Polishing pad
The polishing pad with a polyurethane resin foam layer and softer base layer addresses the challenge of maintaining high hardness and flatness, improving outer periphery flatness and extending the pad's life by evenly distributing pressure.
Patent Information
- Application Number
- JP2023044147
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional polishing pads face limitations in achieving high hardness while maintaining the flatness of the outer periphery of objects being polished, leading to potential damage and reduced pad life due to uneven pressure distribution.
A polishing pad design comprising a polyurethane resin foam polishing layer with a base layer having a 5% modulus ratio of the base layer to polishing layer greater than 5, ensuring the base layer is softer than the polishing layer to distribute pressure evenly and prevent edge roll-off.
The design enhances the flatness of the outer periphery of polished objects by preventing pressure unevenness and extending the pad's lifespan by reducing damage.
Smart Images

Figure 2024134058000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a polishing pad, and more particularly to a polishing pad for polishing an object to be polished. [Background technology]
[0002] Conventionally, polishing pads in which the polishing surface is formed by polyurethane resin foam have been known as polishing pads for polishing (mirror polishing) objects to be polished, such as semiconductor wafers such as silicon wafers and glass plates (for example, Patent Document 1 below).
[0003] The polishing process of the workpiece using the polishing pad is carried out, for example, using a polishing machine having a disk-shaped head and a disk-shaped lower platen arranged opposite the head, according to the following procedure. (1) A disk-shaped workpiece is attached to the lower surface of the head of the polishing machine via a disk-shaped holding material, and a disk-shaped polishing pad is attached to the upper surface of the lower platen of the polishing machine. (2) The head is moved downward and the lower platen is moved upward to bring the workpiece attached to the lower surface of the head into contact with the polishing surface (upper surface) of the polishing pad attached to the lower platen. (3) With the workpiece in contact with the polishing pad, the head and the lower platen are rotated while supplying a polishing slurry to the polishing surface (upper surface) of the polishing pad, whereby the workpiece is polished by the polishing pad.
[0004] In recent years, in the polishing process of the object to be polished, there has been an increasing demand for improving the flatness of the outer periphery of the object to be polished (hereinafter referred to as outer periphery flatness). For example, Patent Document 2 below describes a high-hardness polishing pad (for example, an apparent density of 0.50 g / cm 3It is described that by using a polishing pad having a 5% modulus of 4.00 MPa or more, the peripheral flatness of the object to be polished can be improved. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2010-274361 A [Patent Document 2] JP 2007-250166 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, there is a limit to how hard a polishing pad can be made, that is, how hard the polishing pad can be made. Furthermore, the harder the polishing pad is, the more likely it is to be damaged when polishing an object to be polished. If the polishing pad is damaged in this manner, the pad life of the polishing pad will be shortened, which is undesirable.
[0007] For the reasons mentioned above, there is a demand for polishing pads that can increase the peripheral flatness of the workpiece being polished in addition to having high hardness, but it cannot be said that sufficient research has been conducted on this issue yet.
[0008] In view of the above circumstances, an object of the present invention is to provide a polishing pad that can increase the peripheral flatness of an object to be polished other than by increasing the hardness. [Means for solving the problem]
[0009] The polishing pad according to the present invention comprises: A polishing layer having a polishing surface and a base layer laminated on the polishing layer on the surface opposite to the polishing surface, the polishing surface is formed of a surface of a polyurethane resin foam containing a polyurethane resin, The 5% modulus value M of the underlayer L The 5% modulus value M of the polishing layer P Ratio (M P / M L ) is 5 or greater. Effect of the Invention
[0010] According to the present invention, a polishing pad can be provided that can increase the peripheral flatness of an object to be polished in addition to having a high hardness. [Brief description of the drawings]
[0011] [Figure 1] 1 is a schematic cross-sectional view showing a state in which the polishing pad according to the embodiment is used. [Diagram 2] 1 is a schematic cross-sectional view showing a polishing pad according to an embodiment of the present invention. [Diagram 3] 1 is a schematic cross-sectional view showing a state in which a polishing pad according to this embodiment is attached to a platen of a polishing machine via an adhesive layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, one embodiment of the present invention will be described. In the following, one embodiment of the present invention may be simply referred to as the present embodiment.
[0013] The polishing pad 10 according to this embodiment is used to polish an object 20 in a polishing machine (polishing machine) 1000 including a platen (lower platen) 100 and a head 200, as shown in FIG. In this embodiment, the polishing machine 1000 includes, in addition to the platen 100 and the head 200, a slurry supplying unit 300 for supplying polishing slurry. In this embodiment, the head 200 of the polisher 1000 includes a holder (upper platen) 200a for holding the object 20 to be polished. As shown in FIG. 1, the polishing pad 10 of this embodiment is attached to a base plate 100, and then the polishing surface 10a of the polishing pad 10 is used to polish the polishing surface 20a of the polished object 20 attached to the holding material 200a of the head 200. In addition, Figure 1 illustrates an example in which the polishing pad 10 of this embodiment is attached to a single-sided polisher for polishing one side of the workpiece 20, but the polishing pad 10 of this embodiment may also be attached to a double-sided polisher for use. More specifically, the polishing pad 10 according to this embodiment may be attached to each of a pair of platens in a double-sided polisher having a pair of platens arranged opposite each other.
[0014] As shown in FIG. 2, the polishing pad 10 according to this embodiment includes a polishing layer 1 having a polishing surface 10a, and a base layer 2 laminated on the polishing layer 1 on a surface 10b opposite to the polishing surface 10a. Needless to say, the polishing pad 10 according to this embodiment is attached on the base layer 2 side to the platen 100 of the polisher 1000 so that the polishing surface 10a of the polishing layer 1 is exposed.
[0015] In the polishing pad 10 according to this embodiment, the polishing surface 10a is composed of the surface of a polyurethane resin foam containing a polyurethane resin. In the polishing pad 10 according to this embodiment, the polishing layer 1 may be made of the polyurethane resin foam. In the polishing pad 10 according to this embodiment, the 5% modulus value M of the underlayer 2 L The 5% modulus value M of the polishing layer 1 P Ratio (M P / M L ) is 5 or greater. The polishing pad 10 of this embodiment polishes the polished surface 20a by interposing a polishing slurry containing abrasive grains between the polishing surface 10a and the exposed surface of the workpiece to be polished (polished surface 20a) and bringing the polishing surface 10a and the polished surface 20a into sliding contact with each other. The object 20 to be polished may be an optical material, a semiconductor device, a hard disk, a glass plate, a semiconductor wafer such as a silicon wafer, or the like.
[0016] The 5% modulus value M of the polishing layer 1 P can be determined in accordance with JIS K 6251:2010 by preparing a dumbbell-shaped test piece (dumbbell No. 1 test piece) using the abrasive layer 1 and measuring the value when the dumbbell-shaped test piece is pulled at a tensile speed of 100 mm / min. In addition, the 5% modulus value M of the base layer 2 L The surface roughness of the polishing layer 1 can be measured in the same manner as in the case of the polishing layer 1, except that the dumbbell-shaped test piece is prepared using the underlayer 2.
[0017] In the polishing pad 10 according to this embodiment, the 5% modulus value M L The 5% modulus value M of the polishing layer 1 P Ratio (M P / M L ) is important to be 5 or greater. That is, the 5% modulus value M of the undercoat layer 2 L is the 5% modulus value M of the polishing layer 1. P It is important that the value is sufficiently smaller than
[0018] Here, the 5% modulus refers to the tensile stress δ (unit: MPa) when the strain ε of a test specimen such as a dumbbell-shaped test piece is 5%. The larger the 5% modulus value, the harder the material will be, and the smaller the 5% modulus value, the softer the material will be. In the polishing pad 10 according to this embodiment, as described above, the 5% modulus value M L is the 5% modulus value M of the polishing layer 1. P is significantly smaller than That is, in the polishing pad 10 according to this embodiment, the polishing layer 1 has a sufficient hardness, while the underlayer 2 has a sufficient softness.
[0019] When the polishing layer 1 is polishing the object 20 to be polished, it is thought that stress tends to concentrate at the boundary between the contact portion between the polishing layer 1 and the object 20 to be polished and the non-contact portion between the polishing layer 1 and the object 20 to be polished. That is, it is considered that stress concentration occurs on the outer periphery of the polished object 20. That is, it is considered that pressure unevenness occurs between the contact portion of the polishing layer 1 with the polished object 20 and the non-contact portion of the polishing layer 1 with the polished object 20. In this state, when the polishing layer 1 is used to polish the object 20, the flatness of the outer periphery of the object 20 may be inferior to that of the center of the object 20. In other words, edge roll-off may occur in the object 20. However, in the polishing pad 10 according to this embodiment, the base layer 2 is sufficiently soft, so that the base layer 2 is crushed before the polishing layer 1 is crushed. This makes it possible to prevent pressure unevenness from occurring between the portion of the polishing layer 1 that is in contact with the object 20 to be polished and the portion of the polishing layer 1 that is not in contact with the object 20 to be polished. In other words, the foundation layer 2 is crushed before the polishing layer 1, so that the occurrence of pressure unevenness in the polishing layer 1 can be canceled. Therefore, when the polishing surface 20a of the polishing object 20 is polished by the polishing layer 1, the outer periphery of the polishing object 20 can be prevented from being excessively polished, thereby preventing edge roll-off from occurring. As a result, the surface 20a of the object 20 to be polished can be sufficiently polished so as to increase the flatness of the outer periphery of the object 20 to be polished.
[0020] In the polishing pad 10 according to this embodiment, M P / M L may be 6 or more, or 7 or more. Also, M P / M L The upper limit is usually 20. M P / M LBy setting the pressure within the above range, when the polishing surface 20a of the workpiece 20 is polished with the polishing layer 1 of the polishing pad 10, it is possible to further suppress the occurrence of pressure unevenness in the contact portion of the polishing layer 1 with the workpiece 20 and the non-contact portion of the polishing layer 1 with the workpiece 20. That is, the flatness of the outer periphery of the object 20 to be polished can be further improved.
[0021] In addition, M P / M L can be adjusted by appropriately selecting the materials constituting the polishing layer 1 and the materials constituting the base layer 2, and by appropriately adjusting the thicknesses of the polishing layer 1 and the base layer 2. For example, this can be adjusted by using a foamed resin (such as polyurethane resin) as the material constituting the polishing layer 1 and a material having high elasticity (such as rubber) as the material constituting the base layer 2. Furthermore, when the same type of material (e.g., polyurethane resin foam) is used as the material constituting the polishing layer 1 and the material constituting the base layer 2, the thickness can be adjusted by making the thickness of the polishing layer 1 thicker than the thickness of the base layer 2 (e.g., making the thickness of the polishing layer 1 thicker than the thickness of the base layer 2 by 10 or more times).
[0022] In the polishing pad 10 according to this embodiment, the 5% modulus value M of the underlayer 2 L may be 0.1 MPa or more, may be 0.2 MPa or more, or may be 0.3 MPa or more. Furthermore, in the polishing pad 10 of this embodiment, the 5% modulus value ML of the underlayer 2 may be 1 MPa or less, 0.9 MPa or less, 0.8 MPa or less, or 0.7 MPa or less. 5% modulus value M of base layer 2 L By setting the pressure within the above range, when the polishing surface 20a of the workpiece 20 is polished with the polishing layer 1 of the polishing pad 10, it is possible to more sufficiently suppress the occurrence of pressure unevenness in the contact portion of the polishing layer 1 with the workpiece 20 and the non-contact portion of the polishing layer 1 with the workpiece 20.
[0023] In the polishing pad 10 according to this embodiment, the 5% modulus value M P may be 1 MPa or more, may be 2 MPa or more, or may be 3 MPa or more. In the polishing pad 10 according to this embodiment, the 5% modulus value M P may be 10 MPa or less, may be 8 MPa or less, may be 7 MPa or less, or may be 5 MPa or less. By setting the 5% modulus value MP of the polishing layer 1 in the above range, the polishing layer 1 can be made to have sufficient hardness for polishing the polished surface 20 a of the polished object 20 .
[0024] In the polishing pad 10 of this embodiment, the thickness T1 of the polishing layer 1 may be 0.1 mm or more, 0.2 mm or more, 0.5 mm or more, 0.8 mm or more, or 1.0 mm or more. The upper limit of the thickness T1 of the polishing layer 1 is usually 5.0 mm.
[0025] In the polishing pad 10 of this embodiment, the thickness T2 of the underlayer 2 may be 0.01 mm or more, 0.02 mm or more, 0.05 mm or more, or 0.07 mm or more. The thickness T2 of the underlayer 2 may be 1 mm or less, 0.8 mm or less, 0.5 mm or less, 0.2 mm or less, or 0.1 mm or less.
[0026] In the polishing pad 10 according to this embodiment, it is preferable that the thickness T1 of the polishing layer 1 is greater than the thickness T2 of the underlayer 2. In the polishing pad 10 of this embodiment, the ratio (T2 / T1) of the thickness T2 of the base layer 2 to the thickness T1 of the polishing layer 1 may be 0.03 or more, 0.05 or more, or 0.07 or more. T2 / T1 may be 0.5 or less, 0.2 or less, or 0.1 or less.
[0027] The polyurethane resin contained in the polyurethane resin foam may be the same as that used in general polishing pads. The polyurethane resin contains a polyisocyanate compound (for example, a prepolymer having isocyanate groups at both ends of the molecular chain) and a curing agent. That is, the polyurethane resin foam according to the present embodiment is prepared by preparing a liquid mixture containing the polyisocyanate compound and the curing agent, incorporating air bubbles into the mixture, and curing the mixture.
[0028] The polyisocyanate compound of the present embodiment may be, for example, a urethane prepolymer that contains, as constituent units, one or more types of polyols and one or more types of polyisocyanates and has an isocyanate group at its terminal. The polyisocyanate compound of the present embodiment may be a mixture of a plurality of urethane prepolymers, or may be one or more of the polyisocyanates described later. The polyisocyanate compound of the present embodiment may be a mixture of one or more types of urethane prepolymers and one or more types of polyisocyanates.
[0029] Examples of the polyol include aromatic polyols such as 1,4-benzenedimethanol and 1,4-bis(2-hydroxyethoxy)benzene; aliphatic polyols such as ethylene glycol, propylene glycol, 1,3-propanediol, 1,3-butanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, 2-methyl-1,3-propanediol, 2-butyl-2-ethyl-1,3-propanediol, and 2-methyl-1,8-octanediol; alicyclic polyols such as 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, and water-added bisphenol A; and polyfunctional polyols such as glycerin, trimethylolpropane, tributyrolpropane, pentaerythritol, and sorbitol.
[0030] The polyol may be, for example, a polyol polymer such as a polyester polyol, a polyester polycarbonate polyol, a polyether polyol, or a polycarbonate polyol. The polyol polymer may be a polyfunctional polyol polymer having three or more hydroxy groups in the molecule.
[0031] Examples of the polyester polyol include polyethylene adipate glycol, polybutylene adipate glycol, polycaprolactone polyol, and polyhexamethylene adipate glycol.
[0032] Examples of the polyester polycarbonate polyol include a reaction product of a polyester glycol such as polycaprolactone polyol with an alkylene carbonate, and a reaction product obtained by reacting ethylene carbonate with a polyhydric alcohol, which is then reacted with an organic dicarboxylic acid.
[0033] Examples of the polyether polyol include polytetramethylene ether glycol (PTMG), polypropylene glycol (PPG), polyethylene glycol (PEG), and ethylene oxide-added polypropylene polyol.
[0034] Examples of the polycarbonate polyol include reaction products of diols such as 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, diethylene glycol, polyethylene glycol, polypropylene glycol, or polytetramethylene ether glycol with phosgene, diallyl carbonate (e.g., diphenyl carbonate), or cyclic carbonate (e.g., propylene carbonate).
[0035] Examples of the polyisocyanate include aromatic isocyanates, aliphatic isocyanates, and alicyclic isocyanates.
[0036] Examples of the aromatic isocyanate include tolylene diisocyanate (TDI), 1,5-naphthalene diisocyanate, xylylene diisocyanate, 1,3-phenylene diisocyanate, and 1,4-phenylene diisocyanate. Examples of the aromatic isocyanate include diphenylmethane diisocyanate (MDI) and modified products of diphenylmethane diisocyanate (MDI).
[0037] Examples of modified diphenylmethane diisocyanate (MDI) include carbodiimide modified, urethane modified, allophanate modified, urea modified, biuret modified, isocyanurate modified, oxazolidone modified, etc. Specific examples of such modified products include carbodiimide-modified diphenylmethane diisocyanate (carbodiimide-modified MDI).
[0038] Examples of the aliphatic diisocyanate include ethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, and hexamethylene diisocyanate (HDI).
[0039] Examples of the alicyclic diisocyanate include 1,4-cyclohexane diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, isophorone diisocyanate, norbornane diisocyanate, and methylenebis(4,1-cyclohexylene) diisocyanate.
[0040] The curing agent in this embodiment may be, for example, a polyamine. The polyamine has an amino group as an active hydrogen, that is, the polyamine is an active hydrogen-containing compound.
[0041] Examples of the polyamine include 4,4'-methylenebis(2-chloroaniline) (MOCA), 4,4'-methylenedianiline, trimethylenebis(4-aminobenzoate), 2-methyl-4,6-bis(methylthio)benzene-1,3-diamine, 2-methyl-4,6-bis(methylthio)-1,5-benzenediamine, 2,6-dichloro-p-phenylenediamine, and 4,4'-methylenebis(2,3-dichloroaniline). , 3,5-bis(methylthio)-2,4-toluenediamine, 3,5-bis(methylthio)-2,6-toluenediamine, 3,5-diethyltoluene-2,4-diamine, 3,5-diethyltoluene-2,6-diamine, trimethylene glycol-di-p-aminobenzoate, 1,2-bis(2-aminophenylthio)ethane, 4,4'-diamino-3,3'-diethyl-5,5'-dimethyldiphenylmethane, and the like.
[0042] The curing agent may be the polyol. The polyol has a hydroxyl group as an active hydrogen, that is, the polyol is also an active hydrogen-containing compound. The curing agent may also be a mixture of the polyol and the polyamine.
[0043] Water may be used as a foaming agent for foaming the polyurethane resin. When water is used as the foaming agent, the apparent density of the polyurethane resin foam can be adjusted by adjusting the amount of water added. In addition, the apparent density value of the polyurethane resin foam can also be adjusted by adjusting the R value (active hydrogen / NCO), which is the equivalent ratio of the active hydrogen group of the curing agent to the isocyanate group present at the end of the polyisocyanate compound in the polyurethane resin.
[0044] The polyurethane resin foam may contain a catalyst for promoting the reaction between the polyisocyanate compound and the curing agent, and a foam stabilizer for controlling the formation of bubbles.
[0045] When the polyurethane resin foam contains the catalyst, examples of the catalyst include amine-based catalysts such as N,N-dimethylaminoethyl ether, triethylenediamine, dimethylethanolamine, triethanolamine, N,N,N',N'-tetramethylhexamethylenediamine, and N-methylimidazole, and organometallic catalysts such as dioctyltin dilaurate. The catalysts may be used alone or in combination of two or more.
[0046] When the polyurethane resin foam contains the catalyst, the content of the catalyst in the polyurethane resin foam is preferably 0.03 parts by mass or more and 0.1 parts by mass or less per 100 parts by mass of the polyisocyanate compound, since this makes it easy to adjust the size and number of air bubbles to the desired state. The content of the catalyst is more preferably 0.05 parts by mass or more and 0.1 parts by mass or less.
[0047] Examples of the foam stabilizer used in this embodiment include silicone surfactants, fluorine-based surfactants, and ionic surfactants.
[0048] The content of the foam stabilizer in the polyurethane resin foam is preferably 1 part by mass or more and 10 parts by mass or less based on 100 parts by mass of the polyisocyanate compound in order to ensure the effect of the foam stabilizer.
[0049] In the polishing pad 10 according to this embodiment, when the polishing layer 1 is made of a polyurethane resin foam, the polishing layer 1 is produced, for example, as follows.
[0050] In the manufacturing method of the polishing layer 1 in this embodiment, a urethane prepolymer having an isocyanate group as a terminal group and a foam stabilizer (e.g., the silicone-based surfactant, fluorine-based surfactant, ionic surfactant, etc.) are mixed to obtain a dispersion in which air is dispersed as bubbles. Then, the dispersion liquid is mixed with a curing agent which is an active hydrogen-containing compound (e.g., the polyamine or polyol) to polymerize the urethane prepolymer, thereby obtaining a polishing layer 1 made of polyurethane resin foam. In the method for producing the polishing layer 1 according to this embodiment, the mixing of the urethane prepolymer with the foam stabilizer, and the mixing of the dispersion with the curing agent can be carried out using a mixing head or the like. In addition, in the manufacturing method of the polishing layer 1 according to this embodiment, mixing may be performed while heating in order to improve the mixability of the urethane prepolymer and the foam stabilizer or to improve the polymerization property of the urethane prepolymer.
[0051] In the polishing pad 10 according to this embodiment, the underlayer 2 can be made from an elastomer such as polyurethane resin, butadiene rubber, or isoprene rubber. The underlayer 2 can also be made from a resin such as a polyolefin resin, a polyester resin, or a polyamide resin.
[0052] The polishing pad 10 according to this embodiment can be obtained by bonding the underlayer 2 to the polishing layer 1. The underlayer 2 can be attached to the polishing layer 1 by any of various known methods. Various known methods include a method in which a pressure-sensitive adhesive or glue is interposed between the polishing layer 1 and the base layer 2 to bond them together, a method in which a laminate of the polishing layer 1 and the base layer 2 is obtained and then the laminate is pressed in the thickness direction to bond them together, and a method in which the laminate is subjected to ultrasonic treatment and then bonded together.
[0053] As described above, examples of objects to be polished with the polishing pad according to this embodiment include optical materials, semiconductor devices, hard disks, glass plates, and semiconductor wafers such as silicon wafers. Moreover, the polishing pad according to this embodiment is suitable for use in polishing semiconductor wafers such as silicon wafers and glass plates. Furthermore, the polishing pad according to this embodiment is suitably used for polishing (mirror polishing) for providing a mirror finish to the surface to be polished of an object to be polished.
[0054] As described above, the polishing pad 10 according to this embodiment is attached to the platen (lower platen) 100 of the polisher 1000 when in use. The polishing pad 10 according to this embodiment may be attached to a platen 100 via an adhesive layer 3, as shown in FIG. The adhesive layer 3 may be, for example, a double-sided tape. The double-sided tape includes a substrate and a pressure-sensitive adhesive layer laminated on each of the two surfaces of the substrate. The substrate may be, for example, a resin film. An example of the resin film is a polyethylene terephthalate (PET) film. The pressure-sensitive adhesive layer includes a pressure-sensitive adhesive layer containing an acrylic polymer (an acrylic pressure-sensitive adhesive layer).
[0055] The thickness of the adhesive layer 3 may be 0.05 mm or more, 0.08 mm or more, or 0.10 mm or more. Furthermore, the thickness of the adhesive layer 3 may be 0.50 mm or less, 0.30 mm or less, or 0.15 mm or less. In addition, when the adhesive layer 3 is the double-sided tape, the thickness of the adhesive layer 3 means the combined thickness of the substrate and the thicknesses of the pressure-sensitive adhesive layers (two layers) laminated on both sides of the substrate.
[0056] The matters disclosed in this specification include the following.
[0057] (1) A polishing layer having a polishing surface and a base layer laminated on the polishing layer on the surface opposite to the polishing surface, the polishing surface is formed of a surface of a polyurethane resin foam containing a polyurethane resin, The 5% modulus value M of the underlayer L The 5% modulus value M of the polishing layer P Ratio (M P / M L ) is 5 or more Polishing pad.
[0058] According to this configuration, the 5% modulus value M of the underlayer L The 5% modulus value M of the polishing layer P can be made much smaller than This allows the polishing layer to have a sufficient hardness, while allowing the base layer to have a sufficient softness. Therefore, when an object to be polished is polished with the polishing layer, the base layer is crushed before the polishing layer. As a result, it is possible to suppress the occurrence of pressure unevenness between the portion of the polishing layer that contacts the workpiece and the portion of the polishing layer that does not contact the workpiece. Therefore, when the polishing surface of the workpiece is polished by the polishing layer, the outer periphery of the workpiece is prevented from being excessively polished, thereby preventing edge roll-off from occurring. This makes it possible to sufficiently polish the surface of the object to be polished so as to increase the flatness of the outer periphery of the object to be polished.
[0059] (2) The 5% modulus value M of the underlayer L is 1MPa or less The polishing pad described in (1) above.
[0060] With this configuration, when the polishing surface of the workpiece is polished with the polishing pad polishing layer, pressure unevenness can be more effectively prevented from occurring between the contact portion of the polishing layer with the workpiece and the non-contact portion of the polishing layer with the workpiece. The surface of the object to be polished can be sufficiently polished so as to further increase the peripheral flatness of the object to be polished.
[0061] The polishing pad according to the present invention is not limited to the above embodiment. The polishing pad according to the present invention is not limited by the above-mentioned action and effect. Furthermore, the polishing pad according to the present invention can be modified in various ways without departing from the gist of the present invention. EXAMPLES
[0062] The present invention will now be described in more detail with reference to examples and comparative examples. The following examples are provided to further explain the present invention in detail, and are not intended to limit the scope of the present invention.
[0063] Example 1 [Polishing layer] A polishing layer A made of a first polyurethane resin foam was prepared. The thickness of the abrasive layer A was 1.00 mm.
[0064] [Base layer] A first polyurethane film was prepared as the underlayer. In the following, the underlayer according to Example 1 is referred to as underlayer β. The thickness of the underlayer β was 0.07 mm.
[0065] [Polishing pad] The polishing pad of Example 1 was obtained by bonding the polishing layer A and the underlayer β together. The abrasive layer A and the underlayer β were bonded together by obtaining a laminate in which the abrasive layer A and the underlayer β were laminated together, and then pressing the laminate in the thickness direction.
[0066] Example 2 [Polishing layer] As in Example 1, abrasive layer A was used.
[0067] [Base layer] As the underlayer, a second polyurethane film different from the first polyurethane film was prepared. In the following, the underlayer according to Example 2 is referred to as underlayer γ. The thickness of the underlayer γ was 0.07 mm.
[0068] [Polishing pad] In the same manner as in Example 1, the polishing layer A and the underlayer γ were bonded together to obtain a polishing pad according to Example 2.
[0069] Comparative Example 1 As in Example 1, a polishing pad according to Comparative Example 1 was obtained using a polishing layer A as the polishing layer, without using an underlayer. That is, the polishing pad according to Comparative Example 1 was provided with the polishing layer A only.
[0070] Comparative Example 2 [Polishing layer] A polishing layer B composed of a second polyurethane resin foam different from the first polyurethane resin foam was prepared. The thickness of the abrasive layer B was 1.00 mm.
[0071] [Base layer] As the underlayer, a polishing pad (manufactured by Nitta DuPont under the trade name "SUBA (registered trademark) 400") made by impregnating a nonwoven fabric with a resin was prepared. In the following, the underlayer according to Comparative Example 2 is referred to as underlayer α. The thickness of the underlayer α was 1.30 mm.
[0072] [Polishing pad] In the same manner as in Example 1, the polishing layer B and the underlayer α were bonded together to obtain a polishing pad according to Comparative Example 2.
[0073] The configuration of the polishing pad for each example is shown in Table 1 below.
[0074] [Table 1]
[0075] (5% modulus) For the polishing pads according to each example, the 5% modulus value M of the polishing layer P , and the 5% modulus value M of the base layer L was measured. The 5% modulus value M of the abrasive layer P , and the 5% modulus value M of the base layer L was measured according to the method previously described. The measurement results are shown in Table 1 above. In addition, for the polishing pads according to each example, the 5% modulus value M L The 5% modulus value M of the polishing layer P Ratio (M P / M L The results of the calculations are also shown in Table 1 above.
[0076] (Compression displacement) The amount of compression displacement after repeated compression was measured for the polishing pads of each example. Repeated compression is performed on an area of 1 cm 2 The experiment was carried out using a circular plate. Specifically, the repeated compression was performed under a condition of a frequency of 1.0 Hz, with the load applied by the circular plate fluctuating between 10 gf and 200 gf. The amount of compression displacement was determined by measuring the amount of change in thickness of the polishing pad after 2000 repeated compressions relative to the thickness of the polishing pad before the repeated compressions. The results are shown in Table 1 above.
[0077] (Polishing test) Using the polishing pad according to each example, polishing of an object to be polished was carried out under the polishing conditions described below. Polished object: Etched wafer (thickness approx. 790μm) ·Polishing machine: DSM 20B-5P-4D (manufactured by Speed FAM) Slurry type: Nanopure® NP6610 (contains colloidal silica as abrasive grains. Manufactured by Nitta DuPont) Slurry flow rate: 5L / min Evaluation machine: Nanometro 300TT-A The "etched wafer" to be polished had a disk shape.
[0078] In the polishing test, the evaluation machine was used to measure the peripheral flatness when the workpiece was polished using the polishing pad of each example. Specifically, the measurement of the peripheral flatness was carried out by calculating the PV value (Peak to Valley) for the average data string of the radial data strings in a specified range on the peripheral portion of the workpiece. The PV value was calculated for the best-fit data sequence within the analysis range of the target radial data sequence. The results are shown in Table 1 above. In Table 1 above, the peripheral flatness of Example 1 is set to 1.00, and for Example 2, Comparative Example 1, and Comparative Example 2, the relative values to the peripheral flatness of Example 1 are shown. That is, for Example 2, Comparative Example 1, and Comparative Example 2, the greater the peripheral flatness value is from 1.00, the more inferior the peripheral flatness becomes.
[0079] From Table 1, it can be seen that when a workpiece is polished using the polishing pad according to each example, the workpiece exhibits a small peripheral flatness value. In other words, it can be seen that the peripheral flatness is sufficiently increased. In contrast, when the polishing pads according to the comparative examples are used to polish an object, the object exhibits a large peripheral flatness, which indicates that the peripheral flatness is not sufficiently improved. From this result, the 5% modulus value M L The 5% modulus value M of the polishing layer P Ratio (M P / M L It can be seen that by making the ratio of the surface roughness to the surface roughness of the workpiece to be polished 5 or more, the peripheral flatness of the workpiece can be sufficiently improved. [Explanation of symbols]
[0080] 1 abrasive layer, 2 undercoat layer, 3 adhesive layer, 10 abrasive pad, 20 object to be polished, 100 platen, 200 head, 300 slurry supply unit, 1000 polishing machine, 10a polished surface, 20a polished surface, 200a holding material.
Claims
1. A polishing layer having a polishing surface and a base layer laminated on the polishing layer on the surface opposite to the polishing surface, the polishing surface is formed of a surface of a polyurethane resin foam containing a polyurethane resin, The 5% modulus value M of the underlayer L The 5% modulus value M of the polishing layer P The ratio (M P / M L ) is 5 or more Polishing pad.
2. The 5% modulus value M of the underlayer L is 1 MPa or less 2. The polishing pad of claim 1.
Citation Information
Patent Citations
Manufacturing method of glass substrate for magnetic disk
JP2007250166A
Polishing pad
JP2010274361A
Cited By
Polishing pad
JP2026108972A