Resin film, circuit board material, circuit board, and electronic device

The use of a PEKK resin film with specific inorganic fillers addresses low-temperature lamination and thermal expansion issues, improving dielectric properties and signal stability in circuit boards.

JP2024135030AInactive Publication Date: 2024-10-04MITSUBISHI CHEM CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023045521
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional insulating materials for circuit boards face challenges in low-temperature lamination, high thermal expansion, and high dielectric properties, leading to issues like warping, peeling, and signal loss in high-frequency operations.

Method used

A resin film composed of polyetherketoneketone (PEKK) and inorganic fillers with specific particle sizes and ratios, such as fluorine-containing mica, is used to achieve low-temperature lamination and reduce thermal expansion while maintaining excellent dielectric properties.

Benefits of technology

The resin film allows for low-temperature lamination, reduces thermal expansion, and enhances dielectric performance, ensuring stable signal transmission and structural integrity in circuit boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135030000001
    Figure 2024135030000001
  • Figure 2024135030000002
    Figure 2024135030000002
  • Figure 2024135030000003
    Figure 2024135030000003
Patent Text Reader

Abstract

To provide a thermoplastic resin film which enables lamination at low temperature, has small heat expansion, and is excellent in dimensional stability by heat.SOLUTION: A resin film contains polyether ketone ketone (A), and an inorganic filler (B), wherein a 50% length (median diameter) in a long axis direction of the inorganic filler (B) in the resin film is 0.25 μm or more and 1.0 μm or less, and a 50% length (median diameter) in a short axis direction thereof is 0.03 μm or more and 0.25 μm or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin film, a circuit board material, a circuit board, and an electronic device. [Background technology]

[0002] Insulating materials for circuit boards are required to have solder heat resistance in the manufacturing process. If heat-resistant thermoplastic resins such as polyether ketone resins and polyimide resins can be used as insulating materials for printed wiring boards, they are expected to have excellent electrical properties at high temperatures and to ensure the reliability of circuits in high-temperature environments. However, because these heat-resistant thermoplastic resins have high molding temperatures, they require the use of adhesives such as epoxy resins or high-temperature hot press molding in a molten state of 260°C or higher when bonding to copper foil or forming into a multilayer board, which poses problems such as the time it takes to heat up and cool down. Furthermore, with crystalline resins, adhesiveness cannot be achieved unless they are heated to a temperature close to their melting point, and there is also the problem that the resin flows and deforms when the melting point is exceeded.

[0003] Meanwhile, polyether ether ketone (PEEK) resin, known as a super engineering plastic, is a highly functional thermoplastic resin that has excellent heat resistance, high-temperature properties, hydrolysis resistance, mechanical strength, flame retardancy, chemical resistance, electrical properties, etc., and is therefore used in the manufacture of rigid or flexible boards in the electrical and electronic fields, semiconductor package boards, and other electronic boards. This type of electronic board is manufactured using, for example, a two- or three-layer copper-clad laminate (FCCL) in which copper foil is bonded to a polyetheretherketone resin film, and the copper foil functions as a circuit pattern (see Patent Documents 1 and 2). When a multilayer board is manufactured using a polyetheretherketone resin film, it is heated to a temperature (e.g., 360°C) equal to or higher than its melting point (e.g., 343°C), and the polyetheretherketone resin is bonded to the substrate in a molten state.

[0004] As described above, conventional multilayer boards are bonded with the polyether ether ketone resin in a molten state, which can result in distortion of the conductor pattern and warping of the board due to the difference in linear expansion coefficient between the polyether ether ketone resin film and the copper foil. Therefore, Patent Document 3 proposes a laminate characterized by laminating, on at least one side of a polyarylene ether ketone resin layer containing an inorganic filler, a resin adhesive layer containing a polyarylene ether ketone resin having a melting point that is 5°C or more lower than the melting point of the polyarylene ether ketone resin layer, and laminating a metal layer on this resin adhesive layer. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Special Publication No. 2015-536555 [Patent Document 2] Special Publication No. 2009-545878 [Patent Document 3] JP 2022-148547 A Summary of the Invention [Problem to be solved by the invention]

[0006] In the laminate proposed in Patent Document 3, a resin adhesive layer is provided so that a metal layer is indirectly laminated to a polyarylene ether ketone resin layer via a low-melting resin adhesive layer, and therefore the polyarylene ether ketone resin is unlikely to be directly bonded to the metal layer in a molten state. Therefore, it is said that by laminating the metal layer at a temperature at which the polyarylene ether ketone resin layer does not melt, it is possible to prevent the dimensional characteristics from deteriorating and the metal layer from peeling off. However, the lamination temperature of polyarylene ether ketone itself is still high, and it is difficult to laminate at a low temperature, for example, 200° C. In addition, if the dielectric constant and dielectric tangent of the insulating material used in the circuit board are high, the transmission loss increases when a high-frequency signal flows, causing problems in communication operations. Therefore, an object of the present invention is to provide a thermoplastic resin film which can be laminated at low temperatures, has small thermal expansion, and is excellent in low dielectric properties. [Means for solving the problem]

[0007] In view of the above circumstances, the present inventors have conducted extensive research and found that the above problems can be solved by using a resin film containing polyether ketone ketone and an inorganic filler having a specific particle size, and have completed the present invention. That is, the present invention provides the following items [1] to

[14] .

[0008] [1] A resin film comprising a polyether ketone ketone (A) and an inorganic filler (B), wherein the 50% length (median diameter) of the inorganic filler (B) in the long axis direction in the resin film is 0.25 μm or more and 1.0 μm or less, and the 50% length (median diameter) of the inorganic filler (B) in the short axis direction in the resin film is 0.03 μm or more and 0.25 μm or less. [2] The resin film according to the above [1], wherein the aspect ratio of the inorganic filler (B) in the resin film is 5 or more and 10 or less. [3] The resin film according to [1] or [2] above, wherein the 90% length of the inorganic filler (B) in the long axis direction is 1 μm or more and 5 μm or less, and the 90% length of the inorganic filler (B) in the short axis direction is 0.01 μm or more and 0.5 μm or less. [4] The resin film according to any one of the above [1] to [3], wherein the polyether ketone ketone (A) has a repeating unit (a-1) represented by the following structural formula (1) and / or a repeating unit (a-2) represented by the following structural formula (2): [ka] [ka] [5] The resin film according to the above [4], wherein the content ratio of the repeating unit (a-1) to the repeating unit (a-2) is (a-1):(a-2)=55:45 to 75:25 (mol %). [6] The resin film according to any one of the above [1] to [5], having a glass transition temperature of 150° C. or higher and 170° C. or lower. [7] The resin film according to any one of the above [1] to [6], wherein the inorganic filler (B) is synthetic mica. [8] The resin film according to any one of the above [1] to [7], wherein the inorganic filler (B) is 10 parts by mass or more and less than 45 parts by mass per 100 parts by mass of the polyether ketone ketone (A). [9] The resin film according to any one of the above [1] to [8], which has a relative crystallinity of 90% or less.

[10] The resin film according to any one of the above [1] to [9], which has a linear expansion coefficient of 50 ppm / ° C. or less.

[11] The resin film according to any one of the above [1] to

[10] , which is used for a circuit board.

[12] A circuit board material having a configuration in which the resin film according to any one of the above [1] to

[11] and a conductor are laminated together.

[13] A circuit board comprising the circuit board material described in

[12] above.

[14] An electronic device comprising the circuit board described in

[13] above. Effect of the Invention

[0009] According to the present invention, it is possible to provide a thermoplastic resin film which allows lamination at low temperatures, has small thermal expansion, and is excellent in dimensional stability due to heat. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] An example of an embodiment of the present invention will be described in detail below. However, the present invention is not limited to the embodiment described below, and can be modified as desired without departing from the gist of the present invention.

[0011] [Resin film] The resin film of the present invention (hereinafter sometimes referred to as "the present resin film") contains polyether ketone ketone (A) and an inorganic filler (B). Each of the constituent elements will be described in detail below.

[0012] <Polyetherketoneketone> The resin film of the present invention contains polyether ketone ketone (hereinafter, sometimes referred to as "PEKK") as component (A). PEKK is a thermoplastic resin that has a high tensile modulus and a suitable heat of crystalline fusion from the viewpoint of moldability. PEKK preferably has a repeating unit (a-1) represented by the following structural formula (1) and a repeating unit (a-2) represented by the following structural formula (2). That is, it preferably has two types of repeating units. Both repeating units (a-1) and (a-2) have one ether group and two ketone groups.

[0013] [ka]

[0014] [ka]

[0015] The content ratio of repeating units (a-1) and (a-2) in PEKK ((a-1):(a-2) (mol%)) is not particularly limited, but is preferably 55:45 to 75:25. When the molar ratio of (a-1) is 55% or more, the glass transition temperature (Tg) does not decrease and excellent heat resistance can be maintained. On the other hand, when the molar ratio of (a-1) is 75% or less, the crystallization rate becomes slow and sufficient heat fusion and adhesion between substrates can be obtained. From the above viewpoints, (a-1):(a-2) is more preferably in the range of 58:42 to 73:27, and even more preferably in the range of 60:40 to 70:30. The PEEK having the above structure may be used alone or in combination of two or more types, with the repeating units (a-1) and (a-2) contained in the above ratio. Here, the molar content ratio of the repeating units (a-1) and (a-2) in PEKK can be measured, for example, by using NMR.

[0016] The total number (degree of polymerization) of repeating units (a-1) and (a-2) is preferably 10-100, and more preferably 20-50, from the viewpoint of ensuring mechanical properties.

[0017] The Tg of PEKK is preferably 150° C. or higher, more preferably 153° C. or higher, and even more preferably 155° C. or higher. If the Tg is 150° C. or higher, a film having sufficient heat resistance can be obtained. On the other hand, the upper limit of Tg is not particularly limited, but from the viewpoint of molding processability at low temperatures, it is preferably 200°C or less, more preferably 190°C or less, even more preferably 180°C or less, and particularly preferably 170°C or less.

[0018] In addition, the heat of crystal fusion (ΔHm) of PEKK is preferably 60 J / g or less, more preferably 50 J / g or less, and even more preferably 40 J / g or less. If ΔHm is 60 J / g or less, shrinkage due to crystallization during molding can be suppressed. On the other hand, the upper limit of ΔHm is preferably 10 J / g or more, more preferably 15 J / g or more, and even more preferably 20 J / g or more. If ΔHm is 10 J / g or more, solder heat resistance due to crystallization can be imparted.

[0019] In the present invention, Tg and ΔHm are determined from a DSC (Differential Scanning Calorimetry) curve detected when the temperature is increased in the temperature range of 25 to 400° C. at a heating rate of 10° C. / min using a differential scanning calorimetry (DSC) in accordance with JIS K 7121:2012 and JIS K 7122:2012.

[0020] PEKK can be produced by known methods (for example, see JP-A-61-195122 and JP-A-62-129313). Commercially available products can also be used, such as the "KEPSTAN" series manufactured by Arkema, the "Kstone" series manufactured by Shandong Kaishen New Materials Co., Ltd., and the "NovaSpire" manufactured by Solvay.

[0021] <Inorganic filler> The resin film of the present invention contains an inorganic filler as component (B). The inorganic filler is not particularly limited as long as it has the physical properties described below, and various types can be used. Specific examples include scale-like, plate-like, or flaky (flat) powders made of inorganic substances such as mica clay, glass, silica, aluminum nitride, silicon nitride, boehmite, talc, sericite, illite, kaolinite, montmorillonite, vermiculite, smectite, alumina, titanates such as magnesium potassium titanate and lithium potassium titanate, and calcium carbonate. Other examples include glass fibers, aramid fibers, carbon fibers, and potassium titanate fibers. Among these, particles of mica, silica, glass, talc, kaolin, calcium carbonate, etc. are preferred, and fluorine-containing inorganic fillers that contain fluorine are preferred. Among these, fluorine-containing mica (fluorine mica), particularly fluorine phlogopite, is preferred in terms of improving dielectric properties.

[0022] Mica is a plate-like crystal belonging to the mica family of phyllosilicate minerals, and is classified into two types: natural mica (muscovite, biotite, phlogopite, etc.) and artificially produced synthetic mica. In particular, synthetic mica in which the hydroxyl groups (OH) of naturally occurring mica are replaced with fluorine (F) to enable use at high temperatures. Known methods for synthesizing synthetic mica include hydrothermal synthesis, solid-phase synthesis, melting, and the like, and any method may be used, but it is preferable to synthesize synthetic mica by a melting method in which 100% of the hydroxyl groups are replaced with fluorine. Among the synthetic mica particles, non-swelling synthetic mica is particularly preferred from the viewpoints of dimensional stability under heating and water resistance. As an example of a non-swelling synthetic mica, there is fluorine mica (K2Mg6Al2(SiO 20 )F4), potassium tetrasilicic mica (K2Mg5(SiO 20 )F4), potassium taeniolite (K2Mg4Li2(Si8O 20Among them, fluorine-containing mica capable of further reducing the dielectric tangent is particularly preferable. Examples of synthetic mica include the "PDM" series manufactured by Topy Industries, the "MK" series manufactured by Katakura Coop Agri, and the "NK" and "NS" series manufactured by Nihon Kohken Kogyo.

[0023] (long axis diameter) The 50% length (median diameter) in the long axis direction of the inorganic filler (B) in the present resin film is preferably 0.25 μm or more and 1.0 μm or less. If the 50% length in the long axis direction is 0.25 μm or more, it is advantageous in terms of low dielectric tangent and low linear expansion. From the above viewpoints, the median diameter in the long axis direction is preferably 0.3 μm or more, more preferably 0.35 μm or more, and even more preferably 0.4 μm or more. On the other hand, if the 50% length in the long axis direction is 1.0 μm or less, it is advantageous in terms of mechanical properties. From the above viewpoints, the median diameter in the long axis direction is preferably 0.9 μm or less, more preferably 0.85 μm or less, and even more preferably 0.8 μm or less. In addition, the 90% length (hereinafter sometimes referred to as "d90(L)") of the inorganic filler (B) in the resin film in the long axis direction is preferably 1 μm or more and 5 μm or less. In this range, the resin film has good film formability and appearance, and the effect of reducing the linear expansion coefficient of the film can be expected. From the above viewpoints, the d90(L) of the filler (B) in the present resin film is more preferably 1.5 μm or more and 4.5 μm or less, and further preferably 2 μm or more and 4 μm or less.

[0024] (minor axis diameter) The 50% length (median diameter) in the minor axis direction of the inorganic filler (B) in the present resin film is preferably 0.03 μm or more and 0.25 μm or less. If the 50% length in the minor axis direction is 0.03 μm or more, it is advantageous in terms of the dispersibility of the filler. From the above viewpoint, the median diameter in the minor axis direction is preferably 0.04 μm or more, more preferably 0.05 μm or more, and even more preferably 0.06 μm or more. On the other hand, if the 50% length in the minor axis direction is 0.25 μm or less, it is advantageous in terms of low linear expansion. From the above viewpoints, the median diameter in the minor axis direction is preferably 0.24 μm or less, more preferably 0.23 μm or less, and even more preferably 0.22 μm or less. In addition, the 90% length in the minor axis direction of the inorganic filler (B) in the resin film (hereinafter sometimes referred to as "d90(S)") is preferably 0.01 μm or more and 0.5 μm or less. When the d90(S) of the inorganic filler (B) in the resin film is in this range, the film formability and appearance of the resin film are good, and the effect of reducing the linear expansion coefficient of the film can be expected. From this viewpoint, the d90(S) of the filler (B) in the present resin film is more preferably 0.05 μm or more and 0.45 μm or less, and even more preferably 0.1 μm or more and 0.4 μm or less.

[0025] (Aspect Ratio) The aspect ratio (= major axis diameter / minor axis diameter) of the filler (B) in the present resin film is preferably from 5 to 10. When the aspect ratio is within this range, the filler is less likely to aggregate in the present resin film, making film formation easier, and a reduction in the linear expansion coefficient of the film can be expected. From the above viewpoints, the aspect ratio of the filler (B) in the resin film is more preferably 6 or more and 10 or less, and further preferably 7 or more and 10 or less.

[0026] The 50% length in the long axis direction, the 50% length in the short axis direction, the 90% length in the long axis direction, the 90% length in the short axis direction, and the aspect ratio of the inorganic filler (B) are values ​​in the resin film. They are not values ​​for the inorganic filler (B) in the resin composition for forming the resin film. This is because the inorganic filler (B) is partially pulverized in the process of forming the resin film from the resin composition. In addition, the inorganic filler (B) in the resin composition for forming the resin film may be pulverized or the like so that the physical properties of the inorganic filler (B) in the resin film can be obtained. In addition, the 50% length in the long axis direction, the 50% length in the short axis direction, the 90% length in the long axis direction, the 90% length in the short axis direction, and the aspect ratio of the filler (B) in this resin film are measured by the methods shown in the examples.

[0027] (Particle size of inorganic filler alone) The particle size of the inorganic filler (B) before being blended in the resin film is not particularly limited, but the 90% average particle size is preferably 1 μm or more and less than 100 μm, more preferably 2 μm or more and less than 80 μm, even more preferably 3 μm or more and less than 60 μm, and particularly preferably 5 μm or more and less than 50 μm. If it is within this range, the particle size of the inorganic filler in the film can be kept within the above range. The particle size of the inorganic filler alone can be measured by a laser diffraction particle size distribution analyzer using water as a dispersion medium and a neutral surfactant as a dispersant.

[0028] (Content ratio) The present resin film preferably contains PEKK (A) and an inorganic filler (B), with the inorganic filler (B) being 20 parts by mass or more per 100 parts by mass of PEKK (A). If the content is within this range, the film formability and appearance are good, and the effect of reducing the linear expansion coefficient of the film can be expected. From this viewpoint, it is more preferable to contain 22 parts by mass or more of the inorganic filler (B) per 100 parts by mass of the PEKK (A), and it is even more preferable to contain 24 parts by mass or more. In addition, although there is no particular upper limit, from the viewpoint of film formability, it is preferable to contain 50 parts by mass or less of the inorganic filler (B) per 100 parts by mass of the PEKK (A), and more preferably 40 parts by mass or less.

[0029] (Other Ingredients) PEKK (A) may be used in the form of a random copolymer, alternating copolymer, block copolymer, or modified product with other copolymerizable monomers as long as the effects of the present invention are not impaired. In addition to the above-mentioned components, the resin film may be appropriately blended with other resins, fillers, and various additives, such as heat stabilizers, ultraviolet absorbers, light stabilizers, nucleating agents, colorants, lubricants, and flame retardants, as necessary. For example, a resin compatible with PEKK(A) may be blended to adjust the crystallization rate of PEKK(A). Specifically, polyetherimide resins can be used because they are compatible with PEKK(A). The blending amount is preferably 40% by mass or less, more preferably 30% by mass or less, and even more preferably 20% by mass or less, relative to 100% by mass of PEKK(A). By being within the above range, the crystallization rate of PEKK(A) can be adjusted while maintaining the Tg of the film low. The lower limit is not particularly limited, but is, for example, 1% by mass or more.

[0030] <Physical properties of resin film> (film thickness) When used as a circuit board material for electric and electronic devices, the thickness of the present resin film is preferably from 10 μm to 300 μm, more preferably from 20 μm to 200 μm, and even more preferably from 30 μm to 100 μm. In addition, the present resin film is preferably produced so that the anisotropy of the physical properties in the machine direction (MD) and the perpendicular direction (TD) is minimized.

[0031] (Glass transition temperature (Tg)) The glass transition temperature (Tg) of the resin film is preferably 150° C. or higher and 170° C. or lower. When the Tg is 150° C. or higher, the heat resistance of the resin film is sufficient. On the other hand, when the Tg is 170° C. or lower, the resin film is easily processed at low temperatures, and when used as an insulating film for a circuit board, for example, the circuit board can be easily embedded at a low temperature of 200° C. From the above viewpoints, it is more preferable that the Tg of the present resin film is 155° C. or more and 165° C. or less.

[0032] (Dielectric tangent) The dielectric tangent is an index of the electrical energy loss inside an insulator, and is calculated from the ratio of the charging current to the current lost. In an ideal insulator, the electrical energy loss is zero, so it is desirable for the insulator to have a small dielectric tangent value. In high-frequency circuit boards, power absorption causes signal transmission loss, which is converted into heat. The dielectric dissipation factor affects the quality of signal transmission; therefore, the larger the dielectric dissipation factor, the greater the absorption and the greater the signal loss; conversely, the lower the dielectric dissipation factor, the less the signal loss. From the viewpoint of use in high-frequency circuit boards, the dielectric loss tangent of the resin film at a frequency of 10 GHz, a temperature of 23°C, and a relative humidity of 50% is preferably 0.004 or less, more preferably 0.0038 or less, and even more preferably 0.0035 or less. By setting it in this range, the dielectric loss is small, and the transmission efficiency and speed of the electrical signal of the circuit board can be increased. The lower limit of the dielectric loss tangent is not particularly limited, but is usually 0.001 or more.

[0033] (Dielectric constant) One purpose of increasing the frequency is to transmit signals faster, that is, to increase the signal speed in high frequency circuits. The lower the dielectric constant, the faster the signal speed will be, approaching the speed of light. Therefore, a material with a low dielectric constant is appropriate. From this viewpoint, the relative dielectric constant of the resin film at a frequency of 10 GHz, a temperature of 23°C, and a relative humidity of 50% is preferably 3.5 or less, more preferably 3.4 or less, and even more preferably 3.3 or less. By setting it in this range, the dielectric loss is small, and the transmission efficiency and speed of the electrical signal of the circuit board can be increased. The lower limit of the relative dielectric constant is not particularly limited, but is usually 2.0 or more.

[0034] The dielectric constant and the dielectric loss tangent are measured by the methods shown in the following examples.

[0035] (Water absorption rate) Water absorption, or water absorption rate, affects the dielectric constant and dielectric loss. The resin film has a low water absorption rate, which makes it easier to prevent peeling from the copper foil of the substrate. In addition, the migration resistance is improved, making it easier to prevent the occurrence of short circuits. Therefore, the water absorption rate of the present resin film is preferably 1% or less, more preferably 0.8% or less, and even more preferably 0.6% or less. The lower limit of the water absorption rate is not particularly limited, but is usually 0.1 or more. As shown in the examples below, the water absorption rate is measured by preparing a test piece from the resin film, immersing the test piece in water at 23° C. for 24 hours, and measuring the change in mass before and after immersion.

[0036] (Linear expansion coefficient) Assuming that this resin film is laminated onto a substrate such as copper foil, there is a possibility that the copper foil may peel off due to a mismatch between hot and cold changes. Therefore, it is preferable to reduce the linear expansion coefficient of this resin film and make it as close as possible to the linear expansion coefficient of copper. From this viewpoint, the linear expansion coefficient of the resin film in both MD and TD is preferably 50 ppm / ° C. or less, more preferably 40 ppm / ° C. or less, and even more preferably 35 ppm / ° C. or less. Since the linear expansion coefficient of copper foil is about 20 ppm / ° C., the lower limit is expected to be 15 ppm / ° C. or more. The linear expansion coefficient is measured by the method shown in the following examples.

[0037] (Relative Crystallinity) The resin film of the present invention preferably has a relative crystallinity of 90% or less. When the relative crystallinity is 90% or less, the processability of the resin film is ensured, and embedding of circuits, etc. becomes easy. From the above viewpoints, the relative crystallinity of the present resin film is more preferably 50% or less, further preferably 30% or less, and particularly preferably 20% or less. There is no particular lower limit for the relative crystallinity of the resin film, but it is usually 0% or more. The relative crystallinity can be calculated by the following formula. Relative crystallinity (%) = {(|ΔHm|-|ΔHc|) / ΔHm} × 100 Here, ΔHc is the heat of crystallization, and ΔHm is the heat of crystal fusion.

[0038] <Method of manufacturing the resin film> The resin film can be produced, for example, by melt-kneading materials such as PEKK (A) and an inorganic filler (B) and then quenching the mixture to form a film. In this case, examples of the film-forming method include inflation molding, extrusion cast molding using a T-die, and calendar molding. Among them, extrusion cast molding using a T-die is preferred from the viewpoints of film-forming properties and stable productivity. Alternatively, the film may be formed by press molding.

[0039] The molding temperature in the extrusion cast molding method using a T-die is appropriately adjusted depending on the flow characteristics and film-forming properties of the composition, but is generally from the melting point to 430° C. The thickness of the molded product is not particularly limited, but is usually about 10 μm to 800 μm. For the melt kneading, a commonly used single screw extruder, twin screw extruder, kneader, mixer, etc. can be used, and there is no particular limitation. The rotation speed of the extruder or mixer varies depending on the shape and size of the screw used, but is preferably 10 rpm or more, particularly preferably 15 rpm or more, from the viewpoint of dispersing the inorganic filler (B). There is no particular upper limit to the rotation speed, but it is preferably less than 100 rpm from the viewpoint of suppressing pulverization of the inorganic filler (B) and suppressing decomposition of the resin due to shear heat.

[0040] As described above, the resin film of the present invention preferably has a relative crystallinity of 90% or less. In the case of an extrusion casting method using a T-die, a film with a low relative crystallinity can be obtained by quenching the film extruded from the T-die.

[0041] As a method for adjusting the cooling conditions when cooling the molten material to form a film, for example, a cast roll is used as a cooling machine and the extruded molten resin is brought into contact with the cast roll.

[0042] In the case of press molding, for example, the molten and mixed material is poured between two metal plates, and press molded under conditions of a temperature of 330°C to 380°C, a pressure of 2 MPa to 10 MPa, and a molding time of 10 seconds to 60 seconds, and then rapidly cooled with water to 200°C or less to form a film.

[0043] <Circuit board materials> A circuit board material according to an embodiment of the present invention is configured by laminating the above-mentioned present resin film and a conductor. For example, a circuit can be formed from the conductor to constitute a circuit board.

[0044] The conductor may be a copper foil. The copper foil can be patterned into a predetermined shape by etching or the like in a circuit board to form wiring or the like. The thickness of the copper foil is, for example, preferably from 1 μm to 80 μm, more preferably from 3 μm to 50 μm, and even more preferably from 5 μm to 30 μm. The copper foil may be directly attached to the base film without an adhesive layer, or may be attached via an adhesive layer. The adhesive layer is not particularly limited, but may be a polyimide resin adhesive, an epoxy resin adhesive, an acrylic resin adhesive, a phenol resin adhesive, or the like. Among these, the polyimide resin adhesive and the epoxy resin adhesive are preferred.

[0045] In addition, the copper foil may be surface-treated with a surface treatment agent such as a silane coupling agent, and the copper foil may be bonded to the base film via the surface treatment agent, or the copper foil may be bonded directly to the base film without the use of a surface treatment agent or an adhesive layer.

[0046] The present resin film preferably constitutes either a base film or a cover film. The base film is a substrate for the circuit board, and it is preferable that a copper foil is provided on the base film. A cover film, sometimes called a coverlay film, is a film for covering and protecting the copper foil and the like provided on a base film. The cover film is used by being attached to the copper foil surface of a base film or a rigid board, which is the base material for a circuit board. The cover film is generally attached to a substrate such as a base film or a rigid substrate via an adhesive layer. The adhesive used for this adhesive layer can be any of the above-mentioned. The adhesive layer may be omitted as appropriate, in which case the cover film may be attached to a copper foil that has been surface-treated with a surface treatment agent such as a silane coupling agent, or may be directly attached to the copper foil without an adhesive layer or a surface treatment agent.

[0047] Copper foil is generally patterned and provided partially on the substrate, but in the portions of the substrate where the copper foil is not provided, the cover film may be directly adhered to the substrate or may be attached to the substrate via an adhesive layer.

[0048] <Circuit board> A circuit board according to an embodiment of the present invention includes the above-mentioned circuit board material. The circuit board includes a high-frequency circuit board, and specific examples of its use include FPC (Flexible Printed Circuits) and FCCL (Flexible Cupper Clad Laminate). As described above, in the present invention, the molded product such as the resin film has a good balance of various performances such as dielectric properties and has low water absorption. Therefore, it satisfies the required properties for a circuit board and is suitable for use in the circuit board. In particular, the present invention is particularly suitable for the above-mentioned FPC and FCCL.

[0049] <Electronic equipment> An electronic device according to an embodiment of the present invention includes the above-described circuit board. Examples of such electronic devices include portable electronic devices such as mobile phones, smartphones (mobile phones), electronic organizers, digital still cameras, and video cameras, electronic paper, televisions, DVD players, various audio devices, car navigation devices, in-vehicle displays such as instrument panels, calculators, printers, scanners, copiers, refrigerators, and washing machines.

[0050] <Explanation of terms> In the present invention, the term "film" also includes the term "sheet", and the term "sheet" also includes the term "film". Furthermore, when the term "panel" is used, such as an image display panel or a protective panel, it encompasses a plate, a sheet, and a film. In the present invention, when it is described as "X to Y" (X and Y are any numbers), unless otherwise specified, it includes the meaning of "X or more and Y or less", as well as the meaning of "preferably larger than X" or "preferably smaller than Y". In addition, when it is stated that the amount is "X or more" (X is any number), it also means that the amount is "preferably greater than X" unless otherwise specified, and when it is stated that the amount is "Y or less" (Y is any number), it also means that the amount is "preferably smaller than Y" unless otherwise specified. EXAMPLES

[0051] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples as long as it does not deviate from the gist of the invention. The evaluation methods in the examples and comparative examples are as follows.

[0052] [Evaluation method] (1) The length of the inorganic filler in the long and short axis directions The major axis length and minor axis length of the inorganic filler were measured by observing the thickness cross section in the width direction of the obtained film (sample) with an electron microscope, extracting 100 inorganic fillers, and measuring the maximum diameter of each inorganic filler as the major axis diameter. The values ​​corresponding to 50% and 90% of the cumulative frequency from the particle side with the small major axis diameter were defined as the 50% major axis length and the 90% major axis length, respectively. In addition, the diameter perpendicular to the maximum diameter of the inorganic filler was measured as the minor axis diameter, and the values ​​corresponding to 50% and 90% of the cumulative frequency from the particle side with the smaller minor axis diameter were defined as the 50% minor axis length and the 90% minor axis length, respectively.

[0053] (2) Aspect ratio of inorganic filler in resin film The aspect ratio (= long axis diameter / short axis diameter) of the inorganic filler was determined by observing the thickness cross section in the width direction of the obtained film (sample) using an electron microscope, extracting 100 inorganic fillers, measuring the maximum diameter of each inorganic filler as the long axis diameter and the direction perpendicular to the maximum diameter as the short axis diameter, and calculating the aspect ratio (= long axis diameter / short axis diameter). The value corresponding to 90% of the cumulative frequency from the particle side with the small aspect ratio was defined as the 90% average aspect ratio. When the inorganic filler was scaly, the average particle size of each filler, i.e., the major axis diameter, was divided by the average thickness of each filler to determine the particle size.

[0054] (3) Glass transition temperature (Tg), melting point (Tm), crystallization temperature (Tc) and relative crystallinity The raw material pellets and film were measured in accordance with JIS K7121:2012 using a differential scanning calorimeter Pyris1 DSC (PerkinElmer) at a temperature range of 25 to 380°C and a heating rate of 10°C / min. The glass transition temperature was determined from the inflection point of the DSC curve detected during the reheating process, the melting point was determined from the endothermic peak top temperature, and the crystallization temperature (Tc) was determined from the exothermic peak top temperature. The relative crystallinity of the film was calculated according to the following formula. Relative crystallinity (%) = {(|ΔHm|-|ΔHc|) / ΔHm} × 100 Here, ΔHc is the heat of crystallization, and ΔHm is the heat of crystal fusion.

[0055] (4) Dielectric constant The obtained film (sample) was measured according to JIS C2565:1992. The measurements were taken using the cavity resonator method under conditions of 23°C temperature, 50% RH humidity, and 10GHz frequency. Ta.

[0056] (5) Dielectric tangent The obtained film (sample) was measured according to JIS C2565:1992. The measurements were taken using the cavity resonator method under conditions of 23°C temperature, 50% RH humidity, and 10GHz frequency. Ta. In this example, a dielectric tangent of less than 0.004 was evaluated as ◯, and a dielectric tangent of 0.004 or more was evaluated as x.

[0057] (6) Linear expansion coefficient The obtained film (sample) was cut to a size of 4 mm x 10 mm, and a tensile test was performed in the MD or TD direction using a thermomechanical analysis (TMA) device (Hitachi High-Tech Science Corporation, model: TMA / SS7100) at a constant heating rate (5°C / min) in the temperature range of 30°C to 150°C while applying a load of 1 mN, and the coefficient of linear expansion (CTE) was measured from the elongation of the film with respect to temperature. In this example, an average CTE in MD / TD of less than 30 ppm / °C was evaluated as ◯, 30 ppm or more and less than 40 ppm / °C as △, and more than 40 ppm / °C as ×.

[0058] (7) 200℃ Lamination Evaluation Five sheets of the obtained film (sample) were stacked to a size of 100 mm x 100 mm, then sandwiched between two metal plates and hot pressed under conditions of temperature = 200 ° C, pressure = 3 MPa, and time = 20 minutes to obtain a laminate. The obtained laminate was allowed to absorb moisture using a pressure cooker tester under conditions of temperature = 121 ° C, pressure = 2 atm, humidity = 100% RH, and time = 2 hours. It was then immersed in a solder bath at 240 ° C for 20 seconds to evaluate deformation. In this example, samples that showed no deformation after immersion in the solder bath were evaluated as ◯, and samples in which swelling occurred between the films, peeling occurred, or the film was not crystallized and deformed were evaluated as x.

[0059] <Raw materials> [Polyetherketoneketone resin (A)] (A)-1: KEPSTAN7002 (Arkema, (a-1):(a-2)=70:30 (mol%), Tg=158° C., Tm=331° C.) (A)-2: KEPSTAN6002 (Arkema, (a-1):(a-2)=60:40 (mol%), Tg=153° C., Tm=306° C.) Here, Tg indicates the glass transition temperature, and Tm indicates the melting point.

[0060] [Inorganic filler (B)] (B)-1: Fluorine-containing mica (Topy Industries PDM-5L (flat shape), particle size (D50) at 50% cumulative number from the small particle size side is 6.4 μm when measured with a laser diffraction particle size distribution analyzer) (B)-2: Potassium tetrasilicic mica (MK-100 (flat shape) manufactured by Co-op Chemical Co., Ltd., particle size (D50) at 50% cumulative number from the small particle size side is 5.1 μm when measured with a laser diffraction particle size distribution analyzer) (B)-3: Fused silica (Denka GT130MC (spherical shape), particle size (D50) at 50% cumulative number from the small particle size side is 0.6 μm when measured with a laser diffraction particle size distribution analyzer)

[0061] [Other resins (C)] (C)-1: Polyether ether ketone VESTAKEEP 3300G (manufactured by Daicel-Evonik, Tg=143°C, Tm=338°C) (C)-2: Polyetherimide Ultem 1000-1000 (Sabic, Tg: 212°C, Tm=none)

[0062] Example 1 A mixed composition obtained by mixing (A)-1 and (B)-1 as shown in Table 1 was kneaded at 360°C using a Φ40 mm co-rotating single screw extruder equipped with a T-die, and then extruded from the T-die and cooled with a casting roll at approximately 150°C to produce a film (sample) with a thickness of 50 μm. The 50% major axis length and 50% minor axis length of the inorganic filler (B)-1 in the film were 0.5 μm and 0.1 μm, respectively, the 90% major axis length and 90% minor axis length were 2.9 μm and 0.2 μm, respectively, and the average aspect ratio was 9. The relative crystallinity of the film was 2%.

[0063] (Examples 2 to 4) A film (sample) was produced in the same manner as in Example 1, except that the mixing mass ratio of (A)-1, (A)-2, (B)-1 and (C)-2 was changed as shown in Table 1. The 50% major axis length and 50% minor axis length of the inorganic filler (B)-1 in each film were 0.5 μm and 0.1 μm, respectively, the 90% major axis length and 90% minor axis length were 2.9 μm and 0.2 μm, respectively, and the average aspect ratio was 9. In addition, the relative crystallinity of the film was 1% for the film of Example 2, 1% for the film of Example 3, and 1% for the film of Example 4.

[0064] Example 5 A mixed composition obtained by mixing (A)-1 and (B)-1 as shown in Table 1 was supplied to a Plastograph Mixer manufactured by Toyo Seiki Seisakusho, and melt-kneaded for 5 minutes at a temperature of 360°C and a rotation speed of 60 rpm to obtain a resin composition. This resin composition was sandwiched between two metal plates and press-molded under the conditions of a temperature of 360°C, a pressure of 3 MPa, and a molding time of 30 seconds, and then quenched with water to 150°C or less to produce a resin film (sample) having a thickness of 200 μm. The 50% major axis length and 50% minor axis length of the inorganic filler (B)-1 in the resin film were 0.7 μm and 0.2 μm, respectively, the 90% major axis length and 90% minor axis length were 4.2 μm and 0.4 μm, respectively, and the average aspect ratio was 8. In addition, the relative crystallinity of the film was 0%.

[0065] (Comparative Examples 1 and 2) A film (sample) was produced in the same manner as in Example 1, except that the mixing mass ratio of (B)-1, (C)-1, and (C)-2 was changed as shown in Table 1. The 50% major axis length and 50% minor axis length of the inorganic filler (B)-1 in each film were 0.5 μm and 0.1 μm, respectively, the 90% major axis length and 90% minor axis length were 2.9 μm and 0.2 μm, respectively, and the average aspect ratio was 9. In addition, the relative crystallinity of the film was 1% and 100% in Comparative Example 1 and Comparative Example 2, respectively.

[0066] Comparative Example 3 A film (sample) was produced in the same manner as in Example 5, except that the mixing mass ratio of (A)-1, (A)-2, and (B)-2 was changed as shown in Table 1. The 50% major axis length and 50% minor axis length of the inorganic filler (B)-2 in the film were 1.1 μm and 0.2 μm, respectively, the 90% major axis length and 90% minor axis length were 3.3 μm and 0.7 μm, respectively, and the average aspect ratio was 5. In addition, the relative crystallinity of the film was 0%.

[0067] Comparative Example 4 A film (sample) was produced in the same manner as in Example 5, except that the mixing mass ratio of (A)-1, (A)-2, and (B)-3 was changed as shown in Table 1. The 50% major axis length and 50% minor axis length of the inorganic filler (B)-3 in the film were 0.2 μm and 0.2 μm, respectively, the 90% major axis length and 90% minor axis length were 0.8 μm and 0.8 μm, respectively, and the average aspect ratio was 1. In addition, the relative crystallinity of the film was 0%.

[0068] Comparative Example 5 A film (sample) was produced in the same manner as in Example 1, except that the mixing mass ratio of (A)-1 and (A)-2 was changed as shown in Table 1. The relative crystallinity of the film was 2%.

[0069] [Table 1]

[0070] The results of Examples 1 to 5 in Table 1 above show that by using PEKK resin blended with fluorine-containing inorganic fillers of a specific diameter, it is possible to soften and laminate at 200°C, and to achieve both low dielectric tangent and low linear expansion.

[0071] On the other hand, in the case of the blend of PEEK and PEI or the single PEI having no crystallinity as in Comparative Examples 1 and 2, the Tg was high and lamination was not possible at 200°C. When inorganic fillers having diameters outside the range specified in the present invention were used as in Comparative Examples 3 and 4, the effect of reducing the linear expansion coefficient was insufficient. When no inorganic filler was included as in Comparative Example 5, the dielectric tangent value was high and the linear expansion coefficient value was also high. [Industrial Applicability]

[0072] According to the present invention, it is possible to provide a thermoplastic resin film that can be laminated at a low temperature and has excellent thermal properties. For example, when used as an insulating film for a circuit board, etc., since the resin film of the present invention can be laminated at a low temperature, it can conform to the shape of the circuit board and fill it, and can exhibit high functionality as an insulating film. Therefore, the technology according to the present invention is of great industrial value.

Claims

1. A resin film containing polyether ketone ketone (A) and an inorganic filler (B), A resin film in which the 50% length (median diameter) of the inorganic filler (B) in the major axis direction in the resin film is 0.25 μm or more and 1.0 μm or less, and the 50% length (median diameter) of the inorganic filler (B) in the minor axis direction in the resin film is 0.03 μm or more and 0.25 μm or less.

2. The resin film according to claim 1 , wherein the aspect ratio of the inorganic filler (B) in the resin film is 5 or more and 10 or less.

3. The resin film according to claim 1, wherein the inorganic filler (B) has a 90% length in the major axis direction of 1 μm or more and 5 μm or less, and a 90% length in the minor axis direction of 0.01 μm or more and 0.5 μm or less.

4. The resin film according to claim 1, wherein the polyether ketone ketone (A) has a repeating unit (a-1) represented by the following structural formula (1) and / or a repeating unit (a-2) represented by the following structural formula (2): 【Chemical 1】 【Chemistry 2】

5. The resin film according to claim 4, wherein the content ratio of the repeating unit (a-1) to the repeating unit (a-2) is (a-1):(a-2)=55:45 to 75:25 (mol %).

6. The resin film according to claim 1, having a glass transition temperature of 150°C or higher and 170°C or lower.

7. The resin film according to claim 1 , wherein the inorganic filler (B) is synthetic mica.

8. 2. The resin film according to claim 1, wherein the inorganic filler (B) is 10 parts by mass or more and less than 45 parts by mass per 100 parts by mass of the polyether ketone ketone (A).

9. The resin film according to claim 1, having a relative crystallinity of 90% or less.

10. The resin film according to claim 1, having a linear expansion coefficient of 50 ppm / °C or less.

11. The resin film according to claim 1, which is used for a circuit board.

12. A circuit board material having a configuration in which the resin film according to any one of claims 1 to 11 and a conductor are laminated.

13. A circuit board comprising the circuit board material of claim 12.

14. An electronic device comprising the circuit board according to claim 13.

Citation Information

Patent Citations

  • Flexible substrate on which electronic devices are formed

    JP2009545878A

  • Organic light-emitting element including a flexible substrate and method for manufacturing the same

    JP2015536555A

  • Laminate, and production method thereof