Method for manufacturing hollow member

The method of extruding and rapidly cooling hollow members within a cooling means addresses the challenge of achieving both high strength and precision by refining crystal grains and restraining the inner surface, resulting in improved structural integrity and accuracy.

JP2024134927APending Publication Date: 2024-10-04RINASCIMETALLI
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023045379
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing methods for manufacturing hollow members, such as hollow pipes, fail to achieve both high strength and high precision due to issues like buckling during shearing and insufficient molding accuracy.

Method used

A method involving extruding a metal body to a predetermined temperature range, followed by rapid cooling using a cooling means within the hollow part to refine crystal grains and restrain the inner surface, thereby achieving both high strength and precision.

Benefits of technology

The method results in finer crystal grains, preventing coarsening and excessive shrinking, leading to improved strength and precision of the hollow members.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134927000001_ABST
    Figure 2024134927000001_ABST
Patent Text Reader

Abstract

To provide a method for manufacturing an aluminum pipe with which it is possible to achieve high accuracy as well as high strength.SOLUTION: After a hollow billet 2 composed of A6061 is extruded at 530°C, a hollow pipe 7 is shrunk by spraying cooling air to the hollow pipe 7, and is then quickly cooled by bringing the hollow pipe 7 into contact with a cooling punch 10. Thereafter, the hollow pipe is air-cooled by being held at 180°C for 12-18 hours.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a hollow member, and more particularly to a method for manufacturing a hollow member that can achieve high strength and high precision. [Background technology]

[0002] Hollow members (hollow pipes, etc.) made of aluminum alloys are used in automobile frames, aircraft and drone frames, bicycle frames, etc. Hollow members (hollow pipes, etc.) made of steel materials are used in side impact beams and steering wheels for automobiles, suspension-related parts for automobiles, etc.

[0003] In order to reduce the size and weight of structural components for automobiles and aircraft, there is a demand for these hollow components to have even higher strength.

[0004] Meanwhile, because grain refinement of metallic materials can significantly improve properties such as strength, many grain refinement processes utilizing large strains have been developed and proposed. The inventor of the present invention has also proposed a method for improving the strength of a metal body by refining the metal structure (see Patent Document 1). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2004 / 028718 Summary of the Invention [Problem to be solved by the invention]

[0006] Although the strength of the metal body can be improved by the crystal grain refinement using the processing method described in the above-mentioned Patent Document 1, the forming precision is not sufficient for application to hollow members. In other words, when an apparatus for realizing the processing method described in Patent Document 1 (for example, the SVSP apparatus shown in FIG. 9 of Patent Document 1) is provided in a downstream portion of an apparatus for forming a hollow member (a specific molding apparatus for performing extrusion molding, etc.), buckling occurs when the low deformation resistance region formed in the hollow member is subjected to shear deformation, and the method is not sufficient in terms of molding accuracy.

[0007] The present invention has been made in view of the above-mentioned points, and an object of the present invention is to provide a method for manufacturing a hollow member which is capable of realizing high precision as well as high strength. [Means for solving the problem]

[0008] In order to achieve the above-mentioned object, the manufacturing method of the hollow member of the present invention includes a processing step of extruding a metal body heated to a predetermined temperature range to form a hollow member, and then cooling the metal body from the predetermined temperature range by contacting the metal body with a cooling means located within the hollow portion of the hollow member.

[0009] Here, by bringing the metal body into contact with the cooling means, heat is transferred from the metal body to the cooling means by thermal conduction, and the metal body can be rapidly cooled. By rapidly cooling the metal body, the residual heat of the metal body can be used to prevent the recrystallized structure (fine-grained structure) from becoming coarse, and the crystal grains can be refined.

[0010] In order to achieve fine crystal grains, it is necessary to bring the metal body into contact with a cooling means and cool (quench) it before the structure (fine-grained structure) recrystallized by the residual heat of the metal body becomes coarse due to further residual heat of the metal body.

[0011] In addition, by bringing the metal body into contact with the cooling means located inside the hollow portion, the inner surface of the hollow member can be restrained by the cooling means. By restraining the inner surface of the hollow member, it is possible to prevent the metal body from shrinking excessively due to cooling (quenching), thereby improving the molding accuracy.

[0012] That is, by bringing the metal body into contact with the cooling means, it is possible to realize high strength by making the crystal grains finer, and high precision by restricting the inner surface of the hollow member.

[0013] In this case, the "predetermined temperature range" is a temperature range in which the metal body can be extruded to form a hollow member, but if the metal body is a heat-treatable alloy, heating up to the solution temperature range will achieve a supersaturated solid solution of the elements, thereby achieving even greater strength.

[0014] In addition, it is preferable to cool the device from a predetermined temperature range by placing the cooling means in the hollow portion of the hollow member with a predetermined gap therebetween, contracting the metal body, and bringing the metal body into contact with the cooling means. In this case, the structure of the cooling means can be simplified, and the device as a whole can be made smaller and less expensive.

[0015] In other words, since the hollow member inevitably shrinks when cooled, by adopting a cooling means that does not come into contact before shrinkage (when the diameter of the hollow portion is large) but comes into contact after shrinkage (when the diameter of the hollow portion is small), there is no need to change the size of the cooling means, and as described above, the structure of the cooling means can be simplified.

[0016] In addition, when the metal body is contracted by supplying cooling air to it (when the metal body is contracted to bring it into contact with the cooling means), corrosion of the metal body can be suppressed more effectively than when a liquid (such as water) is supplied.

[0017] Furthermore, when the metal body is made of a heat-treatable aluminum alloy and the processing step involves extruding the heat-treatable aluminum alloy heated to the solution temperature range and then cooling it from the solution temperature range at a rate at which the dissolved elements do not precipitate, high strength is achieved due to the supersaturated solid solution of the elements.

[0018] That is, in the processing step, elements can be dissolved in the matrix by heating to the solution temperature range, and a supersaturated solution of the elements is realized. Then, by cooling from the solution temperature range at a rate at which the dissolved elements do not precipitate (in other words, at a rate at which the dissolved elements cannot diffuse), high strength is realized without problems such as coarsening.

[0019] If the cooling rate is slow, the elements dissolved in the matrix will precipitate partially, causing problems such as coarsening and resulting in a decrease in strength. Therefore, as described above, it is necessary to cool at a rate that does not cause the elements dissolved in the matrix to precipitate.

[0020] Similarly, cooling in the processing step must start before the dissolved elements in the matrix precipitate, so as to prevent partial precipitation of the dissolved elements in the matrix, which may cause problems such as coarsening and result in a decrease in strength.

[0021] Furthermore, by performing extrusion in the solution temperature range and imparting strain, the interatomic distance of the aluminum alloy can be increased and the solubility limit can be raised, making it possible to achieve a more supersaturated solid solution, thereby realizing higher strength.

[0022] Here, the "solution temperature range" refers to the temperature range in which an element can be dissolved (dissolved) into the matrix, and depends on the material of the heat-treatable aluminum alloy in question, but is 450°C to 515°C for the 7000 series, 500°C to 590°C for the 6000 series, and 490°C to 530°C for the 2000 series.

[0023] Furthermore, when an aging treatment step is performed after the processing step, the elements dissolved in the matrix can be finely precipitated, thereby realizing further increased strength and increased toughness.

[0024] In addition, when the metal body is made of a steel material and the processing step involves extruding the steel material heated to the solution temperature range and then cooling it from the solution temperature range and quenching it, high strength is achieved through the supersaturated solid solution of the elements.

[0025] That is, in the processing step, elements can be dissolved in the matrix by heating to the solution temperature range, realizing a supersaturated solid solution of the elements. Then, by cooling from the solution temperature range and quenching (in other words, by rapid cooling from the austenite temperature range), the austenite structure of the matrix is ​​transformed into martensite, realizing high strength.

[0026] In this case, the "austenite temperature range" refers to a temperature range in which the matrix of the metal body has an austenite structure, and if the matrix has an austenite structure, it may contain carbides, nitrides, intermetallic compounds, etc.

[0027] Here, since martensitic transformation is a transformation that does not involve diffusion, it is possible for strain (strain imparted by extrusion) to remain after quenching. The locations of such strain become carbide precipitation sites during tempering, realizing an increase in the number of precipitation sites. One example is rapid cooling to the Mf point or below at a cooling rate of about 20° C. / sec or more.

[0028] In addition, by performing extrusion within the solution temperature range and imparting strain, (1) the interatomic distance of the steel material can be increased, raising the solid solubility limit, and (2) the aggregated carbides can be broken down and dispersed, promoting solid solution, making it possible to achieve even more supersaturated solid solution and achieving higher strength.

[0029] As in the case of the aluminum alloy described above, the "solution temperature range" here refers to the temperature range at which elements can be dissolved (dissolved) in the matrix, and is 850°C to 1200°C (1000°C to 1200°C for tool steel), depending on the type of steel material in question.

[0030] Furthermore, when a tempering process is performed after quenching to cause carbides of the elements dissolved in the martensite structure to precipitate, further increased strength and toughness can be achieved. Effect of the Invention

[0031] The method for manufacturing a hollow member of the present invention can realize high precision as well as high strength due to fine crystal grains. [Brief description of the drawings]

[0032] [Figure 1] FIG. 2 is a schematic diagram for explaining a method for producing an aluminum pipe according to the present invention. [Diagram 2] FIG. 1 is a schematic diagram (1) for explaining the processing process. [Diagram 3] FIG. 2 is a schematic diagram for explaining the processing step. [Figure 4] FIG. 1 is a schematic diagram (1) for explaining the state of crystal grains. [Diagram 5] FIG. 2 is a schematic diagram for explaining the state of crystal grains (2). [Figure 6] 1A to 1C are schematic diagrams for explaining a conventional method for manufacturing an aluminum pipe. [Figure 7] FIG. 2 is a schematic diagram for explaining a method for manufacturing an iron pipe according to the present invention. [Figure 8] FIG. 3 is a schematic diagram for explaining the state of crystal grains. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0033] Hereinafter, modes for carrying out the invention (hereinafter, referred to as "embodiments") will be described. The description will be made in the following order. 1. First embodiment 2. Second embodiment 3. Variations

[0034] In this embodiment, the case where the processing device (hollow member processing device) shown in FIG. 2(a) is used will be described as an example.

[0035] The processing device shown here is one in which a through hole is formed in advance in a billet 2 in a container 1, and a rod-shaped mandrel 3 is passed through the through hole, and then extrusion processing is performed using a die 4. In Fig. 2(a), reference numeral 5 denotes a stem and reference numeral 6 denotes a dummy block.

[0036] A cooling punch 10 made of a metal material with large heat capacity is disposed in front of the mandrel 3 in the extrusion direction. A rod-shaped portion 11 of the cooling punch 10 parallel to the extrusion direction is formed to have a diameter slightly smaller than that of the mandrel 3.

[0037] Furthermore, cooling water W is supplied inside the cooling punch, and the cooling punch is cooled by the cooling water W. Although the reference symbol W is omitted in Figures 2(b), 3(a), 3(b), 5, and 8, cooling water W is supplied in the same manner as in Figure 2(a).

[0038] <1. First embodiment> FIG. 1 is a schematic diagram illustrating a method for producing an aluminum pipe, which is one example of a method for producing a hollow member of the present invention.

[0039] In the first embodiment, an aluminum alloy is used as a material (billet) for extrusion processing. Specifically, A6061, a commercially available material, is used, and contains, by weight, 0.40-0.8% Si, 0.7% or less Fe, 0.15-0.40% Cu, 0.15% or less Mn, 0.8-1.2% Mg, 0.04-0.35% Cr, 0.25% or less Zn, 0.15% or less Ti, and the balance being Al and unavoidable impurities.

[0040] [Processing process] In the method for producing an aluminum pipe according to the first embodiment, first, a hollow billet made of an aluminum alloy is heated to 530° C. over one hour and held at that temperature for one hour (see symbol S1 in FIG. 1).

[0041] Here, in the first embodiment, an example is described in which heating is performed up to 530°C. However, it is sufficient to heat the alloy up to the solution temperature range (500°C to 590°C in the case of A6061) so that the elements can be dissolved in the matrix, and the temperature does not necessarily have to be 530°C.

[0042] Similarly, the heating time (1 hour) and the holding time (1 hour) are sufficient as long as they allow the element to dissolve in the matrix, and do not necessarily have to be 1 hour.

[0043] Next, as shown in FIG. 2(a), a billet 2 heated to 530°C is placed in a container 1, and a dummy block 6 is pushed in via a stem 5. As shown in FIG. 2(b), the billet 2 is pushed out of the hole (die hole) of a die 4, and a hollow pipe 7 is obtained (see symbol S2 in FIG. 1).

[0044] Here, in the first embodiment, an example is described in which extrusion processing is performed by a method called "mandrel extrusion" using the processing device shown in Figure 2(a), but it is sufficient if a hollow pipe 7 can be obtained, and extrusion processing by other methods (for example, a method called "porthole extrusion") may also be used.

[0045] In the extrusion process of the first embodiment, the billet temperature (530°C) during extrusion is close to the melting point of the billet (aluminum alloy), so the extrusion speed is relatively slow in order to suppress heat generation due to extrusion. Also, the degree of extrusion in the first embodiment is 90% or more.

[0046] Here, since the diameter (outer diameter) of the rod-shaped portion 11 of the cooling punch 10 is formed slightly smaller than the diameter (outer diameter) of the mandrel 3, the extruded hollow pipe 7 does not come into contact with the rod-shaped portion 11.

[0047] In FIG. 2(b), for ease of explanation, a sufficient gap is provided between the hollow pipe 7 and the rod-shaped portion 11. However, it is preferable that the gap between the hollow pipe 7 and the rod-shaped portion 11 be the minimum distance that does not allow them to come into contact with each other.

[0048] Next, as shown in FIG. 3(a), cooling air K is blown onto the outer periphery of the hollow pipe 7 to cool and shrink the hollow pipe 7.

[0049] As long as the hollow pipe 7 can be contracted, it is not necessarily required to use cooling air (gas), and water cooling by spraying or the like may also be used. However, from the viewpoint of not corroding the hollow pipe 7, air cooling (cooling air) is more preferable than water cooling.

[0050] Then, when the hollow pipe 7 shrinks due to the blowing of cooling air K, the gap between the hollow pipe 7 and the rod-shaped portion 11 disappears, as shown in Figure 3(b), the hollow pipe 7 and the rod-shaped portion 11 come into contact with each other, and the hollow pipe 7 is forcibly cooled (quenched) by the cooling punch 10, which is water-cooled with cooling water W (see symbol S3 in Figure 1).

[0051] [Aging treatment process] In the manufacturing method of the aluminum pipe according to the first embodiment, the hollow pipe 7 is then heated to 180°C (see symbol S4 in Figure 1) before natural aging (room temperature aging) occurs, held for 12 to 18 hours (see symbol S5 in Figure 1), and then air-cooled to room temperature (see symbol S6 in Figure 1), thereby finely precipitating the elements dissolved in the matrix.

[0052] [effect] In the manufacturing method of the aluminum pipe to which the present invention is applied, a supersaturated solid solution of elements is realized, and the strength of the aluminum pipe is increased. In other words, the aluminum pipe is heated to 530°C (the solution temperature range) to dissolve the elements into the matrix, and then rapidly cooled with a cooling punch (cooled at a rate that does not cause the dissolved elements to precipitate), resulting in improved mechanical properties (higher strength) of the aluminum pipe.

[0053] Furthermore, in the manufacturing method of aluminum pipe to which the present invention is applied, extrusion processing is performed at 530°C (the solution temperature range). This extrusion processing (imparting strain) increases the solubility limit, which is also a factor in achieving high strength.

[0054] Furthermore, in the manufacturing method of an aluminum pipe to which the present invention is applied, the hollow pipe 7 is cooled (quenched) by contacting the cooling punch 10, i.e., the hollow pipe 7 is cooled (quenched) while its inner surface is restrained by the cooling punch 10, thereby achieving high precision of the aluminum pipe.

[0055] Furthermore, in the method for producing an aluminum pipe to which the present invention is applied, the hollow pipe 7 is cooled (rapidly cooled) by the cooling punch 10, which allows the crystal grains to be refined and achieves high strength of the aluminum pipe. The grain refinement will be described below in comparison with the case where the hollow pipe 7 is air-cooled (where the cooling punch 10 is not used).

[0056] First, in the extrusion process, as shown in Fig. 4, the crystal grains are crushed (see symbol A in Fig. 4), and dislocations are introduced by applying large plastic strain to the extrusion process (see symbol B in Fig. 4). Note that at the stage shown by symbol B in Fig. 4, the structure has a high dislocation density, but the crystal grains are not fine. The high dislocation density structure is then recrystallized by the residual heat of the material to form fine crystal grains (see symbol C in Figure 4).

[0057] (When air-cooled) When the hollow pipe 7 is air-cooled (which is a commonly used method for manufacturing aluminum pipes), the cooling rate is so slow that the recrystallized structure (fine crystal grains) coarsens and softens due to the additional residual heat of the material (see symbol D in Figure 4).

[0058] (When quenched) In contrast, when the hollow pipe 7 is rapidly cooled as in the first embodiment, the cooling rate is fast, so that coarsening due to further residual heat of the material can be suppressed, and the recrystallized structure (fine crystal grains) can be maintained (see FIG. 5).

[0059] Furthermore, in the manufacturing method of an aluminum pipe to which the present invention is applied, there is no need to perform solution treatment after the processing step of forming the hollow pipe 7, so that the crystal grains do not become coarse due to reheating for heat treatment (heat treatment for the purpose of solution treatment).

[0060] In addition, in a commonly used method for manufacturing an aluminum pipe, after forming the hollow pipe 7, reheating is performed for heat treatment (heat treatment for the purpose of solid solution treatment), which causes the crystal grains to become coarse and reduces toughness. In addition, the need for heat treatment (heat treatment for the purpose of solid solution treatment) inevitably leads to an increase in costs.

[0061] [Characteristics comparison] In order to confirm the characteristics of the hollow pipe 7 obtained by the aluminum pipe manufacturing method according to the present invention, a hollow pipe was manufactured using the billet used in the first embodiment by a commonly used aluminum pipe manufacturing method.

[0062] Specifically, a hollow billet of an aluminum alloy was heated to 450° C. over one hour and held at that temperature for one hour (see symbol S1 in FIG. 6). Next, as in the first embodiment, a billet heated to 450°C was placed in the container, and the dummy block was pushed in through the stem to extrude the billet from the die hole to obtain a hollow pipe (see reference S2 in FIG. 6). The extruded hollow pipe was air-cooled (see reference S3 in FIG. 6).

[0063] Next, the hollow pipe was heated to 570° C. (see reference symbol S4 in FIG. 6), and after the elements were dissolved in the matrix (see reference symbol S5 in FIG. 6), it was rapidly cooled (see reference symbol S6 in FIG. 6). Thereafter, similar to the aging treatment process of the first embodiment, the hollow pipe was heated to 180°C (see symbol S7 in FIG. 6), held at that temperature for 12 to 18 hours (see symbol S8 in FIG. 6), and then air-cooled to room temperature (see symbol S9 in FIG. 6).

[0064] Table 1 shows the strength, toughness, and precision of a "hollow pipe obtained by the aluminum pipe manufacturing method applying this invention (invented technology)" and a "hollow pipe obtained by a commonly used aluminum pipe manufacturing method (existing technology)."

[0065] [Table 1]

[0066] As shown in Table 1, the "hollow pipe obtained by the aluminum pipe manufacturing method applying this invention (invented technology)" has better results in terms of strength, toughness, and precision than the "hollow pipe obtained by the commonly used aluminum pipe manufacturing method (existing technology)."

[0067] <2. Second embodiment> FIG. 7 is a schematic diagram illustrating a method for producing an iron pipe, which is another example of the method for producing a hollow member of the present invention.

[0068] In the second embodiment, a case where tool steel is used as a material (billet) used in extrusion processing will be described as an example. Specifically, hot work tool steel is used, and contains, by weight, 0.35-2.20% C, 0.15-0.90% Si, 0.30-1.20% Mn, 2.0-5.50% Cr, 1.20-1.60% W, 0.2-1.60% Mo, 0.1-2.20% V, with the balance being Fe and unavoidable impurities.

[0069] [Processing process] In the method for manufacturing an iron pipe according to the second embodiment, first, a hollow billet made of tool steel is heated to 1070° C. over one hour and held at that temperature for one hour (see symbol S1 in FIG. 7).

[0070] Here, in the second embodiment, the case of heating up to 1070°C is taken as an example for explanation, but it is sufficient to heat up to the solution temperature range (1000°C to 1200°C in the case of tool steel) so that the elements can be dissolved into the matrix, and the temperature does not necessarily have to be 1070°C.

[0071] Similarly, the heating time (1 hour) and the holding time (1 hour) are sufficient as long as they allow the element to dissolve in the matrix, and do not necessarily have to be 1 hour.

[0072] Next, as shown in FIG. 2(a), a billet 2 heated to 1070°C is placed in a container 1, and a dummy block 6 is pushed in via a stem 5. As shown in FIG. 2(b), the billet 2 is pushed out of the hole (die hole) of a die 4, and a hollow pipe 7 is obtained (see symbol S2 in FIG. 7).

[0073] As in the first embodiment, the extrusion process is not limited to the method called "mandrel extrusion" and may be performed by other methods.

[0074] Here, since the diameter (outer diameter) of the rod-shaped portion 11 of the cooling punch 10 is formed slightly smaller than the diameter (outer diameter) of the mandrel 3, the extruded hollow pipe 7 does not come into contact with the rod-shaped portion 11, as in the first embodiment described above.

[0075] Next, as shown in FIG. 3(a), cooling air K is blown onto the outer periphery of the hollow pipe 7 to cool and shrink the hollow pipe 7.

[0076] When the hollow pipe 7 shrinks due to the blowing of cooling air K, the gap between the hollow pipe 7 and the rod-shaped portion 11 disappears, as shown in Figure 3(b), the hollow pipe 7 and the rod-shaped portion 11 come into contact with each other, and the hollow pipe 7 is forcibly cooled (rapidly cooled) to below the Mf point by the cooling punch 10, which is cooled by cooling water W (see symbol S3 in Figure 7), and then it is air-cooled to room temperature (see symbol S4 in Figure 7). By such quenching, a martensite structure can be formed.

[0077] [Tempering process] In the manufacturing method of the iron pipe according to the second embodiment, the hollow pipe 7 is then heated to 550°C (see symbol S5 in Figure 7) and air-cooled to room temperature (see symbol S6 in Figure 7), thereby precipitating carbides of the elements dissolved in the martensite structure.

[0078] [effect] In the manufacturing method of the iron pipe to which the present invention is applied, a supersaturated solid solution of elements is realized, and the strength of the iron pipe is increased. That is, by heating to 1070℃ (solution temperature range) to dissolve the elements into the matrix, and then quenching with a cooling punch, the austenite phase of the matrix transforms into martensite, but since martensite transformation is a diffusionless transformation and the supersaturated dissolved elements do not reprecipitate or coagulate, it is possible to obtain a martensite structure while maintaining the effect of the supersaturated solution and, moreover, while retaining the strain imparted by the extrusion process. This results in improved mechanical properties (higher strength) of the iron pipe.

[0079] Furthermore, in the manufacturing method of iron pipe to which the present invention is applied, extrusion processing is performed at 1,070°C (the solution temperature range). This extrusion processing (imparting strain) increases the solubility limit in combination with dispersing the solid solution, making it possible to achieve a supersaturated solid solution in a state in which the elements are sufficiently dispersed, thereby achieving high strength.

[0080] Furthermore, in the manufacturing method of the iron pipe to which the present invention is applied, by performing tempering, precipitates of elements finely dispersed in the matrix can be obtained, thereby realizing high toughness.

[0081] Furthermore, in the manufacturing method of an iron pipe to which the present invention is applied, the hollow pipe 7 is cooled (rapidly cooled) by contacting the cooling punch 10, i.e., the hollow pipe 7 is cooled (rapidly cooled) while its inner surface is restrained by the cooling punch 10, thereby achieving high precision of the iron pipe.

[0082] Furthermore, in the method for manufacturing an iron pipe to which the present invention is applied, the hollow pipe 7 is cooled (quenched) with a cooling punch, which makes it possible to realize high strength iron pipes. In other words, in the manufacturing method of iron pipes to which the present invention is applied, the cooling rate is fast, so that the coarsening of the recrystallized structure (fine crystal grains) due to further residual heating of the material (see Figure 4) can be suppressed, and in addition to being able to maintain the recrystallized structure (fine crystal grains) (see symbol C in Figure 8), it is possible to obtain a martensitic structure (see symbol D in Figure 8), thereby achieving high strength iron pipes.

[0083] Furthermore, in the manufacturing method of the iron pipe to which the present invention is applied, the crystal grains do not become coarse when reheated for heat treatment (heat treatment for the purpose of hardening) after the processing step of forming the hollow pipe 7.

[0084] In addition, in a commonly used method for manufacturing iron pipes, after the hollow pipe 7 is formed, it is reheated for heat treatment (heat treatment for hardening), which causes the crystal grains to become coarse and reduces toughness. In addition, the need for heat treatment (heat treatment for hardening) inevitably increases costs.

[0085] <3. Modifications> The first and second embodiments described above have both been explained using examples in which a heat-treatable alloy is used, but the metal body of the present invention does not need to be limited to a heat-treatable alloy and may also be a non-heat-treatable alloy (e.g., a 5000 series aluminum alloy). In the case of non-heat-treatable alloys, although it is not possible to increase strength by forming a supersaturated solid solution of elements, it is possible to increase strength by making the crystal grains finer (see FIG. 5). [Explanation of symbols]

[0086] 1 Container 2 Billet 3 Mandrel 4 Dice 5. Stem 6 Dummy Block 7 Hollow Pipe 10. Cooling Punch 11 Rod part

Claims

1. The method includes a processing step of extruding a metal body heated to a predetermined temperature range to form a hollow member, and then cooling the metal body from the predetermined temperature range by contacting the metal body with a cooling means located in the hollow portion of the hollow member. A method for manufacturing a hollow member.

2. The cooling from the predetermined temperature range is The cooling means is positioned in the hollow portion of the hollow member with a predetermined gap therebetween, and the metal body is then contracted to bring the metal body into contact with the cooling means. The method for producing the hollow member according to claim 1 .

3. The metal body is contracted by supplying cooling air to the metal body. The method for producing the hollow member according to claim 2 .

4. the metal body is made of a heat-treatable aluminum alloy; The processing step includes extruding a heat-treatable aluminum alloy heated to a solution temperature range, and then cooling the alloy from the solution temperature range at a rate at which the dissolved elements do not precipitate. The method for producing a hollow member according to claim 1, 2 or 3.

5. The processing step is followed by an aging treatment step. The method for producing a hollow member according to claim 4 .

6. The metal body is a 7000 series metal body, The solution temperature range is 450°C to 515°C. The method for producing a hollow member according to claim 4 .

7. The metal body is a 6000 series metal body, The solution temperature range is 500° C. to 590° C. The method for producing a hollow member according to claim 4 .

8. The metal body is a 2000 series metal body, The solution temperature range is 490°C to 530°C. The method for producing a hollow member according to claim 4 .

9. The metal body is made of a steel material, The processing step includes extruding a steel material heated to a solution temperature range, and then cooling the steel material from the solution temperature range to perform quenching. The method for producing a hollow member according to claim 1, 2 or 3.

10. After the quenching, a tempering process is performed to precipitate carbides of the elements dissolved in the martensite structure. The method for producing a hollow member according to claim 9 .

11. The solution temperature range is 850° C. to 1200° C. The method for producing a hollow member according to claim 9 .

Citation Information

Patent Citations

  • Method of working metal, metal body obtained by the method and metal-containing ceramic body obtained by the method

    WO2004028718A1