Manufacturing method of regenerated fine aggregate for concrete, and manufacturing method of ready mixed concrete
By using a treatment agent with microbubble water and iron oxide to swell and remove cement from concrete debris during crushing and grinding, the method addresses the issue of low-quality recycled fine aggregates, producing high-quality aggregates for superior ready-mixed concrete.
Patent Information
- Application Number
- JP2023044552
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-10-03
- Estimated Expiration
- 2043-03-20
AI Technical Summary
Existing methods for producing recycled fine aggregate for concrete often result in low-quality aggregates due to insufficient removal of cement content, particularly in fine aggregates, which affects the properties of ready-mixed concrete, leading to issues such as high water absorption and easy solidification.
A method involving the use of a treatment agent containing microbubble water and iron oxide during the crushing and grinding process to swell and remove cement content from concrete debris, followed by wet grinding to produce high-quality recycled fine aggregate.
The method effectively removes cement content from fine aggregates, resulting in high-quality recycled fine aggregate with improved properties, such as reduced water absorption and stability, which in turn produces high-quality ready-mixed concrete.
Smart Images

Figure 2024134316000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing recycled fine aggregate for concrete, a method for producing ready-mix concrete, recycled fine aggregate for concrete, and ready-mix concrete. [Background technology]
[0002] When structures and buildings that use concrete are demolished, concrete debris is discharged. This discharged concrete debris was sometimes discarded. Furthermore, ready mixed concrete produced at a ready mixed concrete plant is delivered to a construction site by an agitator truck, but if there is any left over at the construction site, it is returned to the ready mixed concrete plant while still loaded on the agitator truck. This type of ready mixed concrete is called returned ready mixed concrete, leftover ready mixed concrete, etc., and was sometimes discarded. On the other hand, rather than being discarded, this concrete debris, returned ready mixed concrete, and leftover ready mixed concrete were sometimes crushed and used as road surface material for paving purposes, with the aim of effectively reusing resources and reducing the volume of waste.
[0003] In order to reuse resources more effectively, concrete rubble, returned ready mixed concrete, and residual ready mixed concrete are being sought for reuse in applications other than as pavement surface materials.
[0004] As a method for reusing concrete debris, returned ready mixed concrete, and leftover ready mixed concrete, attention has been focused on reusing them as recycled aggregate for concrete. Examples of a method for producing recycled aggregate for concrete from concrete debris, returned ready mixed concrete, and leftover ready mixed concrete include the methods described in Patent Documents 1 to 3.
[0005] Patent Document 1 describes a process for crushing a raw material made of concrete debris into particles of a predetermined particle size or smaller; a first classification process for classifying the raw material crushed in the crushing process into small diameter components of a first standard particle size or smaller and large diameter components of a first standard particle size or larger; a grinding process for supplying the large diameter components and small diameter components classified in the first classification process to a grinding machine having no grinding media in a ratio such that the volume of the large diameter components is equal to or larger than the volume of the small diameter components, and grinding them together in the grinding machine; The method includes a second classification step of classifying the aggregate into small diameter components having a second standard particle size or less, which are smaller than the first standard particle size, and large diameter components having a second standard particle size or more, and a reprocessing step of supplying both the large diameter components and the small diameter components classified in the second classification step to the grinder and sequentially carrying out the grinding step and the second classification step, and after carrying out the reprocessing step at least once, recovering the large diameter components and the small diameter components classified in the second classification step in the final reprocessing step as recycled aggregate. Patent Document 1 discloses that a high quality recycled aggregate can be produced.
[0006] Patent Document 2 describes a method for producing aggregate from returned concrete, which includes the steps of: charging returned concrete into a high-intensity mixer; adding an organic or inorganic coagulant mixture, either alone or in combination; mixing the returned concrete for 20 seconds to 5 minutes until the returned concrete is set to a substantially dry, cement paste-free, larger particle size fraction consisting mainly of the original natural aggregate contained in the returned concrete, and a smaller particle size fraction consisting mainly of agglomerates containing water, coagulant mixture, fresh cement, and fine fractions of the mixture (sand and silt); and separating the mixture through a vibrating, rotating, or cyclone sieve to separate it into at least two particle size classes, one of which is a substantially dry, cement paste-free, larger particle size fraction consisting mainly of the original natural aggregate contained in the returned concrete, and one of which is a smaller particle size fraction consisting mainly of agglomerates containing water, coagulant mixture, fresh cement, and fine fractions of the mixture (sand and silt). According to US Pat. No. 5,399,436, aggregates can be produced from concrete residues not used for construction purposes or, more generally, from cement mixtures that are not used for any reason and are returned to the production facility in the mixer truck.
[0007] Patent Document 3 describes a method for producing recycled fine aggregate, which is characterized in that coarsely crushed raw concrete chunks such as concrete waste are first treated in a screw grinding processing device, and the raw fine aggregate obtained by the treatment, which has a particle size of 10 mm or less and has hardened cement attached to its surface, is further lightly treated in a rotary drum grinder to such an extent that the hardened cement attached to the surface does not leave unevenness or voids that would cause strength defects. Patent Document 3 discloses that a recycled fine aggregate can be obtained that can give a cement-based hardened body that exhibits strength development almost equal to or greater than that when the raw fine aggregate is mixed. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] International Publication No. 2013 / 114526 [Patent Document 2] Special Publication No. 2020-528858 [Patent Document 3] JP 2009-40655 A Summary of the Invention [Problem to be solved by the invention]
[0009] Recycled concrete aggregates produced from concrete rubble, returned ready-mix concrete, and residual ready-mix concrete have sometimes been of low quality. Specifically, recycled concrete aggregates contain residual cement (cement paste) derived from concrete rubble, etc., and tend to have a higher water absorption capacity than ordinary aggregates. The high water absorption capacity of recycled concrete aggregates can adversely affect the properties of ready-mix concrete produced using the recycled concrete aggregates. In addition, when recycled concrete aggregates are stored in silos, etc., they tend to harden. This affects the operating conditions, etc., when ready-mix concrete is produced using the recycled concrete aggregates. These effects are more pronounced in recycled fine aggregates than in recycled coarse aggregates.
[0010] For these reasons, even recycled aggregates for concrete manufactured from concrete debris are required to have higher quality. Specifically, examples of recycled aggregates for concrete include recycled aggregates for concrete H, recycled aggregates for concrete M, and recycled aggregates for concrete L, and among these, a manufacturing method for obtaining recycled aggregates for concrete H is required. The recycled aggregates for concrete H are specified in JIS A 5021:2018, and are recycled aggregates for concrete manufactured by subjecting concrete blocks generated by the demolition of structures to advanced processing such as crushing, grinding, and classification. The recycled aggregates for concrete M are specified in JIS A 5022:2018, and can be handled in a manner similar to that of ordinary aggregates, and are high-quality aggregates that can be used regardless of the part of a building. In addition, recycled aggregates for concrete manufactured from returned ready mixed concrete and residual ready mixed concrete are also required to have higher quality, as are recycled aggregates for concrete manufactured from concrete debris. For these reasons, there is a demand for a production method capable of obtaining high-quality recycled aggregate for concrete, such as the recycled aggregate for concrete H, from concrete rubble, returned ready mixed concrete, and residual ready mixed concrete.
[0011] However, the current situation is that a manufacturing method capable of obtaining a sufficiently high-quality recycled aggregate for concrete from concrete debris and the like has not been established. Specifically, the current situation is that a manufacturing method capable of producing recycled aggregate H for concrete from concrete debris and the like has not been established. For example, in the invention described in Patent Document 1, since the crushing or grinding is performed in a dry manner, the obtained recycled aggregate may have insufficient (incomplete) peeling of the cement content (cement paste) contained in the concrete debris. Also, in the method described in Patent Document 2, there are cases where the problem is not sufficiently solved due to the remaining cement content (cement paste) contained in the returned concrete in the aggregate (recycled aggregate) obtained from the returned concrete. In particular, among recycled aggregates, recycled fine aggregate is more difficult to remove the cement content than when producing recycled coarse aggregate, and it is more difficult to obtain a high-quality recycled fine aggregate. For this reason, a manufacturing method capable of obtaining a high-quality recycled fine aggregate for concrete is required.
[0012] The present invention has been made in consideration of the above circumstances, and aims to provide a method for producing recycled fine aggregate for concrete that can produce high-quality recycled fine aggregate for concrete, and high-quality recycled fine aggregate for concrete. Another aim of the present invention is to provide a method for producing ready-mixed concrete that can produce high-quality ready-mixed concrete, and high-quality ready-mixed concrete. [Means for solving the problem]
[0013] As a result of various investigations, the present inventors have found that the above object can be achieved by the present invention described below.
[0014] The first aspect of the present invention relates to a method for producing recycled fine aggregate for concrete, which includes a step of crushing concrete debris, a step of adding a treating agent containing microbubble water and iron oxide to the crushed material obtained by crushing the concrete debris, and a step of grinding the crushed material to which the treating agent has been added.
[0015] According to this configuration, a method for producing recycled fine aggregate for concrete that can produce high-quality recycled fine aggregate for concrete can be provided. Specifically, in the method, crushed concrete debris obtained by crushing the concrete debris is ground together with a treatment agent containing microbubble water and iron oxide. As a result, even if the cement content is difficult to remove from fine aggregate, it is considered that the cement content can be suitably removed. Specifically, it is considered that the cement content in the crushed material (for example, the cement content of cement paste derived from concrete debris, etc.) is swollen by the treatment agent. Then, it is considered that the swollen cement content can be suitably removed from the crushed material by grinding the crushed material together with the treatment agent without the crushed material being over-ground. Therefore, even if the cement content is difficult to remove from fine aggregate, it is considered that the cement content can be suitably removed while suppressing excessive grinding. By doing so, a high-quality recycled fine aggregate for concrete from which the cement content has been suitably removed can be obtained.
[0016] A second aspect of the method for producing recycled fine aggregate for concrete is the method for producing recycled fine aggregate for concrete according to the first aspect, wherein the grinding is wet grinding.
[0017] According to this configuration, a higher quality recycled fine aggregate for concrete can be obtained. This is believed to be because the crushed material is wet-grinded to more suitably remove cement from the crushed material.
[0018] The third aspect of the manufacturing method for recycled fine aggregate for concrete is the method for manufacturing recycled fine aggregate for concrete according to the first or second aspect, wherein the amount of the treatment agent added in the adding step is 0.05 to 30 volume % with respect to the crushed material.
[0019] According to this configuration, a higher quality recycled fine aggregate for concrete can be obtained, which is believed to be because the cement content is more suitably removed from the crushed material by the grinding.
[0020] A method for producing recycled fine aggregate for concrete according to a fourth aspect is a method for producing recycled fine aggregate for concrete according to any one of the first to third aspects, wherein the amount of the treatment agent added in the adding step is 1 / m of the crushed material. 3 This is a method for producing recycled fine aggregate for concrete, which is 1 to 300 kg per unit weight.
[0021] According to this configuration, a higher quality recycled fine aggregate for concrete can be obtained, which is believed to be because the cement content is more suitably removed from the crushed material by the grinding.
[0022] The fifth aspect of the method for producing recycled fine aggregate for concrete is a method for producing recycled fine aggregate for concrete according to any one of the first to fourth aspects, in which at least one of the adding step and the grinding step is carried out two or more times.
[0023] According to this configuration, by performing at least one of the adding step and the grinding step two or more times, a higher quality recycled fine aggregate for concrete can be obtained from which the cement content has been further removed.
[0024] The sixth aspect of the method for producing recycled fine aggregate for concrete includes an adding step of adding a treating agent containing microbubble water and iron oxide to a hardened material derived from returned fresh concrete or residual fresh concrete, and a grinding step of grinding the crushed material to which the treating agent has been added.
[0025] According to this configuration, a method for producing recycled fine aggregate for concrete that can produce high-quality recycled fine aggregate for concrete can be provided. Specifically, in the method, a hardened material derived from returned fresh concrete or residual fresh concrete is ground together with a treatment agent containing microbubble water and iron oxide. As a result, even if the fine aggregate has a tendency to have a cement content that is difficult to remove, the cement content is thought to be suitably removed. Specifically, the cement content in the hardened material (for example, the cement content contained in the returned fresh concrete, the cement content contained in the residual fresh concrete, and the cement content of the cement paste derived from the hardened material, etc.) is thought to be swollen by the treatment agent. Then, by grinding the hardened material together with the treatment agent, the hardened material is thought to be not ground too much, and the swollen cement content is thought to be suitably removed from the hardened material. Therefore, even if the fine aggregate has a tendency to have a cement content that is difficult to remove, the cement content is thought to be suitably removed while suppressing excessive grinding. By doing so, a high-quality recycled fine aggregate for concrete from which the cement content has been suitably removed can be obtained.
[0026] A seventh aspect of the method for producing recycled fine aggregate for concrete is the method for producing recycled fine aggregate for concrete according to the sixth aspect, wherein the grinding is wet grinding.
[0027] According to this configuration, a higher quality recycled fine aggregate for concrete can be obtained. This is believed to be because the cement content is more suitably removed from the hardened material by subjecting the hardened material to wet grinding.
[0028] The eighth aspect of the method for producing recycled fine aggregate for concrete is the method for producing recycled fine aggregate for concrete according to the sixth or seventh aspect, wherein the amount of the treatment agent added in the adding step is 0.05 to 30 volume % with respect to the hardened product.
[0029] According to this configuration, a higher quality recycled fine aggregate for concrete can be obtained, which is believed to be because the cement content is more suitably removed from the hardened material by the grinding.
[0030] A ninth aspect of the present invention relates to a method for producing recycled fine aggregate for concrete, and in the method for producing recycled fine aggregate for concrete according to any one of the sixth to eighth aspects, the amount of the treatment agent added in the addition step is 1 / m of the hardened material. 3 This is a method for producing recycled fine aggregate for concrete, which is 1 to 300 kg per unit weight.
[0031] According to this configuration, a higher quality recycled fine aggregate for concrete can be obtained, which is believed to be because the cement content is more suitably removed from the hardened material by the grinding.
[0032] The tenth aspect of the method for producing recycled fine aggregate for concrete is a method for producing recycled fine aggregate for concrete according to any one of the sixth to ninth aspects, in which at least one of the adding step and the grinding step is carried out two or more times.
[0033] According to this configuration, by performing at least one of the adding step and the grinding step two or more times, a higher quality recycled fine aggregate for concrete can be obtained from which the cement content has been further removed.
[0034] The method for producing ready-mix concrete according to the 11th aspect includes a step of mixing cement, aggregate, and water, and uses, as the aggregate, aggregate containing recycled fine aggregate for concrete produced by the method for producing recycled fine aggregate for concrete according to any one of the first to tenth aspects.
[0035] According to this configuration, it is possible to provide a method for producing ready-mixed concrete that can produce high-quality ready-mixed concrete. Specifically, by using as aggregate an aggregate containing recycled fine aggregate for concrete produced by the method for producing recycled fine aggregate for concrete according to any one of the first to tenth aspects, it is possible to produce high-quality ready-mixed concrete.
[0036] The recycled fine aggregate for concrete according to the twelfth aspect has an oven-dry density of 1.5 g / cm 3 The recycled fine aggregate for concrete has a water absorption rate of 7% or less, and when the color tone is expressed by the Lab system, the a value is 0 to 3 and the b value is 5 to 15.
[0037] According to this configuration, it is possible to provide high-quality recycled fine aggregate for concrete.
[0038] A thirteenth aspect of the present invention relates to a recycled fine aggregate for concrete, which is the recycled fine aggregate for concrete according to the eighth aspect of the present invention, and which has an angle of repose of 45° or less.
[0039] According to this configuration, it is possible to provide a higher quality recycled fine aggregate for concrete.
[0040] The ready mixed concrete according to the fourteenth aspect is ready mixed concrete containing the recycled fine aggregate for concrete according to the twelfth or thirteenth aspect, cement, and water.
[0041] According to this configuration, it is possible to provide high-quality ready-mix concrete. Specifically, by using the recycled fine aggregate for concrete according to the twelfth or thirteenth aspect as an aggregate, high-quality ready-mix concrete can be obtained. Effect of the Invention
[0042] According to the present invention, it is possible to provide a method for producing recycled fine aggregate for concrete, which can produce high-quality recycled fine aggregate for concrete, and high-quality recycled fine aggregate for concrete. Another object of the present invention is to provide a method for producing ready-mixed concrete, which can produce excellent ready-mixed concrete, and excellent ready-mixed concrete. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0043] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to these.
[0044] [Method of manufacturing recycled fine aggregate for concrete] The method for producing recycled fine aggregate for concrete according to one embodiment of the present invention includes a step of crushing concrete debris (crushing step), an addition step of adding a treatment agent containing microbubble water and iron oxide to the crushed material obtained by crushing the concrete debris, and a grinding step of grinding the crushed material to which the treatment agent has been added.
[0045] The concrete rubble is, for example, concrete-containing debris. Examples of the concrete rubble include concrete rubble discharged when structures and buildings using concrete are demolished, raw materials such as concrete blocks generated with the demolition of concrete structures (buildings, etc.), and concrete debris generated with the construction, reconstruction, or removal of structures. Examples of the concrete rubble to be subjected to the crushing step include concrete rubble that has passed an acceptance inspection. The concrete rubble may be stored in a hopper, and the concrete rubble stored in the hopper may be supplied to the crushing step.
[0046] As described above, the manufacturing method includes a step of crushing the concrete rubble (crushing step). The crushing method in the crushing step is not particularly limited as long as it can crush the concrete rubble, and examples thereof include a method of crushing the concrete rubble with a crusher. The crusher is not particularly limited, and a general concrete crusher can be used. Examples of the crusher include a jaw crusher, an impact crusher, a hammer crusher, a roll crusher, and a rotary crusher, and an impact crusher is preferably used. Examples of the impact crusher include a Haldpact.
[0047] In the crushing step, the crushing may be followed by classification. The crushing conditions are not particularly limited as long as the crushed material has a particle size within the above range. For example, the crushing time is preferably 30 seconds to 24 hours. The classification may be performed by classifying the crushed material with a classifier. The classifier may be built into the crusher. The classifier is not particularly limited, and a general classifier may be used. For example, a sieve classifier such as a vibrating sieve classifier and an in-plane motion sieve classifier, a gravity classifier, an inertia force classifier, a centrifugal classifier such as a cyclone, and a centrifugal classifier with a rotating blade such as a cyclone air separator may be used. For the classification, a method of classifying the crushed material with a vibrating sieve classifier is preferred. If the concrete debris contains reinforcing bars, the reinforcing bars are removed during the crushing and classification. The removed reinforcing bars are stored, for example, in a reinforcing bar storage area.
[0048] In the adding step, a treatment agent containing microbubble water and iron oxide is added to the crushed material obtained by crushing the concrete debris. The method of adding the treatment agent to the crushed material is not particularly limited as long as the crushed material and the treatment agent come into contact with each other, and examples of the method include a method of immersing the crushed material in the treatment agent and a method of applying the treatment agent to the crushed material. Examples of the method of applying the treatment agent to the crushed material include a method of spraying the treatment agent on the crushed material and a method of sprinkling (dispersing) the treatment agent on the crushed material.
[0049] When the crushed material is immersed in the treatment agent, the immersion time is not particularly limited as long as the treatment agent can sufficiently contact the crushed material, and is preferably, for example, 30 seconds to 24 hours, and more preferably, 5 minutes to 2 hours. The temperature of the treatment agent in which the crushed material is immersed is not particularly limited, and is preferably, for example, 0 to 50°C, and more preferably, 5 to 35°C, and may be, for example, room temperature.
[0050] When the treatment agent is sprayed on the crushed material, the spraying time is not particularly limited as long as the treatment agent can be sufficiently contacted with the crushed material, and is preferably 30 seconds to 24 hours, and more preferably 5 minutes to 2 hours. When the treatment agent is sprinkled (dispersed) on the crushed material, the number of times of spraying is not particularly limited as long as the treatment agent can be sufficiently contacted with the crushed material, and is preferably 2 times or more, more preferably 2 to 5 times, and even more preferably 2 to 4 times. The spraying may be performed using, for example, a spiral water washer, a spiral cleaning machine, and a spiral classifier. When the treatment agent is sprayed on the crushed material, the temperature of the treatment agent is not particularly limited, and is preferably 0 to 50°C, and more preferably 5 to 35°C, and may be, for example, room temperature.
[0051] The amount of the treatment agent added in the addition step is not particularly limited as long as the treatment agent can be sufficiently brought into contact with the crushed material. The amount of the treatment agent added is, for example, preferably 0.05 to 30% by volume, more preferably 1 to 20% by volume, and even more preferably 3 to 10% by volume, relative to the crushed material. The amount of the treatment agent added is particularly suitable when the addition step is carried out on a batch scale, such as by immersing the crushed material in the treatment agent. The amount of the treatment agent added is, for example, 0.05 to 30% by volume, relative to the crushed material, more preferably 1 to 20% by volume, and even more preferably 3 to 10% by volume. 3 The amount is preferably 1 to 300 kg, more preferably 5 to 100 kg. The amount of addition is particularly suitable when the addition step is performed as a continuous step, such as by applying the treatment agent to the crushed material. If the amount of addition is too small, the quality of the finally obtained recycled fine aggregate for concrete tends not to be sufficiently improved. This is considered to be because the cement content in the crushed material (for example, the cement content of cement paste derived from concrete debris, etc.) is not sufficiently swollen by the treatment agent, and the cement content is difficult to be suitably removed from the crushed material even if the crushed material is ground together with the treatment agent. Also, if the amount of addition is too large, not only is the effect of improving the quality of the finally obtained recycled fine aggregate for concrete saturated, but there is also a risk that the subsequent grinding step and the like may become difficult to perform. Therefore, if the amount of addition is within the above range, a high-quality recycled fine aggregate for concrete can be suitably obtained.
[0052] The treatment agent is not particularly limited as long as it contains microbubble water and iron oxide, and examples thereof include a treatment liquid (dispersion liquid) in which iron oxide is dispersed in microbubble water. Examples of the treatment liquid include a liquid obtained by immersing an iron-containing object (iron-containing material) in microbubble water. It is considered that this liquid becomes a treatment liquid in which iron oxide is dispersed in microbubble water by immersing the iron-containing object in microbubble water, whereby iron present near the surface of the iron-containing object is oxidized, and the iron oxide is separated from the iron-containing object. The iron-containing object is not particularly limited as long as iron is present near its surface, and may be made of iron, for example. Examples of the iron-containing object that is the raw material for the iron oxide include iron nails and iron in disposable hand warmers. Examples of the iron in the disposable hand warmers include iron in used disposable hand warmers. The conditions for preparing the treatment agent are not particularly limited as long as the treatment agent can be obtained. For example, the time for immersing the iron-containing material in the microbubble water is preferably 5 minutes to 60 hours, and more preferably 30 minutes to 60 hours. The temperature of the microbubble water in which the iron-containing material is immersed is not particularly limited. For example, it is preferably 5 to 50°C, more preferably 5 to 40°C, even more preferably 10 to 40°C, and particularly preferably 10 to 35°C, and may be, for example, room temperature. The amount of the microbubble water added is preferably 10 to 10,000 parts by mass, and more preferably 50 to 1,000 parts by mass, relative to 100 parts by mass of the iron-containing material. When the iron-containing material is immersed in the microbubble water, the microbubble water may be subjected to a bubbling treatment. The treatment agent may be, for example, a liquid or semi-solid state. The liquid state may be, for example, a paste state. The semi-solid state is classified as a state of 30 Pa·s or more in the JAS standard, and examples of such a state include a state of 30 Pa·s or more.
[0053] The microbubble water is water containing microbubbles, and examples of the microbubble water include those specified in ISO 20480-1:2017. The average particle size of the microbubbles is preferably 0.1 to 100 μm, and more preferably 0.1 to 50 μm. Examples of the average particle size of the microbubbles include a volume-equivalent sphere diameter, such as a diameter derived based on the volume of a bubble assuming a spherical shape.
[0054] The method for producing the microbubble water is not particularly limited, and examples thereof include an ejector method, a cavitation method, a swirling flow method, and a pressurized dissolution method. Examples of the ejector method include a method in which a pressurized liquid is sent to an ejector, and the gas self-absorbed by countless separation flows generated inside the ejector is atomized to generate bubbles. Examples of the cavitation method include a method in which a pressurized liquid is sent to a generator having a cavitation structure, and the dissolved gas contained in the liquid is precipitated by utilizing the cavitation phenomenon (cavitation phenomenon) generated in the structure to generate bubbles. Examples of the swirling flow method include a method in which a pressurized liquid is sent from an eccentric direction to a generator having a cylindrical structure, and the air is self-absorbed by an air column formed in the center of the cylinder, and bubbles are generated by the shear force generated by the speed difference when the liquid is discharged. Examples of the pressurized dissolution method include a method in which gas is forcibly dissolved under pressure, and bubbles are precipitated by decompression (opening to the atmosphere). As a microbubble generating device, a swirling type microbubble generating device that is not easily affected by water quality is preferable. Specifically, a microbubble generator using a YJ nozzle manufactured by Bay Clean Co., Ltd. is preferred. That is, the microbubble water is preferably microbubble water obtained by a swirling flow method, and specifically, microbubble water produced by a microbubble generator using a YJ nozzle manufactured by Bay Clean Co., Ltd. is preferred.
[0055] The iron oxide is not particularly limited, but examples thereof include iron oxide generated by immersing an iron-containing material in microbubble water as described above (iron oxide formed by oxidizing the iron of the iron-containing material).
[0056] The concentration of the iron oxide in the treatment agent is preferably 0.01 to 50% by mass, more preferably 0.1 to 20% by mass, and even more preferably 0.1 to 10% by mass, relative to the treatment agent. If the concentration of the iron oxide is too low, the quality of the finally obtained recycled fine aggregate for concrete tends not to be sufficiently improved. This is considered to be because the cement content is difficult to be suitably removed from the crushed material even if the crushed material is ground together with the treatment agent. Also, if the concentration of the iron oxide is too high, not only will the effect of improving the quality of the finally obtained recycled fine aggregate for concrete be saturated, but there is also a risk that the subsequent grinding process and the like will be difficult to carry out. Therefore, if the concentration of the iron oxide is within the above range, a high-quality recycled fine aggregate for concrete can be suitably obtained.
[0057] In the grinding step, the crushed material to which the treatment agent has been added is ground. The grinding may be dry grinding or wet grinding, but wet grinding is preferred because the cement content can be more suitably removed from the crushed material. The wet grinding is not particularly limited and can be performed using a wet grinder. Examples of the wet grinder include a sand mill, a ball mill, a rod mill, a dyno mill, and a pit mill. In addition, it is preferable to use a grinder containing a grinding medium as the grinding medium, and it is more preferable to use iron balls as the grinding medium in a ball mill, and iron rods as the grinding medium in a rod mill. The grinding medium is preferably a medium that can be removed by magnetic force in the removal step described below. In addition, the wet grinder may be any of a vertical type, a horizontal type, a batch type, and a continuous type. The grinding conditions are not particularly limited as long as they are conditions that allow the cement to be removed from the crushed material, but the grinding treatment time is, for example, preferably 30 seconds to 24 hours, more preferably 10 minutes to 12 hours, and even more preferably 1 to 6 hours.
[0058] The manufacturing method may include a step (removing step) of removing magnetic body components from the crushed material (crushed material) by magnetic force. In the removing step, for example, iron components derived from concrete debris and magnetic body components such as iron oxide contained in the treatment agent are removed from the crushed material by magnetic force. Even if the crushing step is wet-grinding with a grinding machine containing grinding media, the grinding media of the grinding machine used during the crushing step are also removed in the removing step. That is, in the manufacturing method, it is preferable that the grinding step is wet-grinding with a grinding machine containing grinding media, and the magnetic body components removed in the removing step are iron components derived from concrete debris, grinding media of the grinding machine used during the grinding, and magnetic body components such as iron oxide contained in the treatment agent. In such a manufacturing method, not only is the cement content more suitably removed by wet grinding with a grinding machine containing grinding media, but the removal step also removes the grinding media in the removal step, resulting in a higher quality recycled fine aggregate for concrete. The removal is not particularly limited, and can be performed using a magnetic separator (magnetic separator) or the like. Examples of the magnetic separator include a drum-type magnetic separator using a permanent magnet, a belt-type magnetic separator using a permanent magnet, a drum-type magnetic separator using an electromagnet, and a belt-type magnetic separator using an electromagnet. Examples of the magnetic separator include a hanging electromagnet for removing iron. The magnetic body components removed in the removal step are not particularly limited as long as they are components that should not be contained in the recycled fine aggregate for concrete, and examples of the magnetic body components removed in the removal step include iron components derived from the concrete debris, the grinding media, and the iron oxide (iron oxide contained in the treatment agent). Examples of the iron components derived from the concrete debris include reinforcing bars that were not removed in the crushing and classification. The removed reinforcing bars are stored, for example, in a reinforcing bar storage area.
[0059] The method for producing recycled fine aggregate for concrete can produce high-quality recycled fine aggregate for concrete. For example, the method for producing recycled fine aggregate for concrete can produce recycled aggregate H for concrete specified in JIS A 5021:2018, recycled aggregate M for concrete specified in JIS A 5022:2018, and recycled aggregate specified in 9.5 of JIS A 5308:2019.
[0060] The manufacturing method may also include a step of extracting the crushed material of a size suitable for use as fine aggregate from the crushed material from which the magnetic material components have been removed. Specifically, the crushed material larger than the size suitable for use as fine aggregate (i.e., the crushed material of a size suitable for use as coarse aggregate) may be removed from the crushed material using a trommel rotary separator or the like. The crushed material from which the large crushed material has been removed may be removed from the crushed material using a spiral water washer, a spiral cleaning machine, a spiral screw sand recovery machine, a spiral classifier, or the like, at which time the treatment agent after the removal step is removed. By doing so, the crushed material of a size suitable for use as fine aggregate may be extracted from the crushed material from which the magnetic material components have been removed. In this case, the crushed material of a size suitable for use as fine aggregate extracted in the manner described above is obtained as recycled fine aggregate for concrete.
[0061] In the method for producing recycled fine aggregate for concrete, at least one of the adding step and the grinding step may be performed two or more times. Specifically, the recycled fine aggregate obtained after the removing step may be subjected to the crushing step, the adding step, the grinding step, or the removing step. That is, the recycled fine aggregate obtained after the removing step may be subjected to any of the crushing step, the adding step, and the grinding step. In addition, in the method for producing recycled fine aggregate for concrete, from the viewpoint of obtaining a higher quality recycled fine aggregate for concrete, it is preferable to perform any one of the steps two or more times, and it is more preferable to perform both of these two steps two or more times. Specifically, it is preferable to perform the recycled fine aggregate obtained after the removing step to the crushing step and the adding step.
[0062] The manufacturing method of the recycled fine aggregate for concrete may use a hardened material derived from returned fresh concrete or residual fresh concrete instead of the crushed material obtained by crushing the concrete debris. That is, the manufacturing method of the recycled fine aggregate for concrete according to another embodiment of the present invention is the same as the manufacturing method described above, except that a hardened material derived from returned fresh concrete or residual fresh concrete is used instead of the crushed material obtained by crushing the concrete debris. Specifically, the manufacturing method of the recycled fine aggregate for concrete includes an addition step of adding a treatment agent containing microbubble water and iron oxide to the hardened material derived from returned fresh concrete or residual fresh concrete, a grinding step of grinding the crushed material to which the treatment agent has been added, and a removal step of removing magnetic material components from the grounded crushed material by magnetic force. The grinding step may be, for example, the same step as the grinding step in the manufacturing method (the manufacturing method using the crushed material obtained by crushing the concrete debris), and in addition, a step of grinding by friction mixing using an agitator may also be included. This manufacturing method may or may not further include a step of crushing the hardened material derived from the returned fresh concrete or the residual fresh concrete. With the manufacturing method as described above, a high-quality recycled fine aggregate can be obtained from the hardened material derived from the returned fresh concrete or the residual fresh concrete. Furthermore, the cement content removed from the hardened material is not the cement content derived from concrete debris, but is, for example, the cement content contained in the returned fresh concrete, the cement content contained in the residual fresh concrete, and the cement content such as cement paste derived from the hardened material, etc.
[0063] The returned ready-mixed concrete and the remaining ready-mixed concrete are ready-mixed concrete produced at a ready-mixed concrete plant or the like, which is transported to a construction site by an agitator truck or the like, but is returned to the ready-mixed concrete plant. The returned ready-mixed concrete is ready-mixed concrete that is not used at a construction site or the like and is returned to the ready-mixed concrete plant as is, and the remaining ready-mixed concrete is ready-mixed concrete that remains in an agitator truck or the like that has returned from a construction site or the like. The ready-mixed concrete starts hardening immediately after production, and even before it is completely hardened, for example, hardens on the surface of fine aggregate, and a hardened material containing the fine aggregate exists. For this reason, the hardened material derived from the returned ready-mixed concrete or the remaining ready-mixed concrete used in the manufacturing method includes not only crushed material obtained by crushing the hardened returned ready-mixed concrete or the remaining ready-mixed concrete, but also hardened material containing the fine aggregate present in the returned ready-mixed concrete or the remaining ready-mixed concrete. In addition, when the hardened material derived from the returned ready-mixed concrete or the remaining ready-mixed concrete is large, or is a hardened material of the returned ready-mixed concrete or the remaining ready-mixed concrete, the manufacturing method further includes a step of crushing these hardened materials. This step is the same as the step of crushing the concrete debris. In addition, when the hardened material derived from the returned fresh concrete or the residual fresh concrete is small, the manufacturing method does not need to include a step of crushing the hardened material. The hardened material may be in a solid or gel form. Unlike the concrete debris and its crushed material, the hardened material does not usually contain reinforcing bars, and therefore, examples of the magnetic material components removed in the removal step in this manufacturing method include the grinding media and the iron oxide.
[0064] [Recycled fine aggregate for concrete] The recycled fine aggregate for concrete obtained by the method for producing recycled fine aggregate for concrete has, for example, an oven-dry density of 1.5 g / cm 3 or more, the water absorption rate is 7% or less, and when the color tone is expressed by the Lab system, the a value is 0 to 3 and the b value is 5 to 15. That is, the recycled fine aggregate for concrete according to another embodiment of the present invention has an oven-dry density of 1.5 g / cm3 or more, the water absorption rate is 7% or less, and when the color tone is expressed by the Lab system, the a value is 0 to 3 and the b value is 5 to 15. Such recycled fine aggregate for concrete is a high-quality recycled aggregate for concrete. An example of the recycled fine aggregate for concrete is recycled fine aggregate H for concrete. In addition, fine aggregates other than recycled fine aggregates (normal fine aggregates) have an oven-dry density of 1.5 g / cm 3 It is possible to obtain fine aggregate having the above mentioned properties, water absorption rate of 7% or less, and color tone expressed by the Lab system with an a value of 0 to 3 and a b value of 5 to 15. However, it has not been possible to produce such fine aggregate from recycled fine aggregate in the past. The method for producing recycled fine aggregate for concrete according to this embodiment can obtain the recycled fine aggregate for concrete.
[0065] The bone dry density of the recycled fine aggregate for concrete is 1.5 g / cm3 as described above. 3 More than 2g / cm 3 It is preferable that the content is 2.5 g / cm or more. 3 It is more preferable that the bone dry density of the recycled fine aggregate for concrete is 4.5 g / cm or more. 3 It is preferable that the bone dry density is less than 100 g / cm. The higher the bone dry density, the higher the quality of the recycled fine aggregate. Therefore, if the bone dry density is within the above range, the recycled fine aggregate is of high quality. In other words, if the bone dry density is within the above range, it is understood that there are few voids. From this, it is considered that the cement content in the crushed material has been sufficiently removed, and therefore the recycled fine aggregate is of high quality. Note that the bone dry density (g / cm 3 ) is the mass (g) of a substance in a dry state divided by its volume (cm 3 ) The bone-dry state is the state in which a sample is left in a hot air dryer at 110°C and the mass of the sample is measured at 15-minute intervals, with the difference in mass before and after being within 0.1% of the mass after. The bone-dry state mass is the mass of the sample when it has reached a bone-dry state. The bone-dry state volume is the volume of the sample when it has reached a bone-dry state.
[0066] As described above, the water absorption rate of the recycled fine aggregate for concrete is 7% or less, preferably 5% or less, more preferably 4.5% or less, even more preferably 4% or less, particularly preferably 3.5% or less, and particularly more preferably 3% or less. The water absorption rate of the recycled fine aggregate for concrete is preferably as low as possible, but in reality, the limit is often about 0.5%, and the lower limit of the water absorption rate range of the recycled fine aggregate for concrete is, for example, 0.5%. The lower the water absorption rate, the higher the quality of the recycled fine aggregate. Therefore, if the water absorption rate is within the above range, the recycled fine aggregate is of high quality. In other words, if the water absorption rate is within the above range, the cement content in the crushed material is considered to have been sufficiently removed, and the recycled fine aggregate is of high quality. The water absorption rate is the percentage of the total amount of water contained in the aggregate in a surface-dried water-saturated state relative to the mass of the aggregate in an absolute dry state. In other words, it is a numerical value that expresses the amount of water that the aggregate can contain as a percentage. The surface dry water-saturated state (surface dry state) is a state in which there is no water on the surface of the aggregate and all of the voids inside the aggregate grains are filled with water. The total amount of water contained in aggregate in the surface dry water-saturated state is the difference between the mass of the aggregate in the surface dry state and the mass of the aggregate in the bone dry state.
[0067] When the color tone of the recycled fine aggregate for concrete is expressed by the Lab system, the a value is 0 to 3, preferably 0.5 to 3, and more preferably 0.5 to 2.5. The b value is 5 to 15, preferably 7 to 15, and more preferably 7 to 12. If the a value and the b value are within the above ranges, the recycled fine aggregate is of high quality. Furthermore, even if the a value and the b value of a conventional fine aggregate for concrete (fine aggregate that is not recycled fine aggregate) are within the above ranges, it is difficult to make the a value and the b value within the above ranges for recycled fine aggregate for concrete. With the above production method, the a value and the b value can be easily made within the above ranges even for recycled fine aggregate for concrete.
[0068] The angle of repose of the recycled fine aggregate for concrete is preferably 45° or less, more preferably 42° or less, even more preferably 40° or less, and particularly preferably 38° or less. The smaller the angle of repose of the recycled fine aggregate for concrete, the better, but in practice, the limit is often about 10°, and the lower limit of the range of the angle of repose of the recycled fine aggregate for concrete is, for example, 10°. The angle of repose is the angle formed by the cone-shaped deposit formed when powder (in this case, recycled fine aggregate for concrete) is regularly dropped onto a horizontal surface from a slightly elevated position and the horizontal surface.
[0069] The fine powder content of the recycled fine aggregate for concrete is preferably 7% or less, more preferably 5% or less, and even more preferably 3% or less. The fine powder content is the ratio of the fine powder contained in the aggregate that passes through a 75 μm (0.075 mm) mesh sieve to the total mass of the aggregate.
[0070] The Ca content in the entire recycled fine aggregate for concrete is preferably 25% by mass or less, and more preferably 5 to 20% by mass. The Si content in the entire recycled fine aggregate for concrete is preferably 70% by mass or more, and more preferably 70 to 95% by mass. Furthermore, the ratio of the Ca content to the Si content (Ca content / Si content) in the entire recycled fine aggregate for concrete is preferably 0 to 0.5, and more preferably 0 to 0.4. The Si content and Ca content in the entire recycled fine aggregate for concrete can be measured, for example, by energy dispersive X-ray fluorescence analysis. Furthermore, the ratio of the Ca content to the Si content (Ca content / Si content) in the entire recycled fine aggregate for concrete can be calculated from these Si content and Ca content.
[0071] The amount of Ca on the surface of the recycled fine aggregate for concrete is preferably 9% by mass or less, more preferably 0.5 to 7% by mass. The amount of Si on the surface of the recycled fine aggregate for concrete is preferably 12 to 40% by mass, more preferably 15 to 30% by mass. The ratio of the amount of Ca to the amount of Si on the surface of the recycled fine aggregate for concrete (Ca amount / Si amount) is preferably 0.22 or less, more preferably 0.05 to 0.2. The amount of Si and the amount of Ca on the surface of the recycled fine aggregate for concrete can be measured, for example, by energy dispersive X-ray analysis, more specifically, by an energy dispersive X-ray analyzer (EDS) provided in a scanning electron microscope. From these amounts of Si and Ca, the ratio of the amount of Ca to the amount of Si in the entire recycled fine aggregate for concrete (Ca amount / Si amount) can be calculated.
[0072] [Ready-mix concrete] The ready-mixed concrete according to another embodiment of the present invention is not particularly limited as long as it is ready-mixed concrete containing the recycled fine aggregate for concrete, cement, and water. By containing the recycled fine aggregate for concrete, it is possible to obtain an excellent ready-mixed concrete. Furthermore, the ready-mixed concrete may contain only the recycled fine aggregate for concrete as a fine aggregate, or may contain the recycled fine aggregate for concrete and other fine aggregates. Furthermore, the ready-mixed concrete may contain coarse aggregate.
[0073] The cement is not particularly limited as long as it is a cement used in producing ready-mixed concrete. Specifically, portland cement such as ordinary portland cement, early-strength portland cement, ultra-early-strength portland cement, moderate-heat portland cement, low-heat portland cement, and white portland cement, blast-furnace cement, alumina cement, silica cement, and silica fume cement can be mentioned. Among these, portland cement is preferable, and ordinary portland cement is more preferable. In addition, examples of ordinary portland cement include those described in JIS R 5210:2009. It is considered that the use of such cement can more suitably advance the hydration reaction and the porazon reaction of the cement. Therefore, by using such cement, ready-mixed concrete that can obtain a concrete structure having higher strength and higher stability can be obtained. The content of the cement is preferably 8.84 to 18.13% by volume with respect to the ready-mixed concrete.
[0074] The aggregate is not particularly limited as long as it contains the recycled fine aggregate for concrete as described above, and may contain aggregates other than the recycled fine aggregate for concrete. Examples of the aggregate include fine aggregate and coarse aggregate. As described above, the ready-mixed concrete may contain the recycled fine aggregate for concrete alone as the fine aggregate, or may use the recycled fine aggregate for concrete in combination with other fine aggregates. Even if the recycled fine aggregate for concrete is used alone as the fine aggregate for the ready-mixed concrete, aggregates other than the recycled fine aggregate for concrete may be used as the coarse aggregate. The aggregates other than the recycled fine aggregate for concrete are not particularly limited as long as they are aggregates that are generally used when producing ready-mixed concrete. The fine aggregates other than the recycled fine aggregate for concrete are not particularly limited as long as they are fine aggregates to be contained in the ready-mixed concrete. Examples of the fine aggregates include natural sand such as silica sand, and crushed stone powder. Examples of fine aggregates other than the recycled fine aggregate for concrete include sand and the like specified in JIS A 5005:2020. The coarse aggregate is not particularly limited as long as it is a fine aggregate to be contained in the fresh concrete. Examples of the coarse aggregate include crushed stone and the like. Examples of the coarse aggregate include coarse aggregate 1505 and coarse aggregate 2010 specified in JIS A 5005:2020, and mixtures thereof. Examples of aggregates other than the recycled fine aggregate for concrete include mountain sand, which is a sandy soil that is collected as a construction material from alluvial sedimentary soil in land areas such as mountains, hills, and plateaus. The content of the aggregate is preferably 66.80 to 90.33% by volume with respect to the fresh concrete. Among the aggregates, the content of the recycled fine aggregate for concrete is preferably 31.31 to 43.10% by volume with respect to the fresh concrete.
[0075] The water is not particularly limited as long as it is water that is generally used when producing ready-mix concrete. Examples of the water include general water such as tap water and industrial water. The content of the water is preferably 6.84 to 8.85% by volume relative to the ready-mix concrete.
[0076] The ready-mix concrete may contain, in addition to the cement, the aggregate, and water, other components that are generally added to ready-mix concrete, etc. Examples of the other components include coal ash, slag powder, surfactants such as air entraining agents (AE agents), and admixtures such as AE water reducing agents.
[0077] The coal ash is not particularly limited as long as it is ash generated when coal is burned. Examples of the coal ash include fly ash and clinker ash, and fly ash is preferably used.
[0078] The slag powder is not particularly limited, and examples thereof include blast furnace slag powder, copper slag powder, etc. That is, the slag powder is preferably blast furnace slag powder, copper slag powder, or a mixture of blast furnace slag powder and copper slag powder.
[0079] The admixture is not particularly limited as long as it is an admixture to be contained in the ready-mixed concrete. Examples of the admixture include surfactants such as air entraining agents and AE water reducing agents, and specifically, water reducing agents (high-performance AE water reducing agents) specified in JIS A 6204:2011. If the amount of cement is too small, the strength of the obtained concrete structure tends to be insufficient. Also, if the amount of cement is too much, the stability of the obtained concrete structure tends to be insufficient. This is considered to be because if the amount of cement is too much, the amount of the coal ash is relatively small, the pozzolanic reaction does not proceed favorably, and the effect of improving stability by the pozzolanic reaction becomes insufficient. If the coal ash is used so that the content of the cement is within the above range relative to the mixture of the cement, the coal ash, and the aggregate, ready-mixed concrete that can obtain a concrete structure with higher strength and higher stability can be obtained. This is considered to be because the hydration reaction and the pozzolanic reaction of the cement can be proceeded more favorably by using the coal ash in place of a part of the cement so that it is within the above range.
[0080] [Method of manufacturing ready-mix concrete] The method for producing the ready-mixed concrete is not particularly limited as long as the ready-mixed concrete can be produced. Specifically, the method for producing the ready-mixed concrete may be a method similar to a method for producing a general ready-mixed concrete, except that the recycled fine aggregate for concrete is used as the aggregate. That is, the method for producing ready-mixed concrete according to another embodiment of the present invention is a method for producing the ready-mixed concrete, which includes a step (mixing step) of mixing cement, aggregate, and water, and uses an aggregate containing the recycled fine aggregate for concrete (recycled fine aggregate for concrete produced by the method for producing recycled fine aggregate for concrete) as the aggregate. By using the recycled fine aggregate for concrete as the aggregate, excellent ready-mixed concrete can be produced. In the mixing step in the method for producing the ready-mixed concrete, in addition to the cement, aggregate, and water, the other components may be mixed as necessary, for example. The mixing step is a step of mixing cement, aggregate, water, and the other components as necessary. The mixing step is not particularly limited except that the crushed sand is used as the aggregate, and may be, for example, a mixing step in a general method for producing ready-mixed concrete.
[0081] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these. EXAMPLES
[0082] [Preparation of treatment agent] (Treatment agent 1) 2 kg of iron nails were immersed in 100 kg of microbubble water produced using a swirl-type microbubble water generator (a microbubble water generator using a YJ nozzle manufactured by By-Clean Co., Ltd.). By doing so, a treatment agent containing microbubble water and iron oxide (a treatment liquid in which iron oxide is dispersed in microbubble water) was obtained. The concentration of iron oxide in this treatment agent was 1% by mass relative to the treatment agent.
[0083] (Treatment agent 2) 2 kg of iron oxide from a used disposable hand warmer was immersed in 100 kg of microbubble water produced using a swirl-type microbubble water generator (a microbubble water generator using a YJ nozzle manufactured by By Clean Co., Ltd.). By doing so, a treatment agent containing microbubble water and iron oxide (a treatment liquid in which iron oxide is dispersed in microbubble water) was obtained. The concentration of iron oxide in this treatment agent was 0.5% by mass relative to the treatment agent.
[0084] [Example 1] 10 kg of concrete rubble with a diameter of about 10 cm was dry-crushed using an impact crusher (Hardpact, manufactured by Nittetsu Mining Co., Ltd.) and classified using a vibrating sieve classifier (manufactured by Kitagawa Iron Works Co., Ltd.). The crushing and classification removed the reinforcing steel contained in the concrete rubble. Crushed material was obtained by the crushing and classification.
[0085] 0.5 kg of the treatment agent 1 was sprayed onto the crushed material, and the crushed material sprayed with the treatment agent 1 was poured into a ball mill (manufactured by Kitagawa Iron Works, Ltd.). By doing so, the cement paste in the crushed material was swollen by the treatment agent 1 and softened. Then, iron balls were put into the ball mill as a grinding medium. The crushed material was wet-ground in the ball mill containing balls as a grinding medium. By doing so, the cement paste was removed from the crushed material. Then, the reinforcing bars, the iron balls, and magnetic components such as iron oxide that were not removed during the crushing and classification were removed from the crushed material (grinded material) that had been wet-ground using a hanging electromagnet for iron removal (manufactured by Kitagawa Iron Works, Ltd.).
[0086] From the crushed material from which the magnetic material components had been removed, the crushed material larger than the size required for fine aggregate (i.e., the crushed material of a size required for coarse aggregate) was removed using a trommel rotary separator (manufactured by Kitagawa Iron Works, Ltd.). Then, the treatment agent 1 was removed from the crushed material using a spiral classifier (manufactured by Kitagawa Iron Works, Ltd.). By doing so, the crushed material of a size required for fine aggregate was obtained as recycled fine aggregate for concrete. Note that 9 kg of the recycled fine aggregate for concrete was obtained.
[0087] [Example 2] 1000 kg of dehydrated residual concrete (hardened residual concrete) was dry crushed using an impact crusher (Hardpact, manufactured by Nittetsu Mining Co., Ltd.) and classified using a vibrating sieve classifier (manufactured by Kitagawa Iron Works Co., Ltd.). The crushed material was obtained by this crushing and classification.
[0088] 50 kg of the treatment agent 2 was sprayed onto the crushed material, and the crushed material sprayed with the treatment agent 2 was poured into a ball mill (manufactured by Kitagawa Iron Works, Ltd.). By doing so, the cement paste in the crushed material was swelled by the treatment agent 2 and softened. Then, iron balls were put into the ball mill as a grinding medium. The crushed material was wet-ground in the ball mill containing balls as a grinding medium. By doing so, the cement paste was removed from the crushed material. Then, the iron balls and magnetic components such as the iron oxide were removed from the crushed material (grinded material) that had been wet-ground using a hanging electromagnet for iron removal (manufactured by Kitagawa Iron Works, Ltd.).
[0089] From the crushed material from which the magnetic material components had been removed, the crushed material larger than the size required for fine aggregate (i.e., the crushed material of a size required for coarse aggregate) was removed using a trommel rotary separator (manufactured by Kitagawa Iron Works, Ltd.). Thereafter, the treating agent 2 was removed from the crushed material using a spiral screw sand recovery machine (manufactured by Kitagawa Iron Works, Ltd.). By doing so, the crushed material of a size required for fine aggregate was obtained as recycled fine aggregate for concrete. The amount of the recycled fine aggregate for concrete obtained was 45 kg.
[0090] [Example 3] 10 kg of concrete rubble with a diameter of about 10 cm was dry-crushed using an impact crusher (Hardpact, manufactured by Nittetsu Mining Co., Ltd.) and classified using a vibrating sieve classifier (manufactured by Kitagawa Iron Works Co., Ltd.). The crushing and classification removed the reinforcing steel contained in the concrete rubble. Crushed material was obtained by the crushing and classification.
[0091] 0.5 kg of the treatment agent 1 was sprayed onto the crushed material, and the crushed material sprayed with the treatment agent 1 was poured into a ball mill (manufactured by Kitagawa Iron Works, Ltd.). By doing so, the cement paste in the crushed material was swollen by the treatment agent 1 and softened. Then, iron balls were put into the ball mill as a grinding medium. The crushed material was wet-ground in the ball mill containing balls as a grinding medium. By doing so, the cement paste was removed from the crushed material. Then, the reinforcing bars, the iron balls, and magnetic components such as iron oxide that were not removed during the crushing and classification were removed from the crushed material (grinded material) that had been wet-ground using a hanging electromagnet for iron removal (manufactured by Kitagawa Iron Works, Ltd.).
[0092] From the crushed material from which the magnetic material components had been removed, the crushed material larger than the size required for fine aggregate (i.e., the crushed material of a size required for coarse aggregate) was removed using a trommel rotary separator (manufactured by Kitagawa Iron Works, Ltd.). Then, the treatment agent 1 was removed from the crushed material using a spiral classifier (manufactured by Kitagawa Iron Works, Ltd.). By doing so, the crushed material of a size required for fine aggregate was obtained as recycled fine aggregate for concrete. Note that 9 kg of the recycled fine aggregate for concrete was obtained.
[0093] Next, the grinding and wet grinding steps were carried out again.
[0094] 0.5 kg of the treatment agent 1 was sprayed onto the crushed material, and the crushed material sprayed with the treatment agent 1 was poured into a ball mill (manufactured by Kitagawa Iron Works, Ltd.). By doing so, the cement paste remaining in the crushed material was swelled by the treatment agent 1 and softened. Then, iron balls were put into the ball mill as a grinding medium. The crushed material was wet-ground in the ball mill containing balls as a grinding medium. By doing so, the cement paste was removed from the crushed material. Then, the reinforcing bars, the iron balls, and magnetic components such as the iron oxide that were not removed during the crushing and classification were removed from the crushed material (grinded material) that had been wet-ground using a hanging electromagnet for iron removal (manufactured by Kitagawa Iron Works, Ltd.).
[0095] From the crushed material from which the magnetic material components had been removed, the crushed material larger than the size required for fine aggregate (i.e., the crushed material of a size required for coarse aggregate) was removed using a trommel rotary separator (manufactured by Kitagawa Iron Works). Then, the treatment agent 1 was removed from the crushed material using a spiral classifier (manufactured by Kitagawa Iron Works). By doing so, the crushed material of a size required for fine aggregate was obtained as recycled fine aggregate for concrete. The amount of the recycled fine aggregate for concrete obtained was 7 kg.
[0096] [Comparative Example 1] 2m 3 The returned fresh concrete is poured into a 3m 3 The concrete was loaded into a double twin-shaft intensive mixer with a working capacity of 100 kg. After the concrete was loaded into the mixer, 2 kg of an organic powder flocculant mixture based on anionic polyacrylamide was added and this was mixed for 1 minute 30 seconds. Once the mixing was over, the coarse material was discharged and separated in a vibrating sieve consisting of one separator with 5 mm openings. Two fractions were thus obtained: the first fraction was represented by aggregates larger than 5 mm, the second fraction was the material that passed the 5 mm sieve and was collected at the bottom.
[0097] [Comparative Example 2] Recycled aggregate for concrete was produced using concrete rubble consisting of the first raw material (sandstone-based raw material) generated by concrete rubble and the second raw material (lime-based raw material) consisting of returned ready-mix concrete. The volume ratio of the large diameter component (10-25 mm) to the small diameter component (0-10 mm) was set to five types: 100:0, 50:50, 70:30, 30:70, and 0:100. The volume ratio of the first raw material to the second raw material supplied to the grinder (109) was set to 50:50, and finally, recycled coarse aggregate (RHG 2005) consisting of the large diameter component (5-20 mm) and recycled fine aggregate (RHS) consisting of the small diameter component (0-5 mm) were collected. The grinders (109) used were "Super Gaos 1300" (product name: Daito Doboku Co., Ltd.) and "Super Gaos 500" (product name: Daito Doboku Co., Ltd.).
[0098] [Comparative Example 3] 10 kg of concrete rubble with a diameter of about 10 cm was dry-crushed using an impact crusher (Hardpact, manufactured by Nittetsu Mining Co., Ltd.) and classified using a vibrating sieve classifier (manufactured by Kitagawa Iron Works Co., Ltd.). The crushing and classification removed the reinforcing steel contained in the concrete rubble. Crushed material was obtained by the crushing and classification.
[0099] The crushed material was sprayed with industrial water, and the crushed material sprayed with the industrial water was poured into a ball mill (manufactured by Kitagawa Iron Works, Ltd.). Then, iron balls manufactured by Kitagawa Iron Works, Ltd. were put into the ball mill as a grinding medium. The crushed material was wet-ground in the ball mill containing balls as a grinding medium. Then, the reinforcing bars, the iron balls, and magnetic components such as iron oxide that were not removed during the crushing and classification were removed from the crushed material (grinded material) that had been wet-ground using a hanging electromagnet for iron removal (manufactured by Kitagawa Iron Works, Ltd.).
[0100] From the crushed material from which the magnetic material had been removed, the crushed material larger than the size required for fine aggregate (i.e., the crushed material of a size required for coarse aggregate) was removed using a trommel rotary separator (manufactured by Kitagawa Iron Works, Ltd.). Then, the industrial water was removed from the crushed material using a spiral classifier (manufactured by Kitagawa Iron Works, Ltd.). By doing so, the crushed material of a size required for fine aggregate was obtained as recycled fine aggregate for concrete. Note that 9 kg of the recycled fine aggregate for concrete was obtained.
[0101] The bone dry density, water absorption rate, angle of repose, and color values (L value, a value, and b value) of the recycled fine aggregate for concrete produced as described above were measured by the following methods.
[0102] (absolutely dry density) Each of the recycled fine aggregates for concrete obtained was left in a hot air dryer at a temperature of 110°C, and its mass was measured at 15-minute intervals. It was left in the hot air dryer until the difference in mass before and after was within 0.1% of the mass after (absolutely dry state). The mass (g) and volume (cm3) of the recycled fine aggregate for concrete in this absolute dry state were 3 ) and the mass (g) of the bone-dry recycled fine aggregate for concrete was calculated by multiplying the volume (cm 3 ) to obtain the bone dry density (g / cm 3 ) was calculated.
[0103] (Water absorption rate) The water absorption rate of each of the obtained recycled fine aggregates for concrete was measured by a method conforming to JIS A 1109:2020. Specifically, first, the recycled fine aggregate for concrete was placed in a state in which there was no surface water and all of the internal voids were filled with water (surface dry water-saturated state), and the mass (g) of the recycled fine aggregate for concrete in this surface dry water-saturated state was measured. Then, the difference between the mass (g) of the recycled fine aggregate for concrete in the surface dry water-saturated state and the mass (g) of the recycled fine aggregate for concrete in the bone dry state was calculated to obtain the total amount of water (g) contained in the recycled fine aggregate for concrete in the surface dry water-saturated state. Then, the total amount of water (g) contained in the recycled fine aggregate for concrete in this surface dry water-saturated state was divided by the mass (g) of the recycled fine aggregate for concrete in the bone dry state to calculate the water absorption rate (%). That is, the water absorption rate (%) was obtained by calculating [(mass (g) of recycled fine aggregate for concrete in a surface-dry water-saturated state - mass (g) of recycled fine aggregate for concrete in an absolute dry state) / mass (g) of recycled fine aggregate for concrete in an absolute dry state × 100].
[0104] (Angle of repose) Each of the recycled fine aggregates for concrete obtained was dropped regularly onto a horizontal plane from a slightly elevated position to form a cone-shaped pile. The pile was photographed so that the angle between its side and the horizontal plane was captured, and the angle between the side of the pile and the horizontal plane in the obtained image was measured with a protractor to obtain the angle of repose (°).
[0105] (L value, a value, and b value) Each of the obtained recycled fine aggregates for concrete was placed in a 3 cm petri dish, and the L value, a value, and b value of the recycled fine aggregates for concrete in this state were measured using a spectrophotometer (CM-700 manufactured by Konica Minolta, Inc.).
[0106] (Si content, Ca content, and Ca content / Si content) The Si content (mass%) and Ca content (mass%) in the entire recycled fine aggregate for concrete obtained were measured using an energy dispersive X-ray fluorescence analyzer (SEA6000VX HSFinder manufactured by Hitachi High-Tech Science Corp.) From the obtained Si content and Ca content, the ratio of the Ca content to the Si content (Ca content / Si content) in the entire recycled fine aggregate for concrete obtained was calculated.
[0107] In addition, the Si content (mass%) and Ca content (mass%) on the surface of the recycled fine aggregate for concrete were measured using a scanning electron microscope (TM3030Plus manufactured by Hitachi High-Tech Technologies Corporation) equipped with an energy dispersive X-ray analyzer (EDS). From the obtained Si and Ca contents, the ratio of the Ca content to the Si content (Ca content / Si content) on the surface of the recycled fine aggregate for concrete was calculated.
[0108] [evaluation] The obtained recycled fine aggregate for concrete was evaluated by the following methods.
[0109] (External Observation) The appearance of the recycled fine aggregate for concrete was observed with a digital microscope manufactured by Sanwa Supply Co., Ltd. to observe the degree of adhesion of cement paste to the surface of the recycled fine aggregate for concrete. Specifically, the area where the cement paste was attached was visually determined from the image obtained by this observation, and the area was calculated. The results were evaluated according to the following criteria.
[0110] When the presence of cement paste could not be confirmed by visual inspection (i.e., when the area ratio of cement paste was 0%), it was evaluated as "1", when the area ratio of cement paste was more than 0% but not more than 20%, it was evaluated as "2", when the area ratio of cement paste was more than 20% but not more than 50%, it was evaluated as "3", when the area ratio of cement paste was more than 50% but not more than 80%, it was evaluated as "4", and when the area ratio of cement paste was more than 80%, it was evaluated as "5". The smaller the evaluation value, the more suitable the recycled fine aggregate for concrete was obtained.
[0111] (Powder properties: cohesiveness) The recycled fine aggregate for concrete was stored at room temperature for one month. After this storage, the condition of the fine aggregate for concrete was visually observed. The results were evaluated according to the following criteria.
[0112] When no cohesion was observed, it was rated as "1", when only slight cohesion was observed, it was rated as "2", when cohesion was observed relatively throughout, it was rated as "3", when cohesion was observed relatively throughout and further when strong cohesion was partially observed, it was rated as "4", and when cohesion was observed relatively throughout, it was rated as "5". The smaller the rating number, the more suitable recycled fine aggregate for concrete has been obtained.
[0113] Next, ready-mix concrete was produced using each of the recycled fine aggregates for concrete obtained. Specifically, ready-mix concrete was produced by mixing the following mixture composition (mass %).
[0114] The mixture was mixed to give 12.91% by mass of cement, 42.97% by mass of recycled coarse aggregate, 35.86% by mass of recycled fine aggregate for concrete, 8.13% by mass of industrial water, and 0.13% by mass of admixture (Flolic SV-10, an AE water-reducing agent manufactured by Flolic Co., Ltd.). Ready-mix concrete was obtained in this manner.
[0115] Then, using each of the obtained ready mixed concretes, tests were conducted by a known method so as to obtain a nominal strength of 21 N and a target slump of 15 cm. The ready mixed concrete with the above mix was the standard mix for the above test. Specifically, the following evaluations were conducted. The evaluation results are shown in Table 1 below.
[0116] (Liquidity) The fluidity of the resulting ready mixed concrete was visually confirmed. The fluidity of ready mixed concrete is one of the indicators of workability on site, and if 9 to 10 workers on site judged the fluidity to be good, it was rated as "◎". If 6 to 8 workers on site judged the fluidity to be good, it was rated as "○". If 3 to 5 workers on site judged the fluidity to be good, it was rated as "△". If 0 to 2 workers on site judged the fluidity to be good, it was rated as "×".
[0117] (slump) The slump evaluation of the ready-mixed concrete was carried out in accordance with JIS A 1101:2020. Specifically, the height of the slump was measured immediately after the slump was formed as described above. In addition, the difference in the measured height from the target slump height of 15 cm (slump difference) was evaluated.
[0118] The evaluation of the slump height was carried out using ready mixed concrete immediately after production and ready mixed concrete 30 minutes after production.
[0119] (flow) The flow evaluation of the ready-mix concrete was performed in accordance with JIS A 1101:2020. Specifically, as described above, the spread of slump immediately after the slump was formed was evaluated as "standard," "large," or "small" according to the criteria in JIS A 1101:2020.
[0120] (Air volume) The air content of the ready-mixed concrete was measured by a method conforming to JIS A 1101:2020. The air content was then evaluated as "standard," "large," or "small" according to the standards of JIS A 1101:2020. Specifically, when the ratio of the volume of air mixed into the ready-mixed concrete to the volume of the ready-mixed concrete is 4 to 5% by volume, it is evaluated as "standard," when it exceeds 5% by volume, it is evaluated as "large," and when it is less than 4% by volume, it is evaluated as "small." In Comparative Example 1, the air content was 6.5% by volume.
[0121] (Mixed state) The mixed state of the obtained ready-mixed concrete was evaluated based on the viscosity of the ready-mixed concrete. For example, a good ready-mixed concrete is one that is soft but viscous. If 9 to 10 out of 10 workers on-site judged the mixed state of the ready-mixed concrete to be good, it was evaluated as "◎". If 6 to 8 out of 10 workers on-site judged the mixed state to be good, it was evaluated as "○". If 3 to 5 out of 10 workers on-site judged the mixed state to be good, it was evaluated as "△". If 0 to 2 out of 10 workers on-site judged the mixed state to be good, it was evaluated as "×".
[0122] As mentioned above, good ready-mix concrete is one that is soft but sticky. Therefore, the mixing state is more important in evaluating ready-mix concrete than the fluidity.
[0123] (strength) The strength of the concrete obtained by solidifying the resulting ready-mix concrete was measured according to a method in accordance with JIS A 1108:2018.The air content was then evaluated as "standard" or "poor" according to the criteria in JIS A 1108:2018.
[0124] (comprehensive evaluation) From the above evaluations, ready-mix concrete that was judged to be very good was rated as "○", that was inferior but still usable was rated as "△", and that was judged to be difficult to use as ready-mix concrete was rated as "×".
[0125] The results are shown in Table 1.
[0126] [Table 1]
[0127] It was found that when recycled fine aggregate for concrete (Examples 1 to 3) obtained by adding a treatment agent containing microbubble water and iron oxide to crushed material obtained by crushing concrete debris or crushed material obtained by crushing returned ready-mix concrete or hardened residual ready-mix concrete, and then grinding the crushed material, was used, it was possible to obtain better ready-mix concrete than recycled fine aggregate for concrete obtained by other manufacturing methods (Comparative Examples 1 to 3).
Claims
1. Crushing the concrete debris; An addition step of adding a treatment agent containing microbubble water and iron oxide to the crushed material obtained by crushing the concrete rubble; and a grinding step of grinding the crushed material to which the treatment agent has been added.
2. The method for producing recycled fine aggregate for concrete according to claim 1, wherein the grinding is performed by wet grinding.
3. 2. The method for producing recycled fine aggregate for concrete according to claim 1, wherein the amount of the treatment agent added in the adding step is 0.05 to 30 volume % relative to the crushed material.
4. The amount of the treatment agent added in the addition step is 1 / m 3 The method for producing recycled fine aggregate for concrete according to claim 1, wherein the amount of recycled fine aggregate is 1 to 300 kg per unit area.
5. The method for producing recycled fine aggregate for concrete according to claim 1, wherein at least one of the adding step and the grinding step is carried out two or more times.
6. An addition step of adding a treatment agent containing microbubble water and iron oxide to a hardened material derived from returned fresh concrete or residual fresh concrete; and a grinding step of grinding the hardened material to which the treatment agent has been added.
7. The method for producing recycled fine aggregate for concrete according to claim 6, wherein the grinding is wet grinding.
8. The method for producing recycled fine aggregate for concrete according to claim 6, wherein the amount of the treatment agent added in the adding step is 0.05 to 30 volume % relative to the hardened material.
9. The amount of the treatment agent added in the addition step is 1 / m 3 The method for producing recycled fine aggregate for concrete according to claim 6, wherein the amount of recycled fine aggregate is 1 to 300 kg per unit area.
10. The method for producing recycled fine aggregate for concrete according to claim 6, wherein at least one of the adding step and the grinding step is carried out two or more times.
11. The method includes a step of mixing cement, aggregate, and water, A method for producing ready-mix concrete, using as the aggregate an aggregate containing recycled fine aggregate for concrete produced by the method for producing recycled fine aggregate for concrete according to any one of claims 1 to 10.
12. Bone dry density is 1.5g / cm 3 That's all. The water absorption rate is 7% or less, A recycled fine aggregate for concrete, having a color tone expressed using the Lab system, with an a value of 0 to 3 and a b value of 5 to 15.
13. The recycled fine aggregate for concrete according to claim 12, having an angle of repose of 45° or less.
14. Ready-mix concrete comprising the recycled fine aggregate for concrete according to claim 12 or 13, cement, and water.
Citation Information
Patent Citations
Water for producing concrete, method for producing water for producing concrete, and ready mixed concrete
JP2022072175A
A carbonization apparatus of recycled aggregates using nano-bubble
KR101740697B1
Recycled aggregate manufacturing method and recycled aggregate obtained from said method
WO2013114526A1
Surface treatment method for sand aggregate and method for producing ready-mixed concrete
WO2018074580A1
Cement hardened body and manufacturing method of recycled fine aggregate used as the hardened body
JP2009040655A