Method for producing power storage device
By pre-placing ethylene carbonate in the central part of the wound electrode body, the method addresses uneven electrolyte penetration in power storage devices, ensuring uniform SEI film formation and reducing resistance.
Patent Information
- Application Number
- JP2023044820
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-21
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2043-03-21
AI Technical Summary
In power storage devices with wound electrode bodies, uneven penetration of electrolyte leads to non-uniform formation of the negative electrode SEI film, resulting in increased resistance due to varying EC concentrations along the electrode body, especially near the center where EC penetration is slow.
A manufacturing method that includes forming a strip-shaped negative electrode with a film-forming substance like ethylene carbonate pre-placed in the central part of the wound electrode body, ensuring uniform SEI film formation by advancing the electrolyte penetration and maintaining consistent EC concentration.
This method ensures uniform SEI film formation across the electrode body, reducing resistance and enhancing the performance of power storage devices by maintaining consistent EC distribution, thereby improving charge-discharge efficiency.
Smart Images

Figure 2024134567000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing an electricity storage device. [Background technology]
[0002] Conventionally, in an electricity storage device such as a battery having an electrode body and an electrolyte in a case, it was necessary to consider the uneven penetration (uneven impregnation) of the electrolyte into the electrode body. For example, Patent Document 1 discloses a method for producing a lithium ion battery in which an electrolyte is impregnated in at least one of the separator and the electrode active material layer (B) before a lamination step in which an electrode active material layer (A), a separator, and an electrode active material layer (B) are laminated to obtain a lamination unit, thereby preventing or suppressing the uneven penetration of the electrolyte. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2019-212464 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, as described in Patent Document 1, when a wound-type electrode body is used instead of a stacked unit, i.e., a stacked-type electrode body, it becomes necessary to handle a strip-shaped separator impregnated with an electrolyte or a strip-shaped electrode plate impregnated with an electrolyte, which makes handling difficult.
[0005] On the other hand, as a solvent for the electrolyte of an electricity storage device, ethylene carbonate (hereinafter also referred to as EC) which forms an SEI film may be used in addition to dimethyl carbonate (hereinafter also referred to as DMC), ethyl methyl carbonate (hereinafter also referred to as EMC), etc., in order to facilitate the formation of an SEI film on the negative electrode active material layer during initial charging. For example, an EC / DMC / EMC mixed solvent may be used for the electrolyte.
[0006] However, when an electrolyte containing EC is introduced into the electrode from the end of the electrode where the electrolyte has not yet been introduced, DMC, EMC, and LiPF dissolved in them are 6 It has been found that the permeation speed of EC is relatively slow compared to supporting electrolytes such as DMC (melting point 2-4°C) and EMC (melting point -53°C). EC has a melting point of about 34-37°C, which is relatively high compared to DMC (melting point 2-4°C) and EMC (melting point -53°C), and it also has a high viscosity, so it is thought that it is more difficult for EC to permeate into the electrode body along the negative electrode active material layer and separator than DMC.
[0007] For example, in a power storage device using a wound electrode assembly, in which the belt-shaped electrode plate is wide and the electrolyte permeates a long distance, even if the electrolyte is allowed to permeate from both ends in the axial direction and reaches the center in the axial direction to permeate the entire electrode assembly, there may be cases where the EC has not yet sufficiently reached the center in the axial direction. In other words, during initial charging, there may be cases where the amount of EC per unit area (hereinafter also referred to as area density) present in various places in the electrode body is non-uniform.
[0008] In this state, when an electric storage device such as a secondary battery is initially charged and an attempt is made to form an anode SEI coating on the anode active material layer, it is difficult for an anode SEI coating derived from EC to be formed in the axial center of the electrode body where the EC content is low. For this reason, it has been found that the characteristics of the anode active material layer are different in the axial center of the electrode body where the EC area density is low, compared to the parts of the electrode body where the EC area density is high, such as the axial ends, specifically, the anode active material layer has a relatively high resistance. This results in a high resistance for the entire electric storage device.
[0009] The present invention has been made in consideration of the above-mentioned current situation, and provides a method for manufacturing an electricity storage device in which uneven formation of a negative electrode SEI coating in a negative electrode active material layer in a wound-type electrode body is suppressed, thereby suppressing an increase in resistance. [Means for solving the problem]
[0010] (1) One aspect of the present invention for solving the above problem is a method for producing an electricity storage device comprising: an electrolyte solution containing ethylene carbonate and a solvent having a melting point lower than that of ethylene carbonate; a wound-type electrode body having a strip-shaped positive electrode plate, a strip-shaped negative electrode plate having a strip-shaped negative electrode active material layer, and a strip-shaped separator, the electrolyte solution permeating into the inside; and a case containing the electrode body and the electrolyte solution, the electrode body having a width dimension of the negative electrode active material layer being 180 mm or more, the method comprising the steps of: forming an unpermeated electrode body that is not permeated with the electrolyte solution; and wrapping the unpermeated electrode body in the case. the unpermeated electrode body is disposed in a central portion of the unpermeated electrode body in the axial direction, and a coating material that forms the negative electrode SEI coating on the negative electrode active material layer is disposed in advance in the central portion of the unpermeated electrode body in the axial direction.
[0011] The electricity storage device according to this manufacturing method uses an electrolyte solution containing EC. Moreover, the width dimension of the band-shaped negative electrode active material layer of the wound electrode body is 180 mm or more. Therefore, as described above, even if the electrolyte solution permeates the entire non-permeated electrode body after the waiting time has elapsed, the initial charging process is performed without sufficient EC reaching the center of the axial direction of the wound electrode body, and there is a risk that the generation of the negative electrode SEI coating in the negative electrode active material layer in the electrode body will be non-uniform.
[0012] However, in the present manufacturing method, in the unpermeated electrode body forming step, a film-forming substance that forms a negative electrode SEI film on the negative electrode active material layer is pre-disposed in the central portion of the axial direction of the unpermeated electrode body to form the unpermeated electrode body. Therefore, even if the initial charging step is performed in a state in which the EC derived from the electrolyte does not sufficiently reach the central portion in the waiting step, the pre-disposed film-forming substance can appropriately form a negative electrode SEI film. Thus, it is possible to manufacture an electricity storage device in which the non-uniformity of the formation of the negative electrode SEI film in the negative electrode active material layer in the electrode body is suppressed and an increase in resistance is suppressed.
[0013] Examples of the power storage device include secondary batteries such as lithium ion secondary batteries and sodium ion secondary batteries, and capacitors such as lithium ion capacitors. Examples of the wound electrode body include cylindrical wound electrode bodies and flat wound electrode bodies.
[0014] As the electrolyte, a non-aqueous electrolyte obtained by dissolving a supporting salt in an organic solvent can be used. Examples of organic solvents used in the electrolyte include ethylene carbonate (EC), as well as dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC), which can be mixed with EC to form a mixed solvent and have a lower melting point than EC.
[0015] The electrolyte contains a lithium salt, such as LiBF, as a supporting salt. 4 , LiAsF 6 , LiPF 6 , LiCF 3 SO 3 , LiN(SO 2 CF 3 ) 2 , LiN(SO 2 C 2 F 5 ) 2 , LiN(SO 2 CF 3 )(SO 2 C 4 F 9 ) and the like. Sodium salts, for example, NaPF 6 , Na+ (CF 3 SO 2 ) 2 N - (NaTFSI), etc.
[0016] The coating material is a material capable of forming a negative electrode SEI coating on the negative electrode active material particles in the initial charging step, and examples thereof include EC, which is used separately from the electrolyte, as well as vinylene carbonate, fluoroethylene carbonate, LiBOB, and the like.
[0017] In the unpermeated electrode body forming step, examples of the method for forming an unpermeated electrode body on which a coating material has been previously disposed include a method for forming an unpermeated electrode body using an additional negative electrode plate having a widthwise central portion of a strip-shaped negative electrode active material layer impregnated with a coating material, and a method for forming an unpermeated electrode body using an additional separator having a strip-shaped separator impregnated with a coating material in a portion facing the widthwise central portion of the negative electrode active material layer.
[0018] (2) In the method for producing an electricity storage device described in (1) above, the unpermeated electrode body forming step may preferably include an additional negative electrode plate forming step of forming an additional negative electrode plate in which a central portion in the width direction of the band-shaped negative electrode active material layer is made into a band-shaped additional negative electrode active material layer containing the coating film-forming substance, while both edge portions on both sides in the width direction are made into band-shaped non-containing negative electrode active material layers not containing the coating film-forming substance.
[0019] In this method for producing an electric storage device, the unpermeated electrode body forming step includes an additional negative plate forming step of forming an additional negative plate having a strip-shaped additional negative electrode active material layer and strip-shaped non-containing negative electrode active material layers on both sides of the width direction of the additional negative electrode plate. Since the additional negative electrode plate thus formed is used, a wound-type unpermeated electrode body can be formed in the same manner as a strip-shaped negative electrode plate not provided with an additional negative electrode active material layer, and a coating-forming material can be disposed in advance on the unpermeated electrode body.
[0020] (3) In the method for producing an electricity storage device described in (2) above, the additional negative electrode plate forming step may include forming the additional negative electrode active material layer using an additional negative electrode paste that contains negative electrode active material particles but does not contain the film-forming material, and forming the additional negative electrode active material layer using an additional negative electrode paste that contains the negative electrode active material particles and the film-forming material.
[0021] In this method for producing an electric storage device, in the additional negative plate forming step, the additional negative plate is formed by using the additional negative plate paste to form the additional negative plate active material layer, and the additional negative plate is formed by using the additional negative plate paste. Therefore, the additional negative plate can be formed inexpensively.
[0022] A method for forming an uncontaining negative electrode active material layer using an uncontaining negative electrode paste and an additional negative electrode active material layer using an additional negative electrode paste includes a method in which negative electrode paste / additional negative electrode paste / negative electrode paste are applied in a stripe pattern onto a band-shaped negative electrode current collector foil using a die coater having partitions between the portion for ejecting the additional negative electrode paste and one side portion and the other side portion for ejecting the negative electrode paste, and then dried. Also included is a method of providing a time lag in the application, for example, a method of applying an additional negative electrode paste in a strip shape onto a strip-shaped negative electrode current collector foil, then applying negative electrode paste in a strip shape on both sides in the width direction of the layer of the additional negative electrode paste, and then drying the resulting mixture.
[0023] In addition, in the method for producing the above-mentioned electricity storage device, the additional negative electrode plate forming step is preferably a step of forming an additional negative electrode plate having an additional negative electrode active material layer by forming a non-containing negative electrode active material layer that contains negative electrode active material particles but does not contain the film-forming material, and then applying a paste containing the film-forming material to a widthwise central portion of the non-containing negative electrode active material layer and drying it.
[0024] (4) In the method for producing an electric storage device according to (2) or (3) above, the additional negative electrode plate forming step may be performed in such a manner that the additional negative electrode active material layer is formed by forming the central portion of the band-shaped negative electrode active material layer that is 80 mm or more away from both end edges in the width direction.
[0025] Due to the difference in the ease of penetration between EC and other solvents, EC tends to reach relatively less in areas where the penetration distance along the negative electrode active material layer is 80 mm or more, and as described above, it becomes difficult to form a negative electrode SEI coating derived from EC in the electrolyte. In contrast, in the above-mentioned manufacturing method, the widthwise central portion of the wound-type unpermeated electrode body, which is 80 mm or more away from both widthwise ends of the band-shaped curved active material layer, is used as an additional negative electrode active material layer, which can reliably assist in the formation of a negative electrode SEI coating.
[0026] (5) In the method for producing an electricity storage device according to any one of (1) to (4) above, the film-forming substance may be ethylene carbonate.
[0027] In this method for manufacturing an electricity storage device, ethylene carbonate is placed in advance as a coating material in areas where there is a shortage of ethylene carbonate derived from the electrolyte, so that a negative electrode SEI coating derived from ethylene carbonate can be formed over the entire negative electrode active material layer. [Brief description of the drawings]
[0028] [Figure 1] FIG. 2 is a partially cutaway perspective view of a battery according to an embodiment. [Diagram 2] FIG. 4 is an explanatory diagram illustrating a state in which a negative electrode SEI coating is formed on a negative electrode active material particle in a negative electrode active material layer in the embodiment. [Diagram 3] FIG. 2 is a perspective view of a flat wound electrode body and an unpermeated electrode body in the embodiment. [Figure 4] FIG. 2 is an explanatory diagram illustrating a flat wound type unpermeated electrode body developed to show a positive electrode plate, a negative electrode, and a separator according to the embodiment. [Diagram 5] 1 is a flowchart of a method for manufacturing a battery according to an embodiment. [Figure 6] FIG. 4 is an explanatory diagram showing a manufacturing process of an unpermeated negative electrode plate according to the embodiment. [Figure 7]FIG. 11 is an explanatory diagram showing a stripe pattern in which the non-containing negative electrode paste and the additional negative electrode paste are applied to a wide negative electrode foil by a die coater in the embodiment. [Figure 8] FIG. 11 is an explanatory diagram relating to Comparative Example 1, in which a flat wound type unpermeated electrode body is developed to show a positive electrode plate, a negative electrode, and a separator. [Figure 9] FIG. 11 is an explanatory diagram relating to Comparative Example 2, showing a flat wound type unpermeated electrode body developed to show a positive electrode plate, a negative electrode, and a separator. [Figure 10] FIG. 2 is an explanatory diagram showing an examination site in an electrode body of the battery according to the embodiment and comparative examples 1 and 2. [Figure 11] 1 is a graph showing the relationship between the investigated sites in the electrode bodies of the batteries according to the embodiment and comparative examples 1 and 2 and the relative content of ethylene carbonate. [Figure 12] 1 is a graph showing the relationship between the relative IV resistance value and the examined portion in the electrode body of the batteries according to the embodiment and comparative examples 1 and 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0029] (Embodiment) Hereinafter, a battery 1 (an example of an electricity storage device) which is a lithium ion secondary battery according to an embodiment of the present invention and its manufacture will be described with reference to Figures 1 to 7. The battery 1 is a rectangular, sealed lithium ion secondary battery, and is mounted in vehicles such as hybrid cars, plug-in hybrid cars, and electric cars, as well as in various devices.
[0030] The battery 1 of this embodiment includes a case 7, and an electrode assembly 2 and an electrolyte 6 housed inside the case 7. The case 7 is made of metal (aluminum in this embodiment) and has a rectangular box shape. The case 7 is made of a metal and has a square cylindrical case body 7H with a bottom and a lid 7L located at the upper BH1 in the height direction BH. A positive electrode terminal 8P and a negative electrode terminal 8N are fixed to the lid 7L via an insulating member 9. The lid 7L is perforated with a liquid injection hole 7LH for injecting the electrolyte 6, and is sealed by a liquid injection plug 7LP after the liquid is injected. The electrode assembly 2 is covered in a bag-shaped insulating film (not shown) inside the case 7. A part of the electrolyte 6 housed in the case 7 is impregnated in the electrode assembly 2, and the remaining part is collected at the bottom of the case 7.
[0031] The non-permeated electrode body 12 (see Figs. 3 and 4) not impregnated with the electrolyte 6 is a so-called flat wound type electrode body, in which a strip-shaped non-permeated positive electrode plate 13 and a strip-shaped non-permeated negative electrode plate 14 (an example of an additional negative electrode plate) are wound via a pair of strip-shaped non-permeated separators 15, and pressed in the thickness direction CH to be flattened. For this reason, the electrode body 2 (see Figs. 1, 3, and 4) housed in the case 7 and having the non-permeated electrode body 12 impregnated with the electrolyte 6 is also housed in the case 7 and has a strip-shaped positive electrode plate 3 and a strip-shaped negative electrode plate 4, each of which is impregnated with the electrolyte 6, wound via a pair of strip-shaped separators 5, and is thinned and flattened in the thickness direction CH perpendicular to the paper surface in Fig. 1. This electrode body 2 is housed in the case 7 in a horizontal position in which the winding axis AX coincides with the width direction AH (the left-right direction in Fig. 1).
[0032] As described below, the electrode body 2 in the battery 1 is subjected to initial charging after the electrolyte solution 6 is impregnated into the unpermeated electrode body 12 housed in the case 7. Therefore, as shown in Fig. 2, a negative electrode SEI coating 4AC derived from ethylene carbonate 6VE and lithium salt 6S, which are solvents contained in the electrolyte solution 6, is formed around the negative electrode active material particles 4AP constituting the negative electrode active material layer 4A formed on the negative electrode foil 4F of the electrode body 2. The formation of this negative electrode SEI coating 4AC enables the battery 1 to be charged and discharged stably with low resistance, compared to a case in which the negative electrode SEI coating 4AC is not formed.
[0033] Of the flat wound electrode body 2 and the unpermeated electrode body 12, one side XH1 of the axial direction XH along the winding axis AX (in this embodiment, this corresponds to one side AH1 in the width direction AH of the battery 1; upper side in FIG. 3) is provided with positive current collecting parts 2P, 12P formed by winding current collecting parts 3S, 13S of the positive plate 3 or the unpermeated positive plate 13. Conversely, the other side XH2 of the axial direction XH (in this embodiment, this corresponds to the other side AH2 in the width direction AH of the battery 1; lower side in FIG. 3) is provided with negative current collecting parts 2N, 12N formed by winding current collecting parts 4S, 14S of the negative plate 4 or the unpermeated negative plate 14. The portion between the positive electrode collector 2P, 12P and the negative electrode collector 2N, 12N is a main body portion 2H, 12H in which a positive electrode plate 3 and a negative electrode plate 4 are wound with a separator 5 between them, or an unpermeated positive electrode plate 13 and an unpermeated negative electrode plate 14 are wound with a unpermeated separator 15 between them.
[0034] The positive electrode terminal 8P is made of an aluminum plate bent into a predetermined shape. An inner connection part 8PI forming one end of the positive electrode terminal 8P is connected to a positive electrode current collector 2P arranged on one side AH1 in the width direction AH of the electrode body 2. On the other hand, the other end of the positive electrode terminal 8P is drawn out of the case 7 (specifically, onto the lid body 7L) to form an external terminal part 8PO. In addition, the negative electrode terminal 8N is made of a copper plate bent into a predetermined shape. An inner connection part 8NI forming one end of this negative electrode terminal 8N is connected to a negative electrode current collector 2N arranged on the other side AH2 in the width direction AH of the electrode body 2. On the other hand, the other end of the negative electrode terminal 8N is drawn out of the case 7 (specifically, onto the lid body 7L) to form an external terminal part 8NO.
[0035] The electrolyte 6 is a non-aqueous electrolyte containing an organic solvent 6V and a lithium salt 6S (an example of a supporting salt). In this embodiment, the organic solvent 6V is a mixture of ethylene carbonate (EC) 6VE and another solvent 6VL, dimethyl carbonate (DMC) and ethyl methyl carbonate (EMC), in a weight ratio of 3:4:3. The lithium salt 6S is LiPF 6 The electrolyte used is LiPF 6 The concentration is 1.1 mol / L.
[0036] As shown in FIG. 4, the strip-shaped unpermeated positive electrode plate 13 of the unpermeated electrode body 12 includes a positive electrode foil 13F made of aluminum foil and a positive electrode active material layer 13A laminated on both surfaces of the positive electrode foil 13F. The positive electrode active material layer 13A is made of positive electrode active material particles, conductive particles, and a binder (not shown). In this embodiment, lithium transition metal composite oxide particles, specifically, for example, lithium nickel cobalt manganese composite oxide particles, are used as the positive electrode active material particles. For example, acetylene black (AB) is used as the conductive particles. Also, for example, polyvinylidene fluoride (PVDF) is used as the binder. At the end of one side WH1 (upper side in FIG. 4) of the strip-shaped unpermeated positive electrode plate 13 in the width direction WH, the positive electrode active material layer 13A does not exist on the positive electrode foil 13F, and the positive electrode foil 13F is exposed to form a current collecting portion 13S. On the other hand, the remaining portion of the non-permeated positive electrode plate 13 is a positive electrode portion 13P in which positive electrode active material layers 13A are laminated on both surfaces of a positive electrode foil 13F. As can be seen from Fig. 3 and Fig. 4, the width direction WH (the vertical direction in Fig. 4) of the non-permeated positive electrode plate 13 etc. coincides with the axial direction XH, and one side WH1 coincides with one side XH1.
[0037] On the other hand, of the unpermeated electrode body 12, the strip-shaped unpermeated negative electrode plate 14 includes a negative electrode foil 14F made of copper foil and a negative electrode active material layer 14A laminated on both surfaces of the negative electrode foil 14F. The negative electrode active material layer 14A is made of a negative electrode active material particle 14AP and a binder (not shown). In this embodiment, graphite particles are used as the negative electrode active material particle 14AP. Also, as the binder, for example, carboxymethyl cellulose (CMC) is used. Note that, at the end of the other side WH2 (lower in FIG. 4) of the width direction WH of the strip-shaped unpermeated negative electrode plate 14, the negative electrode active material layer 14A does not exist on the negative electrode foil 14F, and the negative electrode foil 14F is exposed as a current collecting portion 14S. On the other hand, the remaining part of the unpermeated negative electrode plate 14 is a negative electrode portion 14N in which the negative electrode active material layer 14A is laminated on both surfaces of the negative electrode foil 14F. In this embodiment, the width dimension AW of the negative electrode active material layers 4A, 14A in the width direction WH is AW=180 mm.
[0038] In addition, a pair of strip-shaped unpermeated separators 15 of the unpermeated electrode body 12 are made of a porous resin. As shown in FIG. 4, the unpermeated separators 15 are stacked so as to be interposed between the unpermeated negative electrode plate 14 and the unpermeated positive electrode plate 13 when wound. The unpermeated negative electrode plate 14 and the negative electrode portion 14N are slightly wider in the width direction WH than the unpermeated positive electrode plate 13 and the positive electrode portion 13P. Moreover, the negative electrode portion 14N is arranged so as to cover the entire positive electrode portion 13P in the width direction WH, that is, so that the negative electrode active material layer 14A facing the positive electrode active material layer 13A exists at any part of the positive electrode active material layer 13A. In addition, the unpermeated separator 15 is slightly wider in the width direction WH than the negative electrode portion 14N and the positive electrode portion 13P. Moreover, the unpermeated separator 15 is arranged so as to cover the entire width direction WH of the negative electrode portion 14N and the positive electrode portion 13P, i.e., so that the unpermeated separator 15 covering the positive electrode active material layer 13A and the negative electrode active material layer 14A is present in every portion of the positive electrode active material layer 13A and the negative electrode active material layer 14A.
[0039] When the unpermeated electrode body 12 is connected to the positive electrode terminal 8P and the negative electrode terminal 8N and housed in the case 7, and the electrolyte 6 is poured into the case 7, the electrolyte 6 permeates from the outside XHO in the axial direction XH of the unpermeated electrode body 12, i.e., from one side XH1 and the other side XH2, toward the inside of the unpermeated electrode body 12. Specifically, the electrolyte 6 permeates along the unpermeated positive electrode plate 13, the unpermeated negative electrode plate 14, and the unpermeated separator 15 from one side WH1 and the other side WH2 (upper and lower in FIG. 4) in the width direction WH that coincides with the axial direction XH, respectively, toward the center line ML of the width direction WH of the negative electrode active material layer 14A, i.e., toward the inner side WHI of the width direction WH.
[0040] However, as described above, when the electrolyte solution 6 permeates into the unpermeated electrode body 12, the ethylene carbonate 6VE, among the components of the organic solvent 6V, has a slower permeation speed than the other solvents 6VL (in this embodiment, DMC and EMC, which have a lower melting point than EC). For this reason, when considering the distance EL from both end edges 14AE1, 14AE2 in the width direction WH of the negative electrode active material layer 14A of the unpermeated negative electrode plate 14 as the starting point toward the inner side WHI in the width direction WH, it is considered that the concentration of ethylene carbonate 6VE in the electrolyte solution at the leading portion of the electrolyte solution 6 permeating toward the inner side WHI decreases as the distance EL increases. For this reason, when the electrolyte solution 6 has permeated up to the center line ML of the width direction WH of the negative electrode active material layer 14A, shown by a dotted line in Figure 4, and the permeation of the electrolyte solution 6 has been completed throughout the unpermeated electrode body 12, resulting in an electrode body 2 impregnated with the electrolyte solution 6 (for example, when the waiting time TT from the start of injection to the completion of permeation of the electrolyte solution 6 has elapsed), it is considered that the concentration of ethylene carbonate 6VE in the permeated electrolyte solution 6 located near the center line ML is relatively lower than that of the electrolyte solution 6 located outside (upper or lower in Figure 4) in the width direction WH rather than near the center line ML.
[0041] Here, the electrolyte 6 that permeates (advances) to the inner side WHI in the width direction WH along the negative electrode active material layer 14A has been described. However, the electrolyte 6 that permeates (advances) to the inner side WHI in the width direction WH along the positive electrode active material layer 13A of the non-permeated positive electrode plate 13 and the non-permeated separator 15 also causes non-uniformity in the concentration of ethylene carbonate 6VE in the electrolyte 6 due to differences in permeation speed. That is, when the electrolyte 6 is poured into the case 7 and permeates into the non-permeated electrode body 12, the amount of ethylene carbonate 6VE that reaches the vicinity of the center 2M in the axial direction XH of the electrode body 2 (see FIG. 3) impregnated with the electrolyte 6 tends to be small.
[0042] In particular, in the case where the electrode body 2 (unpermeated electrode body 12) has a width dimension AW of the negative electrode active material layers 4A and 14A of 180 mm or more (in the present embodiment, the width dimension AW=180 mm), the electrolyte solution 6 that has permeated from both ends 14AE1 and 14AE2 in the width direction WH of the negative electrode active material layer 14A must permeate (move) a distance EL of 90 mm or more along the negative electrode active material layer 14A before reaching the center line ML. Therefore, due to the difference in permeation speed with other solvents 6VL, the concentration of ethylene carbonate 6VE in the electrolyte solution 6 located near the center line ML becomes low, and the area density of ethylene carbonate 6VE present near the center line ML also becomes low.
[0043] In addition, when the electrolyte 6 permeated from both ends 14AE1, 14AE2 of the negative electrode active material layer 14A toward the inner side WHI reaches the vicinity of the center line ML and meets with each other, the electrolyte 6 does not move to the inner side WHI in the width direction WH by permeation thereafter. Therefore, it is considered that the unevenness in the concentration of the ethylene carbonate 6VE occurring between the electrolyte 6 located near the center line ML and the electrolyte 6 located outside (upper or lower in FIG. 4) in the width direction WH among the permeated electrolyte 6 is gradually eliminated by diffusion movement due to the concentration gradient of the ethylene carbonate 6VE. However, it is estimated that it takes longer to eliminate the unevenness in the concentration than the movement of the electrolyte 6 by permeation (for example, several days). For this reason, it is difficult to wait for a long time from the time when the electrolyte 6 has completely permeated the entire electrode body 2 until the unevenness in the concentration is eliminated before moving to the initial charge.
[0044] Therefore, if initial charging of the battery 1 is started immediately after the waiting time TT has elapsed until the electrolyte 6 has completely permeated the case 7, the initial charging will be performed in a state in which the concentration of ethylene carbonate 6VE in the electrode body 2 is uneven.
[0045] However, as described above, the ethylene carbonate 6VE contained in the electrolytic solution 6 serves as a raw material for forming the anode SEI coating 4AC around the anode active material particles 4AP constituting the anode active material layer 4A. For this reason, as described above, when the amount per unit area of the ethylene carbonate 6VE present in the vicinity of the center line ML of the anode active material layer 4A is small, the anode SEI coating 4AC derived from ethylene carbonate cannot be appropriately formed around the anode active material particles 4AP in the vicinity of the center line ML of the anode active material layer 4A, and this tends to cause problems such as an increase in the resistance of the battery 1.
[0046] In the battery 1 of this embodiment, as shown in Fig. 4, the negative electrode active material layer 14A of the non-permeated negative electrode plate 14 forming the non-permeated electrode body 12 is formed such that the central portion 14AM in the width direction WH, where the distance EL from both ends 14AE1, 14AE2 is equal to or greater than the additional portion distance ELF (in this embodiment, the additional portion distance ELF = 80 mm), is a strip-shaped additional negative electrode active material layer 14AF that contains a coating material CS in advance. On the other hand, the one side portion 14AS1 on one side WH1 in the width direction WH and the other side portion 14AS2 on the other side WH2 in the width direction WH are strip-shaped non-containing negative electrode active material layers 14AN1, 14AN2 that do not contain the coating material CS, as in the past. In this embodiment, ethylene carbonate CS1 is used as the coating material CS. This results in an unpermeated electrode body 12 having a coating material CS (ethylene carbonate CS1) that forms a negative electrode SEI coating 4AC on the negative electrode active material layer 4A pre-disposed in a central portion 12M in the axial direction XH.
[0047] To form the negative electrode active material layer 14A of the non-permeated negative electrode plate 14, the negative electrode active material layers 14AN1 and 14AN2 are formed using the same negative electrode paste PAN as before, which does not contain the film-forming material CS, as described later, while the additional negative electrode active material layer 14AF is formed in the central portion 14AM in the width direction WH using the additional negative electrode paste PAF containing the film-forming material CS. In this embodiment, the negative electrode paste PAN is a mixture of 99% by weight of graphite particles and 1% by weight of a binder (CMC) mixed with water as a solvent. The additional negative electrode paste PAF is the above-mentioned negative electrode paste PAN to which 5% by weight of ethylene carbonate CS1 is added as the film-forming material CS.
[0048] In this way, since the additional negative electrode active material layer 14AF is provided in the central portion 14AM of the negative electrode active material layer 14A, when the electrolyte 6 permeating from both ends 14AE1, 14AE2 in the width direction WH of the negative electrode active material layer 14A toward the inside WHI reaches the additional negative electrode active material layer 14AF, the electrolyte 6 further permeates toward the center line ML while the film-forming substance CS in the additional negative electrode active material layer 14AF is dissolved in the electrolyte 6. Therefore, even in the electrode body 2 in which the electrolyte 6 has completely permeated, the concentration of ethylene carbonate 6VE derived from the electrolyte 6 is reduced in the electrolyte 6 located near the center line ML of the negative electrode active material layer 14A, i.e., in the central portion 14AM. However, the electrolyte 6 in the central portion 14AM contains the film-forming substance CS (ethylene carbonate CS1) in the additional negative electrode active material layer 14AF.
[0049] Therefore, even if the initial charging step is performed in a state in which ethylene carbonate 6VE derived from the electrolyte 6 has not sufficiently reached the central portion 14AM as described above, the pre-deposited coating material CS can adequately form the anode SEI coating 4AC on the anode active material particles 4AP (see FIG. 2). Thus, it is possible to manufacture a battery 1 in which the non-uniformity of the formation of the anode SEI coating in the anode active material layer 4A is suppressed, the non-uniformity of the resistance of the anode active material layer 4A in the electrode body 2 is suppressed, and an increase in resistance is suppressed.
[0050] Particularly in this embodiment, ethylene carbonate CS1 is used as the film-forming substance CS. That is, ethylene carbonate CS1 is disposed in advance as the film-forming substance CS in the central portion 14AM of the negative electrode active material layer 14A where the ethylene carbonate 6VE derived from the electrolytic solution 6 is insufficient. Therefore, a negative electrode SEI film derived from ethylene carbonate can be appropriately formed over the entire negative electrode active material layer 4A without causing a shortage of ethylene carbonate in each portion of the negative electrode active material layer 4A.
[0051] Next, the manufacture of this battery 1 will be described with reference to Figures 5 to 7. First, in an electrode body forming step S1 (an example of an unpermeated electrode body forming step), a wound-type unpermeated electrode body 12 is formed that is not permeated with the electrolyte 6. More specifically, in an unpermeated negative electrode plate forming step S11 (an example of an additional negative electrode plate forming step), an unpermeated negative electrode plate 14 having a strip-shaped negative electrode active material layer 14A is formed.
[0052] More specifically, the central portion 14AM in the width direction WH of the strip-shaped negative electrode active material layer 14A is a strip-shaped additional negative electrode active material layer 14AF containing the coating-forming substance CS, while one side portion 14AS1 and the other side portion 14AS2 of the strip-shaped non-containing negative electrode active material layer 14AN1 and 14AN2 not containing the coating-forming substance CS are formed in the strip-shaped negative electrode active material layer 14A (see FIG. 4). As described above, in this embodiment, ethylene carbonate CS1 is used as the coating-forming substance CS.
[0053] In this unpermeated negative electrode plate formation step S11, the negative electrode active material-free layers 14AN1 and 14AN2 are formed using the negative electrode paste PAN that contains the negative electrode active material particles 14AP and a binder but does not contain the film-forming material CS, while the additional negative electrode paste PAF that contains the negative electrode active material particles 4AP and the film-forming material CS is used to form the additional negative electrode active material layer 14AF.
[0054] Specifically, in the coating step S111, as shown in Fig. 6, a wide negative electrode paste layer 24AT is coated on a wide negative electrode foil 24F wound around a backup roll BR1 and having a width twice that of the negative electrode foil 4F of the negative electrode plate 4, using a die coater DC. More specifically, in the die coater DC, the uncontaining negative electrode paste PAN is stored in a storage tank DCT1, and the additional negative electrode paste PAF is stored in a storage tank DCT2. Using a die DCD provided with a plurality of partitions (not shown), the uncontaining negative electrode paste PAN supplied from the storage tank DCT1 and the additional negative electrode paste PAF supplied from the storage tank DCT2 are discharged in a stripe shape from a slit DCS of the die DCD, and coated on the wide negative electrode foil 24F wound around the backup roll BR1 (see Fig. 7). Specifically, a wide negative electrode paste layer 24AT having a width twice that of the negative electrode foil 14F is applied to both sides of the wide negative electrode foil 24F, leaving a portion to be the current collector 14S of the non-permeated negative electrode plate 14. The wide negative electrode paste layer 24AT is formed symmetrically with respect to the cutting center line CL shown by the dashed line in FIG. 7, and is applied in a five-stripe pattern in which two additional negative electrode paste layers 24ATF are interposed between three non-containing negative electrode paste layers 24ATN. The non-containing negative electrode paste layer 24ATN becomes the non-containing negative electrode active material layers 14AN1 and 14AN2 of the negative electrode active material layer 14A after drying and cutting as described below. The additional negative electrode paste layer 24ATF becomes the additional negative electrode active material layer 14AF after drying and cutting.
[0055] Thereafter, in a drying step S112, the wide negative electrode paste layer 24AT applied to the wide negative electrode foil 24F is dried in a drying oven DR to form a wide negative electrode active material layer 24A. The application step S111 and the drying step S112 are repeated for the front and back sides of the wide negative electrode foil 24F to form a wide unpermeated negative electrode plate 24 in which the wide negative electrode active material layer 24A is provided on both sides of the wide negative electrode foil 24F. FIG. 6 shows the application and drying of the wide negative electrode paste layer 24AT to a wide single-sided negative electrode plate 24S in which the wide negative electrode active material layer 24A is provided on one side of the wide negative electrode foil 24F.
[0056] Furthermore, in a cutting step S113, the wide unpermeated negative electrode plate 24 having the wide negative electrode active material layer 24A provided on both sides of the wide negative electrode foil 24F is cut along a cutting center line CL (see FIG. 7) to form two strip-shaped unpermeated negative electrode plates 14. Thereafter, the unpermeated negative electrode plates 14 are sorted by a sorting roll FR and wound up on winding rolls SR1 and SR2, respectively. Thus, the unpermeated negative electrode plate forming step S11 obtains the unpermeated negative electrode plate 14 (see FIG. 4).
[0057] Next, in a winding step S12, the unpermeated negative electrode plate 14 is wound together with a separately formed unpermeated positive electrode plate 13 and an unpermeated separator 15 to form a cylindrical wound-type electrode body (not shown). Furthermore, in a flattening step S13, this cylindrical electrode body is pressed to form a plate-like flat wound-type unpermeated electrode body 12 (see FIG. 3). Thus, the unpermeated electrode body 12 is obtained by the electrode body forming step S1.
[0058] Thereafter, in the accommodation step S2, the unpermeated electrode body 12 is accommodated in the case 7. Specifically, first, in a terminal connection step S21, the positive electrode current collector 12P of the unpermeated electrode body 12 is welded to the inside connection portion 8PI of the positive electrode terminal 8P fixed to the lid body 7L via the insulating member 9, and similarly, the positive electrode current collector 12P is welded to the inside connection portion 8NI of the negative electrode terminal 8N, respectively, to fix the unpermeated electrode body 12 to the lid body 7L via the positive electrode terminal 8P and the negative electrode terminal 8N (see FIG. 1).
[0059] In the subsequent insertion step S22, a bag-shaped resin cover (not shown) made of a resin film is placed over the unpermeated electrode body 12, and the unpermeated electrode body 12 is inserted into the case body 7H, and the case body 7H is sealed with the lid body 7L. Furthermore, in a sealing step S23, the periphery of the lid body 7L is hermetically welded and sealed to the case body 7H by laser welding all around. Thus, the unpermeated electrode body 12 is accommodated in the case 7 by the accommodation step S2.
[0060] Thereafter, in the liquid injection step S3, a predetermined amount of electrolyte 6 is injected into the case 7 through the liquid injection hole 7LH of the lid 7L. As a result, as described above, the electrolyte 6 is impregnated into the unpermeated electrode body 12 in the case 7. Note that in the liquid injection step S3, the electrolyte 6 is injected in a predetermined injection pattern. Furthermore, prior to the injection, the unpermeated battery 1 may be placed in a chamber and the pressure may be reduced or pressurized while the electrolyte 6 is impregnated into the unpermeated electrode body 12.
[0061] In the waiting step S4, it is waited until a predetermined waiting time TT has elapsed from the start of the injection. The waiting time TT is the time from the start of the injection until the electrolyte 6 has permeated the entire inside of the unpermeated electrode body 12 (until the electrode body 2 is impregnated with the electrolyte 6), and this waiting time TT is obtained in advance by disassembling battery samples with different elapsed times from the start of the injection and observing the permeation state of the electrolyte 6, for example.
[0062] After the waiting time TT has elapsed, the process proceeds to an initial charging step S5, in which a power source (not shown) is connected to the positive electrode terminal 8P and the negative electrode terminal 8N, and a voltage is applied to the electrode body 2 of the battery 1 through the positive electrode terminal 8P and the negative electrode terminal 8N to perform initial charging. That is, a voltage is applied between the positive electrode plate 3 and the negative electrode plate 4 of the electrode body 2 in a predetermined initial charging pattern, and a negative electrode SEI coating 4AC is formed on the negative electrode active material layer 4A of the negative electrode plate 4 (see FIG. 2). In this embodiment, initial charging is performed in an initial charging pattern of 0.5C-CCCV charging (SOC 90%). Thereafter, the liquid injection hole 7LH is sealed with the liquid injection plug 7P.
[0063] As described above, in the battery 1 of this embodiment, the additional negative electrode active material layer 14AF is provided in the central portion 14AM of the negative electrode active material layer 14A of the unpermeated negative electrode plate 14 of the unpermeated electrode body 12. Therefore, in the electrode body 2 in which the waiting time TT has elapsed and the electrolyte 6 has permeated the entire unpermeated electrode body 12, it is possible to prevent a decrease in the area density of ethylene carbonate present near the center line ML of the negative electrode active material layer 4A of the negative electrode plate 4. Therefore, in the initial charging step S5, the negative electrode SEI coating 4AC can be appropriately formed on the negative electrode active material particles 4AP at any location of the negative electrode active material layer 4A.
[0064] Next, in a high-temperature aging step S6, the battery 1 is subjected to high-temperature aging by being left in an environment of 60° C. for 20 hours, and in an inspection step S7, the battery 1 is inspected, and the battery 1 is completed.
[0065] (Comparative forms 1 and 2) To compare with the battery 1 according to the embodiment, batteries 1C1 and 1C2 according to comparative embodiments 1 and 2 were also manufactured and examined as described below. First, the manufacture of the batteries 1C1 and 1C2 according to comparative embodiments 1 and 2 will be described with reference to FIGS.
[0066] The battery 1C1 according to the comparative embodiment 1 is a battery similar to the conventional battery. In the battery 1 of the embodiment, the non-permeated electrode body 12 was formed using the non-permeated negative electrode plate 14 in which the additional negative electrode active material layer 14AF was provided in the central portion 14AM of the negative electrode active material layer 14A, and the electrolyte 6 was impregnated. In contrast, in the battery 1C1 of the comparative embodiment 1, as shown in FIG. 8, the additional negative electrode active material layer 14AF was not provided in the negative electrode active material layer 14A, and the entire negative electrode active material layer 14A was made into the non-permeated negative electrode plate 14C1 in which the non-containing negative electrode active material layer 14AN that does not contain the coating material CS was formed. Then, the non-permeated electrode body 12C1 was formed using this non-permeated negative electrode plate 14C1. The rest was the same as the battery 1 of the embodiment 1, and the initial charging step S5 and the high-temperature aging step S6 were also performed in the same manner to obtain the battery 1C1 of the comparative embodiment 1.
[0067] On the other hand, the battery 1C2 according to the comparative embodiment 2 is a battery opposite to the non-permeated negative electrode plate 14C1 of the battery 1C1 of the comparative embodiment 1. That is, as shown in FIG. 9, the non-permeated negative electrode plate 14C2 was formed in which the negative electrode active material layer 14A was not provided with a non-containing negative electrode active material layer 14AN that did not contain a film-forming material CS, and the entire negative electrode active material layer 14A was made into an additional negative electrode active material layer 14AF that contained a film-forming material CS (ethylene carbonate CS1), and the non-permeated negative electrode plate 14C2 was used to form the non-permeated electrode body 12C2. The rest was the same as the battery 1 of the embodiment 1, and the initial charging step S5 and the high-temperature aging step S6 were also performed in the same manner to obtain the battery 1C2 of the comparative embodiment 2.
[0068] (Ethylene carbonate content survey) The manufactured batteries 1, 1C1, and 1C2 are disassembled in a glove box with an inert atmosphere, and the electrode bodies 2, 2C1, and 2C2 are taken out. Furthermore, the electrode bodies 2, 2C1, and 2C2 are unwound, and the negative electrode plate 4 is taken out and left to dry. The middle part of the winding (approximately the center in the longitudinal direction LH) of each negative electrode plate 4, and the parts corresponding to the inspection positions I, II, III, IV, and V in FIG. 10 are cut out to a size of 20 x 20 mm to obtain a total of 15 types of negative electrode samples for extraction. Each negative electrode sample for extraction is immersed in an extraction solvent to extract ethylene carbonate, and NMR measurements are performed on a standard solution with a known ethylene carbonate concentration and each extraction solution, and the content of ethylene carbonate contained in each extraction solution is calculated from the ratio of the detection intensity of ethylene carbonate in the standard solution and the extraction solution. Furthermore, in each of the electrode assemblies 2, 2C1, and 2C2, the ethylene carbonate content obtained at the inspection position I was defined as 100%, and the relative EC content (%) at each of the inspection positions I to V was obtained.
[0069] As shown in FIG. 10, the inspection positions I, II, III, IV, and V are flat plate-shaped portions of the negative electrode active material layer 4A of the negative electrode plate 4 in each electrode body 2, 2C1, and 2C2, and are arranged in the axial direction XH. The distances EL measured from the edge 4AE2 (see FIG. 4) of the current collector 4S side that becomes the negative electrode current collector 2N to the inner side XHI in the axial direction XH (inner side WHI in the width direction WH) are the distances EL1, EL2, EL3, EL4, and EL5, respectively (in the present embodiment, specifically, EL1=10 mm, EL2=30 mm, EL3=50 mm, EL4=70 mm, and EL5=90 mm). The inspection position V is a position on the center line ML of the negative electrode active material layer 4A. That is, the distance EL5 is 1 / 2 the width dimension AW (AW=180 mm in the present embodiment, etc.) of the negative electrode active material layer 4A in the width direction WH.
[0070] The results are shown in the graph of Figure 11. In the electrode body 2C1 of the battery 1C1 of Comparative Form 1, indicated by the thick dashed line, the content of ethylene carbonate 6VE gradually decreases generally from inspection position I to inspection position IV, that is, from the edge 4AE2 to the inner side XHI in the axial direction XH. However, at inspection position V, that is, at the central portion 2M in the axial direction XH of the electrode body 2C1 (see Figure 3), it is found that the content of ethylene carbonate 6VE is significantly reduced (in this Comparative Form 1, the content is reduced by approximately 30% compared to inspection position I).
[0071] This is believed to be due to the following reasons. As described above, the permeation speed of the ethylene carbonate 6VE contained in the electrolyte 6 is slower than that of other solvents 6VL (specifically, DMC, EMC). For this reason, it is believed that the greater the distance EL from the end edge 4AE2 to the inspection position V, the lower the concentration of the ethylene carbonate 6VE in the electrolyte 6 located at the tip of the permeation, among the electrolyte 6 permeating into the electrode body 2C1. In particular, when the distance EL exceeds 80 mm, the concentration of the ethylene carbonate 6VE decreases significantly. Moreover, in the vicinity of the inspection position V located on the center line ML of the negative electrode active material layer 4A, that is, in the central portion 2M of the electrode body 2C1, the electrolyte 6 that permeates from both end edges 4AE1, 4AE2 (see FIG. 8) of the negative electrode active material layer 4A to the inner side WHI in the width direction WH (the inner side XHI in the axial direction XH) meets and stops permeating, so that the content (area density) of the ethylene carbonate 6VE that reaches the central portion 2M tends to remain low.
[0072] On the other hand, in the electrode body 2C2 of the battery 1C2 of Comparative Form 2, indicated by a thick dashed dotted line, the ethylene carbonate content is maintained at a high value of nearly 100% from inspection position I to inspection position IV. In particular, the ethylene carbonate content is slightly higher at inspection positions II and III than at inspection position I near the edge 4AE2 of the outer side WHO in the width direction WH. However, at inspection position IV, the ethylene carbonate content is slightly reduced. However, at inspection position V, i.e., at the central portion 2M in the axial direction XH of the electrode body 2C1 (see FIG. 9), it is found that the ethylene carbonate content is significantly reduced (approximately 35% reduced compared to inspection position I in Comparative Form 2).
[0073] This is believed to be due to the following reason. The electrode body 2C2 of the battery 1C2 of Comparative Form 2 uses an unpermeated negative electrode plate 14C2 in which the entire negative electrode active material layer 14A is made of an additional negative electrode active material layer 14AF containing a coating-forming material CS (specifically, ethylene carbonate CS1). For this reason, in the range from the investigation positions I to III where the distance EL from the edge 4AE2 is relatively small, the decrease in concentration due to the slow permeation speed of ethylene carbonate 6VE contained in the electrolyte solution 6 (see the graph of Comparative Form 1) is compensated for by the dissolution of ethylene carbonate CS1 derived from the additional negative electrode active material layer 14AF in the electrolyte solution 6, and rather the concentration of ethylene carbonate increases with the permeation of the electrolyte solution 6.
[0074] However, as described above, the ethylene carbonate dissolved in the electrolyte solution 6 has a slower permeation rate and a higher viscosity than other solvents 6VL (specifically, DMC and EMC). Therefore, when the concentration of ethylene carbonate dissolved in the electrolyte solution 6 increases near the investigation positions II and III, the increase in viscosity causes the permeation rate of the ethylene carbonate to decrease rapidly, and the concentration of ethylene carbonate in the electrolyte solution 6 reaching the investigation position V decreases significantly. Therefore, even if the ethylene carbonate CS1 derived from the additional negative electrode active material layer 14AF near the investigation position V compensates, it is presumed that it cannot fully compensate for the large decrease in the ethylene carbonate content at the investigation position V, i.e., the central portion 2M.
[0075] In contrast, in the battery 1 (electrode body 2) of this embodiment shown by the thick solid line, the ethylene carbonate content gradually decreases at the inspection positions I to IV, generally similar to the battery 1C1 of Comparative Form 1, from inspection position I to inspection position IV, i.e., from the edge 4AE2 to the inner side XHI in the axial direction XH. However, unlike the battery 1C1 of Comparative Form 1, the ethylene carbonate content at inspection position V in the battery 1 of this embodiment is approximately the same as that at inspection position IV. That is, in the electrode body 2 of the battery 1 of this embodiment, the decrease in the ethylene carbonate content at the central portion 2M in the axial direction XH (see FIG. 3) is suppressed. Specifically, in this embodiment, the decrease in the content at inspection position V compared to inspection position I remains approximately 10% or less.
[0076] This is believed to be due to the following reason. In the electrode body 2 of the battery 1 of this embodiment, an unpermeated negative electrode plate 14 is used in which an additional negative electrode active material layer 14AF containing a film-forming substance CS (specifically, ethylene carbonate CS1) is formed only in a central portion 14AM of the negative electrode active material layer 14A, the central portion being at a distance EL of 80 mm or more including the inspection position V (see FIG. 4). For this reason, in the range from the inspection positions I to IV, it is believed that the decrease in concentration occurred due to the slow permeation speed of ethylene carbonate 6VE derived from the electrolyte solution 6, as in Comparative Form 1.
[0077] However, as described above, when the permeated electrolyte solution 6 reaches the additional negative electrode active material layer 14AF in the central portion 14AM of the negative electrode active material layer 14A, the ethylene carbonate CS1 originating from the additional negative electrode active material layer 14AF dissolves in and replenishes the electrolyte solution 6. This is thought to have allowed the ethylene carbonate content at the investigation position V to be kept at the same level as at the investigation position IV.
[0078] (IV resistance value survey) In order to study the effect of the difference in ethylene carbonate concentration on the battery characteristics, the following investigation was also carried out. The manufactured batteries 1, 1C1, and 1C2 were charged to SOC 50%, disassembled in a glove box under an inert atmosphere, and the electrode bodies 2, 2C1, and 2C2 were taken out. Furthermore, the electrode bodies 2, 2C1, and 2C2 were unwound, and the positive electrode plate, the negative electrode plate facing it, and the separator sandwiched between them were cut out in the middle of the winding and in the areas corresponding to the investigation positions I, III, and V in FIG. 10, each with a size of 20×20 mm, to obtain a total of nine small cell samples consisting of a small positive electrode plate, a small negative electrode plate, and a small separator. These were washed and dried with EMC, stacked with a small separator sandwiched between the small positive electrode plate and the small negative electrode plate, surrounded by a laminate film, and new electrolyte 6 was poured in and sealed to form a new small cell (not shown).
[0079] For the small cells (total of nine types) corresponding to the investigation positions I, III, and V of each electrode body 2, 2C1, and 2C2, constant current discharge was performed with current A at a magnitude equivalent to discharge current rates of 0.2C, 0.5C, 1C, and 2C in an environment of 25°C, and the voltage drop ΔV was obtained after 10 seconds. The obtained data was plotted on a graph with current A on the X-axis and voltage drop ΔV on the Y-axis, and the slope of the approximated straight line was taken as the IV resistance value of each small cell (IV resistance = voltage drop ΔV / current A). Furthermore, for each form, the relative IV resistance value of the small cells at each investigation position I, III, and V was obtained, with the IV resistance value obtained for the small cell at investigation position I set to 100%.
[0080] The results are shown in the graph of Figure 12. Among the small cells of electrode body 2C1 of battery 1C1 of comparative form 1, indicated by the thick dashed line, the small cells at inspection positions I and III had almost the same relative IV resistance value. However, it can be seen that the small cell at inspection position V had a significantly increased relative IV resistance value compared to the small cells at inspection positions I and III (in comparative form 1, an increase of approximately 18% compared to inspection position I).
[0081] This is believed to be due to the following reasons. As described above, the ethylene carbonate content does not change much at the check positions I to III in the electrode body 2C1 of the battery 1C1 of Comparative Form 1 (see FIG. 11). Specifically, the content at check positions II and III is reduced by at most about -7% compared to check position I. For this reason, when the battery 1C1 of Comparative Form 1 is initially charged in the initial charge step S5, the negative electrode SEI coating 4AC derived from ethylene carbonate is appropriately formed on the negative electrode active material particles 4AP in the negative electrode active material layer 4A of the negative electrode plate 4 near the check positions I and III. It is believed that this resulted in the relative IV resistance values being approximately the same in the small cells using the small positive electrode plate, small negative electrode plate, and small separator at the check positions I and III.
[0082] However, as described above, the ethylene carbonate content was significantly reduced (-28%) at the examination position V of the electrode body 2C1. Therefore, in the negative electrode active material layer 4A of the negative electrode plate 4 after the initial charge, near the examination position V, i.e., near the center line ML (see FIG. 10), the negative electrode SEI coating 4AC derived from ethylene carbonate cannot be sufficiently formed on the negative electrode active material particles 4AP. Therefore, it is considered that the relative IV resistance value of the small cell using the small positive electrode plate, small negative electrode plate, and small separator at the examination position V was 18% higher than that of the small cell at the examination position I. From this, it can be seen that the IV resistance value is locally high at the center portion 2M in the electrode body 2C1 of the battery 1C1 of Comparative Form 1, and the IV resistance value is also high in the electrode body 2C1 as a whole.
[0083] In the electrode body 2C2 of the battery 1C2 of Comparative Form 2 shown by the thick dashed dotted line, the small cells at the inspection positions I and III had almost the same relative IV resistance values. However, it can be seen that the small cell at the inspection position V had a significantly increased relative IV resistance value compared to the small cells at the inspection positions I and III (in Comparative Form 2, an increase of approximately 24% compared to inspection position I).
[0084] This is believed to be due to the following reasons. As described above, at the examination positions I to III in the electrode body 2C2 of the battery 1C2 of the comparative embodiment 2, the content of ethylene carbonate in the electrolyte 6 hardly changes (see FIG. 11). For this reason, when the battery 1C2 of the comparative embodiment 2 is initially charged in the initial charge step S5, the negative electrode SEI coating 4AC derived from ethylene carbonate is appropriately formed on the negative electrode active material particles 4AP in the negative electrode active material layer 4A of the negative electrode plate 4 near the examination positions I and III. As a result, it is believed that the relative IV resistance values became approximately the same in the small cells using the small positive electrode plate, small negative electrode plate, and small separator at the examination positions I and III.
[0085] However, as described above, the ethylene carbonate content was significantly reduced (-36%) at the examination position V of the electrode body 2C2. Therefore, in the negative electrode active material layer 4A of the negative electrode plate 4 after the initial charge, near the examination position V, i.e., near the center line ML (see FIG. 10), the negative electrode SEI coating 4AC derived from ethylene carbonate cannot be sufficiently formed on the negative electrode active material particles 4AP. As a result, it is considered that the relative IV resistance value of the small cell using the small positive electrode plate, small negative electrode plate, and small separator at the examination position V was 24% higher than that of the small cell at the examination position I. From this, it can be seen that the IV resistance value is locally high at the center portion 2M in the electrode body 2C2 of the battery 1C2 of the comparative embodiment 2, and the IV resistance value of the electrode body 2C2 as a whole is also high.
[0086] In contrast, in the battery 1 (electrode body 2) of this embodiment indicated by the thick solid line, no significant change occurs in the relative IV resistance value at any of the investigation positions I, III, and V.
[0087] This is believed to be due to the following reasons. As described above, in the electrode body 2 of the battery 1 of this embodiment, the content of ethylene carbonate contained in the electrolyte 6 is not so low not only at the inspection positions II to IV but also at the inspection position V, as compared to the inspection position I (see FIG. 11). Specifically, the content at the inspection position V is only -9% lower than the inspection position I. Therefore, when the battery 1 of this embodiment is initially charged in the initial charging step S5, the negative electrode SEI coating 4AC derived from ethylene carbonate can be appropriately formed on the negative electrode active material particles 4AP of the negative electrode plate 4 not only near the inspection positions I and III but also near the inspection position V. Therefore, it is believed that the relative IV resistance values of the small cells using the small positive electrode plate, small negative electrode plate, and small separator at the inspection positions I, III, and V are approximately the same. This shows that the electrode body 2 of the battery 1 of this embodiment can suppress uneven formation of the negative electrode SEI coating in the negative electrode active material layer 4A in the wound electrode body 2, and the IV resistance value does not become locally high in the central portion 2M, and an increase in the IV resistance value can be suppressed in the entire electrode body 2. That is, it is seen that the battery 1 of this embodiment has a lower IV resistance than the batteries 1C1 and 1C2 of the comparative embodiments 1 and 2.
[0088] Although the present invention has been described above based on the embodiment, the present invention is not limited to the embodiment, and can be appropriately modified and applied within the scope of the gist of the present invention. For example, in the embodiment, in addition to the uncontaining negative electrode paste PAN as in the past, an additional negative electrode paste PAF containing a film-forming material CS was prepared, and applied to the wide negative electrode foil 24F at once with a die coater DC to form an additional negative electrode paste layer 24ATF and an uncontaining negative electrode paste layer 24ATN, which were then dried and cut to form an unpermeated negative electrode plate 14 having an additional negative electrode active material layer 14AF and uncontaining negative electrode active material layers 14AN1 and 14AN2. However, it is also possible to first apply the additional negative electrode paste PAF to the wide negative electrode foil 24F to form the additional negative electrode paste layer 24ATF, and then apply the non-containing negative electrode paste PAN to the wide negative electrode foil 24F to form the non-containing negative electrode paste layer 24ATN, which is then dried and cut to form the unpermeated negative electrode plate 14 having the additional negative electrode active material layer 14AF and the non-containing negative electrode active material layers 14AN1, 14AN2.
[0089] Conversely, the unpermeated negative electrode plate 14 may be formed by applying the unpermeated negative electrode paste PAN to the wide negative electrode foil 24F to form the unpermeated negative electrode paste layer 24ATN, and then applying the additional negative electrode paste PAF to form the additional negative electrode paste layer 24ATF, which is then dried and cut.
[0090] Alternatively, only the uncontaining negative electrode paste PAN is applied to the wide negative electrode foil 24F in the same manner as before, and dried to form an uncontaining negative electrode active material layer, and then a separately prepared solution containing a coating material CS (a solution of water, alcohol, organic solvent, etc.) is applied to a band-shaped portion that will become the central portion 14AM of the negative electrode active material layer 14A, dried, and cut to form an unpermeated negative electrode plate 14. Alternatively, after applying only the non-containing negative electrode paste PAN, a solution containing the coating material CS can be applied before drying or when it is semi-dried, and then the non-containing negative electrode paste PAN and the solution can be dried and cut to form the non-permeated negative electrode plate 14.
[0091] In addition, for example, in the embodiment, a strip-shaped additional negative electrode active material layer 14AF containing a coating film forming material CS is formed in the central portion 14AM in the width direction WH of the negative electrode active material layer 14A of the unpermeated negative electrode plate 14 constituting the unpermeated electrode body 12. Alternatively, a strip-shaped additional layer containing the coating material CS may be formed in the center portion in the width direction WH of the unpermeated separator 15 constituting the unpermeated electrode body 12, i.e., in the portion facing the center portion 14AM in the width direction WH of the negative electrode active material layer 14A. This strip-shaped additional layer may be formed by applying a solution containing the above-mentioned coating material CS to the unpermeated separator 15. Furthermore, a strip-shaped additional positive electrode active material layer containing the coating material CS may be formed in the central portion in the width direction WH of the positive electrode active material layer 13A of the unpermeated positive electrode plate 13 constituting the unpermeated electrode body 12. Furthermore, the unpermeated electrode body 12 may be formed by combining two or all of the three components: the unpermeated negative electrode plate 14 containing the coating-forming substance CS, the unpermeated separator 15, and the unpermeated positive electrode plate 13. [Explanation of symbols]
[0092] 1, 1C1, 1C2 battery (energy storage device) 2,2C1,2C2 electrode body 2M central part 3 Positive plate 4 Negative plate 4A negative electrode active material layer AW (negative electrode active material layer) width dimension 4AE1,4AE2 (widthwise) edges 4AP negative electrode active material particles 4AC negative electrode SEI coating 5. Separator 6 Electrolyte 6V Organic Solvent 6VE Ethylene Carbonate 6VL Other Solvents 7 Cases 12,12C1,12C2 Unpenetrated electrode body 12M central part 13 Unpermeated positive plate 14 Unpermeated negative plate (additional negative plate) 14C1,14C2 Non-penetrated negative electrode plate 14N negative electrode part 14A Anode active material layer 14AE1, 14AE2 (widthwise) edges ML Centerline 14AM Central part 14AS1 One side part (edge side part) 14AS2 Other side part (edge side part) CS film forming substance CS1 Ethylene Carbonate EL Distance 14AF Additional negative electrode active material layer 14AN1, 14AN2, 14AN Negative electrode active material layer-free 14AP Negative electrode active material particles PAF Additional negative electrode paste PAN Negative electrode paste-free AX Winding axis XH Axis direction XH1 One side XH2 The other side XHI Inner side XHO Outer side WH Width direction WH1 One side WH2 The other side WHI Inner side WHO Outer side S1 Electrode body forming process (unpenetrated electrode body forming process) S11 Unpenetrated negative electrode plate forming process (additional negative electrode plate forming process) S2 Accommodation process S3 Liquid injection process S4 Standby process TT Standby time S5 Initial charging process
Claims
1. an electrolyte solution containing ethylene carbonate and a solvent having a melting point lower than that of ethylene carbonate; a wound electrode body having a strip-shaped positive electrode plate, a strip-shaped negative electrode plate having a strip-shaped negative electrode active material layer, and a strip-shaped separator, the electrolyte being permeated into the inside; A case that accommodates the electrode body and the electrolyte, The electrode body has a width dimension of the negative electrode active material layer of 180 mm or more. A method for manufacturing an electricity storage device, comprising: an unpermeated electrode body forming step of forming a wound-type unpermeated electrode body that is not permeated with the electrolyte; a housing step of housing the unpermeated electrode body in the case; a liquid injection step of injecting the electrolyte into the case containing the non-permeated electrode body; a waiting step of waiting for a predetermined waiting time to elapse after the injection step, during which the electrolyte is permeated into the entire unpermeated electrode body; and an initial charging step of performing an initial charging step of forming a negative electrode SEI coating on the negative electrode active material layer after the waiting step, The non-permeated electrode body forming step includes: a step of forming an unpermeated electrode body in which a coating material for forming the negative electrode SEI coating on the negative electrode active material layer is previously disposed in a central portion of the unpermeated electrode body in the axial direction. A method for manufacturing an electricity storage device.
2. A method for producing the electricity storage device according to claim 1, comprising the steps of: The non-permeated electrode body forming step includes: The method includes the step of forming an additional negative electrode plate in which the central portion in the width direction of the strip-shaped negative electrode active material layer is a strip-shaped additional negative electrode active material layer containing the film-forming material, while the edge portions on both sides in the width direction are strip-shaped negative electrode active material layers not containing the film-forming material. A method for manufacturing an electricity storage device.
3. A method for producing the electricity storage device according to claim 2, comprising the steps of: The additional negative electrode plate forming step includes: The negative electrode active material layer is formed using a negative electrode paste containing negative electrode active material particles 1 but not containing the coating material, The additional negative electrode active material layer is formed using an additional negative electrode paste containing the negative electrode active material particles 1 and the film forming material. A method for manufacturing an electricity storage device.
4. A method for producing the electricity storage device according to claim 2 or 3, comprising the steps of: The additional negative electrode plate forming step includes: The central portion of the strip-shaped negative electrode active material layer, which is spaced apart from both end edges in the width direction by 80 mm or more, is defined as the additional negative electrode active material layer. A method for manufacturing an electricity storage device.
5. A method for producing the electricity storage device according to any one of claims 1 to 3, comprising the steps of: The film-forming material is ethylene carbonate. A method for manufacturing an electricity storage device.
Citation Information
Patent Citations
Nonaqueous secondary battery
JP1999144711A
Nonaqueous electrolyte secondary battery and manufacturing method thereof
JP2013182712A
Method for manufacturing nonaqueous electrolyte secondary battery
JP2014157748A
Negative electrode for secondary battery and manufacturing method therefor, and secondary battery using the same
JP2015018775A
Secondary battery and manufacturing method for secondary battery
JP2022127950A