that.
[0055] Each step will be described in detail below.
[0056] [A process of heating the steel slab having the above-mentioned composition to 900 to 1250°C] A steel slab having the above-mentioned composition is heated to 900 to 1250°C at which hot rolling is possible. If the heating temperature is low, the austenite grain size is small, resulting in poor hardenability and poor strength. Therefore, the heating temperature is set to 900°C or higher. The heating temperature is preferably 1000°C or higher, more preferably 1050°C or higher. On the other hand, if the heating temperature is too high, the austenite grain size becomes large, resulting in an increase in the bainite block diameter and poor toughness. Therefore, the heating temperature is set to 1250°C or lower. The heating temperature is preferably 1200°C or lower, more preferably 1150°C or lower.
[0057] [A process in which rolling is performed at a finish rolling temperature of 800°C to 970°C on the surface, and then cooling is performed from a cooling start temperature of Ar3 point or higher to a cooling stop temperature of 400°C or lower at an average cooling rate of 1.0°C / s or higher] If the finish rolling temperature is below 800°C, the austenite grains are significantly flattened and acoustic anisotropy increases. Therefore, the finish rolling temperature is set to 800°C or higher. The finish rolling temperature is preferably set to 810°C or higher, more preferably 820°C or higher. On the other hand, if the finish rolling temperature exceeds 970°C, the effect of refining the austenite grains becomes small, and toughness deteriorates. Therefore, the finish rolling temperature is set to 970°C or lower. The finish rolling temperature is preferably set to 960°C or lower, more preferably 950°C or lower.
[0058] After rolling at the above finish rolling temperature, the material is cooled from a cooling start temperature of the Ar3 point or higher to a cooling stop temperature of 400°C or lower at an average cooling rate of 1.0°C / s or higher. The Ar3 point is the temperature at which transformation starts during continuous cooling, and is calculated by the above formulas (4) and (5).
[0059] The morphology of bainite changes depending on the cooling conditions after rolling, and the structure size of bainite also changes. Therefore, by controlling the cooling conditions after rolling, the morphology of bainite can be controlled to obtain a desired structure size of bainite. When the cooling start temperature of cooling at a predetermined average cooling rate is below the Ar3 point or the cooling stop temperature is above 400°C, bainite with a wide lath spacing is formed, and a coarse hard structure is formed in the subsequent two-phase region normalizing, resulting in a deterioration in toughness. Therefore, the cooling start temperature at a predetermined average cooling rate is set to the Ar3 point or higher. The cooling start temperature is preferably Ar3 point + 20°C or higher, more preferably Ar3 point + 40°C or higher. The upper limit of the cooling start temperature can be, for example, the finish rolling temperature. Moreover, the cooling stop temperature at a predetermined average cooling rate is 400°C or lower, preferably 390°C or lower, more preferably 380°C or lower. The lower limit of the cooling stop temperature is not particularly limited, and can be, for example, 20°C.
[0060] If the average cooling rate is less than 1.0°C / sec, the structure size of the bainite formed becomes coarse, and the toughness deteriorates. The average cooling rate is preferably 1.3°C / sec or more, and more preferably 1.5°C / sec or more. The upper limit of the average cooling rate is not particularly limited.
[0061] After cooling to the cooling stop temperature at the average cooling rate, the material may be cooled once to a temperature lower than the cooling stop temperature, for example, to room temperature, and then normalized in the two-phase region. Alternatively, the material may be heated from the cooling stop temperature to the heating temperature for the two-phase region normalizing without being cooled to room temperature.
[0062] [After the cooling, within the temperature range of Ac1 point to Ac3 point, and the parameter P obtained by the following method N A process in which normalization is performed in the two-phase region when the value of
[0063] In order to realize a low yield ratio, it is effective to perform a two-phase heat treatment to form a two-phase structure of a hard phase and a soft phase, but in the conventional method, the hardness ratio between the hard phase and the soft phase is not large, and it is difficult to stably obtain a low yield ratio after the steel pipe processing, for example, during strong bending processing such as D / t (D: steel pipe diameter, t: steel plate thickness) = 10 to 20. Therefore, the inventors of the present invention conducted research and found that a steel plate that satisfies a sufficient low yield ratio even after strong bending processing can be obtained by performing two-phase normalizing under the conditions shown below, generating extremely hard MA in the reverse transformation part, and increasing the hardness ratio between the hard structure and the soft structure. The conditions of the two-phase normalizing are explained below.
[0064] In order to secure the above-mentioned predetermined fraction of hard structure and realize a lower yield ratio, two-phase normalizing is performed. The two-phase normalizing is performed within the temperature range of Ac1 to Ac3, where the value of the parameter PN obtained by the following method is in the range of 21.04 to 22.12. Note that the Ac1 point is the temperature at which reverse transformation starts during continuous heating and is obtained by the above formula (6), and the Ac3 point is the temperature at which reverse transformation ends during continuous heating and is obtained by the above formula (7).
[0065] Above P Nis a parameter that correlates with the fraction of reverse transformation structure, i.e., the fraction of hard structure. When normalizing a steel plate with a thickness of less than 80 mm in the two-phase region, the heating time until the steel plate center temperature reaches the soaking temperature is short, so the effect of the temperature and time during heating on the degree of two-phase region normalization is minor. In this case, the desired fraction of hard structure can be obtained by controlling the soaking temperature and time. In contrast, in the case of a thick plate with a thickness of 80 mm or more, the heating time until the steel plate center temperature reaches the soaking temperature is long, and the temperature effect during heating is large, so it is difficult to estimate the fraction of reverse transformation structure only from the soaking temperature and soaking time.
[0066] In the present invention, therefore, assuming that the thick object is subjected to two-phase region normalizing, the two-phase region normalizing conditions are set taking into consideration the influence of the temperature and time during heating on the degree of two-phase region normalizing.
[0067] [Parameter P N Calculation method] P N The calculation method is as follows. The following formula (8) is a parameter P that indicates the degree of normalization when the temperature Tx (℃) and time Kx (sec) are isothermally held. x That is, since the following formula (8) is used when maintaining an isothermal temperature, the degree of normalizing when the temperature of the steel sheet increases with time cannot be calculated by using the following formula (8) as it is. Therefore, the parameter P N Calculate. P x =(T x +273) × log(K x / 3600+20) ···(8)
[0068] [1] As shown in FIG. 5, a temperature rise curve of the steel plate center temperature is created, with the vertical axis being the steel plate center temperature (°C) and the horizontal axis being the elapsed time (seconds) from the start of heating. The curve is then divided into 1-second intervals and approximated as a rectangle. In the above temperature rise curve, the point when the steel sheet center temperature is at point Ac1 is set as the starting point, and the elapsed time from the start of temperature rise at this starting point is t 0 (=0)(seconds), steel plate center temperature T 0 Let (=Ac1)(℃). As shown in Fig. 5, the time and the temperature at the center of the steel sheet 1 second after the starting point are t 1 (seconds), T 1 (℃), and the time and the temperature at the center of the steel plate after X seconds from the starting point are t X (seconds), T X (℃), and t X The time and the temperature at the center of the steel sheet 1 second after t X+1 (seconds), T X+1 (℃). The time when the two-phase normalizing is completed and the temperature at the center of the steel sheet are expressed as t f (seconds), T f (°C).
[0069] [2] Degree of normalization after 1 second from the starting point P 0 The degree of normalization P 0 In equation (8), X = 0, that is, T x =T 0 = Ac1 (℃), K x =K 0 =1 (seconds) to calculate.
[0070] [3] The degree of normalization P obtained in [2] above after 1 second has elapsed from the starting point 0 The temperature T at the center of the steel sheet after 1 second has elapsed since the starting point. 1 Required retention time k 1 Request.
[0071] The required retention time k 1 is calculated using the following formula (9). The following formula (9) means that "the temperature at the center of the steel sheet is x+1 (℃) P x T required to obtain X k is the equivalent holding time (seconds) at +1 temperature x+1 This is the formula for calculating k x+1=(exp(P X / (T X+1 +273))-20)×3600 ···(9)
[0072] The required retention time k 1 In the above formula (9), X = 0, that is, P x =P 0 , T x+1 =T 1 (℃) is substituted. Figure 6 shows the case where X=0. In Figure 6, the degree of normalization P after 1 second has elapsed from the starting point is 0 The area of the bold frame showing the steel plate center temperature T 1 ×Required holding time k 1 The areas of the filled areas (P values) are equal.
[0073] [4] Steel plate center temperature T 1 The converted retention time at k is calculated from the following equation (10): 1 +1=K 1 (Seconds) and then. K x+1 =k x+1 +1 ···(10) In equation (10), K x+1 is the steel plate center temperature T x+1 indicates the reduced retention time at X+1 is from the starting point (Ac1) to T x+1 (℃) P x The steel plate center temperature T required to obtain x+1 The required retention time at
[0074] [5] P shown in [2] to [4] above x , k x+1 , K x+1 The calculation of X = 1, 2, 3, ... is repeated until normalization in the two-phase region is completed, and P X =P f In search of this P f P N Let us assume that.
[0075] As above, P 1 , k 2 , K2 A method for determining the above will be described below with reference to Fig. 7. Fig. 7 shows the case where X=1.
[0076] In the above formula (8), T 1 (℃), K 1 =k 1 Substitute +1 (seconds) and get T 1 (℃)K 1 (Seconds) P when held 1 (The area of the bold frame in FIG. 7) is calculated. Then, in the above formula (9), 1 , T 2 (℃) and P 1 Equivalent to T 2 Required holding time k at (℃) 2 In Figure 7, the degree of normalization P after 2 seconds has elapsed from the starting point is calculated. 1 The area of the bold frame showing the steel plate center temperature T 2 ×Required holding time k 2 The area of the filled area (P value) is equal. From the above formula (10), as shown in Figure 3, 2 =k 2 +1 (seconds).
[0077] As shown in Figures 6 and 7 above, the calculation is repeated to obtain P x , k x+1 , K x+1 (X=2,3,4…) are calculated in sequence. Then, as shown in Figure 8, T X is the temperature Tf (℃) at the end of normalizing in the two-phase region. X (=P f ) to P N Let us assume that.
[0078] The present inventors have N The relationship between the amount of P and the fraction of hard tissue obtained was examined separately. N 1 is a graph showing the relationship between the hard tissue fraction and the P N There is a correlation between the fraction of hard structure and P. As mentioned above, in order to secure a fraction of hard structure of 23.3% or more by area and achieve high yield strength, NOn the other hand, in order to secure superior low-temperature toughness by suppressing the fraction of hard structures to 29.4 area % or less as mentioned above, P N must be less than or equal to 22.12.
[0079] According to an embodiment of the present invention, the parameter P, which is correlated with the fraction of the hard structure that is a reverse transformation structure, N By performing two-phase normalizing so that the value falls within a predetermined range, the fraction of hard structures that affect the properties can be controlled with high precision even in the case of thick steel plates.
[0080] After the normalizing, the material is cooled to, for example, 100° C. or less, and then the next tempering is carried out.
[0081] [After the normalizing, a process of tempering in a temperature range of 300°C to 600°C] By performing tempering, mobile dislocations generated during cooling after two-phase region normalization can be annihilated, and the yield strength can be improved. In particular, by setting the tempering temperature in the temperature range of 300°C to 600°C, appropriate strength can be obtained. If the tempering temperature exceeds Ac1 point, two-phase region normalization occurs, and mobile dislocations are reintroduced during cooling, making it impossible to ensure strength. If the tempering temperature exceeds 600°C, the strength of the hard phase decreases, making it impossible to ensure strength. Therefore, the upper limit of the tempering temperature is 600°C, and the preferred upper limit is 560°C. On the other hand, if the tempering temperature is less than 300°C, the annihilation of mobile dislocations is insufficient, making it impossible to ensure appropriate strength. Therefore, the tempering temperature is 300°C or higher, preferably 400°C or higher. After the above tempering, the material can be left to cool to room temperature, for example. EXAMPLES
[0082] The present invention will be described in more detail below with reference to examples. The present invention is not limited to the following examples, and can be practiced with appropriate modifications within the scope of the above and below-mentioned aims, and all such modifications are included in the technical scope of the present invention.
[0083] (Steel plate manufacturing) Steel materials having the chemical composition shown in Table 1 were produced in a converter or by vacuum melting of 150 kg. In Table 1, a line (-) indicates that the corresponding chemical component was not detected. In addition, Pcm, Ac1, Ac3, Ar3, DI, and Dh in Table 1 were calculated from the above-mentioned formulas (1) to (7).
[0084] After completion of the melting, slabs were obtained by continuous casting or forging. The slabs were heated to the heating temperature shown in Table 2 and hot rolled. The finishing temperature of the hot rolling was as shown in Table 2. After hot rolling, the slabs were cooled under the conditions shown in Table 2. After cooling to the cooling stop temperature shown in Table 2, they were allowed to cool to room temperature, and steel plates having the plate thicknesses shown in Table 2 were obtained.
[0085] Next, two-phase region normalizing and tempering were performed under the heat treatment conditions shown in Table 2. The two-phase region normalizing was performed at the heating temperature shown in Table 2 and with the P N The heating and holding time was set so as to satisfy the above P N After normalizing in the two-phase region, the specimens were tempered at the heating temperatures shown in Table 2 for about 15 minutes.
[0086] In the manufacture of the above steel plates, the finish rolling temperatures shown in Table 2 were measured at the surface temperature of the steel plate. The heating temperature is the atmospheric temperature of the heating furnace, the cooling start temperature and cooling end temperature after rolling are the temperatures on the surface of the steel plate, the heating temperature for dual-phase normalizing is the temperature at the center of the thickness of the steel plate, and the heating temperature for tempering is the temperature at the center of the thickness of the steel plate. The temperatures at the center of the thickness during dual-phase normalizing and tempering were measured by inserting a thermocouple.
[0087] To evaluate the steel structure of the obtained steel plate, the fraction and size of the hard structure were measured, and a tensile test and a Charpy impact test were performed as described below.
[0088] [Measurement of hard tissue fraction and size] A sample was taken from the above steel sheet so that the observation surface was a thickness cross section including the front and back surfaces of the steel sheet, parallel to the rolling direction and perpendicular to the steel sheet surface. The observation surface was then mirror-polished and then etched with a nital solution to reveal the hard structure. The hard structure subjected to this treatment was observed as a white structure when observed with a scanning electron microscope (SEM).
[0089] The exposed structure was photographed at a field of view of 1000 times at the plate thickness t / 4 portion. The photograph was imported into an image analyzer. The area of the photograph corresponds to 128 μm × 95 μm. The area fraction and average circle equivalent diameter of the hard structure observed as white structure were calculated in the image analyzer.
[0090] [Tensile test] JIS Z2241 No. 4 test pieces were prepared from each thick steel plate. The No. 4 test pieces were cut from the surface of the thick steel plate at a depth of t / 4 of the plate thickness, so that the longitudinal direction of the test piece was perpendicular to the rolling direction. Using these test pieces, tensile tests were performed according to JIS Z2241 to measure the yield strength YS and tensile strength TS. The yield ratio YR was calculated by dividing YS by TS and multiplying the result by 100. A yield strength YS of 600 MPa or more was evaluated as high strength. A YR of 85% or less was evaluated as low yield ratio.
[0091] [Charpy impact test] V-notch Charpy impact test pieces according to JIS Z2242 were taken from each thick steel plate. Twelve test pieces were cut out from the surface of the thick steel plate at a depth of t / 4 of the plate thickness, so that the longitudinal direction of the test piece was the rolling direction. The absorbed energy and brittle fracture rate were determined under four test temperature conditions (three test pieces were used for each test temperature condition) using the twelve test pieces taken. Then, vTrs was calculated from the relationship between the test temperature and the obtained brittle fracture rate. Then, when vTrs was -13°C or less, it was evaluated as having excellent low-temperature toughness.
[0092] The results of these measurements are shown in Table 3.
[0093] [Table 1]
[0094] [Table 2]
[0095] [Table 3]
[0096] The following can be seen from Tables 1 to 3. K1, K4 to K11, and K15 to K20 satisfied the specified chemical composition and manufacturing conditions, and the obtained steel sheets had the desired structure, exhibited high strength, a lower yield ratio, and further exhibited excellent low-temperature toughness. In contrast, K2, K3, K12 to K14, K21, and K22 did not satisfy at least one of the chemical composition and manufacturing conditions, as explained below, and therefore did not obtain the desired structure, resulting in poor yield strength, yield ratio, and / or low-temperature toughness.
[0097] K2 and K3 are normalized in the two-phase region, N However, since the test was performed under conditions below the specified range, an excessive amount of hard structure was formed, resulting in poor low-temperature toughness.
[0098] K12~K14 are normalized in two-phase region, P N However, because the test was performed under conditions that exceeded the specified range, the hard structure was insufficient and high strength could not be achieved.
[0099] K21 was not tempered, so it was unable to achieve high strength.
[0100] In K22, since Dh was below the specified range, the average circular equivalent diameter of the hard structure exceeded the specified range and became large, resulting in poor low-temperature toughness. [Industrial Applicability]
[0101] The steel plate of the present invention can be used, for example, as a steel material for construction, mainly as a thick steel plate with a low yield ratio and high strength suitable for four-sided box column skin plates.
Claims
[Claim 1] C: 0.040% by mass to 0.060% by mass, Si: 0.20% by mass to 0.30% by mass, Mn: 1.80% by mass to 2.00% by mass, P: more than 0% by mass, 0.010% by mass or less, S: more than 0 mass%, 0.003 mass% or less, Al: 0.040% by mass to 0.080% by mass, Cu: 0.40% by mass to 0.50% by mass, Ni: 1.40% by mass to 1.50% by mass, Cr: 0.90% by mass to 1.10% by mass, Mo: 0.17% by mass to 0.23% by mass, V: 0% by mass to 0.005% by mass, Nb: 0% by mass to 0.005% by mass, Ti: 0.010% by mass to 0.020% by mass, B: 0.0005% by mass to 0.0020% by mass, N: 0.0030% by mass to 0.0065% by mass, and Ca: 0.0005% by mass to 0.0035% by mass; The balance is iron and unavoidable impurities, Pcm represented by the following formula (1) is 0.30 or less, and Dh represented by the following formula (2) is 21.7 or more, A steel plate in which a hard structure constituted by one or more of bainite and island martensite MA accounts for 23.3 area % to 29.4 area % of the total steel structure, and the average equivalent circle diameter thereof is 5.2 μm or less. Pcm=[C]+[Si] / 30+[Mn] / 20+[Cu] / 20+[Ni] / 60+[Cr] / 20+[Mo] / 15+[V] / 10+5×[B]...(1) Dh=DI×([C]+0.91×[Mn]+0.97×[Cr]+0.88×[Mo])...(2) In formula (2), DI=1.16×([C] / 10) 0.5 ×(0.7×[Si]+1)×(5.1×([M]]-1.2)+5)×(0.35×[[]+1)×(0.36×[Ni]+1)×(2.16×[[]++1)×(3×[[]++1)×(1.75×[V]++1)×(200×[[]+1) ・・・(3) In formulas (1) to (3), the [element symbol] indicates the content of each element in the steel expressed in mass%, and elements that are not contained are set to zero.
Citation Information
Patent Citations
Steel plate for low yield ratio thick-walled circular steel pipe having tensile strength of 780 mpa or more, method for manufacturing the same, and low yield ratio thick-walled circular steel pipe having tensile strength of 780 mpa or more