Packaging material

A laminate structure with a paper base and sealant layer, devoid of polyethylene resin, addresses sealing and tearing issues in packaging materials, ensuring high adhesive strength and clean peeling.

JP2024134140APending Publication Date: 2024-10-03TOYO ALUMINIUM KK
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023044272
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-20
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional packaging materials face issues with poor sealing performance and unintended tearing due to reduced resin content, leading to pinholes and difficulty in opening, especially when polyethylene resin is omitted from the adhesive layer.

Method used

A laminate structure comprising a paper base material with a basis weight of 40-120 g/m² and a sealant layer with a softening point of 69-75°C, devoid of a polyethylene resin layer, and optionally incorporating a primer layer of acrylic, vinyl chloride-vinyl acetate copolymer, or polyester resin, enhances adhesive strength and prevents unintended tearing.

Benefits of technology

The packaging material maintains high adhesive strength and prevents unintended tearing, ensuring clean peeling without resin fusion during heat sealing, thus promoting environmental friendliness and productivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134140000001_ABST
    Figure 2024134140000001_ABST
Patent Text Reader

Abstract

To provide a packaging material with reduced paper base material tear and high adhesive strength even without a resin layer for adhesion made of polyethylene resin between the paper base material and the sealant layer.SOLUTION: The packaging material includes: a laminate including a paper base material 11 and a sealant layer 12, characterized in that: (1) paper has a loading capacity of 40 to 120 g / m2; (2) the sealant layer 12 contains a resin component having sealant properties and a softening point of 69 to 75°C; and (3) no polyethylene resin-contained layer is interposed between the paper base material 11 and the sealant layer 12.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a novel packaging material. More specifically, the present invention relates to a packaging material having sealability.

Background Art

[0002] Conventionally, packaging materials used for foods, pharmaceuticals, etc. have been required to consider the environment, and measures such as reducing the amount of resin and using paper instead have been taken. However, when forming a three-dimensional package (such as a packaging bag or container) from a packaging material by heat sealing, if the amount of resin is reduced, pinholes and the like are likely to occur, resulting in a problem that the performance such as the sealing property required for the packaging material deteriorates.

[0003] Therefore, studies have been made to reduce the amount of resin while also reducing pinholes and attempting to reduce the environmental impact of the packaging material. For example, a paper laminated sheet including a paper base material layer, an anchor coat layer, an adhesive resin layer made of a polyolefin resin, and a sealant layer made of a polyolefin resin in this order, where the weight of the paper base material layer is X g / m 2 , and the weight of the entire paper laminated sheet is Y g / m 2 , a paper laminated sheet characterized by Y / 2 < X < 120 has been proposed (Patent Document 1).

[0004] In a packaging material such as the prior art, an adhesive resin layer is formed between the paper base material and the sealant layer. As the adhesive resin layer, a polyethylene resin or the like is generally used. Without such an adhesive resin layer, the paper base material cannot be imparted with strength, and problems such as the paper base material being torn accidentally and the contents being exposed, or the paper base material being torn irregularly when opening and unable to be opened properly may occur.

Prior Art Documents

Patent Documents

[0005]

Patent Document 1

[0006] However, as in Patent Document 1, in a layer structure in which a sealant layer is formed on an adhesive resin layer of a polyethylene resin, the packaging material is designed to be opened by cohesive peeling at the sealant layer when it is opened. However, if the polyethylene resin adhesive layer reaches the container side during heat sealing, the polyethylene and the container will fuse together, making it difficult to open the packaging material with fingers.

[0007] On the other hand, a method of eliminating the adhesive resin layer of polyethylene resin is also conceivable, but simply eliminating the adhesive resin layer of polyethylene resin reduces the strength of the entire packaging material, and there is a risk that the paper base material will tear when opening, etc., and that the package will open in an unintended manner. As another method, there is a method of providing a release layer or the like to facilitate peeling of the paper base material and the sealant layer in order to prevent tearing of the paper base material, but in that case, the adhesive strength between the paper base material and the sealant layer will be reduced, and as a result, there is a risk that the package will be opened unintendedly.

[0008] Therefore, the main object of the present invention is to provide a packaging material that reduces tearing of the paper base material and has high adhesive strength, even when there is no adhesive resin layer made of a polyethylene-based resin between the paper base material and the sealant layer. [Means for solving the problem]

[0009] Means of the Invention The present inventors have conducted extensive research in light of the problems in the prior art and have found that the above object can be achieved by a laminate having a specific composition and structure, thereby completing the present invention.

[0010] That is, the present invention relates to the following packaging material. 1. A laminate comprising a paper substrate and a sealant layer, (1) The paper has a basis weight of 40 to 120 g / m 2 and (2) The sealant layer contains a resin component having a sealant property and has a softening point of 69 to 75° C., (3) There is no polyethylene resin-containing layer between the paper base material and the sealant layer. A packaging material characterized by: 2. The packaging material according to item 1, further comprising a primer layer between the paper substrate and the sealant layer, the primer layer containing at least one of an acrylic resin, a vinyl chloride-vinyl acetate copolymer resin, and a polyester resin. 3. The paper has a density of 0.8 to 1.0 g / cm 3 2. The packaging material according to claim 1, which is a high-density paper. 4. A package or container comprising the packaging material according to any one of items 1 to 3. Effect of the Invention

[0011] According to the present invention, it is possible to provide a packaging material that reduces tearing of the paper base material and has high adhesive strength, even if there is no adhesive resin layer made of a polyethylene-based resin between the paper base material and the sealant layer.

[0012] Therefore, in a package or container using the packaging material of the present invention, the paper base material is not easily torn before opening and can maintain high adhesive strength, so that the phenomenon of the package or container tearing unintentionally can be reduced. Furthermore, when opening, the paper base material itself is not easily torn, so that the phenomenon of unintentional opening or irregular opening can be avoided.

[0013] In particular, in the present invention, when a specific primer layer is formed between the paper substrate and the sealant layer, the peeling interface can be peeled off in a state where it is between the primer layer and the sealant layer when opening. This makes it difficult for the paper to tear when opening (when peeling off the packaging material), and as a result, it is possible to prevent the paper from tearing in an unexpected way, and it is possible to open or peel off the packaging material with fingers as designed. In addition, even if the composition is a paper substrate other than a paper substrate containing metal foil (for example, paper / PET film, etc.), it is possible to obtain the same good adhesion, peelability, etc. by selecting the type of primer.

[0014] Furthermore, in the packaging material of the present invention, since it is not necessary to form an adhesive resin layer of a polyethylene resin between the base layer and the sealant layer, it is possible to reduce the amount of polyethylene resin used, which makes it possible to provide a high-quality environmentally friendly product. In addition, since the extrusion process of the polyethylene resin, which was previously required, can be omitted, it is also advantageous in terms of productivity and economy. [Brief description of the drawings]

[0015] [Figure 1] FIG. 2 is a diagram showing an example of a layer structure of the packaging material of the present invention. [Diagram 2] FIG. 2 is a diagram showing another example of the layer structure of the packaging material of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] 1. Packaging material The packaging material of the present invention is a laminate including a paper base material including paper and a sealant layer, (1) The paper has a basis weight of 40 to 120 g / m 2 and (2) The sealant layer contains a resin component having a sealant property and has a softening point of 69 to 75° C., (3) There is no polyethylene resin-containing layer between the paper base material and the sealant layer. It is characterized by:

[0017] An example of the basic layer structure of the packaging material of the present invention is shown in Figure 1. The packaging material 10 of the present invention has a structure in which a sealant layer 12 is laminated on a paper base material 11 containing paper. Usually, the sealant layer 12 is a layer that is joined by heat sealing (HS) or the like in a state of contact with a container 20, as shown in Figure 1, for example. Therefore, in the present invention, it is usually preferable that the sealant layer is disposed as the outermost layer of the packaging material of the present invention. The sealant layer may be formed on the entire surface of the paper base material, or on only a part of it.

[0018] In addition, as shown in Fig. 1, the packaging material of the present invention does not have a polyethylene resin-containing layer between the paper substrate 11 and the sealant layer 12, which is used in conventional packaging materials. This makes it possible to effectively avoid the problem of peeling that occurs in conventional packaging materials.

[0019] In FIG. 1, the paper substrate 11 and the sealant layer 12 are laminated so as to be in direct contact with each other, but they may be laminated with other layers interposed therebetween. However, no polyethylene resin-containing layer is included between the paper substrate and the sealant layer. For example, in the packaging material 10' shown in FIG. 2A, a primer layer PR is formed between the paper substrate 11 and the sealant layer 12. In this case, the sealant layer 12 may be formed on the entire surface of the primer layer PR material, or may be formed on a part of it. Furthermore, as in the packaging material 10" shown in FIG. 2B, other layers (e.g., a printing layer, an overcoat layer, a surface protection layer, etc.) may be laminated on the surface opposite to the side where the paper substrate 11 contacts the primer layer PR. In particular, in the present invention, as shown in the packaging material 10' or the packaging material 10", a laminate including at least a paper substrate / primer layer / sealant layer configuration is preferable. These layers are preferably laminated in a state of direct contact with each other. This makes it possible to obtain high adhesive strength and good peelability. Therefore, for example, as shown in Fig. 1, after the packaging material is joined to a container, the packaging material can be peeled off cleanly from the container or the like while maintaining a desired sealability, without any trouble such as the packaging material being torn during peeling. Each layer that can constitute the packaging material of the present invention will be described below.

[0020] a) Paper base material The paper substrate functions as a support layer of the packaging material of the present invention and plays a role in imparting rigidity, etc. to the laminate. The paper substrate may be either a single layer or multiple layers as long as at least one layer contains paper.

[0021] When the paper base material is a multi-layer, the material other than paper is not particularly limited, and may be, for example, one or more layers composed of at least one of metal foil, metal vapor deposition film (resin film vapor-deposited with metal components), resin film, etc. Examples of the metal component of the metal foil or metal vapor deposition film include aluminum, iron, copper, etc., and alloys containing these. Examples of the resin component of the resin film, etc. include polyester resin films such as polyethylene terephthalate (PET), olefin resin films such as polypropylene and polyethylene, etc.

[0022] In particular, in the present invention, it is preferable to use a paper base material in which one or more layers of aluminum foil or aluminum vapor deposition film are laminated on paper. This makes it possible to obtain higher barrier properties against, for example, light, oxygen, moisture, etc. In addition, when the paper base material is a laminate of multiple materials, an adhesive layer may be provided between the materials. Therefore, for example, "paper / adhesive layer / aluminum foil", "paper / adhesive layer / metal vapor deposition film", "aluminum foil / adhesive layer / paper / adhesive layer / aluminum foil", "metal vapor deposition film / adhesive layer / paper / adhesive layer / metal vapor deposition film" and the like can be suitably adopted as a multi-layer paper base material.

[0023] In addition, a paper base material having any layer such as an OP layer (overprint layer, print protection layer, surface protection layer) or a print layer laminated on the side opposite to the sealant layer can also be used.

[0024] The paper substrate may be subjected to a surface treatment such as plasma treatment at least on the surface on the sealant layer side. This can further increase the adhesion (adhesion) between the substrate and the sealant layer. In addition, the paper substrate or the sealant layer surface may be subjected to a treatment such as unevenness treatment using an additive (preferably filler particles) or unevenness treatment by embossing. The height of such unevenness is not limited, but is preferably about 5 to 60 μm, more preferably 20 to 50 μm. This can suppress adhesion to contents when used as a packaging material.

[0025] The weight of the paper in the paper base material is usually 40 to 120 g / m 2 Approximately 45 to 90 g / m 2 It is preferable that the thickness is 50 to 70 g / m 2 By setting the weight per unit area in this range, it is possible to obtain the necessary adhesive strength when the sealant layers are bonded to each other, to a paper substrate, or to another packaging material while maintaining the strength required for the packaging material.

[0026] The density of the paper is not particularly limited, but is usually 0.6 to 1.0 g / cm 3 It is preferable that the density is about 0.8 to 1.0 g / cm. 3 Such so-called high density paper is particularly preferred in terms of preventing the paper from tearing.

[0027] When the paper base material contains aluminum foil, the thickness of the aluminum foil is preferably in the range of 6 to 20 μm. The composition of the aluminum foil is not particularly limited, and any aluminum foil used as a packaging material can be suitably used. The condition of the aluminum foil is not particularly limited, but it is preferably a soft foil.

[0028] When the paper base material contains an aluminum vapor-deposited film, the thickness of the aluminum vapor-deposited film is usually preferably in the range of 10 nm to 1 μm.

[0029] The thickness (total thickness) of the paper base material is not limited, and can be appropriately set depending on the materials of the layers constituting the paper base material, the application of the laminate of the present invention, etc. Generally, it can be appropriately set within the range of about 9 to 80 μm, but is not limited thereto.

[0030] b) Primer layer In the laminate of the present invention, although the primer layer is not essential, it is preferable to provide a primer layer between the paper substrate and the sealant layer. In the present invention, the primer layer mainly serves to make the sealant layer more easily adhered to the paper substrate. It can also contribute to better peelability.

[0031] The type of primer layer is not particularly limited, and known or commercially available primer components can be used. For example, a primer containing at least one resin component selected from acrylic resin, vinyl chloride-vinyl acetate copolymer resin, and polyester resin can be suitably used. These can be appropriately selected according to the material of the substrate. For example, when the paper substrate is a single piece of paper, it is preferable to use an acrylic resin as a primer. Also, for example, when the paper substrate is provided with a metal foil such as an aluminum foil, it is preferable to use a vinyl chloride-vinyl acetate copolymer resin as a primer. By selecting each of these resin components, it is possible to reduce the tearing of the paper substrate and obtain high adhesive strength.

[0032] The amount of the primer layer formed is not particularly limited, but is preferably 0.1 to 3.0 g / m2 in terms of dry weight. 2 From the viewpoint of adhesive strength, it is preferable to set the thickness to about 0.3 to 0.8 g / m. 2 It can also be about the same.

[0033] The method for forming the primer layer is not limited as long as it can form a layer having the above-mentioned configuration, but usually, a method including a step of applying a coating liquid for forming a primer layer to the surface of a substrate can be suitably adopted.

[0034] As the coating liquid for forming the primer layer, for example, a solution in which the above-mentioned resin component (adhesive resin) is dissolved in a solvent or a dispersion in which the above-mentioned resin component is dispersed in a solvent can be suitably used.

[0035] The solvent is not limited and can be appropriately selected depending on the type of resin component, etc. For example, in addition to water, ethanol, methanol, cyclohexane, toluene, acetone, isopropyl alcohol (IPA), propylene glycol, hexylene glycol, butyl diglycol, pentamethylene glycol, normal pentane, normal hexane, hexyl alcohol, methyl ethyl ketone, methyl acetate, ethyl acetate, butyl acetate, isobutyl acetate, isopropyl acetate, isopentyl acetate, normal butyl acetate, normal propyl acetate, normal pentyl acetate (also known as normal amyl acetate), cyclohexane, isobutyl alcohol, isopropyl alcohol, isopentyl alcohol, ethyl ether, ethylene glycol monoethyl ether, ethylene glycol monoethyl ether acetate, ethylene glycol mono-n-butyl ether, ethylene glycol monomethyl ether, ortho-dichlorobenzene, xylene, cresol, chlorobenzene, cyclohexanol, cyclohexanone, N,N-dimethylformamide, tetrahydrofuran, 1,1,1-trichloroethane, toluene, etc. can be mentioned. These can be used alone or in combination of two or more.

[0036] The solid content concentration of the primer layer-forming coating liquid can be appropriately set in consideration of, for example, coatability, and can be, for example, in the range of about 5 to 60 mass %, but is not limited thereto.

[0037] The method for preparing the primer layer-forming coating liquid is not particularly limited, and the coating liquid can be obtained by adding the resin component and the like to a solvent and mixing them. The order of adding each component is also not particularly limited.

[0038] The method for applying the primer layer-forming coating liquid is not particularly limited, and the primer layer can be applied onto the base layer by a known method such as roll coating, various gravure coatings, a bar coater, a doctor blade coating, a comma coater, a spray coat, or a brush coating.

[0039] Next, the formed coating film can be dried as necessary. The solvent is evaporated by drying, and a primer layer can be formed on the substrate layer. Drying conditions can be appropriately set depending on, for example, the type of solvent, the amount of coating, etc. The temperature can be set in the range of, for example, 50 to 250°C, but is not limited thereto. The drying time can be performed in the range of, for example, 5 seconds to 60 minutes, but is not limited thereto.

[0040] c) Sealant layer In the present invention, the sealant layer is a layer that is primarily heat-sealable. When the sealant layer is formed into a packaging material, it is melted by heating and adheres to itself or to a paper substrate or other packaging material (container), allowing it to be formed into a desired shape.

[0041] The sealant layer is composed of a composition (sealant component) containing a resin component having sealant properties. In the present invention, the softening point of the sealant layer (sealant component) is set to a range of 69 to 75°C. By setting the softening point within such a range, when actually used as a packaging material, the sealant layer has high adhesive strength and a certain degree of flexibility at room temperature, and the paper of the paper substrate can be reduced from breaking. When a resin component having a softening point of less than 69°C is used, heat sealing is difficult, so that it is difficult to use the resin component as a packaging material in the first place. In addition, when the softening point exceeds 75°C, there is a problem that layers other than the sealant layer are easily damaged by high temperatures during heat sealing.

[0042] The softening point can be designed not only by the main component of the resin component, but also by additives. Specifically, the main component of the resin constituting the sealant component is not limited, and can be at least one of ethylene-vinyl acetate copolymer, polyolefin, synthetic rubber, polyurethane, polyamide, etc., for example. Therefore, for example, an ethylene-vinyl acetate copolymer-based hot melt agent can be preferably used. Also, for example, a sealant component containing a polyolefin resin (polyethylene, etc.) and containing wax, a tackifier, an ethylene-vinyl acetate copolymer, etc. as additives can be adopted. In this case, it can be preferably adjusted by the composition and / or the amount of addition of the tackifier (terpene resin). These can also be used as commercially available products.

[0043] The viscosity of the sealant component is not particularly limited, but a melt viscosity at 160°C of about 3 to 6 Pa·s (particularly 3.5 to 5.5 Pa·s) is preferred from the viewpoint of obtaining suitable adhesion to the paper substrate.

[0044] The amount of the sealant layer formed is not particularly limited, but is preferably 5 to 25 g / m2 in terms of dry weight. 2 From the viewpoint of adhesive strength, it is preferable to set the thickness to about 15 to 20 g / m. 2 It can also be about the same.

[0045] The method for forming the sealant layer is not limited as long as it can form a layer having the above-mentioned configuration, but usually a method including a step of applying a sealant liquid to the surface of the paper substrate or the sealant layer can be preferably used.

[0046] As the sealant liquid, for example, a solution in which a resin component having a sealant property is dissolved in a solvent or a dispersion in which a resin component having a sealant property is dispersed in a solvent can be suitably used. In addition, a commercially available sealant agent (such as a hot melt agent) can also be used.

[0047] When a solvent is used, the type thereof is not limited and can be appropriately selected depending on the type of resin component having sealant properties, etc. Examples of the solvent include water, ethanol, methanol, cyclohexane, toluene, acetone, isopropyl alcohol (IPA), propylene glycol, hexylene glycol, butyl diglycol, pentamethylene glycol, normal pentane, normal hexane, hexyl alcohol, methyl ethyl ketone, methyl acetate, ethyl acetate, butyl acetate, isobutyl acetate, isopropyl acetate, isopentyl acetate, normal butyl acetate, normal propyl acetate, normal pentyl acetate (also known as normal amyl acetate), cyclohexane, isobutyl alcohol, isopropyl alcohol, isopentyl alcohol, ethyl ether, ethylene glycol monoethyl ether, ethylene glycol monoethyl ether acetate, ethylene glycol mono-n-butyl ether, ethylene glycol monomethyl ether, ortho-dichlorobenzene, xylene, cresol, chlorobenzene, cyclohexanol, cyclohexanone, N,N-dimethylformamide, tetrahydrofuran, 1,1,1-trichloroethane, toluene, etc. These can be used alone or in combination of two or more.

[0048] The solid content concentration of the sealant liquid can be appropriately set in consideration of, for example, coatability, and can be, for example, in the range of about 5 to 60 mass %, but is not limited thereto.

[0049] The method for preparing the sealant liquid is not particularly limited, and the sealant liquid can be obtained by adding the resin components to a solvent and mixing them. The order of adding each component is also not particularly limited.

[0050] The method for applying the sealant liquid is not particularly limited, and the sealant liquid can be applied onto the paper base layer by known methods such as roll coating, various gravure coatings, bar coater, doctor blade coating, comma coater, spray coating, and brush coating.

[0051] Then, the formed coating film can be dried as necessary. The solvent can be evaporated by drying, and a sealant layer can be formed on the surface of the paper base layer or the primer layer. Drying conditions can be appropriately set depending on, for example, the type of solvent, the amount of coating, etc. The temperature can be set in the range of, for example, 50 to 250°C, but is not limited thereto. The drying time can be performed in the range of, for example, 5 seconds to 60 minutes, but is not limited thereto.

[0052] d) Polyethylene resin-containing layer One of the features of the packaging material of the present invention is that it does not include a polyethylene resin-containing layer formed between the base layer and the sealant layer (heat seal layer) in conventional packaging materials. This makes it possible to reduce the amount of polyethylene resin used, while the disadvantages associated with this reduction (problems with peelability, adhesion, etc.) can be solved by the configuration of the laminate of the present invention.

[0053] 3. Use of the packaging material of the present invention The packaging material of the present invention can be suitably used as a material for forming a package for packaging or containing various products. The packaging material of the present invention can also be suitably used as a material for forming a molded body such as a container as a package. That is, the present invention includes a package or container containing the packaging material of the present invention. More specifically, the package or container can include a package or container in which at least a part or all of the sealant layer in the packaging material is heat sealed, and the packaging material is opened at the heat-sealed part when the packaged item is removed.

[0054] As an embodiment of the packaging material of the present invention, it is preferable to have a layer structure including at least three layers, namely, a paper substrate, a primer layer, and a sealant layer. Examples of the embodiment including these three layers include "OP layer (overprint layer) / printing layer / primer layer / paper substrate / aluminum foil / primer layer / sealant layer", "OP layer / printing layer / primer layer / paper substrate / primer layer / sealant layer", etc. In this way, by adopting a packaging material including the above three layers and arranged so that the sealant layer is the outermost layer, it is possible to obtain higher adhesion between the sealant layers, between the sealant layer and other packaging materials, between the sealant layer and other containers, etc. (particularly heat sealing), and it is possible to obtain good peelability without the paper substrate being torn during peeling off the packaging material (when opening).

[0055] In this way, since the packaging material of the present invention has the sealant layer exposed as the outermost layer, the desired package can be formed by heat sealing the sealant layers together or with the sealant layer of another packaging material. Furthermore, the packaging material of the present invention can be suitably used as a lid material that is a component of a package, so that the contents can be sealed by heat sealing the sealant layer to a container (opening).

[0056] The shape of the package is not particularly limited, and the package can be suitably applied to, for example, a molded package, a strip-shaped side cover, a wrapping paper, a tray, a tube, and various bags. The bag is also not particularly limited in shape, and can be suitably used to, for example, any type of bottom-sealed bag, side-sealed bag, pillow bag, gusset bag, pouch (standing pouch), etc. In addition, the container can be any shape, such as a bottle shape or a cup shape. EXAMPLES

[0057] The features of the present invention will be described in more detail below with reference to examples and comparative examples, although the scope of the present invention is not limited to the examples.

[0058] [Example 1] Commercially available Ryuo coated paper (weight 80g / m 2 A 7 μm thick aluminum foil (1N30, manufactured by Toyo Aluminum Co., Ltd.) of the same size was attached to a paper substrate (A4 size) using a commercially available ester-based adhesive, and then dried to prepare a paper substrate. Next, a commercially available vinyl chloride-vinyl acetate copolymer resin (water-based) was applied as a primer to the aluminum foil side of the paper substrate at a dry weight of 0.5 g / m. 2 A primer layer was formed by coating and drying. In addition, a commercially available ethylene-vinyl acetate copolymer hot melt agent (softening point 72°C, melt viscosity 4.5 Pa s at 160°C) was applied at 20 g / m2 as a sealant layer. 2 was applied to obtain a packaging material.

[0059] [Example 2] The paper was a commercially available high-quality paper (weight 40 g / m 2 A packaging material was obtained in the same manner as in Example 1, except that

[0060] [Example 3] The paper used was commercially available Ryuo coated paper (weight 120 g / m 2 A packaging material was obtained in the same manner as in Example 1, except that

[0061] [Example 4] The paper was a commercially available high-density paper (weight 60 g / m 2 , density 0.80g / cm 3 A packaging material was obtained in the same manner as in Example 1, except that

[0062] [Example 5] A packaging material was obtained in the same manner as in Example 1, except that the hot melt agent had a softening point of 69°C and a melt viscosity of 4.0 at 160°C.

[0063] [Example 6] A packaging material was obtained in the same manner as in Example 1, except that the hot melt agent had a softening point of 75°C and a melt viscosity of 5.0 at 160°C.

[0064] [Example 7] As a primer, a commercially available acrylic resin (containing acetone as a solvent) was used at a dry weight of 0.5 g / m 2 A packaging material was obtained in the same manner as in Example 1, except that a primer layer was formed by coating and drying the mixture so as to form a primer layer.

[0065] [Example 8] The paper base material was a commercially available Ryuo coated paper (weight 80 g / m 2 On one side of the plate, a commercially available vinyl chloride-vinyl acetate copolymer resin (water-based) was applied at a dry weight of 0.5 g / m2 as a primer. 2 After coating and drying, 20 g / m of a commercially available ethylene-vinyl acetate copolymer hot melt agent (softening point 72°C, melt viscosity 4.5 at 160°C) was applied to the formed primer layer. 2 A sealant layer was formed by coating the coating material onto the packaging material.

[0066] [Example 9] The paper base material was a commercially available Ryuo coated paper (weight 80 g / m 2 A commercial acrylic resin was applied as a primer to one side of the plate at a dry weight of 0.5 g / m2. 2 On the formed primer layer, 20 g / m of a commercially available ethylene-vinyl acetate copolymer hot melt agent (softening point 72°C, melt viscosity 4.5 at 160°C) was applied. 2 A sealant layer was formed by coating to obtain a packaging material.

[0067] [Comparative Example 1] A packaging material was obtained in the same manner as in Example 1, except that the hot melt agent had a softening point of 76°C and a melt viscosity of 7.0 at 160°C.

[0068] [Comparative Example 2] The paper used was a commercially available Japanese paper (weight 37 g / m 2 A packaging material was obtained in the same manner as in Example 1, except that

[0069] [Comparative Example 3] The paper was a commercially available OS coated paper (weight 127 g / m 2A packaging material was obtained in the same manner as in Example 1, except that

[0070] [Reference example 1] A packaging material was obtained in the same manner as in Example 1, except that a polyethylene-based resin layer having a thickness of 20 μm was formed between the paper substrate and the sealant layer.

[0071] [Test Example 1] The packaging materials (lid materials) obtained in each of the above Examples and Comparative Examples were each placed in a 71-diameter paper / PE container and heated at 150° C. and 1 kg / cm 2 A seal sample was prepared by heat sealing under the condition of ×1 second. The packaging was then opened by hand by pinching the edge of the material, and the paper base material was rated as "X" if it was torn and severely torn, as "△" if the paper base material was not torn but part of the paper peeled off, and as "O" if the paper base material was not torn at all and no paper peeled off. The results are shown in Table 1.

[0072] [Test Example 2] The adhesive strength between the paper substrate and the sealant layer was measured. Specifically, each packaging material was cut to a width of 15 mm and attached to a commercially available 20 μm thick polyethylene sheet that resembled a PE container at 150 °C and 1 kg / cm 2 A sealed sample was prepared by heat sealing under conditions of 100 x 1 second, and a tensile tester (Shimadzu Corporation, EZ-LX 100N) was used at room temperature (20°C) to peel off a small portion of the paper base from one end of the sheet sample, bend the paper base by 180°, and not bend the polyethylene sheet. The peeling test was performed at a peel speed of 200 mm / min, sample width of 7 mm, and chuck distance of 100 mm, with the interface between the paper base and polyethylene sheet peeling off at 180°. The peel strength (N / 15mm) referred to in this specification is obtained by measuring the peel strength of the above-mentioned strip-shaped sample with a width of 7mm, and converting the value into the peel strength when the sample width is 15mm (15 / 7 times). As a guideline for a sample having a necessary and sufficient adhesive strength and also capable of being peeled off, a peel strength of 0.5N / 15mm or more and less than 2.5N / 15mm was evaluated as "○", and a peel strength of less than 0.5N / 15mm and more than 2.5N / 15mm was evaluated as "×". The results are shown in Table 1.

[0073] [Table 1]

[0074] As is clear from the above results, the packaging material of the present invention, even without an adhesive resin layer made of a polyethylene resin between the paper base material and the sealant layer, has high adhesive strength similar to Reference Example 1, which contains a polyethylene resin layer, and when opened or peeled off, the paper base material is less likely to break, and can be easily peeled off with fingers as designed. At the same time, since there is no adhesive resin layer made of a polyethylene resin, the problem of fusion between the adhesive resin layer and a container, etc., during heat sealing can be avoided in advance.

Claims

1. A laminate comprising a paper substrate and a sealant layer, (1) The paper has a basis weight of 40 to 120 g / m 2 and (2) The sealant layer contains a resin component having a sealant property and has a softening point of 69 to 75° C., (3) No polyethylene resin-containing layer is interposed between the paper base material and the sealant layer. A packaging material characterized by:

2. 2. The packaging material according to claim 1, further comprising a primer layer between the paper substrate and the sealant layer, the primer layer containing at least one of an acrylic resin, a vinyl chloride-vinyl acetate copolymer resin, and a polyester resin.

3. The paper has a density of 0.8 to 1.0 g / cm 3 2. The packaging material according to claim 1, which is a high density paper.

4. A package or container comprising the packaging material according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • Lid material for preventing content adhesion

    JP2012206731A

  • Laminated sheet for lid, lid, and chilled food packaging container

    JP2022134344A

  • Paper-laminated sheet, packaging sheet using the sheet, bag, and method for manufacturing paper-laminated sheet

    JP2022069297A