High-performance premixed concrete and preparation method thereof
By adding specific agents to the ready-mixed concrete, the problems of high cost, strong time sensitivity and limited adaptability are solved, and the preparation of high-performance concrete is realized and the construction needs are met.
Patent Information
- Application Number
- CN202411148492.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-12
AI Technical Summary
Ready-mixed concrete has high cost, strong time sensitivity and limited adaptability, making it difficult to meet certain special engineering needs.
By adding a reinforcement slurry composed of silane coupling agent, thickener, antifreeze, toughener and water reducing agent to the ready-mixed concrete, and adding inorganic fillers, the physical properties and compressive strength of the concrete are improved and the working performance is extended. time, reduce costs and increase adaptability.
It significantly reduces the cost of ready-mixed concrete, extends its use time, improves compressive strength and crack resistance, enhances adaptability, and meets construction needs.
Abstract
Description
Technical Field
[0001] The invention relates to the field of concrete preparation, in particular to high-performance ready-mixed concrete and a preparation method thereof. Background Art
[0002] Ready-mixed concrete is a type of construction material that is prepared in advance in a concrete batching plant and then transported to the construction site by concrete mixer trucks. The main feature of this type of concrete is that it is produced in specialized equipment and factories to ensure concrete quality and consistency.
[0003] Although ready-mixed concrete has many advantages, such as controlled quality, convenience and efficiency, it also has some disadvantages and limitations. The first is cost. Ready-mixed concrete is usually more expensive than concrete on site. This is mainly due to its cumbersome preparation method and high raw material prices, which increase costs. The second is time sensitivity. Ready-mixed concrete has a limited working time and is usually poured within a few hours after mixing. This may put some pressure on the construction schedule because the concrete must be used in time or it will lose its working performance. Finally, it has limited adaptability. The formula of ready-mixed concrete is formulated in the concrete mixing plant, so it may not be suitable for some special engineering needs. In some cases, concrete preparation may need to be carried out on site to meet specific requirements. Summary of the invention
[0004] In view of the deficiencies in the prior art, the present invention provides a high-performance ready-mixed concrete and a preparation method thereof, which solves the problems of high cost, time sensitivity and limited adaptability of ready-mixed concrete.
[0005] To achieve the above objectives, the present invention is implemented through the following technical scheme: a high-performance premixed concrete, comprising the following components by mass: 180-220 parts of water, 120-150 parts of cement, 250-300 parts of mixed sand, 500-600 parts of fine aggregate, 700-900 parts of coarse aggregate, 100-150 parts of fly ash, 20-30 parts of silane coupling agent, 10-12 parts of thickener, 10-15 parts of antifreeze agent, 5-8 parts of toughening agent, 2-3 parts of water reducer, and 50-80 parts of inorganic filler.
[0006] Preferably, the mixed sand is made by mixing coarse sand and fine sand in a weight ratio of 3:4.
[0007] Preferably, the silane coupling agent is one of tetraisopropyl titanate, tetrabutyl titanate, dodecyltrimethoxysilane or n-octyltriethoxysilane.
[0008] Preferably, the thickener is one of propylene glycol alginate, methyl cellulose, sodium starch phosphate or sodium carboxymethyl cellulose.
[0009] Preferably, the antifreeze agent is a mixture of one or more of acidic phosphate amine salts, alkylamines, fatty acid amides, organic acid esters or alkyl succinimide.
[0010] Preferably, the toughening agent is prepared by mixing carbon fiber and polyphenylene sulfide fiber in a ratio of 1:0.3 to obtain a fiber mixture, and then mixing the fiber mixture with PET, tackifying resin and pyromellitic anhydride in a ratio of 1:1.5:2.5:0.3:0.1, and extruding at 180-220°C.
[0011] Preferably, the water reducer is one of polycarboxylic acid water reducer powder and naphthalene water reducer powder.
[0012] Preferably, the inorganic filler is prepared by mixing white carbon black, kaolin, mica powder, alumina, diatomaceous earth, calcium carbonate and wollastonite powder in a mass ratio of 1:4:2:1:2:3:5.
[0013] A method for preparing high-performance ready-mixed concrete comprises the following steps:
[0014] Step 1: Put the silane coupling agent, thickener, antifreeze agent, toughening agent and water reducer into a mixing chamber for heating, stirring and mixing, the heating temperature is 70-85°C, the stirring rate is 100-150r / min, and the stirring time is 10-15min to obtain a reinforcing agent slurry;
[0015] Step 2: Put water, cement, mixed sand, fine aggregate, coarse aggregate and fly ash into a mixer and stir for 5-10 minutes, then introduce the reinforcing agent slurry into the mixer and continue mixing and stirring for 5-10 minutes;
[0016] Step 3: Introduce the inorganic filler into the mixer and continue mixing for 5-10 minutes to obtain high-performance ready-mixed concrete.
[0017] The present invention provides a high-performance ready-mixed concrete and a preparation method thereof. It has the following beneficial effects:
[0018] The invention can greatly improve the physical properties of ready-mixed concrete by adding a reinforcing agent slurry composed of a silane coupling agent, a thickener, an antifreeze agent, a toughening agent and a water reducer to the raw materials, while reducing the time sensitivity of the ready-mixed concrete, and prolonging the aging time of the working performance by about three to five hours. In addition, inorganic fillers are added to the raw materials to improve the compressive strength and crack resistance of the ready-mixed concrete, and increase the adaptability range. The invention has low raw material cost, a simple, convenient and fast preparation process, and better meets the use requirements. DETAILED DESCRIPTION
[0019] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0020] Embodiment 1:
[0021] The present embodiment provides a high-performance ready-mixed concrete, which includes the following components in parts by mass: 180 parts of water, 120 parts of cement, 250 parts of mixed sand, 500 parts of fine aggregate, 700 parts of coarse aggregate, 100 parts of fly ash, 20 parts of silane coupling agent, 10 parts of thickener, 10 parts of antifreeze agent, 5 parts of toughening agent, 2 parts of water reducer, and 50 parts of inorganic filler.
[0022] In this embodiment, the mixed sand is prepared by mixing coarse sand and fine sand in a weight ratio of 3:4.
[0023] Furthermore, the silane coupling agent is one of tetraisopropyl titanate, tetrabutyl titanate, dodecyltrimethoxysilane or n-octyltriethoxysilane.
[0024] Furthermore, the thickener is one of propylene glycol alginate, methyl cellulose, sodium starch phosphate or sodium carboxymethyl cellulose.
[0025] Furthermore, the antifreeze agent is a mixture of one or more of acidic phosphate amine salts, alkylamines, fatty acid amides, organic acid esters or alkyl succinimide.
[0026] Furthermore, the toughening agent is prepared by mixing carbon fiber and polyphenylene sulfide fiber in a ratio of 1:0.3 to obtain a fiber mixture, and then mixing the fiber mixture with PET, tackifying resin and isomellitic anhydride in a ratio of 1:1.5:2.5:0.3:0.1, and extruding at 180-220°C.
[0027] Furthermore, the water reducer is one of polycarboxylic acid water reducer powder and naphthalene water reducer powder.
[0028] Furthermore, the inorganic filler is prepared by mixing white carbon black, kaolin, mica powder, alumina, diatomaceous earth, calcium carbonate and wollastonite powder in a mass ratio of 1:4:2:1:2:3:5.
[0029] A method for preparing high-performance ready-mixed concrete comprises the following steps:
[0030] Step 1: Put the silane coupling agent, thickener, antifreeze agent, toughening agent and water reducer into a mixing chamber for heating, stirring and mixing, the heating temperature is 70-85°C, the stirring rate is 100-150r / min, and the stirring time is 10-15min to obtain a reinforcing agent slurry;
[0031] Step 2: Put water, cement, mixed sand, fine aggregate, coarse aggregate and fly ash into a mixer and stir for 5-10 minutes, then introduce the reinforcing agent slurry into the mixer and continue mixing and stirring for 5-10 minutes;
[0032] Step 3: Introduce the inorganic filler into the mixer and continue mixing for 5-10 minutes to obtain high-performance ready-mixed concrete.
[0033] Embodiment 2:
[0034] The present embodiment provides a high-performance ready-mixed concrete, which includes the following components in parts by mass: 220 parts of water, 150 parts of cement, 300 parts of mixed sand, 600 parts of fine aggregate, 900 parts of coarse aggregate, 150 parts of fly ash, 30 parts of silane coupling agent, 12 parts of thickener, 15 parts of antifreeze agent, 8 parts of toughening agent, 3 parts of water reducer, and 80 parts of inorganic filler.
[0035] A method for preparing high-performance ready-mixed concrete, wherein the preparation steps are the same as those in Example 1.
[0036] Comparative Example 1:
[0037] The present embodiment provides a high-performance ready-mixed concrete, which includes the following components in parts by mass: 200 parts of water, 150 parts of cement, 280 parts of mixed sand, 550 parts of fine aggregate, 800 parts of coarse aggregate, 120 parts of fly ash, 15 parts of antifreeze agent, 8 parts of toughening agent, 3 parts of water reducer, and 80 parts of inorganic filler.
[0038] A method for preparing high-performance ready-mixed concrete, wherein the preparation steps are the same as those in Example 1.
[0039] Comparative Example 2:
[0040] The present embodiment provides a high-performance ready-mixed concrete, which includes the following components in parts by mass: 200 parts of water, 150 parts of cement, 280 parts of mixed sand, 550 parts of fine aggregate, 800 parts of coarse aggregate, 120 parts of fly ash, 30 parts of silane coupling agent, 12 parts of thickener, and 80 parts of inorganic filler.
[0041] A method for preparing high-performance ready-mixed concrete, wherein the preparation steps are the same as those in Example 1.
[0042] Comparative Example 3:
[0043] The present embodiment provides a high-performance ready-mixed concrete, which includes the following components in parts by mass: 200 parts of water, 150 parts of cement, 280 parts of mixed sand, 550 parts of fine aggregate, 800 parts of coarse aggregate, 120 parts of fly ash, 30 parts of silane coupling agent, 12 parts of thickener, 15 parts of antifreeze agent, 8 parts of toughening agent, and 3 parts of water reducer.
[0044] A method for preparing high-performance ready-mixed concrete, wherein the preparation steps are the same as those in Example 1.
[0045] Performance testing:
[0046] Performance tests were performed on Examples 1-2 and Comparative Examples 1-3 to compare and detect the anti-permeability, anti-freeze performance, porosity and compressive strength, and the following table was obtained.
[0047] Refer to the national standard GB / T 50082-2009 "Standard for test methods of long-term performance and durability of ordinary concrete" to test the anti-permeability performance of concrete.
[0048] The rapid freeze-thaw cycle test method in GB / T50082-2009 standard is used to detect the frost resistance of concrete.
[0049] Calculate the porosity according to the test method in the "Test Code for Hydraulic Concrete".
[0050] According to GB / T50081-2016 "Standard for Test Methods for Mechanical Properties of Ordinary Concrete", the environmentally friendly high-performance ready-mixed concrete prepared in each embodiment and comparative example was made into a standard test block, and the 28d compressive strength test of the test block was carried out.
[0051] Impermeability grade Frost resistance level Porosity % Compressive strengthMpa Embodiment 1 P9 F350 9.4 42.6 Embodiment 2 P8 F300 9.2 41.4 Comparative Example 1 P6 F200 11.6 35.9 Comparative Example 2 P5 F100 12.4 35.7 Comparative Example 3 P5 F150 14.5 30.7
[0052] As can be seen from the above table, the high-performance premixed concrete in Example 1 and Example 2 performs well in terms of impermeability, frost resistance, porosity and compressive strength, while Comparative Example 1 and Comparative Example 2 perform poorly in terms of impermeability, frost resistance, porosity and compressive strength, and Comparative Example 3 performs the worst. The reason is that no silane coupling agent and thickener are added in Comparative Example 1, and no antifreeze agent, toughening agent and water reducer are added in Comparative Example 2, which affects the physical properties of the premixed concrete. No inorganic filler is added in Comparative Example 3, and its performance is poor, and the overall performance is most affected.
[0053] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A high performance ready-mixed concrete, characterized in that: The composition includes the following components by mass: 180-220 parts of water, 120-150 parts of cement, 250-300 parts of mixed sand, 500-600 parts of fine aggregate, 700-900 parts of coarse aggregate, 100-150 parts of fly ash, 20-30 parts of silane coupling agent, 10-12 parts of thickener, 10-15 parts of antifreeze agent, 5-8 parts of toughening agent, 2-3 parts of water reducer and 50-80 parts of inorganic filler.
2. A high performance ready-mixed concrete according to claim 1, characterized in that: The mixed sand is prepared by mixing coarse sand and fine sand in a weight ratio of 3:
4.
3. A high performance ready-mixed concrete and a preparation method thereof according to claim 1, characterized in that: The silane coupling agent is one of tetraisopropyl titanate, tetrabutyl titanate, dodecyltrimethoxysilane or n-octyltriethoxysilane.
4. A high performance ready-mixed concrete and a preparation method thereof according to claim 1, characterized in that: The thickener is one of propylene glycol alginate, methyl cellulose, sodium starch phosphate or sodium carboxymethyl cellulose.
5. A high performance ready-mixed concrete and a preparation method thereof according to claim 1, characterized in that: The antifreeze agent is a mixture of one or more of acidic phosphate amine salts, alkylamines, fatty acid amides, organic acid esters or alkyl succinimide.
6. A high performance ready-mixed concrete and a preparation method thereof according to claim 1, characterized in that: The preparation method of the toughening agent comprises the following steps: mixing carbon fiber and polyphenylene sulfide fiber in a ratio of 1:0.3 to obtain a fiber mixture; then mixing the fiber mixture with PET, tackifying resin and pyromellitic anhydride in a ratio of 1:1.5:2.5:0.3:0.1, and extruding at 180-220°C.
7. A high performance ready-mixed concrete and a preparation method thereof according to claim 1, characterized in that: The water reducer is one of polycarboxylic acid water reducer powder and naphthalene water reducer powder.
8. A high performance ready-mixed concrete and a preparation method thereof according to claim 1, characterized in that: The inorganic filler is prepared by mixing white carbon black, kaolin, mica powder, alumina, diatomaceous earth, calcium carbonate and wollastonite powder in a mass ratio of 1:4:2:1:2:3:
5.
9. A method for preparing high performance ready-mixed concrete according to any one of claims 1 to 8, characterized in that: The following steps are involved: Step 1: Put the silane coupling agent, thickener, antifreeze agent, toughening agent and water reducer into a mixing chamber for heating, stirring and mixing, the heating temperature is 70-85°C, the stirring rate is 100-150r / min, and the stirring time is 10-15min to obtain a reinforcing agent slurry; Step 2: Put water, cement, mixed sand, fine aggregate, coarse aggregate and fly ash into a mixer and stir for 5-10 minutes, then introduce the reinforcing agent slurry into the mixer and continue mixing and stirring for 5-10 minutes; Step 3: Introduce the inorganic filler into the mixer and continue mixing for 5-10 minutes to obtain high-performance ready-mixed concrete.