Conductive film

A conductive film with a carbon black and palladium-containing layer structure enhances adhesion and durability of thin wires, addressing peeling issues in touch panels and other applications.

JP2024133934AInactive Publication Date: 2024-10-03FUJIFILM CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023043964
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-20
Publication Date
2024-10-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conductive films with conductive thin wires experience reduced adhesion and peeling issues after durability tests, particularly in touch panels and other applications.

Method used

A conductive film structure comprising a transparent base material with a mesh pattern of conductive thin wires, including a black layer containing carbon black, a palladium-containing layer, and a metal plating layer, where the metal plating layer has a specific line width ratio to the black layer, enhancing adhesion.

Benefits of technology

The proposed structure significantly improves the adhesion of conductive thin wires, reducing peeling during durability tests and maintaining conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024133934000001_ABST
    Figure 2024133934000001_ABST
Patent Text Reader

Abstract

To provide a conductive film excellent in adhesion of a conductive thin wire after an endurance test.SOLUTION: A conductive film includes a transparent substrate and a mesh pattern that is disposed on the transparent substrate and is configured with a conductive fine wire. The conductive fine wire includes a black layer containing carbon black, a palladium-containing layer, and a metal plating layer in sequence from a side of the transparent substrate.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a conductive film. [Background technology]

[0002] Conductive films having conductive thin wires (thin wire-like wiring that exhibits conductivity) are widely used for various applications such as touch panels, solar cells, and EL (electroluminescence) elements. In particular, in recent years, the rate at which touch panels are installed in mobile phones and portable game devices has increased, and the demand for conductive films for capacitive touch panels capable of multi-point detection has been growing rapidly.

[0003] As an example of a conductive film having conductive thin lines, Patent Document 1 discloses a technology relating to a transparent substrate with a conductive pattern, which comprises a transparent substrate, a thin line pattern portion on one side of the transparent substrate containing a coating composition for electroless plating that contains metal particles that serve as nuclei for electroless plating, and an electroless plating layer provided on the surface of the transparent substrate opposite the thin line pattern portion. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2018-150584 A Summary of the Invention [Problem to be solved by the invention]

[0005] The present inventors, with reference to Patent Document 1, produced a conductive film having a mesh pattern composed of conductive thin wires, and investigated the properties of the produced conductive film. As a result, they found that in the conductive film after a durability test, the adhesion of the conductive thin wires decreases, and the conductive thin wires may peel off from the transparent substrate.

[0006] In view of the above circumstances, an object of the present invention is to provide a conductive film that has excellent adhesion to conductive thin wires after a durability test. [Means for solving the problem]

[0007] As a result of extensive research into the above problems, the present inventors have found that the above problems can be solved by the following configuration.

[0008] [1] A conductive film comprising a transparent substrate and a mesh pattern disposed on the transparent substrate and composed of conductive thin wires, the conductive thin wires having, in order from the transparent substrate side, a black layer containing carbon black, a palladium-containing layer, and a metal plating layer. [2] The conductive film according to [1], wherein the metal plating layer has a line width of 1.0 to 2.5 μm. [3] The conductive film according to [1] or [2], wherein the black layer has a line width of 0.85 to 1.90 μm. [4] The conductive film according to any one of [1] to [3], wherein a ratio of the line width of the metal plating layer to the line width of the black layer is greater than 1 and is 1.1. [5] The conductive film according to any one of [1] to [4], wherein the black layer has a thickness of 0.2 to 2.0 μm. [6] The conductive film according to any one of [1] to [5], wherein the carbon black contained in the black layer has an average particle size of 10 to 120 nm. [7] The conductive film according to any one of [1] to [6], wherein the content of the carbon black is 2 to 20 mass % based on the total mass of the black layer. Effect of the Invention

[0009] According to the present invention, it is possible to provide a conductive film that has excellent adhesion to conductive thin wires even after a durability test. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of the configuration of a conductive film of the present invention. [Diagram 2] FIG. 2 is a plan view showing an example of the configuration of a mesh pattern of the conductive film of the present invention. [Diagram 3] FIG. 2 is a plan view showing an example of the configuration of a mesh pattern of a conductive film produced in an example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention will be described in detail below. The following description of the components is based on a representative embodiment of the present invention, and the present invention is not limited to such an embodiment. The drawings shown below are conceptual diagrams for explaining the present invention, and the positional relationship, size, thickness, shape, etc. of each component may differ from the actual ones. In this specification, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the lower and upper limits. In this specification, when two or more types of a component are present, the "content" of the component means the total content of those two or more components. As used herein, the term "substantially free" of a certain component means that the content of the target component is 0.1 mass % or less, relative to the total mass of the component or composition.

[0012] In this specification, "g" and "mg" represent "g mass" and "mg mass", respectively. In this specification, the term "polymer" or "polymer compound" refers to a compound having a weight average molecular weight of 2000 or more. Here, the weight average molecular weight is defined as a polystyrene equivalent value measured by GPC (Gel Permeation Chromatography).

[0013] In this specification, angles expressed by specific numerical values ​​and expressions relating to angles such as "parallel," "perpendicular," and "orthogonal" include error ranges generally accepted in the relevant technical field, unless otherwise specified. In this specification, the "width direction" of the conductive thin wire or each layer constituting the conductive thin wire means a direction along the surface of the substrate that is perpendicular to the direction in which the conductive thin wire extends, and the "line width" of the conductive thin wire or each of the above layers means the overall length of the conductive thin wire or each of the above layers in the width direction.

[0014] [Conductive film] The conductive film of the present invention has a transparent substrate and a mesh pattern composed of conductive thin wires arranged on the transparent substrate, and the conductive thin wires have, from the transparent substrate side, a black layer containing carbon black, a palladium-containing layer, and a metal plating layer.

[0015] The inventors have investigated the durability of a conductive film having a transparent substrate and a mesh pattern composed of thin conductive wires, and have found that the adhesion of the thin conductive wires after a durability test can be improved by providing a laminate structure in which the thin conductive wires have a palladium-containing layer (hereinafter also referred to as a "Pd-containing layer") and a metal plating layer, and further a black layer containing carbon black is inserted between the transparent substrate and the Pd-containing layer, thereby completing the present invention. The present inventors have found that in a conductive film in which a conductive thin wire having a Pd-containing layer and a metal plating layer is disposed on a transparent substrate, the conductive thin wire may easily peel off over time. In contrast, the present inventors have found that the conductive film of the present invention having a black layer containing carbon black between the transparent substrate and the Pd-containing layer can suppress the above-mentioned phenomenon in which the conductive thin wire easily peels off. Hereinafter, in this specification, when the adhesiveness of the conductive thin wires is excellent after a durability test is performed on the conductive film, it is also stated that "the effect of the present invention is excellent."

[0016] Hereinafter, the conductive film according to the present invention (hereinafter also referred to as "the conductive film") will be described in more detail with reference to the drawings. FIG. 1 is a schematic cross-sectional view showing an example of the configuration of the conductive film. 1 includes a transparent substrate 12 and thin conductive wires 20 disposed on the transparent substrate 12. The thin conductive wires 20 have a layered structure including, in order from the transparent substrate 12 side, a black layer 22, a Pd-containing layer 24, and a metal plating layer 26. A mesh pattern is formed by the conductive thin wires 20 arranged on the transparent base material 12. That is, on the transparent base material 12, there are conductive thin wires 20 arranged in a mesh pattern and non-thin wire regions 30 where the conductive thin wires 20 are not arranged.

[0017] In the conductive film 10 shown in Fig. 1, conductive thin wires 20 constituting a mesh pattern are arranged on both sides of a transparent substrate 12. However, the conductive film is not limited to the embodiment shown in Fig. 1, and the conductive thin wires may be arranged on only one surface of the transparent substrate. For example, when used in a display device such as a touch panel, the conductive thin wires may be arranged only on the visible side surface of the transparent substrate (hereinafter also referred to as the "top surface"), or only on the display element side surface of the transparent substrate (hereinafter also referred to as the "bottom surface"). When a conductive film has a conductive thin wire having a black layer, a Pd-containing layer, and a metal plating layer in this order disposed on the bottom surface of a transparent substrate, the adhesion of the conductive thin wire after a durability test can be improved, and further, the phenomenon in which reflected light from the Pd-containing layer and / or the metal plating layer is visible when external light is irradiated onto the conductive film (the so-called "line visibility") can be suppressed.

[0018] FIG. 2 is a plan view showing an example of the configuration of a mesh pattern of the present conductive film. Fig. 2 is a plan view of the conductive film 10 shown in Fig. 1 when observed from the normal direction of the surface on which the conductive thin wires 20 of the transparent substrate 12 are arranged. As shown in Fig. 2, a mesh pattern 28 constituted by the conductive thin wires 20 is arranged on one surface of the transparent substrate 12 of the conductive film 10, and there are also a plurality of non-thin wire regions 30 surrounded by the mesh pattern 28 and spaced apart from each other. The arrangement and number of the conductive thin wires in the conductive film and the shape and size of the mesh pattern are not limited to the embodiments shown in Figures 1 and 2. Details of the mesh pattern in the conductive film will be described later. Hereinafter, unless otherwise specified, the mere expression "mesh pattern" refers to a mesh pattern formed of conductive thin wires that is possessed by the present conductive film.

[0019] Each component of the conductive film will be described below.

[0020] [Transparent base material] The type of transparent substrate is not particularly limited as long as it is a member capable of supporting a mesh pattern, and examples thereof include resin substrates.

[0021] In this specification, the term "transparent substrate" refers to a substrate having a total light transmittance of 80% or more. The total light transmittance is measured according to "Plastics - Determination of total light transmittance and total light reflectance" as specified in JIS (Japanese Industrial Standards) K 7375:2008. The total light transmittance of the transparent substrate is preferably 85 to 100%.

[0022] The transparent substrate is preferably flexible. The flexible transparent substrate means a transparent substrate that can be folded, specifically, a transparent substrate that does not crack even when folded with a bending curvature radius of 2 mm. The flexible transparent substrate has processability that allows the substrate to be formed into a three-dimensional shape. Examples of the flexible transparent substrate include a resin substrate.

[0023] As the resin constituting the transparent substrate, for example, polyethylene terephthalate (PET) (258°C), polycycloolefin (134°C), polycarbonate (250°C), acrylic film (128°C), polyethylene naphthalate (PEN) (269°C), polyethylene (PE) (135°C), polypropylene (163°C), polystyrene (230°C), polyvinyl chloride (180°C), polyvinylidene chloride (212°C), and triacetyl cellulose (290°C) are preferable, and PET, polycycloolefin, or polycarbonate are more preferable. Among them, PET is more preferable because of its excellent adhesion to the conductive thin wire. The value in parentheses above is the melting point or glass transition temperature.

[0024] The material constituting the transparent substrate may be a material that, when forming a mesh pattern on the transparent substrate, allows exposure light such as ultraviolet light to pass through from the back side, thereby exposing a photoresist provided on the transparent substrate. Photoresists are often designed to be exposed using ultraviolet light, and g-line (436 nm) is particularly often used due to the photoresist's light wavelength sensitivity characteristics and the ability to precisely process patterns at the μm level. In addition to g-line, short-wavelength ultraviolet light such as i-line (365 nm), KrF excimer laser (248 nm), ARF excimer laser (193 nm), and F2 excimer laser (157 nm) may also be used. In the process of forming a member on a transparent substrate, when a process of exposing a photoresist through the transparent substrate is performed, it is preferable to select a transparent substrate having good light transmittance for the exposure light. Alternatively, when a process of exposing a photoresist through the transparent substrate is performed, it is preferable to select the material of the photoresist and the wavelength of the exposure light source according to the light transmittance of the transparent substrate according to the wavelength. As the material constituting the transparent substrate, PET, polycycloolefin, or acrylic resin is preferable in terms of superior transmittance to the above-mentioned ultraviolet light. In addition, PEN or PET is preferred in that it has superior durability in the environment in which it is used as an electronic material.

[0025] The thickness of the transparent substrate is not particularly limited and is often 25 to 500 μm. When the conductive film is applied to a touch panel and the surface of the transparent substrate is used as a touch surface, the thickness of the transparent substrate may exceed 500 μm.

[0026] [Mesh pattern] The mesh pattern is a component composed of conductive thin wires arranged in a mesh pattern on a transparent substrate. The conductive thin wires are thin-line components with a laminated structure that includes a Pd-containing layer and a metal plating layer, and are responsible for the main conductive properties of the conductive film. The conductive thin wire has a layered structure composed of, in order from the transparent substrate side, a black layer, a Pd-containing layer, and a metal plating layer.

[0027] The mesh shape refers to a shape including a plurality of non-thin-wire regions 30 that are formed by intersecting conductive thin wires 20 and are spaced apart from each other, as in the mesh pattern 28 shown in FIG. 2. In FIG. 2, the non-thin-wire region 30 has a square shape with a length of one side of L, but the non-thin-wire region partitioned by the conductive thin wires of the mesh pattern may have other shapes, for example, a polygonal shape (for example, a triangle, a quadrangle (diamond, rectangle, etc.), a hexagon, and a random polygon). The shape of the sides may be a curved shape other than a straight line, or may be an arc shape. When the sides are arc-shaped, for example, two opposing sides may be arc-shaped convex outward, and the other two opposing sides may be arc-shaped convex inward. The shape of each side may be a wavy line shape in which an outwardly convex arc and an inwardly convex arc are continuous. Of course, the shape of each side may be a sine curve.

[0028] The length L of one side of the square lattice-shaped non-thin line region 30 is not particularly limited, but is preferably 1500 μm or less, more preferably 1300 μm or less, and even more preferably 1000 μm or less. The lower limit of the length L is not particularly limited, but is preferably 5 μm or more, more preferably 30 μm or more, and even more preferably 80 μm or more. When the length of one side of the non-thin line region is within the above-mentioned range, it is possible to further maintain good transparency, and when the conductive film is attached to the front of a display device, the display can be viewed without any sense of incongruity.

[0029] In terms of visible light transmittance, the opening ratio of the mesh pattern is preferably 90% or more, more preferably 95% or more, and even more preferably 99% or more. There is no particular upper limit, but it may be less than 100%. The aperture ratio means the ratio (area ratio) of the area where no conductive thin wires are arranged to the total area of ​​the surface of the transparent substrate on the side where the mesh pattern of the conductive film is formed.

[0030] The line width Wa of the conductive thin line is preferably 5.0 μm or less, more preferably 2.5 μm or less, and even more preferably 2.0 μm or less, in terms of the effects of the present invention being more excellent, and the lower limit is not particularly limited, but is preferably 0.5 μm or more, more preferably 1.0 μm or more, and even more preferably 1.5 μm or more, in terms of the effects of the present invention and the conductivity of the conductive film being more excellent.

[0031] The thickness Ta of the conductive thin wire is not particularly limited, but is preferably 0.1 μm or more, more preferably 0.3 μm or more, in terms of superior conductivity of the conductive film. The upper limit is not particularly limited, but is preferably 10 μm or less, more preferably 3 μm or less.

[0032] The line width Wa and thickness Ta of the conductive thin line are obtained by the following method. First, a platinum coating layer is formed on the surface of the conductive film on the conductive thin wire side by a sputtering method. Next, the conductive film having the platinum coating layer is cut along a plane including the width direction and the thickness direction by focused ion beam (FIB) processing to prepare a cross-sectional slice. The cross-section of the obtained slice is subjected to elemental analysis using a transmission electron microscope (TEM) equipped with an energy dispersive X-ray spectrometer (EDS) (for example, "Talos F200X S / TEM" manufactured by Thermo Fisher Scientific, etc.), thereby obtaining an elemental mapping image of the cross-section including the width direction and the thickness direction of the conductive thin wire. Based on the obtained elemental mapping image of the cross-section of the conductive thin wire, the line width and thickness of the conductive thin wire are obtained. For 10 arbitrarily selected locations of the conductive thin wire, cross-sectional slices are prepared using the above-described method, and elemental mapping images of the obtained cross sections are obtained. The arithmetic mean of the line widths measured at the 10 measured points and the arithmetic mean of the thicknesses measured at the 10 measured points are calculated to determine the line width Wa and thickness Ta of the conductive thin wire, respectively. A more detailed method for measuring the width Wa and thickness Ta of the conductive thin wires, and the width and thickness of each layer constituting the conductive thin wires, will be described in the examples described later.

[0033] The line resistance of the conductive thin wire is preferably less than 200 Ω / mm. In particular, from the viewpoint of operability when used as a touch panel, it is more preferably less than 100 Ω / mm, and even more preferably less than 60 Ω / mm. There is no particular lower limit, but it is preferably 1 Ω / mm or more. The linear resistance is obtained by dividing the resistance measured by the four-probe method by the distance between the measurement terminals. More specifically, after cutting both ends of any one conductive thin wire constituting the mesh pattern and separating it from the mesh pattern, four microprobes (A, B, C, D) (tungsten probes (diameter 0.5 μm) manufactured by Micro Support Co., Ltd.) are brought into contact with the separated conductive thin wire, and a constant current I is applied to the outermost probes A and D using a source meter (KEITHLEY source meter 2400 type general-purpose source meter) so that the voltage V between the inner probes B and C is 5 mV, and the resistance value Ri=V / I is measured, and the obtained resistance value Ri is divided by the distance between B and C to obtain the linear resistance value.

[0034] In addition, the thin conductive wire may or may not be electrically connected to an external member of the conductive film. A part of the thin conductive wire may be a dummy electrode that is electrically insulated from the outside. Each layer constituting the conductive thin wire will be described below. Note that the method for forming each of the layers below and the method for producing the conductive thin wire will be described in detail later.

[0035] <Black layer> The conductive film has a black layer that includes carbon black. The carbon black contained in the black layer is not particularly limited, and any known carbon black can be used.

[0036] The average particle diameter of the carbon black contained in the black layer is preferably 5 to 1000 nm, more preferably 10 to 120 nm, further preferably 20 to 80 nm, and particularly preferably 30 to 40 nm, in terms of the equivalent sphere diameter, from the viewpoint of better effects of the present invention. Note that the equivalent sphere diameter is the diameter of a spherical particle having the same volume, and the average particle diameter of carbon black is obtained by measuring the equivalent sphere diameters of 100 objects and arithmetically averaging them. The average primary particle size of the carbon black may be a catalog value.

[0037] The content of carbon black in the black layer is preferably 1 to 30 mass%, more preferably 2 to 20 mass%, even more preferably 5 to 20 mass%, and particularly preferably 10 to 15 mass%, relative to the total mass of the black layer, in terms of better effects of the present invention.

[0038] The black layer preferably further contains a resin. Examples of resins contained in the black layer include polyurethane resins, poly(meth)acrylic resins, poly(meth)acrylamide resins, epoxy resins, phenolic resins, polyimide resins, polyester resins, bismaleimide resins, polyolefin resins, isocyanate resins, phenoxy resins, polyethersulfone, polysulfone, polyphenylene sulfone, polyphenylene sulfide, polyphenyl ether, polyetherimide, and ABS resin (acrylonitrile-butadiene-styrene copolymer). The resin contained in the black layer is preferably a polyurethane resin or a poly(meth)acrylic resin. An example of a material for forming the polyurethane resin is Itron Z-913-3 (manufactured by Aica Kogyo Co., Ltd.). An example of a material for forming the poly(meth)acrylic resin is polyethylene glycol diacrylate. An example of the polyethylene glycol diacrylate that can be used is Aronix M240 (manufactured by Toagosei Co., Ltd.).

[0039] The weight average molecular weight of the resin contained in the black layer is not particularly limited, and is preferably from 2,000 to 1,000,000, more preferably from 2,000 to 750,000, and even more preferably from 3,000 to 500,000. The resin contained in the black layer may be one type alone or a combination of two or more types. The resin content in the black layer is preferably from 65 to 95% by mass, and more preferably from 75 to 90% by mass, based on the total mass of the black layer.

[0040] The Pd content in the black layer is preferably 10 mass % or less based on the total mass of the black layer, and more preferably the black layer does not substantially contain Pd. The lower limit is not particularly limited, and may be 0 mass %. The metal content in the black layer is preferably 10% by mass or less based on the total mass of the black layer, and more preferably the black layer does not substantially contain metal. The lower limit is not particularly limited, and may be 0% by mass.

[0041] The black layer may contain additives other than the above-mentioned components, if necessary. Additives include, for example, colorants other than carbon black, UV absorbers, and light stabilizers. The content of the additive in the black layer is preferably 20% by mass or less, and more preferably 5% by mass or less, based on the total mass of the black layer. There is no particular lower limit, and it may be 0% by mass.

[0042] The line width W1 of the black layer is preferably 2.00 μm or less, more preferably 1.90 μm or less, and even more preferably 1.50 μm or less, in terms of better transmittance. There is no particular lower limit, but it is preferably 0.80 μm or more, more preferably 0.85 μm or more, and even more preferably 1.00 μm or more. The thickness T1 of the black layer is not particularly limited, but in terms of obtaining better effects of the present invention, it is preferably 0.1 to 3.0 μm, more preferably 0.2 to 2.0 μm, and even more preferably 0.5 to 1.5 μm. The line width W1 of the black layer can be measured in accordance with the method for measuring the line width Wa of the thin conductive wire, and the thickness T1 of the black layer can be measured in accordance with the method for measuring the thickness Ta of the thin conductive wire.

[0043] <Palladium-containing layer> The palladium-containing layer (Pd-containing layer) is a layer constituting the conductive thin wires and contains palladium (Pd). The form of Pd contained in the Pd-containing layer (hereinafter also referred to as "Pd component") is not particularly limited, and may be Pd alone or a mixture of Pd and a metal other than Pd (Pd alloy). Examples of metals other than Pd include silver, copper, gold, and nickel. In particular, the Pd-containing layer preferably contains simple Pd.

[0044] The Pd component (preferably Pd alone) contained in the Pd-containing layer is often solid Pd particles. The average particle size of the Pd particles is preferably 10 to 1000 nm, more preferably 10 to 200 nm, in terms of sphere-equivalent diameter. It is even more preferably 50 to 150 nm, in that the change in resistance value of the conductive thin wire in a humid and hot environment is smaller. The sphere-equivalent diameter is the diameter of a spherical particle having the same volume, and the average particle size of the Pd particles is obtained by measuring the sphere-equivalent diameters of 100 objects and arithmetically averaging them. The shape of the Pd particles is not particularly limited, and examples thereof include spherical, cubic, tabular, octahedral, tetradecahedral, etc. In addition, the Pd particles may be bonded in part or entirely by fusion.

[0045] The Pd-containing layer may have a structure in which the Pd component is dispersed in a polymeric compound described later, or the Pd component may be aggregated in the polymeric compound and exist as aggregates. Furthermore, at least some of the Pd components contained in the Pd-containing layer may be bonded to each other by a metal derived from metal ions used in a plating process described later. The content of the Pd component in the Pd-containing layer is not particularly limited. In order to obtain a conductive film with superior conductivity, the content of the Pd component per area of ​​the region on the transparent substrate surface where the Pd-containing layer is disposed (in terms of Pd element) is preferably 1.0 to 20.0 g / m. 2 and preferably 2.0 to 10.0 g / m 2 It is more preferable that:

[0046] The Pd-containing layer may contain a binder component. The binder component contained in the Pd-containing layer is not particularly limited, and for example, a known polymer compound can be used.

[0047] The polymer compound contained in the Pd-containing layer may be a hydrophobic polymer (a water-insoluble polymer), such as at least one resin selected from the group consisting of (meth)acrylic resins, styrene resins, vinyl resins, polyolefin resins, polyester resins, polyurethane resins, polyamide resins, polycarbonate resins, polydiene resins, epoxy resins, silicone resins, cellulose polymers, chitosan polymers, and gelatin, or a copolymer consisting of monomers constituting these resins. In addition, the polymer compound preferably has a reactive group that reacts with a crosslinking agent described below. The polymer compound is preferably in the form of particles, that is, the Pd-containing layer preferably contains particles of a specific polymer. The polymer compound can be synthesized by referring to, for example, Japanese Patent No. 3305459 and Japanese Patent No. 3754745.

[0048] The weight average molecular weight of the polymer compound is not particularly limited, and is preferably from 2,000 to 1,000,000, more preferably from 2,000 to 750,000, and even more preferably from 3,000 to 500,000. The polymer compound contained in the Pd-containing layer may be one type alone or a combination of two or more types. The content of the polymer compound in the Pd-containing layer is preferably 1% by mass or more, more preferably 5% by mass or more, based on the total mass of the Pd-containing layer. The upper limit is not particularly limited and may be the remainder other than the Pd component, and is preferably 50% by mass or less.

[0049] The Pd-containing layer may contain a metal other than Pd, such as silver, copper, gold, nickel, and iron. The content of metals other than Pd is preferably 20 mass % or less, and more preferably 5 mass % or less, based on the total mass of the Pd-containing layer.

[0050] The Pd-containing layer may contain additives other than the above-mentioned components, if necessary. Examples of the additives include antistatic agents, nucleation accelerators, spectral sensitizing dyes, surfactants, antifoggants, hardeners, anti-black spot agents, redox compounds, monomethine compounds, and dihydroxybenzenes, as described in paragraphs 0220 to 0241 of JP2009-004348A. The Pd-containing layer may also contain a crosslinking agent used for crosslinking the above-mentioned polymer compounds together. By containing the crosslinking agent, crosslinking between specific polymers progresses, and the bonds between metals in the Pd-containing layer are maintained.

[0051] On the other hand, the content of carbon black in the Pd-containing layer is preferably 10 mass % or less based on the total mass of the Pd-containing layer, and more preferably the Pd-containing layer does not substantially contain carbon black. The lower limit is not particularly limited and may be 0 mass %. The content of the colorant in the Pd-containing layer is preferably 5% by mass or less based on the total mass of the Pd-containing layer, and more preferably the Pd-containing layer does not substantially contain a colorant. The lower limit is not particularly limited and may be 0% by mass.

[0052] The line width W2 of the Pd-containing layer is preferably 0.5 μm or more, more preferably 0.8 μm or more, and even more preferably 1.0 μm or more, in terms of the effects of the present invention and electrical conductivity being more excellent. It is presumed that when the line width W2 is equal to or greater than the above lower limit, the adhesion area with the metal plating layer increases. The upper limit of the line width W2 is not particularly limited, but is preferably 2.5 μm or less, more preferably 1.9 μm or less, and even more preferably 1.5 μm or less, in terms of the effects of the present invention being more excellent. It is presumed that when the line width W2 is equal to or less than the above upper limit, the stress generated between the Pd-containing layer and the metal plating layer can be suppressed. The thickness T2 of the Pd-containing layer is not particularly limited, but is preferably 0.05 to 1.5 μm, more preferably 0.1 to 0.8 μm, and further preferably 0.2 to 0.5 μm. The line width W2 of the Pd-containing layer can be measured in accordance with the method for measuring the line width Wa of the thin conductive wire, and the thickness T2 of the Pd-containing layer can be measured in accordance with the method for measuring the thickness Ta of the thin conductive wire.

[0053] <Metal plating layer> The metal plating layer is a layer that constitutes the conductive thin wires, and is a layer that is disposed on the side of the Pd-containing layer opposite the transparent substrate.

[0054] The metal contained in the metal plating layer is not particularly limited, and any known metal can be used. Examples of the metal contained in the metal plating layer include a simple metal selected from the group consisting of silver, copper, gold, nickel, cobalt, and palladium, and a mixture (alloy) of two or more metals selected from the above group. Among them, at least one of silver and copper is preferred in terms of superior electrical conductivity, and simple copper or a copper alloy of copper and a metal selected from the group consisting of silver, gold, nickel, cobalt, and palladium is more preferred, and simple copper is even more preferred.

[0055] The metal plating layer preferably contains the above metal as a main component. The metal plating layer "contains a metal as a main component" means that the metal content is 50 mass% or more based on the total mass of the metal plating layer. The metal (more preferably copper or copper alloy) content in the metal plating layer is preferably 90 mass% or more, more preferably 95 mass% or more, based on the total mass of the metal plating layer. There is no particular upper limit, and it may be 100 mass% based on the total mass of the metal plating layer.

[0056] The line width W3 of the metal plating layer is preferably 0.5 μm or more, more preferably 1.0 μm or more, and even more preferably 1.5 μm or more, in terms of the effects of the present invention and electrical conductivity being more excellent. There is no particular upper limit, but in terms of the effects of the present invention being more excellent, it is preferably 5.0 μm or less, more preferably 2.5 μm or less, and even more preferably 2.0 μm or less. The thickness T3 of the metal plating layer is preferably 0.1 μm or more, more preferably 0.3 μm or more, in terms of better electrical conductivity. There is no upper limit, but the thickness is preferably 3.0 μm or less, more preferably 1.0 μm or less. The line width W3 and thickness T3 of the metal plating layer can be measured in accordance with the method for measuring the line width Wa and thickness Ta of the conductive thin wire.

[0057] In order to obtain a more excellent effect of the present invention, the ratio (W3 / W1) of the line width W3 of the metal plating layer to the line width W1 of the black layer is preferably 1.00 to 1.25, and more preferably greater than 1 to 1.1.

[0058] [Other components] The conductive film may have other components in addition to the above-mentioned transparent substrate, black layer, conductive thin wires, and transparent insulating portion. Other members that the conductive film may have include a blackened layer, a transparent insulating portion, and a conductive portion having a configuration different from that of the conductive thin wires described below.

[0059] <Blackened layer> The conductive thin wires of the conductive film may have a blackened layer disposed on the side of the metal plating layer opposite the transparent substrate, i.e., the conductive thin wires may have, in order from the transparent substrate side, the black layer, the palladium-containing layer, the metal plating layer, and the blackened layer. The blackening layer has a function of preventing light reflection from the conductive thin wires arranged on the top surface (the surface on the viewing side) of the transparent substrate, and further improving visibility. Examples of the blackening layer include known black plating layers such as a black chrome plating layer, a black nickel plating layer, and a black alumite plating layer. These blackened layers can be formed by plating using a known black metal material.

[0060] <Transparent insulation part> The conductive film may have a transparent insulating portion in a non-fine wire region on the surface on which the thin conductive wires are arranged, where the thin conductive wires are not arranged. The transparent insulating portion is preferably disposed alongside the thin conductive wires and adjacent to the thin conductive wires in the width direction of the thin conductive wires.

[0061] The transparent insulating part is a member that does not contain conductive metal and does not exhibit conductivity. Here, the transparent insulating part "does not contain metal" means that the metal content in the transparent insulating part is 0.1 mass % or less with respect to the total mass of the transparent insulating part. The material constituting the transparent insulating portion is preferably a polymer compound. Examples of the polymer compound include the polymer compound contained in the conductive thin wire. The polymer compound constituting the transparent insulating portion may be the same as or different from the polymer compound contained in the conductive thin wire.

[0062] The thickness of the transparent insulating portion is not particularly limited, and is preferably 1 to 15 μm, and more preferably 2 to 10 μm. The thickness of the transparent insulating portion can be measured in accordance with the method for measuring the thickness Ta of the conductive thin wire. The method for forming the transparent insulating part using the composition for forming the transparent insulating part is not particularly limited. For example, the composition is applied to the surface of the transparent substrate on the side where the conductive thin wires are arranged, and the applied film is cured as necessary to form the transparent insulating part.

[0063] [Method for producing conductive film] Next, a method for producing the conductive film will be described. The method for producing the conductive film of the present invention is not particularly limited as long as the conductive film having the above-mentioned configuration can be produced. For example, the method for producing the conductive film of the present invention includes a black layer forming step of forming a black layer on at least one surface of a transparent substrate by a known method, a Pd-containing layer forming step of forming a Pd-containing layer on the black layer formed, and a metal plating layer forming step of selectively forming a metal plating layer on the surface of the Pd-containing layer formed by plating.

[0064] <Black layer formation process> The method of forming the black layer is not particularly limited, and the known method of forming a patterned coating film on a transparent substrate can be applied.The method of forming the black layer includes, for example, the method of printing the composition for forming the black layer, which contains optional components such as carbon black, resin and other colorants, on a transparent substrate in a pattern, the method of printing the composition for forming the black layer, which further contains a polymerizable compound, on the entire surface of the transparent substrate, exposing and developing to form a patterned black layer, and the method of printing the composition for forming the black layer on the entire surface of the transparent substrate, and irradiating ultraviolet light or laser or the like through a mask pattern to remove unnecessary parts to form a patterned black layer.

[0065] Specific examples of the method for forming the black layer by pattern printing include screen printing, screen offset printing, gravure printing, gravure offset printing, flexographic printing, imprint printing, reverse printing, and inkjet printing. Among these, screen printing and inkjet printing are preferred.

[0066] The black layer forming composition used in the black layer forming step contains carbon black. The content of carbon black in the composition for forming a black layer is not particularly limited, but it is preferable that the content of carbon black relative to the total solid content of the composition is the same as the content of carbon black relative to the total mass of the above-mentioned black layer, including a more preferred range. The composition for forming a black layer may contain, in addition to carbon black, at least one selected from the group consisting of a solvent, the above-mentioned resin or its precursor, and the above-mentioned additives.

[0067] From the viewpoint of handling, the black layer forming composition preferably contains a solvent. The type of the solvent is not particularly limited, and examples thereof include water and organic solvents. Examples of the organic solvent include known organic solvents (e.g., alcohol-based solvents, ester-based solvents, ketone-based solvents, amide-based solvents, nitrile-based solvents, carbonate-based solvents, halogen-based solvents, and hydrocarbon-based solvents). The content of the solvent in the composition for forming the black layer is not particularly limited, but it is preferably 50 to 98% by mass, more preferably 60 to 95% by mass, based on the total mass of the composition. If it is within the above range, the handleability of the composition for forming the black layer is excellent, and the control of the thickness is facilitated. The method for preparing the composition for forming the black layer is not particularly limited, and examples thereof include a method of mixing all the above-described components at once and a method of mixing the components step by step.

[0068] <Pd-containing layer forming step> As the Pd-containing layer forming step, there is no particular limitation as long as it is a method of forming a Pd-containing layer on the black layer formed by the black layer forming step, and a known method is adopted. As a method for forming the Pd-containing layer, for example, a method of forming the Pd-containing layer by pattern printing a composition containing a Pd component and a binder component on the black layer, and a method of forming a coating film containing a Pd component and a binder component on the entire surface of the transparent substrate where the black layer is formed, and then removing the coating film formed in the region where the black layer does not exist using a resist pattern to form the Pd-containing layer. As a specific pattern printing method for forming the Pd-containing layer, the pattern printing methods mentioned in the black layer forming step can be mentioned, and among them, the screen printing method or the inkjet printing method is preferable.

[0069] In the Pd-containing layer forming step, as the composition for forming the Pd-containing layer used for forming the above coating film or pattern printing, for example, a composition containing a Pd component or its precursor, a binder component, and optionally a solvent can be mentioned. The Pd component and the binder component contained in the composition for forming the Pd-containing layer are as described above. The composition for forming the Pd-containing layer may contain a colloid of Pd. Further, the composition for forming the Pd-containing layer may contain Pd ions as a precursor of the Pd component.

[0070] From the viewpoint of handling, the composition for forming the Pd-containing layer preferably contains a solvent. Examples of the solvent contained in the composition for forming the Pd-containing layer include various solvents that may be contained in the composition for forming the black layer. The content of the solvent in the Pd-containing layer-forming composition is not particularly limited, but from the above-mentioned viewpoints, it is preferably 50 to 98 mass %, more preferably 60 to 95 mass %, based on the total mass of the composition. The method for preparing the composition for forming the Pd-containing layer is not particularly limited, and examples thereof include a method in which the above-mentioned components are mixed together, and a method in which the components are mixed stepwise.

[0071] <Metal plating layer formation process> The metal plating layer forming step is a step of selectively forming a metal plating layer on the surface of the Pd-containing layer formed in the Pd-containing layer forming step, and more specifically, is a step of subjecting the Pd-containing layer to a plating treatment.

[0072] The plating method is not particularly limited, and examples thereof include electroless plating (chemical reduction plating or displacement plating) and electrolytic plating, with electroless plating being preferred. Electroless plating is a process in which a solution containing the metal ions to be deposited as plating is used to deposit the metal through a chemical reaction. For electroless plating, a known electroless plating technique is used.

[0073] Examples of plating treatments include copper plating treatment, silver plating treatment, nickel plating treatment, and cobalt plating treatment. In terms of superior conductivity of the conductive thin wire, copper plating treatment or silver plating treatment is preferred, and copper plating treatment is more preferred. The components contained in the plating solution used in the plating process are not particularly limited, but in addition to a solvent (e.g., water), the plating solution often contains metal ions for plating, a reducing agent, an additive (stabilizer) for improving the stability of the metal ions, and a pH adjuster. In addition to these, the plating solution may contain known additives. The type of metal ion contained in the plating solution for plating can be appropriately selected depending on the type of metal to be deposited, and examples thereof include copper ions, silver ions, nickel ions, and cobalt ions.

[0074] The procedure for the plating treatment is not particularly limited as long as it is a method for bringing the Pd-containing layer on the transparent substrate into contact with a plating solution. Examples of the method include a method of immersing the transparent substrate having the black layer and the Pd-containing layer in a plating solution, and a method of applying a plating solution to the surface of the transparent substrate on which the black layer and the Pd-containing layer are disposed. The contact time between the Pd-containing layer and the plating solution is not particularly limited, and is preferably 20 seconds to 30 minutes in terms of superior conductivity of the conductive thin wire and productivity.

[0075] By carrying out the above black layer forming step, Pd-containing layer forming step and metal plating layer forming step, conductive fine wires having a laminated structure in which a black layer, a Pd-containing layer and a metal plating layer are laminated in that order are formed, and a mesh pattern is provided on the transparent substrate.

[0076] The method for producing the conductive film is not limited to the method having the above black layer forming step, Pd-containing layer forming step, and metal plating layer forming step. The conductive film can also be produced, for example, by coating the above black layer forming composition on the entire surface of a transparent substrate, coating the above Pd-containing layer forming composition on the entire surface of the formed coating layer to form a laminate, subjecting the formed laminate to pattern exposure and development treatment, removing unnecessary areas of the laminate, and then selectively forming a metal plating layer by plating on the surface of the patterned laminate consisting of the black layer and the Pd-containing layer.

[0077] A conductive film having a mesh pattern arranged on both sides of a transparent substrate can be manufactured by carrying out the above-mentioned series of steps on both sides of the transparent substrate. The order of each step to be carried out at this time is not particularly limited, and for example, the conductive film can be manufactured by forming a patterned laminate consisting of a black layer and a Pd-containing layer on both sides of the transparent substrate by the above-mentioned method, and then forming a metal plating layer on each of the formed Pd-containing layers. The conductive film can also be manufactured by sequentially forming a black layer, a Pd-containing layer, and a metal plating layer on one surface of the transparent substrate, and then sequentially forming a black layer, a Pd-containing layer, and a metal plating layer on the other surface of the transparent substrate.

[0078] [Uses of conductive films] The conductive film obtained as described above can be used in a variety of applications, including touch panels (or touch panel sensors), semiconductor chips, various electric wiring boards, FPCs (Flexible Printed Circuits), COFs (Chip on Film), TABs (Tape Automated Bonding), antennas, multilayer wiring boards, and motherboards, etc. Among these, the conductive film is preferably used for touch panels (capacitive touch panels). In a touch panel having the conductive film, the conductive thin wires can effectively function as detection electrodes. When the conductive film is used in a touch panel, examples of the display panel to be used in combination with the conductive film include a liquid crystal panel and an OLED (Organic Light Emitting Diode) panel, and it is preferable to use the conductive film in combination with an OLED panel.

[0079] In addition to the conductive thin wires, the conductive film may further have a conductive part having a different configuration from the conductive thin wires. This conductive part may be electrically connected to the conductive thin wires and be conductive. Examples of the conductive part include peripheral wiring having a function of applying a voltage to the conductive thin wires and alignment marks for adjusting the position of the conductive film and the member to be laminated.

[0080] Other uses of the conductive film include, for example, electromagnetic shielding that blocks electromagnetic waves such as radio waves and microwaves (ultra-high frequency waves) generated by electronic devices such as personal computers and workstations, and prevents static electricity. Such electromagnetic shielding can be used not only in personal computers, but also in electronic devices such as video recording devices and electronic medical devices. The conductive film can also be used as a transparent heating element.

[0081] The conductive film may be used in the form of a laminate having the conductive film and other members such as an adhesive sheet and a release sheet during handling and transportation. The release sheet functions as a protective sheet for preventing the conductive film from being scratched during transportation of the laminate. The conductive film may also be handled in the form of a composite having, for example, a conductive film, an adhesive sheet, and a protective layer in this order.

[0082] The present invention is basically configured as described above. The present invention is not limited to the above-described embodiment, and various improvements and modifications may be made without departing from the spirit and scope of the present invention. EXAMPLES

[0083] The present invention will be described in more detail below with reference to the following examples. The materials, amounts, ratios, processing contents, processing procedures, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention is not limited to the following examples. Moreover, unless otherwise specified, parts and percentages are intended to be on a mass basis.

[0084] [Example 1] <Preparation of black layer-forming composition> The following components were mixed with stirring to prepare a black layer-forming composition 1. Carbon black 4.7% by mass · Acrylic monomer (DPHA, manufactured by Daicel Ornex Co., Ltd.) 34.9 mass% · Photoinitiator (Omnirad907, IGM RESINS) 0.4 mass% · Solvent (2-butanone) 30.0 mass% · Solvent (cyclopentanone) 30.0 mass% The above carbon black is "RCF#20" manufactured by Mitsubishi Chemical Corporation, and its average particle diameter was 50 nm.

[0085] <Preparation of Composition for Forming Pd-Containing Layer> The following components were mixed while stirring to prepare Composition 1 for forming a Pd-containing layer. · Nanopalladium dispersion (manufactured by Renaissance Energy Research) 5.0 mass% · Acrylic monomer (DPHA, manufactured by Daicel Ornex Co., Ltd.) 75.0 mass% · Photoinitiator (Omnirad907, IGM RESINS) 1.0 mass% · Dispersant (Solspers24000, manufactured by Lubrizol) 1.0 mass% · Solvent 2-butanone 18.0 mass%

[0086] <Fabrication of Conductive Film> Composition 1 for forming a black layer was applied to the surface of a polyethylene terephthalate film (manufactured by Fujifilm Corporation) with a thickness of 38 μm using a lip coater. After drying, Composition 1 for forming a Pd-containing layer was applied to the surface of the obtained coating film using a lip coater and dried to obtain a laminate. A negative mask pattern having the pattern shown in Figure 3 was placed on the surface of the obtained laminate, and ultraviolet light with a wavelength of 365 nm was irradiated onto the laminate through the negative mask pattern using a high-pressure mercury lamp for pattern exposure. The exposure amount was 500 mJ / cm 2 It was. Next, after removing the mask pattern, the entire exposed surface of the laminate was immersed in a 1 mass% aqueous sodium carbonate solution (alkali developer, solution temperature 30 °C) for 60 seconds at 0.18 MPa (1.8 kgf / cm 2) to dissolve and remove the coating film of the black layer-forming composition 1 and the coating film of the Pd layer-forming composition 1 in the unexposed areas of the laminate. By the above-mentioned development treatment, a patterned laminate consisting of a black layer and a Pd-containing layer as shown in FIG. 3 was formed.

[0087] Next, the above series of steps was repeated on the other surface of the transparent substrate, thereby forming a patterned laminate consisting of a black layer and a Pd-containing layer on both sides of the transparent substrate.

[0088] Next, the transparent substrate having a patterned laminate consisting of a black layer and a Pd-containing layer on both sides was immersed in an electroless copper plating solution, Thru-cup PEA (manufactured by Uemura Kogyo Co., Ltd.), at room temperature for 30 minutes, and then washed with pure water. Thus, a conductive film 1 was produced, which has a mesh pattern consisting of conductive thin lines on both sides of the transparent substrate, which has a black layer, a Pd-containing layer, and a copper plating layer in that order from the transparent substrate side.

[0089] Fig. 3 is a plan view showing an example of the configuration of a mesh pattern of the conductive film produced in Example 1. The conductive film 40 shown in Fig. 3(a) has a mesh pattern 42 in which unit patterns P are arranged in two orthogonal directions in a plane. Fig. 3(b) is an enlarged plan view of the unit pattern P shown in Fig. 3(a). As shown in Fig. 3(b), the unit pattern P has a shape in which two parallel line segments and two parallel line segments are perpendicular to each other. Each of the four line segments constituting the unit pattern P is a conductive thin wire 20 made of a black layer, a Pd-containing layer, and a copper plating layer. The distance between the centers of the two parallel line segments was 300 μm in each unit pattern P. That is, each unit pattern P was surrounded by four thin conductive wires, forming a square non-thin wire region with one side measuring 300 μm minus the line width Wa of the thin conductive wire. The distance between adjacent unit patterns P was 15 μm. That is, the line segment of one unit pattern P and the line segment of the adjacent unit pattern P, which were on the same straight line, were spaced 15 μm apart from each other.

[0090] <Measurement of the line width and thickness of conductive thin wires and each layer> The conductive film obtained in Example 1 was cut to prepare a square sample having a size of 1 cm on each side, with each side perpendicular or perpendicular to the width direction of the conductive thin wire. A platinum coating layer having a thickness of 40 nm was deposited on the surface of the obtained sample on which the mesh pattern was formed, using an ion sputtering device. Next, the sample with the platinum coating layer formed was cut along a plane including the line width direction and thickness direction by FIB processing using a FIB-SEM device (Helios600i, manufactured by Thermo Fisher Scientific) at an acceleration voltage of 30 kV to prepare slices with a thickness of 100 nm. Elemental analysis was performed on the cross-section of the obtained slice using a TEM device equipped with EDS ("Talos F200X S / TEM" manufactured by Thermo Fisher Scientific, accelerating voltage 200 kV), and an elemental mapping image (hereinafter also referred to as "cross-sectional image") of the cross-section including the line width direction and thickness direction of the conductive thin wire was obtained.

[0091] Based on the element distribution of the platinum coating layer in the cross-sectional image obtained by the above method, the maximum line width and the average thickness of the conductive thin wires were measured. In addition, the black layer, the Pd-containing layer, and the metal plating layer were identified based on the element distribution of the cross-sectional image obtained by the above method. Specifically, the region where Pd was detected in the element distribution of Pd was determined as the Pd-containing layer. Next, the region where Pd was not present in the element distribution of Pd and was located closer to the transparent substrate than the Pd-containing layer was determined as the black layer. The region of the black layer also coincided with the region where C was present in the element distribution of C. Next, the region where Cu was present in the element distribution of Cu and where Pd was not present in the element distribution of Pd was determined as the metal plating layer. Regarding the measurement of the line widths of the black layer, the Pd-containing layer and the metal plating layer obtained by the above method, when the line width of each layer differed depending on the position in the thickness direction in one cross-sectional image, or when the thickness of each layer differed depending on the position in the width direction, a representative value of the line width and a representative value of the thickness of each layer were determined by the following method. Taking the Pd-containing layer as an example, the maximum distance in the width direction of the region where Pd is detected in the Pd element distribution of the cross-sectional image was used as the representative value of the line width of the Pd-containing layer. Also, the entire width of the region where Pd is detected in the Pd element distribution of the cross-sectional image was divided into 10 parts in order from the end, the distance in the thickness direction of each divided region was measured, and the average value obtained by arithmetically averaging the 10 measured values ​​was used as the representative value of the thickness of the Pd-containing layer. The representative values ​​of the line width and thickness of the black layer and the line width and thickness of the metal plating layer were also measured according to the above-mentioned measurement methods.

[0092] According to the above method, the conductive thin wire was cut at 10 different positions in the platinum-coated sample, and the line width and thickness of the conductive thin wire and each layer of the conductive thin wire were obtained from the cross-sectional image of the obtained cut. The line width Wa and thickness Ta of the conductive thin wire, the line width W1 and thickness T1 of the black layer, the line width W2 and thickness T2 of the Pd-containing layer, and the line width W3 and thickness T3 of the metal plating layer were calculated by arithmetically averaging the representative values ​​of the line width and the thickness of the 10 points obtained. The line width and thickness of each layer obtained in the conductive film 1 of Example 1 are listed in Table 1 below. The line width Wa of the conductive thin wire was the same as the maximum value among the line width W1 of the black layer, the line width W2 of the Pd-containing layer, and the line width W3 of the metal plating layer, and the thickness Ta of the conductive thin wire was the same as the sum of the thickness T1 of the black layer, the thickness T2 of the Pd-containing layer, and the thickness T3 of the metal plating layer.

[0093] [Examples 2 to 7, 24] The conductive films of Examples 2 to 7 and 24 were produced according to the method described in Example 1, except that the line width of the black layer formed in the black layer forming step, the line width W2 of the Pd-containing layer formed in the Pd-containing layer forming step, and the immersion time in the plating solution in the metal plating layer forming step were changed so that the line width W1 and thickness T1 of the black layer, the line width W2 and thickness T2 of the Pd-containing layer, and the line width W3 and thickness T3 of the metal plating layer were the numerical values ​​shown in Table 1 below.

[0094] [Examples 8 to 12] The conductive films of Examples 8 to 12 were produced according to the method described in Example 3, except that carbon black having an average particle diameter shown in Table 1 below was used instead of the carbon black used in preparing the composition 1 for forming a black layer. In Examples 8 to 12, commercially available carbon black such as "SB935" manufactured by Asahi Carbon Co., Ltd. was used.

[0095] [Examples 13 to 17] The conductive films of Examples 13 to 17 were produced according to the method described in Example 3, except that the content of carbon black contained in the composition for forming a black layer was adjusted so that the content of carbon black contained in the black layer was the value shown in Table 1 below.

[0096] [Examples 18 to 23] The conductive films of Examples 18 to 23 were produced according to the method described in Example 3, except that the thickness of the printed layer of the black layer-forming composition 1 printed in the black layer formation process was adjusted so that the thickness T1 of the black layer would be the value shown in Table 1 below.

[0097] [Comparative Example 1] The conductive film of Comparative Example 1 was produced according to the method described in Example 1, except that the black layer forming step was not performed and a patterned Pd-containing layer was directly formed on the transparent substrate in the Pd-containing layer forming step.

[0098] [Comparative Example 2] The conductive film of Comparative Example 2 was produced according to the method described in Example 1, except that no carbon black was used and a black layer-forming composition not containing carbon black was prepared.

[0099] [evaluation] For the conductive films of each of the Examples and Comparative Examples, a durability test was carried out in the following manner, and then the adhesion of the conductive thin wires was evaluated.

[0100] First, the conductive film was cut into a sample measuring 50 mm in length and 50 mm in width. The obtained sample was evaluated in a test tank equipped with a black panel under the following conditions in accordance with the method described in JIS B 7753 (2007). Sunshine Carbon Arc ·Illuminance 255W / m 2 (300~700nm) Test time: 1,083h (78.5W / m 2 ) Black panel temperature: 63℃ ·Battle humidity: 55%

[0101] Next, a 3M tape "610" (width 25.4 mm) was adhered to the bottom surface of the sample on which the durability test was conducted (the surface of the conductive film opposite the light source side) for a length of 1 cm or more, and the adhered tape was then peeled off from the bottom surface of the sample. For each unit pattern P that was entirely contained within the area where the tape was attached (in other words, each unit pattern P in which all of the conductive thin wires were attached to the tape), the presence or absence of peeled conductive thin wires was confirmed using an optical microscope. The ratio of the number of unit patterns P in which at least one conductive thin wire had peeled off to the total number of unit patterns P that were entirely contained within the area where the tape was attached (peeling rate of unit pattern P) was calculated using the following formula. (Number of peeled unit patterns P) / (Total number of unit patterns P)×100(%)

[0102] From the calculated peeling rate of the unit pattern P, the adhesion of the conductive thin wires in the conductive film of each Example or Comparative Example after the durability test was evaluated based on the following criteria. (Evaluation Criteria) A: Peeling rate is between 0% and 20% B: Peeling rate is 20% or more but less than 40% C: Peeling rate is 40% or more but less than 60% D: Peeling rate is 60% or more and 100% or less

[0103] The measurement results and evaluation results of the conductive films produced in each example are summarized in Table 1 below. In the table, the column "W3 / W1" indicates the ratio of the line width W3 (μm) of the metal plating layer to the line width W1 (μm) of the black layer.

[0104] [Table 1]

[0105] From the results shown in the above table, it was confirmed that the conductive films of the present invention produced in each Example can provide conductive films having superior adhesion of conductive thin wires after durability tests, compared to the conductive film of Comparative Example 1 having no black layer and the conductive film of Comparative Example 2 having an intermediate layer having no carbon black. [Explanation of symbols]

[0106] 10,40 Conductive film 12 Transparent base material 20 Conductive thin wire 22 Black layer 24 Pd-containing layer 26 Metal plating layer 30 Non-thin line area 42 Mesh Pattern P unit pattern

Claims

1. A transparent substrate; A mesh pattern is disposed on the transparent substrate and is made of conductive thin wires. The conductive thin wire has, from the transparent substrate side, a black layer containing carbon black, a palladium-containing layer, and a metal plating layer.

2. The conductive film according to claim 1, wherein the line width of the metal plating layer is 1.0 to 2.5 μm.

3. The conductive film according to claim 1 or 2, wherein the line width of the black layer is 0.85 to 1.90 μm.

4. 3. The conductive film according to claim 1, wherein the ratio of the line width of the metal plating layer to the line width of the black layer is greater than 1 to 1.

1.

5. The conductive film according to claim 1 or 2, wherein the black layer has a thickness of 0.2 to 2.0 μm.

6. 3. The conductive film according to claim 1, wherein the carbon black contained in the black layer has an average particle size of 10 to 120 nm.

7. 3. The conductive film according to claim 1, wherein the content of the carbon black is 2 to 20 mass % based on the total mass of the black layer.

Citation Information