Method for slicing crystal material, method for manufacturing wafer, and member consisting of crystal material
The method of forming controlled modified layers within crystalline materials addresses the challenge of unintended crack extensions, enabling efficient production of large-area thin plates and wafers from hard materials like diamond.
Patent Information
- Application Number
- JP2023045708
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-22
- Publication Date
- 2024-10-04
AI Technical Summary
Existing methods for slicing hard single-crystal materials like SiC, GaN, sapphire, and diamond struggle with difficulty in achieving large-area thin plates due to unintended crack extensions and require expensive, precise equipment for narrow windows, making it challenging to produce inch-sized wafers.
A method involving the formation of planar modified layers with first and second modified portions at specific intervals within the crystal material, allowing controlled crack bonding and peeling along the (100) plane, preventing crack extension in the cleavage direction.
Enables stable peeling of large-area thin plates from crystalline materials, facilitating the production of large-diameter wafers with reduced cutting costs and equipment complexity, suitable for semiconductor applications.
Smart Images

Figure 2024135160000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for slicing a crystalline material, a method for producing a wafer, and a component made of a crystalline material. [Background technology]
[0002] When manufacturing substrates for semiconductor devices such as ICs and LSIs, it is necessary to slice wafers from ingots of single crystal material. Until now, slicing has generally been performed using a wire saw. In recent years, the use of hard single crystal materials such as SiC (silicon carbide), GaN (gallium nitride), sapphire, and diamond, which have excellent thermal conductivity, chemical resistance, and mechanical properties, as wafers has been considered, but the hardness of these single crystal materials makes slicing with a wire saw difficult.
[0003] As a method for slicing such hard single crystal materials, the following Patent Document 1 proposes a technique in which a laser beam having a wavelength that is transparent to the single crystal material is irradiated with the focal point positioned inside the ingot to form a modified layer and cracks on the intended cutting surface, and an external force is applied to break the ingot along the intended cutting surface on which the modified layer and cracks have been formed, thereby separating the ingot from the wafer. A similar slicing method is described in the following Non-Patent Document 1. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2016-111145 A [Non-patent literature]
[0005] [Non-Patent Document 1] Akito Ohno and 3 others, "Research on Laser Slicing of Diamond - Observation of Processing Traces Formed Inside the Material -", Proceedings of the 2017 Japan Society for Precision Engineering Spring Meeting Academic Lecture Conference, p.429-430 Summary of the Invention [Problem to be solved by the invention]
[0006] Single crystal materials have planes (cleavage planes) that are easy to peel off, and the direction of the cleavage planes is determined by the orientation of the crystal. For example, the (111) plane is the cleavage plane of diamond, but the (111) plane is tilted at about 55 degrees to the (100) plane. In this way, the direction of the cleavage planes in relation to the crystal planes is significantly different in diamond, so even if you try to cleave the (100) plane, it often ends up bending in a direction that cleaves in the (111) plane.
[0007] When diamond is used as a wafer, the surface that is generally used is the (100) plane. When attempting to cleave diamond along the (100) plane by applying the method described in Patent Document 1, if the modified layer has a small area of up to about 100 μm on a side, the crack can be extended along the (100) plane and the diamond can be peeled off along the (100) plane. However, since the modified layer undergoes volume expansion due to graphitization, if a modified layer with a larger area is formed, the crack will extend to an area away from the modified layer. When the crack extends a certain distance away from the modified layer, the direction of the crack bends from the direction parallel to the modified layer and the crack begins to extend toward the cleavage plane, making it difficult to cleave along the (100) plane parallel to the modified layer.
[0008] In the method described in Non-Patent Document 1, the dot pitch, line pitch, etc. are precisely controlled to prevent large cracks. Therefore, in order to process a narrow window with good reproducibility, it is necessary to use high-precision and expensive equipment. In addition, if the wafer is changed, the irradiation conditions of the laser light must be reconsidered, which requires complicated work. Therefore, it is desirable to provide a slicing method with a wide window and a wide range of options for materials and equipment.
[0009] When using the wafer as a substrate material for semiconductor devices, an inch-sized wafer is required. However, for the reasons mentioned above, it is difficult to obtain a diamond wafer of the required size using the methods described in Patent Document 1 and Non-Patent Document 1.
[0010] SUMMARY OF THE PRESENT EMBODIMENTS An object of the present invention is to provide a slicing method for a crystal material that can peel off a large-area thin plate from the crystal material. [Means for solving the problem]
[0011] In order to achieve the above-mentioned objective, the method for slicing a crystalline material according to the present invention is characterized in that planar modified layers including a first modified portion are formed at multiple locations spaced apart from each other on the same plane inside a raw material made of a crystalline material, the crystalline material having cleavage properties, and then a second modified portion is formed between adjacent modified layers, and by forming the second modified portion, cracks generated in each of the adjacent modified layers are joined, thereby peeling off a plate (thin plate) from the raw material.
[0012] The above method can prevent unintended crack propagation during slicing (e.g., propagation of a crack in the cleavage plane direction), making it possible to peel a large-area thin plate from a material.
[0013] In order to obtain such an effect, it is preferable that the modified layer before the second modified portion is formed has a size that does not allow a crack to propagate in the cleavage plane direction.
[0014] In addition, it is preferable that the interval between the adjacent modified layers before the formation of the second modified portion is set to a size such that cracks generated in the respective modified layers do not join together.
[0015] In the above-described slicing method, the crystalline material can be diamond, and the first modified portion and the second modified portion can be graphitized. Volume expansion accompanying graphitization causes a crack-existing region to form around the first modified portion. By providing the second modified portion between adjacent modified layers, the cracks in the crack-existing regions of the adjacent modified layers are bonded together, allowing the thin plate to be peeled off from the material.
[0016] By using diamond as the crystalline material and arranging the modified layers formed in multiple locations on the same plane parallel to the (100) plane, it is possible to peel off the thin plate along the (100) plane direction.
[0017] The first modified portions of the modified layer can be formed at aligned positions in the row direction and the column direction of the modified layer, whereby the intervals between the first modified portions are uniform, and therefore cracks occurring around the first modified portions in the modified layer can be stably bonded.
[0018] By providing, as the first modified portion of the modified layer, main modified portions formed at aligned positions in each of the row and column directions of the modified layer, and sub-modified portions located between adjacent main modified portions in the row direction and between adjacent main modified portions in the column direction, a modified layer with a larger area can be formed, making it possible to efficiently slice large-area thin plates from the material.
[0019] By slicing the material using the method described above, it is possible to form large diameter wafers.
[0020] Furthermore, the member made of a crystalline material according to the present invention is characterized in that planar modified layers including a first modified portion are formed at multiple locations on the same plane and spaced apart from each other within a material made of the crystalline material, the crystalline material has cleavage properties, and a second modified portion is formed between adjacent modified layers.
[0021] By subjecting a member made of such a crystalline material to post-treatment such as application of an external force, the thin plate can be separated from the base material with the plane including all of the modified layers as the interface. Effect of the Invention
[0022] As described above, according to the present invention, it is possible to stably peel off a large-area thin plate from a crystal material. [Brief description of the drawings]
[0023] [Figure 1] 2 is a cross-sectional view showing an outline of a first modified portion formed inside a material, taken in a direction perpendicular to the (100) plane. FIG. [Diagram 2] FIG. 2 is a cross-sectional view showing an outline of a modified layer formed inside a material in a direction perpendicular to the (100) plane. [Diagram 3] FIG. 3 is a cross-sectional view taken along line AA in FIG. 2. [Figure 4] 3 is a cross-sectional view taken along line AA in FIG. 2, showing modified layers formed at a plurality of locations. [Diagram 5] 3 is a cross-sectional view taken along line AA in FIG. 2, showing a material provided with a second modified portion. [Figure 6] 5 is a cross-sectional view showing the stress distribution in the state of FIG. 4 in a direction perpendicular to the (100) plane. [Figure 7] FIG. 6 is a cross-sectional view showing the stress distribution in the state shown in FIG. 5 in a direction perpendicular to the (100) plane. [Figure 8] 1A to 1C are cross-sectional views taken in a direction perpendicular to the (100) plane, showing a process of peeling a thin plate from a material. [Figure 9] 3 is a cross-sectional view taken along the line AA in FIG. 2, showing another arrangement pattern of the first modified portions. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] Hereinafter, an embodiment of a crystal material slicing method according to the present invention will be described with reference to FIGS.
[0025] In this embodiment, the crystalline material to be sliced is a single crystal or polycrystal, and is a material having cleavage. In many cases, single crystal materials have cleavage, but polycrystalline materials, such as highly oriented polycrystalline materials in which the crystal grains are aligned, have cleavage, and can be included in the slicing target of this embodiment. In addition, materials that can be considered as substantially single crystals, which are produced by heteroepitaxial growth in which diamond is grown on a heterogeneous material substrate, are also included in the "single crystal material". In the following explanation, a slicing method will be explained using diamond as an example of a single crystal material. Single crystal diamond has useful physical properties such as high hardness, high thermal conductivity, wide light transmission wavelength band and band gap, low dielectric constant, and excellent chemical stability, and is therefore considered to be promising as a material for next-generation semiconductor device substrates or high-precision magnetic sensors.
[0026] The slicing method according to this embodiment includes (1) a modified layer forming step of forming planar modified layers at multiple locations inside a material (ingot or block), (2) a crack joining step of joining cracks in each modified layer formed in the modified layer forming step, and (3) a peeling step of peeling a thin plate from the material 1 that has been through the crack joining step. By going through each step in the order of (1) to (3), the material 1 made of diamond is sliced. Each step will be described in detail below.
[0027] [Modified layer formation process] The modified layer forming step is a step of forming a planar modified layer 3 including a large number of dot-shaped first modified portions 2 inside a base material 1 made of a single crystal material, as shown in FIG.
[0028] The diamond material 1 is manufactured by a high-temperature, high-pressure (HTPT) method or a chemical vapor deposition (CVD) method. There are three types of diamond: Ia, IIa, and IIb. Any type of diamond can be used. The surface 11 of the material 1 is polished to be flat and extends in a direction parallel to the (100) plane.
[0029] As shown in Fig. 1, the first modified region 2 is formed by irradiating a surface 11 of the material 1 with laser light L having a wavelength that transmits through the material 1 and focusing the laser light L from the surface 11 to a predetermined depth inside the material 1 using an objective lens 4. In the first modified region 2, the diamond structure is graphitized by pyrolysis. The first modified region 2 is formed so as to extend from the focusing area C toward the optical axis direction, and the length in the optical axis direction is approximately 10 µm to 50 µm.
[0030] As shown in FIG. 2, the first modified regions 2 are formed at a plurality of locations inside the material 1 at a predetermined pitch P. Each of the first modified regions 2 is formed by focusing laser light at the same depth from the surface 11. Therefore, each of the first modified regions 2 is located on the same plane parallel to the (100) plane. The position of the focusing portion C is determined according to the thickness of the thin plate 9 (see FIG. 8) to be obtained; for example, by making the position of the focusing portion C deeper, the thickness of the thin plate 9 can be increased. The focusing portion C can be set to a depth of, for example, 50 μm to 700 μm from the surface 11.
[0031] The laser light is emitted from a laser light source (not shown) in the form of, for example, picosecond pulses. The pulse width (pulse duration) can be selected within the range of several ps to several hundred ps.
[0032] In the first modified region 2, volume expansion occurs due to graphitization, and cracks occur around the region due to a wedge effect caused by the volume expansion. FIGS. 1 and 2 are diagrams conceptually showing the structure around the first modified region 2, in which the black parts represent the graphitized first modified region 2, and the gray parts around the first modified region 2 represent regions 5 where cracks have occurred due to the volume expansion of the first modified region 2 (hereinafter referred to as "crack existing regions"). As shown in FIG. 1, the pitch P of adjacent first modified regions 2 is set to a size that connects the crack existing regions 5 in the (100) plane direction. For example, by setting the pitch P to about 10 μm to 30 μm, the crack existing regions 5 of adjacent first modified regions 2 can be connected to each other.
[0033] As shown in Figures 2 and 3, the first modified portion 2 and the crack-existing region 5 around the first modified portion 2 form a planar modified layer 3 extending in the (100) plane direction. Here, "planar" means that the modified layer 3 appears to be formed in a planar shape when viewed with the naked eye. The modified layer 3 is formed, for example, by repeating a procedure of scanning the pulsed laser along the surface 11 of the material 1 in the X direction, and then scanning the pulsed laser again in the X direction at a position shifted in the Y direction (direction perpendicular to the X direction) along the surface 11. As a result, the first modified portions 2 are formed in a state where they are aligned at multiple positions in each of the row direction (X direction) and column direction (Y direction).
[0034] 3, the first modified parts 2 adjacent in the X direction and the Y direction have their respective crack existing regions 5 connected to each other. It is not necessary for the crack existing region 5 of any of the first modified parts 2 to be connected to all of the surrounding crack existing regions 5, and it is sufficient that the crack existing region 5 is connected to at least one of the surrounding crack existing regions 5. In addition, there is no particular problem even if a small number of independent crack existing regions 5 that are not connected to any of the surrounding crack existing regions 5 are formed in the modified layer 3.
[0035] As already mentioned, if the area of the modified layer 3 is too large, the stress caused by the volume expansion will accumulate, causing the cracks to naturally extend even without the application of an external force to the material 1. As a result, cracks will develop in areas away from the modified layer 3, and a crack α (hereinafter referred to as an "out-of-plane crack") will develop in the cleavage plane direction (the direction of the (111) plane) as shown by the dashed line in Fig. 2. When a crack α develops in the cleavage plane direction in this way, it becomes difficult to peel the thin plate along the (100) plane.
[0036] Therefore, it is preferable to make the area of the modified layer 3 as large as possible within a range in which the cracks α in the cleavage plane direction do not extend. For example, if the modified layer 3 has a square outline with one side S of about 50 μm to 100 μm when viewed from the front surface 11 side, it is possible to prevent the occurrence of such cracks α in the cleavage plane direction. The shape of the modified layer 3 may be other shapes such as a square, a rectangle, a circle, etc.
[0037] The modified layers 3 described above are formed at intervals Q at multiple locations inside the material 1, as shown in FIG. 4. The regions with the intervals Q become non-modified regions 6 that are not graphitized. The modified layers 3 are disposed at the same depth from the surface 11, that is, on the same plane parallel to the (100) plane. In this case, the intervals Q between adjacent modified layers 3 are made larger than the pitch P of the first modified portions 2 contained in the modified layer 3 (Q>P). As shown by the arrows in FIG. 6, a stress acts on the edge of each modified layer 3 in a direction that propagates the crack, but the intervals Q between adjacent modified layers 3 are set so that the stress is slightly smaller than the stress when the crack propagates between the adjacent modified layers 3 and the cracks in both modified layers 3 join together.
[0038] If the interval Q between the modified layers 3 is too small, the cracks in the adjacent modified layers 3 will connect without the application of external force, and if the interval Q is too large, the cracks in the adjacent modified layers 3 will not connect even after the formation of the second modified portion 7 described below, making it difficult to peel off a large-area thin plate. From the above perspectives, it is preferable that the interval Q between the adjacent modified layers 3 is greater than 30 μm and less than or equal to 1 mm. From the perspectives of mass productivity and stability, it is even more preferable that the interval Q is greater than 50 μm and less than or equal to 100 μm.
[0039] The number of modified layers 3 formed inside the raw material 1 is arbitrary. Therefore, in addition to forming four modified layers 3 in one raw material 1 as shown in Fig. 4, five or more modified layers 3 may be formed, or three or less modified layers 3 may be formed.
[0040] [Crack joining process] In the crack joining process, as shown in FIG. 5, a dot-shaped second modified portion 7 is newly formed in the non-modified region 6 between adjacent modified layers 3, for example, in the middle position between adjacent modified layers 3. The shape and formation method of the second modified portion 7 are the same as those of the first modified portion 2 formed in the modified layer 3. That is, the laser light L is focused at the same depth as the focusing position when forming the first modified portion 2, and the material is modified (graphitized) to form the second modified portion 7. A new crack existing region 8 is formed around the second modified portion 7 due to its volume expansion.
[0041] In the stress accumulation state shown in FIG. 6, when the second modified portion 7 is provided in the non-modified region 6 between the adjacent modified layers 3, as shown in FIG. 5 and FIG. 7, a new crack generated with the formation of the second modified portion 7 triggers a chain reaction of the cracks in the adjacent modified layers 3 through the new crack existing region 8. In this case, the entire region surrounded by the line connecting the adjacent second modified portions 7 often becomes the new crack existing region 8. Even if the number of second modified portions 7 formed is less (for example, one) than the number of first modified portions 2 (five in FIG. 5) of the first modified portions 2 of the other modified layer 3 facing the first modified portions 2 arranged on the edge of one of the adjacent modified layers 3, the cracks can be connected between the adjacent modified layers 3. In FIG. 5, one second modified portion 7 is provided in each of the non-modified regions 6 sandwiched between the adjacent modified layers 3, but the number of second modified portions 7 provided in each non-modified region 6 may be two or more. Furthermore, it is not necessary to provide the second modified portion 7 in all of the non-modified regions 6 sandwiched between adjacent modified layers 3 of the material 1, and the second modified portion 7 may be formed only in some of the non-modified regions 6.
[0042] [Peeling process] By applying an external force to the material 1 (a member made of a crystalline material) on which multiple modified layers 3 and second modified portions 7 have been formed by the above procedure, cracks generated in each modified layer 3 reach the edge of the material 1, and the thin plate 9 is separated from the material 1 with the plane including all modified layers 3 as the interface, as shown in FIG. 8. The external force can be applied, for example, by applying an impact to the side surface of the material 1. Thereafter, the modified layers 3 remaining on the peeled thin plate 9 are removed by polishing or the like to obtain a wafer. The peeling process can also be performed by etching, in addition to applying an external force to the material 1 as described above.
[0043] In the existing slicing method as described in Patent Document 1, it was difficult to peel off a large-area thin plate 9 because the extension of the crack α (see FIG. 2) in the cleavage plane direction was unavoidable. In the slicing method of the present embodiment, however, small-area modified layers 3 are formed at multiple locations with appropriate intervals so that the extension of the crack α in the cleavage plane direction does not occur, and then a second modified portion 7 is newly formed between adjacent modified layers 3, so that the crack extends in a chain reaction, and the large-area thin plate 9 is peeled off. This makes it possible to slice a large-area thin plate 9, for example, a thin plate 9 of 1 mm square or more, or even an inch-sized thin plate 9, from the material 1. This makes it possible to increase the diameter of the diamond wafer. Since the thickness of the modified layer 3 is at most about 50 μm, the cutting allowance required for slicing is reduced, and the material 11 can be used economically. In addition, compared to the slicing method described in Non-Patent Document 1, the window can be widened and the options for materials and devices can be expanded.
[0044] Moreover, according to this embodiment, the thin plate 9 can be peeled off in a direction along the (100) plane. While the (111) plane is difficult to smooth by mechanical polishing in a later process, the (100) plane can be easily smoothed by polishing. Therefore, by peeling off the thin plate 9 in a direction along the (100) plane, it is possible to obtain the advantage that the thin plate 9 can be polished in a later process and easily used as a wafer. Substrates with a (100) surface are in the greatest demand for applications of diamond single crystals, including semiconductor elements and semiconductor devices, and the present invention is of great significance in that it has made it possible to make such substrates larger in area.
[0045] FIG. 9 shows another example of the arrangement pattern of the first modified portions 2 formed in the modified layer 3. In the embodiment shown in FIG. 9, the first modified portions 2 of the modified layer 3 have main modified portions 2a formed at positions aligned in the row direction X and column direction Y of the modified layer 3, and sub modified portions 2b located between adjacent main modified portions 2a in the row direction and between adjacent main modified portions 2a in the column direction. With such an arrangement pattern of the first modified portions 2a, 2b, the area of each modified layer 3 can be increased while suppressing the extension of the crack α in the cleavage plane direction. Therefore, it is possible to efficiently obtain a thin plate 9 with a larger area.
[0046] In the above embodiment, the modified layer 3 is formed by concentrating a laser beam inside the material 11, but the method of forming the planar modified layer 3 is not limited to this, and any method capable of forming a planar modified layer 3 can be adopted. For example, a planar modified layer 3 including a large number of first modified portions 2 may be formed by implanting an ion beam into the material to graphitize it, and further embrittling the ion-implanted layer by annealing or etching. In this case, a laser beam is irradiated between a plurality of modified layers 3 located on the same plane to form dot-shaped second modified portions 7, thereby enabling slicing of the material 1.
[0047] Furthermore, although diamond has been used as an example of a crystalline material, the slicing method described above can be widely used for slicing crystalline materials that are difficult to slice using a wire saw and have cleavage properties, such as SiC, GaN, sapphire, etc. [Explanation of symbols]
[0048] 1. Materials 2. First reforming section 2a Main reforming section 2b Sub-reforming section 3 Modification layer 5. Crack area 7 Second Reforming Section 8 New crack areas 9 thin plate
Claims
1. A planar modified layer including a first modified portion is formed at a plurality of locations on the same plane at intervals within a material made of a crystalline material, the crystalline material having cleavage properties; Next, a second modified portion is formed between adjacent modified layers, A method for slicing crystalline material, in which the formation of the second modified portion causes cracks generated in each of the adjacent modified layers to bond, thereby peeling off a thin plate from the raw material.
2. 2. The method for slicing a crystal material according to claim 1, wherein the modified layer before the second modified portion is formed has a size that does not allow a crack to propagate in the cleavage plane direction.
3. A method for slicing a crystal material as described in claim 1, wherein the distance between adjacent modified layers before forming the second modified portion is set to a size such that cracks generated in each modified layer do not join together.
4. 2. The method for slicing a crystal material according to claim 1, wherein the crystal material is diamond, and the first modified portion and the second modified portion have a graphitized structure.
5. 2. The method for slicing a crystal material according to claim 1, wherein the crystal material is diamond, and the modified layers formed in a plurality of places are arranged on the same plane parallel to a (100) plane.
6. 2. The method for slicing a crystal material according to claim 1, wherein the first modified portions of the modified layer are formed at positions aligned in both the row direction and the column direction of the modified layer.
7. A method for slicing a crystalline material as described in claim 1, wherein the first modified portion of the modified layer comprises main modified portions formed at aligned positions in each of the row and column directions of the modified layer, and sub-modified portions located between adjacent main modified portions in the row direction and between adjacent main modified portions in the column direction.
8. A method for manufacturing a wafer, comprising slicing the material by the method according to any one of claims 1 to 7 to form a wafer.
9. A planar modified layer including a first modified portion is formed at a plurality of locations on the same plane at intervals within a material made of a crystalline material, the crystalline material having cleavage properties; A member made of a crystalline material, characterized in that a second modified portion is formed between adjacent modified layers.
Citation Information
Patent Citations
Method for manufacturing diamond substrate
JP2023029250A
Cutting method for processing material
WO2017199784A1
Processing device and processing method
WO2020213478A1
Generation method of wafer
JP2016111145A
Cited By
Diamond processing method
WO2025047896A1